Y-type molecular sieve containing rare earth, its manufacturing method, and catalytic cracking catalyst containing said molecular sieve
Pressurized hydrothermal calcination enhances the movement of rare earth ions into the sodalite cage, improving the hydrothermal stability and catalytic activity of Y-type molecular sieves, addressing the limitations of current production methods and enhancing heavy oil catalyst performance.
Patent Information
- Application Number
- JP2022501264
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-02-28
- Filing Date
- 2020-07-09
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-07-09
Smart Images

Figure 0007595638000011 
Figure 0007595638000012 
Figure 0007595638000013
Abstract
Description
Detailed Description of the Invention
[0001] [Technical field] The present invention relates to a rare earth-containing Y-type molecular sieve, a method for producing the same, and a catalytic cracking catalyst containing the molecular sieve.
[0002] [Background technology] In modern refineries, catalytic cracking is the most important production technology, and catalytic cracking units are used to convert heavy oils and residual oils into gasoline, diesel and light gas components.
[0003] In industry, catalytic cracking equipment must include both reaction and high-temperature catalyst regeneration, so catalysts must consider factors such as catalytic activity and selectivity. Compared with other types of molecular sieves, Y-type molecular sieves are often used in catalytic cracking. As the active component of catalytic cracking catalyst, its main role in catalytic cracking catalyst is to produce gasoline molecular products.
[0004] Rare earth exchange rare earth Y-type molecular sieve is a highly active component of catalytic cracking catalyst.
[0005] The rare earth ions in the rare earth Y-type molecular sieve move from the supercage to the sodalite cage to form a polynuclear cationic structure containing oxygen bridges, which improves the stability of the acid center of the molecular sieve in high-temperature hydrothermal environment, and improves the catalytic cracking activity and activity stability of the molecular sieve catalyst, thereby improving the heavy oil conversion activity and selectivity of the catalyst.
[0006] When ion exchange is carried out between a NaY molecular sieve and an aqueous solution of a rare earth salt, it is difficult for a hydrated rare earth ion with a diameter of about 0.79 nm to enter the sodalite cage through the six-membered ring window (diameter about 0.26 nm) of the Y molecular sieve.
[0007] Therefore, in the manufacturing process of rare earth Y-type molecular sieves, it is necessary to remove the hydration layer surrounding the rare earth ions through calcination so that the rare earth ions can enter the sodalite cages and be placed in the hexagonal columns. At the same time, the sodium ions in these cages will also move to the supercages through the calcination process. In short, the result of calcination is to accelerate the intracrystalline exchange between solid ions, and to increase the exchange rate between the molecular sieve and other cations in the aqueous solution, such as NH4 + and R.E. 3+ , creating conditions for exchange of the molecular sieve Na + The content was reduced (USP3402996).
[0008] How to promote the migration of rare earth ions and improve the occupancy rate of the fixable cation sites (within the sodalite cage) by rare earth ions is directly related to the performance of the rare earth Y-type molecular sieve, and also affects the activity stability of the catalyst using the rare earth Y-type molecular sieve as the active component.
[0009] In industry, high-temperature calcination or high-temperature hydrothermal calcination is usually used to promote the migration of rare earth ions into sodalite cages; however, excessively high calcination temperatures not only place strict requirements on the materials of industrial calcination furnaces, but also tend to cause the rare earth ions fixed in the appropriate positions to return to the supercages (Zerolites, 6(4), 235, 1986).
[0010] Current status of industrial calcination technology: NaY and RE 3+ The rare earth NaY (sodium oxide content 4.5-6.0%) molecular sieve filter cake obtained after the exchange with is subjected to solid ion exchange by high temperature calcination (550-580°C), and then subjected to aqueous solution exchange to remove sodium.
[0011] The main challenge now is to further improve the degree of ion exchange in the current solid state.
[0012] Therefore, how to move more rare earth ions to the sodalite cage sites at a limited calcination temperature to improve the stability of the molecular sieve has become a technical problem to be solved in industry.
[0013] CN1026225 describes a method for producing rare earth Y-type molecular sieves, in which NaY-type molecular sieves and RE 3+ After ion-exchanging once in an aqueous solution, the mixture is calcined at 450 to 600°C in a 100% steam stream for 1 to 3 hours.
[0014] CN103508467A describes a rare earth Y-type molecular sieve and a method for producing the same, in which the NaY-type molecular sieve is contacted with a rare earth salt solution or a mixed solution of an ammonium salt and a rare earth salt solution, filtered, washed with water, dried, and then calcined to obtain a rare earth NaY-type molecular sieve. The rare earth NaY-type molecular sieve is then strongly mixed and stirred with water to contact with an ammonium salt solution, mixed with a rare earth salt solution, and the pH value of the slurry is adjusted with an alkaline liquid to perform rare earth precipitation. Or the rare earth NaY-type molecular sieve is strongly mixed and stirred with water to contact with a mixed solution of an ammonium salt and a rare earth salt solution, and the pH value of the slurry is adjusted with an alkaline liquid to perform rare earth precipitation, filtered, dried, and then calcined for the second time to obtain a rare earth Y-type molecular sieve.
[0015] This method requires two exchange steps, two calcination steps, and a step of precipitating rare earths.
[0016] In the prior art, due to the limitations of calcination technology, in the process of rare earth ions moving to sodalite cage sites in rare earth Y-type molecular sieves at limited calcination temperatures, some rare earth ions still remain in supercages and cannot move to sodalite cages, which limits the hydrothermal stability of rare earth Y-type molecular sieves, thus affecting the heavy oil catalytic cracking conversion ability of catalytic cracking catalysts.
[0017] Summary of the Invention The inventors of the present invention have unexpectedly found through a large amount of testing that a rare earth-containing Y-type molecular sieve with unique mesopore properties can be obtained by hydrothermal calcination under pressure. The rare earth-containing Y-type molecular sieve has higher activity stability and hydrothermal stability. Based on this, the present invention is formed.
[0018] The present invention provides a rare earth-containing Y-type molecular sieve. The molecular sieve has at least two types of mesopore pore size distributions, 2-3 nm and 3-4 nm. For example, the molecular sieve has at least three types of mesopore pore size distributions, 2-3 nm, 3-4 nm, and 10-30 nm, respectively.
[0019] The present invention also provides a catalytic cracking catalyst, which comprises the rare earth-containing Y-type molecular sieve and an inorganic oxide binder and / or a natural mineral.
[0020] The present invention provides a method for producing a rare earth-containing Y-type molecular sieve. The method includes a step of subjecting a rare earth-containing NaY-type molecular sieve to hydrothermal calcination treatment in an environment where pressure is applied from the outside and water is added from the outside. The above environment has a gauge pressure of 0.01 to 1.0 MPa and contains 1 to 100% water vapor, and the hydrothermal calcination treatment is performed at 300 to 800°C, preferably 400 to 600°C. The rare earth-containing NaY-type molecular sieve is obtained through a step of contacting the NaY-type molecular sieve with a rare earth salt solution or a mixed solution of a rare earth salt solution and an ammonium salt.
[0021] The present invention provides a method for producing a rare earth-containing Y-type molecular sieve, which includes the following steps: (1) a step of partially exchanging a NaY-type molecular sieve with an ammonium salt to remove 10-80% of sodium ions, followed by filtering, washing with water, and drying to obtain an NH4NaY-type molecular sieve; (2) a step of contacting the NH4NaY-type molecular sieve obtained in step (1) with a rare earth salt solution or a mixed solution of a rare earth salt solution and an ammonium salt, followed by filtering, washing with water, and drying to obtain an NaY-type molecular sieve containing a rare earth; and (3) a step of applying pressure from the outside and adding an aqueous solution containing an acidic or alkaline substance from the outside to obtain an NaY-type molecular sieve containing a rare earth. or contacting the NaY type molecular sieve containing a rare earth obtained in the step (2) with an acidic or alkaline substance to obtain a NaY type molecular sieve containing a rare earth containing an acidic or alkaline substance, and then performing a hydrothermal calcination treatment in an environment to which pressure is applied from the outside and water is added from the outside; the above environment has a gauge pressure of 0.01 to 1 MPa and contains 1 to 100% water vapor, and the hydrothermal calcination treatment is performed at 300 to 800°C, preferably 400 to 600°C.
[0022] The rare earth-containing Y-type molecular sieve provided by the present invention has higher hydrothermal structure stability and higher catalytic cracking activity stability, and has reduced coke selectivity, and may be widely used in the field of heavy oil catalyst.
[0023] The method for producing the rare earth-containing Y-type molecular sieve provided by the present invention can promote the migration of rare earth ions from the supercages to the sodalite cages, and form a unique pore size distribution characteristic. The method is simple and easy to operate, and the mesopores of the Y-type molecular sieve are significantly increased. The method can form a certain degree of mesopores of the molecular sieve, improve the accessibility, and improve the utilization rate of the active center. The method is a new method for enlarging the pores of molecular sieve crystals at low cost and with low emissions.
[0024] BRIEF DESCRIPTION OF THE DRAWINGS FIG. 1 shows the pore size distribution curve of PAY-1 calculated based on the BJH model calculation.
[0025] FIG. 2 is an X-ray diffraction (XRD) spectrum of PAY-1.
[0026] FIG. 3 shows the pore size distribution curve on DAY-1 calculated based on the BJH model calculation.
[0027] FIG. 4 shows the pore size distribution curve of PDY-1 calculated based on the BJH model calculation.
[0028] FIG. 5 shows the pore size distribution curve of DDY-1 calculated based on the BJH model calculation.
[0029] FIG. 6 shows the pore size distribution curves of PBY-1 (curve a), DBY-1.1 (curve b) and PCY-1 (curve A) calculated based on the BJH model calculation.
[0030] FIG. 7 shows the adsorption-desorption curves of PBY-1 (curve c), DBY-1.1 (curve d) and PCY-1 (curve c).
[0031] [Mode for carrying out the invention] (Y-type molecular sieve containing rare earths) The present invention provides a rare earth-containing Y-type molecular sieve. The molecular sieve has at least two types of mesopore pore size distributions, 2-3 nm and 3-4 nm. For example, the molecular sieve has at least three types of mesopore pore size distributions, 2-3 nm, 3-4 nm, and 10-30 nm, respectively.
[0032] According to one embodiment of the present invention, in the BJH pore size distribution curve, the ratio of the peak area of the pore size distribution of 2-3 nm to the peak area of the pore size distribution of 3-4 nm is ≧0.05, for example ≧0.1, or 0.1-0.4.
[0033] According to one embodiment of the present invention, the rare earth-containing Y-type molecular sieve of the present invention is characterized by having at least 2-3 nm, 3-4 nm, and 10-30 nm mesopore pore size distributions. In the BJH pore size distribution graph, the ratio of the peak area of the 2-3 nm pore size distribution to the peak area of all pores is greater than 0.1, and the ratio of the peak area of the 10-30 nm pore size distribution to the peak area of all pores is greater than 0.2. For example, the ratio of the peak area of the 2-3 nm pore size distribution to the peak area of all pores is greater than 0.12, and the ratio of the peak area of the 10-30 nm pore size distribution to the peak area of all pores is greater than 0.22. Or, the ratio of the peak area of the 2-3 nm pore size distribution to the peak area of all pores is greater than 0.15, and the ratio of the peak area of the 10-30 nm pore size distribution to the peak area of all pores is greater than 0.25. Alternatively, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of all pores is 0.18 to 0.26, and the ratio of the peak area of the pore size distribution of 10 to 30 nm to the peak area of all pores is 0.27 to 0.32. Alternatively, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of all pores is greater than 0.12, preferably greater than 0.15, and more preferably 0.18 to 0.26, and the ratio of the peak area of the pore size distribution of 10 to 30 nm to the peak area of all pores is greater than 0.22, preferably greater than 0.25, and more preferably 0.27 to 0.32.
[0034] According to one embodiment of the present invention, the rare earth-containing Y-type molecular sieve of the present invention is characterized by having at least three types of mesopore pore size distributions of 2-3 nm, 3-4 nm, and 10-30 nm. In a BJH pore size distribution graph, the ratio of the peak area of the pore size distribution of 2-3 nm to the peak area of all pores is greater than 0.1, and the ratio of the peak area of the pore size distribution of 10-30 nm to the peak area of all pores is greater than 0.2. For example, the ratio of the peak area of the pore size distribution of 2-3 nm to the peak area of all pores is greater than 0.12, and the ratio of the peak area of the pore size distribution of 10-30 nm to the peak area of all pores is greater than 0.22. Alternatively, the ratio of the peak area of the pore size distribution of 2-3 nm to the peak area of all pores is greater than 0.15, and the ratio of the peak area of the pore size distribution of 10-30 nm to the peak area of all pores is greater than 0.25. Alternatively, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of all pores is 0.18 to 0.26, the ratio of the peak area of the pore size distribution of 10 to 30 nm to the peak area of all pores is 0.27 to 0.32, and the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of the pore size distribution of 3 to 4 nm is ≧0.05, for example ≧0.1, or 0.1 to 0.4.
[0035] According to one embodiment of the present invention, the rare earth content of the rare earth-containing Y-type molecular sieve of the present invention is 1 to 20% by weight, for example, 2 to 18% by weight, or 8 to 15% by weight, as rare earth oxide, the unit lattice constant is 2.440 to 2.470 nm, and the crystallinity is 30 to 60%.
[0036] According to one embodiment of the present invention, the mesopore volume of the rare earth-containing Y-type molecular sieve of the present invention is greater than 0.03 cc / g, for example, greater than 0.031 cc / g, or 0.031 cc / g to 0.037 cc / g, or 0.031 cc / g to 0.057 cc / g. The mesopore refers to a pore having a pore diameter of 2 to 50 nm.
[0037] In the X-ray diffraction pattern of the rare earth-containing Y-type molecular sieve, the peak at 2θ=11.8±0.1° can be used to represent the distribution of rare earths in the sodalite cage, and I1 indicates its peak intensity. The peak at 2θ=12.3±0.1° can be used to represent the distribution of rare earths in the supercages, and I2 indicates its peak intensity. The ratio of I1 to I2 indicates the degree of migration of rare earth ions from the supercages to the sodalite cages, with a higher ratio indicating a better degree of migration and vice versa.
[0038] In the case of using a rare earth-containing Y-type molecular sieve obtained by calcining with ordinary water vapor under normal pressure, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° in the X-ray diffraction pattern is usually <4.
[0039] In the rare earth-containing Y-type molecular sieve of the present invention, the ratio of the peak intensity I1 at 2θ=11.8±0.1° to the peak intensity I2 at 2θ=12.3±0.1° in the X-ray diffraction pattern may be >4.0, ≧4.0, >4.3, ≧4.8, ≧4.9, for example, 4.5 to 6.0, for example, 4.8 to 6.0, or 4.8 to 7.0.
[0040] (catalyst) The present invention also provides a catalytic cracking catalyst, which comprises the rare earth-containing Y-type molecular sieve and an inorganic oxide binder and / or a natural mineral.
[0041] According to one embodiment of the present invention, the catalytic cracking catalyst comprises, on a dry weight basis, a Y-type molecular sieve containing 20-60 wt % of rare earth, 10-30 wt % of an inorganic oxide binder, and 30-50 wt % of a natural mineral.
[0042] According to one embodiment of the present invention, the rare earth-containing Y-type molecular sieve is the main catalytic cracking active component.
[0043] Both inorganic oxide binders and natural minerals are commonly used in the art.
[0044] In the catalytic cracking catalyst of the present invention, the natural mineral includes at least one selected from kaolin, halloysite, montmorillonite, diatomite, attapulgite, sepiolite, keramite, hydrotalcite, bentonite and rectorite, and the inorganic oxide binder or its precursor includes at least one selected from silica sol, alumina sol, peptized pseudoboehmite, silica alumina sol and phosphorus-containing alumina sol.
[0045] The method for producing a catalytic cracking catalyst of the present invention includes the following steps: mixing raw materials for producing a catalytic cracking catalyst, including a Y-type molecular sieve containing rare earth, a natural mineral, and an inorganic oxide binder, with water, vigorously stirring, and spray-drying, so that the catalyst contains, on a dry weight basis, 20 to 60 wt % of the Y-type molecular sieve containing rare earth, 10 to 30 wt % of the inorganic oxide binder, and 30 to 50 wt % of the natural mineral.
[0046] (Production method of Y-type molecular sieve containing rare earth) The first method for producing a rare earth-containing Y-type molecular sieve of the present invention includes a step of subjecting a rare earth-containing NaY-type molecular sieve to hydrothermal calcination treatment in an environment where pressure is applied from the outside and water is added from the outside. The environment has a gauge pressure of 0.01 to 1 MPa and contains 1 to 100% water vapor, and the hydrothermal calcination treatment is performed at 300 to 800°C, preferably 400 to 600°C.
[0047] In the method of the present invention, the rare earth-containing NaY type molecular sieve is obtained through step A of contacting the NaY type molecular sieve with a rare earth salt solution or a mixed solution of a rare earth salt solution and an ammonium salt.
[0048] In step A, the rare earth salt solution is an aqueous chloride solution containing one or more of lanthanum, cerium, praseodymium and neodymium ions, and the ammonium salt is selected from ammonium chloride, ammonium nitrate, ammonium carbonate and ammonium bicarbonate, or any mixture thereof.
[0049] In the method of the present invention, step A is preferably carried out at a pH of 3.0 to 5.0, a water / molecular sieve weight ratio of 5 to 30, and an exchange temperature of room temperature to 100°C.
[0050] After the contact treatment in step A, step A includes the usual filtration, washing with water, and drying, the purpose of which is, for example, to remove chloride ions and prevent corrosion of equipment in the subsequent calcination step, and also to partially remove sodium.
[0051] In the method of the present invention, the hydrothermal calcination treatment is carried out in an environment where pressure is applied from the outside and water is added from the outside.
[0052] The above environment is obtained by applying pressure from the outside and adding water from the outside, and preferably has a gauge pressure of 0.1 to 0.8 MPa, more preferably has a gauge pressure of 0.3 to 0.6 MPa, and preferably the environment contains 30 to 100% water vapor, more preferably the environment contains 60 to 100% water vapor.
[0053] The application of pressure from the outside refers to applying a constant pressure from the outside to the raw materials during the hydrothermal calcination treatment, and is carried out, for example, by introducing an inert gas from the outside to maintain a constant back pressure.
[0054] The amount of water added from the outside is such that the environment contains 1 to 100% water vapor.
[0055] The method of the present invention may include a step of ammonium exchange after the hydrothermal calcination treatment.
[0056] The ammonium exchange is carried out for at least 0.3 hours at room temperature to 100° C. The weight ratio of the rare earth NaY-type molecular sieve, the ammonium salt, and water is 1:(0.05-0.5):(5-30) based on the dry weight of the molecular sieve.
[0057] The second method for preparing the rare earth-containing Y-type molecular sieve of the present invention is characterized in that it comprises the following steps: (1) a process for partially exchanging the NaY-type molecular sieve with an ammonium salt to remove 10-80% of sodium ions, and then filtering, washing with water, and drying to obtain an NH4NaY-type molecular sieve; (2) a process for contacting the NH4NaY-type molecular sieve obtained in the process (1) with a rare earth salt solution or a mixed solution of a rare earth salt solution and an ammonium salt, and then filtering, washing with water, and drying to obtain an NaY-type molecular sieve containing rare earths; (3) A step of subjecting the NaY-type molecular sieve containing rare earth obtained in the step (2) to hydrothermal calcination in an environment where pressure is applied from the outside and water is added from the outside. The above environment has a gauge pressure of 0.01 to 1 MPa and contains 1 to 100% water vapor, and the hydrothermal calcination is performed at 300 to 800°C, preferably 400 to 600°C.
[0058] In the production method of the present invention, the ammonium salt in the steps (1) and (2) is selected from ammonium chloride, ammonium nitrate, ammonium carbonate, ammonium bicarbonate, or any mixture thereof.
[0059] In the process of the present invention, in the step (1), the NaY type molecular sieve and the ammonium salt are partially exchanged with ammonium for the purpose of removing 10 to 80%, preferably 20 to 60%, of the sodium ions.
[0060] The process may, for example, include exchanging the NaY-type molecular sieve with an ammonium salt solution at a NaY-type molecular sieve exchange temperature of room temperature to 100°C for at least 0.3 hours, with the weight ratio of water to molecular sieve being 5-30 and the weight ratio of ammonium salt to molecular sieve being 0.01-3.
[0061] In the production method of the present invention, in the step (2), the rare earth salt solution is an aqueous chloride solution containing one or more of lanthanum, cerium, praseodymium, and neodymium ions.
[0062] In the step (2) of the production method of the present invention, the contact treatment of the NaY type molecular sieve with the rare earth salt solution or the mixed solution of the rare earth salt solution and the ammonium salt includes exchanging the NaY type molecular sieve with the rare earth salt solution or the mixed solution of the ammonium salt and the rare earth salt solution at a slurry pH of 3.0 to 5.0, a water / molecular sieve weight ratio of 5 to 30, and an exchange temperature of room temperature to 100° C. for at least 0.3 hours.
[0063] After the contact treatment in step (2), step (2) also includes the usual filtration, washing with water, and drying, the purpose of which is, for example, to remove chloride ions and prevent corrosion of equipment in the subsequent calcination step, and also to partially remove sodium.
[0064] In the production method of the present invention, the hydrothermal calcination treatment in step (3) is carried out in an environment where pressure is applied from the outside and water is added from the outside.
[0065] The above environment is obtained by applying pressure from the outside and adding water from the outside, and preferably has a gauge pressure of 0.1 to 0.8 MPa, more preferably has a gauge pressure of 0.3 to 0.6 MPa, and preferably the environment contains 30 to 100% water vapor, more preferably the environment contains 60 to 100% water vapor.
[0066] The application of pressure from the outside refers to applying a constant pressure from the outside to the raw materials during the hydrothermal calcination treatment, and is carried out, for example, by introducing an inert gas from the outside to maintain a constant back pressure.
[0067] The amount of water added from the outside is such that the environment contains 1 to 100% water vapor.
[0068] The production method of the present invention may include a step (4) of carrying out ammonium exchange after the step (3).
[0069] The ammonium exchange in step (4) is carried out for at least 0.3 hours at room temperature to 100° C. The weight ratio of the rare earth NaY-type molecular sieve, the ammonium salt, and water is 1:(0.05-0.5):(5-30), based on the dry weight of the molecular sieve.
[0070] According to the above-mentioned preparation method of the present invention, the rare earth-containing Y-type molecular sieve of the present invention is prepared, which has unique pore size distribution characteristics, and the molecular sieve has mesopore pore size distributions of at least 2-3 nm, 3-4 nm and 10-30 nm, the ratio of the peak area of the pore size distribution of 2-3 nm to the peak area of all pores is greater than 0.1, and the ratio of the peak area of the pore size distribution of 10-30 nm to the peak area of all pores is greater than 0.2.
[0071] The third method for producing the rare earth-containing Y-type molecular sieve of the present invention includes the following steps: hydrothermal calcination of the rare earth-containing NaY-type molecular sieve in an environment where pressure is applied from the outside and an aqueous solution containing an acidic or alkaline substance is added from the outside, and recovery of the product. The above environment has a gauge pressure of 0.01 to 1 MPa and contains 1 to 100% water vapor.
[0072] In the production method of the present invention, the rare earth-containing NaY type molecular sieve is preferably obtained through contact treatment of the NaY type molecular sieve with a rare earth salt solution or a mixed solution of a rare earth salt solution and an ammonium salt, followed by filtration, washing with water, and drying.
[0073] The rare earth salt solution is an aqueous chloride solution containing one or more of lanthanum, cerium, praseodymium and neodymium ions.
[0074] The ammonium salt is selected from ammonium chloride, ammonium nitrate, ammonium carbonate and ammonium bicarbonate, or any mixture thereof.
[0075] The contact treatment of the NaY type molecular sieve with the rare earth salt solution or the mixed solution of the rare earth salt solution and the ammonium salt includes exchanging the NaY type molecular sieve with the rare earth salt solution or the mixed solution of the rare earth salt solution and the ammonium salt at a slurry pH of 3.0 to 5.0, a water / molecular sieve weight ratio of 5 to 30, and an exchange temperature of room temperature to 100° C. for at least 0.3 hours.
[0076] In the method of the present invention, the hydrothermal calcination treatment is carried out in an environment where pressure is applied from the outside and water is added from the outside.
[0077] The above environment is obtained by applying pressure from the outside and adding water from the outside, and preferably has a gauge pressure of 0.1 to 0.8 MPa, more preferably has a gauge pressure of 0.3 to 0.6 MPa, and preferably the above environment contains 30 to 100% water vapor, more preferably the above environment contains 60 to 100% water vapor.
[0078] The application of pressure from the outside refers to applying a constant pressure from the outside to the raw materials during the hydrothermal calcination treatment, and is carried out, for example, by introducing an inert gas from the outside to maintain a constant back pressure.
[0079] The amount of water added from the outside is such that the environment contains 1 to 100% water vapor.
[0080] The process of the invention may include a subsequent ammonium exchange step.
[0081] The ammonium exchange is carried out for at least 0.3 hours at room temperature to 100° C. The weight ratio of the rare earth NaY-type molecular sieve, the ammonium salt, and water is 1:(0.05-0.5):(5-30), based on the dry weight of the molecular sieve.
[0082] The NaY type molecular sieve containing rare earth is calcined in an environment having a gauge pressure of 0.01 to 0.1 MPa, containing 1 to 100% water vapor, and containing an acidic or alkaline substance, preferably at 300 to 800°C, 0.1 to 0.8 MPa, and 30 to 100% water vapor for at least 0.1 hours, and more preferably at 400 to 600°C, 0.3 to 0.6 MPa, and 60 to 100% water vapor for 1 to 3 hours.
[0083] The acidic substance includes ammonium chloride, ammonium sulfate, ammonium carbonate, ammonium bicarbonate, ammonium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, hydrochloric acid, sulfuric acid, nitric acid, or any mixture thereof. The acidic substance is preferably selected from ammonium carbonate, ammonium bicarbonate, ammonium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, or any mixture thereof. The alkaline substance includes one or more selected from ammonia water, a buffer solution of ammonia water and ammonium chloride, sodium hydroxide, sodium metaaluminate, sodium carbonate, sodium bicarbonate, or any mixture thereof. The alkaline substance preferably includes ammonia water, or a buffer solution of ammonia water and ammonium chloride.
[0084] The production method of the present invention may further include subjecting the product rare earth NaY type molecular sieve to an ammonium salt aqueous solution exchange treatment, filtering, washing with water, and drying to obtain a Y type molecular sieve containing rare earth.
[0085] The exchange treatment is carried out for at least 0.3 hours at room temperature to 100° C. The weight ratio of the rare earth Y-type molecular sieve, the ammonium salt, and water is 1:(0.05-0.5):(5-30), based on the dry weight of the molecular sieve.
[0086] The fourth method for producing the rare earth-containing Y-type molecular sieve of the present invention includes the steps of: contacting a rare earth-containing NaY-type molecular sieve with an acidic or alkaline substance to obtain a rare earth-containing NaY-type molecular sieve containing an acidic or alkaline substance, and subjecting the rare earth-containing NaY-type molecular sieve to hydrothermal calcination treatment in an environment where pressure is applied from the outside and water is added from the outside, the environment having a gauge pressure of 0.01 to 1.0 MPa and containing 1 to 100% water vapor.
[0087] In the production method of the present invention, the rare earth-containing NaY-type molecular sieve is preferably obtained by a step A including contacting the NaY-type molecular sieve with a rare earth salt solution or a mixed solution of a rare earth salt solution and an ammonium salt, filtering, washing with water, and drying.
[0088] The rare earth salt solution in step A is an aqueous chloride solution containing one or more of lanthanum, cerium, praseodymium and neodymium ions.
[0089] The ammonium salt in step A is selected from ammonium chloride, ammonium nitrate, ammonium carbonate and ammonium bicarbonate, or any mixture thereof.
[0090] The contact treatment of the NaY type molecular sieve with the rare earth salt solution or the mixed solution of the rare earth salt solution and the ammonium salt in the step A usually includes exchanging the NaY type molecular sieve with the rare earth salt solution or the mixed solution of the ammonium salt and the rare earth salt solution at a slurry pH of 3.0-5.0, a water / molecular sieve weight ratio of 5-30, and an exchange temperature of room temperature to 100° C. for at least 0.3 hours.
[0091] In the manufacturing method of the present invention, an acidic or alkaline substance is used to modify the rare earth-containing NaY-type molecular sieve. The acidic substance includes ammonium chloride, ammonium sulfate, ammonium carbonate, ammonium bicarbonate, ammonium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, hydrochloric acid, sulfuric acid, nitric acid, or any mixture thereof. The alkaline substance includes one or more of ammonia water, a buffer solution of ammonia water and ammonium chloride, sodium hydroxide, sodium metaaluminate, sodium carbonate, sodium bicarbonate, or any mixture thereof. The contact with the acidic or alkaline substance may be in a conventional manner, such as impregnation or filling.
[0092] In the production method of the present invention, the hydrothermal calcination treatment is carried out in an environment where pressure is applied from the outside and water is added from the outside.
[0093] The above environment is obtained by applying pressure from the outside and adding water from the outside, and preferably has a gauge pressure of 0.1 to 0.8 MPa, more preferably has a gauge pressure of 0.3 to 0.6 MPa, and preferably the above environment contains 30 to 100% water vapor, more preferably the above environment contains 60 to 100% water vapor.
[0094] The application of pressure from the outside refers to applying a constant pressure from the outside to the raw materials during the hydrothermal calcination treatment, and is carried out, for example, by introducing an inert gas from the outside to maintain a constant back pressure.
[0095] The amount of water added from the outside is such that the environment contains 1 to 100% water vapor.
[0096] The hydrothermal calcination is carried out at a temperature of 300 to 800° C., preferably 400 to 600° C. The calcination time is at least 0.1 hour, preferably 0.5 to 3 hours.
[0097] The fifth method for preparing the rare earth-containing Y-type molecular sieve of the present invention includes the following steps: (1) partially exchanging the NaY molecular sieve with an ammonium salt to remove 10-80% of sodium ions, and then filtering, washing with water, and drying to obtain a NHNaY molecular sieve; (2) contacting the NH4NaY-type molecular sieve obtained in step (1) with a rare earth salt solution or a mixed solution of a rare earth salt solution and an ammonium salt, filtering, washing with water, and drying to obtain a NaY-type molecular sieve containing rare earths; (3) A step of subjecting the NaY-type molecular sieve containing rare earth obtained in step (2) to hydrothermal calcination in an environment where pressure is applied from the outside and an aqueous solution containing an acidic or alkaline substance is added from the outside, or contacting the NaY-type molecular sieve containing rare earth obtained in step (2) with an acidic or alkaline substance to obtain a NaY-type molecular sieve containing rare earth containing an acidic or alkaline substance, and then subjecting the NaY-type molecular sieve to hydrothermal calcination in an environment where pressure is applied from the outside and water is added from the outside; the above environment has a gauge pressure of 0.01 to 1.0 MPa (e.g., 0.1 to 0.8 MPa or 0.3 to 0.6 MPa) and contains 1 to 100% (e.g., 30 to 100% or 60 to 100%) water vapor, and the hydrothermal calcination is performed at 300 to 800°C, preferably 400 to 600°C.
[0098] In the production method of the present invention, the ammonium salt in the steps (1) and (2) is selected from ammonium chloride, ammonium nitrate, ammonium carbonate, ammonium bicarbonate, or any mixture thereof.
[0099] In the production method of the present invention, the purpose of partially exchanging the NaY type molecular sieve with an ammonium salt in the step (1) is to remove 10 to 80%, preferably 20 to 60%, of sodium ions.
[0100] The process may include, for example, exchanging the NaY type molecular sieve with an ammonium salt solution at an exchange temperature of room temperature to 100°C for at least 0.3 hours, with the weight ratio of water to molecular sieve being 5-30 and the weight ratio of ammonium salt to molecular sieve being 0.01-3.
[0101] In the production method of the present invention, in the step (2), the rare earth salt solution is an aqueous chloride solution containing one or more of lanthanum, cerium, praseodymium, and neodymium ions.
[0102] In the step (2) of the production method of the present invention, the contact treatment of the NaY type molecular sieve with the rare earth salt solution or the mixed solution of the rare earth salt solution and the ammonium salt includes exchanging the NaY type molecular sieve with the rare earth salt solution or the mixed solution of the ammonium salt and the rare earth salt solution at a slurry pH of 3.0 to 5.0, a water / molecular sieve weight ratio of 5 to 30, and an exchange temperature of room temperature to 100° C. for at least 0.3 hours.
[0103] After the contact treatment in step (2), step (2) also includes the usual filtration, washing with water, and drying, the purpose of which is, for example, to remove chloride ions and prevent corrosion of equipment in the subsequent calcination step, and also to partially remove sodium.
[0104] In the production method of the present invention, the hydrothermal calcination treatment in step (3) is carried out in an environment where pressure is applied from the outside and water is added from the outside.
[0105] The acidic substance may include, but is not limited to, ammonium chloride, ammonium sulfate, ammonium carbonate, ammonium bicarbonate, ammonium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, hydrochloric acid, sulfuric acid, nitric acid, or any mixture thereof. The acidic substance may preferably include ammonium carbonate, ammonium bicarbonate, ammonium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, or any mixture thereof. The alkaline substance may include, but is not limited to, ammonia water, a buffer solution of ammonia water and ammonium chloride, sodium hydroxide, sodium metaaluminate, sodium carbonate, sodium bicarbonate, or any mixture thereof. The alkaline substance may preferably include ammonia water, or a buffer solution of ammonia water and ammonium chloride.
[0106] The above environment is obtained by applying pressure from the outside and adding water from the outside, and preferably has a gauge pressure of 0.1 to 0.8 MPa, more preferably has a gauge pressure of 0.3 to 0.6 MPa, and preferably the above environment contains 30 to 100% water vapor, more preferably the above environment contains 60 to 100% water vapor.
[0107] The application of pressure from the outside refers to applying a constant pressure from the outside to the raw materials during the hydrothermal calcination treatment, and is carried out, for example, by introducing an inert gas from the outside to maintain a constant back pressure.
[0108] The amount of water in the aqueous solution containing an acidic or alkaline substance added from outside is such that the environment contains 1 to 100% water vapor.
[0109] The production method of the present invention may include a step (4) of carrying out ammonium exchange after the step (3).
[0110] The ammonium exchange in step (4) is carried out for at least 0.3 hours at room temperature to 100° C. The weight ratio of the rare earth NaY-type molecular sieve, the ammonium salt, and water is 1:(0.05-0.5):(5-30), based on the dry weight of the molecular sieve.
[0111] According to the above-mentioned manufacturing method of the present invention, the rare earth-containing Y-type molecular sieve of the present invention is manufactured, which has unique pore size distribution characteristics, and the molecular sieve has mesopore pore size distributions of at least 2-3 nm, 3-4 nm, and 10-30 nm. The ratio of the peak area of the pore size distribution of 2-3 nm to the peak area of all pores is greater than 0.1, and the ratio of the peak area of the pore size distribution of 10-30 nm to the peak area of all pores is greater than 0.2. Furthermore, in the BJH pore size distribution curve, the ratio of the peak area of the pore size distribution of 2-3 nm to the peak area of the pore size distribution of 3-4 nm is ≧0.05, for example ≧0.1, or 0.1-0.4.
[0112] In the method for preparing the rare earth-containing Y-type molecular sieve provided by the present invention, the calcination may be included only once, and preferably, the calcination is included only once.
[0113] The present invention also provides the following technical solutions: A1. A rare earth-containing Y-type molecular sieve having at least two types of mesopore pore size distributions of 2-3 nm and 3-4 nm.
[0114] A2. The molecular sieve according to technical proposal A1, wherein in a BJH pore size distribution curve, the ratio of the peak area of the pore size distribution of 2-3 nm to the peak area of the pore size distribution of 3-4 nm is ≧0.05, preferably ≧0.1, more preferably 0.1-0.4.
[0115] A3. The molecular sieve according to technical proposal A1, wherein the rare earth content is 2-18 wt. % as rare earth oxide, preferably 8-15 wt. %, the unit lattice constant is 2.440-2.470 nm, and the crystallinity is 30-60%.
[0116] A4. The molecular sieve according to Technical Proposal A1, wherein the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° in the X-ray diffraction pattern is ≧4.0, preferably 4.5-6.0.
[0117] A5. A method for producing the rare earth-containing Y-type molecular sieve according to any one of technical proposals A1 to A4, comprising the step of subjecting the rare earth-containing NaY-type molecular sieve to hydrothermal calcination treatment in an environment where pressure is applied from the outside and water is added from the outside. The above environment has a gauge pressure of 0.01 to 1.0 MPa and contains 1 to 100% water vapor.
[0118] A6. The method according to Technical Proposal A5, in which the NaY-type molecular sieve containing rare earth is obtained through a step A of contacting the NaY-type molecular sieve with a rare earth salt solution or a mixed solution of a rare earth salt solution and an ammonium salt.
[0119] A7. The method according to technical solution A6, wherein the rare earth salt solution is an aqueous chloride solution containing one or more of lanthanum, cerium, praseodymium and neodymium ions.
[0120] A8. The method according to technical proposal A6, wherein the ammonium salt is selected from ammonium chloride, ammonium nitrate, ammonium carbonate and ammonium bicarbonate, or any mixture thereof.
[0121] A9. The method according to technical proposal A6, wherein step A is carried out at pH=3.0-5.0, water / molecular sieve weight ratio of 5-30, and exchange temperature of room temperature-100°C.
[0122] A10. The method according to Technical Proposal A5, wherein the environment preferably has a gauge pressure of 0.1-0.8 MPa, more preferably 0.3-0.6 MPa, and contains 30-100% water vapor, preferably 60-100% water vapor.
[0123] A11. The method according to Technical Proposal A5, wherein the hydrothermal calcination step is carried out at 300 to 800°C, preferably 400 to 600°C.
[0124] B1. A rare earth-containing Y-type molecular sieve, which has at least mesopore pore size distributions of 2-3 nm, 3-4 nm, and 10-30 nm, and in a BJH pore size distribution graph, the ratio of the peak area of the 2-3 nm pore size distribution to the peak area of all pores is greater than 0.1, and the ratio of the peak area of the 10-30 nm pore size distribution to the peak area of all pores is greater than 0.2.
[0125] B2. The molecular sieve according to technical proposal B1, wherein the ratio of the peak area of the pore size distribution of 2-3 nm to the peak area of all pores is greater than 0.12, preferably greater than 0.15, more preferably 0.18-0.26, and the ratio of the peak area of the pore size distribution of 10-30 nm to the peak area of all pores is greater than 0.22, preferably greater than 0.25, more preferably 0.27-0.32.
[0126] B3. The molecular sieve according to technical proposal B1, wherein the rare earth content is 2-18 wt. % as rare earth oxide, preferably 8-15 wt. %, the unit lattice constant is 2.440-2.470 nm, and the crystallinity is 30-60%.
[0127] B4. The molecular sieve according to Technical Proposal B1, wherein the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° in the X-ray diffraction pattern is greater than 4.0, preferably greater than 4.3, more preferably 4.8 to 6.0.
[0128] B5. A method for producing a rare earth-containing Y-type molecular sieve, comprising the steps of: (1) partially exchanging the NaY molecular sieve with an ammonium salt to remove 10-80% of sodium ions, and then filtering, washing with water, and drying to obtain a NHNaY molecular sieve; (2) contacting the NH4NaY-type molecular sieve obtained in step (1) with a rare earth salt solution or a mixed solution of a rare earth salt solution and an ammonium salt, filtering, washing with water, and drying to obtain a NaY-type molecular sieve containing rare earths; (3) subjecting the NaY-type molecular sieve containing rare earths obtained in the step (2) to hydrothermal calcination in an environment in which pressure is applied from the outside and water is added from the outside, the environment having a gauge pressure of 0.01 to 1.0 MPa and containing 1 to 100% water vapor; method.
[0129] B6. The method according to technical proposal B5, wherein in step (1) and step (2), the ammonium salt is selected from ammonium chloride, ammonium nitrate, ammonium carbonate and ammonium bicarbonate, or any mixture thereof.
[0130] B7. The method according to technical proposal B5, wherein in step (2), the rare earth salt solution is an aqueous chloride solution containing one or more of lanthanum, cerium, praseodymium and neodymium ions.
[0131] B8. The method according to Technical Proposal B5, in which in step (2), the NaY-type molecular sieve is exchanged with a rare earth salt solution or a mixed solution of a rare earth salt solution and an ammonium salt at a slurry pH of 3.0-5.0, a water / molecular sieve weight ratio of 5-30, and an exchange temperature of room temperature to 100°C for at least 0.3 hours.
[0132] B9. The method according to Technical Proposal B5, wherein the environment in step (3) has a gauge pressure of 0.1-0.8 MPa, more preferably 0.3-0.6 MPa, and the environment contains 30-100% water vapor, preferably 60-100% water vapor.
[0133] B10. The method according to Technical Solution B5, wherein the hydrothermal calcination in step (3) is carried out at 300-800°C, preferably 400-600°C.
[0134] C1. A method for producing a Y-type molecular sieve containing a rare earth, comprising the steps of: hydrothermally calcining a NaY-type molecular sieve containing a rare earth in an environment where pressure is applied from the outside and an aqueous solution containing an acidic or alkaline substance is added from the outside; and recovering the product, the environment having a gauge pressure of 0.01-1.0 MPa and containing 1-100% water vapor.
[0135] C2. The method according to the technical proposal C1, in which the NaY-type molecular sieve containing rare earth is obtained by contacting the NaY-type molecular sieve with a rare earth salt solution or a mixed solution of a rare earth salt solution and an ammonium salt, filtering, washing with water, and drying.
[0136] C3. The method according to technical proposal C2, wherein the rare earth salt solution is an aqueous chloride solution containing one or more of lanthanum, cerium, praseodymium and neodymium ions.
[0137] C4. The method according to technical proposal C2, wherein the ammonium salt is selected from ammonium chloride, ammonium nitrate, ammonium carbonate and ammonium bicarbonate, or any mixture thereof.
[0138] C5. The method according to technical proposal C2, wherein the contacting treatment of the NaY-type molecular sieve with the rare earth salt solution or the mixed solution of the rare earth salt solution and the ammonium salt includes exchanging the NaY-type molecular sieve with the rare earth salt solution or the mixed solution of the ammonium salt and the rare earth salt solution at a pH of the slurry=3.0-5.0, a weight ratio of water / molecular sieve of 5-30, and an exchange temperature of room temperature-100°C for at least 0.3 hours.
[0139] C6. The method according to technical proposal C1 or 2, wherein the acidic substance comprises ammonium chloride, ammonium sulfate, ammonium carbonate, ammonium bicarbonate, ammonium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, hydrochloric acid, sulfuric acid, nitric acid, or any mixture thereof.
[0140] C7. The method according to technical proposal C1, wherein the alkaline substance comprises one or more of ammonia water, a buffer solution of ammonia water and ammonium chloride, sodium hydroxide, sodium carbonate, sodium bicarbonate, or any mixture thereof.
[0141] C8. The method according to Technical Proposal C1, wherein the environment preferably has a gauge pressure of 0.1-0.8 MPa, more preferably 0.3-0.6 MPa, and the hydrothermal calcination temperature is 300-800°C, preferably 400-600°C.
[0142] C9. The method according to technical proposal C1, wherein the environment contains 30-100% water vapor, preferably 60-100% water vapor.
[0143] C10. A rare earth-containing Y-type molecular sieve obtained by any one of the methods described in technical proposals C1 to C9.
[0144] C11. The molecular sieve according to technical proposal C10, having at least two kinds of mesopore pore size distributions of 2-3 nm and 3-4 nm, and the volume of the mesopores is greater than 0.03 cc / g.
[0145] C12. The molecular sieve according to technical proposal C10, wherein the volume of the mesopores is 0.031cc / g-0.037cc / g.
[0146] C13. The molecular sieve according to technical proposal C10, wherein the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° in the X-ray diffraction pattern is ≧4.0, preferably 4.5-6.0.
[0147] C14. The molecular sieve according to technical proposal C10, wherein the rare earth content is 2-18 wt. % as rare earth oxide, preferably 8-15 wt. %, the unit lattice constant is 2.440-2.470 nm, and the crystallinity is 30-60%.
[0148] D1. A method for modifying a Y-type molecular sieve, comprising the steps of: contacting a rare earth-containing NaY-type molecular sieve with an alkaline substance to obtain a rare earth-containing NaY-type molecular sieve containing an alkaline substance, and then carrying out a hydrothermal calcination treatment in an environment where pressure is applied from the outside and water is added from the outside, the environment having a gauge pressure of 0.01 to 1.0 MPa and containing 1 to 100% water vapor; method.
[0149] D2. The method according to technical proposal D1, wherein the rare earth-containing NaY-type molecular sieve is obtained by contacting the NaY-type molecular sieve with a rare earth salt solution or a mixed solution of a rare earth salt solution and an ammonium salt, and then filtering, washing, and drying the resulting product.
[0150] D3. The method according to technical proposal D2, wherein in step A, the rare earth salt solution is an aqueous chloride solution containing one or more of lanthanum, cerium, praseodymium and neodymium ions.
[0151] D4. The method according to technical proposal D2, wherein in step A, the ammonium salt is selected from ammonium chloride, ammonium nitrate, ammonium carbonate and ammonium bicarbonate, or any mixture thereof.
[0152] D5. The method according to technical proposal D2, wherein step A is carried out at pH=3.0-5.0, water / molecular sieve weight ratio of 5-30, and exchange temperature of room temperature-100°C.
[0153] D6. The method according to technical proposal D1, wherein the alkaline substance is selected from ammonia water, a buffer solution of ammonia water and ammonium chloride, sodium hydroxide, sodium carbonate, sodium bicarbonate, and any mixture thereof.
[0154] D7. The method according to Technical Proposal D1, wherein the environment has a gauge pressure of 0.1-0.8 MPa, preferably 0.3-0.6 MPa, and the hydrothermal calcination temperature is 300-800°C, preferably 400-600°C.
[0155] D8. The method according to technical proposal D1 or D7, wherein the environment contains 30-100% water vapor, preferably 60-100% water vapor.
[0156] D9. A rare earth-containing Y-type molecular sieve obtained by any one of the methods described in technical proposals D1 to D8.
[0157] D10. The molecular sieve according to technical proposal D9, having at least two kinds of mesopore pore size distributions of 2-3 nm and 3-4 nm, and the volume of the mesopores is greater than 0.031 cc / g.
[0158] D11. The molecular sieve according to technical proposal D9, wherein the volume of the mesopores is 0.031 cc / g-0.057 cc / g.
[0159] D12. The molecular sieve according to technical proposal D9, wherein the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° in the X-ray diffraction pattern is ≧4.0, preferably 4.5-6.0.
[0160] D13. The molecular sieve according to technical proposal D9, wherein the rare earth content is 2-18% by weight, preferably 8-15% by weight, as rare earth oxide; the unit lattice constant is 2.440-2.470 nm; and the crystallinity is 30-60%.
[0161] E1. A catalytic cracking catalyst comprising an inorganic oxide binder, a natural mineral, and a Y-type molecular sieve containing a rare earth, the Y-type molecular sieve containing a rare earth having at least two types of mesopore pore size distributions of 2-3 nm and 3-4 nm.
[0162] E2. The catalyst according to technical proposal E1, which comprises, on a dry weight basis, 10-30 wt% of an inorganic oxide binder, 30-50 wt% of a natural mineral, and a Y-type molecular sieve containing 20-60 wt% of rare earth.
[0163] E3. The catalyst according to technical proposal E1, wherein the rare earth-containing Y-type molecular sieve has a BJH pore size distribution curve in which the ratio of the peak area of the pore size distribution of 2-3 nm to the peak area of the pore size distribution of 3-4 nm is ≧0.05, preferably ≧0.1, and more preferably 0.1-0.4.
[0164] E4. The catalyst according to technical proposal E1, wherein the rare earth content of the rare earth-containing Y-type molecular sieve is 1-20% by weight, preferably 8-15% by weight, as rare earth oxide, the unit lattice constant is 2.440-2.470 nm, and the crystallinity is 30-60%.
[0165] E5. The catalyst according to technical proposal E1, wherein the rare earth-containing Y-type molecular sieve has an X-ray diffraction pattern in which the ratio of the peak intensity I1 at 2θ=11.8±0.1° to the peak intensity I2 at 2θ=12.3±0.1° is ≧4.0, preferably 4.5-6.0.
[0166] E6. The catalyst according to any one of technical proposals E1 to E5, wherein the rare earth-containing Y-type molecular sieve is obtained by a process including hydrothermal calcination of a rare earth-containing NaY-type molecular sieve in an environment where pressure is applied from the outside and water is added from the outside, and the above environment has a gauge pressure of 0.01 to 1.0 MPa and contains 1 to 100% water vapor.
[0167] E7. The catalyst according to Technical Proposal E6, wherein the NaY-type molecular sieve containing rare earth is obtained from step A of contacting the NaY-type molecular sieve with a rare earth salt solution or a mixed solution of a rare earth salt solution and an ammonium salt, and preferably, step A is carried out at pH=3.0-5.0, a weight ratio of water / molecular sieve of 5-30, and an exchange temperature of room temperature to 100°C.
[0168] E8. The catalyst according to technical proposal E7, wherein the rare earth salt solution is an aqueous chloride solution containing one or more of lanthanum, cerium, praseodymium and neodymium ions, and the ammonium salt is selected from ammonium chloride, ammonium nitrate, ammonium carbonate and ammonium bicarbonate, or any mixture thereof.
[0169] E9. The catalyst according to Technical Proposal E6, wherein the environment preferably has a gauge pressure of 0.1-0.8 MPa, more preferably 0.3-0.6 MPa, contains 30-100% water vapor, preferably 60-100% water vapor, and the hydrothermal calcination treatment step is carried out at 300-800°C, preferably 400-600°C.
[0170] E10. The catalyst according to technical proposal E1, wherein the natural mineral is at least one selected from kaolin, halloysite, montmorillonite, diatomite, attapulgite, sepiolite, keramite, hydrotalcite, bentonite and rectorite, and the inorganic oxide binder is at least one selected from silica sol, alumina sol, peptized pseudoboehmite, silica alumina sol and phosphorus-containing alumina sol.
[0171] F1. A catalytic cracking catalyst comprising a rare earth-containing Y-type molecular sieve, the catalyst comprising a rare earth-containing Y-type molecular sieve, an inorganic oxide binder and a natural mineral, the rare earth-containing Y-type molecular sieve having at least a pore size distribution of 2-3 nm and 3-4 nm mesopores, and in a BJH pore size distribution graph, a ratio of a peak area of a pore size distribution of 2-3 nm to a peak area of all pores is greater than 0.1, and a ratio of a peak area of a pore size distribution of 10-30 nm to a peak area of all pores is greater than 0.2.
[0172] F2. The catalyst according to technical proposal F1, comprising, based on the dry weight of the catalyst, a Y-type molecular sieve containing 20-60 wt.% of rare earth, 10-30 wt.% of an inorganic oxide binder, and 30-50 wt.% of natural minerals.
[0173] F3. The catalyst according to technical proposal F1, wherein the ratio of the peak area of the pore size distribution of 2-3 nm to the peak area of all pores of the rare earth-containing Y-type molecular sieve is greater than 0.12, preferably greater than 0.15, more preferably 0.18-0.26, and the ratio of the peak area of the pore size distribution of 10-30 nm to the peak area of all pores is greater than 0.22, preferably greater than 0.25, more preferably 0.27-0.32.
[0174] F4. The catalyst according to technical proposal F1, wherein the rare earth-containing Y-type molecular sieve has a rare earth content of 1-20% by weight, preferably 8-15% by weight, calculated as rare earth oxide, a unit lattice constant of 2.440-2.470 nm, and a crystallinity of 30-60%.
[0175] F5. The catalyst according to technical proposal F1, wherein the rare earth-containing Y-type molecular sieve has an X-ray diffraction pattern in which the ratio of the peak intensity I1 at 2θ=11.8±0.1° to the peak intensity I2 at 2θ=12.3±0.1° is greater than 4.0, preferably greater than 4.3, more preferably 4.8-6.0.
[0176] F6. The catalyst according to technical proposal F1, wherein the rare earth-containing Y-type molecular sieve is obtained by a method including the following steps: (1) partially exchanging the NaY molecular sieve with an ammonium salt to remove 10-80% of sodium ions, and then filtering, washing with water, and drying to obtain a NHNaY molecular sieve; (2) contacting the NH4NaY-type molecular sieve obtained in step (1) with a rare earth salt solution or a mixed solution of a rare earth salt solution and an ammonium salt, filtering, washing with water, and drying to obtain a NaY-type molecular sieve containing rare earths; (3) A step of subjecting the NaY-type molecular sieve containing rare earths obtained in the step (2) to hydrothermal calcination treatment in an environment where pressure is applied from the outside and water is added from the outside, the above environment having a gauge pressure of 0.01 to 1.0 MPa and containing 1 to 100% water vapor; catalyst.
[0177] F7. The catalyst according to technical proposal F6, wherein the ammonium salt in step (1) and step (2) is selected from ammonium chloride, ammonium nitrate, ammonium carbonate and ammonium bicarbonate, or any mixture thereof; the rare earth salt solution in step (2) is an aqueous chloride solution containing one or more of lanthanum, cerium, praseodymium and neodymium ions.
[0178] F8. The catalyst according to technical proposal F6, wherein the contact treatment in step (2) is performed at a slurry pH of 3.0-5.0, a water / molecular sieve weight ratio of 5-30, and an exchange temperature of room temperature-100°C for at least 0.3 hours.
[0179] F9. The catalyst according to Technical Proposal F6, wherein the environment in step (3) has a gauge pressure of 0.1-0.8 MPa, more preferably 0.3-0.6 MPa, and contains 30-100% water vapor, preferably 60-100% water vapor; and the hydrothermal calcination treatment in step (3) is carried out at 300-800°C, preferably 400-600°C.
[0180] F10. The catalyst according to technical proposal F1, wherein the natural mineral is at least one selected from kaolin, halloysite, montmorillonite, diatomite, attapulgite, sepiolite, keramite, hydrotalcite, bentonite and rectorite; and the inorganic oxide binder is at least one selected from silica sol, alumina sol, peptized pseudoboehmite, silica alumina sol and phosphorus-containing alumina sol.
[0181] G1. A cracking catalyst comprising a rare earth-containing Y-type molecular sieve, an inorganic oxide binder and a natural mineral, wherein the rare earth-containing Y-type molecular sieve has at least two types of mesopore pore size distributions of 2-3 nm and 3-4 nm, and the mesopore volume is greater than 0.03 cc / g.
[0182] G2. The cracking catalyst according to technical proposal G1, comprising, based on the dry weight of the cracking catalyst, a Y-type molecular sieve containing 20-60 wt.% of rare earth, 10-30 wt.% of an inorganic oxide binder, and 30-50 wt.% of a natural mineral.
[0183] G3. The cracking catalyst according to technical proposal G1, wherein the volume of the mesopores is greater than 0.031 cc / g.
[0184] G4. The cracking catalyst according to technical proposal G1, wherein the volume of the mesopores is 0.031cc / g-0.057cc / g.
[0185] G5. The cracking catalyst according to technical proposal G1, wherein the rare earth-containing Y-type molecular sieve has an X-ray diffraction pattern in which the ratio of the peak intensity I1 at 2θ=11.8±0.1° to the peak intensity I2 at 2θ=12.3±0.1° is ≧4.0, preferably 4.5-6.0.
[0186] G6. The decomposition catalyst according to Technical Proposal G1, wherein the rare earth-containing Y-type molecular sieve is obtained by a step 1 of hydrothermal calcination of a rare earth-containing NaY-type molecular sieve in an environment in which pressure is applied from the outside and an aqueous solution containing an acidic or alkaline substance is added from the outside; or the rare earth-containing Y-type molecular sieve is obtained by a step 2 of hydrothermal calcination of a rare earth-containing NaY-type molecular sieve in an environment in which pressure is applied from the outside and water is added from the outside, the gauge pressure being 0.01-1 MPa, and the water vapor being 1-100%.
[0187] G7. The decomposition catalyst according to technical proposal G6, wherein the NaY-type molecular sieve containing rare earth is obtained by contacting the NaY-type molecular sieve with a rare earth salt solution or a mixed solution of a rare earth salt solution and an ammonium salt, and then filtering, washing, and drying the resulting decomposition catalyst.
[0188] G8. The decomposition catalyst according to technical proposal G6, wherein the rare earth salt solution is a chloride aqueous solution containing one or more of lanthanum, cerium, praseodymium and neodymium ions, and the ammonium salt is selected from ammonium chloride, ammonium nitrate, ammonium carbonate and ammonium bicarbonate, or any mixture thereof.
[0189] G9. The decomposition catalyst according to technical proposal G6, wherein the acidic substance is selected from ammonium chloride, ammonium sulfate, ammonium carbonate, ammonium bicarbonate, ammonium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, hydrochloric acid, sulfuric acid, nitric acid, and any mixture thereof.
[0190] G10. The decomposition catalyst according to technical proposal G6, wherein the alkaline substance comprises one or more of ammonia water, a buffer solution of ammonia water and ammonium chloride, sodium hydroxide, sodium carbonate, sodium bicarbonate, and any mixture thereof.
[0191] G11. The decomposition catalyst according to technical proposal G6, wherein the environment is preferably a gauge pressure of 0.1 to 0.8 MPa, more preferably 0.3 to 0.6 MPa, and the hydrothermal calcination temperature is 300 to 800°C, preferably 400 to 600°C.
[0192] G12. The decomposition catalyst according to technical proposal G6, wherein the environment contains 30-100% water vapor, preferably 60-100% water vapor.
[0193] G13. The decomposition catalyst according to technical proposal G1, wherein the inorganic oxide binder is at least one selected from silica sol, alumina sol, peptized pseudo-boehmite, silica alumina sol and phosphorus-containing alumina sol, and the natural mineral is at least one selected from kaolin, halloysite, montmorillonite, diatomite, attapulgite, sepiolite, keramite, hydrotalcite, bentonite and rectorite.
[0194] H1. A rare earth-containing Y-type molecular sieve having at least two types of mesopore pore size distribution of 2-3 nm and 3-4 nm, the volume of the mesopores of the molecular sieve is greater than 0.03 cc / g, and / or the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° in the X-ray diffraction pattern of the molecular sieve is ≧4.0.
[0195] H2. The molecular sieve according to Technical Proposal H1, wherein in a BJH pore size distribution curve of the molecular sieve, the ratio of the peak area of the pore size distribution of 2-3 nm to the peak area of the pore size distribution of 3-4 nm is ≧0.05, preferably ≧0.1, more preferably 0.1-0.4.
[0196] H3. The molecular sieve according to any one of the above technical solutions, wherein the rare earth content is 2-18% by weight, preferably 8-15% by weight, as rare earth oxide; the unit lattice constant is 2.440-2.470 nm; and the crystallinity is 30-60%.
[0197] H4. The molecular sieve according to any one of the above technical solutions, wherein the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° in the X-ray diffraction pattern is ≧4.0, preferably 4.5-6.0, for example ≧4.8, or 4.9-7.0.
[0198] H5. The molecular sieve according to any one of the above technical solutions, wherein in the BJH pore size distribution curve of the molecular sieve, the molecular sieve has a pore size distribution of 10-30 nm mesopores, and the ratio of the peak area of the pore size distribution of 2-3 nm to the peak area of all pores is greater than 0.1, for example, greater than 0.12, greater than 0.15, more preferably 0.18-0.26. The ratio of the peak area of the pore size distribution of 10-30 nm to the peak area of all pores is greater than 0.2, for example, greater than 0.22, greater than 0.25, more preferably 0.27-0.32.
[0199] H6. The molecular sieve according to any one of the above technical solutions, wherein the volume of the mesopores is 0.031 cc / g to 0.057 cc / g.
[0200] H7. A method for producing a rare earth-containing Y-type molecular sieve according to any one of Technical Schemes H1 to H6, wherein the rare earth-containing Y-type molecular sieve is obtained by a process of hydrothermal calcination of a rare earth-containing NaY-type molecular sieve in an environment where pressure is applied from the outside and an aqueous solution containing an acidic or alkaline substance is added from the outside; or the rare earth-containing Y-type molecular sieve is obtained by a process of contacting a rare earth-containing NaY-type molecular sieve with an acidic or alkaline substance to obtain a rare earth-containing NaY-type molecular sieve containing an acidic or alkaline substance, and then hydrothermal calcination in an environment where pressure is applied from the outside and water is added from the outside, wherein the above-mentioned environment has a gauge pressure of 0.01 to 1.0 MPa, for example, 0.1 to 0.8 MPa, and preferably 0.3 to 0.6 MPa, and contains 1 to 100% water vapor, for example, 30 to 100% water vapor, and preferably 60 to 100% water vapor.
[0201] H8. The method according to Technical Proposal H7, in which the rare earth-containing NaY-type molecular sieve is obtained through a step A of contacting the NaY-type molecular sieve with a rare earth salt solution or a mixed solution of a rare earth salt solution and an ammonium salt.
[0202] H9. The method according to technical proposal H7, in which the NaY-type molecular sieve containing rare earth is obtained by the following steps (1) and (2): (1) partially exchanging the NaY molecular sieve with an ammonium salt to remove 10-80% of sodium ions, and then filtering, washing with water, and drying to obtain a NHNaY molecular sieve; (2) contacting the NH4NaY-type molecular sieve obtained in step (1) with a rare earth salt solution or a mixed solution of a rare earth salt solution and an ammonium salt, filtering, washing with water, and drying to obtain a NaY-type molecular sieve containing rare earths; method.
[0203] H10. The method according to any one of technical proposals H7 to H9, wherein the rare earth salt solution is an aqueous chloride solution containing one or more of lanthanum, cerium, praseodymium and neodymium ions.
[0204] H11. The method according to any one of technical proposals H7 to H10, wherein the ammonium salt is selected from ammonium chloride, ammonium nitrate, ammonium carbonate and ammonium bicarbonate, or any mixture thereof.
[0205] H12. The method according to any one of technical proposals H7 to H11, wherein step A or step (2) is carried out at pH=3.0-5.0, a weight ratio of water / molecular sieve is 5-30, and an exchange temperature is room temperature-100°C, and optionally, the exchange time is at least 0.3 hours.
[0206] H13. A method according to any one of Technical Proposals H7 to H12, wherein the environment has a gauge pressure of 0.1 to 0.8 MPa, more preferably 0.3 to 0.6 MPa, and contains 30 to 100% water vapor, preferably 60 to 100% water vapor.
[0207] H14. A method according to any one of Technical Proposals H7 to H13, wherein the hydrothermal calcination step is carried out at 300 to 800°C, preferably 400 to 600°C.
[0208] H15. A method according to any one of Technical Proposals H7 to H14, wherein the environment having water is an environment having an aqueous solution containing an acidic substance or an alkaline substance, the acidic substance being selected from ammonium chloride, ammonium sulfate, ammonium carbonate, ammonium bicarbonate, ammonium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, hydrochloric acid, sulfuric acid, nitric acid, and any mixture thereof, and the alkaline substance being one or more of ammonia water, a buffer solution of ammonia water and ammonium chloride, sodium hydroxide, sodium metaaluminate, sodium carbonate, sodium bicarbonate, and any mixture thereof.
[0209] H16. A method according to any one of Technical Proposals H7 to H15, wherein the mass concentration of the aqueous solution containing the acidic substance or alkaline substance is 0.1 to 20%.
[0210] H17. A catalytic cracking catalyst, comprising: a Y-type molecular sieve containing 20-60% by weight of the rare earth described in any one of technical proposals 1-6; 10-30% by weight of an inorganic oxide binder; and 30-50% by weight of a natural mineral.
[0211] H18. The catalytic cracking catalyst according to technical proposal H17, wherein the natural mineral is at least one selected from kaolin, halloysite, montmorillonite, diatomite, attapulgite, sepiolite, keramite, hydrotalcite, bentonite and rectorite, and the inorganic oxide binder is at least one selected from silica sol, alumina sol, peptized pseudoboehmite, silica alumina sol and phosphorus-containing alumina sol.
[0212] M1. A rare earth-containing Y-type molecular sieve having at least two mesopore pore size distributions of 2-3 nm and 3-4 nm.
[0213] M2. The molecular sieve according to technical proposal M1, wherein in a BJH pore size distribution curve, the ratio of the peak area of the pore size distribution of 2-3 nm to the peak area of the pore size distribution of 3-4 nm is ≧0.05, preferably ≧0.1, more preferably 0.1-0.4.
[0214] M3. The molecular sieve according to any one of the above technical solutions, wherein the rare earth content is 2-18% by weight, preferably 8-15% by weight, as calculated as rare earth oxide; the unit lattice constant is 2.440-2.470 nm; and the crystallinity is 30-60%.
[0215] M4. The molecular sieve according to any one of the above technical solutions, wherein the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° in the X-ray diffraction pattern is ≧4.0, preferably 4.5-6.0, for example ≧4.8, or 4.9-7.0.
[0216] M5. The molecular sieve according to any one of the above technical solutions, wherein in the BJH pore size distribution curve of the molecular sieve, the molecular sieve has a pore size distribution of 10-30 nm mesopores, and the ratio of the peak area of the pore size distribution of 2-3 nm to the peak area of all pores is greater than 0.1, for example, greater than 0.12, greater than 0.15, more preferably 0.18-0.26. The ratio of the peak area of the pore size distribution of 10-30 nm to the peak area of all pores is greater than 0.2, for example, greater than 0.22, greater than 0.25, more preferably 0.27-0.32.
[0217] M6. The molecular sieve according to any one of the above technical solutions, wherein the mesopore volume of the molecular sieve is greater than 0.03 cc / g, for example, 0.031 cc / g-0.037 cc / g or 0.031 cc / g-0.057 cc / g.
[0218] M7. A method for producing the rare earth-containing Y-type molecular sieve according to any one of technical proposals M1 to M6, comprising a step of subjecting the rare earth-containing NaY-type molecular sieve to hydrothermal calcination treatment in an environment to which pressure is applied from the outside and water is added from the outside, wherein the environment has a gauge pressure of 0.01 to 1.0 MPa, for example, 0.1 to 0.8 MPa, and preferably 0.3 to 0.6 MPa, and contains 1 to 100% water vapor, for example, 30 to 100% water vapor, and preferably 60 to 100% water vapor.
[0219] M8. The method according to technical proposal M7, wherein the rare earth-containing NaY-type molecular sieve is obtained through a step A of contacting the NaY-type molecular sieve with a rare earth salt solution or a mixed solution of a rare earth salt solution and an ammonium salt.
[0220] M9. The method according to technical proposal M7, in which the NaY-type molecular sieve containing rare earth is obtained by the following steps (1) and (2): (1) partially exchanging the NaY molecular sieve with an ammonium salt to remove 10-80% of sodium ions, and then filtering, washing with water, and drying to obtain a NHNaY molecular sieve; (2) contacting the NH4NaY-type molecular sieve obtained in step (1) with a rare earth salt solution or a mixed solution of a rare earth salt solution and an ammonium salt, filtering, washing with water, and drying to obtain a NaY-type molecular sieve containing rare earths; method.
[0221] M10. A method according to any one of technical proposals M7 to M9, wherein the environment having water is an environment having pure water, or an environment having an aqueous solution containing an acidic substance or an alkaline substance.
[0222] M11. The method according to any one of technical proposals M7 to M10, wherein the rare earth salt solution is an aqueous chloride solution containing one or more of lanthanum, cerium, praseodymium and neodymium ions; the ammonium salt is selected from ammonium chloride, ammonium nitrate, ammonium carbonate and ammonium bicarbonate, or any mixture thereof.
[0223] M12. The method according to any one of technical proposals M7 to M11, wherein step A or step (2) is carried out at pH=3.0-5.0, the weight ratio of water / molecular sieve is 5-30, and the exchange temperature is room temperature-100°C, and optionally the exchange time is at least 0.3 hours.
[0224] M13. A method according to any one of technical proposals M7 to M12, wherein the environment has a gauge pressure of preferably 0.1 to 0.8 MPa, more preferably 0.3 to 0.6 MPa, and contains 30 to 100% water vapor, preferably 60 to 100% water vapor.
[0225] M14. A method according to any one of technical proposals M7 to M13, wherein the hydrothermal calcination step is carried out at 300 to 800°C, preferably 400 to 600°C.
[0226] M15. The method according to any one of technical proposals M7 to M14, wherein the environment having water is an environment having an aqueous solution containing an acidic substance or an alkaline substance, the acidic substance being selected from ammonium chloride, ammonium sulfate, ammonium carbonate, ammonium bicarbonate, ammonium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, hydrochloric acid, sulfuric acid, nitric acid, and any mixture thereof, and the alkaline substance being one or more of ammonia water, a buffer solution of ammonia water and ammonium chloride, sodium hydroxide, sodium metaaluminate, sodium carbonate, sodium bicarbonate, and any mixture thereof.
[0227] M16. The method according to any one of technical proposals M7 to M15, wherein the mass concentration of the aqueous solution containing the acidic substance or alkaline substance is 0.1 to 20%.
[0228] M17. A catalytic cracking catalyst, comprising: a Y-type molecular sieve containing 20-60% by weight of the rare earth according to any one of the technical proposals M1-M6; 10-30% by weight of an inorganic oxide binder; and 30-50% by weight of a natural mineral.
[0229] M18. The catalytic cracking catalyst according to technical proposal M17, wherein the natural mineral is at least one selected from kaolin, halloysite, montmorillonite, diatomite, attapulgite, sepiolite, keramite, hydrotalcite, bentonite and rectorite, and the inorganic oxide binder is at least one selected from silica sol, alumina sol, peptized pseudoboehmite, silica alumina sol and phosphorus-containing alumina sol.
[0230] The method for producing the rare earth-containing Y-type molecular sieve provided by the present invention can promote the migration of rare earth ions from the supercages to the sodalite cages, and form a unique pore size distribution characteristic. The method is simple and easy to operate, and the mesopores of the Y-type molecular sieve are significantly increased. The method can form a certain degree of mesopores of the molecular sieve, improve the accessibility, and improve the utilization rate of the active center. The method is a new method for enlarging the pores of molecular sieve crystals at low cost and with low emissions.
[0231] As shown in the examples below, the method for producing the rare earth-containing Y-type molecular sieve of the present invention can provide a rare earth-containing Y-type molecular sieve with unique pore size distribution characteristics, i.e., at least two kinds of mesopore nanopore size distributions of 2-3 nm and 3-4 nm. The mesopore volume is larger than 0.03 cc / g, for example, 0.031 cc / g-0.037 cc / g, even up to 0.057 cc / g. A hysteresis loop with a larger area can be provided, in which the rare earth content is 8-15 wt% based on the rare earth oxide, the unit lattice constant is 2.440-2.470 nm, and the crystallinity is 30-60%.
[0232] The rare earth-containing Y-type molecular sieve provided by the present invention has higher hydrothermal structure stability and higher catalytic cracking activity stability, and has reduced coke selectivity, and may be widely used in the field of heavy oil catalyst.
[0233] [Example] The present invention will be further described below with reference to examples, but the contents of the present invention are not limited thereto.
[0234] In each of the examples and comparative examples, the unit cell constant and crystallinity of the rare earth-containing Y-type molecular sieve product of the present invention were determined by X-ray diffraction (XRD), the XRF analysis of the chemical composition of the product was performed by a Rigaku Denki Co., Ltd. (Japan) 3013 type X-ray fluorescence spectrometer, and the BJH pore size distribution curve of the product was measured by low-temperature nitrogen adsorption / desorption method.
[0235] (Example A1) Example A1 illustrates the preparation of rare earth-containing Y-type molecular sieve of the present invention, which can be used to prepare catalytic cracking catalyst.
[0236] 100g of NaY molecular sieve (China Petrochemical Catalyst Corporation Changling Branch, calcination loss 74.1% by weight, crystallinity 89.3%, the same below) and 1800g of deionized water were vigorously mixed and stirred, and 20mL of rare earth chloride salt solution with a concentration of 357g RE2O3 / L and 2g of solid ammonium chloride were added. The resulting mixture was stirred uniformly and the temperature was raised to 70℃. The pH value of the slurry was adjusted to 4.5 using dilute hydrochloric acid, and stirred at a constant temperature for 1.0 hour.
[0237] After filtering, washing and drying, pressure was applied from the outside, water was added, and then pressure hydrothermal calcination was performed in a 100% steam environment at 500°C, with a gauge pressure of 0.3 MPa for 2.0 hours to obtain a Y-type molecular sieve sample containing rare earths, which is designated as PAY-1.
[0238] In the chemical composition of PAY-1, the rare earth oxide content was 10.1 wt%.
[0239] FIG. 1 shows the pore size distribution curve of PAY-1 obtained from the BJH model calculation.
[0240] As can be seen from the pore size distribution curve, there are at least two types of mesopore pore size distributions, located at 2-3 nm and 3-4 nm, respectively, with the peak area ratio of the two being 0.15.
[0241] Figure 2 is the XRD pattern of PAY-1, which shows that the PAY-1 molecular sieve has a pure FAU crystal structure and no miscellaneous crystals are formed.
[0242] As shown in the XRD pattern, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 5.6.
[0243] The unit cell and crystallinity data are given in the table below.
[0244] (Comparative Example A1) Comparative Example A1 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by hydrothermal calcination at atmospheric pressure.
[0245] The process was the same as in Example A1, except that the firing conditions were atmospheric pressure (gauge pressure 0 MPa).
[0246] The obtained comparative sample of Y-type molecular sieve containing rare earth is designated as DAY-1.
[0247] In the chemical composition of DAY-1, the rare earth oxide content was 10.1 wt%.
[0248] FIG. 3 shows the pore size distribution curve on DAY-1 calculated based on the BJH model calculation.
[0249] As can be seen from the pore size distribution curve, there is mainly one type of mesopore pore size distribution, i.e., there is one type of mesopore pore size distribution at the position of 3–4 nm, but there is no other mesopore pore size distribution at the position of 2–3 nm.
[0250] Therefore, in the BJH pore size distribution curve, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of the pore size distribution of 3 to 4 nm was 0.
[0251] The XRD pattern of DAY-1 had similar features to the XRD pattern of PAY-1.
[0252] As shown in the XRD pattern, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 3.4.
[0253] The unit cell and crystallinity data are given in the table below.
[0254] (Example A2) Example A2 illustrates the preparation of rare earth-containing Y-type molecular sieve of the present invention, which can be used to prepare catalytic cracking catalyst.
[0255] 100g of NaY molecular sieve and 1000g of deionized water were mixed and stirred vigorously, and 16mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L and 8g of solid ammonium chloride were added. The mixture was stirred uniformly, the temperature was raised to 60℃, and the pH value of the slurry was adjusted to 4.0 with dilute hydrochloric acid, and stirred at constant temperature for 1.5 hours.
[0256] After filtering, washing and drying, pressure was applied from the outside, water was added, and then pressurized hydrothermal calcination was performed in an environment of 430°C, gauge pressure 0.8 MPa, and 50% water vapor for 0.5 hours to obtain a Y-type molecular sieve sample containing rare earths, which is designated as PAY-2.
[0257] In the chemical composition of PAY-2, the rare earth oxide content was 8.2 wt%.
[0258] The BJH pore size distribution curve and XRD pattern of PAY-2 had similar characteristics to those of PAY-1, respectively.
[0259] In the BJH pore size distribution curve, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of the pore size distribution of 3 to 4 nm was 0.3.
[0260] As shown in the XRD pattern, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 4.3.
[0261] The unit cell and crystallinity data are given in the table below.
[0262] (Comparative example A2) Comparative Example A2 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by hydrothermal calcination at atmospheric pressure.
[0263] The process was the same as in Example A2, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0264] The obtained comparative sample of Y-type molecular sieve containing rare earth is referred to as DAY-2.
[0265] In the chemical composition of DAY-2, the rare earth oxide content was 8.2 wt%.
[0266] The BJH pore size distribution curve and XRD pattern on DAY-2 had similar characteristics to those of the BJH pore size distribution curve on DAY-1 and the XRD pattern of PAY-1, respectively.
[0267] In the BJH pore size distribution curve, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of the pore size distribution of 3 to 4 nm was 0.
[0268] As shown in the XRD pattern, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 2.8.
[0269] The unit cell and crystallinity data are given in the table below.
[0270] (Example A3) Example A3 illustrates the preparation of rare earth-containing Y-type molecular sieve of the present invention, which can be used to prepare catalytic cracking catalyst.
[0271] 100g of NaY-type molecular sieve and 2200g of deionized water were mixed and stirred vigorously, and 24mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L was added. After the mixture was stirred uniformly, the temperature was raised to 70℃. The pH value of the slurry was adjusted to 3.5 with dilute hydrochloric acid, and stirred at a constant temperature for 1.0 hour.
[0272] After filtering, washing and drying, pressure was applied from the outside, water was added, and then pressurized hydrothermal calcination was performed in a 100% steam environment at 520°C, a gauge pressure of 0.4 MPa, for 1.5 hours to obtain a rare earth-containing Y-type molecular sieve sample, which is designated as PAY-3.
[0273] In the chemical composition of PAY-3, the rare earth oxide content was 11.4 wt%.
[0274] The BJH pore size distribution curve and XRD pattern of PAY-3 had similar characteristics to those of PAY-1, respectively.
[0275] In the BJH pore size distribution curve, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of the pore size distribution of 3 to 4 nm was 0.25.
[0276] As shown in the XRD pattern, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 5.2.
[0277] The unit cell and crystallinity data are given in the table below.
[0278] (Comparative example A3) Comparative Example A3 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by hydrothermal calcination at atmospheric pressure.
[0279] The process was the same as in Example A3, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0280] The obtained comparative sample of Y-type molecular sieve containing rare earth is designated as DAY-3.
[0281] In the chemical composition of DAY-3, the rare earth oxide content was 11.4 wt%.
[0282] The BJH pore size distribution curve and XRD pattern on DAY-3 had similar characteristics to those of the BJH pore size distribution curve on DAY-1 and the XRD pattern of PAY-1, respectively.
[0283] In the BJH pore size distribution curve, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of the pore size distribution of 3 to 4 nm was 0.
[0284] As shown in the XRD pattern, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 3.7.
[0285] The unit cell and crystallinity data are given in the table below.
[0286] (Example A4) Example A4 illustrates the preparation of rare earth-containing Y-type molecular sieve of the present invention, which can be used to prepare catalytic cracking catalyst.
[0287] 100g of NaY-type molecular sieve and 2800g of deionized water were mixed and stirred vigorously, and 28mL of rare earth chloride salt solution with a concentration of 357g RE2O3 / L was added. The mixture was stirred uniformly and the temperature was raised to 80℃. The pH value of the slurry was adjusted to 3.8 using dilute hydrochloric acid, and stirred at a constant temperature for 1.0 hour.
[0288] After filtering, washing and drying, pressure was applied from the outside, water was added, and then pressure hydrothermal calcination was performed in a 100% steam environment at 580°C, gauge pressure 0.5MPa, for 2.0 hours to obtain a Y-type molecular sieve sample containing rare earths, which is designated as PAY-4.
[0289] In the chemical composition of PAY-4, the rare earth oxide content was 12.6 wt%.
[0290] The BJH pore size distribution curve and XRD pattern of PAY-4 had similar characteristics to those of PAY-1, respectively.
[0291] In the BJH pore size distribution curve, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of the pore size distribution of 3 to 4 nm was 0.22.
[0292] As shown in the XRD pattern, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 4.9.
[0293] The unit cell and crystallinity data are given in the table below.
[0294] (Comparative example A4) Comparative Example A4 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by hydrothermal calcination at atmospheric pressure.
[0295] The process was the same as in Example A4, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0296] The obtained comparative sample of Y-type molecular sieve containing rare earth is designated as DAY-4.
[0297] In the chemical composition of DAY-4, the rare earth oxide content was 12.6 wt%.
[0298] The BJH pore size distribution curve and XRD pattern on DAY-4 had similar characteristics to those of the BJH pore size distribution curve on DAY-1 and the XRD pattern of PAY-1, respectively.
[0299] In the BJH pore size distribution curve, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of the pore size distribution of 3 to 4 nm was 0.
[0300] As shown in the XRD pattern, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 3.9.
[0301] The unit cell and crystallinity data are given in the table below.
[0302] (Example A5) Example A5 illustrates the preparation of rare earth-containing Y-type molecular sieve of the present invention, which can be used to prepare catalytic cracking catalyst.
[0303] 100g of NaY-type molecular sieve and 2000g of deionized water were mixed and stirred vigorously, and 32mL of rare earth chloride salt solution with a concentration of 357g RE2O3 / L was added. The mixture was stirred uniformly and the temperature was raised to 70℃. The pH value of the slurry was adjusted to 4.0 with dilute hydrochloric acid, and stirred at a constant temperature for 1.0 hour.
[0304] After filtering, washing, and drying, pressure was applied from the outside, water was added, and then pressure hydrothermal calcination was performed in a 100% steam environment at 550°C, a gauge pressure of 0.4 MPa, for 1.5 hours to obtain a rare earth-containing Y-type molecular sieve sample, which is designated as PAY-5.
[0305] In the chemical composition of PAY-5, the rare earth oxide content was 13.4 wt%.
[0306] The BJH pore size distribution curve and XRD pattern of PAY-5 had similar characteristics to those of PAY-1.
[0307] In the BJH pore size distribution curve, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of the pore size distribution of 3 to 4 nm was 0.23.
[0308] As shown in the XRD pattern, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 5.1.
[0309] The unit cell and crystallinity data are given in the table below.
[0310] (Comparative Example A5) Comparative Example A5 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by hydrothermal calcination at atmospheric pressure.
[0311] The process was the same as in Example A5, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0312] The obtained comparative sample of Y-type molecular sieve containing rare earth is designated as DAY-5.
[0313] In the chemical composition of DAY-5, the rare earth oxide content was 13.4 wt%.
[0314] The BJH pore size distribution curve and XRD pattern on DAY-5 had similar characteristics to those of the BJH pore size distribution curve on DAY-1 and the XRD pattern of PAY-1, respectively.
[0315] In the BJH pore size distribution curve, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of the pore size distribution of 3 to 4 nm was 0.
[0316] As shown in the XRD pattern, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 4.3.
[0317] The unit cell and crystallinity data are given in the table below.
[0318] (Example A6) Example A6 illustrates the preparation of rare earth-containing Y-type molecular sieve of the present invention, which can be used to prepare catalytic cracking catalyst.
[0319] 100g of NaY-type molecular sieve and 1800g of deionized water were mixed and stirred vigorously, and 20mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L and 2g of solid ammonium chloride were added. The mixture was stirred uniformly and the temperature was raised to 70°C. The pH value of the slurry was adjusted to 4.5 using dilute hydrochloric acid and stirred at a constant temperature for 1.0 hour.
[0320] After filtering, washing, and drying, pressure was applied from the outside, water was added, and then pressurized hydrothermal calcination was performed in a 100% steam environment at 430°C, with a gauge pressure of 0.6 MPa, for 2.0 hours to obtain a rare earth-containing Y-type molecular sieve sample, designated as PAY-6.
[0321] In the chemical composition of PAY-6, the rare earth oxide content was 10.0 wt%.
[0322] The BJH pore size distribution curve and XRD pattern of PAY-6 had similar characteristics to those of PAY-1.
[0323] In the BJH pore size distribution curve, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of the pore size distribution of 3 to 4 nm was 0.20.
[0324] As shown in the XRD pattern, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 4.7.
[0325] The unit cell and crystallinity data are given in the table below.
[0326] (Comparative example A6) Comparative Example A6 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by hydrothermal calcination at atmospheric pressure.
[0327] The process was the same as in Example A6, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0328] The obtained comparative sample of Y-type molecular sieve containing rare earth is designated as DAY-6.
[0329] In the chemical composition of DAY-6, the rare earth oxide content was 10.0 wt%.
[0330] The BJH pore size distribution curve and XRD pattern of DAY-6 had similar characteristics to those of DAY-1 and the XRD pattern of PAY-1, respectively.
[0331] In the BJH pore size distribution curve, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of the pore size distribution of 3 to 4 nm was 0.
[0332] As shown in the XRD pattern, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 2.7.
[0333] The unit cell and crystallinity data are given in the table below.
[0334] (Example A7) Example A7 illustrates the preparation of rare earth-containing Y-type molecular sieve of the present invention, which can be used to prepare catalytic cracking catalyst.
[0335] 100g of NaY-type molecular sieve and 1800g of deionized water were mixed and stirred vigorously, and 20mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L and 2g of solid ammonium chloride were added. The mixture was stirred uniformly and the temperature was raised to 70°C. The pH value of the slurry was adjusted to 4.5 using dilute hydrochloric acid and stirred at a constant temperature for 1.0 hour.
[0336] After filtering, washing, and drying, pressure was applied from the outside, water was added, and then pressure hydrothermal calcination was performed in a 100% steam environment at 400°C, with a gauge pressure of 0.8 MPa for 2.0 hours to obtain a rare earth-containing Y-type molecular sieve sample, designated as PAY-7.
[0337] In the chemical composition of PAY-7, the rare earth oxide content was 9.8 wt%.
[0338] The BJH pore size distribution curve and XRD pattern of PAY-7 had similar characteristics to those of PAY-1.
[0339] In the BJH pore size distribution curve, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of the pore size distribution of 3 to 4 nm was 0.11.
[0340] As shown in the XRD pattern, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 4.1.
[0341] The unit cell and crystallinity data are given in the table below.
[0342] (Comparative example A7) Comparative Example A7 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by hydrothermal calcination at atmospheric pressure.
[0343] The process was the same as in Example A3, except that the firing conditions were atmospheric pressure (gauge pressure 0 MPa).
[0344] The obtained comparative sample of Y-type molecular sieve containing rare earth is designated as DAY-7.
[0345] In the chemical composition of DAY-7, the rare earth oxide content was 9.8 wt%.
[0346] The BJH pore size distribution curve and XRD pattern of DAY-7 had similar characteristics to those of DAY-1 and the XRD pattern of PAY-1, respectively.
[0347] In the BJH pore size distribution curve, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of the pore size distribution of 3 to 4 nm was 0.
[0348] As shown in the XRD pattern, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 3.2.
[0349] The unit cell and crystallinity data are given in the table below.
[0350] (Test Example A1) Test Example A1 illustrates the hydrothermal stability test of the rare earth-containing Y-type molecular sieve sample of the present invention.
[0351] The rare earth-containing Y-type molecular sieve samples PAY-1 to PAY-7 of Examples A1 to A7 and the comparative samples DAY-1 to DAY-7 of Comparative Examples D1 to D7 were mixed and exchanged with ammonium chloride solution, respectively, to reduce the Na2O% to less than 0.3 wt%, filtered, and dried to obtain fresh samples.
[0352] The fresh samples were hydrothermally aged at 800°C in a 100% steam environment for 17 h to obtain aged samples.
[0353] The unit cell and crystallinity data for the fresh and aged samples are given in the table below.
[0354] [Table 1]
[0355] The rare earth-containing Y-type molecular sieve of the present invention still has a high degree of crystallinity after hydrothermal aging treatment in 800℃, 100% steam environment for 17 hours. It is clear that the degree of crystallinity is higher than that of the comparative sample. Compared with the steam calcination at atmospheric pressure, the rare earth-containing Y-type molecular sieve after treatment under pressurized steam condition has higher hydrothermal stability, and the hydrothermal stability is obviously improved.
[0356] (Example D1) Example D1 illustrates the preparation of rare earth-containing Y-type molecular sieve of the present invention, which can be used to prepare catalytic cracking catalyst.
[0357] 100g of NaY-type molecular sieve and 1800g of deionized water were mixed and stirred vigorously, and 10g of solid ammonium chloride was added. The resulting mixture was stirred uniformly, the temperature was raised to 70℃, and stirred at a constant temperature for 2.0 hours. After filtering, washing with water, and drying, 20mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L and 2g of solid ammonium chloride were added. The resulting mixture was stirred uniformly, and the temperature was raised to 70℃. The pH value of the slurry was adjusted to 4.5 using dilute hydrochloric acid, and stirred at a constant temperature for 1.0 hour.
[0358] After filtering, washing, and drying, pressure was applied from the outside, water was added, and then pressurized hydrothermal calcination was performed in a 100% steam environment at 500°C, with a gauge pressure of 0.3 MPa, for 2.0 hours to obtain a rare earth-containing Y-type molecular sieve sample, designated PDY-1.
[0359] In the chemical composition of PDY-1, the content of rare earth oxides was 10.1 wt%.
[0360] Figure 4 shows the pore size distribution curve of PDY-1 calculated based on the BJH model. There are at least three types of mesopore size distributions, with three prominent mesopore distributions at the positions of 2-3 nm, 3-4 nm, and 10-30 nm, respectively.
[0361] For PDY-1, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of all pores was 0.25, and the ratio of the peak area of the pore size distribution of 10 to 30 nm to the peak area of all pores was 0.3.
[0362] The XRD pattern of PDY-1 had similar features to that of PAY-1.
[0363] For PDY-1, as shown in the XRD pattern, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 5.8.
[0364] The unit cell and crystallinity data are given in the table below.
[0365] (Comparative Example D1) Comparative Example D1 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by partial ammonium exchange and hydrothermal calcination at atmospheric pressure.
[0366] The process was the same as in Example D1, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0367] The obtained comparative sample of Y-type molecular sieve containing rare earth is designated as DDY-1.
[0368] In the chemical composition of DDY-1, the rare earth oxide content was 10.1 wt%.
[0369] FIG. 5 shows the pore size distribution curve of DDY-1 calculated based on the BJH model calculation.
[0370] As can be seen from the pore size distribution curve, there is mainly one type of mesopore pore size distribution, i.e., there is one type of mesopore pore size distribution at the position of 3–4 nm, but there are no other mesopore pore size distributions at the positions of 2–3 nm and 10–30 nm.
[0371] For DDY-1, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of all pores was 0, and the ratio of the peak area of the pore size distribution of 10 to 30 nm to the peak area of all pores was 0.
[0372] The XRD pattern of DDY-1 had similar features to that of PAY-1.
[0373] For DDY-1, as shown in the XRD pattern, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 3.5.
[0374] The unit cell and crystallinity data are given in the table below.
[0375] (Example D2) Example D2 illustrates the preparation of rare earth-containing Y-type molecular sieve of the present invention, which can be used to prepare catalytic cracking catalyst.
[0376] 100g of NaY-type molecular sieve and 1000g of deionized water were mixed and stirred vigorously, and 5g of solid ammonium sulfate was added. The resulting mixture was stirred uniformly, the temperature was raised to 80°C, and stirred at a constant temperature for 2.0 hours. After filtering, washing with water, and drying, 16mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L and 8g of solid ammonium chloride were added. The resulting mixture was stirred uniformly, and the temperature was raised to 60°C. The pH value of the slurry was adjusted to 4.0 using dilute hydrochloric acid, and stirred at a constant temperature for 1.5 hours.
[0377] After filtering, washing and drying, pressure was applied from the outside, water was added, and then pressurized hydrothermal calcination was performed in an environment of 430°C, gauge pressure 0.8 MPa, and 50% water vapor for 0.5 hours to obtain a Y-type molecular sieve sample containing rare earths, which is designated as PDY-2.
[0378] In the chemical composition of PDY-2, the rare earth oxide content was 8.2 wt%.
[0379] The BJH pore size distribution curve of PDY-2 had similar characteristics to that of PDY-1.
[0380] For PDY-2, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of all pores was 0.12, and the ratio of the peak area of the pore size distribution of 10 to 30 nm to the peak area of all pores was 0.25.
[0381] The XRD pattern of PDY-2 had similar features to that of PAY-1.
[0382] For PDY-2, as shown in the XRD pattern, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 4.4.
[0383] The unit cell and crystallinity data are given in the table below.
[0384] (Comparative example D2) Comparative Example D2 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by partial ammonium exchange and calcination at atmospheric pressure.
[0385] The process was the same as in Example D2, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0386] The obtained comparative sample of rare earth-containing Y-type molecular sieve is designated as DDY-2.
[0387] In the chemical composition of DDY-2, the rare earth oxide content was 8.2 wt%.
[0388] The BJH pore size distribution curve of DDY-2 had similar characteristics to the BJH pore size distribution curve of DDY-1.
[0389] For DDY-2, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of all pores was 0, and the ratio of the peak area of the pore size distribution of 10 to 30 nm to the peak area of all pores was 0.
[0390] The XRD pattern of DDY-2 had similar features to that of PAY-1.
[0391] For DDY-2, as shown in the XRD pattern, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 3.2.
[0392] The unit cell and crystallinity data are given in the table below.
[0393] (Example D3) Example D3 illustrates the preparation of rare earth-containing Y-type molecular sieve of the present invention, which can be used to prepare catalytic cracking catalyst.
[0394] 100g of NaY-type molecular sieve and 2200g of deionized water were mixed and stirred vigorously, and 20g of solid ammonium sulfate was added. The resulting mixture was stirred uniformly, the temperature was raised to 80℃, and stirred at a constant temperature for 1.5 hours. After filtering, washing with water, and drying, 24mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L was added. The resulting mixture was stirred uniformly, and the temperature was raised to 70℃. The pH value of the slurry was adjusted to 3.5 using dilute hydrochloric acid, and stirred at a constant temperature for 1.0 hour.
[0395] After filtering, washing, and drying, pressure was applied from the outside, water was added, and then pressurized hydrothermal calcination was performed in a 100% steam environment at 520°C, a gauge pressure of 0.4 MPa, for 1.5 hours to obtain a rare earth-containing Y-type molecular sieve sample, designated as PDY-3.
[0396] In the chemical composition of PDY-3, the rare earth oxide content was 11.4 wt%.
[0397] The BJH pore size distribution curve of PDY-3 had similar characteristics to that of PDY-1.
[0398] For PDY-3, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of all pores was 0.23, and the ratio of the peak area of the pore size distribution of 10 to 30 nm to the peak area of all pores was 0.25.
[0399] The XRD pattern of PDY-3 had similar features to that of PAY-1.
[0400] For PDY-3, as shown in the XRD pattern, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 5.4.
[0401] The unit cell and crystallinity data are given in the table below.
[0402] (Comparative Example D3) Comparative Example D3 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by partial ammonium exchange and calcination at atmospheric pressure.
[0403] The process was the same as in Example D3, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0404] The obtained comparative sample of Y-type molecular sieve containing rare earth is designated as DDY-3.
[0405] In the chemical composition of DDY-3, the rare earth oxide content was 11.4 wt%.
[0406] The BJH pore size distribution curve of DDY-3 had similar characteristics to the BJH pore size distribution curve of DDY-1.
[0407] For DDY-3, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of all pores was 0, and the ratio of the peak area of the pore size distribution of 10 to 30 nm to the peak area of all pores was 0.
[0408] The XRD pattern of DDY-3 had similar features to that of PAY-1.
[0409] As shown in the XRD pattern of DDY-3, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 4.1.
[0410] The unit cell and crystallinity data are given in the table below.
[0411] (Example D4) Example D4 illustrates the preparation of rare earth-containing Y-type molecular sieve of the present invention, which can be used to prepare catalytic cracking catalyst.
[0412] 100g of NaY-type molecular sieve and 2800g of deionized water were mixed and stirred vigorously, and 50g of solid ammonium chloride was added. The resulting mixture was stirred uniformly, the temperature was raised to 60℃, and stirred at a constant temperature for 2 hours. After filtering, washing with water, and drying, 28mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L was added. The resulting mixture was stirred uniformly, and the temperature was raised to 80℃. The pH value of the slurry was adjusted to 3.8 using dilute hydrochloric acid, and stirred at a constant temperature for 1.0 hour.
[0413] After filtering, washing, and drying, pressure was applied from the outside, water was added, and then pressurized hydrothermal calcination was performed in a 100% steam environment at 580°C, with a gauge pressure of 0.5 MPa, for 2.0 hours to obtain a rare earth-containing Y-type molecular sieve sample, designated PDY-4.
[0414] In the chemical composition of PDY-4, the rare earth oxide content was 12.6 wt%.
[0415] The BJH pore size distribution curve of PDY-4 had similar characteristics to that of PDY-1.
[0416] For PDY-4, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of all pores was 0.23, and the ratio of the peak area of the pore size distribution of 10 to 30 nm to the peak area of all pores was 0.21.
[0417] The XRD pattern of PDY-4 had similar features to that of PAY-1.
[0418] As shown in the XRD pattern of PDY-4, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 5.2.
[0419] The unit cell and crystallinity data are given in the table below.
[0420] (Comparative Example D4) Comparative Example D4 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by partial ammonium exchange and calcination at atmospheric pressure.
[0421] The process was the same as in Example D4, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0422] The obtained comparative sample of rare earth-containing Y-type molecular sieve is designated as DDY-4.
[0423] In the chemical composition of DDY-4, the rare earth oxide content was 12.6 wt%.
[0424] The BJH pore size distribution curve of DDY-4 had similar characteristics to the BJH pore size distribution curve of DDY-1.
[0425] For DDY-4, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of all pores was 0, and the ratio of the peak area of the pore size distribution of 10 to 30 nm to the peak area of all pores was 0.
[0426] The XRD pattern of DDY-4 had similar features to that of PAY-1.
[0427] As shown in the XRD pattern of DDY-4, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 4.2.
[0428] The unit cell and crystallinity data are given in the table below.
[0429] (Example D5) Example D5 illustrates the preparation of rare earth-containing Y-type molecular sieve of the present invention, which can be used to prepare catalytic cracking catalyst.
[0430] 100g of NaY-type molecular sieve and 2000g of deionized water were mixed and stirred vigorously, and 200g of solid ammonium chloride was added. After the resulting mixture was stirred uniformly, the temperature was raised to 60°C and stirred at a constant temperature for 1 hour. After filtering, washing with water and drying, 32mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L was added. The resulting mixture was stirred uniformly, and the temperature was raised to 70°C. The pH value of the slurry was adjusted to 4.0 using dilute hydrochloric acid, and stirred at a constant temperature for 1.0 hour.
[0431] After filtering, washing, and drying, pressure was applied from the outside, water was added, and then pressurized hydrothermal calcination was performed in a 100% steam environment at 550°C, a gauge pressure of 0.4 MPa, for 1.5 hours to obtain a rare earth-containing Y-type molecular sieve sample, designated PDY-5.
[0432] In the chemical composition of PDY-5, the rare earth oxide content was 13.4 wt%.
[0433] The BJH pore size distribution curve of PDY-5 had similar characteristics to that of PDY-1.
[0434] For PDY-5, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of all pores was 0.24, and the ratio of the peak area of the pore size distribution of 10 to 30 nm to the peak area of all pores was 0.29.
[0435] The XRD pattern of PDY-5 had similar features to that of PAY-1.
[0436] As shown in the XRD pattern of PDY-5, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 5.5.
[0437] The unit cell and crystallinity data are given in the table below.
[0438] (Comparative Example D5) Comparative Example D5 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by partial ammonium exchange and calcination at atmospheric pressure.
[0439] The process was the same as in Example D5, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0440] The obtained comparative sample of Y-type molecular sieve containing rare earth is designated as DDY-5.
[0441] In the chemical composition of DDY-5, the rare earth oxide content was 13.4 wt%.
[0442] The BJH pore size distribution curve of DDY-5 had similar characteristics to the BJH pore size distribution curve of DDY-1.
[0443] For DDY-5, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of all pores was 0, and the ratio of the peak area of the pore size distribution of 10 to 30 nm to the peak area of all pores was 0.
[0444] The XRD pattern of DDY-5 had similar features to that of PAY-1.
[0445] As shown in the XRD pattern of DDY-5, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 4.4.
[0446] The unit cell and crystallinity data are given in the table below.
[0447] (Example D6) Example D6 illustrates the preparation of rare earth-containing Y-type molecular sieve of the present invention, which can be used to prepare catalytic cracking catalyst.
[0448] 100g of NaY-type molecular sieve and 1800g of deionized water were mixed and stirred vigorously, and 50g of solid ammonium sulfate was added. The resulting mixture was stirred uniformly, the temperature was raised to 70℃, and stirred at a constant temperature for 2.0 hours. After filtering, washing with water, and drying, 20mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L and 2g of solid ammonium sulfate were added. The resulting mixture was stirred uniformly, and the temperature was raised to 70℃. The pH value of the slurry was adjusted to 4.5 using dilute hydrochloric acid, and stirred at a constant temperature for 1.0 hour.
[0449] After filtering, washing, and drying, pressure was applied from the outside, water was added, and then pressure hydrothermal calcination was performed in a 100% steam environment at 430°C, with a gauge pressure of 0.6 MPa for 2.0 hours to obtain a rare earth-containing Y-type molecular sieve sample, designated PDY-6.
[0450] In the chemical composition of PDY-6, the content of rare earth oxides was 10.0 wt%.
[0451] The BJH pore size distribution curve of PDY-6 had similar characteristics to that of PDY-1.
[0452] For PDY-6, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of all pores was 0.18, and the ratio of the peak area of the pore size distribution of 10 to 30 nm to the peak area of all pores was 0.22.
[0453] The XRD pattern of PDY-6 had similar features to that of PAY-1.
[0454] As shown in the XRD pattern of PDY-6, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 4.9.
[0455] The unit cell and crystallinity data are given in the table below.
[0456] (Comparative Example D6) Comparative Example D6 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by partial ammonium exchange and calcination at atmospheric pressure.
[0457] The process was the same as in Example D6, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0458] The obtained comparative sample of Y-type molecular sieve containing rare earth is designated as DDY-6.
[0459] In the chemical composition of DDY-6, the rare earth oxide content was 10.0 wt%.
[0460] The BJH pore size distribution curve of DDY-6 had similar characteristics to the BJH pore size distribution curve of DDY-1.
[0461] For DDY-6, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of all pores was 0, and the ratio of the peak area of the pore size distribution of 10 to 30 nm to the peak area of all pores was 0.
[0462] The XRD pattern of DDY-6 had similar features to that of PAY-1.
[0463] As shown in the XRD pattern of DDY-6, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 2.8.
[0464] The unit cell and crystallinity data are given in the table below.
[0465] (Example D7) Example D7 illustrates the preparation of rare earth-containing Y-type molecular sieve of the present invention, which can be used to prepare catalytic cracking catalyst.
[0466] 100g of NaY-type molecular sieve and 1800g of deionized water were mixed and stirred vigorously, and 20g of solid ammonium sulfate was added. The resulting mixture was stirred uniformly, the temperature was raised to 80°C, and stirred at a constant temperature for 2.0 hours. After filtering, washing with water, and drying, 20mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L and 2g of solid ammonium sulfate were added. The resulting mixture was stirred uniformly, and the temperature was raised to 70°C. The pH value of the slurry was adjusted to 4.5 using dilute hydrochloric acid, and stirred at a constant temperature for 1.0 hour.
[0467] After filtering, washing, and drying, pressure was applied from the outside, water was added, and then pressurized hydrothermal calcination was performed in a 100% steam environment at 400°C, with a gauge pressure of 0.8 MPa, for 2.0 hours to obtain a rare earth-containing Y-type molecular sieve sample, designated PDY-7.
[0468] In the chemical composition of PDY-7, the rare earth oxide content was 9.8 wt%.
[0469] The BJH pore size distribution curve of PDY-7 had similar characteristics to that of PDY-1.
[0470] For PDY-7, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of all pores was 0.13, and the ratio of the peak area of the pore size distribution of 10 to 30 nm to the peak area of all pores was 0.21.
[0471] The XRD pattern of PDY-7 had similar features to that of PAY-1.
[0472] As shown in the XRD pattern of PDY-7, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 4.4.
[0473] The unit cell and crystallinity data are given in the table below.
[0474] (Comparative example D7) Comparative Example D7 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by partial ammonium exchange and calcination at atmospheric pressure.
[0475] The process was the same as in Example D7, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0476] The obtained comparative sample of Y-type molecular sieve containing rare earth is designated as DDY-7.
[0477] In the chemical composition of DDY-7, the rare earth oxide content was 9.8 wt%.
[0478] The BJH pore size distribution curve of DDY-7 had similar characteristics to the BJH pore size distribution curve of DDY-1.
[0479] For DDY-7, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of all pores was 0, and the ratio of the peak area of the pore size distribution of 10 to 30 nm to the peak area of all pores was 0.
[0480] The XRD pattern of DDY-7 had similar features to that of PAY-1.
[0481] As shown in the XRD pattern of DDY-7, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 3.4.
[0482] The unit cell and crystallinity data are given in the table below.
[0483] (Test Example D1) Test Example D1 illustrates the hydrothermal stability test of the rare earth-containing Y-type molecular sieve sample of the present invention.
[0484] The rare earth-containing Y-type molecular sieve samples PDY-1 to PDY-7 of Examples D1 to D7 and the comparative samples DDY-1 to DDY-7 of Comparative Examples D1 to D7 were mixed and exchanged with ammonium chloride solution, respectively, to reduce the Na2O% to less than 0.3 wt%, and then filtered and dried to obtain fresh samples.
[0485] The fresh samples were hydrothermally aged at 800°C in a 100% steam environment for 17 h to obtain aged samples.
[0486] The unit cell and crystallinity data for the fresh and aged samples are given in the table below.
[0487] [Table 2]
[0488] As can be seen from the table, the rare earth-containing Y-type molecular sieve samples PDY-1 to PDY-7 still had high crystallinity after being hydrothermal aged at 800°C in a 100% steam environment for 17 hours. It is clear that the crystallinity of each of the samples PDY-1 to PDY-7 is higher than that of the comparative sample. Compared with hydrothermal calcination at atmospheric pressure, the rare earth-containing Y-type molecular sieve obtained by hydrothermal treatment under the environmental conditions of the present invention has higher hydrothermal stability, and the hydrothermal stability is obviously improved.
[0489] (Example B1) Example B1 illustrates the rare earth-containing Y-type molecular sieve obtained by the third method.
[0490] 100g of NaY-type molecular sieve and 1800g of deionized water were mixed and stirred vigorously, and 20mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L and 2g of solid ammonium chloride were added. The mixture was stirred uniformly and the temperature was raised to 70°C. The pH value of the slurry was adjusted to 4.5 using dilute hydrochloric acid and stirred at a constant temperature for 1.0 hour.
[0491] After filtering, washing, and drying, 7 g of ammonia water was added under external pressure, and then pressurized hydrothermal calcination was performed for 2.0 hours in a 100% steam environment at 500°C and a gauge pressure of 0.3 MPa to obtain a rare earth-containing Y-type molecular sieve sample, designated PBY-1.
[0492] In the chemical composition of PBY-1, the rare earth oxide content was 10.1 wt%.
[0493] Curve a in Figure 6 is the pore size distribution curve of PBY-1 calculated based on the BJH model calculation. As can be seen from curve a, there are at least two types of mesopore pore size distributions, one type of mesopore pore size distribution at the 2-3 nm position and another type of mesopore pore size distribution at the 3-4 nm position.
[0494] Curve c in Figure 7 is the adsorption / desorption curve of sample PBY-1. As can be seen from curve c, there is a hysteresis loop with a large area, which indicates that sample PBY-1 has a rich mesopore structure.
[0495] The XRD pattern of PBY-1 had similar features to that of PAY-1, indicating that the PBY-1 molecular sieve had a pure FAU crystal structure and no impure crystals were formed. The XRD characteristic parameters and pore parameters are shown in the table below.
[0496] (Comparative Example B1.1) Comparative Example B1.1 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by hydrothermal calcination at atmospheric pressure without adding ammonia water.
[0497] The process was the same as in Example B1, except that the calcination conditions were atmospheric pressure (gauge pressure: 0 MPa) and no ammonia water was added.
[0498] The obtained comparative sample of rare earth-containing Y-type molecular sieve is designated as DBY-1.1.
[0499] In the chemical composition of DBY-1.1, the rare earth oxide content was 10.1 wt%.
[0500] The curve b in Fig. 6 is the pore size distribution curve of the comparative sample DBY-1.1 calculated based on the BJH model calculation. There is mainly one type of mesopore pore size distribution, that is, there is one type of mesopore pore size distribution at the position of 3 to 4 nm, but there is no other mesopore pore size distribution at the position of 2 to 3 nm.
[0501] 7 is the adsorption / desorption curve of the comparative sample DBY-1.1. The area of the hysteresis loop is small, which indicates that the volume of the mesopores is relatively small.
[0502] The XRD pattern of DBY-1.1 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0503] (Comparative Example B1.2) Comparative Example B1.2 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by adding ammonia water and hydrothermal calcination at atmospheric pressure.
[0504] The process was the same as in Example B1, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0505] The obtained comparative sample of rare earth-containing Y-type molecular sieve is designated as DBY-1.2.
[0506] In the chemical composition of DBY-1.2, the rare earth oxide content was 10.1 wt%.
[0507] The pore size distribution curve of DBY-1.2 calculated based on the BJH model calculation had the same characteristics as the curve b in FIG. 6, and the adsorption / desorption curve had the same characteristics as the curve d in FIG.
[0508] The XRD pattern of DBY-1.2 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0509] (Example C1) Example C1 illustrates the rare earth-containing Y-type molecular sieve obtained by the fourth method.
[0510] 100g of NaY-type molecular sieve and 1800g of deionized water were mixed and stirred vigorously, and 20mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L and 2g of solid ammonium chloride were added. The mixture was stirred uniformly and the temperature was raised to 70°C. The pH value of the slurry was adjusted to 4.5 using dilute hydrochloric acid and stirred at a constant temperature for 1.0 hour.
[0511] After filtering, washing and drying, 7g of ammonia water was added by impregnation, and the mixture was dried. Then, the mixture was subjected to pressurized hydrothermal calcination treatment at 500℃, gauge pressure of 0.3MPa, and 100% steam for 2.0 hours to obtain a rare earth-containing Y-type molecular sieve sample, which is designated as PCY-1.
[0512] In the chemical composition of PCY-1, the content of rare earth oxides was 10.1 wt%.
[0513] Curve A in Figure 6 is the pore size distribution curve of sample PCY-1 calculated based on the BJH model calculation. As can be seen from curve A, there are at least two types of mesopore pore size distributions, located at 2 to 3 nm and 3 to 4 nm, respectively.
[0514] Curve C in Fig. 7 is the adsorption / desorption curve of sample PCY-1. As can be seen from curve C, the adsorption / desorption curve of sample PCY-1 has a hysteresis loop with a large area, which indicates that sample PCY-1 has a rich mesopore structure.
[0515] The XRD pattern of sample PCY-1 had similar features to that of PAY-1. It is evident that the PCY-1 molecular sieve has a pure FAU crystal structure and no impure crystals are formed. The XRD characteristic parameters and pore parameters are shown in the table below.
[0516] (Comparative Example C1) Comparative Example C1 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by impregnating with ammonia water and hydrothermal calcining at atmospheric pressure.
[0517] The process was the same as in Example C1, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0518] The obtained comparative sample of rare earth-containing Y-type molecular sieve is designated as DCY-1.
[0519] In the chemical composition of DCY-1, the content of rare earth oxides was 10.1 wt%.
[0520] The pore size distribution curve of DCY-1 calculated based on the BJH model calculation had the same characteristics as the curve b in FIG. 6, and the adsorption / desorption curve had the same characteristics as the curve d in FIG.
[0521] The XRD pattern of DCY-1 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0522] (Example B2) Example B2 illustrates the rare earth-containing Y-type molecular sieve obtained by the third method.
[0523] 100g of NaY-type molecular sieve and 1000g of deionized water were mixed and stirred vigorously, and 16mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L and 8g of solid ammonium chloride were added. The mixture was stirred uniformly and the temperature was raised to 60°C. The pH value of the slurry was adjusted to 4.0 using dilute hydrochloric acid, and stirred at a constant temperature for 1.5 hours.
[0524] After filtering, washing, and drying, an aqueous solution of ammonium chloride containing 10 g of ammonium chloride was added under external pressure, and then pressurized hydrothermal calcination was performed at 430°C, a gauge pressure of 0.8 MPa, and an environment of 100% water vapor for 0.5 hours to obtain a Y-type molecular sieve sample containing rare earths, which is designated as PBY-2.
[0525] In the chemical composition of PBY-2, the rare earth oxide content was 8.2 wt%.
[0526] The characteristics of the pore size distribution curve of PBY-2 calculated based on the BJH model calculation were identical to the curve a in FIG. 6, and the characteristics of the adsorption / desorption curve were identical to the curve c in FIG.
[0527] The XRD pattern of PBY-2 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0528] (Comparative example B2.1) Comparative Example B2.1 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by hydrothermal calcination at atmospheric pressure without adding ammonium chloride.
[0529] The process was the same as in Example B2, except that the calcination conditions were atmospheric pressure (gauge pressure: 0 MPa) and no ammonium chloride was added.
[0530] The obtained comparative sample of rare earth-containing Y-type molecular sieve is designated as DBY-2.1.
[0531] In the chemical composition of DBY-2.1, the rare earth oxide content was 8.2 wt%.
[0532] The pore size distribution curve of DBY-2.1 calculated based on the BJH model calculation had the same characteristics as the curve b in FIG. 6, and the adsorption / desorption curve had the same characteristics as the curve d in FIG.
[0533] The XRD pattern of DBY-2.1 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0534] (Comparative example B2.2) Comparative Example B2.2 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by adding ammonium chloride and hydrothermal calcination at atmospheric pressure.
[0535] The process was the same as in Example B2, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0536] The obtained comparative sample of rare earth-containing Y-type molecular sieve is designated as DBY-2.2.
[0537] In the chemical composition of DBY-2.2, the rare earth oxide content was 8.2 wt%.
[0538] The pore size distribution curve of DBY-2.2 calculated based on the BJH model calculation had the same characteristics as the curve b in FIG. 6, and the adsorption / desorption curve had the same characteristics as the curve d in FIG.
[0539] The XRD pattern of DBY-2.2 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0540] (Example C2) Example C2 illustrates the rare earth-containing Y-type molecular sieve obtained by the fourth method.
[0541] 100g of NaY-type molecular sieve and 1000g of deionized water were mixed and stirred vigorously, and 16mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L and 8g of solid ammonium chloride were added. The mixture was stirred uniformly and the temperature was raised to 60°C. The pH value of the slurry was adjusted to 4.0 using dilute hydrochloric acid, and stirred at a constant temperature for 1.5 hours.
[0542] After filtering, washing and drying, 7g of ammonium chloride was filled by impregnation, dried and then subjected to pressurized hydrothermal calcination treatment at 430℃, gauge pressure of 0.8MPa, and 100% steam environment for 0.5 hours to obtain a rare earth-containing Y-type molecular sieve sample, designated as PCY-2.
[0543] In the chemical composition of PCY-2, the rare earth oxide content was 8.2 wt%.
[0544] The pore size distribution curve of PCY-2 calculated based on the BJH model calculation had the same characteristics as curve A in FIG. 6, and the adsorption / desorption curve had the same characteristics as curve C in FIG.
[0545] The XRD pattern of PCY-2 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0546] (Comparative Example C2) Comparative Example C2 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by loading ammonium chloride by impregnation and performing hydrothermal calcination at atmospheric pressure.
[0547] The process was the same as in Example C2, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0548] The obtained comparative sample of rare earth-containing Y-type molecular sieve is designated as DCY-2.
[0549] In the chemical composition of DCY-2, the rare earth oxide content was 8.2 wt%.
[0550] The pore size distribution curve of DCY-2 calculated based on the BJH model calculation had the same characteristics as the curve b in FIG. 6, and the adsorption / desorption curve had the same characteristics as the curve d in FIG.
[0551] The XRD pattern of DCY-2 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0552] (Example B3) Example B3 illustrates the rare earth-containing Y-type molecular sieve obtained by the third method.
[0553] 100g of NaY-type molecular sieve and 2200g of deionized water were mixed and stirred vigorously, and 24mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L was added. The mixture was stirred uniformly and the temperature was raised to 70℃. The pH value of the slurry was adjusted to 3.5 with dilute hydrochloric acid, and stirred at a constant temperature for 1.0 hour.
[0554] After filtering, washing, and drying, an aqueous solution containing 6% by weight of ammonium bicarbonate was added, and then pressurized hydrothermal calcination was performed at 520°C, a gauge pressure of 0.4 MPa, and an environment of 100% water vapor for 1.5 hours to obtain a sample of Y-type molecular sieve containing rare earths, which is designated as PBY-3.
[0555] In the chemical composition of PBY-3, the rare earth oxide content was 11.4 wt%.
[0556] The characteristics of the pore size distribution curve of PBY-3 calculated based on the BJH model calculation were identical to the curve a in FIG. 6, and the characteristics of the adsorption / desorption curve were identical to the curve c in FIG.
[0557] The XRD pattern of PBY-3 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0558] (Comparative Example B3.1) Comparative Example B3.1 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by hydrothermal calcination at atmospheric pressure without adding ammonium bicarbonate.
[0559] The process was the same as in Example B3, except that the calcination conditions were atmospheric pressure (gauge pressure: 0 MPa) and no ammonium bicarbonate was added.
[0560] The obtained comparative sample of rare earth-containing Y-type molecular sieve is designated as DBY-3.1.
[0561] In the chemical composition of DBY-3.1, the rare earth oxide content was 11.4 wt%.
[0562] The pore size distribution curve of DBY-3.1 calculated based on the BJH model calculation had the same characteristics as the curve b in FIG. 6, and the adsorption / desorption curve had the same characteristics as the curve d in FIG.
[0563] The XRD pattern of DBY-3.1 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0564] (Comparative Example B3.2) Comparative Example B3.2 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by hydrothermal calcination at atmospheric pressure without adding ammonium bicarbonate.
[0565] The process was the same as in Example B3, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0566] The obtained rare earth-containing Y-type molecular sieve is referred to as DBY-3.2.
[0567] In the chemical composition of DBY-3.2, the rare earth oxide content was 11.4 wt%.
[0568] The pore size distribution curve of DBY-3.2 calculated based on the BJH model calculation had the same characteristics as the curve b in FIG. 6, and the adsorption / desorption curve had the same characteristics as the curve d in FIG.
[0569] The XRD pattern of DBY-3.2 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0570] (Example C3) Example C3 illustrates the rare earth-containing Y-type molecular sieve obtained by the fourth method.
[0571] 100g of NaY-type molecular sieve and 2200g of deionized water were mixed and stirred vigorously, and 24mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L was added. The mixture was stirred uniformly and the temperature was raised to 70℃. The pH value of the slurry was adjusted to 3.5 with dilute hydrochloric acid, and stirred at a constant temperature for 1.0 hour.
[0572] After filtering, washing and drying, 12g of ammonium bicarbonate was filled by impregnation, dried, and then pressurized hydrothermal calcination was performed at 520℃, 0.4MPa gauge pressure, and 100% steam environment for 1.5 hours to obtain a rare earth-containing Y-type molecular sieve sample, designated as PCY-3.
[0573] In the chemical composition of PCY-3, the content of rare earth oxides was 11.4 wt%.
[0574] The pore size distribution curve of PCY-3 calculated based on the BJH model calculation had the same characteristics as curve A in FIG. 6, and the adsorption / desorption curve had the same characteristics as curve C in FIG.
[0575] The XRD pattern of PCY-3 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0576] (Comparative Example C3) Comparative Example C3 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by loading ammonium bicarbonate by impregnation and performing hydrothermal calcination at atmospheric pressure.
[0577] The process was the same as in Example C3, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0578] The obtained comparative sample of rare earth-containing Y-type molecular sieve is designated as DCY-3.
[0579] In the chemical composition of DCY-3, the rare earth oxide content was 11.4 wt%.
[0580] The pore size distribution curve of DCY-3 calculated based on the BJH model calculation had the same characteristics as the curve b in FIG. 6, and the adsorption / desorption curve had the same characteristics as the curve d in FIG.
[0581] The XRD pattern of DCY-3 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0582] (Example B4) Example B4 illustrates the rare earth-containing Y-type molecular sieve obtained by the third method.
[0583] 100g of NaY-type molecular sieve and 2800g of deionized water were mixed and stirred vigorously, and 28mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L was added. The mixture was stirred uniformly and the temperature was raised to 80℃. The pH value of the slurry was adjusted to 3.8 with dilute hydrochloric acid, and stirred at a constant temperature for 1.0 hour.
[0584] After filtering, washing, and drying, an aqueous solution containing 9% by weight of sodium carbonate was added, and then pressurized hydrothermal calcination was performed at 580°C, a gauge pressure of 0.5 MPa, and an environment of 100% water vapor for 2.0 hours to obtain a sample of Y-type molecular sieve containing rare earths, which is designated as PBY-4.
[0585] In the chemical composition of PBY-4, the rare earth oxide content was 12.6 wt%.
[0586] The characteristics of the pore size distribution curve of PBY-4 calculated based on the BJH model calculation were identical to the curve a in FIG. 6, and the characteristics of the adsorption / desorption curve were identical to the curve c in FIG.
[0587] The XRD pattern of PBY-4 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0588] (Comparative example B4.1) Comparative Example B4.1 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by hydrothermal calcination at atmospheric pressure without adding sodium carbonate.
[0589] The process was the same as in Example B4, except that the calcination conditions were atmospheric pressure (gauge pressure: 0 MPa) and no sodium carbonate was added.
[0590] The obtained comparative sample of rare earth-containing Y-type molecular sieve is designated as DBY-4.1.
[0591] In the chemical composition of DBY-4.1, the rare earth oxide content was 12.6 wt%.
[0592] The pore size distribution curve of DBY-4.1 calculated based on the BJH model calculation had the same characteristics as the curve b in FIG. 6, and the adsorption / desorption curve had the same characteristics as the curve d in FIG.
[0593] The XRD pattern of DBY-4.1 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0594] (Comparative example B4.2) Comparative Example B4.2 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by adding sodium carbonate and performing hydrothermal calcination at atmospheric pressure.
[0595] The process was the same as in Example B4, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0596] The obtained rare earth-containing Y-type molecular sieve is referred to as DBY-4.2.
[0597] In the chemical composition of DBY-4.2, the rare earth oxide content was 12.6 wt%.
[0598] The pore size distribution curve of DBY-4.2 calculated based on the BJH model calculation had the same characteristics as the curve b in FIG. 6, and the adsorption / desorption curve had the same characteristics as the curve d in FIG.
[0599] The XRD pattern of DBY-4.2 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0600] (Example C4) Example C4 illustrates the rare earth-containing Y-type molecular sieve obtained by the fourth method.
[0601] 100g of NaY-type molecular sieve and 2800g of deionized water were mixed and stirred vigorously, and 28mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L was added. The mixture was stirred uniformly and the temperature was raised to 80℃. The pH value of the slurry was adjusted to 3.8 with dilute hydrochloric acid, and stirred at a constant temperature for 1.0 hour.
[0602] After filtering, washing and drying, 9g of sodium carbonate was filled by impregnation, dried and then pressurized hydrothermal calcination was performed at 580℃, gauge pressure 0.5MPa, and 100% steam environment for 2.0 hours to obtain a rare earth-containing Y-type molecular sieve sample, which is designated as PCY-4.
[0603] In the chemical composition of PCY-4, the rare earth oxide content was 12.6 wt%.
[0604] The pore size distribution curve of PCY-4 calculated based on the BJH model calculation had the same characteristics as curve A in FIG. 6, and the adsorption / desorption curve had the same characteristics as curve C in FIG.
[0605] The XRD pattern of PCY-4 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0606] (Comparative example C4) Comparative Example C4 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by loading sodium carbonate by impregnation and performing hydrothermal calcination at atmospheric pressure.
[0607] The process was the same as in Example C4, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0608] The obtained comparative sample of rare earth-containing Y-type molecular sieve is designated as DCY-4.
[0609] In the chemical composition of DCY-4, the rare earth oxide content was 12.6 wt%.
[0610] The pore size distribution curve of DCY-4 calculated based on the BJH model calculation had the same characteristics as the curve b in FIG. 6, and the adsorption / desorption curve had the same characteristics as the curve d in FIG.
[0611] The XRD pattern of DCY-4 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0612] (Example B5) Example B5 illustrates the rare earth-containing Y-type molecular sieve obtained by the third method.
[0613] 100g of NaY-type molecular sieve and 2000g of deionized water were mixed and stirred vigorously, and 32mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L was added. The mixture was stirred uniformly and the temperature was raised to 70℃. The pH value of the slurry was adjusted to 4.0 with dilute hydrochloric acid, and stirred at a constant temperature for 1.0 hour.
[0614] After filtering, washing, and drying, a buffer solution of ammonium chloride and aqueous ammonia containing 10 g of ammonium chloride was added, and then pressurized hydrothermal calcination treatment was performed at 550°C, a gauge pressure of 0.4 MPa, and an environment of 100% water vapor for 1.5 hours to obtain a sample of Y-type molecular sieve containing rare earths, which is designated as PBY-5-1.
[0615] In the chemical composition of PBY-5, the rare earth oxide content was 13.4% by weight.
[0616] The characteristics of the pore size distribution curve of PBY-5 calculated based on the BJH model calculation were identical to the curve a in FIG. 6, and the characteristics of the adsorption / desorption curve were identical to the curve c in FIG.
[0617] The XRD pattern of PBY-5 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0618] (Comparative Example B5.1) Comparative Example B5.1 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by hydrothermal calcination at atmospheric pressure without adding a buffer solution of ammonium chloride and aqueous ammonia.
[0619] The process was the same as in Example B5, except that the calcination conditions were atmospheric pressure (gauge pressure: 0 MPa) and the buffer solution of ammonium chloride and aqueous ammonia was not added.
[0620] The obtained comparative sample of rare earth-containing Y-type molecular sieve is designated as DBY-5.1.
[0621] In the chemical composition of DBY-5.1, the rare earth oxide content was 13.4 wt%.
[0622] The pore size distribution curve of DBY-5.1 calculated based on the BJH model calculation had the same characteristics as the curve b in FIG. 6, and the adsorption / desorption curve had the same characteristics as the curve d in FIG.
[0623] The XRD pattern of DBY-5.1 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0624] (Comparative Example B5.2) Comparative Example B5.2 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by hydrothermal calcination at atmospheric pressure without adding a buffer solution of ammonium chloride and aqueous ammonia.
[0625] The process was the same as in Example B5, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0626] The obtained rare earth-containing Y-type molecular sieve is referred to as DBY-5.2.
[0627] In the chemical composition of DBY-5.2, the rare earth oxide content was 13.4 wt%.
[0628] The pore size distribution curve of DBY-5.2 calculated based on the BJH model calculation had the same characteristics as the curve b in FIG. 6, and the adsorption / desorption curve had the same characteristics as the curve d in FIG.
[0629] The XRD pattern of DBY-5.2 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0630] (Example C5) Example C5 illustrates the rare earth-containing Y-type molecular sieve obtained by the fourth method.
[0631] 100g of NaY-type molecular sieve and 2000g of deionized water were mixed and stirred vigorously, and 32mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L was added. The mixture was stirred uniformly and the temperature was raised to 70℃. The pH value of the slurry was adjusted to 4.0 with dilute hydrochloric acid, and stirred at a constant temperature for 1.0 hour.
[0632] After filtering, washing and drying, the sample was impregnated with 10 g of a buffer solution of ammonium chloride and aqueous ammonia, dried and then subjected to a pressurized hydrothermal calcination treatment at 550°C, a gauge pressure of 0.4 MPa and a 100% steam environment for 1.5 hours to obtain a rare earth-containing Y-type molecular sieve sample, designated PCY-5.
[0633] In the chemical composition of PCY-5, the rare earth oxide content was 13.4 wt%.
[0634] The pore size distribution curve of PCY-5 calculated based on the BJH model calculation had the same characteristics as curve A in FIG. 6, and the adsorption / desorption curve had the same characteristics as curve C in FIG.
[0635] The XRD pattern of PCY-5 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0636] (Comparative example C5) Comparative Example C5 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by impregnation with a buffer solution of ammonium chloride and aqueous ammonia, followed by hydrothermal calcination at atmospheric pressure.
[0637] The process was the same as in Example C5, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0638] The obtained comparative sample of rare earth-containing Y-type molecular sieve is designated as DCY-5.
[0639] In the chemical composition of DCY-5, the content of rare earth oxides was 13.4 wt%.
[0640] The pore size distribution curve of DCY-5 calculated based on the BJH model calculation had the same characteristics as the curve b in FIG. 6, and the adsorption / desorption curve had the same characteristics as the curve d in FIG.
[0641] The XRD pattern of DCY-5 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0642] (Example B6) Example B6 illustrates the rare earth-containing Y-type molecular sieve obtained by the third method.
[0643] 100g of NaY-type molecular sieve and 1800g of deionized water were mixed and stirred vigorously, and 20mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L and 2g of solid ammonium chloride were added. The mixture was stirred uniformly and the temperature was raised to 70°C. The pH value of the slurry was adjusted to 4.5 using dilute hydrochloric acid and stirred at a constant temperature for 1.0 hour.
[0644] After filtering, washing, and drying, an aqueous hydrochloric acid solution (6% by weight) was added, and then pressurized hydrothermal calcination treatment was performed at 430°C, a gauge pressure of 0.6 MPa, and an environment of 100% water vapor for 2.0 hours to obtain a sample of Y-type molecular sieve containing rare earths, which is designated as PBY-6.
[0645] In the chemical composition of PBY-6, the rare earth oxide content was 10.0 wt%.
[0646] The characteristics of the pore size distribution curve of PBY-6 calculated based on the BJH model calculation were identical to the curve a in FIG. 6, and the characteristics of the adsorption / desorption curve were identical to the curve c in FIG.
[0647] The XRD pattern of PBY-6 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0648] (Comparative example B6.1) Comparative Example B6.1 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by hydrothermal calcination at atmospheric pressure without adding hydrochloric acid.
[0649] The process was the same as in Example B6, except that the calcination conditions were atmospheric pressure (gauge pressure: 0 MPa) and no hydrochloric acid was added.
[0650] The obtained comparative sample of rare earth-containing Y-type molecular sieve is designated as DBY-6.1.
[0651] In the chemical composition of DBY-6.1, the rare earth oxide content was 10.0 wt%.
[0652] The pore size distribution curve of DBY-6.1 calculated based on the BJH model calculation had the same characteristics as the curve b in FIG. 6, and the adsorption / desorption curve had the same characteristics as the curve d in FIG.
[0653] The XRD pattern of DBY-6.1 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0654] (Comparative example B6.2) Comparative Example B6.2 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by adding hydrochloric acid and performing hydrothermal calcination at atmospheric pressure.
[0655] The process was the same as in Example B6, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0656] The obtained comparative sample of rare earth-containing Y-type molecular sieve is designated as DBY-6.2.
[0657] In the chemical composition of DBY-6.2, the rare earth oxide content was 10.0 wt%.
[0658] The pore size distribution curve of DBY-6.2 calculated based on the BJH model calculation had the same characteristics as the curve b in FIG. 6, and the adsorption / desorption curve had the same characteristics as the curve d in FIG.
[0659] The XRD pattern of DBY-6.2 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0660] (Example C6) Example C6 illustrates the rare earth-containing Y-type molecular sieve obtained by the fourth method.
[0661] 100g of NaY-type molecular sieve and 1800g of deionized water were mixed and stirred vigorously, and 20mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L and 2g of solid ammonium chloride were added. After the mixture was stirred uniformly, the temperature was raised to 70°C. The pH value of the slurry was adjusted to 4.5 using dilute hydrochloric acid, and stirred at a constant temperature for 1.0 hour.
[0662] After filtering, washing and drying, the sample was filled with 2g of hydrochloric acid solution by impregnation, dried, and then subjected to pressurized hydrothermal calcination treatment at 430℃, gauge pressure of 0.6MPa, and 100% steam environment for 2.0 hours to obtain a rare earth-containing Y-type molecular sieve sample, designated as PCY-6.
[0663] In the chemical composition of PCY-6, the content of rare earth oxides was 10.0 wt%.
[0664] The pore size distribution curve of PCY-6 calculated based on the BJH model calculation had the same characteristics as curve A in FIG. 6, and the adsorption / desorption curve had the same characteristics as curve C in FIG.
[0665] The XRD pattern of PCY-6 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0666] (Comparative example C6) Comparative Example C6 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by impregnation with hydrochloric acid and hydrothermal calcination at atmospheric pressure.
[0667] The process was the same as in Example C6, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0668] The obtained comparative sample of rare earth-containing Y-type molecular sieve is designated as DCY-6.
[0669] In the chemical composition of DCY-6, the content of rare earth oxides was 10.0 wt%.
[0670] The pore size distribution curve of DCY-6 calculated based on the BJH model calculation had the same characteristics as the curve b in FIG. 6, and the adsorption / desorption curve had the same characteristics as the curve d in FIG.
[0671] The XRD pattern of DCY-6 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0672] (Example B7) Example B7 illustrates the rare earth-containing Y-type molecular sieve obtained by the third method.
[0673] 100g of NaY-type molecular sieve and 1800g of deionized water were mixed and stirred vigorously, and 20mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L and 2g of solid ammonium chloride were added. The mixture was stirred uniformly and the temperature was raised to 70°C. The pH value of the slurry was adjusted to 4.5 using dilute hydrochloric acid and stirred at a constant temperature for 1.0 hour.
[0674] After filtering, washing, and drying, an aqueous sodium hydroxide solution (6% by weight) was added, and then pressurized hydrothermal calcination was performed at 400°C, a gauge pressure of 0.8 MPa, and an environment of 100% water vapor for 2.0 hours to obtain a sample of Y-type molecular sieve containing rare earths, which is designated as PBY-7.
[0675] In the chemical composition of PBY-7, the rare earth oxide content was 9.8% by weight.
[0676] The characteristics of the pore size distribution curve of PBY-7 calculated based on the BJH model calculation were identical to the curve a in FIG. 6, and the characteristics of the adsorption / desorption curve were identical to the curve c in FIG.
[0677] The XRD pattern of PBY-7 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0678] (Comparative Example B7.1) Comparative Example B7.1 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by hydrothermal calcination at atmospheric pressure without adding solid sodium hydroxide.
[0679] The procedure was the same as in Example B7, except that the calcination conditions were atmospheric pressure (gauge pressure: 0 MPa) and no solid sodium hydroxide was added.
[0680] The obtained comparative sample of rare earth-containing Y-type molecular sieve is designated as DBY-7.1.
[0681] In the chemical composition of DBY-7.1, the rare earth oxide content was 9.8 wt%.
[0682] The pore size distribution curve of DBY-7.1 calculated based on the BJH model calculation had the same characteristics as the curve b in FIG. 6, and the adsorption / desorption curve had the same characteristics as the curve d in FIG.
[0683] The XRD pattern of DBY-7.1 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0684] (Comparative Example B7.2) Comparative Example B7.2 is a comparative sample of rare earth-containing Y-type molecular sieve obtained by adding solid sodium hydroxide and carrying out hydrothermal calcination at atmospheric pressure.
[0685] The process was the same as in Example B7, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0686] The obtained comparative sample of rare earth-containing Y-type molecular sieve is designated as DBY-7.2.
[0687] In the chemical composition of DBY-7.2, the rare earth oxide content was 11.4 wt%.
[0688] The pore size distribution curve of DBY-7.2 calculated based on the BJH model calculation had the same characteristics as the curve b in FIG. 6, and the adsorption / desorption curve had the same characteristics as the curve d in FIG.
[0689] The XRD pattern of DBY-7.2 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0690] (Example C7) Example C7 illustrates the rare earth-containing Y-type molecular sieve obtained by the fourth method.
[0691] 100g of NaY-type molecular sieve and 1800g of deionized water were mixed and stirred vigorously, and 20mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L and 2g of solid ammonium chloride were added. After the mixture was stirred uniformly, the temperature was raised to 70°C. The pH value of the slurry was adjusted to 4.5 using dilute hydrochloric acid, and stirred at a constant temperature for 1.0 hour.
[0692] After filtering, washing and drying, 3g of solid sodium hydroxide was filled by impregnation, dried, and then pressurized hydrothermal calcination treatment was performed at 400℃, gauge pressure 0.8MPa, and 100% steam environment for 2.0 hours to obtain a rare earth-containing Y-type molecular sieve sample, which is designated as PCY-7.
[0693] In the chemical composition of PCY-7, the rare earth oxide content was 9.8 wt%.
[0694] The pore size distribution curve of PCY-7 calculated based on the BJH model calculation had the same characteristics as curve A in FIG. 6, and the adsorption / desorption curve had the same characteristics as curve C in FIG.
[0695] The XRD pattern of PCY-7 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0696] (Comparative Example C7) Comparative Example C7 illustrates a comparative sample of rare earth-containing Y-type molecular sieve obtained by loading sodium hydroxide by impregnation and performing hydrothermal calcination at atmospheric pressure.
[0697] The process was the same as in Example C7, except that the firing conditions were atmospheric pressure (gauge pressure: 0 MPa).
[0698] The obtained comparative sample of rare earth-containing Y-type molecular sieve is designated as DCY-7.
[0699] In the chemical composition of DCY-7, the rare earth oxide content was 9.8 wt%.
[0700] The pore size distribution curve of DCY-7 calculated based on the BJH model calculation had the same characteristics as the curve b in FIG. 6, and the adsorption / desorption curve had the same characteristics as the curve d in FIG.
[0701] The XRD pattern of DCY-7 had similar features to that of PAY-1. The XRD characteristic parameters and pore parameters are shown in the table below.
[0702] [Table 3]
[0703] As can be seen from the data in the table, the mesopore area and mesopore volume of the Y-type molecular sieve containing rare earth obtained by the manufacturing method of the present invention are both significantly higher than those of the sample manufactured in the comparative example. The crystallinity shows that by adopting the pressure hydrothermal calcination with controlled environment, the mesopore richness of the Y-type molecular sieve can be significantly increased, and a certain degree of mesopores of the molecular sieve can be formed.
[0704] Example E Example E illustrates the preparation of the rare earth-containing Y-type molecular sieve of the present invention, which can be used to prepare catalytic cracking catalysts.
[0705] 100g of NaY-type molecular sieve and 1800g of deionized water were mixed and stirred vigorously, and 10g of solid ammonium chloride was added. The resulting mixture was stirred uniformly, the temperature was raised to 70℃, and stirred at a constant temperature for 2.0 hours. After filtering, washing with water and drying, 20mL of rare earth chloride salt solution with a concentration of 357gRE2O3 / L and 2g of solid ammonium chloride were added. The resulting mixture was stirred uniformly, and the temperature was raised to 70℃. The pH value of the slurry was adjusted to 4.5 using dilute hydrochloric acid, and stirred at a constant temperature for 1.0 hour.
[0706] After filtering, washing and drying, 7 g of ammonia water was added under external pressure, and then pressurized hydrothermal calcination was performed at 500°C, gauge pressure 0.3 MPa, and 100% steam for 2.0 hours to obtain a sample of Y-type molecular sieve containing rare earths, which is designated as PEY-1.
[0707] In the chemical composition of PEY-1, the rare earth oxide content was 10.1 wt%.
[0708] The pore size distribution curve of PEY-1 calculated based on the BJH model showed that there were at least three types of mesopore size distributions, with three prominent types of mesopore size distributions at the positions of 2–3 nm, 3–4 nm, and 10–30 nm, respectively.
[0709] For PEY-1, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of all pores was 0.25, and the ratio of the peak area of the pore size distribution of 10 to 30 nm to the peak area of all pores was 0.3.
[0710] The XRD pattern of PEY-1 had similar features to that of PAY-1.
[0711] As shown in the XRD pattern of PEY-1, the ratio of the intensity I1 of the peak at 2θ=11.8±0.1° to the intensity I2 of the peak at 2θ=12.3±0.1° was 6.3.
[0712] The following examples illustrate the catalytic cracking catalysts provided by the present invention.
[0713] The characteristics of the raw materials used are as follows: Kaolin (Suzhou China Kaolin Corporation, solid content 75% by weight) Alumina sol (Qilu Catalyst Co., Ltd., alumina content 21.5% by weight) Peptized pseudoboehmite (solid content 10% by weight)
[0714] The catalytic performance test was carried out using Wu-mixed triple oil, whose main characteristics are as follows:
[0715] [Table 4]
[0716] (Examples A8 to A14) The pseudo-boehmite and deionized water were mixed and stirred vigorously, and 36 wt% hydrochloric acid was added to the resulting slurry to peptize it. The ratio of acid to aluminum (weight ratio of 36 wt% hydrochloric acid to dry-based pseudo-boehmite) was 0.20. The temperature of the mixture was raised to 65°C and oxidized for 1 hour, and the dry-based kaolin slurry and alumina sol were added, respectively, and the mixture was stirred for 20 minutes, and then the dry-based Y-type molecular sieve samples PAY-1 to PAY-7 containing rare earth were added, respectively, and stirred for 30 minutes to obtain a slurry with a solid content of 30 wt%, which was spray-dried to produce the microsphere catalyst.
[0717] The microsphere catalyst was then calcined at 500°C for 1 hour, and then washed with an aqueous ammonium chloride solution at 60°C (ammonium chloride: microsphere catalyst: water = 0.2: 1: 10) until the sodium oxide content was less than 0.30% by weight. The catalyst was then washed multiple times with deionized water, filtered, and placed in a thermostatic oven at 120°C for drying for 12 hours. The resulting catalysts are referred to as AC-1 to AC-7, respectively. The specific blending ratios of the dry-based catalysts are shown in the table below.
[0718] (Comparative example A8~Comparative example A14) The catalyst was produced in the same manner as in Example A8, except that the rare earth-containing Y-type molecular sieve of Example A8 was replaced with the rare earth-containing Y-type molecular sieve comparative samples DAY-1 to DAY-7 produced in Comparative Example A1 to Comparative Example A7, respectively. The obtained comparative catalysts are respectively referred to as DAC-1 to DAC7. The specific compounding ratios of the comparative catalysts are shown in the table below.
[0719] [Table 5]
[0720] (Test Example A2) Test Example A2 illustrates the technical effect of the catalytic cracking catalyst of the present invention.
[0721] The above catalyst samples AC-1 to AC-7 and comparative catalyst samples DAC-1 to DAC-7 were subjected to hydrothermal aging treatment in an environment of 800° C. and 100% steam for 17 hours, and then subjected to heavy oil trace activity evaluation.
[0722] Heavy oil trace activity evaluation conditions: catalyst loading amount was 5g, feed oil was Wu-mixed triple oil, oil feeding amount was 1.384g, reaction temperature was 500℃, and regeneration temperature was 600℃.
[0723] The evaluation results are shown in the table below. The catalytic cracking catalyst of the present invention has excellent heavy oil conversion capacity and high gasoline yield.
[0724] [Table 6]
[0725] (Examples D8 to D14) The pseudo-boehmite and deionized water were mixed and stirred vigorously, and 36 wt% hydrochloric acid was added to the resulting slurry to peptize it. The ratio of acid to aluminum (weight ratio of 36 wt% hydrochloric acid to dry-based pseudo-boehmite) was 0.20. The temperature of the mixture was raised to 65°C and oxidized for 1 hour, and the dry-based kaolin slurry and alumina sol were added, respectively, and the mixture was stirred for 20 minutes, and then the dry-based rare earth-containing Y-type molecular sieve samples PDY-1 to PDY-7 were added, respectively, and stirred for 30 minutes to obtain a slurry with a solid content of 30 wt%, which was spray-dried to produce the microsphere catalyst.
[0726] The microsphere catalyst was then calcined at 500°C for 1 hour, and then washed with an aqueous ammonium chloride solution at 60°C (ammonium chloride: microsphere catalyst: water = 0.2: 1: 10) until the sodium oxide content was less than 0.30% by weight. The catalyst was then washed multiple times with deionized water, filtered, and placed in a thermostatic oven at 120°C for drying for 12 hours. The resulting catalysts are referred to as DC-1 to DC-7, respectively. The specific blending ratios of the dry-based catalysts are shown in the table below.
[0727] (Comparative Examples D8 to D14) The catalyst was produced in the same manner as in Example D8, except that the rare earth-containing Y-type molecular sieve of Example D8 was replaced with the rare earth-containing Y-type molecular sieve comparative samples DDY-1 to DDY-7 produced in Comparative Examples D1 to D7, respectively. The obtained comparative catalysts are referred to as DDC-1 to DDC7, respectively. The specific blending ratio of the dry-based catalyst is shown in the table below.
[0728] [Table 7]
[0729] (Test Example D2) Test Example D2 illustrates the technical effect of the catalytic cracking catalyst of the present invention.
[0730] The above catalyst samples DC-1 to DC-7 and comparative catalyst samples DDC-1 to DDC-7 were subjected to hydrothermal aging treatment in an environment of 800° C. and 100% steam for 17 hours, and then subjected to heavy oil trace activity evaluation.
[0731] Heavy oil trace activity evaluation conditions: catalyst loading amount was 5g, feed oil was Wu-mixed triple oil, oil feeding amount was 1.384g, reaction temperature was 500℃, and regeneration temperature was 600℃.
[0732] The evaluation results are shown in the table below. The catalytic cracking catalyst of the present invention has excellent heavy oil conversion capacity and high gasoline yield.
[0733] [Table 8]
[0734] (Example B8 and Example C8) Examples B8 and C8 illustrate the preparation of cracking catalysts of the present invention.
[0735] Pseudo-boehmite and deionized water are mixed and stirred vigorously, and 36% by weight of hydrochloric acid is added to the obtained slurry to peptize it. The ratio of acid to aluminum (weight ratio of 36% by weight of hydrochloric acid to pseudo-boehmite on a dry basis) is 0.20. The temperature of the mixture is raised to 65°C and oxidized for 1 hour, and then the dry-based kaolin slurry and alumina sol are added, respectively, and the mixture is stirred for 20 minutes, and then the dry-based rare earth-containing Y-type molecular sieve samples (Example B1, Example C1) are added, respectively, and stirred for 30 minutes to obtain a slurry with a solid content of 30% by weight, which is spray-dried to prepare a microsphere catalyst.
[0736] The microsphere catalyst was then calcined at 500°C for 1 hour, and then washed with an aqueous ammonium chloride solution at 60°C (ammonium chloride: microsphere catalyst: water = 0.2: 1: 10) until the sodium oxide content was less than 0.30% by weight. It was then washed multiple times with deionized water, filtered, and placed in a thermostatic oven at 120°C for drying for 12 hours. The resulting catalysts are referred to as BC-1 and CC-1, respectively. The specific blending ratios of the dry-based catalysts are shown in the table below.
[0737] (Comparative Example B8.1, Comparative Example B8.2, Comparative Example C8) Catalysts were produced in the same manner as in Example B8, except that the rare earth-containing Y-type molecular sieve of Example B1 was replaced with the rare earth-containing Y-type molecular sieve comparative samples DBY-1.1, DBY-1.2, and DCY-1 produced in Comparative Example B1.1, Comparative Example B1.2, and Comparative Example C1, respectively. The obtained comparative catalysts are referred to as DBC-1.1, DBC-1.2, and DCC-1, respectively. The specific compounding ratios of the dry-based comparative catalysts are shown in the table below.
[0738] (test) Cracking catalysts BC-1, CC-1, and comparative cracking catalysts DBC-1.1, DBC-1.2, and DCC-1 were each subjected to hydrothermal aging treatment at 800°C in a 100% steam environment for 17 hours, and then their heavy oil trace activity was evaluated.
[0739] Heavy oil trace activity evaluation conditions: catalyst loading amount was 5g, feed oil was Wu-mixed triple oil, oil feeding amount was 1.384g, reaction temperature was 500℃, and regeneration temperature was 600℃.
[0740] The evaluation results are shown in the table below.
[0741] (Example B9 and Example C9) Examples B9 and C9 illustrate the preparation of cracking catalysts of the present invention.
[0742] Pseudo-boehmite and deionized water are mixed and stirred vigorously, and 36% by weight of hydrochloric acid is added to the obtained slurry to peptize it. The ratio of acid to aluminum (weight ratio of 36% by weight of hydrochloric acid to pseudo-boehmite on a dry basis) is 0.20. The temperature of the mixture is raised to 65°C and oxidized for 1 hour, and then the dry-based kaolin slurry and alumina sol are added, respectively, and the mixture is stirred for 20 minutes, and then the dry-based rare earth-containing Y-type molecular sieve samples (Example B2, Example C2) are added, respectively, and stirred for 30 minutes to obtain a slurry with a solid content of 30% by weight, which is spray-dried to prepare a microsphere catalyst.
[0743] The microsphere catalyst was then calcined at 500°C for 1 hour, and then washed with an aqueous ammonium chloride solution at 60°C (ammonium chloride: microsphere catalyst: water = 0.2: 1: 10) until the sodium oxide content was less than 0.30 wt%. It was then washed multiple times with deionized water, filtered, and placed in a thermostatic oven at 120°C for drying for 12 hours. The resulting catalysts are referred to as BC-2 and CC-2, respectively. The specific blending ratios of the dry-based catalysts are shown in the table below.
[0744] (Comparative Example B9.1, Comparative Example B9.2, Comparative Example C9) Catalysts were produced in the same manner as in Example B9, except that the rare earth-containing Y-type molecular sieve of Example B2 was replaced with the rare earth-containing Y-type molecular sieve comparative samples DBY-2.1, DBY-2.2, and DCY-2 produced in Comparative Example B2.1, Comparative Example B2.2, and Comparative Example C2, respectively. The obtained comparative catalysts are referred to as DBC-2.1, DBC-2.2, and DCC-2, respectively. The specific compounding ratios of the dry-based comparative catalysts are shown in the table below.
[0745] (test) The cracking catalysts BC-2, CC-2, and the comparative cracking catalysts DBC-2.1, DBC-2.2, and DCC-2 were each subjected to hydrothermal aging treatment at 800°C in a 100% steam environment for 17 hours, and then their heavy oil trace activity was evaluated.
[0746] Heavy oil trace activity evaluation conditions: catalyst amount was 5g, feed oil was Wu-mixed triple oil, oil supply amount was 1.384g, reaction temperature was 500℃, and regeneration temperature was 600℃.
[0747] The evaluation results are shown in the table below.
[0748] (Example B10 and Example C10) Examples B10 and C10 illustrate the preparation of cracking catalysts of the present invention.
[0749] Pseudo-boehmite and deionized water are mixed and stirred vigorously, and 36% by weight of hydrochloric acid is added to the obtained slurry to peptize it. The ratio of acid to aluminum (weight ratio of 36% by weight of hydrochloric acid to pseudo-boehmite on a dry basis) is 0.20. The temperature of the mixture is raised to 65°C and oxidized for 1 hour, and then the dry-based kaolin slurry and alumina sol are added, respectively, and stirred for 20 minutes, and then the dry-based Y-type molecular sieve samples containing rare earth (Example B3, Example C3) are added, respectively, and stirred for 30 minutes to obtain a slurry with a solid content of 30% by weight, which is spray-dried to prepare a microsphere catalyst.
[0750] The microsphere catalyst was then calcined at 500°C for 1 hour, and then washed with an aqueous ammonium chloride solution at 60°C (ammonium chloride: microsphere catalyst: water = 0.2: 1: 10) until the sodium oxide content was less than 0.30% by weight. It was then washed multiple times with deionized water, filtered, and placed in a thermostatic oven at 120°C for drying for 12 hours. The resulting catalysts are referred to as BC-3 and CC-3, respectively. The specific compounding ratios of the dry-based catalysts are shown in the table below.
[0751] (Comparative Example B10.1, Comparative Example B10.2, Comparative Example C10) Catalysts were produced in the same manner as in Example B10, except that the rare earth-containing Y-type molecular sieve of Example B3 was replaced with the rare earth-containing Y-type molecular sieve comparative samples DBY-3.1, DBY-3.2, and DCY-3 produced in Comparative Example B3.1, Comparative Example B3.2, and Comparative Example C3, respectively. The obtained comparative catalysts are referred to as DBC-3.1, DBC-3.2, and DCC-3, respectively. The specific compounding ratios of the dry-based comparative catalysts are shown in the table below.
[0752] (test) The cracking catalysts BC-3, CC-3, and the comparative cracking catalysts DBC-3.1, DBC-3.2, and DCC-3 were each subjected to hydrothermal aging treatment at 800°C in a 100% steam environment for 17 hours, and then their heavy oil trace activity was evaluated.
[0753] Heavy oil trace activity evaluation conditions: catalyst loading amount was 5g, feed oil was Wu-mixed triple oil, oil feeding amount was 1.384g, reaction temperature was 500℃, and regeneration temperature was 600℃.
[0754] The evaluation results are shown in the table below.
[0755] (Example B11 and Example C11) Examples B11 and C11 illustrate the preparation of cracking catalysts of the present invention.
[0756] Pseudo-boehmite and deionized water are mixed and stirred vigorously, and 36% by weight of hydrochloric acid is added to the obtained slurry to peptize it. The ratio of acid to aluminum (weight ratio of 36% by weight of hydrochloric acid to pseudo-boehmite on a dry basis) is 0.20. The temperature of the mixture is raised to 65°C and oxidized for 1 hour, and then the dry-based kaolin slurry and alumina sol are added, respectively, and the mixture is stirred for 20 minutes, and then the dry-based rare earth-containing Y-type molecular sieve samples (Example B4, Example C4) are added, respectively, and stirred for 30 minutes to obtain a slurry with a solid content of 30% by weight, which is spray-dried to prepare a microsphere catalyst.
[0757] The microsphere catalyst was then calcined at 500°C for 1 hour, and then washed with an aqueous ammonium chloride solution at 60°C (ammonium chloride: microsphere catalyst: water = 0.2: 1: 10) until the sodium oxide content was less than 0.30% by weight. It was then washed multiple times with deionized water, filtered, and placed in a thermostatic oven at 120°C for drying for 12 hours. The resulting catalysts are referred to as BC-4 and CC-4, respectively. The specific compounding ratios of the dry-based catalysts are shown in the table below.
[0758] (Comparative Example B11.1, Comparative Example B11.2, Comparative Example C11) The catalyst was produced in the same manner as in Example B11, except that the rare earth-containing Y-type molecular sieve of Example B4 was replaced with the rare earth-containing Y-type molecular sieve comparative samples DBY-4.1, DBY-4.2, and DCY-4 produced in Comparative Example B4.1, Comparative Example B4.2, and Comparative Example C4, respectively. The obtained comparative catalysts are referred to as DBC-4.1, DBC-4.2, and DCC-4, respectively. The specific compounding ratio of the dry-based comparative catalyst is shown in the table below.
[0759] (test) The cracking catalysts BC-4, CC-4, and the comparative cracking catalysts DBC-4.1, DBC-4.2, and DCC-4 were each subjected to hydrothermal aging treatment at 800°C in a 100% steam environment for 17 hours, and then their heavy oil trace activity was evaluated.
[0760] Heavy oil trace activity evaluation conditions: catalyst loading amount was 5g, feed oil was Wu-mixed triple oil, oil feeding amount was 1.384g, reaction temperature was 500℃, and regeneration temperature was 600℃.
[0761] The evaluation results are shown in the table below.
[0762] (Example B12 and Example C12) Examples B12 and C12 illustrate the preparation of cracking catalysts of the present invention.
[0763] Pseudo-boehmite and deionized water are mixed and stirred vigorously, and 36% by weight of hydrochloric acid is added to the obtained slurry to peptize it. The ratio of acid to aluminum (weight ratio of 36% by weight of hydrochloric acid to pseudo-boehmite on a dry basis) is 0.20. The temperature of the mixture is raised to 65°C and oxidized for 1 hour, and then the dry-based kaolin slurry and alumina sol are added, respectively, and the mixture is stirred for 20 minutes, and then the dry-based rare earth-containing Y-type molecular sieve samples (Example B5, Example C5) are added, respectively, and stirred for 30 minutes to obtain a slurry with a solid content of 30% by weight, which is spray-dried to prepare a microsphere catalyst.
[0764] The microsphere catalyst was then calcined at 500°C for 1 hour, and then washed with an aqueous ammonium chloride solution at 60°C (ammonium chloride: microsphere catalyst: water = 0.2: 1: 10) until the sodium oxide content was less than 0.30% by weight. It was then washed multiple times with deionized water, filtered, and placed in a thermostatic oven at 120°C for drying for 12 hours. The resulting catalysts are referred to as BC-5 and CC-5, respectively. The specific blending ratios of the dry-based catalysts are shown in the table below.
[0765] (Comparative Example B12.1, Comparative Example B12.2, Comparative Example C12) Catalysts were produced in the same manner as in Example B12, except that the rare earth-containing Y-type molecular sieve of Example B5 was replaced with the rare earth-containing Y-type molecular sieve comparative samples DBY-5.1, DBY-5.2, and DCY-5 produced in Comparative Example B5.1, Comparative Example B5.2, and Comparative Example C5, respectively. The obtained comparative catalysts are referred to as DBC-5.1, DBC-5.2, and DCC-5, respectively. The specific compounding ratios of the dry-based comparative catalysts are shown in the table below.
[0766] (test) The cracking catalysts BC-5, CC-5, and the comparative cracking catalysts DBC-5.1, DBC-5.2, and DCC-5 were each subjected to hydrothermal aging treatment at 800°C in a 100% steam environment for 17 hours, and then their heavy oil trace activity was evaluated.
[0767] Heavy oil trace activity evaluation conditions: catalyst loading amount was 5g, feed oil was Wu-mixed triple oil, oil feeding amount was 1.384g, reaction temperature was 500℃, and regeneration temperature was 600℃.
[0768] The evaluation results are shown in the table below.
[0769] (Example B13 and Example C13) Examples B13 and C13 illustrate the preparation of cracking catalysts of the present invention.
[0770] Pseudo-boehmite and deionized water are mixed and stirred vigorously, and 36% by weight of hydrochloric acid is added to the obtained slurry to peptize it. The ratio of acid to aluminum (weight ratio of 36% by weight of hydrochloric acid to pseudo-boehmite on dry basis) is 0.20. The temperature of the mixture is raised to 65°C and oxidized for 1 hour, and then the dry-based kaolin slurry and alumina sol are added, respectively, and the mixture is stirred for 20 minutes, and then the dry-based Y-type molecular sieve samples containing rare earth (Example B6, Example C6) are added, respectively, and stirred for 30 minutes to obtain a slurry with a solid content of 30% by weight, which is spray-dried to prepare a microsphere catalyst.
[0771] The microsphere catalyst was then calcined at 500°C for 1 hour, and then washed with an aqueous ammonium chloride solution at 60°C (ammonium chloride: microsphere catalyst: water = 0.2: 1: 10) until the sodium oxide content was less than 0.30% by weight. It was then washed multiple times with deionized water, filtered, and placed in a thermostatic oven at 120°C for drying for 12 hours. The resulting catalysts are referred to as BC-6 and CC-6, respectively. The specific blending ratios of the dry-based catalysts are shown in the table below.
[0772] (Comparative Example B13.1, Comparative Example B13.2, Comparative Example C13) Catalysts were produced in the same manner as in Example B13, except that the rare earth-containing Y-type molecular sieve of Example B6 was replaced with the rare earth-containing Y-type molecular sieve comparative samples DBY-6.1, DBY-6.2, and DCY-6 produced in Comparative Example B6.1, Comparative Example B6.2, and Comparative Example C6, respectively. The obtained comparative catalysts are referred to as DBC-6.1, DBC-6.2, and DCC-6, respectively. The specific compounding ratios of the dry-based comparative catalysts are shown in the table below.
[0773] (test) The cracking catalysts BC-6, CC-6, and the comparative cracking catalysts DBC-6.1, DBC-6.2, and DCC-6 were each subjected to hydrothermal aging treatment at 800°C in a 100% steam environment for 17 hours, and then their heavy oil trace activity was evaluated.
[0774] Heavy oil trace activity evaluation conditions: catalyst loading amount was 5g, feed oil was Wu-mixed triple oil, oil feeding amount was 1.384g, reaction temperature was 500℃, and regeneration temperature was 600℃.
[0775] The evaluation results are shown in the table below.
[0776] (Example B14 and Example C14) Examples B14 and C14 illustrate the preparation of cracking catalysts of the present invention.
[0777] Pseudo-boehmite and deionized water are mixed and stirred vigorously, and 36% by weight of hydrochloric acid is added to the obtained slurry to peptize it. The ratio of acid to aluminum (weight ratio of 36% by weight of hydrochloric acid to pseudo-boehmite on dry basis) is 0.20. The temperature of the mixture is raised to 65°C and oxidized for 1 hour, and then the dry-based kaolin slurry and alumina sol are added, respectively, and the mixture is stirred for 20 minutes, and then the dry-based Y-type molecular sieve samples containing rare earth (Example B7, Example C7) are added, respectively, and stirred for 30 minutes to obtain a slurry with a solid content of 30% by weight, which is spray-dried to prepare a microsphere catalyst.
[0778] The microsphere catalyst was then calcined at 500°C for 1 hour, and then washed with an aqueous ammonium chloride solution at 60°C (ammonium chloride: microsphere catalyst: water = 0.2: 1: 10) until the sodium oxide content was less than 0.30% by weight. It was then washed multiple times with deionized water, filtered, and placed in a thermostatic oven at 120°C for drying for 12 hours. The resulting catalysts are referred to as BC-7 and CC-7, respectively. The specific blending ratios of the dry-based catalysts are shown in the table below.
[0779] (Comparative Example B14.1, Comparative Example B14.2, Comparative Example C14) Catalysts were produced in the same manner as in Example B14, except that the rare earth-containing Y-type molecular sieve of Example B7 was replaced with the rare earth-containing Y-type molecular sieve comparative samples DBY-7.1, DBY-7.2, and DCY-7 produced in Comparative Example B7.1, Comparative Example B7.2, and Comparative Example C7, respectively. The obtained comparative catalysts are referred to as DBC-7.1, DBC-7.2, and DCC-7, respectively. The specific compounding ratios of the comparative catalysts on a dry basis are shown in the table below.
[0780] (test) The cracking catalysts BC-7, CC-7, and the comparative cracking catalysts DBC-7.1, DBC-7.2, and DCC-7 were each subjected to hydrothermal aging treatment at 800°C in a 100% steam environment for 17 hours, and then their heavy oil trace activity was evaluated.
[0781] Heavy oil trace activity evaluation conditions: catalyst loading amount was 5g, feed oil was Wu-mixed triple oil, oil feeding amount was 1.384g, reaction temperature was 500℃, and regeneration temperature was 600℃.
[0782] The evaluation results are shown in the table below.
[0783] As can be seen from the table, the catalyst prepared by the present invention has excellent heavy oil conversion ability and high gasoline yield.For example, compared with DBC-1.1, the BC-1 sample of the present invention has excellent heavy oil cracking activity after hydrothermal aging treatment at 800℃ and 100% steam environment for 17 hours, the conversion rate is increased by 6.22%, the gasoline yield is increased by 5.15%, and the coke / conversion rate is decreased by 0.01.
[0784] [Table 9] JPEG0007595638000010.jpg202169 [Brief description of the drawings]
[0785] [Figure 1] FIG. 1 shows the pore size distribution curve of PAY-1 calculated based on the BJH model calculation. [Diagram 2] FIG. 2 is an X-ray diffraction (XRD) spectrum of PAY-1. [Diagram 3] FIG. 3 shows the pore size distribution curve on DAY-1 calculated based on the BJH model calculation. [Figure 4] FIG. 4 shows the pore size distribution curve of PDY-1 calculated based on the BJH model calculation. [Diagram 5] FIG. 5 shows the pore size distribution curve of DDY-1 calculated based on the BJH model calculation. [Figure 6] FIG. 6 shows the pore size distribution curves of PBY-1 (curve a), DBY-1.1 (curve b) and PCY-1 (curve A) calculated based on the BJH model calculation. [Figure 7]FIG. 7 shows the adsorption-desorption curves of PBY-1 (curve c), DBY-1.1 (curve d) and PCY-1 (curve c).
Claims
1. A rare earth-containing Y-type molecular sieve having at least two types of mesopore pore size distributions of 2-3 nm and 3-4 nm; The mesopore volume of the Y-type molecular sieve is greater than 0.03 cc / g; and / or The intensity I of the peak at 2θ=12.3±0.1° in the X-ray diffraction pattern of the Y-type molecular sieve 2 Intensity I of the peak at 2θ=11.8±0.1° 1 is ≧4.0; Y-type molecular sieve.
2. The Y-type molecular sieve according to claim 1, wherein the mesopore volume of the Y-type molecular sieve is 0.031 cc / g to 0.057 cc / g.
3. The ratio of a peak intensity I 1 at 2θ=11.8±0.1° to a peak intensity I 2 at 2θ=12.3±0.1° in the X-ray diffraction pattern is 4.5 to 6.
0.
3. The Y-type molecular sieve according to claim 1 or 2.
4. The ratio of the intensity I 1 of a peak at 2θ=11.8±0.1° to the intensity I 2 of a peak at 2θ=12.3±0.1° in the X-ray diffraction pattern is ≧4.
8.
3. The Y-type molecular sieve according to claim 1 or 2.
5. The ratio of a peak intensity I 1 at 2θ=11.8±0.1° to a peak intensity I 2 at 2θ=12.3±0.1° in the X-ray diffraction pattern is 4.9 to 7.
0.
3. The Y-type molecular sieve according to claim 1 or 2.
6. In the BJH pore size distribution curve of the Y-type molecular sieve, the ratio of the peak area of the pore size distribution of 2-3 nm to the peak area of the pore size distribution of 3-4 nm is ≧0.05; 3. The Y-type molecular sieve according to claim 1 or 2.
7. In the BJH pore size distribution curve of the Y-type molecular sieve, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of the pore size distribution of 3 to 4 nm is ≧0.
1.
3. The Y-type molecular sieve according to claim 1 or 2.
8. In the BJH pore size distribution curve of the Y-type molecular sieve, the ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of the pore size distribution of 3 to 4 nm is 0.1 to 0.
4.
3. The Y-type molecular sieve according to claim 1 or 2.
9. The rare earth content is 2 to 18 wt % as rare earth oxide, the unit lattice constant is 2.440 to 2.470 nm, and the crystallinity is 30 to 60%.
3. The Y-type molecular sieve according to claim 1 or 2.
10. The rare earth content is 8 to 15 wt % as rare earth oxide, the unit lattice constant is 2.440 to 2.470 nm, and the crystallinity is 30 to 60%.
3. The Y-type molecular sieve according to claim 1 or 2.
11. In the BJH pore size distribution curve of the Y-type molecular sieve, the pore size distribution of mesopores is 10-30 nm, and the ratio of the peak area of the pore size distribution of 2-3 nm to the peak area of all pores is greater than 0.1; The ratio of the peak area of the pore size distribution of 10 to 30 nm to the peak area of all pores is greater than 0.2; 3. The Y-type molecular sieve according to claim 1 or 2.
12. The ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of all pores is greater than 0.12, The ratio of the peak area of the pore size distribution of 10 to 30 nm to the peak area of all pores is greater than 0.22; The Y-type molecular sieve according to claim 11.
13. The ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of all pores is greater than 0.15, The ratio of the peak area of the pore size distribution of 10 to 30 nm to the peak area of all pores is greater than 0.25; The Y-type molecular sieve according to claim 11.
14. The ratio of the peak area of the pore size distribution of 2 to 3 nm to the peak area of all pores is 0.18 to 0.26, The ratio of the peak area of the pore size distribution of 10 to 30 nm to the peak area of all pores is 0.27 to 0.32; The Y-type molecular sieve according to claim 11.
15. A method for producing a Y-type molecular sieve containing rare earth according to any one of claims 1 to 14, comprising the steps of: The rare earth-containing Y-type molecular sieve is obtained by subjecting a rare earth-containing NaY-type molecular sieve to hydrothermal calcination treatment in an environment where pressure is applied from the outside and an aqueous solution containing an acidic or alkaline substance is added from the outside; or the rare earth-containing Y-type molecular sieve is obtained by contacting a rare earth-containing NaY-type molecular sieve with an acidic or alkaline substance to obtain a rare earth-containing NaY-type molecular sieve containing an acidic or alkaline substance, and then subjecting the rare earth-containing Y-type molecular sieve to hydrothermal calcination treatment in an environment where pressure is applied from the outside and water is added from the outside, the environment having a gauge pressure of 0.01 to 1.0 MPa and containing 1 to 100% water vapor; method.
16. The environment has a gauge pressure of 0.1 to 0.8 MPa and contains 30% to 100% water vapor. The method of claim 15.
17. The environment has a gauge pressure of 0.3 to 0.6 MPa and contains 60% to 100% water vapor. The method of claim 15.
18. The rare earth-containing NaY-type molecular sieve is obtained through a step A of contacting the NaY-type molecular sieve with a rare earth salt solution or a mixed solution of a rare earth salt solution and an ammonium salt. The method of claim 15.
19. The rare earth-containing NaY-type molecular sieve can be obtained by the following steps (1) and (2): (1) Partially ammonium exchange the NaY type molecular sieve with ammonium salt to remove 10-80% of sodium ions, filter, wash with water, and dry to obtain NH 4 Obtaining NaY type molecular sieve; (2) The NH obtained in step (1) 4 contacting the NaY-type molecular sieve with a rare earth salt solution or a mixed solution of a rare earth salt solution and an ammonium salt, filtering, washing with water, and drying to obtain the NaY-type molecular sieve containing the rare earth; The method of claim 15.
20. The rare earth salt solution is an aqueous chloride solution containing one or more of lanthanum, cerium, praseodymium and neodymium ions; 20. The method of claim 18 or 19.
21. The ammonium salt is selected from ammonium chloride, ammonium nitrate, ammonium carbonate and ammonium bicarbonate, or any mixture thereof; 20. The method of claim 18 or 19.
22. Step A or step (2) is carried out at a pH of 3.0-5.0, a water / molecular sieve weight ratio of 5-30, and an exchange temperature of room temperature to 100° C., and optionally, the exchange time is at least 0.3 hours; 20. The method of claim 18 or 19.
23. The environment has a gauge pressure of 0.1 to 0.8 MPa and contains 30 to 100% water vapor. The method according to any one of claims 15 to 19.
24. The environment has a gauge pressure of 0.3 to 0.6 MPa and contains 60 to 100% water vapor. The method according to any one of claims 15 to 19.
25. The hydrothermal calcination process is carried out at 300 to 800 ° C. The method according to any one of claims 15 to 19.
26. The hydrothermal calcination treatment step is carried out at 400 to 600 ° C. The method according to any one of claims 15 to 19.
27. The environment having water is an environment having an aqueous solution containing an acidic or alkaline substance, the acidic substance being selected from ammonium chloride, ammonium sulfate, ammonium carbonate, ammonium bicarbonate, ammonium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, hydrochloric acid, sulfuric acid, nitric acid, and any mixture thereof, and the alkaline substance being one or more of ammonia water, a buffer solution of ammonia water and ammonium chloride, sodium hydroxide, sodium metaaluminate, sodium carbonate, sodium bicarbonate, or any mixture thereof; The method according to any one of claims 15 to 19.
28. The mass concentration of the aqueous solution containing the acidic or alkaline substance is 0.1 to 20%. The method according to any one of claims 15 to 19.
29. A catalytic cracking catalyst, comprising: 20 to 60% by weight of a rare earth-containing Y-type molecular sieve according to any one of claims 1 to 14; 10 to 30% by weight of an inorganic oxide binder; and 30 to 50% by weight of a natural mineral. Catalytic cracking catalyst.
30. The natural mineral is at least one selected from kaolin, halloysite, montmorillonite, diatomite, attapulgite, sepiolite, keramite, hydrotalcite, bentonite, and rectorite, and the inorganic oxide binder is at least one selected from silica sol, alumina sol, peptized pseudoboehmite, silica alumina sol, and phosphorus-containing alumina sol; 30. The catalytic cracking catalyst of claim 29.
Citation Information
Patent Citations
Preparation method of Y type molecular sieve enriched with mesopore
CN1789127A
Catalytic cracking catalyst having a Y-type zeolite containing rare earth elements and method for producing the same
JP2015533637A
Y-type molecular sieve containing rare earth, its manufacturing method, and catalytic cracking catalyst containing said molecular sieve
JP2022540629A
Crystallized silica-alumina cogel and catalyst employing the same
US4234457A