Method for diagnosing and predicting the lifespan of lead-acid batteries, particularly lead-acid batteries intended for storing standby power

A method for diagnosing lead-acid batteries using overcharge current and DC resistance measurements provides accurate, in-situ prediction of battery life, addressing the limitations of existing methods by enabling timely replacements and reducing maintenance costs.

JP7595633B2Active Publication Date: 2024-12-06COMMISSARIAT A LENERGIE ATOMIQUE ET AUX ENERGIES ALTERNATIVES
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022198584
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-12-14
Filing Date
2022-12-13
Publication Date
2024-12-06
Estimated Expiration
2042-12-13

AI Technical Summary

Technical Problem

Current methods for diagnosing lead-acid batteries, particularly in standby power applications, are unable to accurately predict their remaining life and require extensive laboratory conditions, making them impractical for real-world implementation.

Method used

A method involving continuous monitoring of overcharge current and internal resistance under DC current, normalized against calibration data from laboratory tests, to diagnose and predict the lifespan of lead-acid batteries by comparing deviations from predetermined thresholds.

Benefits of technology

Enables reliable, in-situ prediction of battery life without moving the cells from their commercial location, allowing for timely replacement of batteries and reducing maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595633000006
    Figure 0007595633000006
  • Figure 0007595633000007
    Figure 0007595633000007
  • Figure 0007595633000008
    Figure 0007595633000008
Patent Text Reader

Abstract

To provide a method for diagnosing a lead-acid battery that employs a liquid electrolyte for a standby energy storage application with the goal of predicting the lifetime.SOLUTION: There is provided a method for diagnosing and predicting the life of a lead-based battery, especially a lead-based battery intended to store standby power. The present invention is essentially a new method for diagnosing the lead-based battery and advantageously estimating the remaining life of the lead-acid battery, which is more specifically intended for a standby storage application. This method is based on a combination of a continuous monitoring measurement that integrates the overcharge current (calculation of the overcharge Ah applied to the battery from the time of installation) and a periodic measurement under the DC current of the battery's internal resistance using short-term discharges at constant current or constant power.SELECTED DRAWING: Figure 12
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of energy storage, and more particularly to the field of lead-acid batteries.

[0002] More specifically, it relates to a method for diagnosing such batteries and advantageously predicting their life.

[0003] Although described with reference to lead-acid batteries, the invention is generally applicable to electrochemical batteries which employ aqueous electrolytes, i.e. "aqueous batteries."

[0004] Although described with reference to a preferred standby storage application, the invention is applicable to any stationary application. [Background technology]

[0005] So-called "stationary" batteries are batteries that remain where they are located, as opposed to traction and starting batteries, which are subject to movement, vibration, etc. Stationary applications are broadly divided into two categories: standby power and solar power.

[0006] In many applications where interruptions to the main power supply, i.e. the power grid, can lead to different kinds of serious consequences (risk to human health, damage to equipment, financial losses, etc.), the systems are backed up by standby power supplies. Here we can mention power grids of telecommunications companies, hospitals, power plants, and large data centers (financial centers, centers controlling air and rail traffic, etc.).

[0007] The function of a standby power supply is to provide the power it is designed to provide in the event of a failure of the main power grid. When a standby power supply replaces the power grid and must provide an AC voltage with the same RMS value, it is commonly referred to by the acronym "UPS" for Uninterruptible Power Supply.

[0008] Standby power sources are designed with a capacity to compensate for disruptions to the power grid they are backing up to. These disruptions can be of various natures, such as blackouts, rolling blackouts and voltage dips, micro-outages, overvoltages, etc. Thus, standby power sources can be required to provide power for periods ranging from tens of milliseconds to several minutes.

[0009] A rechargeable battery is used as a standby power source.

[0010] Lead-acid batteries are the preferred technology in many standby power applications due to their low cost and technological maturity. The low cost requirement is related to the fact that the batteries are rarely used (i.e. discharged) and therefore in standby mode for more than 99% of their life. Such applications require a highly predictable energy storage system that will not suddenly fail during operation, so the technological maturity of lead-acid batteries is another important advantage.

[0011] A lead-acid battery is a set of lead-acid-sulfuric acid accumulators connected in series to obtain the desired voltage and immersed in an electrolyte consisting of demineralized water and sulfuric acid, the accumulators and electrolyte being housed in the same casing.

[0012] To intervene immediately in the event of a grid failure, standby batteries must be kept in a permanent state of charge. The conventional method of maintaining a state of charge is called "float charging", in which the self-discharge effect is compensated for by applying a voltage to the battery higher than its open circuit voltage (around 100 to 150 mV per element).

[0013] This voltage generates the float charge current, or in other words the charge maintenance current, which is permanent and for example for a battery with a capacity of 100 Ah, at 20° C. the amplitude of the float charge current may stabilize at a value of about 30 mA.

[0014] More precisely, float charging is a voltage-controlled overcharge applied continuously to compensate for the process of self-discharge, which can be expressed as follows: At the negative electrode: Pb+H2SO4 → PbSO4+H2↑ (1) At the positive electrode: PbO2+H2SO4→PbSO4+H2O+1 / 2O2↑ (2)

[0015] The excess charge remaining after compensating for the self-discharge process promotes parasitic electrochemical reactions, namely the release of oxygen and corrosion of the current collector at the positive electrode, and the recombination release of hydrogen and oxygen (in the case of primary batteries) at the negative electrode. These parasitic reactions can be expressed as follows: Electrolysis of water: H2O → 2H2↑ + O2↑ (3) Hydrogen release from negative electrode: 4H + +4e - →2H2↑ (4a) Release of oxygen at the positive electrode: 2H2O → O2↑ + 4H + +4e - (4b) Corrosion of electrode grid (positive electrode current collector): Pb+2H2O→PbO2+2H2↑ (5) Recombination of oxygen at the negative electrode: O2 + 4H + +4e - →2H2O (6)

[0016] Reactions (4b) and (6), in combination, form what is called the oxygen cycle, allowing lead-acid batteries designated valve-regulated lead-acid (VRLA) batteries to operate without maintenance. This type of battery is equipped with a valve-based safety vent system designed to relieve excessive internal pressure while maintaining sufficient pressure to allow oxygen and hydrogen to recombine to form water.

[0017] In contrast, reactions (4a) and (5) can be considered irreversible processes that cause the gradual degradation of lead-acid batteries.

[0018] Degradation occurs via two parallel processes. - On the one hand, these reactions consume water and completely dry out the electrolyte. - On the other hand, the metal current collector is converted to highly resistive and brittle PbO2, i.e. the positive electrode loses capacity due to the loss of structural integrity caused by the corrosion process.

[0019] The progression of these two processes leads to an increase in the battery's resistance and ultimately to a loss of energy storage capacity.

[0020] In standby energy storage applications, two types of diagnostic parameters must be known for the batteries used in the standby power system: the actual capacity of each battery, i.e., the battery state of health (SOH), and the remaining battery life, to ensure preventive maintenance of the system.

[0021] Currently, quantitative estimation of standby battery degradation can be performed using two main methods.

[0022] The first main method, which is the most accurate, is to fully discharge the battery at a constant current or power. By convention, the battery is considered to be fully charged before this discharge test for standby energy storage system specifications. The results of this discharge test can be directly presented in terms of "State of Health" by normalizing the discharge capacity (Cd) with a reference capacity value (Cref). The State of Health (SOH) is thus expressed by the following relationship: SOH = 100 × Cd / Cref (7)

[0023] Although accurate, this method can only provide information about the actual state of the battery, i.e. it cannot predict the remaining life of the battery, and the long measurement and charging times make its implementation outside laboratories equipped for this purpose problematic.

[0024] The other main method is to estimate the battery's internal resistance, or its reciprocal when taken into account, either through impedance measurements or through application of a DC discharge pulse and correlation with the battery's capacity or SOH estimated via the full discharge method described above. This approach is widely used in the battery industry and in particular by Midtronics Inc., one of the leading manufacturers of rapid battery testing devices. See also publication [1], which describes this method in detail. As with the full discharge method, this method of estimating the internal resistance does not allow the remaining life of the battery to be predicted. [Prior art documents] [Non-patent literature]

[0025] [Non-Patent Document 1] DOFeder, MJHvalac and SJMcShane, “Updated status of conductance / capacity correlation studies to determine state-of-health of automotive and stand-by lead / acid batteries”, J Power Sources 48 (1994) 135. [Non-Patent Document 2] Webinar presentation on March 11, 2021 by Avicenne Energy “Durable Batteries: a new regulatory framework and market perspectives” organized by EUROBAT, Association of European Automotive and Industrial Battery Manufacturershttps: / / www.eurobat.org / events / event / 48-eurobat-webiinar-sustainable-batteries-a-new-regulatory-framework-and-market-outlook Summary of the Invention [Problem to be solved by the invention]

[0026] Thus, there is a need for improved methods for diagnosing lead-acid batteries employing liquid electrolytes, advantageously with a view to predicting their lifespan, particularly for standby energy storage applications.

[0027] The aim of the present invention is to at least partially meet this requirement. [Means for solving the problem]

[0028] Thus, according to one aspect thereof, the present invention relates to a method for diagnosing an accumulator or battery employing an aqueous electrolyte, and in particular a lead-acid battery, comprising the following steps: a / Overcharge current applied to the battery (I ovch ) continuously measuring b / The internal resistance of the battery under DC current (R 120s ) periodically measuring c) normalizing a parameter derived from the overcharge current measured in step a) and the internal resistance measured in step b); d / estimating the deviation of the logarithmic value of the internal resistance normalized in step c / , taken into account for the parameters derived from the overcharge current normalized in step c / , with respect to a calibration line, obtained from a linear regression of the calibration measurements of the internal resistance and the overcharge current of the reference battery; e) comparing the estimated deviation (Δ) with a predetermined threshold value depending on the type of battery, If the deviation is positive and higher than this threshold, the battery needs replacing due to premature aging; If the deviation is negative and below this threshold, then there is no need to replace the battery.

[0029] According to one advantageous variant, the parameter derived from the measured overcharge current is the integral of the float overcharge current (Q ovch ).

[0030] According to another advantageous variant, the normalization of the internal resistance in step c / is carried out by the measured internal resistance (R 120s ) by the internal resistance of a new battery or a new reference battery of the same type measured under an AC current of 1 kHz.

[0031] According to another advantageous variant, the normalization of the overcharge current in step c / is performed by the integral of the measured overcharge current (Q ovch ) by the nominal capacity of the battery (Cn) to obtain the overcharge index (N ovch )

[0032] According to an advantageous embodiment, the method further comprises the following steps: f / Overcharge limit (N max ) and overcharge index (N ovch ) between (N max / N ovch ) g / step f / estimated ratio (N max / N ovch ) to 1, - Estimated ratio (N max / N ovch ) is less than 1, the battery needs to be replaced since normal aging of the battery has been exceeded.

[0033] According to another advantageous embodiment, the method further comprises the following steps: Ratios compared in steps g / s (N max / N ovch ) is higher than 1, and If the absolute value of the deviation (Δ) estimated at step d / is lower than a predefined threshold, h / expression

[0034]

number

[0035] determining the battery remaining life (RBLT) using the Here, BOT specifies the actual time the battery has been in operation.

[0036] Preferably, the internal resistance (R 120s Periodic measurements of ) are performed by applying a charging or discharging current for a fixed time interval.

[0037] Also preferably, the fixed time interval is between 60 seconds and 180 seconds for a discharge current corresponding to a nominal capacity (Cn).

[0038] Another subject of the invention is a system for controlling a battery employing an aqueous electrolyte (BMS), for implementing the aforementioned method, comprising a measurement sensor and a processor configured to deliver, based on the measurements made by the sensor, a message informing the user either of a failure of the battery or of its correct operation, and preferably indicating the remaining life (RBLT) of the battery.

[0039] Another subject of the invention is the use of the diagnostic method or system just described in applications in which the battery serves as a standby store of power, such as in telecommunications base stations, data centers, nuclear power plants, or serves as base and backup for low-voltage networks in electric vehicles.

[0040] The present invention is therefore essentially a new method for diagnosing and advantageously estimating the remaining life of a lead-acid battery, the battery being more specifically intended for standby storage applications.

[0041] The method is based on a combination of a continuous monitoring measurement integrating the overcharge current (calculating the overcharge Ah applied to the battery from the time of installation) and a periodic measurement under DC current of the battery's internal resistance using a short discharge at constant current or power. This can be a matter of current or nominal power for 1 hour, e.g. 1 A / Ah or 1 W / Wh.

[0042] These measurements are compared to a set of calibration data obtained after linear regression of laboratory tests of selected types of lead-acid-based batteries.

[0043] This comparison triggers a diagnostic indication of whether the monitored battery is aging normally or prematurely (and therefore should be replaced).

[0044] Based on these comparisons, it is also possible to predict remaining life in days, months, or years of operation.

[0045] Compared with the methods of the prior art, the method for diagnosing an accumulator or battery according to the invention has many advantages, among which may be mentioned the following: - a reliable method based on laboratory-tested reference cells used to establish calibration data, which can be reproduced as desired in situ, i.e. without removing the cells from the commercial use site, based on any type of battery technology employing aqueous electrolytes; - Methods for predicting remaining life.

[0046] The diagnostic method according to the invention is applicable to standby energy storage applications implementing batteries employing aqueous electrolytes. These applications include telecommunication base stations, data centers, and nuclear power plants. Such applications require low cost and high predictability, without extensive charge-discharge cycling. These specifications are successfully met by several different lead-acid-based battery technologies, and several recent market studies indicate that this situation will remain largely unchanged, at least in the medium term. For example, a publication [2] gives a forecast for 2030:

[0047] Another sector of the energy storage market, where the diagnostic method according to the invention could be advantageously applied, is the electric vehicle market. Most electric vehicles use 12V lead-acid batteries as base and backup for the vehicle's low-voltage network (i.e. this is a typical case of standby energy storage). According to publication [2], lead-acid batteries will remain the preferred choice in this sector, at least in the medium term until 2030.

[0048] Other advantages and characteristics of the invention will emerge more clearly on reading the detailed description of an implementation of the invention, which description is non-limiting and is given by way of example with reference to the following figures: [Brief description of the drawings]

[0049] [Figure 1A] FIG. 1 shows curves illustrating the change in capacity and high frequency impedance as a function of time for a first group of cells during their aging while applying a float charge of 2.27 V per cell at 60° C., as per the prior art. [Figure 1B] FIG. 1 shows curves illustrating the change in capacity and high frequency impedance as a function of time for a first group of cells during their aging while applying a float charge of 2.27 V per cell at 60° C., as per the prior art. [Figure 2A]FIG. 13 shows curves illustrating the change in capacity and high frequency impedance as a function of time for a second group of cells during their aging while applying a float charge of 2.27 V per cell at 60° C., similar to the prior art. [Figure 2B] FIG. 13 shows curves illustrating the change in capacity and high frequency impedance as a function of time for a second group of cells during their aging while applying a float charge of 2.27 V per cell at 60° C., similar to the prior art. [Figure 3A] FIG. 1 shows curves illustrating the change in capacity and high frequency impedance of a battery as a function of time upon aging while applying a float charge of 2.27 V per battery at 50° C., as in the prior art. [Figure 3B] FIG. 1 shows curves illustrating the change in capacity and high frequency impedance of a battery as a function of time upon aging while applying a float charge of 2.27 V per battery at 50° C., as in the prior art. [Figure 4A] 1 is a curve illustrating the change in test discharge voltage of a battery as a function of time during aging at 60° C. [Figure 4B] 4B is a curve illustrating the change as a function of time in the test discharge voltage of a battery during aging at 60° C., the time-scaled expansion of FIG. 4A. FIG. [Figure 4C] 1 is a curve illustrating the change in test discharge voltage of a battery as a function of time during aging at 60° C. [Figure 4D] 4C is an hourly expanded view of FIG. 4C; FIG. 4D is a curve illustrating the change as a function of time in the test discharge voltage of a battery during aging at 60° C.; FIG. [Figure 5A] FIG. 2 shows a curve illustrating the change as a function of time in the internal resistance (R120s) under DC current of a battery during its aging according to the invention. [Figure 5B] FIG. 2 shows a curve illustrating the change as a function of time in the internal resistance (R120s) under DC current of a battery during its aging according to the invention. [Figure 6A] FIG. 1 shows curves illustrating the change as a function of time in overcharge current of several batteries during accelerated aging thereof while applying a float charge of 2.27 V per battery at 60° C., in accordance with the present invention. [Figure 6B] FIG. 1 shows curves illustrating the change as a function of time in overcharge current of several batteries during accelerated aging thereof while applying a float charge of 2.27 V per battery at 60° C., in accordance with the present invention. [Figure 7A] FIG. 1 shows curves illustrating the change as a function of time in the cumulative overcharge of a battery during accelerated aging thereof while applying a float charge of 2.27 V per battery at 60° C. and 50° C., in accordance with the present invention. [Figure 7B] FIG. 1 shows curves illustrating the change as a function of time in the cumulative overcharge of a battery during accelerated aging thereof while applying a float charge of 2.27 V per battery at 60° C. and 50° C., in accordance with the present invention. [Figure 8A] FIG. 7B is a diagram showing curves illustrating the correlation between overcharge (Qovch) under DC current and internal resistance (R120s) of a battery at 60° C. and 50° C. based on measurements from FIGS. 5A to 7B. [Figure 8B] FIG. 7B is a diagram showing curves illustrating the correlation between overcharge (Qovch) under DC current and internal resistance (R120s) of a battery at 60° C. and 50° C. based on measurements from FIGS. 5A to 7B. [Figure 8C] FIG. 7B is a diagram showing curves illustrating the correlation between overcharge (Qovch) under DC current and internal resistance (R120s) of a battery at 60° C. and 50° C. based on measurements from FIGS. 5A to 7B. [Figure 9] FIG. 1 shows the linear correlation between the logarithm of normalized internal resistance under DC current and normalized overcharge for cells exhibiting correct aging behavior. [Figure 10A]FIG. 10 illustrates the deviation between the logarithm of normalized internal resistance under DC current as a function of normalized overcharge for batteries not showing correct aging behavior with respect to the calibration line obtained from the linear correlation of FIG. 9 for batteries showing correct aging behavior. [Figure 10B] FIG. 10 illustrates the deviation between the logarithm of normalized internal resistance under DC current as a function of normalized overcharge for batteries not showing correct aging behavior with respect to the calibration line obtained from the linear correlation of FIG. 9 for batteries showing correct aging behavior. [Figure 11A] FIG. 1 illustrates the estimation of the remaining life of a battery in the case of correct aging and in the case of early aging, depending on the value of the logarithm of the normalized internal resistance under DC current as a function of the normalized overcharge for the battery. [Figure 11B] FIG. 1 illustrates the estimation of the remaining life of a battery in the case of correct aging and in the case of early aging, depending on the value of the logarithm of the normalized internal resistance under DC current as a function of the normalized overcharge for the battery. [Figure 12] 2 is a flow chart showing the algorithm of the method for diagnosing a battery and estimating the remaining battery life (RBLT) according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0050] Please note that in the following description, a voltage of 2.27V per cell refers to a voltage equal to 2.27V per cell in a battery consisting of three cells in the embodiment.

[0051] Battery Technology The inventors compared prior art diagnostic methods and implemented a method for diagnosing and predicting battery life using a battery model already on the market under the name "Sprinter XP6V2800" -- a battery manufactured by Exide.

[0052] This commercial battery employs valve-regulated lead-acid (VRLA) technology, in which the liquid electrolyte is absorbed and immobilized in a fiberglass mat (AGM technology, AGM stands for "Absorbed Glass Mat"), providing a voltage equal to 6V, has three accumulator cells and has a nominal capacity of 195Ah.

[0053] Typically, these batteries are installed in various data centers as standby energy storage batteries.

[0054] The cells tested herein are designated hereinafter and in the figures by the acronym "XP6Vnn," where nn is a numeric reference designating one of the cells.

[0055] Experimental protocol Three groups of four separate cells were subjected to accelerated ageing using a float charge voltage of 2.27 V per cell and temperature ramping up to two temperature levels. Thus, the group consisting of cells XP6V06, XP6V07, XP6V08, XP6V09 was subjected to a temperature of 50° C. The group consisting of cells XP6V01, XP6V03, XP6V04, XP6V05 on the one hand and cells XP6V11, XP6V12, XP6V13, XP6V14 on the other hand was tested at a temperature of 60° C.

[0056] Cyclic control tests at 25°C were performed after 4 to 5 weeks of accelerated aging at elevated temperature.

[0057] The test protocol started with the measurement of the internal impedance of the battery under an AC current at 1 kHz open circuit, followed by full discharge at a constant current equal to 195 A (current for 1 hour or C / 1h) until the battery voltage reached a value of 1.6 V per accumulator. This measurement was carried out using an instrument sold by the company HIOKI under the name HIOKI HiTESTER 3554.

[0058] After the discharge process, the cells were recharged in the constant current or constant voltage regime starting at 19.5 A with a voltage limit of 2.4 V per cell.

[0059] The float charge voltage reached 2.27 V per battery 24 hours after the start of charging, and this float charge voltage was maintained until the start of the next test procedure.

[0060] The temperature was increased from 25° C. to 50° C. or 60° C. for several days after other battery tests included in the testing procedure were performed. These other tests were non-electrical, non-invasive, and did not affect the electrochemistry of the battery. They therefore did not affect the diagnostic measurements according to the prior art and according to the present invention.

[0061] Prior Art Methods for Diagnosing Batteries Full discharge measurements and measurements of the internal impedance under AC current at a high frequency of 1 kHz were performed on the cells.

[0062] 1A, 1B, 2A, 2B, and 3A, 3B summarize the results of battery diagnostics for aging when applying a float charge of 2.27 V per battery to different groups of cells at 60° C. and 50° C., respectively.

[0063] The first group of cells tested at 60 °C shows a rapid decrease in capacity for three cells, namely XP6V01, XP6V04, and XP6V05, indicating early failure, and slower aging for one other cell, namely XP6V03 (Figure 1A). It is believed that the three poor quality cells belonged to a manufacturing batch labeled with the first manufacturing date (May 2019), whereas the correct quality cell was labeled with the second manufacturing date (November 2018).

[0064] High frequency impedance measurements (internal resistance at 1 kHz) showed a very low correlation with capacity, especially at the beginning of aging (Figure 1B). The internal resistance of the correct cell XP6V03 remained the lowest, while the differences with respect to the other cells, i.e. XP6V01, XP6V04, XP6V05, remained relatively small. These data show that the high frequency internal resistance is not a very sensitive parameter for estimating the state of health (SOH) and cannot be used for predictive purposes. In particular, it is evident from these tests that the change as a function of time in the 1 kHz impedance is similar for good and prematurely failing cells.

[0065] FIG. 2A shows the change in capacity as a function of time for batteries XP6V11, XP6V12, XP6V13, XP6V14, which is very similar to that of the correct battery XP6V03. These results are consistent with the information in the data sheets of these batteries, which show a battery life of 6 months at 60° C. and a voltage of 2.27 V per accumulator. The decrease in capacity is not linear and there is a certain scatter of the data points. FIG. 2B also shows a slow increase in the internal resistance of batteries XP6V11, XP6V12, XP6V13, XP6V14, which has a weak correlation with the change in capacity as a function of time. These results are clearly different from the data in FIG. 1A and FIG. 1B, where a significant increase in high-frequency impedance is observed in the first month of aging.

[0066] Figure 3A shows the evolution of the capacity and high frequency impedance of the batteries XP6V06, XP6V07, XP6V08 and XP6V09 with ageing at 50 °C with a float charge of 2.27 V per accumulator. It can be seen that the ageing of these batteries is significantly slower than that of the batteries mentioned above. The three batteries XP6V06, XP6V07 and XP6V09, corresponding to the production batch with the second production date on the label, lose capacity very slowly, while the battery XP6V08 taken from the production batch with the first production date on the label deteriorates rapidly. This confirms that the premature failure is related to a manufacturing quality problem. The rate of ageing of the correct batteries XP6V06, XP6V07 and XP6V09 is in accordance with the information in the data sheets of these batteries, which indicates a battery life equal to 12 months at 50 °C with a voltage of 2.27 V per accumulator. The capacity change of the correct cell at 50°C corresponds very well to the theoretical behavior of an aged standby cell, where the capacity decreases very slowly in the absence of vigorous charge-discharge cycling, up to an inflection point that corresponds to a certain critical thickness of the corrosion layer that forms on the positive current collector surface.

[0067] Beyond this thickness, the electrical resistance and mechanical integrity of the current collector begin to degrade rapidly, corresponding to a rapid loss of capacity, as shown by the inflection point in the capacity at 8 to 9 months of aging in Figure 3A.

[0068] From reading Figure 3B, it can also be seen that the change in high frequency impedance as a function of time does not correspond well to the change in capacitance as a function of time, and that a significant difference in capacitance can correspond to a very small difference in impedance at 1 kHz.

[0069] Method for diagnosing batteries via measurement of internal resistance under DC current - Patents.com The internal resistance (RDC) of a battery under current can be estimated using Ohm's law as follows: R DC =ΔU / ΔI (8) where ΔU is the change in voltage of the battery due to the application of a charge or discharge current equal to ΔI over a fixed time interval.

[0070] The duration of this time interval is related to the time constants of the various electrical and electrochemical processes occurring in the battery during the charge / discharge operation. For example, a duration in the range of 1 to 5 ms results in an R close to that measured by a Hioki instrument under AC current with a frequency of 1 kHz. DC Supply a value.

[0071] The inventors have determined that the internal resistance R DC In order to select the optimal conditions for the measurement of (more precisely ΔU), the evolution of the voltage curve of the battery as a function of time during controlled discharge with a constant current of 195 A (C / 1 h) at 25° C. was analyzed in detail.

[0072] Figures 4A to 4D show the evolution of two cells of the first group, XP6V03 and XP6V01, when subjected to aging at 60 °C. A zoom of the data for the first 6 min of discharge shows a good correlation between the cell voltage, aging and capacity change, especially in the initial period from 1 to 3 min, corresponding to 1.5 to 5% of the nominal capacity of the cell, where the voltage has a tendency to plateau (Figures 4B and 4D). The results show that the cell voltage (U 120s ) can be considered as one of the parameters that defines ΔU.

[0073] Inspection of all data measured as the tests progressed, and studies of the electrical behavior of other lead-acid-based batteries during discharge at currents approaching 1C, suggests that a base reference voltage equal to 2 V per cell, or for the present study, 6 V per cell, is a good empirical choice.

[0074] Therefore, in the proposed battery diagnosis method, the inventors measure the internal resistance under DC current (hereinafter, R 120s It was decided to adopt the index (expressed as

[0075] This internal resistance is calculated according to the following formula: R 120s =(6V-U 120s ) / 195A (9)

[0076] The internal resistance (R 120s ) as a function of time is shown in Figures 5A and 5B.

[0077] From these figures, the parameter R 120s It is clear that the use of this makes it possible to easily distinguish between correct and defective batteries, the latter of which show a very rapid increase in internal resistance.

[0078] In addition, when the temperature is lowered by 10°C (from 60°C in Figure 5B to 50°C in Figure 5A), the internal resistance R 120s It can also be seen that the change in as a function of time becomes about twice as slow, which corresponds to the Arrhenius equation.

[0079] Internal resistance R 120s A comparison of the change in R as a function of time and the change in capacity of the battery as a function of time is shown for R in the interval from 1 to 2 MΩ. 120s It is shown that the value of can ultimately be used as an indicator that the end of a battery's life is approaching.

[0080] Battery Aging Monitoring Using Integration of Overcharge Current From the data in the previous figures (FIGS. 1A through 5B), it is clear that temperature has a dramatic effect on the rate of aging of batteries, especially those intended for standby storage applications.

[0081] However, the ambient temperature within the space in which the battery is housed is rarely maintained constant.

[0082] This makes quantifying the aging of the battery and estimating remaining life difficult.

[0083] The small number of charge-discharge cycles in standby storage applications makes it possible to assume that the active materials in the two electrodes (anode, cathode) of each battery do not degrade as the battery ages.

[0084] Therefore, the reactions described with reference to equations (3) through (6) can be considered the sole cause of the loss of battery performance.

[0085] According to Faraday's law, which relates the number of species participating in an electrochemical reaction to the number of charge carriers passing through an external electric circuit, the progression of aging of a battery is proportional to the overcharging current and the electrical overcharge, i.e., the ampere-hours overcharged.

[0086] Figures 6A and 6B show the evolution of overcharge current over the course of accelerated aging when applying a float charge of 2.27V per cell at 60°C for the first group of two cells, XP6V03 and XP6V01, respectively. It should be noted that the acronym CU used in these figures stands for "check-up", i.e., periodic measurement of capacity and internal resistance. The numbers 01, 02, 03, etc. following CU for that part are the numbers of each corresponding check-up.

[0087] It can be seen that the overcharge current also increases immediately after the temperature rises, and although it is not constant, it is within a given range. For this reason, the inventors believe that in the float overcharge mode, it would be quite practical to use the integral current signal as a parameter to reveal the aging of the battery.

[0088] The integrated current corresponds to the calculation of the overcharged ampere-hours. The overcharged ampere-hours can be calculated in a number of different ways.

[0089] The most accurate approach is to subtract the ampere-hours discharged from the total charge applied to the battery.

[0090]

number

[0091] Q ovch An approximate method for calculating is to integrate the current applied in float overcharge mode while the battery voltage is maintained at 2.27V per cell.

[0092] Such an approach can be very effective when the batteries are initially recharged in the DC current / DC voltage regime at a voltage of about 2.35 to 2.40 V per cell after the end of charge.

[0093] In this constant voltage charging mode, the battery's state of charge exceeds 99% after 4 to 5 hours, but the overcharge remains negligible.

[0094] 7A and 7B show the cumulative overcharge (Q) measured during the aging progression of the three groups of cells at 60° C. and 50° C., respectively. ovch ) changes.

[0095] From these Figures 7A and 7B, it is clear that most of the cells reach the end of their life when the total amount of applied overcharge reaches 4000 Ah. This value is practically the same at both aging temperatures (50°C and 60°C). The defective cells, which undergo more rapid aging, absorb more overcharge, i.e., they are overcharged with a larger current, which is supported by Figures 6A and 6B. The cumulative overcharge (Q ovch ) as a function of time approaches a linear progression, especially in cells with normal aging behavior, i.e., in correct cells.

[0096] The results show that for standby battery applications using lead-acid electrochemistry or any other electrochemistry employing aqueous electrolytes, the cumulative overcharge (Q ovch) is a convincing indication that it is a suitable electrochemical / electrical aging indicator.

[0097] Internal resistance (R 120s ) and cumulative overcharge (Q ovch Estimating battery life using correlation between 8A, 8B, and 8C show the battery diagnostic parameters R for the aforementioned three groups of batteries at 60° C. and 50° C., respectively. 120s and Q ovch The correlation between

[0098] From Figures 8A to 8C, it is clear that the logarithm of the resistance of a normal battery increases linearly with the applied overcharge until the latter reaches a value of 3500 to 4000 Ah. 120s begins to increase rapidly above this value from 3500 to 4000 Ah, indicating that the end of the battery's life is fast approaching. The segments of these curves are similar at both aging temperatures (50°C and 60°C), which indicates that the internal resistance (R 120s ) and cumulative overcharge (Q ovch ) can be used as calibration data for battery diagnostics and lifetime prediction.

[0099] If so, the internal resistance (R 120s ) and the applied overcharge (Q ovch ) relates to the size of each battery in terms of its nominal capacity and nominal voltage, i.e., the number of accumulators connected in series.

[0100] Furthermore, a wide variety of battery models can be manufactured with identical components, differing only in their overall dimensions, i.e., the same thicknesses of electrode active material and electrode carriers and separators.

[0101] Therefore, in order to make the diagnostic method applicable to a whole series of batteries manufactured using the same type of components, i.e. components with a given chemistry (composition of the current collector carrier alloy, electrolyte, electrode active material and separator), the battery parameter R 120s and Q ovch It is necessary to normalize

[0102] The inventors believe that the most practical parameter for normalizing the applied overcharge is the nominal capacity (Cn) of the battery. The resulting parameter is given by the relationship N ovch =Q ovch / Cn (11) The "overcharge index" or N ovch It can be expressed as:

[0103] Internal resistance R 120s may, for its part, be advantageously normalized using the 1 kHz high frequency internal impedance of a new fully charged battery or using the value given in its data sheet, i.e. the value of a new reference battery of the same type.

[0104] The resulting parameter (rn) is

[0105]

number

[0106] It can be written as:

[0107] FIG. 9 shows the calibration data of the method, obtained from a correct cell using the normalized parameter rn, plotted against N in semi-logarithmic coordinate system. ovch Optionally, a calibration procedure can be performed with batteries of the same type to determine a ratio Rn-max, beyond which the battery should be replaced.

[0108] Thus, a comparison of the ratio Rn to Rn-max also optionally enables the need for battery replacement to be identified.

[0109] The result of a linear fit performed on these calibration data is the internal resistance R 120s and the applied overcharge N ovch The semi-logarithmic relationship between α and β is an empirical modeling approach applicable to battery diagnostics. This line fit is performed on a correctly aged reference cell and allows a linear calibration line to be obtained that is used in the remainder of the method.

[0110] Coefficient of determination (R 2 , i.e. the linear correlation coefficient r squared) is greater than 0.9 at the two measurement temperatures (50°C and 60°C). These coefficients R 2 are close enough to conclude that changes in temperature do not significantly affect the battery's life expectancy.

[0111] Thus, taken together, the experimental data allow two reliable criteria for predicting the end of life to be defined, namely an internal resistance threshold combined with an overcharge index threshold.

[0112] Data obtained from aged defective batteries can be used to derive criteria that allow premature aging behavior to be recognized.

[0113] This analysis of the data is presented in Figures 10A and 10B at 50°C and 60°C, respectively. It can be seen that for a given amount of overcharge, cells exhibiting early aging behavior exhibit a positive deviation Δ from the logarithm of the normalized internal resistance rn. In the first half of the cell's life, this deviation Δ varies from 0.3 to 0.4.

[0114] From these results and the scatter of data points observed in FIG. 9, a deviation Δ less than 0.2 would be considered confirmation of normal aging of the battery, while a deviation Δ greater than 0.2 would be considered indicative of premature aging.

[0115] If the deviation Δ is greater than 0.2, the remaining life of the battery may then be calculated and the user may be notified if the corresponding battery is at risk of failing soon.

[0116] The results in Figures 9, 10A and 10B indicate that subsequent repetition of the same event, i.e. deviation Δ>0.2, can be considered a reliable indicator of future battery failure and require urgent replacement of the battery.

[0117] In contrast, the presence of a battery that has already been replaced recently is indicated through a diagnostic event with a negative deviation, i.e., Δ<−0.2. In this case, the user may be notified via the message “battery replaced recently.”

[0118] The estimation of the remaining life of the battery is shown diagrammatically in Figures 11A and 11B for two different diagnostic data points, respectively. In case of normal aging of the battery, the diagnostic data points of the battery are close to the calibration line, i.e., deviation Δ<0.2.

[0119] In this case, the remaining overcharge index (N rem )teeth, N rem =N max -N ovch (13) It can be expressed as follows: Here, N max corresponds to the maximum amount of overcharge that can be tolerated by the battery before it fails, and N ovch is the overcharge applied to the batteries since the start of commissioning of the standby storage system, assuming that all batteries in the system are new. Here, N max Note that is equal to 20. This value is derived from the data shown in Figures 2A, 3A, 7A, and 7B.

[0120] Using the nominal capacity of the battery (Cn), the remaining overcharge index (N rem) is the relation Q rem =Cn*N rem (14) The remaining number of overcharge ampere hours (Q rem )

[0121] In addition, the number of overcharge ampere hours Q rem is the average overcharge current ovch > and the remaining battery life (RBLT) in hours, i.e., Q rem = ovch >*RBLT (15) is equal to.

[0122] However, the data in Figures 7A and 7B show that the parameters ovch > can be considered as a constant, which allows the applied overcharge, i.e., Q ovch or Cn*N ovch and the battery's actual operating time (BOT) in hours, i.e., ovch >=Cn*N ovch / BOT (16) It can be expressed as:

[0123] The combination of equations (13) to (16) gives the following relationship for the remaining battery life:

[0124]

number

[0125] This allows the information to be obtained.

[0126] This equation (17) is N max / N ovch Obviously, this is not applicable to newly installed batteries, since the term becomes very large. In standby storage applications, this is not an issue, since maintenance of the storage system is typically performed once a year.

[0127] ​​​​For batteries that exhibit very rapid aging, ovch >N max The RBLT indicator becomes negative when , In this case, the battery management system (BMS) of the battery may notify the user with a message indicating that the battery should be replaced urgently.

[0128] 11A and 11B also show the case of early aging of the battery, when the normalized internal resistance deviates significantly from the linear calibration line. In this case, the parameter N ovch can be corrected to accommodate the expected shorter battery life. The experimental data in Figures 10A and 10B show that two successive readings of this kind can cause the generation of a message informing the user to urgently replace the battery.

[0129] Fig. 12 shows a flow chart of the algorithm of the method according to the invention just described, which is advantageously implemented by a battery management system (BMS) of the battery of the accumulator. In Fig. 12, the data parameterizing the algorithm (BMS data) are shown in a dashed box, the measured battery parameters (monitoring parameters) are shown in a dashed box and the output data are shown in a box thereby and given a grey background. Other internal variables and procedures specific to the method according to the invention are shown in a solid box.

[0130] The invention is not limited to the examples described so far, and the features of the examples shown can be combined together, in particular within the scope of variations not illustrated.

[0131] Further modifications and improvements may be contemplated without departing from the scope of the present invention.

[0132] In the illustrated example, the results obtained with the adopted battery technology and experimental protocol are expressed as the internal resistance parameter R 120s It has been shown that R correlates with the electrical resistance of the corrosion layer formed on the positive current collector. At the beginning of the battery operation, the corrosion layer is thin, so R 120sThe values ​​of R are very low. The data in Figures 4A to 4D show that the baseline voltage of the battery can be established within an interval of 60 to 180 seconds after the start of discharge. For example, at 60 seconds (R 60s The same type of analysis was performed on the internal resistance values ​​of , and very similar plots were obtained as illustrated in Figures 8A to 8C.

[0133] If the discharge current applied to the battery is modified, the duration of the trial discharge and the selection of the battery's reference voltage must be adjusted.

[0134] The correction to the discharge time is proportional to the applied discharge current. For example, if the discharge current is equal to Cn / 0.5h (nominal discharge current of 30 min), the time range interval is twice as short, i.e. from 30 to 90 seconds (versus 60 to 180 seconds). In contrast, the application of a lower discharge current, for example Cn / 2h, corresponds to a test discharge period twice as long (from 120 to 360 seconds).

[0135] The correction of the reference voltage at various discharge currents requires the evaluation of the discharge voltage transients in order to obtain a normalized internal resistance under DC current that remains in the range of 0.01 to 0.1 MΩ, i.e. which must be at least one order of magnitude smaller than the internal impedance of the battery measured under AC current at 1 kHz with state of charge SOC=100% and state of health SOH=100%.

[0136] The battery diagnostic method just described requires the separation of the ampere-hours corresponding to the process of discharging the electricity used for the main charging reaction. In the illustrated example, due to the battery technology and experimental protocol adopted, this separation is achieved using data from the discharge experiment, i.e. the number of ampere-hours discharged is subtracted from the total charge applied. This is the most accurate approach from an electrochemical point of view. Overcharge Q ovchAn alternative strategy to estimate is to consider only the ampere-hours injected in float charging mode, i.e. when the voltage is equal to 2.27 V per accumulator, which is appropriate in this case. This approach can be very effective if the charging is performed mainly in constant current / constant voltage mode and the voltage limit is 2.35 to 2.40 V per accumulator for a relatively short time. For example, the constant voltage is applied for 10 to 15 hours. Under such conditions, the pre-discharged capacity is restored to the battery with minimal overcharge, i.e. the faradaic efficiency is between 97 and 98%. If the charging is performed using the limit voltage of 2.27 V per accumulator, a correction for overcharge can be made by omitting the ampere-hours injected into the battery during the first 24 to 48 hours in float charging mode. Such a strategy is reasonable, since the corresponding times are much shorter than the typical life of the battery specified by the manufacturer. For example, the "Sprinter XP6V2800" technology used is specified for a life of 8 years at 20 °C.

Claims

1. 1. A method for diagnosing a battery employing an aqueous electrolyte, comprising: a / the overcharge current applied to the battery (I ovch ) continuously measuring b / The internal resistance of the battery under DC current (R 120s ) periodically measuring c / normalizing the parameters derived from the overcharge current measured in step a / and normalizing the internal resistance measured in step b / ; d / estimating the deviation between the change in the logarithm of the internal resistance normalized in step c / in function of the parameter derived from the overcharge current normalized in step c / and a calibration line obtained from a linear regression of calibration measurements of the overcharge current and the internal resistance of a reference battery; e / comparing said estimated deviation (Δ) with a predetermined threshold value depending on said battery, if the deviation is positive and higher than the threshold, replacement of the battery is necessary due to premature aging; if the deviation is negative and less than the threshold, then the battery does not need to be replaced.

2. The parameter derived from the measured overcharge current is the integral of the float overcharge current (Q ovch 2. The diagnostic method according to claim 1 .

3. The normalization of the internal resistance in step c / is performed by the measured internal resistance (R 120s 2. The diagnostic method of claim 1, wherein the test is performed by dividing the internal resistance of the battery by the internal resistance of a new battery or a new reference battery of the same type measured under an AC current of 1 kHz.

4. The normalization of the overcharge current in step c / is performed by the integral (Q ovch ) by the nominal capacity (Cn) of the battery to obtain the overcharge index (N ovch The diagnostic method according to claim 2, which is carried out by defining

5. f / Overcharge limit value (N max ) and the overcharge index (N ovch ) between the ratio (N max / N ovch ) g / the ratio estimated in step f / (N max / N ovch ) to 1, The estimated ratio (N max / N ovch 5. The method of claim 4, further comprising the step of: if .gtoreq.1, then determining that normal aging of the battery has been exceeded and that the battery needs to be replaced ... needs to be exceeded.

6. Ratios compared at step g / (N max / N ovch ) is higher than 1, and If the absolute value of the deviation (Δ) estimated in step d / is lower than the predetermined threshold, h / formula [0010] determining a remaining battery life (RBLT) using 6. The method of claim 5, further comprising the step of: the BOT specifying the actual time the battery has been in operation.

7. The internal resistance (R 120s 2. The diagnostic method of claim 1, wherein the periodic measurement of (I) is performed by applying a charging or discharging current for a fixed time interval.

8. 8. The diagnostic method according to claim 7, wherein the fixed time interval is between 60 seconds and 180 seconds for a discharge current corresponding to a nominal capacity (Cn) of the battery.

9. 2. A system for controlling a battery employing an aqueous electrolyte (BMS) for implementing the method of claim 1, comprising a measurement sensor and a processor configured to deliver a message to a user notifying either a failure of the battery or correct operation of the battery based on measurements made by the measurement sensor.

10. 10. Use of the method according to claim 1 or the system according to claim 9 in an application in which the battery acts as a standby store of power or as a base and backup for a low voltage network of electric vehicles.

Citation Information

Patent Citations

  • Device for diagnosing service life of battery

    JP1996136629A

  • Method for judging life of sealed lead-acid battery

    JP1999233162A

  • Method for monitoring condition of lead-acid battery

    JP2002334725A

  • Apparatus for determining degradation level

    JP2006010601A

  • Battery performance monitor

    US20090027056A1