Propylene polymer composition and film
A propylene polymer composition with defined propylene and propylene-α-olefin copolymer ratios addresses blocking issues in heat-sealable films, ensuring low-temperature heat-sealability and improved film processing.
Patent Information
- Application Number
- JP2020195378
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-25
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2040-11-25
AI Technical Summary
Films with heat-sealing layers that can be heat-sealed at low temperatures experience blocking issues, making them difficult to process smoothly when wound or stacked.
A propylene polymer composition containing specific proportions of propylene polymer and propylene-α-olefin copolymer, formulated to meet certain elution fractionation criteria, which enhances heat-sealability at low temperatures while preventing blocking.
The composition allows for heat-sealing at relatively low temperatures while significantly reducing blocking, maintaining film processability and improving mechanical properties.
Smart Images

Figure 0007596127000005 
Figure 0007596127000001 
Figure 0007596127000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a propylene polymer composition comprising a propylene polymer, and a film containing the propylene polymer composition. [Background technology]
[0002] As a film used as various packaging materials, one having a base layer and a heat seal layer laminated on the base layer is known. For example, a film using various biaxially oriented films as the base layer and a polypropylene-based biaxially oriented film or a non-oriented film as the heat seal layer is known. Films of such a configuration are widely used as materials for forming various packaging bags. When forming a packaging bag using such a film (performing a bag making process), the ends of the film are overlapped so that the heat seal layers face each other, and the ends are heated and heat sealed to form a packaging bag. This makes it possible to form a sealed packaging bag.
[0003] In recent years, the speed of bag making has been increased and the heating time for heat sealing has been shortened, so that there is a demand for a material capable of forming a heat seal layer that can be heat sealed at a relatively low temperature. For example, Patent Document 1 discloses that a propylene-based copolymer obtained by carrying out a first step of obtaining a copolymer component (A) of a specific propylene and ethylene and / or a specific α-olefin, and a second step of obtaining a copolymer component (B) of a specific propylene and ethylene and / or a specific α-olefin in the presence of the copolymer component (A) can form a heat seal layer that can be heat sealed at a relatively low temperature. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2002-69143 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, when a film having a heat seal layer that can be heat sealed at a relatively low temperature as described above is wound into a roll or stacked in a sheet, the films may become difficult to peel from each other or may have poor sliding properties against each other, which is called blocking. If such blocking occurs, it becomes difficult to smoothly process the film thereafter.
[0006] Therefore, an object of the present invention is to provide a propylene polymer composition that can form a heat sealable layer that can be heat sealed at a relatively low temperature and can suppress the occurrence of blocking in a film having the heat seal layer, and a film containing the propylene polymer composition. [Means for solving the problem]
[0007] The propylene polymer composition according to the present invention comprises: The present invention relates to a propylene polymer (1) and a propylene-α-olefin copolymer (2), the content of the propylene polymer (1) is 2% by mass to 25% by mass relative to 100% by mass of the total content of the propylene polymer (1) and the propylene-α-olefin copolymer (2); A propylene polymer composition satisfying the following requirement (3): Propylene polymer (1): A polymer containing 94% by mass or more of monomer units derived from propylene. Propylene-α-olefin copolymer (2): A copolymer comprising 60% by mass or more and less than 94% by mass of monomer units derived from propylene, and more than 6% by mass and 40% by mass or less of monomer units derived from an α-olefin having 4 to 12 carbon atoms. Requirement (3): In a temperature rising elution fractionation method using orthodichlorobenzene as a solvent in the temperature range of 0°C to 140°C, the following formula (3-1) is satisfied. Wb≦-1.79×Th+150 (3-1) (In the formula, Wb indicates the cumulative amount of elution from 0°C to 50°C. Th indicates the temperature (°C) between 0°C and 80°C or between 110°C and 140°C at which the cumulative amount of elution is 65% by mass, assuming that the sum of the cumulative amount of elution between 0°C and 80°C and the cumulative amount of elution between 110°C and 140°C is 100% by mass.)
[0008] The film according to the present invention contains the above propylene polymer composition. Effect of the Invention
[0009] According to the present invention, it is possible to provide a propylene polymer composition that can form a heat sealable layer that can be heat sealed at a relatively low temperature and can suppress the occurrence of blocking in a film having the heat seal layer, and a film containing the propylene polymer composition. [Brief description of the drawings]
[0010] [Figure 1] 1A is a graph showing the test results of [Example], and FIG. 1B is another graph showing the test results of [Example]. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The propylene polymer composition according to the present invention contains a propylene polymer (1) and a propylene-α-olefin copolymer (2). Such a propylene polymer composition can be obtained by carrying out a first step of obtaining a propylene polymer (1) and a second step of obtaining a propylene-α-olefin copolymer (2) in the presence of the propylene polymer (1).
[0012] The propylene polymer composition according to the present invention has a content of the propylene polymer (1) of 2 to 25% by mass, preferably 3 to 20% by mass, and more preferably 4 to 15% by mass, based on 100% by mass of the total content of the propylene polymer (1) and the propylene-α-olefin copolymer (2). The propylene polymer composition according to the present invention has a content of the propylene-α-olefin copolymer (2) of preferably 75 to 98% by mass, more preferably 80 to 97% by mass, and even more preferably 85 to 96% by mass, based on 100% by mass of the total content of the propylene polymer (1) and the propylene-α-olefin copolymer (2).
[0013] When the content of the propylene polymer (1) is 2% by mass or more (i.e., when the content of the propylene-α-olefin copolymer (2) is 98% by mass or less), the blocking resistance of the film (hereinafter, also simply referred to as "film") formed using the propylene polymer composition according to the present invention is improved while maintaining the heat sealability. Also, when the content of the propylene polymer (1) is 25% by mass or less (i.e., when the content of the propylene-α-olefin copolymer (2) is 75% by mass or more), the heat sealability of the film at low temperatures is improved.
[0014] <Propylene polymer (1)> The propylene polymer (1) contains 94% by mass or more, preferably 95% by mass or more, more preferably 96% by mass or more of monomer units derived from propylene. When the monomer units derived from propylene are 94% by mass or more, the blocking resistance of the film is improved. The propylene polymer (1) may be a copolymer containing monomer units derived from ethylene and / or monomer units derived from an α-olefin having 4 to 12 carbon atoms.
[0015] The propylene polymer (1) may contain less than 6 mass%, less than 5 mass%, or less than 4 mass% of monomer units derived from ethylene. When the monomer units derived from ethylene are less than 6 mass%, the heat sealability of the film at low temperatures is improved, and the blocking resistance of the film is also improved.
[0016] Furthermore, the propylene polymer (1) may contain less than 6% by mass, less than 5% by mass, or less than 4% by mass of monomer units derived from an α-olefin having 4 to 12 carbon atoms. When the monomer units derived from an α-olefin having 4 to 12 carbon atoms are less than 6% by mass, there is an effect of improving the heat sealability of the film at low temperatures, and also an effect of improving the blocking resistance of the film.
[0017] Examples of the monomer units derived from an α-olefin having 4 to 12 carbon atoms in the propylene polymer (1) include 1-butene, 2-methyl-1-propene, 1-pentene, 2-methyl-1-butene, 3-methyl-1-butene, 1-hexene, 2-ethyl-1-butene, 2,3-dimethyl-1-butene, 2-methyl-1-pentene, 3-methyl-1-pentene, 4-methyl-1-pentene, 3,3-dimethyl-1-butene, 1-heptene, methyl-1-hexene, dimethyl-1-pentene, ethyl-1-pentene, trimethyl-1-butene, methylethyl-1-butene, 1-octene, Examples of monomer units include those derived from methyl-1-pentene, ethyl-1-hexene, dimethyl-1-hexene, propyl-1-heptene, methylethyl-1-heptene, trimethyl-1-pentene, propyl-1-pentene, diethyl-1-butene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, and the like. Preferred are monomer units derived from 1-butene, 1-pentene, 1-hexene, and 1-octene. From the viewpoints of copolymerization characteristics, economic efficiency, and the like, more preferred are monomer units derived from 1-butene and 1-hexene, and even more preferred are monomer units derived from 1-butene.
[0018] Examples of the propylene polymer (1) include a propylene homopolymer, a propylene-ethylene copolymer, a propylene-1-butene copolymer, a propylene-1-hexene copolymer, a propylene-ethylene-1-butene copolymer, a propylene-ethylene-1-hexene copolymer, and the like. Of these, a propylene homopolymer and a propylene-ethylene copolymer are preferred, and a propylene homopolymer is more preferred.
[0019] <Propylene-α-olefin copolymer (2)> The propylene-α-olefin copolymer (2) contains 60% by mass or more and less than 94% by mass, preferably 70% to 92% by mass, and more preferably 75% to 90% by mass or less of monomer units derived from propylene. When the monomer units derived from propylene are 60% by mass or more, the blocking resistance of the film is improved. When the monomer units derived from propylene are less than 94% by mass, the heat sealability of the film at low temperatures is improved.
[0020] The propylene-α-olefin copolymer (2) contains more than 6% by mass and not more than 40% by mass, preferably 8% to 30% by mass, and more preferably 10% to 25% by mass of monomer units derived from an α-olefin having 4 to 12 carbon atoms. When the monomer units derived from an α-olefin having 4 to 12 carbon atoms are more than 6% by mass, the heat sealability of the film at low temperatures is improved. When the monomer units derived from an α-olefin having 4 to 12 carbon atoms are not more than 40% by mass, the blocking resistance of the film is improved.
[0021] Examples of the monomer units derived from an α-olefin having 4 to 12 carbon atoms in the propylene-α-olefin copolymer (2) include 1-butene, 2-methyl-1-propene, 1-pentene, 2-methyl-1-butene, 3-methyl-1-butene, 1-hexene, 2-ethyl-1-butene, 2,3-dimethyl-1-butene, 2-methyl-1-pentene, 3-methyl-1-pentene, 4-methyl-1-pentene, 3,3-dimethyl-1-butene, 1-heptene, methyl-1-hexene, dimethyl-1-pentene, ethyl-1-pentene, trimethyl-1-butene, methylethyl-1-butene, 1-oct ... Examples of monomer units include those derived from 1-butene, 1-pentene, ethyl-1-hexene, dimethyl-1-hexene, propyl-1-heptene, methylethyl-1-heptene, trimethyl-1-pentene, propyl-1-pentene, diethyl-1-butene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, and the like. Of these, monomer units derived from 1-butene, 1-pentene, 1-hexene, and 1-octene are preferred, and from the viewpoints of copolymerization characteristics, economic efficiency, and the like, monomer units derived from 1-butene and 1-hexene are more preferred, and monomer units derived from 1-butene are even more preferred.
[0022] The propylene-α-olefin copolymer (2) may further contain 2% by mass to 6% by mass, or 3% by mass to 5% by mass, of monomer units derived from ethylene. When the monomer units derived from ethylene are 2% by mass or more, the effect of improving the heat sealability of the film at low temperatures is achieved. When the monomer units derived from ethylene are 6% by mass or less, the effect of improving the blocking resistance of the film is achieved.
[0023] Examples of the propylene-α-olefin copolymer (2) include a propylene-1-butene copolymer, a propylene-1-hexene copolymer, a propylene-ethylene-1-butene copolymer, a propylene-ethylene-1-hexene copolymer, and the like. Of these, a propylene-1-butene copolymer and a propylene-1-hexene copolymer are preferred, and a propylene-1-butene copolymer is more preferred.
[0024] The melt flow rate (hereinafter, also referred to as MFR) of the propylene polymer composition according to the present invention measured at 230°C is not particularly limited, and is preferably 1 g / 10 min to 50 g / 10 min, and more preferably 3 g / 10 min to 10 g / 10 min. When the MFR is within the above range, the flowability and film formability during molding of the propylene polymer composition are good. Examples of a method for adjusting the MFR include a method of melt-kneading the propylene polymer composition with an organic peroxide. In the present invention, the MFR can be determined by the method described in the following Examples.
[0025] The propylene polymer composition according to the present invention satisfies the following requirement (3). Requirement (3): In a temperature rising elution fractionation method using orthodichlorobenzene as a solvent in the temperature range of 0°C to 140°C, the following formula (3-1) is satisfied. Wb≦-1.79×Th+150 (3-1) (In the formula, Wb indicates the cumulative amount of elution from 0°C to 50°C. Th indicates the temperature (°C) between 0°C and 80°C or between 110°C and 140°C at which the cumulative amount of elution is 65% by mass, assuming that the sum of the cumulative amount of elution between 0°C and 80°C and the cumulative amount of elution between 110°C and 140°C is 100% by mass.) In addition, Wb and Th in the above formula (3-1) can be adjusted by selecting the median particle size of the solid catalyst component for olefin polymerization described later. For example, by setting the median particle size of the solid catalyst component for olefin polymerization to 60 μm or less, Wb becomes small and Th becomes large, by setting it to 20 to 50 μm, Wb becomes small and Th becomes large, and by setting it to 30 to 40 μm, Wb becomes small and Th becomes large. In addition, Wb and Th in the above formula (3-1) can also be adjusted by selecting an external electron donor, which will be described later. For example, by using an alkoxysilane having a cyclic hydrocarbon group, such as cyclohexylethyldimethoxysilane, as the external electron donor, Wb becomes smaller and Th becomes larger. Furthermore, Wb in the above formula (3-1) can also be adjusted by the content of monomer units derived from other than propylene contained in the propylene polymer (1) and the propylene-α-olefin copolymer (2). For example, Wb increases by increasing the content of monomer units derived from other than propylene. Furthermore, Th in the above formula (3-1) can also be adjusted by the content of the propylene polymer (1). For example, Th increases as the content of the propylene polymer (1) increases. Here, "Wb" and "Th" in the above formula (3-1) can be specifically determined by the method described in the following [Examples].
[0026] <Production of Propylene Polymer Composition> The production of the propylene polymer composition according to the present invention can be carried out by multi-stage polymerization comprising a first step and a second step and subsequent steps, using an olefin polymerization catalyst.
[0027] <Olefin polymerization catalyst> The olefin polymerization catalyst can be produced by contacting a solid catalyst component for olefin polymerization with an organoaluminum compound and an external electron donor. Thus, the olefin polymerization catalyst comprises a solid catalyst component for olefin polymerization, an organoaluminum compound and an external electron donor.
[0028] <Solid catalyst component for olefin polymerization> The solid catalyst component for olefin polymerization comprises a titanium atom, a magnesium atom, a halogen atom and an internal electron donor.
[0029] The solid catalyst component for olefin polymerization means a component which exists as a solid content at least in toluene and constitutes an olefin polymerization catalyst by being combined with an organoaluminum compound and an external electron donor.
[0030] A part or all of the titanium atoms in the solid catalyst component for olefin polymerization are derived from a titanium halide compound. A part or all of the halogen atoms in the solid catalyst component for olefin polymerization are derived from a titanium halide compound.
[0031] Examples of the titanium halide compound include titanium tetrahalide, monoalkoxy titanium trihalide, dialkoxy titanium dihalide, and trialkoxy titanium monohalide, and preferably titanium tetrahalide or monoalkoxy titanium trihalide, and more preferably titanium tetrahalide. The titanium halide compound may be used alone or in combination of two or more kinds.
[0032] A part or all of the magnesium atoms in the solid catalyst component for olefin polymerization are derived from a magnesium compound, and a part of the halogen atoms in the solid catalyst component for olefin polymerization may be derived from a magnesium compound.
[0033] The magnesium compound includes dialkylmagnesium, magnesium dialkoxide, alkylmagnesium halide, alkoxymagnesium halide, aryloxymagnesium halide, and magnesium halide, and is preferably a magnesium halide or magnesium dialkoxide.
[0034] The magnesium compounds may be used alone or in combination of two or more kinds.
[0035] The internal electron donor refers to an organic compound capable of donating an electron pair to one or more metal atoms contained in the solid catalyst component for olefin polymerization. Specific examples of the internal electron donor include monoester compounds, dicarboxylate compounds, diol diester compounds, β-alkoxyester compounds, and diether compounds.
[0036] The monoester compound means an organic compound having one ester bond (-CO-O-) in the molecule, and is preferably an aromatic carboxylate compound or an aliphatic carboxylate compound.
[0037] The dicarboxylate compound means a compound having two ester bonds (-CO-O-) in the molecule and having a structure in which two carboxyl groups of a dicarboxylate are esterified with a monohydric alcohol, and an aromatic dicarboxylate compound and an aliphatic dicarboxylate compound are preferred.
[0038] The diol diester compound means a compound having two ester bonds (-CO-O-) in the molecule, and having a structure in which each of the two hydroxyl groups of a diol esterifies a carboxyl group of a monocarboxylic acid or dicarboxylic acid.
[0039] The β-alkoxy ester compound means a compound having an alkoxycarbonyl group and an alkoxy group at the β-position of the alkoxycarbonyl group.
[0040] The diether compound means a compound having two ether bonds in the molecule.
[0041] Further, the internal electron donors described in JP-A-2011-246699 can also be exemplified.
[0042] Among the above internal electron donors, a dicarboxylic acid ester compound, a diol diester compound, or a β-alkoxy ester compound is preferable. The internal electron donors may be used alone or in combination of two or more kinds.
[0043] The median particle size of the solid catalyst component for olefin polymerization is usually 60 μm or less, preferably 20 to 50 μm, and more preferably 30 to 40 μm.
[0044] The median particle size of the solid catalyst component for olefin polymerization can be controlled by the particle size of the magnesium compound in the solid catalyst component for olefin polymerization.
[0045] The organoaluminum compound is a compound having one or more carbon-aluminum bonds, and specific examples thereof include the compounds described in JP-A-10-212319. The organoaluminum compound is preferably trialkylaluminum, a mixture of trialkylaluminum and dialkylaluminum halide, or alkylalumoxane, and more preferably triethylaluminum, triisobutylaluminum, a mixture of triethylaluminum and diethylaluminum chloride, or tetraethyldialumoxane.
[0046] Examples of the external electron donor include compounds described in Japanese Patent No. 2950168, JP 2006-96936, JP 2009-173870, and JP 2010-168545. Of these, oxygen-containing compounds or nitrogen-containing compounds are preferred. Examples of the oxygen-containing compound include alkoxysilanes, ethers, esters, and ketones. Of these, alkoxysilanes or ethers are preferred.
[0047] Specific examples of alkoxysilanes include cyclohexylmethyldimethoxysilane, cyclohexylethyldimethoxysilane, diisopropyldimethoxysilane, tert-butylethyldimethoxysilane, tert-butyl-n-propyldimethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane, dicyclobutyldimethoxysilane, dicyclopentyldimethoxysilane, tetraethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, isobutyltriethoxysilane, vinyltriethoxysilane, sec-butyltriethoxysilane, cyclohexyltriethoxysilane, cyclopentyltriethoxysilane, dimethylaminotrimethoxysilane, and diethylaminotriethoxysilane. Notrimethoxysilane, di-n-propylaminotrimethoxysilane, dimethylaminotriethoxysilane, diethylaminotriethoxysilane, di-n-propylaminotriethoxysilane, methylethylaminotriethoxysilane, methyl-n-propylaminotriethoxysilane, tert-butylaminotriethoxysilane, diisopropylaminotriethoxysilane, methylisopropylaminotriethoxysilane, perhydroquinolinotriethoxysilane, perhydroisoquinolinotriethoxysilane, 1,2,3,4-tetrahydroquinolinotriethoxysilane, 1,2,3,4-tetrahydroisoquinolinotriethoxysilane, and octamethyleneiminotriethoxysilane.
[0048] The external electron donor ether is preferably a cyclic ether compound, which is a heterocyclic compound having at least one -COC- bond in the ring structure, more preferably a cyclic ether compound having at least one -COCOC- bond in the ring structure, and particularly preferably 1,3-dioxolane or 1,3-dioxane.
[0049] Of the above external electron donors, cyclohexylethyldimethoxysilane is preferred.
[0050] The external electron donors may be used alone or in combination of two or more kinds.
[0051] When producing an olefin polymerization catalyst, the method of contacting an olefin polymerization solid catalyst component, an organoaluminum compound, and an external electron donor is not particularly limited as long as an olefin polymerization catalyst is produced. The contact is carried out in the presence or absence of a solvent. The contact mixture may be fed to a polymerization tank, or each component may be fed separately to a polymerization tank and contacted in the polymerization tank, or a contact mixture of any two components and the remaining component may be fed separately to a polymerization tank and contacted in the polymerization tank.
[0052] The amount of the organoaluminum compound used is preferably 0.01 to 1000 μmol, more preferably 0.1 to 500 μmol, per 1 mg of the solid catalyst component for olefin polymerization.
[0053] The amount of the external electron donor used is preferably 0.0001 to 1000 μmol, more preferably 0.001 to 500 μmol, and further preferably 0.01 to 150 μmol, per 1 mg of the solid catalyst component for olefin polymerization.
[0054] <Production of Propylene Polymer Composition> The polymerization method for the propylene polymer composition according to the present invention can be a known polymerization method. For example, a solvent polymerization method using an inert solvent represented by a hydrocarbon compound such as hexane, heptane, octane, decane, cyclohexane, methylcyclohexane, benzene, toluene, xylene, etc., a bulk polymerization method using a liquid monomer as a solvent, a gas phase polymerization method carried out in a gaseous monomer, etc. are included, and the bulk polymerization method or gas phase polymerization method which is easy to post-treat, etc. are preferred. These polymerization methods may be batch-type or continuous-type.
[0055] The method for producing a propylene polymer composition according to the present invention uses the above-mentioned polymerization method to carry out multi-stage polymerization including a first step and a second step and subsequent steps. The polymerization method for the first step and the polymerization method for the second step and subsequent steps may be the same or different. From the viewpoint of polymerization activity and ease of post-treatment, the first step is preferably a step in which polymerization is carried out in the absence of an inert solvent, and the second step and subsequent steps are preferably a step in which polymerization is carried out in a gas phase. Moreover, the polymerization for the first step and the polymerization for the second step and subsequent steps may be carried out in the same polymerization tank (reactor) or different polymerization tanks (reactors).
[0056] Examples of the method for producing the propylene polymer composition according to the present invention include a solvent-solvent polymerization method, a bulk-bulk polymerization method, a gas-gas phase polymerization method, a solvent-gas phase polymerization method, a bulk-gas-gas phase polymerization method, a solvent-gas-gas phase polymerization method, and a bulk-gas-gas phase polymerization method, and preferably the bulk-gas phase polymerization method, the gas-gas phase polymerization method, and the bulk-gas-gas phase polymerization method.
[0057] The polymerization temperature in the first step is not particularly limited, but is preferably 20°C to 180°C, and more preferably 30°C to 100°C from the viewpoints of productivity and control of the content of the propylene polymer (1).
[0058] The polymerization temperature in the second and subsequent steps may be the same as or different from the polymerization temperature in the first step, but is preferably 20°C to 180°C, more preferably 30°C to 100°C.
[0059] The process for producing a propylene polymer composition according to the present invention may, if necessary, include a step of performing post-treatment such as deactivating the catalyst, removing the solvent, removing the monomer, drying, or granulation.
[0060] The propylene polymer composition according to the present invention may contain additives and other resins as necessary within the scope of not impairing the objects and effects of the present invention. Examples of additives include antioxidants, ultraviolet absorbers, antistatic agents, lubricants, nucleating agents, adhesives, antifogging agents, etc. In addition, examples of resins that may be added include polyethylene resins, polypropylene resins, and other polyolefin resins.
[0061] The propylene polymer composition according to the present invention can be used as a material for forming various films. For example, a film consisting of a single layer formed using the propylene polymer composition according to the present invention, and a multi-layer film (at least two layers) including a layer formed using the propylene polymer composition according to the present invention can be mentioned. In addition, examples of films formed using the propylene polymer composition according to the present invention include films for packaging food and films for packaging clothing, and preferably films for packaging food. In addition, such films may be unstretched, uniaxially stretched, or biaxially stretched.
[0062] The method for producing a film using the propylene polymer composition according to the present invention is not particularly limited, and examples thereof include commonly used inflation methods, T-die methods, calendar methods, and the like. In addition, the method for producing a film using the propylene polymer composition according to the present invention may be, for example, a method for forming a film of the propylene polymer composition according to the present invention alone or a method for forming a multilayer film (at least two layers) with other resins using the above-mentioned method. Examples of the multilayer method include commonly used coextrusion molding, extrusion lamination, heat lamination, dry lamination, etc. In addition, a method for producing a film using the propylene polymer composition according to the present invention includes a method for producing a film by stretching a film or sheet obtained by previously molding using the above-mentioned method. Examples of the stretching method include a method of uniaxial or biaxial stretching using a roll stretching method, a tenter stretching method, a tubular stretching method, etc. From the viewpoint of the balance of physical properties such as low-temperature heat sealability, transparency, and rigidity of the film, a non-stretched coextrusion molding method or a biaxial stretching method is preferred. In addition, as a method for producing a film using the propylene polymer composition of the present invention, a method in which various biaxially stretched films or the like are used as a substrate layer, and the propylene polymer composition of the present invention is applied in a molten state to the substrate layer to form a multi-layer (at least two layers) packaging film can be mentioned.
[0063] The packaging film formed as described above can be used as a material for forming a packaging bag. Specifically, the propylene polymer composition according to the present invention can form a heat seal layer that can be heat sealed at a relatively low temperature (preferably 80°C to 120°C, more preferably 96°C to 118°C). Therefore, a packaging bag can be formed by deforming a film having such a heat seal layer to make the heat seal layers face each other, and heating and heat sealing the portion where the heat seal layers face each other. An example of a film for forming a packaging bag is a multilayer film in which a heat seal layer (biaxially stretched or unstretched) formed using the propylene polymer composition according to the present invention is laminated on a base layer of a biaxially stretched film. The use of the packaging bag is not particularly limited, and examples thereof include uses for food, clothing, miscellaneous goods, etc.
[0064] As described above, according to the propylene polymer composition of the present invention, a heat seal layer that can be heat sealed at a relatively low temperature can be formed, and the occurrence of blocking in a film having the heat seal layer can be suppressed.
[0065] That is, the propylene polymer composition according to the present invention contains the following propylene polymer (1) and the following propylene-α-olefin copolymer (2), the content of the propylene polymer (1) is 2% by mass to 25% by mass relative to 100% by mass of the total content of the propylene polymer (1) and the propylene-α-olefin copolymer (2), and satisfies the following requirement (3), whereby a heat seal layer that can be heat sealed at a relatively low temperature can be formed and blocking can be suppressed in a film having the heat seal layer. Propylene polymer (1): A polymer containing 94% by mass or more of monomer units derived from propylene. Propylene-α-olefin copolymer (2): A copolymer comprising 60% by mass or more and less than 94% by mass of monomer units derived from propylene, and more than 6% by mass and 40% by mass or less of monomer units derived from an α-olefin having 4 to 12 carbon atoms. Requirement (3): In a temperature rising elution fractionation method using orthodichlorobenzene as a solvent in the temperature range of 0°C to 140°C, the following formula (3-1) is satisfied. Wb≦―1.79×Th+150 (3-1) (In the formula, Wb indicates the cumulative amount of elution from 0°C to 50°C. Th indicates the temperature (°C) between 0°C and 80°C or between 110°C and 140°C at which the cumulative amount of elution is 65% by mass, assuming that the sum of the cumulative amount of elution between 0°C and 80°C and the cumulative amount of elution between 110°C and 140°C is 100% by mass.)
[0066] In addition, the propylene polymer composition according to the present invention has an advantage that the propylene-α-olefin copolymer can be produced at low cost because the monomer units derived from the α-olefin having 4 to 12 carbon atoms contained in the propylene-α-olefin copolymer (2) are monomer units derived from 1-butene.
[0067] In addition, the propylene polymer composition according to the present invention has an effect of improving the heat sealability of the film at low temperatures, since the propylene-α-olefin copolymer (2) contains 70% by mass to 92% by mass of monomer units derived from propylene and 8% by mass to 30% by mass of monomer units derived from an α-olefin having 4 to 12 carbon atoms.
[0068] In addition, in the propylene polymer composition according to the present invention, the propylene-α-olefin copolymer (2) further contains 2% by mass to 6% by mass of monomer units derived from ethylene, which has the effect of improving the heat sealability of the film at low temperatures.
[0069] In addition, the propylene polymer composition according to the present invention has an effect of improving the blocking resistance of the film, since the propylene polymer (1) contains 95% by mass or more of monomer units derived from propylene.
[0070] In addition, the propylene polymer composition according to the present invention has an effect of improving the blocking resistance of the film by containing the propylene polymer (1) in an amount of 3% by mass to 20% by mass.
[0071] Furthermore, the film according to the present invention, containing any one of the above propylene polymer compositions, can be heat-sealed at a relatively low temperature and is less susceptible to blocking.
[0072] Furthermore, since the film according to the present invention is a biaxially stretched film, it has the effect of being excellent in transparency and mechanical properties. EXAMPLES
[0073] The measured values of each item in the examples and comparative examples were measured by the following methods.
[0074] (1) Median particle size of solid catalyst component for olefin polymerization (unit: μm) The median particle size of the solid catalyst component for olefin polymerization was measured by the laser diffraction / scattering method according to the standard ISO13320:2009. A laser diffraction particle size distribution analyzer (Malvern "Mastersizer 3000") was used as the measuring device, and the refractive index was set to 1.49 for toluene and 1.53-0.1i for the solid catalyst component. The toluene solvent, from which moisture had been removed in advance using alumina or the like, was poured into a dispersing device (Hydro MV) with the opening sealed with nitrogen, and the inside of the circulation system, including the measurement cell, was filled with the toluene solvent. The stirring speed was set to 2,000 rpm, and the solid catalyst component for olefin polymerization was poured in so that the scattering intensity was 3-10% while circulating the toluene solvent in the measurement cell without ultrasonic dispersion treatment, and the particle size was measured. The median particle size was obtained from the obtained particle size volume-based distribution diagram. The solid catalyst component for olefin polymerization was handled so as not to come into contact with the air or moisture, and no pretreatment was performed.
[0075] (2) Melt flow rate (MFR, unit: g / 10 min) The MFR of the propylene polymer composition was measured at a temperature of 230° C. and a load of 21.18 N in accordance with Method A specified in JIS K7210-1:2014.
[0076] (3) Comonomer content (unit: weight %) The comonomer content (content of monomer units other than propylene monomer units) in the propylene polymer composition was determined by infrared spectroscopy measurement according to the method described in Polymer Analysis Handbook (published by Kinokuniya Shoten in 1995) on page 616. Then, the contents of propylene monomer units and other monomer units contained in each polymer were calculated based on the production conditions of the propylene polymer composition.
[0077] (4) Calculation of Wb (unit: wt%), Th (unit: °C), and Th' (unit: °C) by Temperature Rising Elution Fractionation (TREF) The measurements were carried out using a CFC device (cross fractionation chromatograph, PolymerChar Automated 3D analyzer CFC-2). To 40 mg of the propylene polymer composition, 20 mL of ODCB (orthodichlorobenzene) containing 0.05 w / V % BHT (dibutylhydroxytoluene) was added, and the mixture was heated and stirred at 145° C. for 60 minutes to prepare a sample solution. 0.5 mL of the obtained sample solution was injected into a TREF column (manufactured by Polymerchar, packing material is SUS beads) in a CFC apparatus maintained at 145° C., and held for 20 minutes. The temperature of the TREF column in the CFC apparatus was ramped from 145° C. to 100° C. at a rate of 40° C. / min, and then held at 100° C. for 20 min. The temperature of the TREF column in the CFC apparatus was decreased from 100° C. to 0° C. at a rate of 0.5° C. / min, and then held at 0° C. for 30 min. While ODCB was flowed from the piping into the TREF column in the CFC device at a rate of 1 ml / min, the temperature of the TREF column was raised at a rate of 40°C / min, and then held for 30 minutes, and the amount of the propylene polymer composition eluted from the TREF column at each temperature was measured by GPC (built into the CFC) equipped with an infrared spectrophotometer. The measurement was performed at 0°C, 10°C, 20°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 104°C, 108°C, 112°C, 114°C, 116°C, 118°C, 120°C, 122°C, 124°C, 126°C, and 140°C.
[0078] A temperature-integrated elution amount curve from 0°C to 140°C was obtained by calculation using the data processing software built into the CFC device. From the obtained cumulative elution amount curve, the cumulative elution amount up to 50°C was designated as Wb. When the sum of the cumulative elution amount from 0°C to 80°C and the cumulative elution amount from 110°C to 140°C was taken as 100 mass%, the temperature from 0°C to 80°C or 110°C to 140°C at which the cumulative elution amount was 65 mass% was designated as Th. When the cumulative elution amount from 0°C to 140°C was taken as 100 mass%, the temperature from 0°C to 140°C at which the cumulative elution amount was 65 mass% was designated as Th'.
[0079] (5) Preparation of stretched film A propylene polymer composition was used as the surface layer material, and FS2011DG3 (Sumitomo Chemical Co., Ltd., a propylene polymer with Tm=159°C and MFR=3g / 10min) was used as the base layer material, and a coextrusion pilot tenter (Mitsubishi Heavy Industries, Ltd.) equipped with two extruders, one coextrusion T-die, a longitudinal stretching machine, and a transverse stretching machine was used to produce a multilayer biaxially stretched film. Specifically, first, the propylene polymer composition was fed to one extruder and melt-kneaded at 230°C, and FS2011DG3 was fed to the other extruder and melt-kneaded at 260°C. Each melt-kneaded product melt-kneaded in each extruder was fed to one co-extrusion T-die. The melt-kneaded product extruded from this T-die as a two-layer structure of surface layer / base layer was quenched and solidified with a cooling roll at 30°C at a line speed of 5m / min to obtain a cast sheet. The obtained cast sheet was stretched 5 times in the longitudinal direction at a stretching temperature of 120°C by the roll peripheral speed difference of the longitudinal stretching machine, and then stretched 8 times in the transverse direction at a stretching temperature of 157°C and a line speed of 25m / min by a transverse stretching machine equipped with clips, and then heat-treated at 165°C to obtain a multilayer biaxially stretched film with a surface layer thickness / base layer thickness=1μm / 20μm.
[0080] (6) Heat seal temperature (HST, unit: °C) The surface layers of two multilayer biaxially oriented films were overlapped and sealed with a heat sealer (manufactured by Toyo Seiki) heated to a specified temperature. 2 The heat-sealed sample was kept for 24 hours at a temperature of 23°C and a humidity of 50%, and then peeled at a temperature of 23°C, a humidity of 50%, a peel speed of 200 mm / min, and a peel angle of 180°. The sealing temperature at which the peel resistance reached 300 g / 25 mm was determined, and this was taken as the heat-sealing temperature.
[0081] (7) Blocking strength (unit: N / 12 cm 2 ) The surface layers of two multilayer biaxially stretched films (100 mm x 30 mm) were overlapped with each other, and a weight of 500 g with an installation area of 40 mm x 30 mm was placed on top of them, followed by heat treatment for 3 hours at 60°C. After leaving them for 30 minutes or more under conditions of a temperature of 23°C and a humidity of 50%, the shear peel strength was measured at a tensile speed of 200 mm / min, which was taken as the blocking strength.
[0082] <Synthesis of solid catalyst component 1 for olefin polymerization> The gas in the reaction vessel equipped with a stirrer was replaced with nitrogen gas. Then, toluene (60.1 L) and titanium tetrachloride (22.3 L) were added to the reaction vessel and stirred to obtain a toluene solution of titanium tetrachloride. Then, while stirring at a temperature of 0°C or less in the reaction vessel, magnesium diethoxide (particle size 30 μm, 11 kg) was added to the reaction vessel in six portions every 72 minutes. Then, the temperature in the reaction vessel was kept at 2°C or less for 120 minutes, and then the temperature in the reaction vessel was kept at 10°C or less for 120 minutes. Then, toluene (14.3 L) was added to the reaction vessel, the temperature in the reaction vessel was kept at 60°C, and 2-ethoxymethyl-3,3-dimethylbutanoic acid ethyl (4.0 kg) was added. Then, the temperature in the reaction vessel was kept at 110°C and stirred for 3 hours. The reaction mixture obtained was subjected to solid-liquid separation at 110°C, and the obtained solid was washed three times with 83 L of toluene at 95°C. Then, toluene (33 L) was added to the reaction vessel, the temperature in the reaction vessel was increased to 60° C., and titanium tetrachloride (22 L) was added. Then, the temperature in the reaction vessel was increased to 105° C. and the mixture was stirred for 30 minutes. The reaction mixture was subjected to solid-liquid separation at 105° C., and the solid was washed three times with 83 L of toluene at 60° C., then washed three times with hexane (83 L), and then dried to obtain a solid catalyst component 1 for olefin polymerization (median particle size 32 μm, 9.0 kg).
[0083] <Synthesis of solid catalyst component 2 for olefin polymerization> The gas in the reaction vessel equipped with a stirrer was replaced with nitrogen gas. Then, toluene (52.8 L) and titanium tetrachloride (33.3 L) were added to the reaction vessel and stirred to obtain a toluene solution of titanium tetrachloride. Then, while stirring the temperature in the reaction vessel at 0°C or less, magnesium diethoxide (particle size 71 μm, 11 kg) was added to the reaction vessel in six portions every 72 minutes. Then, the temperature in the reaction vessel was kept at 2°C or less for 120 minutes. Then, 2-ethoxymethyl-3,3-dimethylbutanoic acid ethyl (0.77 kg) was added to the reaction vessel while keeping the temperature in the reaction vessel at 2°C or less. Then, the temperature in the reaction vessel was kept at 10°C or less for 120 minutes. Then, toluene (14.3 L) was added to the reaction vessel, the temperature in the reaction vessel was kept at 60°C, and 2-ethoxymethyl-3,3-dimethylbutanoic acid ethyl (4.0 kg) was added. Then, the temperature in the reaction vessel was increased to 110°C and the mixture was stirred for 3 hours. After the reaction mixture was subjected to solid-liquid separation at 110°C, the obtained solid was washed three times with 83 L of toluene at 95°C. Then, toluene (34 L) was added to the reaction vessel, the temperature in the reaction vessel was increased to 60°C, and titanium tetrachloride (22 L) and ethyl 2-ethoxymethyl-3,3-dimethylbutanoate (0.95 kg) were added. Then, the temperature in the reaction vessel was increased to 110°C and the mixture was stirred for 30 minutes. After the reaction mixture was subjected to solid-liquid separation at 110°C, the obtained solid was washed three times with 83 L of toluene at 60°C, then washed three times with hexane (83 L), and then dried to obtain a solid catalyst component 2 for olefin polymerization (median particle size 65 μm, 10.9 kg).
[0084] <Example 1> <Production of Propylene Polymer Composition 1> [Preactivation of solid catalyst components for olefin polymerization] In an autoclave equipped with a stirrer and having an internal volume of 3 L, dehydrated and degassed n-hexane (1.6 L), triethylaluminum (73.7 mmol), cyclohexylethyldimethoxysilane (5.9 mmol) as an external electron donor, and the above-mentioned solid catalyst component 1 for olefin polymerization (22.5 g) were added, and the temperature in the autoclave was kept at 5 to 15°C, and propylene (101.3 g) was continuously fed over 30 minutes to perform preactivation, thereby obtaining a slurry of a prepolymerization catalyst. The obtained slurry of the prepolymerization catalyst was transferred to an autoclave equipped with a stirrer and having an internal volume of 200 L, and then liquid butane (140 L) was added thereto to dilute it.
[0085] [polymerization] (First step) Liquid propylene (75 kg / hr) and hydrogen (13.3 NL / hr) were supplied to a 30 L loop-type bulk polymerization tank, and the above-obtained prepolymerization catalyst (4.7 g / hr), triethylaluminum (33 mmol / hr), and cyclohexylethyldimethoxysilane (11 mmol / hr) as an external electron donor were further supplied. The liquid propylene was then polymerized at a polymerization temperature of 40° C. and a polymerization pressure of 3.8 MPa to obtain a propylene polymer component (1.3 kg / hr). The obtained slurry containing the propylene polymer component was continuously transferred to the second step.
[0086] (Second process) Internal volume 1m 3A gas-phase fluidized bed reactor equipped with an agitator was used, and propylene, hydrogen, ethylene and 1-butene were supplied under the following conditions: polymer holding capacity of the fluidized bed: 85 kg, polymerization temperature: 70°C, polymerization pressure: 1.2 MPa, gas superficial velocity inside the reactor: 0.30 m / sec, effective hydrogen concentration in the gas phase (hydrogen concentration / (hydrogen concentration+propylene concentration+ethylene concentration+1-butene concentration)): 1.2 mol%, effective ethylene concentration (ethylene concentration / (propylene concentration+ethylene concentration+1-butene concentration)): 2.5 mol%, effective 1-butene concentration (1-butene concentration / (propylene concentration+ethylene concentration+1-butene concentration)): 6.7 mol%, to obtain a propylene polymer composition (25.8 kg / hr) in the presence of a slurry containing a propylene polymer component transferred from the loop-type bulk polymerization tank in the first step. The propylene polymer composition was continuously transferred to a post-treatment step.
[0087] (Post-processing) Water (10 mL / hr) and nitrogen gas (20 m 3 / hr) was fed to dry the propylene polymer composition and deactivate the catalyst.
[0088] 100 parts by weight of the obtained polypropylene resin composition was mixed with 0.01 part by weight of DHT-4C (manufactured by Kyowa Chemical Industry Co., Ltd.), 0.1 part by weight of IRGANOX1010 (manufactured by BASF Japan Ltd.), and 0.05 part by weight of IRGAFOS168 (manufactured by BASF Japan Ltd.), and then melt extrusion was performed to obtain pellet-shaped propylene polymer composition 1. The analytical values and evaluation results of the obtained propylene polymer composition 1 are shown in Table 3.
[0089] <Example 2> <Preparation of Propylene Polymer Composition 2> Propylene polymer composition 2 was obtained in the same manner as in Example 1, except that the conditions of the first step and the second step were changed as shown in Table 1. The analytical values and evaluation results of the obtained propylene polymer composition 2 are shown in Table 3.
[0090] <Example 3> <Production of Propylene Polymer Composition 3> Propylene polymer composition 3 was obtained in the same manner as in Example 1, except that the conditions of the first step and the second step were changed as shown in Table 1. The analytical values and evaluation results of the obtained propylene polymer composition 3 are shown in Table 3.
[0091] <Example 4> <Preparation of Propylene Polymer Composition 4> Propylene polymer composition 4 was obtained in the same manner as in Example 1, except that the conditions of the first step and the second step were changed as shown in Table 1. The analytical values and evaluation results of the obtained propylene polymer composition 4 are shown in Table 3.
[0092] <Example 5> <Preparation of Propylene Polymer Composition 5> Propylene polymer composition 5 was obtained in the same manner as in Example 1, except that the conditions of the first step and the second step were changed as shown in Table 1. The analytical values and evaluation results of the obtained propylene polymer composition 5 are shown in Table 3.
[0093] <Example 6> <Preparation of Propylene Polymer Composition 6> A propylene polymer composition 6 was obtained in the same manner as in Example 1, except that the conditions of the first step and the second step were changed as shown in Table 1. The analytical values and evaluation results of the obtained propylene polymer composition 6 are shown in Table 3.
[0094] Comparative Example 1: Production of Propylene Polymer Composition C1 [Preactivation of solid catalyst components for olefin polymerization] In an autoclave equipped with a stirrer and having an internal volume of 3 L, dehydrated and degassed n-hexane (1.6 L), triethylaluminum (65.2 mmol), tert-butyl-n-propyldimethoxysilane (5.2 mmol) as an external electron donor, and the above-mentioned solid catalyst component 2 for olefin polymerization (19.9 g) were added, and the temperature in the autoclave was kept at 5 to 15°C, and propylene (99.5 g) was continuously fed over 30 minutes to perform preactivation, thereby obtaining a slurry of a prepolymerization catalyst. The obtained slurry of the prepolymerization catalyst was transferred to an autoclave equipped with a stirrer and having an internal volume of 200 L, and then liquid butane (140 L) was added thereto to dilute it.
[0095] [polymerization] (First step) Liquid propylene (75 kg / hr) and hydrogen (26.4 NL / hr) were supplied to a 30 L loop-type bulk polymerization tank, and the above-obtained prepolymerization catalyst (4.6 g / hr), triethylaluminum (34 mmol / hr), and tert-butyl-n-propyldimethoxysilane (11 mmol / hr) as an external electron donor were further supplied. The liquid propylene was then polymerized at a polymerization temperature of 50° C. and a polymerization pressure of 3.9 MPa to obtain a propylene polymer component (1.4 kg / hr). The obtained slurry containing the propylene polymer component was continuously transferred to the second step.
[0096] (Second process) Internal volume 1m 3 A gas-phase fluidized bed reactor equipped with an agitator was used, and propylene, hydrogen, ethylene and 1-butene were supplied under the following conditions: polymer holding capacity of the fluidized bed: 69 kg, polymerization temperature: 70°C, polymerization pressure: 1.2 MPa, gas superficial velocity inside the reactor: 0.30 m / sec, effective hydrogen concentration in the gas phase (hydrogen concentration / (hydrogen concentration+propylene concentration+ethylene concentration+1-butene concentration)): 4.4 mol%, effective ethylene concentration (ethylene concentration / (propylene concentration+ethylene concentration+1-butene concentration)): 3.1 mol%, effective 1-butene concentration (1-butene concentration / (propylene concentration+ethylene concentration+1-butene concentration)): 14.5 mol%, to obtain a propylene polymer composition (27.0 kg / hr) in the presence of a slurry containing a propylene polymer component transferred from the loop-type bulk polymerization tank in the first step. The propylene polymer composition was continuously transferred to a post-treatment step.
[0097] (Post-processing) The propylene polymer composition transferred from the gas-phase fluidized bed reactor to the drying tank was then subjected to a gas-phase fluidized bed reaction with 10 mL / hr of nitrogen gas (20 m 3 / hr) was fed to dry the propylene polymer composition and deactivate the catalyst.
[0098] 100 parts by weight of the obtained polypropylene resin composition was mixed with 0.01 parts by weight of DHT-4C (Kyowa Chemical Industry Co., Ltd.), 0.1 parts by weight of IRGANOX1010 (BASF Japan Co., Ltd.), and 0.05 parts by weight of IRGAFOS168 (BASF Japan Co., Ltd.), and then melt extrusion was performed to obtain a pellet-shaped propylene polymer composition C1. The analytical values and evaluation results of the obtained propylene polymer composition C1 are shown in Table 4.
[0099] <Comparative Example 2> <Preparation of Propylene Polymer Composition C2> A propylene polymer composition C2 was obtained in the same manner as in Comparative Example 1, except that the conditions of the first step and the second step were changed as shown in Table 2. The analytical values and evaluation results of the obtained propylene polymer composition C2 are shown in Table 4.
[0100] For each of the above-mentioned Examples and Comparative Examples, the relationship between Wb and Th is shown in the graph of FIG. 1(a), and the relationship between Wb and Th' is shown in the graph of FIG. 1(b). In addition, an approximation line was obtained from the graphs of FIG. 1(a) and (b), and an equation showing each approximation line was obtained. Looking at FIG. 1(a), it can be seen that the plots of each Comparative Example are located above the approximation line, and the plots of each Example are located below it. On the other hand, looking at FIG. 1(b), it can be seen that the plots of each Comparative Example and each Example are located above the approximation line. In other words, by making it a requirement that the following formula (3-1) be satisfied, it is possible to distinguish each Example from each Comparative Example. Wb≦-1.79×Th+150 (3-1) (In the formula, Wb indicates the cumulative amount of elution from 0°C to 50°C. Th indicates the temperature (°C) between 0°C and 80°C or between 110°C and 140°C at which the cumulative amount of elution is 65% by mass, assuming that the sum of the cumulative amount of elution between 0°C and 80°C and the cumulative amount of elution between 110°C and 140°C is 100% by mass.)
[0101] [Table 1]
[0102]
Table 2
[0103]
Table 3
[0104]
Table 4
Claims
1. The present invention relates to a propylene polymer (1) and a propylene-α-olefin copolymer (2), the content of the propylene polymer (1) is 4.7% by mass to 7.3% by mass, and the content of the propylene-α-olefin copolymer (2) is 92.7% by mass to 95.3% by mass, relative to 100% by mass of the total content of the propylene polymer (1) and the propylene-α-olefin copolymer (2); A propylene polymer composition satisfying the following requirement (3): Propylene polymer (1): A homopolymer of propylene. Propylene-α-olefin copolymer (2): A copolymer comprising 81.5% by mass or more and 88.2% by mass or less of monomer units derived from propylene and 8.2% by mass or more and 15.2% by mass or less of monomer units derived from an α-olefin having 4 to 12 carbon atoms, wherein the monomer units derived from an α-olefin having 4 to 12 carbon atoms are monomer units derived from 1-butene. Requirement (3): In a temperature rising elution fractionation method using orthodichlorobenzene as a solvent in the temperature range of 0°C to 140°C, the following formula (3-1) is satisfied. Wb≦−1.79×Th+150 (3-1) (In the formula, Wb indicates the cumulative amount of elution from 0° C. to 50° C., and is 16.5 (mass %) or more and 33.0 (mass %) or less. Th indicates the temperature (°C) between 0°C and 80°C at which the cumulative amount of elution is 65% by mass when the sum of the cumulative amount of elution between 0°C and 80°C and the cumulative amount of elution between 110°C and 140°C is taken as 100% by mass, and is 65.0 (°C) or more and 73.0 (°C) or less.
2. The propylene polymer composition according to claim 1, wherein the propylene-α-olefin copolymer (2) further contains 2% by mass to 6% by mass of monomer units derived from ethylene.
3. A film comprising the propylene polymer composition according to claim 1 or 2.
4. 4. The film of claim 3 which is a biaxially stretched film.
Citation Information
Patent Citations
Propolylene copolymer, its production method, and film composed of the propylene copolymer
JP2002069143A
Propylene resin composition
JP2007084806A
Method for producing propylene polymerized material
JP2016050316A
Process for preparing propylene copolymer compositions
US20190010263A1
Method for producing solid catalyst component for olefin polymerization
WO2018025862A1