Conductive polymer dispersion, conductive laminate and method for producing same

A conductive polymer dispersion with a π-conjugated conductive polymer and unsaturated aliphatic alcohol compound forms a laminate with sustained conductivity after four-fold stretching, addressing the conductivity loss issue in existing technologies.

JP7595534B2Active Publication Date: 2024-12-06SHIN ETSU POLYMER CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021110676
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-07-02
Publication Date
2024-12-06
Estimated Expiration
2041-07-02

AI Technical Summary

Technical Problem

Conductive layers formed from existing conductive polymer dispersions lose conductivity after being stretched four times, failing to maintain sufficient conductivity.

Method used

A conductive polymer dispersion containing a π-conjugated conductive polymer, polyanion, unsaturated aliphatic alcohol compound, and silicone emulsion, which is applied to a base material, then stretched and crystallized to form a conductive laminate with improved conductivity.

Benefits of technology

The conductive laminate maintains sufficient conductivity even after being stretched four times, facilitating the production of conductive films with enhanced durability and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595534000001
    Figure 0007595534000001
Patent Text Reader

Abstract

To provide a conductive polymer dispersion liquid that can form a conductive layer having sufficient conductivity even after being stretched, and a conductive laminate including the same and a method for producing the same.SOLUTION: A conductive polymer dispersion liquid contains a conductive complex containing a π-conjugated conductive polymer and a polyanion, water, silicone emulsionized in the water, and an unsaturated aliphatic alcohol compound having an unsaturated bond between carbon atoms and a hydroxy group in each molecule. The unsaturated aliphatic alcohol compound is preferably, for example, cis-2-butene-1,4-diol, trans-2-butene-1,4-diol, 2-butyn-1,4-diol, and 2,4-hexadiyne-1,6-diol or the like.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a conductive polymer dispersion containing a π-conjugated conductive polymer, a conductive laminate, and a method for producing the same. [Background technology]

[0002] Conductive films with releasability (antistatic release films) are sometimes used in the manufacture of electronic devices, etc. Patent Document 1 discloses an antistatic film obtained by applying a conductive polymer dispersion containing a conductive complex and a silicone emulsion to a film substrate, curing the coating, and then stretching the conductive film to provide a conductive layer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2016-013668 A Summary of the Invention [Problem to be solved by the invention]

[0004] The conductive layer and conductive film formed from the conductive polymer dispersion of Patent Document 1 have sufficient conductivity after being stretched twice, but the conductivity after being stretched four times is not necessarily sufficient (Example 2 of Patent Document 1).

[0005] The present invention provides a conductive polymer dispersion capable of forming a conductive layer having sufficient conductivity even after stretching treatment, a conductive laminate using the same, and a method for producing the same. [Means for solving the problem]

[0006] [1] A conductive polymer dispersion liquid containing a conductive complex containing a π-conjugated conductive polymer and a polyanion, water, silicone emulsified in the water, and an unsaturated aliphatic alcohol compound having an unsaturated bond between carbon atoms and a hydroxyl group in the molecule. [2] The conductive polymer dispersion according to [1], wherein the unsaturated aliphatic alcohol compound is a diol. [3] The conductive polymer dispersion liquid according to [1] or [2], wherein the unsaturated aliphatic alcohol compound has 4 or more and 8 or less carbon atoms. [4] The conductive polymer dispersion according to [1], wherein the unsaturated aliphatic alcohol compound includes at least one selected from the group consisting of cis-2-butene-1,4-diol, trans-2-butene-1,4-diol, 2-butyne-1,4-diol, and 2,4-hexadiyne-1,6-diol. [5] The conductive polymer dispersion according to any one of [1] to [4], wherein the π-conjugated conductive polymer is poly(3,4-ethylenedioxythiophene) or the polyanion is polystyrenesulfonic acid. [6] The conductive polymer dispersion according to any one of [1] to [5], further comprising polyvinyl alcohol. [7] The conductive polymer dispersion according to any one of [1] to [6], further comprising an alkali compound. [8] A method for producing a conductive laminate, comprising applying the conductive polymer dispersion according to any one of [1] to [7] to at least a part of a surface of a substrate. [9] The method for producing a conductive laminate according to [8], wherein the substrate is an amorphous film substrate, the method comprising: applying the conductive polymer dispersion to at least a portion of a surface of the amorphous film substrate to obtain a coated film; and heating and stretching the coated film to obtain a stretched film.

[10] A conductive laminate comprising a substrate and a conductive layer formed on at least a portion of the surface of the substrate, the conductive layer being a cured layer of the conductive polymer dispersion according to any one of [1] to [7]. Effect of the Invention

[0007] According to the conductive polymer dispersion of the present invention, a conductive layer having sufficient conductivity even after four-fold stretching can be formed. The conductive layer of the conductive laminate of the present invention has sufficient conductivity even after being stretched four times. According to the method for producing a conductive laminate of the present invention, the above-mentioned conductive laminate can be easily produced.

[0008] This invention is believed to contribute to SDGs Goal 12, "Responsible Consumption and Production."

[0009] In this specification and claims, the lower limit and upper limit of a numerical range indicated with "to" are included in the numerical range. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] ≪Conductive polymer dispersion liquid≫ A first aspect of the present invention is a conductive polymer dispersion liquid containing a conductive complex containing a π-conjugated conductive polymer and a polyanion, water, silicone emulsified in the water, and an unsaturated aliphatic alcohol compound having an unsaturated bond between carbon atoms and a hydroxyl group in the molecule.

[0011] [Conductive composite] The conductive complex contained in the conductive polymer dispersion of this embodiment contains a π-conjugated conductive polymer and a polyanion. The polyanion in the conductive complex is doped into the π-conjugated conductive polymer to form a conductive complex having electrical conductivity. In the polyanion, only a part of the anionic groups is doped into the π-conjugated conductive polymer, and there are excess anionic groups that are not involved in the doping. Since the excess anionic groups are hydrophilic groups, the conductive composite has water dispersibility.

[0012] (π-conjugated conductive polymer) The π-conjugated conductive polymer may be an organic polymer whose main chain is composed of a π-conjugated system, and examples thereof include polypyrrole-based conductive polymers, polythiophene-based conductive polymers, polyacetylene-based conductive polymers, polyphenylene-based conductive polymers, polyphenylenevinylene-based conductive polymers, polyaniline-based conductive polymers, polyacene-based conductive polymers, polythiophenevinylene-based conductive polymers, and copolymers thereof. From the viewpoint of stability in air, polypyrrole-based conductive polymers, polythiophenes, and polyaniline-based conductive polymers are preferred, and from the viewpoint of transparency, polythiophene-based conductive polymers are more preferred.

[0013] Polythiophene-based conductive polymers include polythiophene, poly(3-methylthiophene), poly(3-ethylthiophene), poly(3-propylthiophene), poly(3-butylthiophene), poly(3-hexylthiophene), poly(3-heptylthiophene), poly(3-octylthiophene), poly(3-decylthiophene), poly(3-dodecylthiophene), poly(3-octadecylthiophene), poly(3-bromothiophene), poly(3-chlorothiophene), and poly(3-iodothiophene). thiophene), poly(3-cyanothiophene), poly(3-phenylthiophene), poly(3,4-dimethylthiophene), poly(3,4-dibutylthiophene), poly(3-hydroxythiophene), poly(3-methoxythiophene), poly(3-ethoxythiophene), poly(3-butoxythiophene), poly(3-hexyloxythiophene), poly(3-heptyloxythiophene), poly(3-octyloxythiophene), poly(3-decyloxythiophene), poly(3-dodecyloxythiophene), oxythiophene), poly(3-octadecyloxythiophene), poly(3,4-dihydroxythiophene), poly(3,4-dimethoxythiophene), poly(3,4-diethoxythiophene), poly(3,4-dipropoxythiophene), poly(3,4-dibutoxythiophene), poly(3,4-dihexyloxythiophene), poly(3,4-diheptyloxythiophene), poly(3,4-dioctyloxythiophene), poly(3,4-didecyloxythiophene), poly(3,4-di dodecyloxythiophene), poly(3,4-ethylenedioxythiophene), poly(3,4-propylenedioxythiophene), poly(3,4-butylenedioxythiophene), poly(3-methyl-4-methoxythiophene), poly(3-methyl-4-ethoxythiophene), poly(3-carboxythiophene), poly(3-methyl-4-carboxythiophene), poly(3-methyl-4-carboxyethylthiophene), and poly(3-methyl-4-carboxybutylthiophene). Examples of polypyrrole-based conductive polymers include polypyrrole, poly(N-methylpyrrole), poly(3-methylpyrrole), poly(3-ethylpyrrole), poly(3-n-propylpyrrole), poly(3-butylpyrrole), poly(3-octylpyrrole), poly(3-decylpyrrole), poly(3-dodecylpyrrole), poly(3,4-dimethylpyrrole), poly(3,4-dibutylpyrrole), poly(3-carboxypyrrole), poly(3-methyl-4-carboxypyrrole), poly(3-methyl-4-carboxyethylpyrrole), poly(3-methyl-4-carboxybutylpyrrole), poly(3-hydroxypyrrole), poly(3-methoxypyrrole), poly(3-ethoxypyrrole), poly(3-butoxypyrrole), poly(3-hexyloxypyrrole), and poly(3-methyl-4-hexyloxypyrrole). Examples of polyaniline-based conductive polymers include polyaniline, poly(2-methylaniline), poly(3-isobutylaniline), poly(2-anilinesulfonic acid), and poly(3-anilinesulfonic acid). Among these π-conjugated conductive polymers, poly(3,4-ethylenedioxythiophene) is particularly preferable because of its excellent conductivity, transparency, and heat resistance. The conductive composite may contain one type of π-conjugated conductive polymer, or two or more types of polymers.

[0014] (Polyanion) A polyanion is a polymer having two or more monomer units each having an anionic group in the molecule. The anionic group of the polyanion functions as a dopant for a π-conjugated conductive polymer, improving the conductivity of the π-conjugated conductive polymer. The anion group of the polyanion is preferably a sulfo group or a carboxy group. Specific examples of such polyanions include polymers having a sulfo group, such as polystyrene sulfonic acid, polyvinyl sulfonic acid, polyallyl sulfonic acid, polyacrylic acid esters having a sulfo group, polymethacrylic acid esters having a sulfo group (for example, poly(4-sulfobutyl methacrylate, polysulfoethyl methacrylate, polymethacryloyloxybenzenesulfonic acid), poly(2-acrylamido-2-methylpropanesulfonic acid), and polyisoprene sulfonic acid; and polymers having a carboxy group, such as polyvinyl carboxylic acid, polystyrene carboxylic acid, polyallyl carboxylic acid, polyacrylic acid, polymethacrylic acid, poly(2-acrylamido-2-methylpropanecarboxylic acid), and polyisoprene carboxylic acid. The polyanion may be a homopolymer in which a single monomer is polymerized, or a copolymer in which two or more monomers are polymerized. Among these polyanions, polymers having a sulfo group are preferred, and polystyrene sulfonic acid is more preferred, since they can provide higher electrical conductivity. The polyanions may be used alone or in combination of two or more kinds. The mass average molecular weight of the polyanion is preferably from 20,000 to 1,000,000, and more preferably from 100,000 to 500,000. The mass average molecular weight is the average molecular weight based on mass measured by gel filtration chromatography and calculated in terms of pullulan.

[0015] The content of the polyanion in the conductive complex is preferably in the range of 1 part by mass to 1000 parts by mass, more preferably 10 parts by mass to 700 parts by mass, and even more preferably 100 parts by mass to 500 parts by mass, per 100 parts by mass of the π-conjugated conductive polymer. If the content of the polyanion is equal to or greater than the lower limit, the doping effect on the π-conjugated conductive polymer tends to be stronger, and the conductivity becomes higher. On the other hand, if the content of the polyanion is equal to or less than the upper limit, the π-conjugated conductive polymer can be sufficiently contained, so that sufficient conductivity can be ensured.

[0016] The content of the conductive complex relative to the total mass of the conductive polymer dispersion of this embodiment is preferably from 0.01 to 5% by mass, more preferably from 0.1 to 3% by mass, and even more preferably from 0.3 to 1.5% by mass. When the content is at least as high as the lower limit of the above range, the conductivity of the conductive layer formed by applying the conductive polymer dispersion can be further improved. When it is equal to or less than the upper limit of the above range, the dispersibility of the conductive complex in the conductive polymer dispersion can be improved, and a uniform conductive layer can be formed.

[0017] [Unsaturated fatty alcohol compounds] The one or more unsaturated aliphatic alcohol compounds contained in the conductive polymer dispersion of this embodiment are alcohols having one or more double bonds or triple bonds between carbon atoms in the molecule and one or more hydroxyl groups (hydroxyl groups) in the molecule.

[0018] From the viewpoint of further improving the conductivity of the conductive layer formed from the conductive polymer dispersion of this embodiment after stretching, the unsaturated aliphatic alcohol compound is preferably a diol having two hydroxyl groups. From the same viewpoint, the unsaturated aliphatic alcohol compound preferably has 4 or more and 12 or less carbon atoms, more preferably 4 or more and 10 or less, further preferably 4 or more and 8 or less, and particularly preferably 4 or more and 6 or less carbon atoms. From the same viewpoint, the number of unsaturated bonds contained in the unsaturated aliphatic alcohol compound is preferably 1 or more and 4 or less, more preferably 1 or more and 3 or less, and even more preferably 1 or 2.

[0019] The unsaturated aliphatic alcohol compound is preferably at least one selected from the group consisting of cis-2-butene-1,4-diol, trans-2-butene-1,4-diol, 2-butyne-1,4-diol, and 2,4-hexadiyne-1,6-diol. Further examples include 3,6-dimethyl-4-octyne-3,6-diol, 2,5-dimethyl-3-hexyne-2,5-diol, and the like.

[0020] In the conductive polymer dispersion of this embodiment, the total content of the unsaturated aliphatic alcohol compounds relative to 100 parts by mass of the conductive complex is preferably 10 parts by mass or more and 10,000 parts by mass or less, more preferably 100 parts by mass or more and 5,000 parts by mass or less, and even more preferably 500 parts by mass or more and 3,000 parts by mass or less. When it is in the above preferred range, the effect of the present invention is further improved.

[0021] The content of the unsaturated aliphatic alcohol compound relative to the total mass of the conductive polymer dispersion of this embodiment is preferably 0.01 mass % or more and 20 mass % or less, more preferably 1 mass % or more and 15 mass % or less, and even more preferably 5 mass % or more and 10 mass % or less. When the amount is within the above range, the electrical conductivity of the conductive layer after stretching can be sufficiently improved.

[0022] [Dispersion medium] Examples of the dispersion medium contained in the conductive polymer dispersion of this embodiment include water, an organic solvent, and a mixture of water and an organic solvent. The unsaturated aliphatic alcohol compound does not fall under the category of the dispersion medium contained in the conductive polymer dispersion liquid of this embodiment.

[0023] Examples of the organic solvent include alcohol-based solvents, ether-based solvents, ketone-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. Examples of alcohol-based solvents include monohydric alcohols such as methanol, ethanol, 1-propanol, 2-propanol, 2-methyl-2-propanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, allyl alcohol, propylene glycol monomethyl ether, and ethylene glycol monomethyl ether. Examples of the ether solvent include diethyl ether, dimethyl ether, ethylene glycol, propylene glycol, and propylene glycol dialkyl ether. Examples of the ketone solvent include diethyl ketone, methyl propyl ketone, methyl butyl ketone, methyl isopropyl ketone, methyl isobutyl ketone, methyl amyl ketone, diisopropyl ketone, methyl ethyl ketone, acetone, and diacetone alcohol. Examples of the ester solvent include ethyl acetate, propyl acetate, and butyl acetate. Examples of aromatic hydrocarbon solvents include benzene, toluene, xylene, ethylbenzene, propylbenzene, and isopropylbenzene. The organic solvents may be used alone or in combination of two or more kinds.

[0024] Since the conductive complex has high dispersibility in water, the dispersion medium of the conductive polymer dispersion of this embodiment is preferably an aqueous dispersion medium containing water. The content of water in the conductive polymer dispersion liquid of this embodiment relative to the total dispersion medium can be, for example, 50% by mass or more and 100% by mass or less, preferably 60% by mass or more and 100% by mass or less, and more preferably 70% by mass or more and 100% by mass or less. As the dispersion medium other than water, a monohydric alcohol is preferable.

[0025] [Silicone emulsion] Silicone emulsion is a silicone (silicone resin) emulsified in water. Silicone emulsion obtained by emulsion polymerization of organosiloxane monomer is preferable. Here, examples of surfactants for emulsifying silicone include anionic surfactants, cationic surfactants, and nonionic surfactants. The silicone is preferably a curable silicone. The curable silicone is a silicone having a reactive group, and can be reacted and cured by a known method. Specifically, addition curable silicone and condensation curable silicone can be mentioned. Among them, addition curable silicone is preferable from the viewpoint of improving releasability (peelability).

[0026] Examples of addition-curable silicones include linear polymers having siloxane bonds (e.g., polydimethylsiloxane), which have a vinyl group at at least one end of the linear polymer, and which have a hydrogen silane at at least one end of the linear polymer. Specific examples of addition curing silicone resins include KM-3951, KM768, and X-52-6015 (all manufactured by Shin-Etsu Chemical Co., Ltd.). Addition-curing silicones cure by forming a crosslinked structure through an addition reaction.

[0027] Examples of condensation-curable silicones include linear polymers having siloxane bonds (e.g., polydimethylsiloxane), in which at least one end of the linear polymer has a hydroxy group, and at least one end of the linear polymer has a hydrogen atom. The condensation reaction type silicone resin hardens by forming a crosslinked structure through a condensation reaction.

[0028] The content of silicone relative to 100 parts by mass of the conductive complex contained in the conductive polymer dispersion of this embodiment is, for example, preferably 10 parts by mass or more and 10,000 parts by mass or less, more preferably 100 parts by mass or more and 5,000 parts by mass or less, and even more preferably 500 parts by mass or more and 3,000 parts by mass or less. It can be considered that almost all of the non-volatile components of the silicone emulsion are silicone.

[0029] [Hardening agent] The conductive polymer dispersion of this embodiment may contain a curing agent that accelerates the curing of the curable silicone. The curing agent is selected depending on the type of curable silicone used. In the case of addition reaction type silicone, it is preferable to use a platinum catalyst as a curing agent. Specific examples of platinum catalysts include CAT-PL-50T and CAT-PM-10A (manufactured by Shin-Etsu Chemical Co., Ltd.). In the case of a condensation reaction type silicone resin, it is preferable to use an organotin catalyst (such as an organotin acylate catalyst) as a curing agent. A specific example of the organotin catalyst is CAT-PS-8S (manufactured by Shin-Etsu Chemical Co., Ltd.).

[0030] [Polyvinyl alcohol] The conductive polymer dispersion of this embodiment preferably contains polyvinyl alcohol. Polyvinyl alcohol functions as a dispersant for the conductive complex and also has the function of improving the stretchability of the conductive layer formed on the substrate. In other words, the conductive layer containing polyvinyl alcohol is easy to follow the stretching of the film, and the conductive layer is less likely to crack or peel off, and the conductivity is high. In addition, polyvinyl alcohol also plays a role as a binder resin in the conductive layer. Therefore, even if the film is not stretched, the conductive polymer dispersion contains polyvinyl alcohol, so that defects in the conductive layer can be reduced and the conductivity can be improved.

[0031] Polyvinyl alcohol is generally produced by saponifying the acetyl group of polyvinyl acetate, but some acetyl groups may not be saponified. Therefore, polyvinyl alcohol may contain vinyl acetate units. The saponification degree of the polyvinyl alcohol used in this embodiment is preferably 70% or more and 100% or less. If the saponification degree of the polyvinyl alcohol is equal to or more than the lower limit, it can be easily dissolved in water. The degree of polymerization of polyvinyl alcohol is preferably from 500 to 10000, and more preferably from 1000 to 5000. When the degree of polymerization of polyvinyl alcohol is equal to or more than the lower limit, the stretchability of the conductive layer can be sufficiently improved, and when it is equal to or less than the upper limit, the solubility in water can be improved. The degree of polymerization of polyvinyl alcohol is a value measured by a known method. The conductive polymer dispersion liquid may contain one type of polyvinyl alcohol or two or more types of polyvinyl alcohol.

[0032] The content of polyvinyl alcohol relative to 100 parts by mass of the conductive composite contained in the conductive polymer dispersion of this embodiment is, for example, preferably 1 part by mass or more and 2000 parts by mass or less, more preferably 10 parts by mass or more and 1000 parts by mass or less, and even more preferably 100 parts by mass or more and 500 parts by mass or less. When the content is equal to or greater than the lower limit, the dispersibility of the conductive complex in the conductive polymer dispersion can be improved, and the stretchability of the conductive layer can be increased. When the content is equal to or less than the upper limit, the decrease in electrical conductivity can be further suppressed.

[0033] [Alkaline compounds] The conductive polymer dispersion of this embodiment may contain an alkaline compound. Examples of the alkaline compound include inorganic alkali, amine compounds, and nitrogen-containing aromatic cyclic compounds. Only one type of alkaline compound may be contained, or two or more types may be contained.

[0034] Examples of inorganic alkalis include sodium hydroxide, potassium hydroxide, calcium hydroxide, ammonia, sodium hydrogen carbonate, potassium hydrogen carbonate, and ammonium hydrogen carbonate. The content of the inorganic alkali relative to the total mass of the conductive polymer dispersion is, for example, 0.1 to 1 mass %. When the silicone emulsion is an emulsion containing an addition reaction type silicone, it is preferable to use an inorganic alkali as the alkali compound. Aliphatic amines or aromatic amines can be catalyst poisons for the platinum catalyst of the curing agent of the addition reaction type silicone, which can lead to insufficient curing of the coating film. On the other hand, inorganic alkalis do not become catalyst poisons.

[0035] The amine compound may be any of primary amines, secondary amines, tertiary amines, and quaternary ammonium salts. For convenience, quaternary ammonium salts are classified as amine compounds. The amine compound may have a substituent selected from a linear or branched alkyl group having 2 to 12 carbon atoms, an aryl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, an alkylene group having 2 to 12 carbon atoms, an arylene group having 6 to 12 carbon atoms, an aralkylene group having 7 to 12 carbon atoms, and an oxyalkylene group having 2 to 12 carbon atoms.

[0036] Specific examples of primary amines include aniline, toluidine, benzylamine, and ethanolamine. Specific examples of secondary amines include diethanolamine, dimethylamine, diethylamine, dipropylamine, diphenylamine, dibenzylamine, and dinaphthylamine. Specific examples of the tertiary amine include triethanolamine, trimethylamine, triethylamine, tripropylamine, tributylamine, triphenylamine, tribenzylamine, and trinaphthylamine. Specific examples of quaternary ammonium salts include tetramethylammonium salts, tetraethylammonium salts, tetrapropylammonium salts, tetraphenylammonium salts, tetrabenzylammonium salts, tetranaphthylammonium salts, etc. Examples of an anion that is paired with ammonium include hydroxide ions. Of these, tertiary amines are preferred, and trimethylamine, triethylamine, tripropylamine, or tributylamine is more preferred.

[0037] The nitrogen-containing aromatic cyclic compound has an aromatic ring containing at least one nitrogen atom, and the nitrogen atom may be contained in the aromatic ring in the form of any of a secondary amine, a tertiary amine, and a quaternary ammonium salt. Specific examples of the nitrogen-containing aromatic cyclic compound include pyrrole, imidazole, 2-methylimidazole, 2-propylimidazole, 2-undecylimidazole, 2-phenylimidazole, N-methylimidazole, 1-(2-hydroxyethyl)imidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, and 1-cyanoethyl-2-ethyl-4-methylimidazole. Examples of the aryl imidazole include ethyl imidazole, 2-phenyl-4,5-dihydroxymethyl imidazole, 1-acetyl imidazole, 4,5-imidazoledicarboxylic acid, dimethyl 4,5-imidazoledicarboxylate, benzimidazole, 2-aminobenzimidazole, 2-aminobenzimidazole-2-sulfonic acid, 2-amino-1-methylbenzimidazole, 2-hydroxybenzimidazole, 2-(2-pyridyl)benzimidazole, 1-ethyl-3-methylimidazolium hydroxide, pyridine, etc. Among these, imidazole, 2-methylimidazole, 2-propylimidazole, or pyridine is more preferred.

[0038] The alkali compound preferably has a solubility in water of 0.1 g / 100 ml (10° C.) or more. An alkali compound having a solubility in water of 0.1 g / 100 ml (10° C.) or more is easily dissolved in a dispersion medium, and the storage stability of the conductive polymer dispersion of this embodiment is improved.

[0039] The content of the alkali compound contained in the conductive polymer dispersion of this embodiment is preferably 0.7 times or more by mole, more preferably 0.9 times or more by mole, relative to the amount added at the inflection point of the neutralization titration curve obtained by neutralizing titrating the conductive complex with the alkali compound, i.e., the number of moles of the neutralization equivalent. If the content of the alkali compound is less than 0.7 times by mole relative to the neutralization equivalent of the conductive complex, the storage stability of the conductive polymer dispersion may decrease. The content of the alkali compound is preferably 1.5 times or less by mole, and more preferably 1.2 times or less by mole, relative to the number of moles of the neutralization equivalent of the conductive complex.

[0040] The pH (25°C) of the conductive polymer dispersion of this embodiment is preferably 10 or less, and more preferably 9 or less. If the pH exceeds 10, the storage stability of the conductive polymer dispersion may decrease. On the other hand, the pH is preferably 3 or more, and more preferably 5 or more. The pH is a value measured using a pH meter calibrated by a known method.

[0041] [Other additives] The conductive polymer dispersion of this embodiment may contain other additives. The additives are not particularly limited as long as the effects of the present invention can be obtained. For example, surfactants, inorganic conductive agents, antifoaming agents, coupling agents, antioxidants, ultraviolet absorbing agents, etc. can be used. However, the additives are other than the above-mentioned π-conjugated conductive polymer, polyanion, unsaturated aliphatic alcohol compound, dispersion medium, polyvinyl alcohol, and alkaline compound. The surfactant may be a nonionic, anionic or cationic surfactant, with the nonionic surfactant being preferred from the standpoint of storage stability. A polymer surfactant such as polyvinylpyrrolidone may also be added. Examples of the inorganic conductive agent include metal ions, conductive carbon, etc. Metal ions can be generated by dissolving a metal salt in water. The antifoaming agent includes silicone resin, polydimethylsiloxane, silicone oil, and the like. The coupling agent may be a silane coupling agent having an epoxy group, a vinyl group or an amino group. Examples of the antioxidant include phenol-based antioxidants, amine-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, and sugars. Examples of the ultraviolet absorber include benzotriazole-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, salicylate-based ultraviolet absorbers, cyanoacrylate-based ultraviolet absorbers, oxanilide-based ultraviolet absorbers, hindered amine-based ultraviolet absorbers, and benzoate-based ultraviolet absorbers.

[0042] When the conductive polymer dispersion contains the additive, the content ratio thereof is appropriately determined depending on the type of additive, but can be, for example, in the range of 0.001 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the conductive composite.

[0043] <Method of manufacturing conductive polymer dispersion> An example of a method for producing the conductive polymer dispersion of this embodiment is a method in which an alkali compound, polyvinyl alcohol, an unsaturated aliphatic alcohol compound, a silicone emulsion, and a curing agent are added in this order to an aqueous dispersion of a conductive complex. The aqueous dispersion of the conductive complex may be obtained by chemically oxidizing and polymerizing a monomer that forms a π-conjugated conductive polymer in an aqueous solution of a polyanion, or a commercially available product may be used.

[0044] The chemical oxidative polymerization can be carried out using a known catalyst and oxidizing agent. Examples of the catalyst include transition metal compounds such as ferric chloride, ferric sulfate, ferric nitrate, and cupric chloride. Examples of the oxidizing agent include persulfates such as ammonium persulfate, sodium persulfate, and potassium persulfate. The oxidizing agent can return the reduced catalyst to its original oxidized state.

[0045] <Conductive laminate> A second aspect of the present invention is a conductive laminate comprising a substrate and a conductive layer formed on at least a partial surface of the substrate, the conductive layer being a cured layer of the conductive polymer dispersion of the first aspect.

[0046] [Conductive layer] The conductive layer may be formed over the entire surface of any surface of the substrate, or over a portion of the entire surface. In the conductive film, it is preferable that a conductive layer of substantially uniform thickness is formed over substantially the entire surface of one surface or the other surface of the film substrate. When a conductive layer is formed only over a portion of the surface of the substrate, the conductive layer may be, for example, a fine conductive pattern such as a circuit or an electrode, or the conductive layer may be provided on the same surface and the conductive layer may be not provided on the same surface and may be roughly divided.

[0047] The average thickness of the conductive layer is, for example, preferably 10 nm or more and 100 μm or less, more preferably 20 nm or more and 50 μm or less, and even more preferably 30 nm or more and 30 μm or less. When the average thickness of the conductive layer is equal to or greater than the lower limit, high conductivity can be exhibited, and when the average thickness is equal to or less than the upper limit, the adhesion of the conductive layer to the substrate is further improved.

[0048] [Base material] The substrate may be a substrate made of an insulating material or a substrate made of a conductive material. The shape of the substrate is not particularly limited, and examples thereof include a shape mainly having a flat surface, such as a film or a substrate. Examples of insulating materials include glass, synthetic resin, and ceramics. The conductive material may be a metal, a conductive metal oxide, carbon, or the like.

[0049] (Film substrate) When a film substrate is used as the substrate, the conductive laminate becomes a conductive film. The film substrate may be, for example, a plastic film made of a synthetic resin, such as ethylene-methyl methacrylate copolymer resin, ethylene-vinyl acetate copolymer resin, polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyvinyl alcohol, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyacrylate, polycarbonate, polyvinylidene fluoride, polyarylate, styrene-based elastomer, polyester-based elastomer, polyethersulfone, polyetherimide, polyetheretherketone, polyphenylene sulfide, polyimide, cellulose triacetate, cellulose acetate propionate, etc. From the viewpoint of improving the adhesion between the film substrate and the conductive layer, the synthetic resin for the film substrate is preferably a polyester resin, and among these, polyethylene terephthalate is preferable.

[0050] The synthetic resin for the film substrate may be either amorphous or crystalline. The film substrate may be either unstretched or stretched. The film substrate may be subjected to a surface treatment such as a corona discharge treatment, a plasma treatment, or a flame treatment in order to further improve the adhesion of the conductive layer.

[0051] The average thickness of the film substrate is preferably 5 μm to 500 μm, more preferably 20 μm to 200 μm. If the average thickness of the film substrate is equal to or more than the lower limit, the film is less likely to break, and if the average thickness is equal to or less than the upper limit, the film can have sufficient flexibility. The average thickness of the film substrate is calculated by measuring the thickness at 10 randomly selected points and averaging the measured values.

[0052] (Glass substrate) Examples of the glass substrate include an alkali-free glass substrate, a soda-lime glass substrate, a borosilicate glass substrate, and a quartz glass substrate. If the substrate contains an alkali component, the conductivity of the conductive layer tends to decrease, so among the above glass substrates, an alkali-free glass is preferred. Here, the alkali-free glass refers to a glass composition in which the content of the alkali component is 0.1 mass% or less with respect to the total mass of the glass composition.

[0053] The average thickness of the glass substrate is preferably from 100 μm to 3000 μm, more preferably from 100 μm to 1000 μm. If the average thickness of the glass substrate is equal to or more than the lower limit, the substrate is less likely to break, and if the average thickness is equal to or less than the upper limit, the substrate can contribute to a thinner conductive laminate. The average thickness of the glass substrate is calculated by measuring the thickness at 10 randomly selected points and averaging the measured values.

[0054] <Method for manufacturing conductive laminate> A third aspect of the present invention is a method for producing a conductive laminate, the method comprising: applying the conductive polymer dispersion of the first aspect to at least a part of a surface of a substrate to form a conductive layer. The conductive laminate of the second aspect can be produced by the production method of this aspect.

[0055] Examples of a method for applying (coating) the conductive polymer dispersion on an arbitrary surface of a substrate include a method using a coater such as a gravure coater, a roll coater, a curtain flow coater, a spin coater, a bar coater, a reverse coater, a kiss coater, a fountain coater, a rod coater, an air doctor coater, a knife coater, a blade coater, a cast coater, or a screen coater; a method using a sprayer such as an air spray, an airless spray, or a rotor dampening; and an immersion method such as dipping.

[0056] The amount of conductive polymer dispersion applied to the substrate is not particularly limited, but taking into consideration uniform and even application, conductivity, and film strength, a solid content of 0.01 g / m 2 More than 10.0g / m 2The following ranges are preferred:

[0057] The conductive layer can be formed by drying the coating film made of the conductive polymer dispersion applied onto the substrate to remove at least a portion of the dispersion medium and curing the coating film. Methods for drying the coating film include heat drying, vacuum drying, etc. Examples of heat drying that can be used include hot air heating and infrared heating. When applying heat drying, the heating temperature is appropriately set depending on the dispersion medium used, but is usually within the range of 50° C. to 200° C. Here, the heating temperature is the set temperature of the drying device. A suitable drying time within the above heating temperature range is preferably 0.5 minutes to 30 minutes, more preferably 1 minute to 15 minutes.

[0058] In the method for producing the conductive laminate of this embodiment, the conductive film that has been subjected to the stretching treatment can be produced as follows. The manufacturing method includes using an amorphous film substrate as the substrate, applying the conductive polymer dispersion to at least a part of the surface of the amorphous film substrate to obtain a coated film (coating step), and heating and stretching the coated film to obtain a stretched film (stretching step). The method may further include crystallizing the film heated in the stretching step (crystallization step). The coating step, stretching step, and crystallization step are described below.

[0059] [Coating process] The film substrate used in this step is not particularly limited as long as it is amorphous, and for example, it can be arbitrarily selected from the film substrates described above. In this step, the method for applying the coating material (conductive polymer dispersion) to the amorphous film substrate to obtain a coated film is not particularly limited, and for example, the above-mentioned coating methods can be applied.

[0060] [Stretching process] The stretching step is a step of heating and stretching the coated film to obtain a stretched film. The dispersion medium contained in the coating material may be dried by heating in this step, or may be dried in a separate drying step before being subjected to this step. By heating and stretching the coated film, a conductive film with a large area can be obtained even if the coated area is small, and the productivity of the conductive film is improved. The stretching may be uniaxial or biaxial, but when a uniaxially stretched film is used as the amorphous film substrate, it is preferable to stretch in a direction perpendicular to the stretching direction. For example, when a uniaxially stretched film stretched along the longitudinal direction is used as the amorphous film substrate, it is preferable to stretch along the width direction. The stretching ratio of the coated film is preferably from 2 to 20 times, more preferably from 3 to 15 times, and even more preferably from 4 to 10 times. The stretching ratio here is a stretching ratio in at least one axial direction, and may be a stretching ratio in each of two orthogonal axial directions.

[0061] As the heating method, for example, a conventional method such as hot air heating or infrared heating can be used. The heating temperature in the stretching step is preferably lower than the crystallization temperature of the amorphous film substrate, and is within the range of 50° C. to 150° C. Here, the heating temperature is the set temperature of the drying device. If the heating temperature in the stretching step is increased to the melting point of the material of the amorphous film substrate, the film may become too soft and stretching may become difficult.

[0062] [Crystallization process] The crystallization step is a step in which the stretched film is heated and then cooled to crystallize the amorphous film substrate. The heating temperature of the stretched film in the crystallization step is equal to or higher than the crystallization temperature of the amorphous film substrate, preferably equal to or higher than 200° C., more preferably equal to or higher than 220° C., and even more preferably equal to or higher than 240° C. If the heating temperature of the stretched film is equal to or higher than the lower limit, the amorphous film substrate can be sufficiently crystallized. On the other hand, from the viewpoint of preventing the film substrate from melting, the heating temperature of the stretched film is preferably equal to or lower than 300° C.

[0063] Since it is easily crystallized when heated at 200° C. or higher, the amorphous film substrate is preferably an amorphous polyethylene terephthalate film. When heated to 200°C or higher, at least a portion of the amorphous polyethylene terephthalate constituting the film substrate begins to melt. After melting, when cooled to a temperature below the crystallization temperature of polyethylene terephthalate, a portion of the molten amorphous polyethylene terephthalate crystallizes and solidifies. This allows the film substrate to become a crystalline polyethylene terephthalate film. The film substrate made of a crystalline polyethylene terephthalate film has excellent mechanical properties such as tensile strength.

[0064] The cooling method after heating is not particularly limited, and may be either blowing air at room temperature or allowing it to cool. Since the amorphous film substrate is prone to crystallization, it is preferable to cool the substrate at a slow temperature drop rate, specifically, at 200° C. / min or less. Through the above steps, a conductive film is obtained that has been subjected to the stretching step and the crystallization step. EXAMPLES

[0065] (Production Example 1) Production of polystyrene sulfonic acid 206 g of sodium styrenesulfonate was dissolved in 1000 ml of ion-exchanged water, and while stirring at 80° C., 1.14 g of an oxidizing agent solution of ammonium persulfate previously dissolved in 10 ml of water was added dropwise over 20 minutes, and the solution was stirred for 12 hours. 1000ml of sulfuric acid diluted to 10% by mass was added to the obtained sodium polystyrene sulfonate-containing solution, and about 1000ml of the solvent was removed from the obtained polystyrene sulfonic acid-containing solution by ultrafiltration. Next, 2000ml of ion-exchanged water was added to the remaining liquid, and about 2000ml of the solvent was removed by ultrafiltration to wash the polystyrene sulfonic acid with water. This water washing operation was repeated three times. Water in the resulting solution was removed under reduced pressure to obtain a colorless solid polystyrene sulfonic acid (PSS). The weight-average molecular weight of this PSS was measured using a high-performance liquid chromatography system equipped with a gel filtration chromatography column and pullulan manufactured by Showa Denko K.K. as a standard substance, and the molecular weight was found to be 300,000.

[0066] (Production Example 2) Production of PEDOT-PSS aqueous dispersion A solution in which 14.2 g of 3,4-ethylenedioxythiophene and 44.0 g of the polystyrenesulfonic acid obtained in Production Example 1 were dissolved in 2000 ml of ion-exchanged water was mixed at 20°C. The resulting mixed solution was kept at 20° C., and while stirring, 29.64 g of ammonium persulfate and 8.0 g of an oxidation catalyst solution of ferric sulfate dissolved in 200 ml of ion-exchanged water were slowly added, followed by stirring for 3 hours to carry out the reaction. 2000 ml of ion-exchanged water was added to the reaction solution, and about 2000 ml of the solution was removed by ultrafiltration. This procedure was repeated three times. Next, 200 ml of sulfuric acid diluted to 10% by mass and 2000 ml of ion-exchanged water were added to the obtained solution, about 2000 ml of the solution was removed by ultrafiltration, 2000 ml of ion-exchanged water was added to this, and about 2000 ml of the solution was removed by ultrafiltration. This operation was repeated three times. Furthermore, 2000 ml of ion-exchanged water was added to the obtained solution, and about 2000 ml of the solution was removed by ultrafiltration. This operation was repeated five times to obtain a polystyrene sulfonate-doped poly(3,4-ethylenedioxythiophene) aqueous dispersion (PEDOT-PSS aqueous dispersion) with a solid content concentration of 1.2 mass% and a PEDOT:PSS=1:3 (mass ratio).

[0067] (Production Example 3) Production of Conductive Polymer-Containing Liquid 0.30 g of sodium bicarbonate dissolved in 3.2 g of ion-exchanged water was added to 100 g of the PEDOT-PSS aqueous dispersion produced in Production Example 2 and stirred. Then, 40 g of a 5 mass % aqueous solution of polyvinyl alcohol (polymerization degree: 4500, saponification degree: 86.5 to 89.5 mol %, manufactured by Nippon Vinyl Acetate & Poval Co., Ltd., model number: JP45) was added, and this was used as conductive polymer-containing liquid A.

[0068] [Example 1] To 143.5 g of the conductive polymer-containing liquid A obtained in Production Example 3, 20 g of 2-butyne-1,4-diol was added, 81.8 g of an addition-curing silicone emulsion KM-3951 (manufactured by Shin-Etsu Chemical Co., Ltd., containing 30% by mass of non-volatile components and approximately 70% by mass of water) was added, and 4.0 g of a platinum catalyst CAT-PM-10A was added, and the mixture was diluted with 81.8 g of ion-exchanged water to obtain the desired conductive polymer dispersion. The mixing ratio of each of these materials is shown in Table 1. The obtained conductive polymer dispersion was applied onto an amorphous polyethylene terephthalate film using a No. 8 bar coater to obtain a coated film. The obtained coated film was stretched four times in each of two perpendicular axial directions at 100°C using a biaxial stretching device (Imoto Manufacturing Co., Ltd., 11A9) to obtain a stretched film. The stretched film was heated at 240°C for 30 seconds, and then slowly cooled so that the temperature drop rate was 100°C / min or less. This crystallized the amorphous polyethylene terephthalate film, and a conductive film having a conductive layer on the surface of the crystalline polyethylene terephthalate film was obtained. The surface resistance of the obtained conductive film was measured using a resistivity meter (Hiresta manufactured by Nitto Seiko Analytech) under the condition of an applied voltage of 10 V. The results are shown in Table 1. In the table, "1.00E+09" represents "1.00×10 9 " "In the table, "OVER" indicates that the surface resistance is so high that it cannot be measured.

[0069] [Example 2] A conductive film was obtained and measured in the same manner as in Example 1, except that 20 g of 2-butyne-1,4-diol was changed to 20 g of cis-2-butene-1,4-diol in Example 1. The results are shown in Table 1.

[0070] [Example 3] A conductive film was obtained and measured in the same manner as in Example 1, except that 20 g of 2-butyne-1,4-diol was changed to 20 g of trans-2-butene-1,4-diol in Example 1. The results are shown in Table 1.

[0071] [Example 4] A conductive film was obtained and measured in the same manner as in Example 1, except that 20 g of 2-butyne-1,4-diol was changed to 20 g of 2,4-hexadiyne-1,6-diol in Example 1. The results are shown in Table 1.

[0072] [Comparative Example 1] A conductive film was obtained and measured in the same manner as in Example 1, except that an unsaturated aliphatic alcohol compound having an unsaturated bond between carbon atoms and a hydroxyl group in the molecule was not added instead of the conductive polymer dispersion liquid of Example 1. The results are shown in Table 1.

[0073] [Table 1]

[0074] The conductive film of the Example containing the unsaturated aliphatic alcohol compound and the silicone emulsion had sufficient conductivity even after stretching four times in two perpendicular axial directions, whereas Comparative Example 1 not containing the unsaturated aliphatic alcohol compound showed no conductivity after the stretching.

Claims

1. a conductive polymer dispersion liquid containing a conductive complex containing a π-conjugated conductive polymer and a polyanion, water, silicone emulsified in the water, and an unsaturated aliphatic alcohol compound which is a diol compound having 4 to 8 carbon atoms and has one or two unsaturated bonds between carbon atoms in the molecule; The content of the unsaturated aliphatic alcohol compound relative to 100 parts by mass of the conductive composite is 10 parts by mass or more and 10,000 parts by mass or less, The conductive polymer dispersion has a content of the silicone of 10 parts by mass or more and 10,000 parts by mass or less relative to 100 parts by mass of the conductive complex.

2. 2. The conductive polymer dispersion according to claim 1, wherein the unsaturated aliphatic alcohol compound comprises at least one selected from the group consisting of cis-2-butene-1,4-diol, trans-2-butene-1,4-diol, 2-butyne-1,4-diol, and 2,4-hexadiyne-1,6-diol.

3. 3. The conductive polymer dispersion according to claim 1, wherein the π-conjugated conductive polymer is poly(3,4-ethylenedioxythiophene), or the polyanion is polystyrenesulfonic acid.

4. The conductive polymer dispersion according to any one of claims 1 to 3, further comprising polyvinyl alcohol.

5. The conductive polymer dispersion according to any one of claims 1 to 4, further comprising an alkali compound.

6. A method for producing a conductive laminate, comprising: applying the conductive polymer dispersion according to any one of claims 1 to 5 to at least a part of a surface of a substrate.

7. the substrate is an amorphous film substrate, and the conductive polymer dispersion is applied to at least a portion of the surface of the amorphous film substrate to obtain a coated film; The method for producing a conductive laminate according to claim 6 , further comprising: heating and stretching the coated film to obtain a stretched film.

8. A conductive laminate comprising a substrate and a conductive layer formed on at least a portion of the surface of the substrate, the conductive layer being a cured layer of the conductive polymer dispersion according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Conductive polymer and conductive composition containing the same, and film having coating film containing the polymer or the composition

    JP2014040549A

  • Antistatic peeling agent, antistatic peelable coating film, and antistatic peeling base material

    JP2014080608A

  • Production method of antistatic release film

    JP2016013668A

  • Conductive polymer dispersion liquid and method for producing the same, and conductive film and method for producing the same

    JP2019099738A

  • Antistatic release agent and antistatic release film

    WO2014042188A1