Magnetic disk substrate and magnetic disk

The magnetic disk substrate with a damping metal film addresses surface defects and vibrations, improving durability and reliability by minimizing contact with external components, even at thinner substrates.

JP7595713B2Active Publication Date: 2024-12-06HOYA CORPORATION
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023126136
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-06-30
Filing Date
2023-08-02
Publication Date
2024-12-06
Estimated Expiration
2038-07-02

AI Technical Summary

Technical Problem

Magnetic disks with aluminum alloy substrates face surface defects post-NiP plating, leading to reduced reading and writing performance, and increasing vibrations due to substrate thinning for higher storage capacity, causing frequent failures and damage from external shocks.

Method used

A magnetic disk substrate with a metal film having a loss coefficient of 0.01 or more is applied to a glass or metal substrate, with specific thickness and vibration damping properties to minimize substrate vibrations and reduce contact with external components.

Benefits of technology

The solution effectively reduces vibrations and contact with external components, enhancing the durability and reliability of magnetic disks, even at thinner substrates, thereby reducing defects and failures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595713000005
    Figure 0007595713000005
  • Figure 0007595713000006
    Figure 0007595713000006
  • Figure 0007595713000007
    Figure 0007595713000007
Patent Text Reader

Abstract

To effectively reduce the number of times of contact between a magnetic disc and an external member due to vibration of the magnetic disc different from flutter vibration caused by impact externally received even with a thinner substrate thickness.SOLUTION: A substrate for a magnetic disc includes: a substrate body which has two main surfaces; and a film which is provided on the main surfaces and which is made from a material the loss coefficient of which is equal to or greater than 0.1. A thickness T of the substrate for a magnetic disc including the film is equal to or less than 0.700 mm, and a thickness D (mm) of the film provided on the main surfaces and the thickness T (mm) of the substrate for a magnetic disc including the film satisfies relation: D≥0.0082 / T-0.0015.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a magnetic disk substrate and a magnetic disk. [Background technology]

[0002] Conventionally, glass substrates and aluminum alloy substrates have been used as substrates for magnetic disks. A magnetic film is formed on the main surface of each of these substrates to form a magnetic disk. Magnetic disks have few surface defects, can read and write information without any problems, and can store large amounts of information. It is desirable to be able to read and write information.

[0003] For example, when an aluminum alloy substrate is used as a non-magnetic substrate for a magnetic disk, the aluminum The surface of the aluminum alloy substrate is plated with NiP, and in this process, surface defects after plating are suppressed. In order to achieve this, an Al alloy substrate for magnetic recording media was developed, on whose surface a metal film was formed by physical vapor deposition. It is known (Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2006-302358 A Summary of the Invention [Problem to be solved by the invention]

[0005] In the above-mentioned Al alloy substrate for magnetic recording media, surface defects after NiP plating formed on the substrate This is said to reduce the number of problems that can occur when reading and writing information. Thus, a magnetic disk capable of reading and writing a large amount of information can be provided without any need for a write.

[0006] In recent years, the hard disk drive industry has been focusing on the issue of magnetic particles in magnetic disks. As miniaturization approaches its limits, the speed at which recording density can be improved is slowing down. On the other hand, for big data analysis, hard disk drive devices (hereafter referred to as HDD) The demand for increased storage capacity for hard disks (HDDs) is becoming increasingly intense. There are plans to increase the number of magnetic disks that can be mounted on one hard disk drive. There are.

[0007] By increasing the number of magnetic disks installed in a hard disk drive, storage capacity can be increased. When trying to increase the size of the magnetic disk, the thickness of the magnetic disk must be increased within the limited space inside the magnetic disk drive device. It is necessary to reduce the thickness of the magnetic disk substrate, which accounts for the majority of the total thickness. Here, if the thickness of the magnetic disk substrate is reduced, the rigidity of the substrate decreases, resulting in large vibrations. It has become clear that vibrations are more likely to occur and that they can be difficult to suppress. For example, cloud data centers use a huge number of hard disk drive devices. As a result, hard disk drive units are frequently replaced due to breakdowns. At this time, the new hard disk drive unit may be damaged by the shock caused when it is installed in the rack. It was found that the time to failure was shortened. When the hard disk drive unit was subjected to an external shock, the hard disk The drive unit is not yet powered, so the magnetic disk is not rotating. I found that I would still take damage.

[0008] The vibrations caused by external shocks are transmitted to the rotating magnetic disk and its surroundings. Unlike the steady-state flutter vibration caused by air flow, which occurs during steady rotation, However, if the amplitude of this vibration is large, the magnetic head may move over the magnetic disk. A ramp member that is provided so as to protrude above the main surface of the magnetic disk in order to allow the magnetic disk to move away from the When the ramp comes into contact with the ground, particles are generated due to scraping of the ramp material, and in some cases, magnetic Scratches and defects occur on the surface of the magnetic disk. In particular, large vibrations are not damped and contact with external parts occurs. If the number of times increases, the same position on the magnetic disk may be Repeated contact occurs during the placement of the disk, which can cause particles, scratches and defects on the magnetic disk surface. Currently, for example, a magnetic disk with a nominal size of 3.5 inches is The thickness of the substrate is 0.8 mm or more, so vibration caused by external shocks becomes a problem. In addition, the number of magnetic disks mounted in the hard disk drive unit is Since the number of disks is six or less, the distance (gap) between the magnetic disk and the ramp is relatively large. Therefore, the magnetic disk and the ramp rarely come into contact with each other. When the thickness of the magnetic disk substrate is reduced in order to increase the storage capacity of the drive device, Vibrations caused by external shocks that did not cause any problems, as well as lamp components, etc. Contact with other components, as well as particles and scratches and dents on the magnetic disk that may result from contact, It is becoming difficult to ignore these issues.

[0009] Therefore, the present invention is a magnetic device that generates a flutter vibration different from the flutter vibration generated by an external shock. The number of times the magnetic disk comes into contact with external parts due to disk vibration is reduced as the thickness of the substrate becomes thinner. To provide a magnetic disk substrate and a magnetic disk capable of effectively reducing The purpose is to: [Means for solving the problem]

[0010] One aspect of the present invention is a substrate for a magnetic disk. A substrate body having two main surfaces; and a film of a metal material having a loss factor of 0.01 or more provided on the main surface. The thickness T of the magnetic disk substrate including the film is 0.700 mm or less, The thickness D [mm] of the film provided on the main surface and the thickness T [mm] of the substrate including the film mm] satisfies the following formula (1). D ≧ 0.0082 / T-0.0015 (1)

[0011] The thickness D [mm] of the film and the thickness T [mm] of the substrate including the film are expressed by the following formula (2): It is preferable that the following is satisfied. D ≧ 0.0094 / T (2)

[0012] The magnetic disk substrate is disk-shaped, The outer diameter of the disk shape is preferably 90 mm or more.

[0013] Another aspect of the present invention is a magnetic disk substrate. A substrate body having two main surfaces; and a film provided on the main surface. The magnetic disk substrate is a disk having an outer diameter of 90 mm or more, The thickness T of the magnetic disk substrate including the film is 0.700 mm or less, With the inner periphery of the substrate fixed, a shock of 120 [G] was applied to the main surface for 2 [msec]. When the substrate is subjected to a force in the normal direction, the thickness direction of the outer peripheral edge of the substrate (the normal direction of the main surface of the substrate) The membrane is provided so that the number of times that the displacement due to vibration becomes 0.2 mm or more is 4 or less. is.

[0014] Here, the substrate body (magnetic disk substrate having no film) is When the impact is applied to the disk substrate, the displacement due to vibration in the thickness direction of the outer peripheral edge of the substrate is The amount may be 0.2 mm or more more than four times.

[0015] The film is provided so as to cover the entire surface of the substrate, a thickness of the film on the end face of the substrate is greater than a thickness of the film on the main surface; The film thickness at the end face is 110% or more of the film thickness at the main surface. It is preferred that the ion exchange membrane is provided.

[0016] The thickness T of the substrate is preferably 0.640 mm or less. The thickness T of the substrate is preferably 0.520 mm or less.

[0017] The Vickers hardness Hv of the film is 100 [kgf / mm 2 ] or more. .

[0018] The material of the film preferably comprises a Ni-P alloy.

[0019] the film is formed on a main surface and an outer peripheral end surface of the substrate body, The maximum height Rz of the surface roughness of the outer peripheral end surface of the substrate body that forms the interface with the film is 0. It is preferable that the thickness is 5 μm or more.

[0020] the film is formed on a main surface and an outer peripheral end surface of the substrate body, The maximum height Rz of the surface roughness of the film on the outer peripheral end face of the non-magnetic substrate for a magnetic disk is , which is smaller than the maximum height Rz of the surface roughness of the substrate body at the outer peripheral end surface of the substrate body; It is preferable.

[0021] Another aspect of the present invention is a magnetic disk substrate having at least a magnetic film on the surface thereof. It is a magnetic disk. Effect of the Invention

[0022] According to the above-mentioned magnetic disk substrate and magnetic disk, the above-mentioned damage caused by an external impact can be prevented. The magnetic disk may come into contact with an external component due to vibration of the magnetic disk, which is different from flutter vibration. The number of times the wafer is subjected to the etching treatment can be effectively reduced even if the thickness of the substrate is reduced. [Brief description of the drawings]

[0023] [Figure 1] 1 is a diagram showing an example of the external shape of a magnetic disk substrate according to an embodiment of the present invention; [Diagram 2] 2A and 2B are diagrams illustrating an example of an edge and a film of a magnetic disk substrate according to the present embodiment. [Diagram 3] 5A and 5B are diagrams illustrating an example of vibration of the magnetic disk substrate of the present embodiment. [Figure 4] FIG. 2 is a diagram for explaining the ranges of thickness T [mm] and thickness D [mm] of the magnetic disk substrate of the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] The magnetic disk substrate of the present invention will be described in detail below. The explanation will be given using a glass substrate for a magnetic disk. In addition to the magnetic substrate, the substrate may be made of a non-magnetic metal. The substrate is a non-magnetic material made of a metal. The glass substrate materials are aluminosilicate glass, soda lime glass, borosilica glass, etc. In particular, chemical strengthening can be performed as necessary. In addition, it is possible to manufacture a glass substrate for a magnetic disk having excellent flatness of the main surface and strength of the substrate. The amorphous aluminosilicate glass is preferably used because it can This can be done. Examples of the metal substrate material include aluminum alloys, titanium alloys, and single crystal silicon. In the case of aluminum alloys, magnesium may be included as a component. Generally, metal substrates such as aluminum alloys have a lower Young's modulus than glass substrates. Therefore, the metal substrate is prone to vibration due to the influence of external shock. Since a particularly large improvement effect can be obtained by applying the above, the application of a metal substrate is preferable.

[0025] FIG. 1 is a diagram showing the external shape of a magnetic disk substrate according to this embodiment. In the present embodiment, the magnetic disk substrate 1 (hereinafter simply referred to as substrate 1) has an inner hole 2. The size of the substrate 1 is not important, but the substrate 1 may be, for example, For example, it can be suitably applied to magnetic disk substrates having a nominal diameter of 2.5 inches or 3.5 inches. For a magnetic disk substrate with a nominal diameter of 3.5 inches, the outer diameter of the disk is 90 mm. It is preferable that the nominal value of the outer diameter of the disk shape is 95 mm or 97 mm. Even with such a large disk shape, a film, which will be described later, can be formed on the main surface. This reduces the generation of particles, scratches, and dents caused by vibrations of the magnetic disk. The upper limit of the outer diameter of the disk shape is, for example, 100 mm. A typical 3.5-inch HDD (size that can be installed in a 3.5-inch bay of a typical PC case) The width of the wall is 101.6 mm, so if it exceeds 100 mm, the wall thickness will not be sufficient. There is a possibility that the magnetic disk may be damaged due to an external shock, which is different from the flutter vibration. The larger the outer diameter of the substrate 1, the stronger the vibration becomes and the harder it is to attenuate. Therefore, the larger the outer diameter of the substrate 1, the more the effect of this embodiment, which will be described later, can be exhibited. That is, the magnetic disk substrate of this embodiment is particularly suitable for a nominal disk size of 3.5 inches or more. This is suitable for use as a substrate for magnetic disks of this size.

[0026] FIG. 2 is a diagram illustrating an example of an edge and a film of the substrate 1. As shown in FIG. 2, the substrate 1 is It has a substrate body 3 and a film 4 . The substrate body 3 has a pair of main surfaces 3a and a pair of ribs 31 extending in a direction perpendicular to the pair of main surfaces 3a. and a pair of chamfers disposed between the pair of main surfaces 3a and the side wall surfaces 3b. The side wall surface 3b and the chamfered surface 3c are located at the outer peripheral end and the inner peripheral end of the substrate 1. It is formed in the part.

[0027] When glass is used for the substrate body 3, the glass composition of the substrate body 3 is, for example, expressed in mol %, as follows: SiO2, 55-78%, Li2O, 0.1-1%, Na2O, 2-15%, Mg O, CaO, SrO and BaO, total amount is 10-25%, MgO, CaO, Sr The molar ratio of the CaO content to the total content of MgO and BaO (CaO / (MgO+Ca The ratio of SrO+BaO) to the total of 0.20 or less can be set. This glass is called glass 1. say. The glass of the substrate body 3 is, for example, 45 to 68% SiO2, 45 to 68% Al2 O3 is 5-20%, and the total content of SiO2 and Al2O3 (SiO2+Al2O3) is 60 ~80%, B2O3 0~5%, MgO 3~28%, CaO 0~18%, B The total content of BaO and SrO (BaO+SrO) is 0-2%, alkaline earth metal oxides The total content (MgO+CaO+SrO+BaO) is 12-30%, and alkali metal oxides The total content of (Li2O+Na2O+K2O) is 3.5-15%, Sn oxide and Ce The oxides include at least one selected from the group consisting of Sn oxide and Ce oxide. It can also be made into an amorphous oxide glass with a total content of 0.05 to 2.00%. This glass is called Glass 2.

[0028] As shown in FIG. 2, the entire surface of the substrate body 3, that is, the main surface 3a, the side wall surface 3b, and the chamfered surface 3b are 3c is provided with a membrane 4. The membrane 4 enhances the vibration isolation properties of the substrate 1. The film 4 is a film made of a material having a loss factor of 0.01 or more. The film is made of a metal material. . The metal material of the film 4 has a higher loss factor than the material of the substrate body 3. is the value at room temperature, for example, 25°C. Hereinafter, the loss factor refers to the value at room temperature. . Here, the loss factor of the film 4 is the same as that of the substrate body 3 and the substrate 1 on which the film 4 is formed. Each of these is used as a test sample, and the resonant frequency and the half-width at the resonant frequency of the test sample are measured by vibration testing. In vibration testing, for example, the "Freedom of Vibration" made by Nippon Technoplus Co., Ltd. A vibration type Young's modulus, rigidity modulus and internal friction measuring device (JE series) can be used. The loss factor of the test sample is calculated from the resonance frequency and half-width of the test sample obtained in the vibration test. In addition, the resonance frequency and loss factor of the substrate 1, the resonance frequency of the substrate body 3, and the thickness of the substrate body 3 are From the ratio of the thickness of the film 4 to the density of the material of the substrate body 3 and the density of the metal material of the film 4, The loss factor of 4 can be calculated, for example, according to the known formula shown below. The resonance frequency and loss factor of the substrate 1 are f1 and η1, respectively, and the resonance frequency of the substrate body 3 is is f3, the ratio of the total thickness of the film 4 to the thickness of the substrate body 3 is a, and the material of the substrate body 3 is When the ratio of the density of the metal material of the film 4 to the density of the film is b, the loss coefficient η4 of the film 4 is α = (f1 / f3) 2 η4=α / (α-1)·η1, where α is the number of a and b is the number of a and b. Cut.

[0029] As a material having the characteristics (loss factor) of the film 4, a Ni-P alloy containing Ni and P is used. In the case of Ni-P alloys, P is added to make them non-magnetic. For example, the content of P may be 5 to 15 mass %. Examples of materials that can be used include Mg alloys, Al-Zn alloys, and Mg-Zr alloys. The film formation method may be, for example, a sputtering method, an electroless plating method, an electrolytic plating method, or the like. It is possible to select an appropriate one from these.

[0030] The thickness T of the substrate 1 including the substrate body 3 and the film 4 is 0.700 mm or less. Furthermore, the thickness D [mm] of the film 4 provided on the main surface 3a and the thickness T of the substrate 1 including the film 4 [mm] satisfies the following formula (1). Note that the thickness of the film 4 varies depending on the location on the main surface. It is preferable that the thickness of the main surface is constant without any change. D ≧ 0.0082 / T-0.0015 (1)

[0031] Such a substrate 1 has a thickness of 0.700 mm or less, and is therefore unlikely to be damaged by external shocks, etc. However, even if the vibration occurs, the film is not formed on the main surface 3a of the substrate body 3. Since the membrane 4 is formed, the vibration can be attenuated early. By seamlessly covering the entire periphery of the metal body 1 including the surface, the degree of suppression of the vibration is improved. In this case, the film 4 is preferably harder than the substrate body 3. It is more preferable that the thickness D1 of the film 4 formed on the main surface 3a of the substrate body 3 is It is more preferable that D2 is equal. In such a case, the deformation is large locally. Therefore, the degree of vibration suppression is higher. This reduces the number of contacts with the pump members and adjacent disks. In this embodiment, the film 4 is formed on each of the main surfaces 3a on both sides. The structure also includes a structure in which the film 4 is formed only on one of the main surfaces 3a. In this case, the thickness D is the thickness of the film 4 formed on one of the main surfaces 3a.

[0032] A magnetic disk made by forming a magnetic film on a substrate 1 is used in a hard disk drive device. The main surface of the inner hole 2 is fixed to the spindle of the hard disk drive device. For example, when a new hard disk drive is installed in a rack for replacement, When removing the hard disk drive unit from the rack to move it to another location, When these operations are performed, the hard disk drive device is subjected to external shocks. Such an impact may cause the main surface 3a of the substrate 1 to move in the normal direction (substrate Vibrations occur that displace the plate 1 in the thickness direction. This displacement is greatest at the outer peripheral edge of the main surface. This vibration is also caused by the rotating magnetic disk and the air flow around it. Unlike the steady-state flutter vibration that occurs in the steady-state rotational state, the flutter vibration occurs in the time-dependent manner as shown in Figure 3. FIG. 3 shows the vibration in the normal direction of the main surface at the outer peripheral edge of the substrate 1. FIG. 13 is a diagram illustrating an example of vibration. Such vibrations occur whether the magnetic disk is rotating or stationary. Therefore, this vibration continues for a long time, and the magnetic disk formed from the substrate 1 becomes a hard disk. In the disk drive device, the ramp member comes into contact with the magnetic disk, causing particles, scratches, and dents on the surface of the magnetic disk. This is undesirable, and may cause damage to the ramp material. In particular, when a stationary magnetic disk vibrates, particles may be generated. When the magnetic disk comes into contact with the ramp member, the same location on the magnetic disk comes into contact with the ramp member multiple times. This can easily result in particles, scratches, and dents.

[0033] However, in the substrate 1, the film 4 is made of a metal material having a loss factor of 0.01 or more. Therefore, the thickness D (=D1+D2) [mm] of the film 4 and the thickness T [mm] of the substrate body 3 are ≧ 0.0082 / T-0.0015. The thinner the thickness T, the smaller the amplitude of vibration. As the thickness increases, the amplitude becomes harder to attenuate, but it is necessary to set a lower limit for the thickness D and ensure the thickness D. Therefore, the vibration of the substrate 1 can be attenuated early. The loss factor of the film 4 is preferably 0.02 or more. There is no particular restriction on the type of material, but if the loss factor is too large, the crystals in the metal material will break down. If the hardness of the film 4 is too low, the magnetic disk may not be able to be used. This can cause the surface to become more susceptible to scratches later, which can lead to HDD crashes. In order to be able to use practical metal materials, it is preferable that the value is, for example, 0.3 or less. .

[0034] If the thickness D is less than 0.0082 / T-0.0015, the thickness D of the film 4 becomes smaller than that of the substrate body 3. Since the thickness is not sufficiently large with respect to the thickness T, it is difficult to quickly damp the vibration in the substrate 1. In addition, the film 4 cannot reduce the initial amplitude of vibration of the main surface 3a. By setting the thickness to .0082 / T-0.0015 or more, the thickness of the film 4 covering the main surface 3a is sufficiently This allows the vibration in the substrate 1 to be attenuated early and reduces the initial amplitude of the vibration. This reduces the possibility of the magnetic disk running due to vibration. The number of contacts with external components such as solder joints can be effectively reduced even if the thickness of the substrate is thin. Furthermore, it is preferable that the thickness D is 0.0094 / T or more. By setting the hardness at 0094 / T or higher, the number of times the magnetic disk comes into contact with external members is reduced. This is preferable as it will have a greater effect and reduce the probability of problems occurring after the HDD is started up. In addition, a magnetic film or the like is formed on the substrate 1 in the media process. The total thickness of the magnetic film and other layers is 0.1 μm or less, so this is not an issue in this specification. In other words, even after it is made into a magnetic disk, the effect on vibration caused by the substrate 1 is negligible. The dynamic characteristics are the same. FIG. 4 is a diagram for explaining the range of thickness T [mm] and thickness D [mm] of the substrate 1 of this embodiment. The range in this embodiment is the area above the solid curve in FIG. In this way, the thinner the thickness T, the thicker the lower limit of the thickness D.

[0035] The film 4 is provided only on the main surface 3a, and not on the side wall surface 3b and the chamfered surface 3c. Although the above-mentioned effects are achieved, as shown in FIG. 2, the film 4 is provided so as to cover the entire surface of the substrate 1. In other words, in addition to the main surface 3a, the end surface of the substrate body 3, i.e., the side wall surface 3b and the chamfered surface 3 It is preferable that the vibration generated in the substrate 1 is in the normal direction of the main surface 3a. The vibration is a vibration in which the substrate is displaced in the normal direction of the main surface 3a. The film 4 is also displaced in the normal direction of the main surface 3a at the end face of the plate body 3. By providing the end surface of the plate body 3, i.e., the side wall surface 3b and the chamfered surface 3c, the main surface 3 The amount of displacement in the normal direction of a, i.e., the amplitude of vibration, can be suppressed. This is because It is presumed that the vibration suppression effect of the membrane 4 is enhanced by connecting the main surfaces with the membrane 4. . The thickness of the film 4 on the side wall surface 3b and the chamfered surface 3c is It is preferable that the thickness is thicker than the thicknesses D1 and D2 of the two main surfaces. It is presumed that this enhances the connectivity and the vibration suppression effect of the membrane 4. The vibration generated in the substrate 1 is The vibration is displaced in the normal direction of the main surface 3a. In conjunction with this displacement, the end face of the substrate body 3 also displaces in the normal direction of the main surface 3a. By suppressing the displacement, the amount of displacement in the normal direction of the main surface 3a, i.e., the amplitude of vibration, is suppressed. Therefore, in addition to the main surface 3a, the end surface of the substrate body 3, i.e., the side wall surface 3b It is also preferable that the film 4 is formed on the chamfered surface 3c. The thickness of the film on the end surface (side wall surface 3b and chamfered surface 3c) of the substrate body 3 is The thickness should be 110% or more of the thickness D1, D2 (if the thicknesses D1, D2 are different, the thicker thickness). It is preferable that the film 4 is provided so as to have a thickness T of the substrate 1. The amplitude of the vibration can be suppressed without increasing the thickness of the substrate. It is preferable that the thickness D1, D2 on the main surface 3a is 150% or less. When the film thickness at the end face exceeds 150% of the film thickness D1, D2 at the main surface 3a, the substrate 1 The increase in mass at the outer edge of the substrate 1 causes it to rotate as a magnetic disk. This is undesirable because the centrifugal force increases and this centrifugal force tends to increase the flutter vibration.

[0036] The thinner the magnetic disk, the larger the amplitude of vibration. However, the frequency of contact with other components inside the hard disk drive increases, and the contact causes This causes problems such as increased particle generation, scratches and dents on the magnetic disk, but In the case of substrate 1, the above problem is unlikely to occur even if the thickness is set to 0.640 mm or less. It may be 0.570 mm or less, or even 0.52 mm or less, and may be 0.400 mm or less. The thickness of the substrate 1 may be, for example, 0.635 mm or less, 0.550 mm or less. The thickness of the substrate 1 can be set to 0.500 mm or less, 0.381 mm or less. From the viewpoint of mechanical durability, the thickness limit is preferably 0.2 mm or more. In principle, there is a problem with particle generation, and in some cases, there is a problem with defects such as scratches and dents. Although this embodiment has the effect of reducing defects such as particles, scratches, and dents, becomes more noticeable. If the thickness T of the board 1 is 0.640 mm or less, the height of a typical 3.5-inch HDD is 26.1mm (size that can be installed in a 3.5-inch bay of a typical PC case) The gap between the ramp members (described later) into which the magnetic disk fits is the thickness of the magnetic disk + 0.4 mm. This is preferable because it allows the number of substrates to be increased from 8 to 9 in the H If the height of the DD is set to 26.1 mm or more, it is possible to mount nine or more. In addition, if the thickness of the board is 0.520 mm or less, the board This is more preferable since it allows the number of mounted sheets to be 10 or more. These HDDs have more circuit boards than conventional HDDs, so they are more susceptible to damage when subjected to external shocks. The disk is likely to come into contact with the ramp material or adjacent disks, and the resulting There was a problem that damage (particles, scratches, dents) was easily generated, but Using a board can reduce the risk of injury.

[0037] According to one embodiment, the Vickers hardness Hv of the film 4 is 100 [kgf / mm 2 ]That's all. By increasing the Vickers hardness Hv, it is possible to improve the hardness of the hard disk drive. When it comes into contact with lamp parts in the device, defects such as scratches and dents are unlikely to occur. Vickers hardness The degree Hv is 100 [kgf / mm 2 If the battery level is less than 100%, the lamp in the hard disk drive When the hard disk drive comes into contact with other components, scratches or dents may occur, causing the hard disk drive to fail. It becomes easier.

[0038] According to one embodiment, the surface of the outer peripheral end surface of the disk-shaped substrate body 3 that forms an interface with the film 4 The maximum height of the surface roughness Rz (JIS B 0601:2001) is 0.5 μm or more. In this specification, the roughness of the substrate body 3 at the interface with the film 4 is preferably The surface roughness of the outer peripheral end surface that forms the interface with the film 4 is called the surface roughness of the outer peripheral end surface of the substrate body 3. The film 4 is formed first, and a cross-sectional image of the outer peripheral end surface of the substrate body 3 is obtained by the following method. In this way, the maximum height Rz can be calculated. The outer peripheral edge of the substrate 1 is polished by ion polishing through the center of the substrate 1 to the main surface. A sample is created by cutting it out along a plane perpendicular to the surface, with the cross section of the outer peripheral end surface exposed. A cross-sectional image of the outer peripheral end surface is taken at a magnification of, for example, 5000 times using a scanning electron microscope (SEM). From the image, the concave portion of the surface of the substrate body 3 that forms the interface with the film 4 is obtained. The convex curve is obtained by, for example, binarizing the cross-sectional image or by visual tracing. , extract a 20μm wide area anywhere on the concave-convex curve and calculate the maximum height Rz .

[0039] The interface of the substrate body 3 in contact with the film 4 has a certain degree of surface unevenness, so that the film 4 This vibration suppression is achieved by the mutual concavities at the interface between the substrate body 3 and the film 4. By penetrating and biting into the part, the adhesion between the two is increased, and the effect of suppressing vibration by the membrane 4 is improved. It is presumed that this is because it affects the substrate body 3. Also, by making the film 4 thicker, the film peeling The film stress that causes peeling increases, but the above maximum height Rz is set to 0.5 μm or more. By doing so, it is possible to prevent the film from peeling off due to film stress. The area of ​​the substrate is smaller than that of the substrate, and the shape is complex. Furthermore, the thickness of the substrate 1 is less than 0.700 mm. Since it is thinner than conventional ones, the outer peripheral edge of the substrate 1 is prone to film peeling. By making the Rz of the surface (interface) 0.5 μm or more, the adhesion between the substrate body 3 and the film 4 is improved. Therefore, peeling of the film 4 can be prevented, and the long-term reliability of the HDD can be improved. In addition, the maximum height Rz of the surface roughness of the outer peripheral end face of the substrate body 3 is set to 100 mm so as to suppress the above-mentioned vibration more effectively. In order to achieve this, it is more preferable that the thickness is 1.0 μm or more, and even more preferable that the thickness is 1.5 μm or more. On the other hand, if the maximum height Rz is excessively large, the surface roughness (substrate roughness) of the film 4 after deposition becomes large. The surface roughness of the outer peripheral end face of the plate 1 becomes larger in accordance with the surface roughness of the substrate body 3, and the main surface During processing such as surface polishing, foreign matter is likely to adhere to the outer peripheral end surface. Furthermore, the magnetic film after deposition may become Since foreign matter is likely to adhere to the outer peripheral edge of the disk, the substrate 1 and the hard disk drive This may result in a decrease in the yield rate during the manufacture of the live device. The location of the outer peripheral end surface where the thickness is to be 1 μm or more may be at least a part of the outer peripheral end surface. In order to enhance the suppression of the peeling of the film and to enhance the effect of preventing peeling of the film, both the side wall surface 3b and the chamfered surface 3c are It is preferable that the above method be used. On the other hand, if the maximum height Rz on the main surface of the substrate body 3 is too large, There is a risk that defects will be formed in the film 4 and propagate, resulting in defects such as depressions and cracks on the surface of the film 4. These defects should be removed as they can cause corrosion and surface defects after polishing. However, since the roots are deep and difficult to remove, it is preferable to form a magnetic film on the magnetic disk. Therefore, the influence remains even after the substrate body 3 is masked. For example, it is preferable to set it to 1 μm or less.

[0040] According to one embodiment, the maximum height Rz of the surface roughness of the film 4 on the outer peripheral end face of the substrate 1 is the maximum surface roughness of the substrate body 3 at the outer peripheral end surface (the boundary surface in contact with the film 4) of the substrate body 3. It is preferable that the height is smaller than the height Rz. The maximum height Rz of the surface roughness of the film 4 on the outer peripheral end face of the substrate 1 is, for example, Using a surface roughness and contour shape measuring instrument, the outer peripheral end surface is measured at multiple points (e.g., three points) under the following conditions. The maximum height Rz of the surface roughness of the film 4 is calculated by averaging the maximum height Rz of the surface roughness of the film 4 at a plurality of points. In this case, the moving (scanning) direction of the stylus is the thickness direction of the non-magnetic substrate 1. Stylus shape: tip radius 2μm, cone taper angle 60° Stylus load: 0.75mN ·Stylus movement speed: 0.02mm / sec Sampling length: 0.08mm Filter λc: 0.08mm Filter λs: 0.0008mm.

[0041] If the maximum height Rz of the surface roughness of the film 4 on the outer peripheral end face of the substrate 1 is excessively large, During subsequent processes such as film formation, this can easily cause foreign matter to adhere to the substrate 1 or scratches due to gripping of the outer edge surface. Therefore, it is preferable that the maximum height Rz is small. The maximum height Rz of the surface roughness of the film 4 at the outer peripheral end face of the substrate body 3 (the boundary surface in contact with the film 4) is It is preferable that the maximum height Rz of the surface roughness of the substrate body 3 is smaller than that of the substrate body 3. This improves the adhesion between the substrate body 3 and the film 4, prevents the film 4 from peeling off, and improves the long-term reliability of the HDD. At the same time, when forming a magnetic film on the substrate 1, the adhesion of foreign matter to the outer peripheral end face and the It is possible to prevent scratches caused by gripping. The maximum height Rz must be 1.0 μm or less. It is more preferable that the maximum height Rz is 0.5 μm or less, and even more preferable that the maximum height Rz is 0.5 μm or less. The location of the outer peripheral edge surface of the substrate 1 that limits the above may be at least a part of the outer peripheral edge surface of the substrate 1. However, in order to enhance the effect of suppressing the vibration and the effect of preventing the film from peeling off, the surface of the substrate 1 The surface portion of the film 4 is formed on both the side wall surface 3b and the chamfered surface 3c. In addition, the surface roughness of the film 4 at the outer peripheral end face is preferably the same as that of the surface of the substrate body 3 serving as the base. Therefore, if the surface roughness of the substrate body 3 is too large, the shape of the film 4 may be easily influenced. Additional processing such as end surface polishing may be required after formation.

[0042] In another embodiment of the substrate 1, the substrate 1 is in the shape of a disk having an outer diameter of 90 mm or more. The thickness of the substrate 1 is 0.700 mm or less. When a shock of 120[G] was applied for 2[msec] in the state, The number of times that the displacement due to vibration (in the normal direction of the main surface) becomes 0.2 mm or more is 4 or less. For example, the loss factor and thickness of the film 4 are set to have the above characteristics. It is set to achieve this. If the number of times the above displacement exceeds 0.2 mm is four or less, In addition, the number of repeated contacts is preferably 2 or less. It is more preferable that the number of times that the above-mentioned occurrence occurs is 2 or less. This means that there is no multiple contacts on one side of the magnetic disk. In this case, there is no repeated collision at the same position on the main surface, so the above displacement amount It is more preferable that the number of times that the thickness becomes 0.2 mm or more is two or less. Here, the characteristics of the substrate body 3 are as follows: when the substrate body 3 is subjected to the above-mentioned impact, the outer surface of the substrate body The number of times that the displacement of the peripheral edge due to vibration in the plate thickness direction becomes 0.2 mm or more exceeds 4 times. By providing a film 4 with an adjusted material and thickness, the displacement amount can be reduced to 0.2 mm. The number of times this occurs can be reduced to four or less. Generally, the substrate 1 is a disk having an outer diameter of 90 mm or more and a thickness of 0.700 mm or less. In this case, the amount of displacement caused by vibration in the thickness direction of the outer peripheral edge of the substrate 1 tends to be large. Due to the effect of the membrane 4, the number of times that the plate 1 experiences a displacement of 0.2 mm or more due to vibration is reduced to four or less. Restricted.

[0043] Such a substrate 1 is fabricated, for example, as follows. The case where a glass substrate is used will be described below. First, a glass blank that is a plate-shaped glass substrate for a magnetic disk having a pair of main surfaces is prepared. Next, the glass blank is roughly ground. The lath blank is then shaped and its edges are polished. The glass substrate is subjected to a fine grinding process using a fixed abrasive. This is followed by a first polishing process, chemical strengthening, and A second polishing is performed on the glass substrate. After this, film formation and film polishing are performed. In the embodiment, the glass substrate is manufactured according to the above-mentioned procedure, but the above-mentioned process does not always have to be performed. These processes may not be performed as appropriate. For example, among the above, the end face polishing, the fine grinding, the first polishing The chemical strengthening and second polishing may not be performed. Each treatment will be explained below. do.

[0044] (a) Forming of glass blanks The glass blank can be formed, for example, by a press molding method. In addition, the down-draw method and the redraw method can be used to obtain a circular glass blank. The polymerizable compound can be produced by using known production methods such as the fusion method and the fusion method. The plate-shaped glass blanks produced by the known manufacturing method are processed into appropriate shapes to produce magnetic Thus, a disk-shaped glass substrate is obtained, which is the base for a glass substrate for a magnetic disk.

[0045] (b)Rough grinding In the rough grinding, grinding of both main surfaces of the glass blank is carried out. In rough grinding, the glass blank is ground to the desired thickness and the main surface The glass blank is ground to a flatness close to the dimensions of the formed glass blank. This is done depending on the accuracy or surface roughness, and may not be done in some cases. .

[0046] (c) Shape processing Next, shaping is performed. In shaping, after forming the glass blank, a known processing method is used. A circular hole is formed using the above method to obtain a disk-shaped glass substrate having a circular hole. Then, the edge of the glass substrate is chamfered. As a result, the edge of the glass substrate has a main surface and Between the side wall surface 3b and the main surface 3a on both sides of the side wall surface 3b, which are perpendicular to each other, Thus, an inclined chamfered surface 3c is formed.

[0047] (d) Edge polishing Next, the edge of the glass substrate is polished. A polishing liquid containing free abrasive grains is supplied between the end surface (side wall surface 3b and chamfered surface 3c) and the polishing brush is In edge polishing, the glass substrate is polished by moving it relative to the surface. The inner peripheral end face and the outer peripheral end face of the lath substrate are polished to a mirror finish. In some cases, the end surface polishing may not be performed.

[0048] (e) Fine grinding Next, the main surfaces of the glass substrate are subjected to precision grinding. For example, a double-sided grinding machine for a planetary gear mechanism is used. The main surface 3a of the glass substrate is ground using a fixed abrasive. Grinding is performed by placing the workpiece on a grinding plate. Alternatively, grinding using loose abrasive grains can also be performed. may not be performed in some cases.

[0049] (f) First polishing Next, the main surface 3a of the glass substrate is subjected to a first polishing. The first polishing is performed using free abrasive grains. The first polishing step is performed by grinding with a fixed abrasive. In the first polishing, cracks and distortions remaining on the main surface 3a are removed. While preventing the shape of the end of the main surface 3a from being excessively depressed or protruding, The surface roughness, for example the arithmetic mean roughness Ra, can be reduced. The free abrasive grains used in the first polishing are not particularly limited, but may be, for example, cerium oxide abrasive grains or Zirconia abrasive grains are used for the first polishing. In some cases, the first polishing is not performed. Good too.

[0050] (g)Chemical strengthening The glass substrate can be appropriately chemically strengthened. For example, potassium nitrate can be used as the chemical strengthening liquid. A molten liquid obtained by heating sodium nitrate, sodium nitrate, or a mixture thereof can be used. The glass substrate is then immersed in a chemical strengthening solution to remove the oxide film on the surface of the glass substrate. The lithium ions and sodium ions in the glass composition react with the ion half of the chemical strengthening liquid. The surface layer is then filled with sodium ions and potassium ions, which have relatively large diameters. A compressive stress layer is formed in the portion, and the glass substrate is strengthened. The timing of chemical strengthening can be determined as appropriate, but it is preferable to perform polishing after chemical strengthening. In this way, the surface is smoothed and the foreign particles adhered to the surface of the glass substrate are removed by chemical strengthening. This is particularly preferable because it allows the removal of impurities. It is not necessary.

[0051] (h) Second polishing (mirror polishing) Next, the glass substrate after chemical strengthening is subjected to a second polishing. The purpose of the second polishing is to polish the surface of the substrate using a polishing device having the same structure as that of the first polishing. In the second polishing, the type and particle size of the free abrasive grains were changed from those in the first polishing, and the resin polymer was used. A soft polishing pad is used to polish the surface to a mirror finish. While preventing the shape of the end of the main surface 3a from being excessively depressed or protruded, The roughness of the main surface 3a can be reduced. The roughness of the main surface 3a is the arithmetic mean roughness Ra (JIS B 0601 2001) is preferably 0.2 nm or less. Since the main surface 3a of the substrate is not the outermost surface of the substrate 1 having the film 4, the second polishing may not be performed in some cases.

[0052] (i) Film formation A film 4 is formed on the main surface 3a, the side wall surface 3b, and the chamfered surface 3c of the fabricated glass substrate. The film 4 is formed by electrolytic plating, electroless plating, sputtering, or the like. Before the deposition, a pretreatment or a base layer may be formed to improve the adhesion of the film 4, if necessary. The film 4 is formed on the main surface 3a, the side wall surface 3b, and the chamfered surface 3c. In order to reduce the internal stress of the formed film 4, the shape of the film 4 can be changed. After the deposition, the film 4 is annealed (heat-treated) as necessary. It is preferable that the material be non-magnetic so as not to cause noise when used as a magnetic disk.

[0053] (j) Film polishing After the film 4 is formed, in order to reduce the surface roughness of the film 4, the film 4 on the main surface 3a of the substrate body 3 is The first polishing is performed. The purpose of the film polishing is to polish the surface to a mirror finish. In the first polishing, the first polishing is performed using a polishing device having a similar structure. The type and size of abrasive grains were changed, and the hardness of the resin polisher was made softer as the polishing pad. In the film polishing, multiple polishings may be performed as necessary. In this case, the later the polishing process, the finer the particle size of the free particles is, and the more precise the polishing is. The film 4 formed on the main surface 3a is polished as shown in FIG. 1, but the film 4 on the side wall surface 3b and the chamfered surface 3c is not polished. By this, the thickness of the film 4 on the side wall surface 3b and the chamfered surface 3c is made smaller than that on the main surface 3a. It can be made thicker than the thickness of the membrane 4 . As described above, the film 4 formed on the side wall surface 3b and the chamfered surface 3c is Therefore, the thickness of the film 4 on the side wall surface 3b and the chamfered surface 3c is The thickness of the film 4 is set to a level that can suppress the amplitude of vibration of the main surface 3a. The thickness is preferably set. After the film is polished, the glass substrate on which the film 4 is formed is cleaned to prepare a magnetic disk substrate. will be done.

[0054] When the substrate body 3 is an Al alloy substrate, the substrate body 3 is prepared by the following method, for example. can be. First, the aluminum alloy substrate that will become the substrate body 3 is machined to the required dimensions and shape by cutting. Thereafter, in order to improve the shape precision and flatness of the substrate body 3, pressure heating and annealing are performed. Furthermore, the end faces (inner peripheral end face and outer peripheral end face) of the substrate body 3 are ground and polished. In the same manner as in the case of the glass substrate, a rotating machine is used in which abrasive grains are fixed to the end surface of the substrate body 3 that has been cut. While pressing the tool against the substrate and rotating the two, grinding fluid is supplied from the nozzle to grind the end surface of the substrate body 3. The chamfered surface of the substrate body 3 is formed by a rotating tool having an end shaped into a chamfered shape. To reduce the surface roughness of the end face, A polisher made of nonwoven fabric is attached to the surface of the rotating tool, and a polishing liquid containing dispersed abrasive grains is supplied. While polishing, the end face of the substrate body 3 is polished. Next, the main surfaces of the substrate body 3 are ground using a double-sided grinding machine, and then further subjected to a double-sided polishing machine. Therefore, the resin polisher made of foamed polyurethane and the alumina abrasive grains or colloidal silica abrasive grains are used. The surface is polished multiple times using an abrasive containing grains, and finally washed. In addition, as a pretreatment for forming the film 4, the substrate body 3 may be subjected to a zincate treatment. After the formation of the film 4, an appropriate annealing process is performed to relieve the internal stress of the film 4. Annealing of the film 4 After the treatment, the main surface 3a is polished. The polishing may be performed multiple times depending on the requirements of the substrate. After that, cleaning is performed, and the magnetic disk substrate 1 is completed.

[0055] The film 4 may be made of any of the above-mentioned Ni-P alloys, Mg alloys, Al-Zn alloys, Mg-Zr alloys, etc. Here, the metal material of the film 4 is preferably a metal material such as a metal alloy, which is suitable for suppressing vibration of the substrate 1. The loss factor is higher than that of the plate body 3, and the loss factor is 0.01 or more. According to the IEEE 802.11b, the loss factor of the metal material of the film 4 is preferably 0.02 or more, and more preferably 0.03 or more. It is more preferable that the loss factor of the substrate body 3 is 0.002 or less. It is preferable that the loss factor of the substrate body 3 is small, and more preferable that the loss factor is 0.001 or less. The smaller the thickness of the substrate, the greater the effect of the film 4 in suppressing vibrations. Amorphous aluminosilicate glass used for magnetic disks For example, the substrate is 0.001 or less. For an Al-Mg alloy substrate for a magnetic disk, For example, it is 0.002 or less. In this way, the loss factor of the film 4 with respect to the loss factor of the substrate body 3 is Since the value of is sufficiently large, the vibration suppression effect can be effectively obtained by forming the film 4. . In addition, according to one embodiment, the material of the film 4 is preferably selected from the viewpoint of being less susceptible to particle, scratches, and dents. Vickers hardness Hv is 100 [kgf / mm 2 ] or more, but 200 [kgf / mm 2 ] or more, and 400 [kgf / mm 2 ]That's all. It is even more preferable to

[0056] The following Table 1 shows the properties of materials that can be suitably used for the substrate body 3 and the film 4. The loss factors shown in Table 1 below were calculated using the loss factor calculation method described above. The loss factor is measured at room temperature. Vickers hardness Hv is measured by measuring the micro Vickers hardness. The film 4 was indented with a hardness tester at a load of 10 gf because it was a thin film, and the substrate body 3 was indented with a hardness tester at a load of 10 gf. The measurements were taken under an indenter load of 300 gf.

[0057] [Table 1]

[0058] In Table 1 above, the loss factor of aluminosilicate glass is the same as that of glass 1 and glass The results were obtained from several glasses including the composition of glass 2. The loss factor is 0.0006, and the Vickers hardness is 741 kgf / mm 2 ] do. The composition of an Al-Mg alloy is, for example, in mass%, Mg: 3.5-5%, Si: 0-0.05. %, Fe:0~0.1%, Cu:0~0.12%, Mn:0~0.3%, Cr:0~0. 1%, Zn: 0-0.5%, Ti: 0-0.1%, and the balance is Al. The composition of the Mg alloy is, by mass%, Mg: 91.57%, Al: 7.6%, Zn: 0.7%. , Mn: 0.13%. The composition of the Al-Zn alloy is, in mass%, Al: 60%, Zn: 40%. The composition of the Mg-Zr alloy is, in mass%, Mg: 99.4%, Zn: 0.6%. The composition of the Ni-P alloy is, in mass%, Ni: 90%, P: 10%.

[0059] As can be seen from Table 1, the material of the substrate body 3 is aluminosilicate glass or An Al-Mg alloy was used, and the material of the film 4 was Ni-P alloy, Mg alloy, Al-Zn alloy, It can be seen that the use of Mg-Zr alloys is preferable from the viewpoint of suppressing vibration. Ni-P alloys, Al-Zn alloys, and Mg-Zr alloys have a Vickers hardness of 100 Hv. kgf / mm 2 ] or more, and is therefore more suitable as a material for the film 4. In addition, Ni-P alloys have a particularly high Vickers hardness Hv, It can be seen that this is even more suitable as a material for 4.

[0060] (Experimental Example 1) In order to examine the effect of the magnetic disk substrate 1, various substrates were produced (Examples 1 to 21). The magnetic disk substrate 1 is made of an aluminum alloy (Al-Mg alloy). When the film 4 was formed, the film 4 was made of a Ni-P alloy (P: 10 mass %, the remainder Ni) which was electrolessly The entire surface of the substrate body 3 was covered with a uniform film thickness by electrolytic plating. The two main surfaces are polished using a polishing device to remove 10% of the thickness of the film 4 on each main surface. The final thickness of the film 4 was the same on both main surfaces, and each film The thickness of the film 4 at the end face is set to 90% of the thickness of the film 4 at the end face. The thickness was set to about 111% of the thickness of the film 4 on the main surface. The loss factor of the Ni-P alloy was Satisfy 0.01 or more. The size of the fabricated substrate 1 was an outer diameter of 95 mm and an inner diameter (circular hole diameter) of 25 mm. A chamfer is formed at each of the outer peripheral end surface and the inner peripheral end surface at the connection portion between the two main surfaces. Regarding the specifications of this chamfer, if T is 0.64 mm or more, the angle with respect to the main surface is 4 5°, the length in the radial direction is 150 μm, and the length in the plate thickness direction is 150 μm. If it is less than .64mm, the angle to the main surface is 45°, the radial length is 100μm, and the plate The length in the thickness direction is 100 μm. At this time, the roughness of the outer peripheral end face is The maximum height Rz of both the surfaces of the plate 1 was adjusted to 0.1 μm.

[0061] The fabricated substrate 1 was attached to an evaluation device equipped with a high-speed camera. External impacts of any magnitude can be applied, and the resulting peripheral edge of the substrate can be The movement (vibration) of the object can be recorded as a video. By analyzing the video, , the displacement of the outer peripheral edge in the normal direction of the main surface can be measured. In actual HDDs, a ramp is built in for the ramp load mechanism of the magnetic head. When each magnetic disk is mounted, there is a gap of 0.2 mm between both main surfaces. In other words, the gap between the ramps where the magnetic disk fits is the thickness of the magnetic disk + 0.4 In an actual HDD, this gap is designed to remain constant even if the thickness of the board changes. On the other hand, the evaluation device is not equipped with this lamp. The amount of displacement of the board determines whether or not the board will come into contact with the lamp in an actual HDD. It is judged by the amount of displacement, and if the amount of displacement is less than 0.2 mm, it is judged that no contact with the lamp will occur. The thickness of the magnetic film formed in the media process can be determined by any one of the following methods. On the surface, even if the undercoat film and soft magnetic layer are included, the thickness is less than 100 nm, so it can be practically ignored. In this evaluation, the substrate was not rotated but was evaluated in a stationary state.

[0062] Using this evaluation device, a shock of 120 [G] was applied for 2 [msec] to the main surface of the substrate 1. An impact test was carried out in a linear direction, and the vibration in the normal direction of the main surface of the outer peripheral edge was measured. The results are shown as waveform data as shown in Figure 3. From this waveform data, Displacement in either direction normal to the center of the displacement amount of 0 is 0.2 mm or more The number of times that the number of times was 1 was counted and evaluated based on the following criteria. The number of counts is 4. The smaller the count, the less the number of times the substrate 1 comes into contact with the external member. Since the number is small, problems may occur after HDD startup in magnetic disks using this board 1. It is assumed that this will reduce the probability of failure and extend the life of the HDD. 5 times or more … ×(Fail) 3~4 times… ○(Good: Passed) 2 times or less…◎(Excellent: Passed) The evaluation results are shown in Table 2 below.

[0063] [Table 2]

[0064] Examples 1, 4, 7, 10, 13, 16, and 19 in Table 2 are comparative examples. This is an embodiment.

[0065] Among Examples 1 to 21 in Table 2, Example 1 is for the substrate thickness T of 0.381 to 0.700 mm. In all cases except for 4, 7, 10, 13, 16, and 19, D ≧ 0.0082 / T-0.00 15, and all of the evaluation results were pass. Furthermore, examples 3, 6, 9, 12, 15, 18, and 21 satisfy D ≧ 0.0094 / T. The evaluation results were excellent.

[0066] (Experimental Example 2) In order to investigate the effect of the substrate 1 using a glass material for the substrate body 3, various substrates were prepared ( Examples 22-30). The glass material used was the above-mentioned Glass 1. The film 4 was made of Ni-P An alloy (P: 10 mass%, balance Ni) was formed by electroless plating in the same manner as in Experimental Example 1, and then As in Experimental Example 1, both main surfaces were polished using a double-sided polishing machine, and The thickness of the film 4 was adjusted in this manner. The evaluation was also performed using the same evaluation method as in Experimental Example 1, and evaluation was performed based on the number of counts. The evaluation results are shown in Table 3 below.

[0067] [Table 3]

[0068] Among Examples 22 to 30 in Table 2, Examples 22, 25, and 28 are comparative examples, and Examples 23 and 24 , 26, 27, 29, and 30 are all examples. When the substrate thickness T is 0.400 to 0.640 mm, all examples except for Examples 22, 25, and 28 The results were D ≧ 0.0082 / T-0.0015, and all evaluation results were acceptable. . Furthermore, the evaluation results for Examples 24, 27, and 30, which satisfy D ≧ 0.0094 / T, are excellent. there were. From the above evaluation results, the effects of the substrate 1 are clear.

[0069] (Experimental Example 3) The maximum height Rz of the surface roughness of the outer peripheral end face of the substrate body 3 that forms the interface with the film 4 is adjusted in various ways. Substrates 1 were produced and peel tests were carried out to examine the effect of maximum height Rz (Examples 31 to 39). The substrate body 3 was made of the aluminum alloy (Al-Mg alloy) used in Experimental Example 1. In the same manner as in Experimental Example 1, a Ni-P alloy (P: 10 mass %, the remainder Ni) was applied to the substrate body 3. The maximum height Rz of the outer peripheral edge of the substrate 1 is The size of the abrasive grains contained in the formed grinding wheel used for grinding and the abrasive grains used for subsequent end surface polishing The size was changed and adjusted. Note that the surface of the outer peripheral end surface of the substrate body 3 that forms the interface with the film 4 By adjusting the surface roughness in various ways, the surface roughness of the film 4 on the outer peripheral end face of the substrate 1 also changes (e.g. For example, if the roughness of the interface between the substrate body 3 and the film 4 is increased, the surface roughness of the film 4 on the front side of the substrate 1 is increased. The maximum height Rz of the surface roughness of the film 4 on the outer peripheral edge of the substrate 1 is 0.5μ. The end faces were polished appropriately to adjust the thickness to 0.05 mm or less.

[0070] A peeling test of the film 4 on the outer peripheral end face of the fabricated substrate 1 was carried out. In terms of long-term reliability of the HDD, a substrate 1 that is easily damaged is not preferable. When the film 4 is partially peeled off, the films 4 on both main surfaces of the substrate 1 are connected to each other. This may reduce the effect of vibration suppression.

[0071] In the peeling test, a diamond pen was used to peel the film 4 formed on the side wall of the outer peripheral end face. The scratch area is made by providing 5 consecutive scratches at 1 mm intervals in the circumferential direction on the side wall surface. A scratched area is formed, adhesive tape is pressed against the scratched area, and the adhesive tape is peeled off. The surface of the film 4 at the scratched area was observed under a microscope to evaluate the degree of peeling of the film 4. The peeling degree of the film 4 was measured at each of 12 points on the outer peripheral end face at 30° intervals. The degree of peeling was checked, and the number of places where peeling of the film 4 occurred was counted. Any peeling was counted as peeling and classified as follows: Level 1: Membrane 4 peeled off in 10 or more places. Level 2: Membrane 4 peeled off in 7 to 9 places. Level 3: Membrane 4 peeled off in 4 to 6 locations. Level 4: Membrane 4 peeled off in 0 to 3 locations. The evaluation results are shown in Table 4 below. Examples 6, 9, and 12 in Table 4 are the same as Examples 6, 9, and 12 in Experimental Example 1. , 12, and the maximum height Rz of the interface between the substrate body 3 and the film 4 in Examples 6, 9, and 12 is 0 The surface roughness of the film 4 on the outer peripheral end surface of Examples 6, 9, and 12 shown in Table 4 (i.e. That is, the surface roughness of the substrate 1 is 0.1 μm in terms of maximum height Rz value, and in Examples 31 to 39 The maximum height Rz value was 0.5 μm.

[0072] [Table 4]

[0073] From the results in Table 4, regardless of the thickness T and D, by setting the maximum height Rz to 0.5 μm or more, It can be seen that the resistance to peeling is improved by setting the maximum height Rz to 1.0 μm or more. By making the maximum height Rz 1.5 μm or more, the peeling resistance is improved. It can be seen that the improvement is further increased. From the above evaluation results, the effect of the maximum height Rz is clear.

[0074] The magnetic disk substrate and the magnetic disk of the present invention have been described in detail above. The present invention is not limited to the above-described embodiments and examples, and may be modified without departing from the spirit and scope of the present invention. Of course, various improvements and modifications may be made. [Explanation of symbols]

[0075] 1 Magnetic disk substrate 2 Inner hole 3. Board body 3a Main surface 3b Side wall surface 3c Chamfered surface 4 membrane

Claims

1. A magnetic disk substrate, The magnetic disk substrate is a disk-shaped substrate body that is an aluminum alloy substrate, the disk-shaped substrate body having two opposing main surfaces and an outer peripheral end surface, the outer peripheral end surface including a side wall surface and a chamfered surface formed between the main surfaces and the side wall surface; a film of an alloy containing Ni and P formed on a surface of the substrate body and continuously formed over the main surface, the chamfered surface and the side wall surface; The outer diameter of the disk-shaped substrate body is 90 mm or more, the thickness T of the magnetic disk substrate including the films provided on the two main surfaces is 0.520 mm or less; The total thickness D [mm] of the film provided on the two main surfaces and the thickness T [mm] satisfy the following formula (1), A magnetic disk substrate, wherein a maximum height Rz of surface roughness of the film formed on the outer peripheral end face is smaller than a maximum height Rz of surface roughness of the substrate body at the outer peripheral end face. D ≧ 0.0082 / T-0.0015 (1)

2. 2. The magnetic disk substrate according to claim 1, wherein the thickness of the film formed on the outer peripheral end face is 110% or more of the thickness of the film formed on the main surface.

3. 3. The magnetic disk substrate according to claim 1, wherein the thickness D [mm] and the thickness T [mm] satisfy the following formula (2): D ≧ 0.0094 / T (2)

4. 4. The magnetic disk substrate according to claim 1, wherein when an impact of 120 [G] is applied for 2 [msec] in a normal direction to the main surface while an inner peripheral portion of the magnetic disk substrate is fixed, the number of times that a displacement amount due to vibration in a plate thickness direction of an outer peripheral end portion of the magnetic disk substrate becomes 0.2 mm or more is 4 or less.

5. The Vickers hardness Hv of the film is 100 [kgf / mm 2 5. The magnetic disk substrate according to claim 1, wherein the thickness of the magnetic disk substrate is 100 nm or more.

6. 6. The magnetic disk substrate according to claim 1, wherein the magnetic disk substrate is for a hard disk drive device having 10 or more substrates mounted thereon.

7. A magnetic disk having at least a magnetic film on the surface of the magnetic disk substrate according to any one of claims 1 to 6.

8. 8. A hard disk drive device comprising the magnetic disk according to claim 7 and a magnetic head.

9. 9. The hard disk drive device according to claim 8, wherein the hard disk drive device comprises ten or more magnetic disks.

Citation Information

Patent Citations

  • Magnetic storage device and magnetic recording medium consisting of multi-layered magnetic layer

    JP1996212518A

  • Magnetic disk

    JP1997198640A

  • Substrate for magnetic disk

    JP1998334445A

  • Disk substrate for vertical magnetic recording medium, vertical magnetic recording medium using substrate and manufacturing method thereof

    JP2005322364A