Ion conductive material, electrolyte, and battery

A novel ion conductive material with a specific composition and structure, produced by ball milling, addresses the low ionic conductivity of halide solid electrolytes, resulting in improved ionic conductivity and enhanced battery performance.

JP7595621B2Active Publication Date: 2024-12-06SUMITOMO CHEM CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022144851
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-09-12
Publication Date
2024-12-06
Estimated Expiration
2042-09-12

AI Technical Summary

Technical Problem

Halide solid electrolytes in lithium ion batteries have room for improvement in ionic conductivity.

Method used

An ion conductive material containing an alkali metal element, a tetravalent metal element, a halogen element, and a dopant element, with a specific composition and structure that includes an amorphous phase and crystallites dispersed in the amorphous phase, and a sea-island structure, achieved through ball milling of raw materials under inert conditions.

Benefits of technology

The material exhibits excellent ionic conductivity with low activation energy, enhancing the performance of electrochemical devices such as batteries by improving charge/discharge capacity and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595621000003
    Figure 0007595621000003
  • Figure 0007595621000004
    Figure 0007595621000004
  • Figure 0007595621000005
    Figure 0007595621000005
Patent Text Reader

Abstract

To provide an ion conductive substance having excellent ionic conductivity, an electrolyte, and battery.SOLUTION: An ion conductive substance contains an alkali metal element, a tetravalent metal element M, a halogen element, a dopant element X, and an oxygen element, wherein a content of the dopant element X is 50 mol% or less with respect to a content of the metal element M, and, in an X-ray diffraction chart obtained by measuring the ion conductive substance using a CuKα ray at 25°C, a diffraction peak having a half width of 2.0-10° in a range of a 2θ angle of 10-20°.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an ionically conductive material, an electrolyte, and a battery. [Background technology]

[0002] In recent years, solid electrolytes have been attracting attention as electrolytes used in electrochemical devices such as lithium ion batteries (Patent Documents 1 to 3). Compared with conventional electrolytic solutions, solid electrolytes are superior in high temperature durability, high voltage resistance, etc., and are therefore considered to be useful for improving battery performance such as safety, high capacity, rapid charge / discharge, and pack energy density.

[0003] As described in Patent Documents 1 to 3, a halide solid electrolyte containing lithium and metal elements other than lithium is known as a material used for the solid electrolyte of a lithium ion battery. Halide solid electrolytes are highly flexible and do not require sintering. 2 It has advantages that oxide- or sulfide-based solid electrolytes do not have, such as being highly safe because it does not emit harmful substances such as S. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2021002064 [Patent Document 2] International Publication No. 2021024785 [Patent Document 3] International Publication No. 2021220577 [Patent Document 4] Patent No. 6947321 Summary of the Invention [Problem to be solved by the invention]

[0005] However, there is still room for improvement in the ionic conductivity of halide solid electrolytes.

[0006] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide an ion-conductive material having excellent ion conductivity, and an electrolyte and a battery using the same. [Means for solving the problem]

[0007] The present invention includes the following embodiments [1] to [6]. [1] An ion-conductive substance comprising an alkali metal element, a tetravalent metal element M, a halogen element, a dopant element X, and an oxygen element, wherein the content of the dopant element X is 50 mol % or less based on the content of the metal element M, and which has a diffraction peak with a half-width of 2.0 to 10° in a 2θ angle range of 10 to 20° in an X-ray diffraction chart obtained by measurement at 25°C using CuKα radiation. [2] An ion-conductive material comprising an amorphous phase and crystallites dispersed in the amorphous phase, the material containing an alkali metal element, a tetravalent metal element M, a halogen element, a dopant element X, and an oxygen element, the crystallites having an average equivalent circular diameter of 20 nm or less. [3] The ion-conductive material according to [1] or [2], wherein the dopant element is at least one of P and S. [4] The ion conductive material according to any one of [1] to [3], wherein the content of the alkali metal element is 20 to 30 mol %, the content of the element M is 5 to 20 mol %, the content of the halogen element is 40 to 60 mol %, and the content of the dopant element X is 0.05 to 5 mol %, relative to the total amount of atoms contained in the ion conductive material. [5] An electrolyte comprising any one of the ion-conducting materials listed in [1] to [4]. [6] A battery comprising the electrolyte according to [5]. Effect of the Invention

[0008] According to the present invention, it is possible to provide an ion-conductive material having excellent ion conductivity, and an electrolyte and a battery using the same. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 shows X-ray diffraction charts obtained for Examples 1 to 6 and Comparative Examples 1 to 3. [Diagram 2] FIG. 2 is a graph showing the Arrhenius plots obtained for the ion-conductive materials of Examples 3, 5 and 6 and Comparative Examples 1 to 3. [Diagram 3] FIG. 3 is a TEM image of the ion-conductive material of Example 3. [Figure 4] FIG. 4 is a graph showing the results of cyclic voltammetry for Examples 1 to 5 and Comparative Example 1. [Diagram 5] FIG. 5 is a graph showing the results of the charge / discharge test of Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The ion-conductive substance (alkali metal-containing halide) of the present embodiment contains an alkali metal element, a tetravalent metal element M (also referred to as element M), a halogen element, a dopant element X, and an oxygen element, and the content of the dopant element X is 50 mol % or less relative to the content of the metal element M, and satisfies at least one of the following (1) and (2): (1) In an X-ray diffraction chart measured at 25° C. using CuKα radiation, it has a diffraction peak with a half-width of 2.0 to 10° in a 2θ angle range of 10 to 20°. (2) It contains an amorphous phase and crystallites dispersed in the amorphous phase, and the average particle size of the crystallites is 20 nm or less.

[0011] Regarding (1), the half width of the diffraction peak may be 4.0 to 9.0°, 4.5 to 8.8°, or 5.0 to 8.7°. In this specification, the half width is the full width at half maximum (FWHM) unless otherwise specified.

[0012] When (2) is satisfied, it can be said that the ion-conductive material has a sea-island structure. The average particle size of the crystallites may be 15 nm or less, 10 nm or less, or 6 nm or less. It may also be 1 nm or more, or 2 nm or more. The average particle size of the crystallites may be, for example, the average of the circle-equivalent diameters calculated from the area of ​​the crystallites in a microscopic image obtained by a transmission electron microscope. The average may be the average of all crystals recognized within a visual field (e.g., 188.6 nm x 188.6 nm) by the method described in the Examples.

[0013] The alkali metal element contained in the ion conductive material of this embodiment may be any one of Li, Na, K, Rb, and Cs, but may include at least one of Li, Na, and K, may include at least one of Li and Na, or may include Li.

[0014] The proportion of one type of alkali metal element among the alkali metal elements contained in the ion conductive material may be 80 mol % or more, 90 mol % or more, or 95 mol % or more. The one type of alkali metal element may be at least one of Li, Na, and K, at least one of Li and Na, or Li.

[0015] The content of the alkali metal element in the ion-conductive substance may be 20 to 30 mol %, 22 to 28 mol %, or 24 to 27 mol % relative to the total amount of atoms contained in the ion-conductive substance.

[0016] Examples of the element M include Zr, Ti, and Hf, and Zr is preferred. The ion conductive material may contain one or more tetravalent metal elements M. The content of the tetravalent metal in the ion conductive material may be 5 to 20 mol%, 8 to 16 mol%, 8 to 15 mol%, or 9 to 13 mol% based on the total amount of atoms contained in the ion conductive material. The element M may include Zr and Hf. Among the tetravalent metal elements contained in the ion conductive material, the content of Zr may be 70 mol% or more, 80 mol% or more, 85 mol% or more, or 90 mol% or more. Among the tetravalent metal elements contained in the ion conductive material, the content of Zr may be 99.9 mol% or less, 99 mol% or less, 98 mol% or less, 97 mol% or less, or 95 mol% or less.

[0017] The ion conductive material may contain a metal element M2 other than a tetravalent element (excluding an alkali metal element). The metal element M2 may be at least one of a divalent, trivalent, or pentavalent metal element. Examples of the divalent metal include alkaline earth metals and Zn. Examples of the trivalent metal element include Sc, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Yb, Lu, Y, Al, Ga, In, Bi, and Sb. Examples of the pentavalent metal element include Nb and Ta. Examples of the alkaline earth metal include at least one of Mg, Ca, Sr, and Ba, at least one of Mg and Ca, and may be Mg. The content of M2 may be 30 mol% or less, 20 mol% or less, 15 mol% or less, or 10 mol% or less with respect to the total amount of metal elements other than alkali metals contained in the ion conductive material (the total amount of the element M and the element M2). The content of M2 may be 0.1 mol% or more, 1 mol% or more, 2 mol% or more, 2 mol% or more, 3 mol% or more, or 5 mol% or more relative to the total amount of divalent to tetravalent metal elements contained in the ion conductive material.

[0018] The halogen element contained in the ion conductive material of the present embodiment may be any one of F, Cl, Br, and I, or may contain at least one of Cl, Br, and I, or may contain at least one of Cl and Br, or may contain Cl. The ion conductive material may contain only one type of halogen element, or may contain two or more types of halogen elements.

[0019] The content of the halogen element in the ion-conductive substance may be 40 to 60 mol %, 43 to 55 mol %, or 45 to 52 mol % based on the total amount of atoms contained in the ion-conductive substance.

[0020] The dopant element X contained in the ion conductive material of this embodiment has a tetrahedral structure of XO with four oxygen atoms. 4 The dopant element X may be an element capable of forming a dopant, and may be at least one of P and S. The dopant element X may include P. The dopant element X may also include S.

[0021] The content of the dopant element X in the ion conductive material may be 0.05 to 5 mol %, 0.1 to 3 mol %, 0.2 to 2 mol %, or 0.3 to 1 mol % relative to the total amount of atoms contained in the ion conductive material. The content of the dopant element X in the ion-conductive material is 50 mol % or less, may be 1 to 30 mol %, may be 1 to 20 mol %, or may be 2 to 10 mol % of the content of the tetravalent metal element M. The content of the dopant element X in the ion-conductive material may be 20 mol % or less, may be 15 mol % or less, may be 10 mol % or less, or may be 8 mol % or less of the content of the tetravalent metal element M. The content of the dopant element X in the ion-conductive material may be 1 to 10 mol %, or may be 2 to 6 mol %, of the content of the oxygen element.

[0022] The content of oxygen element in the ion-conductive substance may be 5 to 20 mol %, 8 to 18 mol %, or 10 to 16 mol % relative to the total amount of atoms contained in the ion-conductive substance.

[0023] The ion-conductive material of the present embodiment may contain a compound represented by the following composition formula (1) (also called an alkali metal-containing halide). A α M β X γ Z δ E η O ε (1) (In the formula, A is an alkali metal element, M is the above-mentioned tetravalent metal element M, X is the above-mentioned dopant element X, Z is a halogen element, and 1.5≦α≦3, 0.5≦β≦2, 0.005≦γ≦0.5, 3≦δ≦6, and 0.5≦ε≦2.) α may be in the range of 1.8≦α≦2.5, 1.9≦α≦2.3, or 1.95≦α≦2.2. The upper and lower limits of α can be combined in any desired manner. β may be in the range of 0.7≦β≦1.4, 0.8≦β≦1.2, or 0.9≦β≦1.1. The upper and lower limits of β can be combined in any desired manner. γ may be in the range of 0.01≦γ≦0.2, 0.02≦γ≦0.15, or 0.025≦γ≦0.10. The upper and lower limits of γ may be combined in any desired manner. δ may be 3.5≦δ≦5, 3.7≦δ≦4.3, or 3.8≦δ≦4.1. The upper and lower limits of δ can be combined in any manner. ε may be in the range of 0.7≦ε≦1.5, 0.8≦ε≦1.3, or 0.9≦ε≦1.1. The upper and lower limits for ε can be arbitrarily combined. E is an element other than A, M, X, and Z, and may be an element added or mixed in other than the essential elements. Examples of E include C, B, and N. η may be 0 to 0.1, 0 to 0.01, 0 to 0.001, or substantially 0.

[0024] The ion-conductive material of the present embodiment may contain a compound represented by the following composition formula (2) (also called an alkali metal-containing halide). A α M β M 2 ζ X γ Z δ E η O ε (2) (In the formula, A is an alkali metal element, M is the above-mentioned tetravalent metal element M, M 2 is a non-tetravalent metal element M 2 (However, alkali metal elements are excluded), where X is the dopant element X described above, and Z is a halogen element.) The preferred ranges for each of α, β, γ, δ, and ε in formula (2) may be the same as those exemplified as the ranges for α, β, γ, δ, and ε in formula (1). ζ may be in the range of 0.01≦ζ≦0.3, 0.03≦ζ≦0.2, or 0.05≦ζ≦0.15. The upper and lower limits of ζ can be arbitrarily combined. E is an element other than A, M, X, and Z, and may be an element added or mixed in other than the essential elements. Examples of E include C, B, and N. η may be 0 to 0.1, 0 to 0.01, 0 to 0.001, or substantially 0.

[0025] The activation energy of the ion conductive material of the present embodiment may be 0.35 eV or less, 0.33 eV or less, or 0.23 to 0.35 eV. The activation energy of the ion conductive material can be determined by measuring the ion conductivity σ at five temperatures (25°C, 40°C, 60°C, 80°C, and 100°C) within a temperature range of 25°C to 100°C, and performing curve fitting based on the following calculation formula. Formula: σT=Aexp(-E a / k b T) where σ is ionic conductivity (S / cm), T is absolute temperature (K), A is frequency factor, E a is the activation energy, k b represents the Boltzmann constant. It is also possible to create a graph (Arrhenius plot) with σ on the vertical axis and 1000 / T (T is absolute temperature) on the horizontal axis.

[0026] The method for producing the ion-conductive material of the present embodiment is not particularly limited, but may be, for example, a production method including a step of subjecting a raw material to ball milling.

[0027] The raw materials are not particularly limited. For example, the alkali metal source may be an alkali metal halide or an oxide of an alkali metal. The metal element M source may be a halide of the metal element M. The metal element M2 source may be a halide of the metal element M2. The dopant element X source may be XO. 4 It may be a compound such as a salt of an ion and an alkali metal. The raw materials are preferably mixed before being ball-milled, and more preferably mixed in an inert atmosphere (for example, an Ar atmosphere).

[0028] The conditions for the ball mill are not particularly limited, but may be a rotation speed of 200 to 700 rpm for 10 to 100 hours. The grinding time may be 1 to 72 hours, 12 to 60 hours, or 20 to 60 hours. The balls used in the ball mill are not particularly limited, but zirconia balls can be used. The size of the balls used is not particularly limited, but balls of 2 mm to 10 mm can be used. By performing the ball milling for the above-mentioned time, the raw materials are thoroughly mixed and the mechanochemical reaction is promoted, thereby making it possible to improve the ionic conductivity of the resulting compound.

[0029] It is preferable not to anneal the product (ion-conductive material) obtained by ball milling. If annealing is performed, the crystallites may grow and become coarse, and the above-mentioned effect may not be obtained. Annealing may be performed, for example, by heating the product after ball milling at 100°C or higher, 150°C or higher, or 200°C or higher.

[0030] The ion conductive material of the present embodiment can be used as a material for electrochemical devices such as capacitors and batteries. Examples of such materials include electrolyte (solid electrolyte) materials. Examples of batteries include batteries that perform charging and discharging by the movement of alkali metal ions between the positive and negative electrodes, such as lithium ion batteries and sodium ion batteries. The ion conductive material of the present embodiment may be contained in the positive or negative electrode of a battery.

[0031] The battery of this embodiment will be described below by taking a lithium ion battery as an example. The lithium ion battery includes a positive electrode, a negative electrode, and an electrolyte (solid electrolyte) disposed between the positive electrode and the negative electrode. The ion conductive material of this embodiment (alkali metal-containing halide (lithium-containing halide in this case)) may be included in the electrolyte of the lithium ion battery. The positive electrode of the lithium ion battery is not particularly limited, and may contain a positive electrode active material and, as necessary, a conductive agent, a binder, and the like. The positive electrode may be a layer containing these materials formed on a current collector. Examples of the positive electrode active material include lithium-containing composite metal oxides containing lithium (Li) and at least one transition metal selected from the group consisting of V, Cr, Mn, Fe, Co, Ni, and Cu. Examples of such lithium composite metal oxides include LiCoO 2 , LiNiO 2 , LiMn 2 O 4 , Li 2 MnO 3 , LiNi x Mn y Co 1-x-y O 2 [0 <x+y<1])、LiNi x Co y Al 1-x-y O 2 [0 <x+y<1])、LiCr 0.5 Mn 0.5 O 2 , LiFePO 4 , Li 2 FeP 2 O 7 , LiMnPO 4 , LiFeBO 3 , Li 3 V 2 (PO 4 ) 3 , Li 2 CuO 2 , Li 2 FeSiO 4 , Li 2 MnSiO 4 etc.

[0032] The negative electrode of the lithium ion battery is not particularly limited, and may contain a negative electrode active material and, if necessary, a conductive assistant, a binder, etc. Examples of the negative electrode include simple elements such as Li, Si, P, Sn, Si-Mn, Si-Co, Si-Ni, In, and Au, alloys or composites containing these elements, carbon materials such as graphite, and materials in which lithium ions are inserted between layers of the carbon materials.

[0033] The material of the current collector is not particularly limited, and may be a simple metal or an alloy of metals such as Cu, Mg, Ti, Fe, Co, Ni, Zn, Al, Ge, In, Au, Pt, Ag, and Pd.

[0034] The solid electrolyte layer may have a plurality of layers. For example, a configuration may be provided that has a sulfide solid electrolyte layer in addition to the solid electrolyte layer containing the ion conductive material of the present embodiment. A configuration may be provided that has a sulfide solid electrolyte layer between the solid electrolyte containing the ion conductive material of the present embodiment and the negative electrode. The sulfide solid electrolyte is not particularly limited, but may be, for example, Li 6 P.S. 5 Cl, Li 2 S-PS 5 , Li 10 GeP 2 S 12 , Li 9.6 P 3 S 12 , Li 9.54 S 1.74 P 1.44 S 11.7 Cl 0.3 , Li 3 P.S. 4 etc. EXAMPLES

[0035] Example 1 Ball mill In an argon atmosphere with a dew point of -70°C or less (hereinafter referred to as a dry argon atmosphere), Li 2 0.1334g of O, ZrCl 4 1.0407g, Li 3 P.O. 4 The raw material was prepared by weighing out 0.0259 g of the above. The above raw material was placed in a 50 ml zirconia pot for a planetary ball mill, and 65 g of zirconia balls with a diameter of 4 mm were added. The mixture was treated for 24 hours at 300 rpm so as to cause a mechanochemical reaction, thereby obtaining the ion-conductive material of Example 1. The ball mill was rotated for 10 minutes, and the interval was 1 minute. The rotation direction was alternately switched between clockwise and counterclockwise. The composition of the ion-conductive material (lithium-containing chloride) was Li 2。15 ZrCl 4 O(P 4 ) 0.05 It is. Planetary ball mill equipment: Verder Scientific PM 400

[0036] Example 2 An ion-conductive material was produced in the same manner as in Example 1, except that the ball milling was carried out for 48 hours.

[0037] Example 3 An ion-conductive material was produced in the same manner as in Example 1, except that the compounding ratio of the raw materials was changed so as to obtain the charged composition shown in Table 2.

[0038] Example 4 Li 3 PO 4 Li instead of 2 SO 4 An ion-conductive material was produced in the same manner as in Example 1, except that the blending ratio of the raw materials was changed so as to obtain the charged composition shown in Table 2.

[0039] Example 5 As a raw material, Li 2 O, ZrCl 4 , HfCl 4 , and Li 3 P.O. 4 An ion-conductive material was produced in the same manner as in Example 1, except that the blending ratio of the raw materials was changed so as to obtain the charged composition shown in Table 2.

[0040] Example 6 As a raw material, Li 2 O, ZrCl 4 , MgCl 2 , and Li 3 P.O. 4An ion-conductive material was produced in the same manner as in Example 1, except that the blending ratio of the raw materials was changed so as to obtain the charged composition shown in Table 2.

[0041] Example 7 As a raw material, Li 2 O, ZrCl 4 , MgCl 2 , and Li 3 P.O. 4 An ion-conductive material was produced in the same manner as in Example 1, except that the blending ratio of the raw materials was changed so as to obtain the charged composition shown in Table 2.

[0042] Comparative Example 1 The raw materials are LiCl and ZrCl 4 An ion-conductive material was produced in the same manner as in Example 1, except that the blending ratio of the raw materials was changed so as to obtain the charged composition shown in Table 2.

[0043] Comparative Example 2 As raw materials, LiCl, Li 2 O and ZrCl 4 An ion-conductive material was produced in the same manner as in Example 1, except that the blending ratio of the raw materials was changed so as to obtain the charged composition shown in Table 2.

[0044] Comparative Example 3 As a raw material, Li 2 O and ZrCl 4 An ion-conductive material was produced in the same manner as in Example 1, except that the raw materials were ball milled using the above-mentioned mixture ratio adjusted to obtain the composition shown in Table 2, and the product obtained was annealed at 200°C for 5 hours.

[0045] Comparative Example 4 Li 3 PO 4 Li instead of 2 SO 4 An ion-conductive material was produced in the same manner as in Example 1, except that the blending ratio of the raw materials was changed so as to obtain the charged composition shown in Table 2.

[0046] <Powder X-ray diffraction> The obtained ion-conductive material was subjected to powder X-ray diffraction measurement at 25° C. to evaluate the diffraction peaks observed within the 2θ range of 10 to 20°. The results are shown in Table 2. The powder X-ray diffraction measurement was performed under the following conditions. Measurement equipment: Ultima IV (Rigaku Corporation) X-ray generator: CuKα source, voltage 40kV, current 40mA X-ray detector: scintillation counter or semiconductor detector Measurement range: Diffraction angle 2θ=5°~80° Scan speed: 4° / min FIG. 1 shows X-ray diffraction charts obtained for the ion-conductive materials of Examples 1 to 6 and Comparative Examples 1 to 3. The half-width of the peak was determined by subtracting the background signal and performing fitting.

[0047] <Evaluation of ionic conductivity> A pressure molding die including a frame, a lower punch, and an upper punch was prepared. The frame was made of insulating polycarbonate. The upper punch and the lower punch were both made of electronically conductive stainless steel and were electrically connected to the terminals of an impedance analyzer (S11260 manufactured by Solatron Analytical).

[0048] Using the above pressure molding die, the ion conductivity of the ion conductive material was measured by the following method. First, in a dry argon atmosphere, the powder of the ion conductive material was filled on the lower part of the punch inserted vertically from below into the hollow part of the frame mold. Then, the upper part of the punch was pressed into the hollow part of the frame mold from above, so that a pressure of 370 MPa was applied to the powder of the ion conductive material inside the pressure molding die. After the pressure was applied, the punch was clamped from above and below with a jig to fix it, and while a constant pressure was maintained, the impedance of the ion conductive material was measured by the electrochemical impedance measurement method using the impedance analyzer.

[0049] A Cole-Cole diagram was created from the impedance measurement results. In the Cole-Cole diagram, the real value of the impedance at the measurement point where the absolute value of the phase of the complex impedance was the smallest was regarded as the resistance value to the ionic conduction of the ion-conductive material. Using this resistance value, the ionic conductivity was calculated based on the following formula (III). The results are shown in Table 2. σ = (R SE ×S / t) -1 (III) Where: σ is the ionic conductivity, S is the contact area of ​​the ion-conductive material with the upper part of the punch (equal to the cross-sectional area of ​​the hollow part of the mold), R SE is the resistance value of the solid electrolyte material in the impedance measurement, t is the thickness of the ionically conductive material when pressure is applied.

[0050] The ionic conductivity was measured at 25°C. In addition, the ionic conductivity was measured at five temperatures (25°C, 40°C, 60°C, 80°C, and 100°C) within the temperature range of 25°C to 100°C. The results are shown in Table 2. The ionic conductivity at each of the five temperature points is expressed as σ T (T=25° C., 40° C., 60° C., 80° C., or 100° C.). Fig. 2 is a graph showing the Arrhenius plots obtained for the ion-conductive materials of Examples 3, 5, and 6, and Comparative Examples 1 to 3. In Fig. 2, the two points with the smallest 1000 / T values ​​in Example 6 and the two points with the smallest 1000 / T values ​​in Example 3 almost overlapped with each other.

[0051] <Observation of microstructure using a transmission electron microscope> Equipment: Analytical electron microscope ARM200F manufactured by JEOL Ltd. Measurement conditions: Acceleration voltage 200kV Sample preparation: Focused ion beam (FIB) processing in an inert atmosphere while cooling with a cryostat FIG. 3 shows a TEM image of the ion-conductive material of Example 3. As shown in FIG. 3, it was found that a sea-island structure was formed in which the island structure was the crystalline phase and the sea structure of the amorphous phase was formed so as to surround it. Here, in the electron diffraction pattern obtained by transmission electron microscope observation, by imaging the crystals in which the diffraction spots exist within the aperture of the selected field of view, the crystals corresponding to the specific diffraction spots can be imaged brighter in real space than the surrounding amorphous phase. This allows the distribution of the crystalline phase in real space to be understood. In FIG. 3, the part surrounded by a white circle is the crystalline phase. In Figure 3, the image was colored to clearly show brightly focused areas, and each crystal phase was numbered. In this way, the spatial distribution of the crystal phases was investigated. In addition, an analysis of the crystalline phase was performed on a total of 51 crystal grains in the field of view in the figure, and the average equivalent circle diameter of the crystalline phase was found to be 4.5 nm.

[0052] <Preparation of a cell for cyclic voltammetry> A cell for cyclic voltammetry was prepared as described below. The preparation of the cell for cyclic voltammetry was carried out in a glove box purged with an inert gas. First, the ion-conductive material of Example 1 was placed in an insulating cylinder having an inner diameter of 10 mm. A pressure of 370 MPa was applied to the ion-conductive material to form a solid electrolyte layer (a layer of the ion-conductive material). Next, 60 mg of In foil was placed in contact with and covering the solid electrolyte layer, and 2 mg of Li foil was placed in contact with and covering the In foil to obtain a laminate. A pressure of 370 MPa was applied to the laminate, and a reference electrode made of a Li-In alloy was formed on the solid electrolyte layer. A stainless steel disk having a diameter of 10 mm and a thickness of 0.1 mm was then placed in contact with and covering the first solid electrolyte layer to obtain a laminate. A pressure of 370 MPa was applied to the resulting laminate to form a working electrode made of stainless steel on the solid electrolyte layer. A current collector made of stainless steel was attached to the reference electrode and the working electrode, and then a lead wire was attached to the current collector. All the components were placed in a desiccator sealed in a glove box. In this way, a cell for cyclic voltammetry was obtained.

[0053] <Cyclic voltammetry test> For the above cyclic voltammetry cell, the reference electrode and working electrode were electrically connected to an impedance analyzer S11260 and a potentiostat S11287A, and a cyclic voltammetry test was carried out under the following conditions. In the cyclic voltammetry test, the sweep rate was 1 mV / s and the reference electrode (Li + The current flowing when the potential of the working electrode was changed relative to the potential of the electrode (Li-In) was measured. First, the potential of the working electrode relative to the reference electrode was increased from the open circuit voltage to 5.5 V, and then turned back and decreased to 0 V. The cyclic voltammetry test was carried out at room temperature (25°C). The potential at which a reduction current of 0.5 μA or more was observed was measured and used as an index of electrochemical stability. The results are shown in Table 2. 4 is a graph showing the results of cyclic voltammetry for Examples 1 to 5 and Comparative Example 1. Compared with Comparative Example 1, the ion conductive materials of Examples 1 and 2 have an expanded potential window toward the low potential side, which indicates improved stability.

[0054] In a dry argon atmosphere, the ion-conductive material of Example 6 and LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O 2 29 parts by mass, 67 parts by mass, and 4 parts by mass of acetylene black were weighed out and mixed in a mortar to obtain a mixture. In an insulating cylinder having an inner diameter of 10 mm, 100 mg of the ion-conductive material of Example 1 and 15 mg of the above mixture were laminated in this order to obtain a laminate. A pressure of 370 MPa was applied to the laminate to form a first electrode (a layer of the above mixture) and a first solid electrolyte layer (a layer of the above ion-conductive material). Next, the first solid electrolyte layer is made of a sulfide solid electrolyte Li 6 P.S. 5 60 mg of Cl was added so as to contact the first electrode and the second electrode to obtain a laminate. A pressure of 370 MPa was applied to the laminate to form a second solid electrolyte layer. The first solid electrolyte layer was sandwiched between the first electrode and the second solid electrolyte layer. Next, 60 mg of In foil was placed in contact with the second solid electrolyte layer, and 2 mg of Li foil was placed in contact with the In foil to obtain a laminate. A pressure of 370 MPa was applied to the laminate to form a second electrode. A current collector made of stainless steel was attached to the first electrode and the second electrode, and then a lead wire was attached to the current collector. All the members were placed in a desiccator and sealed, and thus the secondary battery of Example 1 was obtained.

[0055] <Charge / discharge test> The charge / discharge test was carried out using the following product. Charge / discharge tester: Toyo Systems Co., Ltd. TOSCAT-3100 Charge / discharge tests were carried out at 25°C at three C rates: 0.1C, 1C, and 3C. The discharge capacity at each C rate is as shown in Table 1. The batteries were charged to 3.7 V using a constant current, constant voltage (CCCV) charging method at a current density corresponding to each C rate. The current densities corresponding to each C rate are shown in Table 1. Discharge was performed down to 1.9 V at a current density corresponding to each C rate. FIG. 5 shows the results of the charge / discharge test of Example 1, and Table 1 shows the discharge capacity of Example 1 at each C rate. In Example 1, a high discharge capacity was obtained at any C rate.

[0056]

Table 1

[0057]

Table 2

Claims

1. containing an alkali metal element, a tetravalent metal element M, a halogen element, a dopant element X, and an oxygen element, the content of the dopant element X being 50 mol % or less relative to the content of the metal element M; The alkali metal element includes Li, The tetravalent metal element M includes at least one of Zr and Hf, The halogen element includes Cl, the dopant element X comprises at least one of S and P; An ion-conductive substance having a diffraction peak with a half-width of 2.0 to 10° in a 2θ angle range of 10 to 20° in an X-ray diffraction chart obtained by measurement using CuKα radiation at 25°C.

2. An ion-conductive material comprising an amorphous phase and crystallites dispersed in the amorphous phase, the material comprising an alkali metal element, a tetravalent metal element M, a halogen element, a dopant element X, and an oxygen element, The alkali metal element includes Li, The tetravalent metal element M includes at least one of Zr and Hf, The halogen element includes Cl, the dopant element X comprises at least one of S and P; With respect to the total amount of atoms contained in the ion-conductive material The content of an alkali metal element is 20 to 30 mol %, The content of element M is 5 to 20 mol %, The content of halogen elements is 40 to 60 mol %, The content of the dopant element X is 0.05 to 5 mol %, The average equivalent circular diameter of the crystallites is 20 nm or less.

3. The ionically conductive material according to claim 1 or 2, wherein the dopant element is at least one of P and S.

4. With respect to the total amount of atoms contained in the ion-conductive material The content of an alkali metal element is 20 to 30 mol %, The content of element M is 5 to 20 mol %, The content of halogen elements is 40 to 60 mol %, 2. The ion-conducting material according to claim 1, wherein the content of the dopant element X is 0.05 to 5 mol %.

5. An electrolyte comprising the ion-conductive material according to claim 1 or 2.

6. A battery comprising the electrolyte of claim 5.

Citation Information

Patent Citations

  • NEGATIVE ELECTRODE ACTIVE MATERIAL FOR SECONDARY BATTERY, METHOD FOR PRODUCING THE SAME, NEGATIVE ELECTRODE FOR SECONDARY BATTERY, SECONDARY BATTERY, AND Si-OXIDE SOLID ELECTROLYTE COMPLEX

    JP2014022319A

  • Battery and battery manufacturing method

    JP6947321B1

  • Battery

    WO2021002064A1

  • Solid electrolyte, solid electrolyte layer, and solid electrolyte cell

    WO2021024785A1

  • Solid electrolyte material and battery using same

    WO2021220577A1