Manganese zinc ferrite particles, temperature-sensitive magnetic fluid, and method for producing manganese zinc ferrite particles

By controlling the particle size and variation of manganese-zinc ferrite particles through a specific synthesis method, the magnetic properties and temperature sensitivity of magnetic fluids are enhanced, addressing the limitations of existing production methods.

JP7595865B2Active Publication Date: 2024-12-09ICHINEN CHEM CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021066878
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-04-16
Filing Date
2021-04-12
Publication Date
2024-12-09
Estimated Expiration
2041-04-12

AI Technical Summary

Technical Problem

Existing methods for producing manganese-zinc ferrite particles result in small average particle size and wide particle size distribution, leading to insufficient magnetic properties and temperature sensitivity in temperature-sensitive magnetic fluids.

Method used

Control the average particle size and coefficient of variation of manganese-zinc ferrite particles within specific ranges by using a method that includes mixing a suspension of iron oxyhydroxide, divalent manganese and zinc ions, and a base to form a gel-like mixture, maintaining solubility equilibrium, and adjusting pH and temperature conditions during synthesis.

Benefits of technology

The method produces manganese-zinc ferrite particles with improved saturation magnetization and temperature sensitivity, suitable for use in temperature-sensitive magnetic fluids for heat transport systems and cooling applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595865000009
    Figure 0007595865000009
  • Figure 0007595865000010
    Figure 0007595865000010
  • Figure 0007595865000011
    Figure 0007595865000011
Patent Text Reader

Abstract

To provide manganese zinc ferrite particles which can achieve the increase in saturation magnetization and the rise in thermosensitivity, a thermosensitive magnetic fluid, and a method of manufacturing such manganese zinc ferrite particles.SOLUTION: The manganese zinc ferrite particles are magnetic fine particles to be used for a thermosensitive magnetic fluid. Of the manganese zinc ferrite particles, the average particle diameter RT is 15 nm or more and 50 nm or less, which is determined by a transmission type electron microscope, and the fluctuation coefficient given by a standard deviation (nm) / average particle diameter RT(nm)×100 is 30% or less.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to manganese zinc ferrite particles, a temperature-sensitive magnetic fluid, and a method for producing manganese zinc ferrite particles, and more specifically, to manganese zinc ferrite particles used as magnetic microparticles in a temperature-sensitive magnetic fluid, a temperature-sensitive magnetic fluid containing manganese zinc ferrite particles, and a method for producing manganese zinc ferrite particles. [Background technology]

[0002] Conventionally, a thermal energy to kinetic energy conversion system using a thermosensitive magnetic fluid is known. A thermosensitive magnetic fluid that can be suitably used in such a conversion system and has an extremely sensitive change in magnetization in response to a change in temperature has been proposed (see Patent Document 1).

[0003] The ferromagnetic metal oxide particles in this magnetic fluid are obtained by a wet method and have the composition formula (MnO) X (ZnO) Y (Fe2O3) Z and characterized by a composition in the ranges of 0.35≦X≦0.47, 0.12≦Y≦0.24, 0.36≦Z≦0.46, and X+Y+Z=1. Furthermore, the ferromagnetic oxide particles are produced by a coprecipitation method in which the pH of the solution is set to 10 to 13 and the temperature of the solution is set to 80 to 100°C. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 1-165104 Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the coprecipitation method described in Patent Document 1, the reaction proceeds the moment the metal salt solution comes into contact with the sodium hydroxide aqueous solution, making it difficult to control the average particle size and particle size distribution of the ferromagnetic metal oxide microparticles. Therefore, such ferromagnetic metal oxide microparticles have a small average particle size and a wide particle size distribution. Therefore, the thermosensitive magnetic fluid using such ferromagnetic metal oxide microparticles still has the problem of insufficient magnetic properties such as saturation magnetization and thermosensitivity.

[0006] The present invention has been made in consideration of the problems associated with the conventional techniques, and aims to provide manganese zinc ferrite particles, temperature-sensitive magnetic fluids, and a method for producing manganese zinc ferrite particles that can increase saturation magnetization and improve temperature sensitivity. [Means for solving the problem]

[0007] As a result of extensive research into achieving the above-mentioned object, the inventors discovered that the above-mentioned object can be achieved by setting the average particle size and coefficient of variation of manganese zinc ferrite particles within a predetermined range, and thus completed the present invention.

[0008] The manganese zinc ferrite particles of the present invention are magnetic fine particles used in a temperature-sensitive magnetic fluid. The manganese zinc ferrite particles have an average particle size R T is 15 nm or more and 50 nm or less, and the standard deviation (nm) / average particle size R T The coefficient of variation, expressed as (nm) x 100, is 30% or less.

[0009] The temperature-sensitive magnetic fluid of the present invention is characterized by containing the above-mentioned manganese zinc ferrite particles as magnetic fine particles.

[0010] The method for producing manganese zinc ferrite particles of the present invention is a method for producing magnetic microparticles used in a temperature-sensitive magnetic fluid. The method for producing manganese zinc ferrite particles is characterized by including the following first and second steps. The first step is a step of mixing a suspension containing iron oxyhydroxide and water, an aqueous solution containing divalent manganese ions, divalent zinc ions, and water, and a base to obtain a gel-like mixed solution. The second step is a step of generating and growing manganese zinc ferrite particles in the gel-like mixed solution while maintaining the dissolution equilibrium between FeOOH and Fe(III) hydroxide. Effect of the Invention

[0011] According to the present invention, since the average particle size and coefficient of variation of the manganese zinc ferrite particles are within a predetermined range, it is possible to provide manganese zinc ferrite particles, a temperature-sensitive magnetic fluid, and a method for producing manganese zinc ferrite particles that can realize an increase in saturation magnetization and an improvement in temperature sensitivity. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is an explanatory view that illustrates a method for producing manganese zinc ferrite particles according to a third embodiment of the present invention. [Diagram 2] FIG. 2 is a transmission electron microscope image of an example (Test Example 1) of manganese zinc ferrite particles according to the first embodiment of the present invention. [Diagram 3] FIG. 3 is a transmission electron microscope image of an example of manganese zinc ferrite particles outside the present invention (Comparative Example 1). [Figure 4] FIG. 4 is a graph showing the magnetization curves of each example. [Diagram 5] FIG. 5 is a graph showing the thermomagnetic curves of each example. [Figure 6] FIG. 6 is a graph showing the relationship between the temperature and the derivative of the thermomagnetic curve for each example. [Figure 7] FIG. 7 is a graph showing the magnetization curves of each example. [Figure 8] FIG. 8 is a graph showing the thermomagnetic curves of each example in the absence of a magnetic field. [Figure 9] FIG. 9 is a graph showing the thermomagnetic curves of each example under a magnetic field. [Figure 10] FIG. 10 is a graph showing the relationship between the temperature and the derivative of the thermomagnetic curve for each example. [Figure 11] FIG. 11 is a graph showing the results of measuring the particle size and distribution of each example by dynamic light scattering. [Figure 12] FIG. 12 is a graph showing the magnetization curves of each example. [Figure 13] FIG. 13 is a graph showing the magnetization curves of each example. [Figure 14] FIG. 14 is a graph showing the relationship between the temperature and the derivative of the thermomagnetic curve for each example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, the manganese zinc ferrite particles, the temperature-sensitive magnetic fluid, and the method for producing the manganese zinc ferrite particles according to one embodiment of the present invention will be described in detail.

[0014] (First embodiment) First, a detailed description will be given of manganese zinc ferrite particles according to a first embodiment of the present invention. The manganese zinc ferrite particles of this embodiment are magnetic fine particles used in a temperature-sensitive magnetic fluid.

[0015] Here, it is preferable to use magnetic particles that exhibit a large decrease in magnetization with increasing temperature, particularly fine particles that exhibit superparamagnetism, as the magnetic particles used in the temperature-sensitive magnetic fluid. As such magnetic particles, it is particularly preferable to use manganese zinc ferrite particles.

[0016] Furthermore, the manganese zinc ferrite particles of the present embodiment have an average particle size R T is 15 nm or more and 50 nm or less, and the standard deviation (nm) / average particle size R T The coefficient of variation, expressed as (nm) x 100, is 30% or less.

[0017] Here, the average particle size RT " can be calculated as the arithmetic mean of the circle equivalent diameter of each particle when the obtained manganese zinc ferrite particles are observed by a transmission electron microscope (TEM). Also, the average particle diameter R T In calculating the average particle diameter R, for example, it is sufficient to measure the circle equivalent diameters of about 100 to 200 particles observed in 1 to 10 visual fields. T This can be calculated when calculating

[0018] The manganese zinc ferrite particles of the present embodiment have an average particle size R T and the coefficient of variation are within the above-mentioned ranges. It is considered that the manganese zinc ferrite particles of this embodiment can thereby realize an increase in saturation magnetization and an improvement in temperature sensitivity.

[0019] The mechanism of the increase in saturation magnetization and the improvement in temperature sensitivity in manganese zinc ferrite particles that is currently assumed will be described below.

[0020] The ratio of atoms located on the outermost surface of the particles increases as the particle size decreases. The atoms on the outermost surface of the particles do not have uniform spins and are sometimes called dead layers, so the saturation magnetization decreases relatively as the particle size decreases. Therefore, the average particle size R T It is believed that manganese zinc ferrite particles having a large value and a small coefficient of variation within the above-mentioned range can realize an increase in saturation magnetization and an improvement in temperature sensitivity.

[0021] However, it goes without saying that even if the above-mentioned effects are obtained by a mechanism other than the above-mentioned mechanism, it is still included in the scope of the present invention.

[0022] Furthermore, in the manganese zinc ferrite particles of this embodiment, from the viewpoint of increasing saturation magnetization and improving temperature sensitivity, the average particle size R T is preferably 15 nm or more and 45 nm or less, and the coefficient of variation is preferably 20% or less, and the average particle size R Tis more preferably 15 nm or more and 35 nm or less, and the coefficient of variation is 20% or less, and the average particle size R T More preferably, the average particle size R is 20 nm or more and 35 nm or less, and the coefficient of variation is 20% or less. T When is increased, the saturation magnetization near room temperature is increased and the temperature sensitivity in the low temperature range such as near room temperature is improved.

[0023] Furthermore, in the manganese zinc ferrite particles of this embodiment, from the viewpoint of increasing saturation magnetization and improving temperature sensitivity, the crystallite diameter R calculated by the Scherrer formula is S Average particle size R (nm) T The ratio of the average particle diameter R (nm) is preferably 1 or more and 1.8 or less, more preferably 1 or more and 1.6 or less, even more preferably 1 or more and 1.5 or less, and particularly preferably 1 or more and 1.3 or less. T / Crystallite diameter R S When the value of is small, the saturation magnetization near room temperature becomes large, and the temperature sensitivity improves in the low temperature range such as near room temperature.

[0024] Here, the crystallite size R S " can be calculated by obtaining an X-ray diffraction pattern of the obtained manganese zinc ferrite particles by powder X-ray diffraction (XRD) using Cu-Kα radiation, and determining the diffraction peak θ and half-width β. The Scherrer formula is S = Kλ / (βcosθ), where K = 0.94 and λ = 1.5418 Å.

[0025] Furthermore, in the manganese zinc ferrite particles of the present embodiment, from the viewpoint of easily obtaining single crystal manganese zinc ferrite particles, the molar ratio of the manganese content to the zinc content is preferably 1 / 9 or more and 9 / 1 or less, more preferably 1 / 9 or more and 7 / 3 or less. Note that, in the manganese zinc ferrite, when the ratio of the manganese content to the zinc content is more than 8 / 2, polycrystalline manganese zinc ferrite particles may be included.

[0026] Furthermore, in the manganese zinc ferrite particles of this embodiment, from the viewpoint of increasing saturation magnetization and improving temperature sensitivity, the ratio of manganese content to zinc content is preferably 6 / 4 or more and 7.5 / 2.5 or less in molar ratio.In manganese zinc ferrite, when the ratio of manganese content to zinc content is within the range of 6 / 4 or more and 7.5 / 2.5 or less in molar ratio, saturation magnetization increases with the increase in the ratio of manganese content.In addition, in manganese zinc ferrite, when the ratio of manganese content to zinc content is 8 / 2 or more in molar ratio, saturation magnetization may decrease.

[0027] Furthermore, in the manganese zinc ferrite particles of this embodiment, from the viewpoint of increasing saturation magnetization and improving temperature sensitivity, the crystallite diameter R S is preferably 10 nm or more, more preferably 12.4 nm or more, and further preferably 13.0 nm or more, and the crystallite size R S is preferably 35 nm or less, more preferably 32.0 nm or less, and even more preferably 25.0 nm or less.

[0028] In manganese zinc ferrite, as the ratio of manganese increases, the saturation magnetization increases and the Curie point increases. In addition, in manganese zinc ferrite, as the ratio of manganese increases, the temperature sensitivity improves. On the other hand, in manganese zinc ferrite, as the ratio of manganese decreases, the saturation magnetization decreases and the Curie point decreases. When an external magnetic field is applied to manganese zinc ferrite particles, the temperature at which magnetization disappears is about 300°C, regardless of the Curie point.

[0029] Second embodiment Next, a detailed description will be given of a temperature-sensitive magnetic fluid according to a second embodiment of the present invention. The temperature-sensitive magnetic fluid of this embodiment contains manganese zinc ferrite particles as the above-mentioned magnetic fine particles.

[0030] Since the temperature-sensitive magnetic fluid of this embodiment contains manganese zinc ferrite particles as the above-mentioned magnetic fine particles, it is believed that it can increase saturation magnetization and improve temperature sensitivity. The mechanism of the increase in saturation magnetization and the improvement in temperature sensitivity is believed to be as described above.

[0031] In the case of the thermosensitive magnetic fluid, the manganese zinc ferrite particles may be dispersed in a conventionally known organic solvent or water. In addition, in the case of the thermosensitive magnetic fluid, the surface of the manganese zinc ferrite particles may be coated with a conventionally known surfactant, if necessary.

[0032] The thermosensitive magnetic fluid of this embodiment can be used in a heat transport system that utilizes automobile waste heat. Furthermore, since the thermosensitive magnetic fluid of this embodiment has excellent temperature sensitivity in a low temperature range of 80°C or less, preferably 50°C or less, typically around room temperature, it can quickly respond when the temperature of the object to be cooled rises in a heat transport system intended to cool a CPU, power semiconductor, etc.

[0033] (Third embodiment) Next, the method for producing manganese zinc ferrite particles according to the third embodiment of the present invention will be described in detail. The method for producing manganese zinc ferrite particles according to this embodiment is the method for producing magnetic microparticles used in temperature-sensitive magnetic fluid, and is the suitable method for producing the manganese zinc ferrite particles according to the first embodiment described above.

[0034] The method for producing manganese zinc ferrite particles according to the present embodiment includes the following first and second steps. Each step will be described below.

[0035] In the first step, a suspension containing iron oxyhydroxide and water, an aqueous solution containing divalent manganese ions, divalent zinc ions and water, and a base are mixed to obtain a gel-like mixed liquid.

[0036] Here, the iron oxyhydroxide may be α-, β- or γ-FeOOH, but it is preferable to use β-FeOOH as the iron oxyhydroxide.

[0037] The divalent manganese ion source and the divalent zinc ion source are not particularly limited, but it is preferable to use manganese sulfate and zinc sulfate, respectively.

[0038] The base is not particularly limited, but it is preferable to use sodium hydroxide.

[0039] As the solvent, water can be used. A mixed solvent containing water as a solvent and 1-propyl alcohol, ethylene glycol, or dimethylacetamide (DMAc) as a solvent may also be used.

[0040] When the manganese ratio in the manganese zinc ferrite particles is high, Ostwald ripening is likely to occur. It is believed that Ostwald ripening occurs because manganese has a high solubility. Although not particularly limited, it is preferable to use a mixed solvent of water and dimethylacetamide (DMAc) from the viewpoint of suppressing Ostwald ripening. The concentration of dimethylacetamide (DMAc) in the mixed solvent is preferably 25 vol% or more and 50 vol% or less.

[0041] Furthermore, the ratio of the iron source, manganese source, and zinc source, Fe / (Mn+Zn), is preferably 2 / 1 from the viewpoint of the effort required to remove hydroxides, since particles obtained by adding an excess of divalent metal ions are not particularly superior. However, it is also possible to set the ratio to about 2 / 2 or even 2 / 3.

[0042] When Fe / (Mn+Zn) is greater than 2 / 1, β-FeOOH, a type of iron source, remains. Since β-FeOOH is a solid fine particle, it is necessary to separate the two in order to obtain only ferrite, which is not preferable. On the other hand, when Fe / (Mn+Zn) is less than 2 / 1, Mn(OH)2, and Zn(OH)2 remain. These hydroxides are easily dissolved in dilute acid, so if the solution is made acidic during centrifugal washing, ferrite can be obtained in a single phase.

[0043] For example, when Fe / (Mn+Zn) is set to 2 / 2, the Mn / Zn determined by X-ray fluorescence spectrometry (XRF) measurement of the obtained manganese zinc ferrite particles deviates from the Mn / Zn of the feed material. On the other hand, when Fe / (Mn+Zn) is set to 2 / 1, the Mn / Zn of the obtained manganese zinc ferrite particles matches the Mn / Zn of the feed material.

[0044] Furthermore, when Fe / (Mn+Zn) is set to 2 / 3, the ratio of Mn decreases, so zinc is absorbed into the ferrite at a faster rate. Also, since the particle size is almost constant and there is no change in the particle size distribution, it is believed that an excess of divalent metal ions does not affect the particle size.

[0045] The concentration of sodium hydroxide is not particularly limited, but is preferably 0.48 mol / L or more and 1.60 mol / L or less. If the sodium hydroxide concentration is less than 0.48 mol / L, even if manganese zinc ferrite particles are obtained, β-FeOOH is likely to remain. Also, if the sodium hydroxide concentration is higher than 1.60 mol / L, Ostwald ripening occurs, and the average particle size R T As the concentration of sodium hydroxide increases, coarse polycrystalline particles are generated, and the coefficient of variation tends to increase. Such coarse particles are undesirable because they precipitate during the preparation of the magnetic fluid. When the concentration of sodium hydroxide is 1.20 mol / L, the metal ion concentration is preferably 0.375 mol / L or more and 0.751 mol / L or less.

[0046] When the R value (R value = (NaOH concentration) / (iron ion concentration x 3 + manganese ion concentration x 2 + zinc ion concentration x 2)) is 3.20, the metal ion concentration is preferably 0.188 mol / L or more and 0.375 mol / L or less. When the R value is 1.28, the metal ion concentration is preferably 0.047 mol / L or more and 0.375 mol / L or less. Therefore, it is more preferable that the metal ion concentration is 0.188 mol / L or more and 0.375 mol / L or less.

[0047] When the ratio of the manganese content to the zinc content in the manganese zinc ferrite particles is set to 6 / 4 to 7.5 / 2.5 in molar ratio and the proportion of manganese is increased, the sodium hydroxide concentration is preferably 0.160 mol / L to 0.48 mol / L, the metal ion concentration is preferably 0.081 mol / L to 0.375 mol / L, and the R value is preferably 0.48 to 1.17. This makes it possible to obtain manganese zinc ferrite particles with a high manganese ratio, a narrow particle size distribution, and a large particle size.

[0048] The temperature during mixing is not particularly limited, but the temperatures of the suspension, aqueous solution, and base to be mixed, and further ion-exchanged water used as necessary, are preferably 0° C. or higher and 60° C. or lower. When mixed at 60° C., the coefficient of variation tends to be large, so the mixing temperature is preferably room temperature or lower.

[0049] Although not particularly limited, from the viewpoint of making it possible to further reduce the coefficient of variation, it is preferable to add the base after mixing the suspension and the aqueous solution.

[0050] In the second step, manganese zinc ferrite particles are generated and grown in the gel mixture while maintaining the dissolution equilibrium between FeOOH and Fe(III) hydroxide.

[0051] FIG. 1 is an explanatory diagram showing a schematic diagram of a method for producing manganese zinc ferrite particles according to a third embodiment of the present invention. As shown in FIG. 1, the water-insoluble β-FeOOH (3) contained in the gel-like mixed liquid (5) maintains a dissolution equilibrium with the water-soluble Fe (III) hydroxide, and uniformly supplies Fe (III) hydroxide to the divalent manganese ions and divalent zinc ions (not shown) contained in the gel-like mixed liquid (5). Then, the divalent manganese ions, divalent zinc ions, and Fe (III) hydroxide contained in the gel-like mixed liquid (5) react with each other to generate manganese zinc ferrite particles (1), and the particle size grows. Note that the coprecipitation method cannot realize such uniform supply of iron ions into the system.

[0052] Although not particularly limited, in the second step of the method for producing manganese zinc ferrite particles of this embodiment, from the viewpoint of easily producing manganese zinc ferrite particles with increased saturation magnetization and improved temperature sensitivity, it is preferable to leave the gelled mixture at a pH of 12.5 or higher at 80° C. or higher and 250° C. or lower for 30 minutes to 48 hours.

[0053] If the pH is less than 12.5, the production of manganese zinc ferrite particles stops midway, making it difficult to obtain manganese zinc ferrite particles quantitatively.

[0054] If the synthesis temperature is less than 80°C, the by-product α-FeOOH is likely to be produced. If the synthesis temperature is more than 150°C, an autoclave is required to prevent the water solvent from boiling. From these viewpoints, therefore, the synthesis temperature is more preferably 80°C or higher and 150°C or lower, and from the viewpoint of being able to synthesize in a simple container such as a Duran bottle, the synthesis temperature is preferably 80°C or higher and 100°C or lower. T / R S From the viewpoint of easiness in reducing the amount of ZnO, the synthesis temperature is preferably 100° C. or more and 200° C. or less.

[0055] If the reaction time is less than 30 minutes, it is difficult to quantitatively obtain manganese zinc ferrite particles. In addition, from the viewpoint that Ostwald ripening may occur due to excessive heating, the reaction time is preferably 48 hours or less. From these viewpoints, the reaction time is preferably 1 hour or more and 24 hours or less, more preferably 1 hour or more and 4 hours or less. EXAMPLES

[0056] The present invention will be described in more detail below with reference to test examples, but the present invention is not limited to these test examples.

[0057] (Test Example 1) <Preparation of β-FeOOH> Iron chloride hexahydrate was dissolved in ion-exchanged water to a concentration of 2.0 mol / L, and filtered through a hydrophilic polytetrafluoroethylene (PTFE) membrane filter with a pore size of 0.1 μm to prepare an aqueous solution. The same volume of 5.4 mol / L of sodium hydroxide (NaOH) aqueous solution was added to the obtained iron chloride aqueous solution while stirring to obtain a mixed solution with a pH of 2. After adding the sodium hydroxide (NaOH) aqueous solution, the mixture was stirred for 10 minutes, transferred to a Duran bottle, sealed, transferred to an oven at 100 ° C, and left to stand for 6 hours to obtain a gel-like acidic solution consisting of β-FeOOH. After cooling with running water, the mixture was purified by centrifugal washing with ion-exchanged water. Finally, the precipitate obtained by centrifugation was dispersed in ion-exchanged water, and the pH was adjusted to 3 by adding hydrochloric acid, obtaining a low-viscosity aqueous dispersion consisting of β-FeOOH. The dispersion concentration of β-FeOOH was determined from the solid weight obtained by drying 2 ml of β-FeOOH dispersion at 100 ° C, and used to prepare manganese zinc ferrite particles.

[0058] <Preparation of manganese zinc ferrite particles> 490.0 mmol of manganese sulfate pentahydrate and 219.5 mmol of zinc sulfate heptahydrate were dissolved in ion-exchanged water, and the resulting solution was adjusted to 100 mL using a measuring flask to prepare a manganese-zinc stock solution with Mn = 1.30 mol / L and Zn = 0.70 mol / L. At room temperature, the β-FeOOH dispersion was transferred to a 100 ml perfluoroalkoxyalkane (PFA) bottle with Fe=12.5 mmol, and ion-exchanged water was added to prepare a 15 ml volume. Then, 3.13 ml of manganese zinc stock solution was added and stirred (Fe / Mn / Zn=2.00 / 0.65 / 0.35). At this time, β-FeOOH precipitated by salting out, and became a gel-like solution with high viscosity. Furthermore, 3.0 ml of 8 mol / L sodium hydroxide (NaOH) aqueous solution was added, stirred, and then adjusted to 50 ml with ion-exchanged water using a measuring flask. At this time, the concentrations are Fe=0.250 mol / L, Mn=0.081 mol / L, Zn=0.044 mol / L, and NaOH=0.480 mol / L, respectively. Finally, the bottle was returned to a 100 ml perfluoroalkoxyalkane (PFA) bottle, sealed, and placed in a 100 ° C oven and left to stand for 2 hours. After cooling with running water, purification was performed by centrifugal washing with ion-exchanged water. Finally, the precipitate was dried at 55°C to obtain the manganese zinc ferrite particle powder (R S :21.5nm, R T : 30.5 nm, standard deviation: 5.0 nm, coefficient of variation: 16.4%, R T / R S 2 is a transmission electron microscope image of the manganese zinc ferrite particles of Test Example 1.

[0059] Crystallite diameter R S was calculated by obtaining the X-ray diffraction pattern of the obtained manganese zinc ferrite particles by powder X-ray diffraction (XRD) using Cu-Kα radiation, and determining the diffraction peak θ and half-width β. The Scherrer equation is S =Kλ / (βcosθ), where K=0.94 and λ=1.5418 Å.

[0060] Average particle size R T was calculated as the arithmetic mean of the circle equivalent diameter of each particle when the obtained manganese zinc ferrite particles were observed by a transmission electron microscope (TEM). TWhen calculating, for example, the circular equivalent diameters of about 200 particles observed in one field of view were measured. The standard deviation and coefficient of variation are the average particle size R T Some of the specifications of this example are shown in Table 1.

[0061] (Test Examples 2 to 10) In the manganese zinc ferrite particle production process, the same operations as in Test Example 1 were repeated except that the sodium hydroxide (NaOH) concentration, metal ion concentration, R value, and Mn / Zn were changed, and manganese zinc ferrite particle powders of each example were obtained. Test Examples 5 and 6 further differ from Test Example 1 in that the obtained β-FeOOH was directly used for the production of manganese zinc ferrite particles without being washed.

[0062] The mass magnetization (saturation magnetization) at each temperature (25°C and 100°C) was determined by sealing the sample in a copper capsule and measuring the magnetization curve with a vibrating sample magnetometer (VMS). The Curie temperature was also measured by sealing the sample in a copper capsule and using a vibrating sample magnetometer (VMS). Table 1 shows some of the specifications for each example.

[0063] [Table 1]

[0064] As Comparative Example 1 in Table 1, magnetic fine particles contained in a temperature-sensitive magnetic fluid (Ferricolloid, TS-50K, manufactured by Ichinen Chemicals Co., Ltd.) were used. FIG. 3 is a transmission electron microscope image of the manganese zinc ferrite particles of Comparative Example 1.

[0065] (Test Examples 11 to 14) In the manganese zinc ferrite particle production process, the same operation as in Test Example 1 was repeated except that the Mn / Zn ratio was changed to obtain powders of manganese zinc ferrite particles of each example. Table 2 shows some of the specifications of each example.

[0066] [Table 2]

[0067] (Test Examples 15 and 16) In the manganese zinc ferrite particle preparation process, a mixed solvent of water and dimethylacetamide was used as the solvent, and the Mn / Zn ratio was changed, but the same procedure as in Test Example 1 was repeated to obtain manganese zinc ferrite particle powders of each example. Table 3 shows some of the specifications of each example.

[0068] [Table 3]

[0069] (Test Examples 17 and 18) In the manganese zinc ferrite particle production process, the same operations as in Test Example 1 were repeated except that the sodium hydroxide (NaOH) concentration, R value, and Mn / Zn were changed, to obtain powders of manganese zinc ferrite particles for each example.

[0070] (Test Examples 19 to 22) In the manganese zinc ferrite particle preparation process, the same operations as in Test Example 1 were repeated except that the sodium hydroxide (NaOH) concentration, metal ion concentration, and R value were changed, to obtain powders of manganese zinc ferrite particles for each example.

[0071] (Test Examples 23 to 25) In the manganese zinc ferrite particle preparation process, the same operations as in Test Example 1 were repeated except that the sodium hydroxide (NaOH) concentration, metal ion concentration, R value, and Mn / Zn were changed to obtain manganese zinc ferrite particle powders of each example. Table 4 shows some of the specifications of each example.

[0072] [Table 4]

[0073] (Test Examples 26 to 28) In the manganese zinc ferrite particle production process, the same operation as in Test Example 1 was repeated except that the synthesis temperature was changed and 15 ml was added to a 20 ml Teflon (registered trademark) inner cylinder after preparing 50 ml in a measuring flask, to obtain manganese zinc ferrite particle powder of each example. Table 5 shows some of the specifications of each example.

[0074] [Table 5]

[0075] (Test Example 29, Test Example 30) In the manganese zinc ferrite particle preparation process, the same operations as in Test Example 1 were repeated except that Fe / (Mn+Zn), sodium hydroxide (NaOH) concentration, and metal ion concentration were changed to obtain manganese zinc ferrite particle powders of each example. Table 6 shows some of the specifications of each example.

[0076] [Table 6]

[0077] (Test Examples 31 to 34) In the manganese zinc ferrite particle preparation process, the same operations as in Test Example 1 were repeated except that the sodium hydroxide (NaOH) concentration, R value, mixing temperature, and Mn / Zn were changed to obtain manganese zinc ferrite particle powders of each example. Table 7 shows some of the specifications of each example.

[0078] [Table 7]

[0079] (Test Example 35) The same operations as in Test Example 1 were repeated, except that the obtained β-FeOOH was not washed and was directly used for the production of manganese zinc ferrite particles, thereby obtaining a powder of manganese zinc ferrite particles of this example.

[0080] (Test Examples 36 to 38) In the manganese zinc ferrite particle preparation process, the same operations as in Test Example 1 were repeated except that the sodium hydroxide (NaOH) concentration, R value, mixing temperature, and Mn / Zn were changed to obtain manganese zinc ferrite particle powders of each example. Table 8 shows some of the specifications of each example.

[0081] [Table 8]

[0082] From Table 1, the manganese zinc ferrite particles of Test Examples 1 to 4, which fall within the scope of the present invention, have an average particle size R T In contrast, in the manganese zinc ferrite particles of Comparative Example 1, which is not the present invention, the average particle size R T It can be seen that the average particle size R within the specified range in Test Examples 1 to 4 and the coefficient of variation are not within the specified range. T It is believed that the reason why manganese zinc ferrite particles having the above-mentioned coefficient of variation was obtained is that they were produced by the production method using the above-mentioned specific gel-like mixed liquid.

[0083] Here, Fig. 4 is a graph showing magnetization curves of Test Example 5, Test Example 6, and Comparative Example 1. Fig. 5 is a graph showing thermomagnetic curves of Test Example 5, Test Example 6, and Comparative Example 1. Fig. 6 is a graph showing the relationship between temperature and the derivative of the thermomagnetic curve of Test Example 5, Test Example 6, and Comparative Example 1. From Figs. 4 to 6, it can be seen that the saturation magnetization at room temperature increases with increasing particle size. It can also be seen that the temperature sensitivity (slope) in the low temperature range improves.

[0084] Fig. 7 is a graph showing magnetization curves of Test Examples 7 to 10. Fig. 8 is a graph showing thermomagnetic curves in the absence of a magnetic field of Test Examples 7 to 10. It can be seen from Figs. 7 and 8 that as the ratio of manganese in the manganese zinc ferrite particles increases, the saturation magnetization increases and the Curie point increases.

[0085] Fig. 9 is a graph showing the thermomagnetic curves of Test Example 5, Test Example 6, Test Example 10, and Comparative Example 1 under a magnetic field. Fig. 10 is a graph showing the relationship between the temperature and the derivative of the thermomagnetic curve of Test Example 5, Test Example 6, Test Example 10, and Comparative Example 1. Figs. 9 and 10 show that when a magnetic field is applied, the temperature at which magnetization disappears is about 330°C, regardless of the Curie point. It is also shown that the temperature sensitivity improves with an increase in the proportion of manganese in the manganese zinc ferrite particles.

[0086] 11 is a graph showing the results of measuring particle size and distribution by dynamic light scattering in Test Example 9 and Comparative Example 1. Note that Comparative Example 1 here is TS-50K diluted 10 times. The scattering intensity distribution in Test Example 9 is 23.6±9.1 nm, and the scattering intensity distribution in Comparative Example 1 is 48.3±16.9 nm.

[0087] Test Example 9 will be described in detail below. Once the manganese zinc ferrite particles that have not been surface-modified are dried, it is difficult to completely redisperse them. Therefore, manganese zinc ferrite particles were synthesized, purified by centrifugal washing, and then redispersed in a solvent without drying the precipitate, and used for a dispersion experiment. First, after dispersing the manganese zinc ferrite particles, the dispersion was left to stand on a magnet, and magnetic purification was performed to remove particles that remained precipitated even after removing the magnet. Although it is possible to disperse the obtained particles in a hydrophobic solvent such as oleic acid, a high proportion of particles precipitated by magnetic purification was used as a surfactant that can more stably disperse the particles.

[0088] The surface modification method using a surfactant is described in detail below. The pH of an aqueous dispersion of manganese zinc ferrite particles (100 mg / mL) was adjusted to 4, and the particles were dispersed by ultrasonic irradiation. Next, the same volume of a methanol solution of stearyl gallate (100 mg / mL) was added under ultrasonic irradiation. Then, ultrasonic irradiation was performed for another hour to perform surface modification. After the reaction, the particles were centrifuged and washed with methanol to remove unadsorbed stearyl gallate, and purified. Xylene was added to the obtained precipitate so that the particle dispersion concentration was 10 mass%, and the particles were dispersed. Finally, magnetic purification was performed, and the dispersion concentration and dispersion yield were examined, and they were 3.4 mass% and 24%, respectively.

[0089] From the measurement results of Comparative Example 1, the average particle size R T 11, it was found that no aggregates were present in Test Example 9 and the particles were stably dispersed. In other words, it is believed that the particles in Test Example 9 were dispersed in the form of primary particles.

[0090] From Tables 2 to 7, the manganese zinc ferrite particles of Test Examples 11 to 34, which fall within the scope of the present invention, also have an average particle size R T It can be seen that the average particle size R within the predetermined range in Test Examples 11 to 34. T It is believed that the reason why manganese zinc ferrite particles having the above-mentioned coefficient of variation was obtained is that they were produced by the production method using the above-mentioned specific gel-like mixed liquid.

[0091] Fig. 12 is a graph showing the magnetization curves of Test Example 1 and Test Example 35. From Fig. 12, it can be seen that although the saturation magnetization of Test Example 1 is larger than that of Test Example 35, the opening of the loop near zero magnetic field of Test Example 1 is smaller than that of Test Example 35. This is considered to be because the particle size distribution of Test Example 1 is narrower than that of Test Example 35, and therefore the proportion of coarse particles having spontaneous magnetization is reduced. From the viewpoint of particle dispersibility in the temperature-sensitive magnetic fluid, Test Example 1 is considered to be more advantageous than Test Example 35.

[0092] Fig. 13 is a graph showing the magnetization curves of Test Example 1 and Test Example 35. It is believed that the magnetic susceptibility improved by narrowing the particle distribution because the proportion of particles with small diameters was reduced. From the viewpoint of eliminating the need to use strong magnets when designing a heat transport system using a temperature-sensitive magnetic fluid, Test Example 1 is considered to be more advantageous than Test Example 35. The temperature-sensitive magnetic fluid using the manganese zinc ferrite particles of Test Example 1 can increase the design freedom of the heat transport system.

[0093] Fig. 14 is a graph showing the relationship between temperature and the derivative of the thermomagnetic curve in Test Example 1 and Comparative Example 1. From Fig. 14, it can be seen that excellent temperature sensitivity is exhibited in the low temperature range of 80°C or less. Furthermore, from Table 8, it can be seen that when the ratio of the manganese content to the zinc content is 6 / 4 or more and 7.5 / 2.5 or less in molar ratio, the temperature sensitivity is almost the same as when it is 6.5 / 3.5. From these, it can be seen that Test Examples 36 to 38 also exhibit excellent temperature sensitivity in the low temperature range of 80°C or less, like Test Example 1.

[0094] Although the present invention has been described above with reference to some embodiments and test examples, the present invention is not limited to these, and various modifications are possible within the scope of the gist of the present invention. [Explanation of symbols]

[0095] 1 Manganese zinc ferrite particles 3 β-FeOOH 5. Gel-like mixture

Claims

1. A magnetic microparticle for use in a temperature-sensitive magnetic fluid, comprising: Average particle size R determined by transmission electron microscope T is 15 nm or more and 50 nm or less, Standard deviation (nm) / Above average particle size R T The coefficient of variation, expressed as (nm) x 100, is 30% or less.

3. Manganese zinc ferrite particles comprising:

2. The average particle size R T is 15 nm or more and 35 nm or less, The coefficient of variation is 20% or less.

2. The manganese zinc ferrite particle of claim 1 .

3. Crystallite diameter R calculated by Scherrer formula S (nm) to the average particle size R T 3. The manganese zinc ferrite particle according to claim 1, characterized in that the ratio of (nm) is 1 or more and 1.8 or less.

4. The manganese zinc ferrite particles according to any one of claims 1 to 3, characterized in that the ratio of the manganese content to the zinc content is 1 / 9 or more and 9 / 1 or less in molar ratio.

5. The manganese zinc ferrite particles according to any one of claims 1 to 4, characterized in that the ratio of the manganese content to the zinc content is 6 / 4 or more and 7.5 / 2.5 or less in molar ratio.

6. A temperature-sensitive magnetic fluid comprising manganese zinc ferrite particles as magnetic fine particles according to any one of claims 1 to 5.

7. A method for producing magnetic microparticles for use in a temperature-sensitive magnetic fluid, comprising the steps of: a first step of mixing a suspension containing iron oxyhydroxide and water, an aqueous solution containing divalent manganese ions, divalent zinc ions and water, and a base to obtain a gel-like mixed solution; A second step of generating and growing manganese zinc ferrite particles in the gel mixture while maintaining a dissolution equilibrium between FeOOH and Fe(III) hydroxide. A method for producing manganese zinc ferrite particles, comprising:

8. The method for producing manganese zinc ferrite particles according to claim 7, characterized in that in the second step, the gel-like mixture is allowed to stand at 80°C or higher and 250°C or lower for 30 minutes to 48 hours in a state where the pH of the gel-like mixture is 12.5 or higher.

Citation Information

Patent Citations

  • Magnetic fluid

    JP1989165104A

  • Black magnetic fluid

    JP1990130902A

  • Magnetic composite material and manufacture thereof

    JP1993175031A

  • Method for producing ferrite powder

    JP1995267645A

  • Iron compound particle, method for producing the same, and oxidation catalyst using the same

    JP2017119615A