LAMINATE AND METHOD FOR MANUFACTURING LAMINATE
The laminate with an electron beam curable varnish layer addresses heat resistance, cracking, and odor issues by using a (meth)acrylate compound and nanoindicators, ensuring high hardness and recovery rate, enhancing packaging material performance.
Patent Information
- Application Number
- JP2023198150
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-11-22
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2043-11-22
AI Technical Summary
Existing packaging materials face issues with heat resistance, cracking, peeling, and odor due to the use of ultraviolet (UV) curable varnishes, which contain photopolymerization initiators, and conventional solvent-based or water-based varnishes lack sufficient coating strength.
A laminate structure comprising a heat seal layer, a base material, and a varnish layer formed by curing an electron beam curable composition containing a (meth)acrylate compound with two or more (meth)acryloyl groups, without photopolymerization initiators, and incorporating nanoindicators, extender pigments, and fine resin particles to enhance hardness and slip properties.
The laminate achieves heat resistance, gloss, slip properties, solvent resistance, and low odor, with a varnish layer hardness of 100-180 MPa and recovery rate of 77-100%, addressing the limitations of conventional varnishes.
Smart Images

Figure 0007596491000001 
Figure 0007596491000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate and a method for producing the laminate. [Background technology]
[0002] In recent years, the use of curing technology using active energy rays has expanded in the printing industry because of the following advantages: shortening process time through instant drying, reducing the environmental impact and improving work safety by being non-volatile component (Non-VOC), and realizing strong coating film properties through crosslinking reactions.
[0003] The use of active energy ray curing technology, which began in the field of commercial printing based on paper substrates such as flyers and posters, has spread to various fields due to the development of printing technologies including printing machines and printing inks, and the field of application is expanding to various film substrates, and its use as a packaging material for packaged products such as food, cosmetics, and toys is also expanding.
[0004] Packaging materials are made by bonding multiple films together with adhesive, and most of them are reverse-printed, meaning the printed image is visible through the film. However, from the perspective of reducing environmental impact and shortening process time, there is an increasing demand for front-printed structures, where the outermost layer is an ink or varnish layer.
[0005] Generally, in packaging materials with a surface printing structure, an overcoat varnish is applied to protect the ink coating, but conventional solvent-based or water-based heat-drying overcoat varnishes do not provide sufficient coating strength, so active energy ray-curable varnishes, which have strong coating properties, are used.
[0006] However, when a packaging material with a surface printing structure further has a heat seal layer, the outermost ink / varnish layer is treated at high temperatures, which makes the ink / varnish layer prone to cracking and peeling, even when an active energy ray-curable varnish is used (see Patent Document 1), resulting in problems such as limitations on the design and specifications of the packaging material.
[0007] Here, ultraviolet (UV) curable varnish is the mainstream of active energy ray curable varnish, but ultraviolet (UV) curable varnish contains a considerable amount of photopolymerization initiator, which acts as an inert component and affects the strength and heat resistance of the cured coating film. Furthermore, in the case of packaging materials, there is a large problem of odor caused by decomposition products of the photopolymerization initiator. In addition, in the case of UV curing, damage to the substrate due to heat generated by the lamp that generates the ultraviolet rays is also a problem.
[0008] Against this background, electron beam (EB) curable varnishes, which do not require photopolymerization initiators, cause less thermal damage to the substrate, and can be cured with a high-energy electron beam, are attracting attention as opposed to ultraviolet (UV) curable varnishes, particularly in terms of their heat resistance and odor.
[0009] Surface hardness is often used as an indicator of the heat resistance and strength of the varnish layer in this type of surface printing configuration, but in the case of packaging materials, there are many characteristics that cannot be inferred from hardness, such as cracking during processing and heat resistance during heat sealing, so it is necessary to evaluate brittleness in addition to hardness. In particular, the heat resistance of the varnish layer during heat sealing requires not only resistance to heat being applied to the varnish layer, but also resistance to stress caused by deformation and shrinkage of the heat-sealed layer due to heat and stress caused by the substrate shrinking due to heat, and therefore optimization is required in terms of both hardness and brittleness.
[0010] In addition, packaging materials need to have gloss, slip properties to withstand impacts and friction during transportation, adhesion, etc., and further need to be solvent-resistant so that they can withstand alcohol-based disinfection as a recent measure against infectious diseases. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] JP 2007-204543 A Summary of the Invention [Problem to be solved by the invention]
[0012] The problem to be solved by the present invention is to provide a laminate having heat resistance, gloss, slip properties, solvent resistance and low odor properties. [Means for solving the problem]
[0013] As a result of extensive investigations aimed at solving the above problems, the present inventors have found that the above problems can be solved by the laminate described below, and have thus completed the present invention.
[0014] That is, the present invention is a laminate having a heat seal layer, a substrate, and a varnish layer in this order, The varnish layer is formed by curing an electron beam curable composition containing a (meth)acrylate compound with an electron beam. This is a layer The (meth)acrylate compound has two or more (meth)acryloyl groups in the molecule. The electron beam curable composition contains a compound having a molecular weight of 80% or more by mass based on the total amount of the composition, The electron beam curable composition is substantially free of a photopolymerization initiator, The varnish layer is made of nanoindentation nt Hardness by the thermal expansion method is 100 to 180 MPa, and the nano-indentation nt The laminate has a recovery rate of 77 to 100% by the fusion method.
[0015] The present invention also relates to the above laminate, which further has a printed layer between the substrate and the varnish layer.
[0016] The present invention also relates to the above laminate, wherein the (meth)acrylate compound contains alkylene oxide-modified (3 to 9 mol / mol) trimethylolpropane triacrylate.
[0017] The present invention also relates to the above laminate, wherein the electron beam curable composition further contains an extender pigment.
[0018] The present invention also relates to the above laminate, wherein the electron beam curable composition further contains resin fine particles.
[0019] The present invention also relates to the above laminate, wherein the electron beam curable composition further contains a leveling agent.
[0020] The present invention also relates to a packaging material comprising the above laminate.
[0021] The present invention also relates to a method for producing the above laminate, wherein the conditions for curing with electron beam are an acceleration voltage of 50 to 200 kV and an exposure dose of 15 to 200 kGy. Effect of the Invention
[0022] The present invention can provide a laminate having heat resistance, gloss, slip properties, solvent resistance and low odor properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Hereinafter, the embodiments of the present invention will be described in detail. Note that the present invention is not limited to the following embodiments, and various modifications can be made within the scope of the present invention.
[0024] The terms used in this specification are explained below. "(Meth)acryloyl" means acryloyl and / or methacryloyl (methacryloyl), and "(meth)acrylate" means acrylate and / or methacrylate (methacrylate). "Active energy rays" means energy rays such as ultraviolet rays and electron beams that have the property of causing chemical changes such as chemical reactions in the irradiated object. "PO" stands for "propylene oxide" and "EO" stands for "ethylene oxide".
[0025] <Laminate> The laminate of the present invention is a laminate having a heat seal layer, a substrate, and a varnish layer in this order, and the varnish layer is a layer formed by curing an electron beam-curable composition containing a (meth)acrylate compound with an electron beam. The laminate of the present invention can be used for various purposes, and is particularly suitable for use as a packaging material.
[0026] <Base material> The substrate in the present invention is not particularly limited, and can be a known one, but is preferably a film substrate.For example, polyolefin substrates such as polyethylene and polypropylene, polyester substrates such as polyethylene terephthalate and polylactic acid, polycarbonate substrates, polystyrene-based substrates such as polystyrene, AS resin and ABS resin, nylon substrates, polyamide substrates, polyvinyl chloride substrates, polyvinylidene chloride substrates, cellophane substrates, paper substrates, aluminum substrates, etc., or film substrates made of composite materials thereof can be mentioned.Among them, polyolefin-based films are preferred from the viewpoint of recyclability. Also, a deposition substrate in which an inorganic compound such as silica, alumina, or aluminum is deposited on a film substrate can be used. Furthermore, the deposition-treated surface may be coated with polyvinyl alcohol or the like. It is preferable that the substrate has a surface to be printed (surface in contact with the printing layer) that has been treated to facilitate adhesion. Specific examples of the adhesion-facilitating treatment include corona discharge treatment, ultraviolet / ozone treatment, plasma treatment, oxygen plasma treatment, and primer treatment. In addition, when sufficient adhesion cannot be obtained with a polyethylene terephthalate substrate, a surface treatment such as an acrylic coating treatment, polyester treatment, or polyvinylidene chloride treatment may be performed.
[0027] A paper substrate may be used as the substrate. The paper substrate may be ordinary paper or cardboard, and the thickness is not particularly specified. The thickness of the paper substrate is, for example, 0.2 mm to 1.0 mm and 20 to 150 g / m 2The paper substrate may be one having a surface that is easily adhesively treated. The paper substrate may be one having a surface that is vapor-deposited with a metal such as aluminum in order to impart design. The paper substrate may be one having a surface coating treatment with an acrylic resin, a urethane resin, a polyester resin, a polyolefin resin, or other resin, and may be one having a surface treatment such as a corona treatment. For example, specific examples of surface-treated paper substrates include coated paper and art paper.
[0028] <Heat seal layer> The heat seal layer in the present invention is not particularly limited, and known ones can be used. For example, polyolefin resins such as polyethylenes such as low density polyethylene (LDPE), linear low density polyethylene (LLDPE) and high density polyethylene (HDPE), acid-modified polyethylene, polypropylene (PP), acid-modified polypropylene, copolymerized polypropylene, ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid ester copolymer, ethylene-(meth)acrylic acid copolymer, and ionomer can be mentioned. Among them, polypropylene-based resins are preferred from the viewpoint of recyclability, and unstretched polypropylene is particularly preferred from the viewpoint of heat sealability. The thickness of the heat seal layer is not particularly limited, but taking into consideration the processability and heat sealability of the laminate, the thickness is preferably in the range of 10 to 60 μm, and more preferably in the range of 15 to 40 μm. The method for laminating the heat seal layer is not particularly limited, and examples thereof include a method of laminating an adhesive layer and a sealant film by heat (thermal lamination, dry lamination) and a method of melting a sealant resin, extruding it onto the adhesive layer, and cooling and solidifying it to laminate (extrusion lamination method).
[0029] <Varnish layer> The varnish layer in the present invention is a layer obtained by curing an electron beam-curable composition containing a (meth)acrylate compound with an electron beam.
[0030] The electron beam curable composition of the present invention contains a (meth)acrylate compound in an amount of 80% by mass or more based on the total amount of the composition. The content of the (meth)acrylate compound in the total amount of the composition is preferably 80 to 99% by mass, more preferably 85 to 98% by mass, and particularly preferably 90 to 97% by mass.
[0031] In this specification, the (meth)acrylate compound means a compound having a (meth)acryloyl group in the molecule. Specific examples of the (meth)acrylate compound that can be used to constitute the electron beam curable composition of the present invention include 1,3-butylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, 1,2-dodecanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol (200) di(meth)acrylate, polyethylene glycol (300) di(meth)acrylate, polyethylene glycol (400) di(meth)acrylate, polyethylene glycol (600) di(meth)acrylate, and hydroxypivalate. bifunctional (meth)acrylate compounds such as neopentyl glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, EO-modified 1,6-hexanediol di(meth)acrylate, PO-modified neopentyl glycol di(meth)acrylate, (neopentyl glycol-modified) trimethylolpropane di(meth)acrylate, dimethyloltricyclodecane di(meth)acrylate, EO-modified bisphenol A di(meth)acrylate, PO-modified bisphenol A di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, dimethylol-tricyclodecane di(meth)acrylate, dicyclopentanyl di(meth)acrylate, and tris(2-hydroxyethyl)isocyanurate di(meth)acrylate; trifunctional (meth)acrylate compounds such as trimethylolpropane tri(meth)acrylate, EO-modified trimethylolpropane tri(meth)acrylate, glycerin propoxy triacrylate, PO-modified trimethylolpropane tri(meth)acrylate, ε-caprolactone-modified tris-(2-acryloxyethyl)isocyanurate, ethoxylated isocyanuric acid tri(meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, and pentaerythritol tri(meth)acrylate; tetrafunctional radical (meth)acrylate compounds such as pentaerythritol tetra(meth)acrylate and ditrimethylolpropane tetra(meth)acrylate; pentafunctional (meth)acrylate compounds such as dipentaerythritol penta(meth)acrylate; Examples of the compound include hexafunctional (meth)acrylate compounds such as dipentaerythritol hexa(meth)acrylate.
[0032] As the (meth)acrylate compound, urethane acrylates such as aliphatic urethane acrylates and aromatic urethane acrylates, polyester acrylates, polyether acrylates, epoxy acrylates, and the like can be used.
[0033] The (meth)acrylate compounds may be used alone or in combination of two or more kinds.
[0034] From the viewpoint of curability, the (meth)acrylate compound preferably contains a polyfunctional acrylate having two or more (meth)acryloyl groups in the molecule.
[0035] From the viewpoint of heat resistance, the (meth)acrylate compound preferably contains alkylene oxide-modified (3 to 9 mol / mol) trimethylolpropane triacrylate. By containing alkylene oxide-modified (3 to 9 mol / mol) trimethylolpropane triacrylate, the hardness and recovery rate of the varnish layer become good, and the heat resistance of the laminate becomes good. It is more preferable that the alkylene oxide modification amount of the alkylene oxide-modified trimethylolpropane triacrylate is 3 to 6 mol / mol. Furthermore, the alkylene oxide-modified (3 to 9 mol / mol) trimethylolpropane triacrylate is preferably ethylene oxide-modified (3 to 9 mol / mol) trimethylolpropane triacrylate or propylene oxide-modified (3 to 9 mol / mol) trimethylolpropane triacrylate, more preferably ethylene oxide-modified (3 to 6 mol / mol) trimethylolpropane triacrylate or propylene oxide-modified (3 to 6 mol / mol) trimethylolpropane triacrylate, and particularly preferably ethylene oxide-modified (3 mol / mol) trimethylolpropane triacrylate or propylene oxide-modified (3 mol / mol) trimethylolpropane triacrylate. The content of the alkylene oxide-modified (3 to 9 mol / mol) trimethylolpropane triacrylate is preferably 20 to 90 mass % in the total amount of the electron beam curable composition.
[0036] From the viewpoint of heat resistance, the (meth)acrylate compound preferably contains dipentaerythritol hexaacrylate. By containing dipentaerythritol hexaacrylate, the hardness of the varnish layer is improved, and the heat resistance of the laminate is improved. When dipentaerythritol hexaacrylate is contained, it is preferably 5 to 50 mass % of the total amount of the electron beam curable composition.
[0037] From the viewpoint of gloss, the (meth)acrylate compound preferably contains tripropylene glycol diacrylate. By containing tripropylene glycol diacrylate, the gloss of the laminate becomes good. When tripropylene glycol diacrylate is contained, it is preferably contained in an amount of 5 to 50 mass % of the total amount of the electron beam curable composition.
[0038] The electron beam curable composition of the present invention may further contain an extender pigment, resin fine particles, and a leveling agent.
[0039] <Extender pigment> The electron beam curable composition of the present invention preferably further contains an extender pigment, which enhances the film-forming properties of the coating film and improves the slip properties. Specific examples of the extender pigment include silica, barium sulfate, alumina white, calcium carbonate, magnesium carbonate, aluminum silicate, magnesium silicate, silicon dioxide, aluminum hydroxide, etc. These may be used alone or in combination of two or more. The preferred extender pigment is silica. The content of the extender pigment is preferably from 0.1 to 10% by mass, and more preferably from 1.0 to 5% by mass, based on the total amount of the electron beam curable composition.
[0040] <Resin fine particles> The electron beam curable composition of the present invention preferably further contains fine resin particles, which improves slip properties and heat resistance.
[0041] Specific examples of resin particles include urethane resin particles, acrylic resin particles, acrylic-styrene copolymer resin particles, polycarbonate resin particles, polyethylene resin particles, polystyrene resin particles, silicone resin particles, melamine resin particles, melamine-benzoguanamine resin particles, melamine-benzoguanamine-formaldehyde resin (condensate) particles, polypropylene resin particles, amide resin particles, polytetrafluoroethylene resin particles, and benzoguanamine resin particles. These may be used alone or in combination of two or more kinds, if necessary.
[0042] From the viewpoints of slip property, heat resistance, and gloss, the content of the resin fine particles is preferably 0.1 to 5 mass %, more preferably 0.25 to 3 mass %, based on the total mass of the electron beam curable composition.
[0043] Resin microparticles may be obtained as a commercial product or may be produced by a known production method.For example, specific examples of urethane resin microparticles include Art Pearl C-1000 transparent, Art Pearl C-600 transparent, Art Pearl C-400 transparent, Art Pearl C-800, and Art Pearl MM-120T manufactured by Negami Chemical Industrial Co., Ltd.In addition, urethane resin microparticles may have a crosslinked structure.Specific examples of urethane resin microparticles having a crosslinked structure include crosslinked urethane resin microparticles such as Art Pearl JB-800T, Art Pearl JB-600T, Art Pearl P-800T, and Art Pearl P-400T manufactured by Negami Chemical Industrial Co., Ltd.
[0044] Examples of acrylic resin fine particles include Art Pearl J4PY and Art Pearl J5PY manufactured by Negami Chemical Industrial Co., Ltd., and Ganz Pearl GB08S manufactured by Aica Kogyo Co., Ltd. Other examples include Eposter MA1002, Eposter MA1004, Eposter MA1006, and Eposter MA1010 manufactured by Nippon Shokubai Co., Ltd., Tuftic FH-S005, Tuftic FH-S008, Tuftic FH-S010, Tuftic FH-S015, and Tuftic FH-S020 manufactured by Toyobo Co., Ltd., and Chemisnow MX-80H3wT, MX-150, MX-180TA, MX-300, MX-500, MX-1000, MX-1500H, MX-2000, and MX-3000 manufactured by Soken Chemical & Engineering Co., Ltd.
[0045] Specific examples of acrylic-styrene copolymer resin fine particles include Eposter MA2003 manufactured by Nippon Shokubai Co., Ltd., and FS-102, FS-201, FS-301, MG-451, and MG-351 manufactured by Nippon Paint Industrial Coatings Co., Ltd.
[0046] Specific examples of polycarbonate resin fine particles include fine particles described in JP-A-2014-125495, fine particles obtained by the production method described in JP-A-2011-26471, and fine particles obtained by the method described in JP-A-2001-213970.
[0047] Specific examples of silicone resin microparticles include KMP-594, KMP-597, KMP-598, KMP-600, KMP-601, and KMP-602 manufactured by Shin-Etsu Chemical Co., Ltd., Trefil E-506S and EP-9215 manufactured by Dow Corning Toray Co., Ltd., and the Tosulpearl series manufactured by Momentive Corporation.
[0048] Specific examples of polyethylene resin microparticles include Mipelon XM-220 and XM221U manufactured by Mitsui Chemicals, Inc., Flowbeads LE-1080 manufactured by Sumitomo Seika Chemicals, Inc., and Cerafloure 991 manufactured by BYK Japan K.K.
[0049] Specific examples of polystyrene-based fine particles include Chemisnow SX-130H, SX-350H, and SX-500H manufactured by Soken Chemical & Engineering Co., Ltd.
[0050] Specific examples of melamine resin fine particles include Eposter SS, Eposter S, Eposter FS, Eposter S6, and Eposter S12 manufactured by Nippon Shokubai Co., Ltd.
[0051] A specific example of the melamine-benzoguanamine resin fine particles is Eposter M30 manufactured by Nippon Shokubai Co., Ltd.
[0052] Specific examples of benzoguanamine resin fine particles include Eposter MS, Eposter M05, and Eposter L15 manufactured by Nippon Shokubai Co., Ltd.
[0053] A specific example of the polytetrafluoroethylene resin fine particles is SST-3T1-RC manufactured by Shamrock Technologies.
[0054] The resin microparticles are preferably one or more types selected from the group consisting of silicone resin microparticles, acrylic resin microparticles, polytetrafluoroethylene resin microparticles, and polyethylene resin microparticles, and more preferably one or more types selected from the group consisting of acrylic resin microparticles and polytetrafluoroethylene microparticles. When silicone resin microparticles, acrylic resin microparticles, or polyethylene resin microparticles are used, particle size control is easy, and high sphericity and excellent dispersibility can be easily obtained. Furthermore, these resin microparticles are highly transparent, and good slip properties can be obtained while minimizing loss of gloss. When polytetrafluoroethylene resin microparticles are used, excellent heat resistance and slip properties can be obtained due to their chemical stability, high melting point, and low coefficient of friction.
[0055] From the viewpoints of slip property, heat resistance, and gloss, it is preferable to use resin fine particles having an average particle size of 2 to 12 μm, and more preferably 5 to 10 μm. The resin fine particles may be in the form of particles composed of various resins or particles whose surfaces are coated with various resins. The resin fine particles may be used alone or in combination of two or more kinds.
[0056] <Leveling agent> The electron beam curable composition of the present invention preferably further contains a leveling agent, which improves slip properties. From the viewpoint of surface slipperiness, the leveling agent preferably contains a silicone-modified acrylate compound. The leveling agent may be used alone or in combination of two or more kinds. The content of the leveling agent is preferably from 0.1 to 3 mass %, more preferably from 0.4 to 1.5 mass %, of the total amount of the electron beam curable composition.
[0057] <Other ingredients> In the electron beam curable composition of the present invention, antistatic agents, surfactants, defoamers, ultraviolet absorbers, antioxidants, curing agents, plasticizers, wetting agents, adhesive assistants, defoamers, antistatic agents, trapping agents, antiblocking agents, preservatives, etc. may be used as necessary, so long as the effects of the present invention are not impaired.
[0058] The electron beam curable composition of the present invention does not substantially contain a photopolymerization initiator. Here, "substantially not containing" in the present invention means that it is not intentionally added and the content due to unintentional addition is less than 1 mass%. Examples of unintentional addition include trace amounts contained in each raw material, contamination during the composition production process, the print production process, etc.
[0059] In addition, the electron beam curable composition of the present invention is substantially free of organic solvents. Organic solvents used as viscosity modifiers in printing inks are of concern as they may contain MOSH / MOAH, which are persistent organic pollutants, and since the absence of volatile components (Non-VOC) is expected to reduce the environmental load and improve work safety, it is preferable that the composition of the present invention is substantially free of organic solvents.
[0060] <Method of producing electron beam curable composition> The electron beam curable composition of the present invention can be produced by mixing and stirring the (meth)acrylate compound and other components such as resin fine particles, which are used as required, for about 30 minutes to 3 hours using a mixer, etc. Note that the (meth)acrylate compound may be produced by mixing and stirring two or more (meth)acrylate compounds in advance, and then adding other components such as resin fine particles, which are used as required.
[0061] <Production of varnish layer> Methods for printing or coating the electron beam curable composition include coating using a roll coater, gravure coater, flexo coater, air doctor coater, blade coater, air knife coater, squeeze coater, impregnation coater, transfer roll coater, kiss coater, curtain coater, cast coater, spray coater, die coater, or the like; offset printing (normal lithographic printing using dampening water and waterless lithographic printing not using dampening water), flexo printing, gravure printing, screen printing, or the like. In addition, in in-line printing and offline printing, various types of inks such as UV curing type, electron beam curing type, heat drying type, evaporation drying type, oxidative polymerization type, penetration drying type, thermal polymerization type, two-component curing type, liquid toner type, and powder toner type inks can be used in combination as necessary.
[0062] <Electron beam irradiation conditions> The electron beam curable composition of the present invention is printed by various printing methods, and then cured through an electron beam irradiator to form a printed layer. The electron beam used for curing is preferably adjusted under the conditions of an accelerating voltage of 50 to 200 kV, more preferably 80 to 110 kV, and an exposure dose of 15 to 60 kGy, more preferably 20 to 45 kGy, taking into consideration the balance between damage to the film and the curability of the electron beam curable composition. When the exposure dose is 15 to 60 kGy, sufficient film strength is obtained, and problems due to damage to the film, such as a decrease in film strength, odor, and yellowing, can be suppressed.
[0063] <Print layer> The laminate of the present invention may further have a printed layer between the substrate and the varnish layer. The print layer is obtained by printing an ink, and drying or curing it as necessary. As the ink, a known ink such as a solvent-based ink, a water-based ink, or an actinic energy ray-curable ink can be used, but in consideration of the productivity of the laminate, an actinic energy ray-curable ink is preferable, an electron beam-curable ink is more preferable, and a solventless electron beam-curable ink is particularly preferable. The method for printing ink on the substrate can be selected from known printing methods such as offset printing, gravure printing, flexographic printing, and inkjet printing.
[0064] <Method of manufacturing laminate> The method for producing the laminate in the present invention can be either a method in which a base material having a varnish layer is prepared and then a heat seal layer is laminated thereon, or a method in which a varnish layer is prepared on a base material having a heat seal layer. Here, the electron beam irradiated when creating the varnish layer may affect the heat seal layer depending on the intensity of the electron beam, the type and thickness of the substrate, and the heat seal strength may decrease. In such a case, a laminate can be produced without being affected by using a method in which the heat seal layer is laminated after creating a substrate having a varnish layer.
[0065] <Hardness of varnish layer in laminate> The varnish layer in the laminate of the present invention is made of nanoindentation. nt The hardness by the immersion method is 100 to 180 MPa. Nano Ind nt The hardness by the indentation method is the indentation hardness value measured using a micro-area mechanical property evaluation device (nanoindenter), and in the present invention, it is the value measured using a Hysitron TI Premier (manufactured by Bruker). The nanoindenter indents only the very surface layer of the laminate, so it is not affected by the substrate and can measure the mechanical properties of only the thin varnish layer. With other measurement methods, the indentation load and displacement are too large, making it difficult to measure only the thin layer. In the present invention, the hardness of only the varnish layer is shown.
[0066] The indentation hardness (H) of the varnish layer is measured as follows. A triangular pyramid-shaped Berkovich indenter is used as the indenter of the nanoindenter. The Berkovich indenter is pressed into the measurement sample under the indentation conditions described below, and the indentation depth h (nm) versus indentation load F (μN) is continuously measured to create a load-displacement curve. The maximum indentation load Fmax (μN) is then calculated based on the projected contact area Ac (μm 2 The hardness is calculated by dividing Fmax by Ac. In other words, H=Fmax / Ac. Here, Ac is the contact projected area corrected for the indenter tip curvature using a standard sample of fused quartz by the instrument standard method. The contact projected area Ac is calculated from the contact depth h (nm), and Ac = 24.56h 2 It is. The indentation conditions are as follows: first, at room temperature, the indenter is pressed to a depth of 300 nm for 5 seconds (i.e., 60 nm / s), then held at the depth of 300 nm for 2 seconds, and finally unloaded to 0 nm for 5 seconds.
[0067] <Recovery rate of varnish layer in laminate> The varnish layer in the laminate of the present invention is made of nanoindentation. nt The recovery rate using the osmotic method is 77-100%. Nano Ind nt The recovery rate by the indentation method is a value that indicates the recovery state of the coating film after indentation, measured using a micro-area mechanical property evaluation device (nanoindenter), and in this application, it is a value measured using the same device as that used to measure the hardness of the varnish layer in the laminate. The larger the number, the easier it is to absorb the indentation and return to the original coating state, and in this invention, it indicates the brittleness of the coating film.
[0068] The method for measuring the recovery rate of the varnish layer is as follows. A conical indenter with a cone shape is used as the indenter of the nanoindenter. The conical indenter is driven horizontally on the measurement sample under the indentation conditions described below, and the indentation depth h (nm) versus the horizontal movement distance (um) is continuously measured to create a horizontal distance-vertical displacement curve. The recovery rate (%) is calculated from the horizontal distance-vertical displacement curve that is created. The recovery rate (%) is an index showing the degree of recovery of the coating film that was indented by the horizontal movement of the indenter. The indentation conditions were room temperature, with the indenter moving 6 μm horizontally at 0.4 μm / s, and a maximum load of 300 μN applied vertically at a loading speed of 20 μN / s. The depth of the indentation was also measured by tracing the sample in the same place with a weak load that did not cause any shape after measurement. From the measurement data obtained, The recovery rate (%) was calculated as follows: (max vertical displacement during indentation (nm)-max indentation depth after indentation (nm)) / max vertical displacement during indentation (nm)×100. EXAMPLES
[0069] The present invention will be described in more detail below with reference to examples and comparative examples. However, the present invention is not limited to these. In the examples and comparative examples, "parts" means "parts by mass" and "%" means "% by mass".
[0070] <Production of Electron Beam-Curable Composition> Details of the materials used in the following Production Examples, Examples and Comparative Examples are as follows. <(Meth)acrylate compounds> Miramer M122: MIWON, LA (lauryl acrylate) TPGDA: Daicel-Allnex Corporation's TPGDA (tripropylene glycol di Acrylate) Miramer M300: MIWON, TMPTA (trimethylolpropane triacrylate) LAROMER LR 8863: BASF, TMP(EO)3TA (EO (3 mole) modified trimethylolpropane triacrylate) Miramer M3160: MIWON, TMP(EO)6TA (EO(6 mole) modified trimethylolpropane triacrylate) Miramer M3190: MIWON, TMP(EO)9TA (EO (9 mole) modified trimethylolpropane triacrylate) Miramer M3150: MIWON, TMP(EO)15TA (EO (15 mol) modified trimethylolpropane triacrylate) Etermer EM 2381: Eternal Materials, TMP(PO)3TA (PO(3 mole) modified trimethylolpropane triacrylate) A-TMPT-6PO: Shin-Nakamura Chemical Co., Ltd., TMP(PO)6TA (PO(6 mol) modified trimethylolpropane triacrylate) Miramer M600: Made by MIWON, DPHA (dipentaerythritol hexaacrylate) EBECRYL 130: Daicel-Allnex, TCDDA (tricyclodecane diacrylate) EBECRYL 230: Daicel-Allnex, aliphatic urethane acrylate (with 2 acryloyl groups) EBECRYL 8411: Daicel-Allnex, aliphatic urethane acrylate (with 2 acryloyl groups) SR355NS: Sartomer, ditrimethylolpropane tetraacrylate <Resin fine particles> ·Sekisui Techpolymer BM30X-5: Sekisui Plastics Co., Ltd., average particle size 5μm, acrylic resin fine particles ·Sekisui Techpolymer BM30X-8: Sekisui Plastics Co., Ltd., average particle size 8μm, acrylic resin fine particles ·Sekisui Techpolymer BM30X-12: Sekisui Plastics Co., Ltd., average particle size 12μm, acrylic resin fine particles <Leveling agent> TEGO Rad 2300: Evonik, polyether-modified polydimethylsiloxane resin with acryloyl groups <Extender pigment> AEROSIL R972: Manufactured by Nippon Aerosil Co., Ltd., average primary particle size 16 nm, specific surface area 110 m 2 / g, fumed silica) <Photopolymerization initiator> OMNIRAD 1173: IGM Resins, 2-hydroxy-2-methylpropiophenone <Pigments for ink creation> MOGAL E: Pigment manufactured by Bilra Carbon <Dispersant for ink production> Solsperse 32000: Dispersant manufactured by Lubrizol <Antifoaming agent for ink production> BYK-1790: Defoamer manufactured by BYK <Water-based overcoat varnish> JS 1269 PO Matte Register: Toyo Ink Co., Ltd. <Solvent-based overcoat varnish> HW870 AQUALIONA A Soft Matte Varnish: Toyo Ink Co., Ltd.
[0071] <Production of Electron Beam-Curable Composition> (Production Example 1) A mixture of 76.0 parts of LAROMER LR 8863, 10.0 parts of TPGDA, 10.0 parts of Miramer M600, 0.5 parts of Sekisui Techpolymer BM30X-5, 0.5 parts of TEGO Rad 2300, and 3.0 parts of AEROSIL R972 was mixed and stirred using a rotation / revolution mixer to obtain an electron beam curable composition.
[0072] (Examples 2 to 21) Electron beam curable compositions of Production Examples 2 to 21 were obtained in the same manner as in Example 1, except that materials were used according to the compositions shown in Table 1.
[0073] (Production Example 22) 23 parts of MOGAL E, 6 parts of EBECRYL 8411, 3 parts of Miramer M122, 10 parts of TPGDA, 46.5 parts of Laromer LR 8863, 5 parts of SR355NS, 6 parts of Solsperse 32000, and 0.5 parts of BYK-1790 were mixed in a mixing ratio of 1:1, and milled on a three-roll mill to prepare an electron beam curable flexographic ink.
[0074] <Production of Laminate> Example 1 The electron beam curable composition obtained in Production Example 1 was used to print on a substrate by flexographic printing. The printed coating was immediately irradiated with an electron beam to form a cured coating, thereby producing a laminate. More specifically, the process is as follows. The printing machine used was a Flexiproof 100 manufactured by RK Print Coat Instruments. The printing conditions were a printing speed of 60 m / min, anilox roll line count of 300 lines / inch, and anilox roll cell capacity of 13.09 cm. 3 / m 2 The engraving pattern on the anilox roll was hexagonal. The plate material used was DuPont ESXQ, and the area of the plate material was 106.8 cm. 2 The amount of the electron beam curable composition applied was 2.5 to 3.5 g / m after curing. 2 It was printed so that The electron beam irradiation was carried out using an electron beam irradiator EC250 / 15 / 180L manufactured by Iwasaki Electric Co., Ltd. under conditions of an acceleration voltage of 110 kV and an electron dose of 30 kGy. The substrate was a laminate substrate of a biaxially oriented polypropylene film and a non-oriented polypropylene film. An electron beam curable composition was printed on the biaxially oriented polypropylene film side of the laminate substrate. The laminate substrate was prepared as follows.
[0075] (Method of manufacturing laminated substrate) The diluted adhesive solution was applied to a biaxially oriented polypropylene film (product name: FOR-BT, thickness 20 μm) manufactured by Futamura Chemical Co., Ltd., and the solvent was allowed to evaporate. The diluted adhesive solution was prepared by diluting the adhesive (TM-321A / TM-321B = 2 / 1 manufactured by Toyo-Morton Co., Ltd.) with ethyl acetate so that the active ingredient was 30%. The diluted adhesive solution was applied at room temperature using a bar coater until the solid coating amount after the solvent had evaporated was 2.0 to 2.5 g / m2. 2 The film was then adjusted so that the adhesive was applied to the film. The adhesive-coated surface of the film was then bonded to a non-oriented polypropylene film (FHK 30 μm, manufactured by Futamura Chemical Co., Ltd.). The film was then left for 24 hours in an environment of 35° C. and humidity 60% RT to 80% RT to obtain a laminated substrate. The hardness and recovery rate of the varnish layer of the obtained laminate were measured by the above-mentioned method. The results are shown in Table 1.
[0076] (Examples 2 to 14, Comparative Examples 1 to 7) Laminates of Examples 2 to 14 and Comparative Examples 1 to 7 were obtained in the same manner as in Example 1, except that the types of varnish and base material shown in Table 1 were used. The hardness and recovery rate of the varnish layer of the obtained laminates were measured by the methods described above. The results are shown in Table 1.
[0077] Example 15 The electron beam-curable ink prepared in Production Example 22 was printed on a substrate by flexographic printing in the same manner as in Example 1, and cured by electron beam under the same conditions as in Example 1 to produce a substrate having a printed layer. A varnish layer was formed on the printed surface of the substrate having the obtained printed layer in the same manner as in Example 1, and a laminate having a printed layer between the substrate and the varnish layer was produced. The hardness and recovery rate of the varnish layer of the obtained laminate were measured by the above-mentioned method. The results are shown in Table 1.
[0078] (Comparative Examples 8 and 9) Using a commercially available overcoat varnish, printing was performed on the substrate by flexographic printing in the same manner as in Example 1. The coating film after printing was immediately dried to form a coating film, and a laminate was produced. More details are as follows. The coating was performed using the same equipment and conditions as in Example 1, and the coating amount after curing was 0.9 to 1.5 g / m 2 It was printed so that Drying was carried out at a temperature of 70° C. for a drying time of 3 minutes. The hardness of the varnish layer of the obtained laminate was measured by the method described above. An attempt was also made to measure the recovery rate of the varnish layer, but the strength of the varnish layer was too weak to measure. The results are shown in Table 1.
[0079] [Table 1]
[0080] [Table 1]
[0081] The obtained laminate was evaluated as follows. The evaluation results are shown in Table 1.
[0082] [Heat resistance] The obtained laminate was heated twice from the printed side at 180°C, 0.25 MPa, and 1 second using a heat sealer (TP-705 Ring Seal Tester, Tester Sangyo Co., Ltd.), and the varnish layer in the heat-sealed area was evaluated for cracking and peeling. A rating of 3 or higher is practically preferable. (Evaluation Criteria) 5: A few cracks, no peeling 4: Cracks, no peeling 3: A few cracks, no peeling 2: Many cracks, no peeling 1: Peeling occurs
[0083] [Solvent resistance] The obtained laminate was rubbed with a cotton swab dipped in a 99.5% ethanol solution at a rate of one stroke per second, and the number of strokes until the surface of the cured coating film was scraped off was measured. A rating of 3 or higher is practically preferable. (Evaluation Criteria) 5:50 or more times 4: 40 to less than 50 times 3: 20 to less than 30 times 2: 10 to less than 20 times Less than 1:10 times
[0084] [Slip resistance] The dynamic friction coefficient of the obtained laminate was measured using a friction tester (friction tester HM-3, manufactured by Toyo Seiki Seisakusho, speed 100 mm / min, moving distance 50 mm, sled 63 mm×63 mm, 200 g). A rating of 2 or higher is practically preferable. (Evaluation Criteria) 3: Dynamic friction coefficient less than 0.40 2: Dynamic friction coefficient 0.40 or more and less than 0.45 1: Dynamic friction coefficient 0.45 or more
[0085] [Odor] The obtained laminate was cut into a size of 89 mm x 120 mm, and odor intensity immediately after printing was evaluated by five people and the average value was used for evaluation. A rating of 3 or higher is practically preferable. (Evaluation Criteria) 4: Almost no odor was detected 3: A slight odor was detected 2: The odor was clearly noticeable 1: The odor was strong
[0086] In Examples 1 to 15, the (meth)acrylate compound contained 80% by mass or more of a compound having two or more (meth)acryloyl groups in the molecule, and the varnish layer was made using a composition that did not substantially contain a photopolymerization initiator, and the hardness of the laminate was 100 to 180 MPa, and the recovery rate was 77 to 100%. As a result, the heat resistance, slip property, solvent resistance, and low odor were at practical levels. On the other hand, in Comparative Example 1, the hardness was less than 100 MPa, and the heat resistance and solvent resistance were insufficient, which is considered to be due to the influence of the low crosslink density. In Comparative Example 2, a large amount of a compound having one (meth)acryloyl group in the molecule was used, and as in Comparative Example 1, the hardness was low, and the heat resistance and solvent resistance were insufficient. In Comparative Example 3, the recovery rate was less than 77%, and the heat resistance was insufficient. This is thought to be because the coating film had a moderate hardness but was highly brittle. Comparative Example 4 contained 20% by mass of an inert resin having no (meth)acryloyl group, and the compound having two or more (meth)acryloyl groups in the molecule was less than 80% by mass of the total amount of the composition, and the hardness was less than 100 MPa, and the solvent resistance and slip property were insufficient. This is thought to be because the inert resin not incorporated in the crosslinking was also present on the surface of the coating film. In Comparative Example 5, the hardness exceeded 180 MPa and the recovery rate was less than 77%, and the heat resistance was insufficient. In Comparative Example 6, the recovery rate was within the range, but the hardness exceeded 180 MPa and the heat resistance was insufficient. Comparative Examples 5 and 6 show that the heat resistance during heat sealing cannot be satisfied by simply increasing the hardness. Comparative Example 7 is a system containing a photopolymerization initiator, and the photopolymerization initiator and its decomposition products become inert components. In addition to having inferior heat resistance compared to a system that does not substantially contain a photopolymerization initiator, the photopolymerization initiator and its decomposition products have a strong odor, making it unsuitable for practical use. Comparative Examples 8 and 9 are laminates that use oil-based varnish and water-based varnish as varnish layers, which are not active energy ray curable. Compared with active energy ray curable types, the hardness is significantly smaller, and the recovery rate cannot be measured. As a result, the heat resistance and solvent resistance are significantly inferior. In addition, the odor that seems to be caused by residual agents is strong.
[0087] As is clear from the above, it has been proven that the laminate of the present invention has heat resistance, slip properties, solvent resistance and low odor properties by setting the hardness and recovery rate within specific ranges.
Claims
1. A laminate having a heat seal layer, a substrate, and a varnish layer in this order, The varnish layer is formed by curing an electron beam curable composition containing a (meth)acrylate compound with an electron beam. This is a layer The (meth)acrylate compound has two or more (meth)acryloyl groups in the molecule. the electron beam curable composition contains a compound having the formula (I) in an amount of 80 mass % or more based on the total amount of the electron beam curable composition; The compound having two or more (meth)acryloyl groups in the molecule is selected from the group consisting of alkylene oxide-modified (3 to 9 mol / mol) trimethylolpropane triacrylate, tripropylene glycol di(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and 1,9-nonanediol di(meth)acrylate. , 1,10-decanediol di(meth)acrylate, 1,2-dodecanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polyethylene glycol (200) di(meth)acrylate, polyethylene glycol (300) di(meth)acrylate, polyethylene glycol (400) di(meth)acrylate, polyethylene glycol (600) di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, EO-modified 1,6-Hexanediol di(meth)acrylate, PO-modified neopentyl glycol di(meth)acrylate, (neopentyl glycol-modified) trimethylolpropane di(meth)acrylate, dimethyloltricyclodecane di(meth)acrylate, EO-modified bisphenol A di(meth)acrylate, PO-modified bisphenol A di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, dimethyloltricyclodecane di(meth)acrylate, dicyclopentanyl di(meth)acrylate, tris(2-hydroxyethyl)isocyanurate di(meth)acrylate trimethylolpropane tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, glycerin propoxy triacrylate, ε-caprolactone-modified tris-(2-acryloxyethyl)isocyanurate, ethoxylated isocyanuric acid tri(meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, and dipentaerythritol penta(meth)acrylate, the (meth)acrylate compound contains two or more compounds selected from the group consisting of alkylene oxide-modified (3 to 9 mol / mol) trimethylolpropane triacrylate, tripropylene glycol diacrylate, and dipentaerythritol hexaacrylate, and when dipentaerythritol hexaacrylate is contained, the content of dipentaerythritol hexaacrylate is 50 mass% or less based on the total amount of the electron beam-curable composition; the electron beam curable composition is substantially free of a photopolymerization initiator, The varnish layer has a hardness of 100 to 180 MPa as measured by nanoindentation and a recovery rate of 77 to 100% as measured by nanoindentation.
2. The laminate according to claim 1 , further comprising a printed layer between the substrate and the varnish layer.
3. The laminate according to claim 1, wherein the (meth)acrylate compound comprises alkylene oxide-modified (3 to 9 mol / mol) trimethylolpropane triacrylate.
4. 2. The laminate according to claim 1, wherein the electron beam curable composition further comprises an extender pigment.
5. The laminate according to claim 1 , wherein the electron beam curable composition further contains resin fine particles.
6. The laminate according to claim 1 , wherein the electron beam curable composition further comprises a leveling agent.
7. A packaging material comprising the laminate according to any one of claims 1 to 6.
8. 7. The method for producing a laminate according to claim 1, wherein the conditions for curing with electron beams are an acceleration voltage of 50 to 200 kV and an exposure dose of 15 to 200 kGy.
Citation Information
Patent Citations
Photopolymerizable resin composition
JP2007204543A
Active energy ray-curable resin composition and laminate and molding using cured film of the same
JP2015227437A
Barrier laminate, packaging product, and manufacturing method of barrier laminate
JP2022093288A
Electron beam curable composition and electron beam curable overcoat varnish
JP2022132010A
JPP7371809B