Metallic acid compound-containing liquid and method for producing same
By using low-environmental-influence liquids with components such as trivalent amines and hydrogen peroxide in the production of metallic acid salts, the equipment demand and high waste liquid treatment cost are solved due to the use of high-content ammonia aqueous solution, and the production effect with high diffusion and low environmental impact is achieved.
Patent Information
- Application Number
- JP2024527501
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-02-03
- Filing Date
- 2024-02-02
- Publication Date
- 2025-03-24
- Estimated Expiration
- 2044-02-02
AI Technical Summary
In the production of high-diversity metallic acid liquids, the use of high-content aqueous ammonia solution is required, which leads to an increase in equipment demand and high waste liquid treatment costs, and has a great impact on the environment.
By using a metallic acid containing liquid with low environmental impact, the liquid consists of metal and semi-metal elements with trivalent amines and hydrogen peroxide as the main components, and the particle diameter (D50) was determined to be 1000 nm or less by dynamic light scattering.
The production of metallic acid liquid containing low environmental impact and high diffusion has been achieved, reducing the cost of waste liquid treatment, and improving the environmental protection and production efficiency of the process.
Smart Images

Figure 0007650408000001 
Figure 0007650408000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a metallic acid compound-containing liquid and a method for producing the same. [Background technology]
[0002] Metal acid compound-containing liquids, which are liquids containing oxides of rare metals and semimetal elements such as tantalum (Ta), niobium (Nb), titanium (Ti), molybdenum (Mo), tungsten (W), zirconium (Zr), hafnium (Hf), silicon (Si), and rare earth elements, are materials used in various industrial applications. Many metal acid compound-containing liquids have low dispersibility. Therefore, development of metal acid compound-containing liquids with high dispersibility has been promoted. As one of the metal acid compound-containing liquids with high dispersibility, the applicant of the present application has disclosed a tantalic acid dispersion liquid with high dispersibility in water (Patent Document 1). The tantalum dispersion liquid disclosed in Patent Document 1 is produced by adding a tantalum salt solution to an amine aqueous solution to produce a primary reaction liquid, adding the primary reaction liquid to ammonia water to produce a secondary reaction liquid, washing the tantalum-containing precipitate produced in the secondary reaction liquid, and mixing the washed tantalum-containing precipitate with amine and water. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2022 / 018980 Summary of the Invention [Problem to be solved by the invention]
[0004] However, in order to produce the tantalum dispersion liquid disclosed in Patent Document 1, it is necessary to use a high-content amine aqueous solution, which requires dedicated equipment, and the high-content amine aqueous solution used in the neutralization process is in an excessive amount, which results in huge waste liquid treatment costs for the amine aqueous solution. Furthermore, from the perspective of the SDGs, there is a demand for measures to reduce the environmental burden, such as reducing the amount of high-content amine aqueous solution used.
[0005] In view of the above problems, the present invention provides a metal acid compound-containing liquid that has a low environmental impact and high dispersibility, and a method for producing the same. [Means for solving the problem]
[0006] The metal acid compound-containing liquid of the present invention, which has been made to solve the above problems, is a metal acid compound-containing liquid containing a metal and / or metalloid element and a tertiary amine compound, and is characterized in that the particle diameter (D50) of particles in the metal acid compound-containing liquid measured by dynamic light scattering method is 1000 nm or less. The metal acid compound-containing liquid of the present invention is a metal acid compound-containing liquid containing a metal and / or metalloid element and a tertiary amine compound, and has a particle diameter (D50) of 1000 nm or less as measured by dynamic light scattering, thereby having a low environmental impact and excellent dispersibility.
[0007] The metal acid compounds in the metal acid compound-containing liquid of the present invention are presumed to exist in the liquid as polymetal acid polynuclear complex ions in which metal atoms or metalloid atoms and oxygen atoms are multi-stage condensed in the liquid.Furthermore, the metal acid compounds also include those that exist in the liquid as ions in an ionic state with these metal oxides and alkali metals such as lithium.
[0008] The metal and / or metalloid element contained in the metal acid compound-containing liquid of the present invention is preferably one or more elements selected from Ta, Nb, Ti, Zr, Mo, W, Hf, Si, and rare earth elements.
[0009] In addition, since a tertiary amine compound is used in the manufacturing method of the metal acid compound-containing liquid of the present invention described below, the metal acid compound-containing liquid of the present invention contains a tertiary amine compound.
[0010] It is presumed that the tertiary amine compound in the metallic acid compound-containing liquid of the present invention is present in the liquid as an ion in an ionic state with a metal and / or metalloid element.
[0011] The tertiary amine compound contained in the metal acid compound-containing liquid of the present invention is preferably a tertiary amine compound having 3 to 9 carbon atoms from the viewpoint of good dispersibility and affinity with solvents such as water. Moreover, the tertiary amine compound is more preferably one or more selected from the group consisting of trimethylamine, triethylamine, and tri-n-propylamine.
[0012] The method for measuring the content of the tertiary amine compound in the metal acid compound-containing liquid of the present invention includes gas chromatography (GC), liquid chromatography (LC), mass spectrometry (MS), gas chromatography-mass spectrometry (GC-MS), liquid chromatography-mass spectrometry (LC-MS), etc. In particular, measurement by liquid chromatography (LC) or liquid chromatography-mass spectrometry (LC-MS) is preferred.
[0013] In the present invention, when the particle diameter D50 of the particles in the metal acid compound-containing liquid is 1000 nm or less in particle diameter distribution measurement using a dynamic light scattering method, it is preferable from the viewpoint of stability due to small changes over time, formation of a good coating film with few uncovered areas during film formation, and securing a sufficient coating weight.Furthermore, when the particle diameter (D50) of the particles in the metal acid compound-containing liquid is smaller, it is preferable from the viewpoint of stability due to small changes over time, formation of a good coating film with few uncovered areas during film formation, and securing a sufficient coating weight. The particle diameter (D50) of the particles in the metal acid compound-containing liquid is more preferably 900 nm or less, more preferably 800 nm or less, particularly preferably 700 nm or less, more preferably 600 nm or less, more preferably 500 nm or less, particularly preferably 400 nm or less, more preferably 300 nm or less, more preferably 200 nm or less, particularly preferably 100 nm or less, more preferably 80 nm or less, more preferably 50 nm or less, particularly preferably 30 nm or less, more preferably 20 nm or less, more preferably 10 nm or less, particularly preferably 5 nm or less, and most preferably 3 nm or less. Thus, the particle diameter (D50) of the particles in the metal acid compound-containing liquid of the present invention is measured using a dynamic light scattering method, and the liquid in which the particle diameter (D50) of the particles is 1000 nm or less is the "metal acid compound-containing liquid" of the present invention.
[0014] Here, the dynamic light scattering method is a method in which a solution such as a suspension solution is irradiated with light such as a laser beam to measure the light scattering intensity from a group of particles undergoing Brownian motion, and the particle size and distribution are obtained from the temporal variation of the intensity. Specifically, the particle size distribution is evaluated in accordance with JIS Z 8828:2019 "Particle Size Analysis - Dynamic Light Scattering Method" using a zeta potential, particle size, and molecular weight measurement system (manufactured by Otsuka Electronics Co., Ltd.: ELSZ-2000ZS). Just before the measurement, the solution is filtered through a filter with a pore size of 2 μm, and ultrasonic treatment is performed for 3 minutes at 28 kHz using an ultrasonic cleaner (manufactured by As One Co., Ltd.: VS-100III). The particle size (D50) refers to the median diameter (D50), which is the particle size that indicates the 50% cumulative value of the cumulative distribution curve. Furthermore, in this specification, unless otherwise specified, "particle diameter (D50)" includes both "initial particle diameter D50", which indicates the particle diameter (D50) of particles in the metal acid compound-containing liquid of the present invention whose liquid temperature is adjusted to 25°C immediately after production, and "time-dependent particle diameter D50", which indicates the particle diameter (D50) of particles in the metal acid compound-containing liquid of the present invention after the metal acid compound-containing liquid of the present invention has been left undisturbed for 20 days from the day the liquid is produced in an incubator set at room temperature of 25°C.
[0015] In the present invention, the "containing liquid" is not limited to a solute dispersed or mixed in a solvent in a single molecular state, but also includes an aggregate in which a plurality of molecules are attracted to each other by intermolecular interactions, such as (1) polymer molecules, (2) solvated molecules, (3) molecular clusters, and (4) colloidal particles dispersed in a solvent.
[0016] In addition, the metal acid compound-containing liquid of the present invention is a metal acid compound-containing liquid containing a metal and / or metalloid element and a tertiary amine compound, and is characterized in that the maximum transmittance of the metal acid compound-containing liquid in the wavelength range of 550 nm to 700 nm is 70%T or more. The metal acid compound-containing liquid of the present invention is a metal acid compound-containing liquid containing a metal and / or metalloid element and a tertiary amine compound, and since the maximum transmittance of the metal acid compound-containing liquid in the wavelength range of 550 nm to 700 nm is 70%T or more, the metal acid compound-containing liquid has a low environmental impact and excellent dispersibility.
[0017] The metal and / or metalloid element and tertiary amine compound contained in the metal acid compound-containing liquid of the present invention are as described above, and therefore a detailed description thereof will be omitted.
[0018] The metal acid compound-containing liquid of the present invention is preferably such that the maximum transmittance in the wavelength region of 550 nm to 700 nm is 70%T or more, since the degree of dispersion is high and the uniformity of the liquid components is excellent. The maximum transmittance in the wavelength region of 550 nm to 700 nm is more preferably 75%T or more, even more preferably 80%T or more, particularly preferably 85%T or more, more preferably 90%T or more, even more preferably 95%T or more, particularly preferably 98%T or more, even more preferably 99%T or more, and most preferably 100%T or more. Note that if the measured value exceeds 100%T due to measurement error of the spectrophotometer used to measure the transmittance, it is considered to be 100%T.
[0019] Furthermore, in the metal acid compound-containing liquid of the present invention, at least one of the transmittances at wavelengths of 550 nm, 600 nm, 650 nm, and 700 nm is preferably 70% T or more, more preferably 75% T or more, even more preferably 80% T or more, particularly preferably 85% T or more, more preferably 90% T or more, even more preferably 95% T or more, particularly preferably 98% T or more, even more preferably 99% T or more, and most preferably 100% T or more. Note that if the measured value exceeds 100% T due to measurement error of the spectrophotometer used to measure the transmittance, it is considered to be 100% T.
[0020] Furthermore, the metal acid compound-containing liquid of the present invention preferably has a minimum transmittance in the wavelength region of 550 nm to 700 nm of 70% T or more, more preferably 75% T or more, even more preferably 80% T or more, particularly preferably 85% T or more, more preferably 90% T or more, even more preferably 95% T or more, particularly preferably 98% T or more, even more preferably 99% T or more, and most preferably 100% T or more. Note that if the measured value exceeds 100% T due to measurement error of the spectrophotometer used to measure the transmittance, it is considered to be 100% T.
[0021] Thus, the metal acid compound-containing liquid of the present invention is a liquid in a state in which the maximum value of the transmittance in the wavelength region of 550 nm to 700 nm is 70%T. Furthermore, in this specification, unless otherwise specified, "transmittance" includes both "initial transmittance" which indicates the transmittance of the metal acid compound-containing liquid of the present invention adjusted to a liquid temperature of 25°C immediately after production, and "temporary transmittance" which indicates the transmittance of the metal acid compound-containing liquid of the present invention after it has been left to stand for one month from the day the metal acid compound-containing liquid of the present invention was produced in an incubator set at room temperature of 25°C.
[0022] Here, the transmittance in the wavelength region of 550 nm to 700 nm is measured for the metal acid compound-containing liquid of the present invention using a spectrophotometer in accordance with the following transmittance measurement conditions and in accordance with JIS K 0115, 2004 "General rules for spectrophotometric analysis methods."
[0023] =Transmittance measurement conditions= Measurement equipment: UV-Vis-NIR spectrophotometer UH4150 (manufactured by Hitachi High-Tech Science Corporation) Measurement mode: Wavelength scan Data mode: %T (transparent) Measurement wavelength range: 200nm~2000nm Scan speed: 600nm / min Sampling interval: 2nm
[0024] In addition, the metal acid compound-containing liquid of the present invention is characterized in that the content of the metal and / or metalloid element in the metal acid compound-containing liquid is more than 0 mass% and less than 30% in terms of metal equivalent of the metal and / or metalloid element. The content of the metal and / or metalloid element in the metal acid compound-containing liquid of the present invention is preferably 0.1% by mass or more and 30% by mass or less in terms of metal conversion of the metal and / or metalloid element, in terms of improving the liquid stability of the metal acid compound-containing liquid of the present invention. The content of the metal and / or metalloid element in the metal acid compound-containing liquid is more preferably 0.1% by mass or more and 25% by mass or less, even more preferably 0.15% by mass or more and 20% by mass or less, and particularly preferably 0.15% by mass or more and 15% by mass or less in terms of metal conversion of the metal and / or metalloid element.
[0025] Here, the content of metal and / or metalloid elements in the metal acid compound-containing liquid of the present invention is calculated by diluting the liquid appropriately with dilute hydrochloric acid as necessary, and measuring the mass fraction of the metal and / or metalloid elements in metal equivalent using inductively coupled plasma optical emission spectrometry (ICP optical emission spectrometry (AG-5110 manufactured by Agilent Technologies)) in accordance with JIS K0116:2014.
[0026] The metallic acid compound-containing liquid of the present invention is characterized in that it contains hydrogen peroxide in addition to the above-mentioned metal and / or metalloid element and tertiary amine compound. Since hydrogen peroxide water is used in the manufacturing method of the metal acid compound-containing liquid of the present invention described below, the metal acid compound-containing liquid of the present invention may contain hydrogen peroxide.
[0027] The hydrogen peroxide according to the present invention includes hydrogen peroxide ionized in the metal acid compound-containing liquid of the present invention. As will be described in detail later in the method for producing a metal acid compound-containing liquid of the present invention, it is believed that the addition of hydrogen peroxide in the production process causes anion species containing a metal element and / or a metalloid element to complex, forming a peroxo complex with excellent dissolution stability.
[0028] The amount of hydrogen peroxide present in the hydrogen peroxide-containing liquid is quantitatively analyzed, for example, by measuring the absorbance of the hydrogen peroxide-containing liquid at a wavelength of 410 nm using a spectrophotometer (U-2900 manufactured by Hitachi, Ltd.) to quantify the amount of hydrogen peroxide present in the hydrogen peroxide-containing liquid.
[0029] The metallic acid compound-containing liquid of the present invention may further contain a resin. The metal acid compound-containing liquid of the present invention is preferably one that contains a resin, since the resin is uniformly compatible with the metal acid compound and acts to adhere to the substrate, thereby improving film-forming properties and adhesion to the substrate.
[0030] Examples of the resin contained in the metal acid compound-containing liquid include polyolefin-based compounds and polyvinyl-based compounds.
[0031] Furthermore, the resin contained in the metal acid compound-containing liquid of the present invention may be an anionic water-soluble resin and / or a nonionic water-soluble resin. When the resin contained in the metal acid compound-containing liquid of the present invention is an anionic water-soluble resin and / or a nonionic water-soluble resin, the anionic water-soluble resin and / or the nonionic water-soluble resin is uniformly compatible with the above-mentioned metal acid compound and acts to adhere to the substrate, thereby improving the film-forming properties and adhesion to the plastic film substrate.
[0032] Here, the cationic water-soluble resin is a resin that has a positive charge in the polymer in water of pH=7, and has a functional group of, for example, any one of amino group, imino group, tertiary amine group, quaternary ammonium group, and hydrazino group. The anionic water-soluble resin is a resin that has a negative charge in the polymer in water of pH=7, and has a functional group of, for example, any one of carboxyl group, sulfone group, sulfate ester group, and phosphate ester group. Furthermore, the nonionic water-soluble resin is a resin that does not fall under the above-mentioned cationic water-soluble resin or anionic water-soluble resin, and has a functional group of, for example, any one of hydroxyl group, ether group, and amide group in the polymer.
[0033] Furthermore, these resins may contain one or more water-soluble homopolymers selected from the group consisting of acrylic polymers, urethane polymers, styrene polymers, olefin polymers, amide polymers, siloxane polymers, epoxy polymers, vinyl chloride polymers, and vinyl acetate polymers, and / or water-soluble copolymers consisting of two or more of these polymers. In particular, it is preferable that the resins contain one or more water-soluble homopolymers of acrylic polymers, styrene polymers, and olefin polymers, and / or water-soluble copolymers consisting of two or more of these polymers.
[0034] The metal acid compound-containing liquid of the present invention may further contain a high-boiling point solvent. The high-boiling point solvent is preferably a solvent having a boiling point of 180° C. or higher at 1 atmospheric pressure, and examples of the high-boiling point solvent include polyhydric alcohol solvents and glycol solvents.
[0035] Here, examples of polyhydric alcohol solvents include glycerin (boiling point: 290°C), 1,6-hexanediol (boiling point: 250°C), and 1,7-heptanediol (boiling point: 259°C). Examples of glycol solvents include ethylene glycol (boiling point: 197.3°C), propylene glycol (boiling point: 188.2°C), diethylene glycol (boiling point: 244.3°C), triethylene glycol (boiling point: 287.4°C), oligoethylene glycol (boiling point: 287°C to 460°C), polyethylene glycol (PEG) (boiling point: 460°C or higher), polyethylene glycol (PEG)-polypropylene glycol (PPG) copolymer (boiling point: 460°C). or higher), diethylene glycol monohexyl ether (boiling point: 260°C), polyoxyalkylene monoalkyl ether (boiling point: 260°C or higher), polyoxyethylene sorbitan monolaurate (boiling point: 321°C or higher), other anionic fluorosurfactants (boiling point: 180°C or higher), amphoteric fluorosurfactants (boiling point: 180°C or higher), nonionic fluorosurfactants (boiling point: 180°C or higher), amine oxides (boiling point: 180°C or higher), etc. are particularly preferred. Glycerin is particularly preferred. The above boiling points are those at 1 atmospheric pressure.
[0036] In addition, since a high boiling point solvent has a high boiling point, if the boiling point at 1 atmospheric pressure is excessively high, the high boiling point solvent may decompose before boiling, making it impossible to measure the boiling point accurately. In such a case, the boiling point at reduced pressure may be measured and converted to the boiling point at 1 atmospheric pressure using a general-purpose boiling point conversion table.
[0037] Furthermore, the metal acid compound-containing liquid of the present invention may contain, as unavoidable impurities, components derived from one or more metal and / or semi-metal elements, for example, Ta, Nb, Ti, Zr, Mo, W, Hf, Si, and rare earth elements, and components other than the components derived from ammonia, tertiary amine compounds, and hydrogen peroxide (hereinafter referred to as "other components"), to the extent that the action and effect of the liquid are not impaired.
[0038] The metal acid compound-containing liquid of the present invention may contain additives such as dispersants, pH adjusters, colorants, thickeners, wetting agents, and binder resins, depending on the intended use.
[0039] The composite metal acid compound-containing liquid of the present invention is a liquid containing a metal acid compound of the present invention and Li, Na, M g and at least one element A selected from the group consisting of Al, K, Ca, V, Mn, Fe, Co, Ni, Cu, Zn, Sn, Sr, and Ba. It is presumed that in the complex metal acid compound-containing liquid of the present invention, the complex metal acid compound of the present invention and element A are present in the form of ions in an ionic bond therebetween.
[0040] The element A may contain compounds such as Li, Na, Mg, Al, K, Ca, V, Mn, Fe, Co, Ni, Cu, Zn, Sn, Sr, and Ba. Here, examples of the compounds include oxides, alkali metal salts of metal acids, alkaline earth metal salts of metal acids, chlorides, metal alkoxides, and polyoxometalates. In addition, the content of element A in the composite metal acid compound-containing liquid of the present invention is such that, when the total molar content of each element A in metal conversion is X, the molar ratio X / M of the total molar content (X) of each element A in metal conversion to the total molar content (M) of one or more metal acid compounds selected from the group consisting of Nb, Ta, Ti, Mo, W, Zr, Hf, Si, and rare earth elements in metal conversion is preferably more than 0 to 3.0, more preferably 0.0002 to 2.0. The molar ratio X / M may be 0.001 to 1.0, 0.005 to 0.8, 0.01 to 0.5, 0.1 to 0.4, or 0.2 to 0.3. Since the composite metal acid compound-containing liquid of the present invention is a uniform liquid, even if these compounds are in a suspended state, improvement in uniformity and improvement in reactivity (reaction rate) are expected. If these compounds are dissolved in the composite metal acid compound-containing liquid of the present invention to form a uniform liquid, the most favorable reactivity can be achieved.
[0041] The metal acid compound-containing film of the present invention is characterized by containing metal acid compound particles contained in the metal acid compound-containing liquid of the present invention. The metal acid compound-containing film of the present invention includes a dried film obtained by applying the metal acid compound-containing liquid of the present invention to the surface of a substrate and then drying, for example, vacuum drying, and a fired film obtained by further firing the resulting dried film. The metal acid compound-containing film of the present invention also includes a metal acid compound-containing film having different physical properties such as a crystal structure, which is produced by vacuum drying or firing the metal acid compound-containing liquid of the present invention, and may have an amorphous structure, a single crystal structure, or a polycrystalline structure.
[0042] The complex metal acid compound-containing film of the present invention is characterized in that it contains complex metal acid compound particles contained in a complex metal acid compound-containing liquid. The composite metal acid compound-containing film of the present invention includes a dried film obtained by applying the composite metal acid compound-containing liquid of the present invention to the surface of a substrate, followed by drying, for example, vacuum drying, and a fired film obtained by further firing the resulting dried film. The composite metal acid compound-containing film of the present invention also includes a metal acid compound-containing film having different physical properties, such as a crystal structure, that is produced by vacuum drying or firing the composite metal acid compound-containing liquid of the present invention, and may have an amorphous structure, a single crystal structure, or a polycrystalline structure.
[0043] The above-mentioned method for producing a metal acid compound-containing liquid of the present invention will be described below.
[0044] The method for producing a metal acid compound-containing liquid of the present invention is characterized by comprising the steps of neutralizing an acidic metal aqueous solution containing a metal and / or metalloid element with an alkaline aqueous solution to produce a precipitate containing the metal and / or metalloid element, and adding a tertiary amine compound and hydrogen peroxide to the precipitate to produce a metal acid compound-containing liquid.
[0045] A method for producing a tantalic acid compound-containing liquid, which is the metallic acid compound-containing liquid of the present invention, will be described below.
[0046] First, tantalum, tantalum oxide, tantalum hydroxide, or tantalum alkoxide is reacted with hydrofluoric acid (HF), such as an aqueous solution of hydrofluoric acid, to produce tantalum fluoride (H 2 TaF 7 ) and dissolving it in water to obtain an aqueous tantalum fluoride solution, which is an acidic metal solution. In the case of tantalum chloride, it is possible to omit the step of dissolving in hydrofluoric acid and to produce an acidic tantalum aqueous solution by adding water to tantalum chloride.
[0047] Here, the tantalum fluoride aqueous solution is prepared by adding water (e.g., pure water) to tantalum. 2 O5 It is preferable to adjust the tantalum content to 1 to 100 g / L in terms of Ta 2 O 5 When the tantalum content is 1 g / L or more, it is preferable because the tantalic acid compound hydrate is easily soluble in water. When productivity is taken into consideration, the tantalum content is more preferably 10 g / L or more, and even more preferably 20 g / L or more. 2 O 5 A conversion of 100 g / L or less is preferable since it results in a tantalic acid compound hydrate that is easily soluble in water, and in order to more reliably synthesize a tantalic acid compound hydrate that is easily soluble in water, a conversion of 90 g / L or less is more preferable, a conversion of 80 g / L or less is even more preferable, and a conversion of 70 g / L or less is particularly preferable. Note that, from the viewpoint of completely dissolving tantalum or tantalum oxide, the pH of the tantalum fluoride aqueous solution is preferably 2 or less, and more preferably 1 or less.
[0048] Next, the tantalum fluoride aqueous solution is neutralized with an alkaline aqueous solution to obtain a fluorine-containing tantalum hydrate cake. Here, the alkaline aqueous solution used to neutralize the tantalum fluoride aqueous solution is preferably 10% by mass to 30% by mass of ammonia water.
[0049] The ammonia content of the ammonia water used for neutralization is preferably 10% by mass to 30% by mass. When the ammonia content is 10% by mass, tantalum is less likely to remain undissolved, and tantalum or tantalic acid can be completely dissolved in water. On the other hand, when the ammonia content is 30% by mass or less, it is preferable because it is close to a saturated aqueous solution of ammonia.
[0050] From this viewpoint, the ammonia content of the ammonia water is preferably 10% by mass or more, more preferably 15% by mass or more, even more preferably 20% by mass or more, and particularly preferably 25% by mass or more, while the ammonia content is preferably 30% by mass or less, more preferably 29% by mass or less, and even more preferably 28% by mass or less.
[0051] In the above neutralization reaction, the amount of NH 3 The molar ratio of NH 2 / Ta is preferably 95 to 500, more preferably 100 to 450, and even more preferably 110 to 400. The amount of addition is determined based on the NH 2 / Ta molar ratio from the viewpoint of generating a tantalic acid compound that is soluble in amines or diluted ammonia water. 3 The molar ratio of NH / HF is preferably 3.0 or more, more preferably 4.0 or more, and even more preferably 5.0 or more. 3 The molar ratio of / HF is preferably 100 or less, more preferably 50 or less, and even more preferably 40 or less.
[0052] The addition time in the above-mentioned neutralization reaction is preferably within 10 minutes, more preferably within 8 minutes, and even more preferably within 5 minutes. That is, it is preferable to carry out the neutralization reaction in as short a time as possible, for example, by adding all at once, rather than gradually adding over a long period of time. The tantalum fluoride aqueous solution and ammonia water can be used at room temperature.
[0053] The fluorine-containing tantalum hydrate cake obtained by the above-mentioned neutralization reaction is decanted with dilute ammonia water using a centrifuge, and washing is repeated until the amount of liberated fluoride ions becomes 100 mg / L or less, thereby removing the fluoride ions from the fluorine-containing tantalum hydrate cake and obtaining a tantalum-containing precipitate. Since the fluorine-containing tantalum hydrate cake obtained by the above-mentioned neutralization reaction contains fluorine compounds such as ammonium fluoride as impurities, it is preferable to remove these.
[0054] The tantalum content of the obtained tantalum-containing precipitate was measured by taking a part of the tantalum-containing precipitate, drying it at 110°C for 24 hours, and then calcining it at 1000°C for 4 hours. 2 O 5 The Ta generated in this way 2 O 5The weight of the precipitate is measured, and the tantalum content of the tantalum-containing precipitate can be calculated from the weight.
[0055] The cleaning liquid used to remove fluoride ions is preferably dilute ammonia water. Specifically, dilute ammonia water of 1 mass% or more and 35 mass% or less is preferable. In such dilute ammonia water, ammonia and ammonium ions are suitable for fluorine, and unnecessary cost increase can be avoided.
[0056] The method for removing the fluorine compounds is arbitrary, and may be, for example, a method using a membrane such as reverse osmosis filtration, ultrafiltration, or microfiltration using ammonia water or pure water, or centrifugation or other known methods. In addition, when removing fluoride ions from the fluorine-containing tantalum hydrate cake, there is no particular need to adjust the temperature, and the removal can be carried out at room temperature.
[0057] A tertiary amine compound and pure water are added to the obtained tantalum-containing precipitate and stirred for 10 minutes to obtain a tantalum-containing mixed liquid. After that, 35% by mass of hydrogen peroxide is added to the tantalum-containing mixed liquid and stirred for 30 minutes to obtain a tantalic acid compound-containing liquid.
[0058] From the viewpoint of solubility, the tertiary amine compound is preferably mixed so that the content of the tertiary amine compound in the tantalum-containing mixed solution is 30% by mass or less, and more preferably 20% by mass or less. From the same viewpoint, the tertiary amine compound is preferably mixed so that the content of the tertiary amine compound in the tantalum-containing mixed solution is 0.1% by mass or more, and more preferably 1% by mass or more, and may be 5% by mass or more, or may be 10% by mass or more. Furthermore, the tertiary amine compound is preferably one or more selected from trimethylamine, triethylamine, and tri-n-propylamine.
[0059] The hydrogen peroxide content of the hydrogen peroxide solution is preferably 0.5% by mass to 35% by mass. The hydrogen peroxide is preferably in a molar ratio of hydrogen peroxide to tantalum of H 2O 2 It is preferable to add hydrogen peroxide so that / Ta is 0.6 or more and 1.5 or less, and since there is a possibility that hydrogen peroxide may decompose during mixing, it is more preferable that it is 0.7 or more and 1.2 or less.
[0060] The above-mentioned method for producing a tantalic acid compound-containing liquid preferably includes a step of removing hydrogen peroxide from the obtained tantalic acid compound-containing liquid, because if hydrogen peroxide is contained in the tantalic acid compound-containing liquid, a gas generated by decomposition of hydrogen peroxide will fill the inside of a sealed container, causing the container to expand or, in the worst case, burst.
[0061] The hydrogen peroxide can be removed by any method, for example, stirring under open or reduced pressure conditions, or drying under reduced pressure.
[0062] A method for producing a niobium compound-containing liquid, which is a metal acid compound-containing liquid of the present invention, will be described below. Note that the description of the same points as those of the above-mentioned method for producing a tantalic acid compound-containing liquid will be omitted.
[0063] First, niobium, niobium oxide, or niobium hydroxide is reacted with hydrofluoric acid (HF), such as an aqueous solution of hydrofluoric acid, to produce niobium fluoride (H 2 NbF 7 ) and dissolving it in water to obtain an aqueous niobium fluoride solution, which is an acidic metal solution. In the case of niobium chloride, it is possible to omit the step of dissolving in hydrofluoric acid and to produce an aqueous acidic niobium solution by adding water to niobium chloride.
[0064] Here, the niobium fluoride solution is prepared by adding water (e.g., pure water) to convert niobium to Nb 2 O 5 It is preferable to adjust the niobium content to 1 to 100 g / L in terms of Nb 2 O 5 When the niobium content is 1 g / L or more, it is preferable because the niobium compound hydrate is easily soluble in water. When productivity is taken into consideration, it is more preferable that the niobium content is 10 g / L or more, and even more preferable that the niobium content is 20 g / L or more. 2O 5 A conversion of 100 g / L or less is preferable because it results in a niobium acid compound hydrate that is easily soluble in water, and in order to more reliably synthesize a niobium acid compound hydrate that is easily soluble in water, a conversion of 90 g / L or less is more preferable, a conversion of 80 g / L or less is even more preferable, and a conversion of 70 g / L or less is particularly preferable. Note that, from the viewpoint of completely dissolving niobium or niobium oxide, the pH of the niobium fluoride aqueous solution is preferably 2 or less, and more preferably 1 or less.
[0065] Next, the niobium fluoride aqueous solution is neutralized with an alkaline aqueous solution to obtain a fluorine-containing niobium hydrate cake. Here, the alkaline aqueous solution used to neutralize the niobium fluoride aqueous solution is preferably 10% by mass to 30% by mass ammonia water.
[0066] In the above neutralization reaction, the amount of NH 3 The molar ratio of NH / Nb is preferably 95 to 500, more preferably 100 to 450, and even more preferably 110 to 400. The amount of addition is determined based on the amount of NH / Nb, from the viewpoint of the formation of a niobate compound that dissolves in amines or diluted aqueous ammonia. 3 The molar ratio of NH / HF is preferably 3.0 or more, more preferably 4.0 or more, and even more preferably 5.0 or more. 3 The molar ratio of / HF is preferably 100 or less, more preferably 50 or less, and even more preferably 40 or less.
[0067] The addition time in the above-mentioned neutralization reaction is preferably within 10 minutes, more preferably within 8 minutes, and even more preferably within 5 minutes.
[0068] The fluorine-containing niobium hydrate cake obtained by the above-mentioned neutralization reaction is decanted with dilute ammonia water using a centrifuge, and washing is repeated until the amount of liberated fluoride ions becomes 100 mg / L or less, thereby removing the fluoride ions from the fluorine-containing niobium hydrate cake and obtaining a niobium-containing precipitate. The fluorine-containing niobium hydrate cake obtained by the above-mentioned neutralization reaction contains fluorine compounds such as ammonium fluoride as impurities, so it is preferable to remove these. The washing liquid used to remove the fluoride ions is preferably dilute ammonia water.
[0069] The niobium content of the obtained niobium-containing precipitate was measured by taking a part of the niobium-containing precipitate, drying it at 110°C for 24 hours, and then calcining it at 1000°C for 4 hours. 2 O 5 The resulting Nb 2 O 5 The weight of the precipitate is measured, and the niobium content of the niobium-containing precipitate can be calculated from the weight.
[0070] A tertiary amine compound and pure water are added to the obtained niobium-containing precipitate and stirred for 10 minutes to obtain a niobium-containing mixed liquid. After that, 35 mass% hydrogen peroxide is added to the niobium-containing mixed liquid and stirred for 30 minutes to obtain a niobic acid compound-containing liquid.
[0071] The tertiary amine compound is preferably mixed so that the content of the tertiary amine compound in the niobium-containing mixed liquid is 0.1% by mass or more and 30% by mass or less. The tertiary amine compound is preferably one or more selected from the group consisting of trimethylamine, triethylamine, and tri-n-propylamine.
[0072] The hydrogen peroxide content of the hydrogen peroxide solution is preferably 0.5% by mass to 35% by mass. The hydrogen peroxide is preferably in a molar ratio of hydrogen peroxide to niobium H 2 O 2It is preferable to add hydrogen peroxide so that / Nb is 0.6 or more and 1.5 or less, and since there is a possibility that hydrogen peroxide may decompose during mixing, it is more preferable that it is 0.7 or more and 1.2 or less.
[0073] As in the above-mentioned method for producing a tantalic acid compound-containing liquid, it is preferable to have a step of removing hydrogen peroxide from the obtained niobic acid compound-containing liquid.
[0074] A method for producing a titanic acid compound-containing liquid, which is a metallic acid compound-containing liquid of the present invention, will be described below. Note that the description of the same points as those in the above-mentioned method for producing a tantalic acid compound-containing liquid will be omitted.
[0075] First, titanium, titanium oxide, or titanium hydroxide is reacted with hydrofluoric acid (HF), such as an aqueous solution of hydrofluoric acid, to produce titanium fluoride (H 2 TiF 6 ) and dissolving it in water to obtain an aqueous titanium fluoride solution, which is an acidic metal aqueous solution. In the case of titanium chloride or titanyl sulfate, it is possible to omit the step of dissolving in hydrofluoric acid and to produce an acidic titanium aqueous solution by adding water to these.
[0076] Here, the titanium fluoride aqueous solution is prepared by adding water (e.g., pure water) to convert titanium into TiO 2 It is preferable to adjust the titanium content to 1 to 100 g / L in terms of titanium content. 2 When the titanium content is 1 g / L or more in terms of the amount of the titanium oxide, the titanium oxide hydrate is easily soluble in water, and when productivity is taken into consideration, the titanium content is more preferably 10 g / L or more, and even more preferably 20 g / L or more. 2 A titanic acid compound hydrate having a water-soluble concentration of 100 g / L or less is preferable because it will be a titanic acid compound hydrate that is easily soluble in water, and in order to more reliably synthesize a titanic acid compound hydrate that is easily soluble in water, a concentration of 90 g / L or less is more preferable, a concentration of 80 g / L or less is even more preferable, and a concentration of 70 g / L or less is particularly preferable. From the viewpoint of completely dissolving titanium or titanium oxide, the pH of the titanium fluoride aqueous solution is preferably 2 or less, and more preferably 1 or less.
[0077] Next, the titanium fluoride aqueous solution is neutralized with an alkaline aqueous solution to obtain a fluorine-containing titanium hydrate cake. Here, the alkaline aqueous solution used to neutralize the titanium fluoride aqueous solution is preferably 10% by mass to 30% by mass ammonia water.
[0078] In the above neutralization reaction, the amount of NH 3 The molar ratio of NH / Ti is preferably 95 to 500, more preferably 100 to 450, and even more preferably 110 to 400. The amount of addition is determined based on the amount of NH 3 The molar ratio of NH / HF is preferably 3.0 or more, more preferably 4.0 or more, and even more preferably 5.0 or more. 3 The molar ratio of / HF is preferably 100 or less, more preferably 50 or less, and even more preferably 40 or less.
[0079] The addition time in the above-mentioned neutralization reaction is preferably within 10 minutes, more preferably within 8 minutes, and even more preferably within 5 minutes.
[0080] The fluorine-containing titanium hydrate cake obtained by the above-mentioned neutralization reaction is decanted with dilute ammonia water using a centrifuge, and washing is repeated until the amount of liberated fluoride ions becomes 100 mg / L or less, thereby removing the fluoride ions from the fluorine-containing titanium hydrate cake and obtaining a titanium-containing precipitate. The fluorine-containing titanium hydrate cake obtained by the above-mentioned neutralization reaction contains fluorine compounds such as ammonium fluoride as impurities, so it is preferable to remove these. The washing liquid used to remove the fluoride ions is preferably dilute ammonia water.
[0081] The niobium content of the obtained titanium-containing precipitate was measured by taking a part of the titanium-containing precipitate, drying it at 110°C for 24 hours, and then calcining it at 1000°C for 4 hours to obtain TiO 2 The TiO 2 The weight of the precipitate is measured, and the titanium content of the titanium-containing precipitate can be calculated from the weight.
[0082] A tertiary amine compound and pure water are added to the resulting titanium-containing precipitate and stirred for 10 minutes to obtain a titanium-containing mixed liquid. After that, 35% by mass of hydrogen peroxide is added to the titanium-containing mixed liquid and stirred for 30 minutes to obtain a titanic acid compound-containing liquid.
[0083] The tertiary amine compound is preferably mixed so that the content of the tertiary amine compound in the titanium-containing mixed liquid is 0.1% by mass or more and 30% by mass or less. The tertiary amine compound is preferably one or more selected from the group consisting of trimethylamine, triethylamine, and tri-n-propylamine.
[0084] The hydrogen peroxide content of the hydrogen peroxide solution is preferably 0.5% by mass to 35% by mass. The hydrogen peroxide is preferably in a molar ratio of hydrogen peroxide to titanium of H 2 O 2 It is preferable to add hydrogen peroxide so that / Ti is 0.6 or more and 1.5 or less, and since there is a possibility that hydrogen peroxide may decompose during mixing, it is more preferable that it is 0.7 or more and 1.2 or less.
[0085] As in the above-mentioned method for producing a tantalic acid compound-containing liquid, it is preferable to have a step of removing hydrogen peroxide from the obtained titanic acid compound-containing liquid.
[0086] A method for producing a zirconium oxide compound-containing liquid, which is a metal oxide compound-containing liquid of the present invention, will be described below. Note that the description of the same points as those of the above-mentioned method for producing a tantalum oxide compound-containing liquid will be omitted.
[0087] First, zirconium, zirconium oxide, or titanium hydroxide is reacted with hydrofluoric acid (HF), such as an aqueous solution of hydrofluoric acid, to produce zirconium fluoride (H 2 ZrF 6 ) and dissolving it in water to obtain an acidic metal aqueous solution, that is, an aqueous zirconium fluoride solution. In the case of zirconium chloride or zirconium sulfate, it is possible to omit the step of dissolving in hydrofluoric acid and to produce an acidic titanium aqueous solution by adding water to these.
[0088] Here, the zirconium fluoride aqueous solution is prepared by adding water (e.g., pure water) to convert zirconium to ZrO 2 It is preferable to adjust the zirconium content to 1 to 100 g / L in terms of zirconium content. 2 When the zirconium content is 1 g / L or more, it is preferable because the zirconate compound hydrate is easily soluble in water, and when productivity is taken into consideration, it is more preferable that the zirconium content is 10 g / L or more, and even more preferable that the zirconium content is 20 g / L or more. 2 A converted concentration of 100 g / L or less is preferable because it results in a zirconium oxide hydrate that is easily soluble in water, and in order to more reliably synthesize a zirconium oxide hydrate that is easily soluble in water, a concentration of 90 g / L or less is more preferable, a concentration of 80 g / L or less is even more preferable, and a concentration of 70 g / L or less is particularly preferable. From the viewpoint of completely dissolving zirconium or zirconium oxide, the pH of the aqueous zirconium fluoride solution is preferably 2 or less, and more preferably 1 or less.
[0089] Next, the zirconium fluoride aqueous solution is neutralized with an alkaline aqueous solution to obtain a fluorine-containing zirconium hydrate cake. Here, the alkaline aqueous solution used to neutralize the zirconium fluoride aqueous solution is preferably 10% by mass to 30% by mass ammonia water.
[0090] In the above neutralization reaction, the amount of NH 3The molar ratio of NH 3 / Zr is preferably 95 to 500, more preferably 100 to 450, and even more preferably 110 to 400. The amount of addition is adjusted to NH 3 / Zr from the viewpoint of the formation of zirconate compounds that dissolve in amines or diluted aqueous ammonia. 3 The molar ratio of NH / HF is preferably 3.0 or more, more preferably 4.0 or more, and even more preferably 5.0 or more. 3 The molar ratio of / HF is preferably 100 or less, more preferably 50 or less, and even more preferably 40 or less.
[0091] The addition time in the above-mentioned neutralization reaction is preferably within 10 minutes, more preferably within 8 minutes, and even more preferably within 5 minutes.
[0092] The fluorine-containing zirconium hydrate cake obtained by the above-mentioned neutralization reaction is decanted with dilute ammonia water using a centrifuge, and washing is repeated until the amount of liberated fluoride ions becomes 100 mg / L or less, thereby removing the fluoride ions from the fluorine-containing zirconium hydrate cake and obtaining a zirconium-containing precipitate. The fluorine-containing zirconium hydrate cake obtained by the above-mentioned neutralization reaction contains fluorine compounds such as ammonium fluoride as impurities, so it is preferable to remove these. The washing liquid used to remove the fluoride ions is preferably dilute ammonia water.
[0093] The zirconium content of the obtained zirconium-containing precipitate was measured by taking a part of the zirconium-containing precipitate, drying it at 110°C for 24 hours, and then calcining it at 1000°C for 4 hours to obtain ZrO 2 The resulting ZrO 2 The weight of the precipitate is measured, and the zirconium content of the zirconium-containing precipitate can be calculated from the weight.
[0094] A tertiary amine compound and pure water are added to the obtained zirconium-containing precipitate and stirred for 10 minutes to obtain a zirconium-containing mixed liquid. After that, 35% by mass of hydrogen peroxide is added to the zirconium-containing mixed liquid and stirred for 30 minutes to obtain a zirconium oxide compound-containing liquid.
[0095] The tertiary amine compound is preferably mixed so that the content of the tertiary amine compound in the zirconium-containing mixed liquid is 0.1% by mass or more and 30% by mass or less. The tertiary amine compound is preferably one or more selected from the group consisting of trimethylamine, triethylamine, and tri-n-propylamine.
[0096] The hydrogen peroxide content of the hydrogen peroxide solution is preferably 0.5% by mass to 35% by mass. The hydrogen peroxide is preferably in a molar ratio H 2 O 2 It is preferable to add hydrogen peroxide so that the ratio of Zr is 0.6 or more and 1.5 or less, and since there is a possibility that hydrogen peroxide may decompose during mixing, it is more preferable that the ratio is 0.7 or more and 1.2 or less.
[0097] As in the above-mentioned method for producing a tantalic acid compound-containing liquid, it is preferable to have a step of removing hydrogen peroxide from the obtained zirconium acid compound-containing liquid.
[0098] A method for producing a silicic acid compound-containing liquid, which is a metallic acid compound-containing liquid of the present invention, will be described below. Note that the description of the same points as those of the above-mentioned method for producing a tantalic acid compound-containing liquid will be omitted.
[0099] First, silicon or silicon oxide is reacted with hydrofluoric acid (HF), such as an aqueous solution of hydrofluoric acid, to produce silicon fluoride (H 2 SiF 6 ) and dissolving it in water to obtain an aqueous solution of silicon fluoride, which is an acidic metal solution.
[0100] Here, the silicon fluoride aqueous solution is prepared by adding water (e.g., pure water) to convert silicon into SiO 2It is preferable to adjust the silicon content to 1 to 100 g / L in terms of SiO 2 When the silicon content is 1 g / L or more in terms of SiO, the silicon oxide hydrate is easily soluble in water, and when productivity is taken into consideration, the silicon content is more preferably 10 g / L or more, and even more preferably 20 g / L or more. 2 A conversion of 100 g / L or less is preferable because it results in a silicic acid compound hydrate that is easily soluble in water, and in order to more reliably synthesize a silicic acid compound hydrate that is easily soluble in water, a conversion of 100 g / L or less is more preferable, a conversion of 90 g / L or less is even more preferable, a conversion of 80 g / L or less is even more preferable, and a conversion of 70 g / L or less is particularly preferable. Note that, from the viewpoint of completely dissolving silicon or silicon oxide, the pH of the aqueous silicon fluoride solution is preferably 2 or less, and more preferably 1 or less.
[0101] Next, the silicon fluoride aqueous solution is neutralized with an alkaline aqueous solution to obtain a fluorine-containing silicon hydrate cake. Here, the alkaline aqueous solution used to neutralize the silicon fluoride aqueous solution is preferably 10% by mass to 30% by mass ammonia water.
[0102] In the above neutralization reaction, the amount of NH 3 The molar ratio of NH 3 / Si is preferably 95 to 500, more preferably 100 to 450, and even more preferably 110 to 400. The amount of addition is determined based on the amount of NH 3 / Si, from the viewpoint of the formation of silicon oxide compounds that dissolve in amines or diluted aqueous ammonia. 3 The molar ratio of NH / HF is preferably 3.0 or more, more preferably 4.0 or more, and even more preferably 5.0 or more. 3 The molar ratio of / HF is preferably 100 or less, more preferably 50 or less, and even more preferably 40 or less.
[0103] The addition time in the above-mentioned neutralization reaction is preferably within 10 minutes, more preferably within 8 minutes, and even more preferably within 5 minutes.
[0104] The fluorine-containing silicon hydrate cake obtained by the above-mentioned neutralization reaction is decanted with dilute ammonia water using a centrifuge, and washing is repeated until the amount of liberated fluoride ions is 100 mg / L or less, thereby removing fluoride ions from the fluorine-containing silicon hydrate cake and obtaining a silicon-containing precipitate. The fluorine-containing silicon hydrate cake obtained by the above-mentioned neutralization reaction contains fluorine compounds such as ammonium fluoride as impurities, so it is preferable to remove them. It is preferable that the washing liquid used to remove fluoride ions is dilute ammonia water.
[0105] The silicon content of the obtained silicon-containing precipitate was measured by taking a part of the silicon-containing precipitate, drying it at 110°C for 24 hours, and then calcining it at 1000°C for 4 hours to obtain SiO 2 The SiO 2 The weight of the precipitate is measured, and the silicon content of the silicon-containing precipitate can be calculated from the weight.
[0106] A tertiary amine compound and pure water are added to the silicon-containing precipitate and stirred for 10 minutes to obtain a silicon-containing mixed liquid. Then, 35% by mass hydrogen peroxide is added to the silicon-containing mixed liquid and stirred for 30 minutes to obtain a silicic acid compound-containing liquid.
[0107] The tertiary amine compound is preferably mixed so that the content of the tertiary amine compound in the silicon-containing mixed liquid is 0.1% by mass or more and 30% by mass or less. The tertiary amine compound is preferably one or more selected from the group consisting of trimethylamine, triethylamine, and tri-n-propylamine.
[0108] The hydrogen peroxide content of the hydrogen peroxide solution is preferably 0.5% by mass to 35% by mass. In addition, the hydrogen peroxide is preferably 0.5% by mass to 35% by mass in a molar ratio H 2 O 2It is preferable to add hydrogen peroxide so that / Si is 0.6 or more and 1.5 or less, and since there is a possibility that hydrogen peroxide may decompose during mixing, it is more preferable that it is 0.7 or more and 1.2 or less.
[0109] As in the above-mentioned method for producing a tantalic acid compound-containing liquid, it is preferable to have a step of removing hydrogen peroxide from the obtained silicic acid compound-containing liquid.
[0110] Furthermore, the method for producing the silicic acid compound-containing liquid is not limited to the above-mentioned method, and the liquid may be produced by the following method.
[0111] Another example of a method for producing a silicon oxide compound-containing liquid may include a mixing step of adding an acidic aqueous solution to a raw material material containing silicon and stirring at 15°C or higher and 50°C or lower to obtain a mixed liquid containing a precursor of a silicon compound, and a stirring step of adding a solution containing an organic nitrogen compound to the mixed liquid and stirring at 15°C or higher and 50°C or lower to produce a silicon compound-containing liquid.
[0112] First, in the mixing step, an acidic aqueous solution is added to a raw material containing silicon, and the mixture is stirred at 15° C. or more and 50° C. or less to obtain a mixture containing a precursor of a silicon compound.
[0113] Examples of the silicon-containing raw material include tetraethoxysilane (TEOS), tetramethoxysilane (TMOS), sodium silicate, etc. The silicon-containing raw material preferably contains at least one of tetraethoxysilane and sodium silicate.
[0114] Examples of the acidic aqueous solution include acetic acid, hydrochloric acid, sulfuric acid, phosphoric acid, etc. The acidic aqueous solution preferably contains at least one of acetic acid, hydrochloric acid, and phosphoric acid.
[0115] When the acidic aqueous solution is acetic acid, the acetic acid content is preferably 0.001% by mass to 3.0% by mass. When the silicon-containing raw material is TEOS, the acetic acid content of 0.001% by mass or more efficiently converts the silanol ester group Si-O-CH 2 -OH 3 can be hydrolyzed to form a Si-OH structure. On the other hand, if the acetic acid content is 3.0% by mass or less, the acetic acid content in the silicon oxide compound-containing liquid, which is the final product, can be reduced, which is preferable. From this viewpoint, the acetic acid content is preferably 0.001% by mass or more, more preferably 0.005% by mass or more, and even more preferably 0.01% by mass or more. On the other hand, the acetic acid content is preferably 3.0% by mass or less, more preferably 2.5% by mass or less, even more preferably 2.0% by mass or less, particularly preferably 1.5% by mass or less, more particularly preferably 1.0% by mass or less, even more particularly preferably 0.5% by mass or less, also particularly preferably 0.1% by mass or less, even more particularly preferably 0.05% by mass or less, even more particularly preferably 0.04% by mass or less, even more particularly preferably 0.03% by mass or less, and even more particularly preferably 0.02% by mass or less. The acetic acid content described in this specification is the content when added to the raw material containing silicon in the mixing step, unless otherwise specified.
[0116] The acetic acid content in the silicon oxide compound-containing liquid is preferably 0.02% by mass to 10% by mass. The acetic acid content is more preferably 0.05% by mass or more, even more preferably 0.1% by mass or more, particularly preferably 0.15% by mass or more, and even more particularly preferably 0.2% by mass or more. On the other hand, the acetic acid content is more preferably 5% by mass or less, even more preferably 3% by mass or less, particularly preferably 1% by mass or less, and particularly preferably 0.5% by mass or less.
[0117] Furthermore, the amount of acetic acid added to the silicon-containing raw material is CH 3The molar ratio of COOH / Si is preferably 0.01 to 0.3, more preferably 0.02 to 0.25, and even more preferably 0.03 to 0.2. The time for adding acetic acid to the silicon-containing raw material is preferably 5 minutes or less, more preferably 3 minutes or less, and even more preferably 1 minute or less. The acetic acid content in the silicon oxide compound-containing liquid is preferably 0.01 to 0.3, more preferably 0.02 to 0.25, and even more preferably 0.03 to 0.2. 3 The molar ratio of COOH / Si is preferably 0.01 or more and 0.3 or less, more preferably 0.02 or more and 0.25 or less, and even more preferably 0.03 or more and 0.2 or less.
[0118] When the acidic aqueous solution added to the silicon-containing raw material is hydrochloric acid, the hydrochloric acid content is preferably 0.001% by mass to 3.0% by mass. When the silicon-containing raw material is sodium silicate, if the hydrochloric acid content is 0.001% by mass or more, sodium chloride can be efficiently produced from sodium silicate. On the other hand, if the hydrochloric acid content is 3.0% by mass or less, it is preferable because chlorine is less likely to remain in the final product, the silicon oxide compound-containing liquid. From this viewpoint, the hydrochloric acid content is preferably 0.001% by mass or more, more preferably 0.005% by mass or more, and even more preferably 0.01% by mass or more. On the other hand, the hydrochloric acid content is preferably 3.0% by mass or less, more preferably 2.5% by mass or less, even more preferably 2.0% by mass or less, particularly preferably 1.5% by mass or less, more particularly preferably 1.0% by mass or less, even more particularly preferably 0.5% by mass or less, even more particularly preferably 0.1% by mass or less, even more particularly preferably 0.05% by mass or less, even more particularly preferably 0.04% by mass or less, even more particularly preferably 0.03% by mass or less, and even more particularly preferably 0.02% by mass or less. The hydrochloric acid content described in this specification is the content when added to the silicon-containing raw material in the mixing step, unless otherwise specified, and is the value converted by the weight of HCl in 0.5N hydrochloric acid aqueous solution.
[0119] The hydrochloric acid content in the silicon oxide compound-containing liquid is preferably 0.02% by mass to 10% by mass. The hydrochloric acid content is more preferably 0.05% by mass or more, even more preferably 0.1% by mass or more, particularly preferably 0.15% by mass or more, and even more particularly preferably 0.2% by mass or more. On the other hand, the hydrochloric acid content is more preferably 5% by mass or less, even more preferably 3% by mass or less, particularly preferably 1% by mass or less, and particularly preferably 0.5% by mass or less.
[0120] The amount of hydrochloric acid added to the silicon-containing raw material is preferably such that the molar ratio of HCl / Si is 0.5 or more and 1.5 or less, more preferably 0.55 or more and 1.3 or less, and even more preferably 0.6 or more and 1.1 or less. The time for adding hydrochloric acid to the silicon-containing raw material is preferably 10 minutes or less, more preferably 5 minutes or less, and even more preferably 3 minutes or less. The content of hydrochloric acid in the silicon oxide compound-containing liquid is preferably such that the molar ratio of HCl / Si is 0.5 or more and 1.5 or less, more preferably 0.55 or more and 1.3 or less, and even more preferably 0.6 or more and 1.1 or less.
[0121] In the mixing step, after the acidic aqueous solution is added to the silicon-containing raw material, the temperature of the mixture during stirring is preferably 15° C. to 50° C., more preferably 20° C. to 45° C., and even more preferably 25° C. to 40° C. If the temperature of the mixture exceeds 50° C., the water in the mixture evaporates too much, and Si-OH undergo dehydration condensation in the mixture to form SiO 2 Fine particles may be partially formed, and may not dissolve when a solution containing an organic nitrogen compound is added during the stirring step.
[0122] Furthermore, in the mixing step, the time required for stirring after the acidic aqueous solution is added to the silicon-containing raw material varies depending on the type of silicon-containing raw material, the amount of the acidic aqueous solution added, the reduced pressure conditions, and the like.
[0123] Specifically, when the silicon-containing raw material is TEOS and the acidic aqueous solution is acetic acid, the stirring time is preferably from 30 minutes to 24 hours, more preferably from 1 hour to 15 hours, and even more preferably from 2 hours to 12 hours.
[0124] Furthermore, when the silicon-containing raw material is sodium silicate and the acidic aqueous solution is hydrochloric acid, the stirring time is preferably from 10 minutes to 10 hours, more preferably from 30 minutes to 7 hours, and even more preferably from 1 hour to 5 hours.
[0125] In this manner, an acidic aqueous solution is added to a raw material containing silicon, and the mixture is stirred at 15° C. or higher and 50° C. or lower, thereby obtaining a mixed solution containing a precursor of a silicon compound.
[0126] It is speculated that the precursor of silicon compounds, when an acidic aqueous solution is added to a raw material containing silicon, results in a linear structure of the silicic acid produced. This is speculated from the fact that the absorption maximum intensity attributed to the Si-OH stretching vibration increases in the infrared spectrum measured by a Fourier transform infrared spectrophotometer (FT-IR).
[0127] Furthermore, when the silicon-containing raw material is tetraethoxysilane and the acidic aqueous solution is acetic acid, the resulting mixture containing the precursor of the silicon compound is subjected to the next stirring step.
[0128] On the other hand, when the silicon-containing raw material is sodium silicate and the acidic aqueous solution is hydrochloric acid, the obtained mixed solution containing the precursor of the silicon compound needs to be treated as follows as a pretreatment before proceeding to the next stirring step. During the above-mentioned stirring, a part of Na in the sodium silicate reacts with a part of Cl in the hydrochloric acid, and the generated NaCl is contained in the precursor of the silicon compound, so it is advisable to remove NaCl from the precursor of the silicon compound. As a method for removing the NaCl, first, the mixed solution containing the precursor of the silicon compound is placed in a centrifuge tube and centrifuged (4500 rpm, 10 minutes) to recover the precipitated transparent gel. Next, water is added to the recovered transparent gel, which is placed in a centrifuge tube and centrifuged (4500 rpm, 20 minutes) multiple times while replacing the water, thereby removing NaCl from the precursor of the silicon compound.
[0129] Next, in the stirring step, the solution containing the organic nitrogen compound is added to the mixed liquid containing the precursor of the silicon compound, and the mixture is stirred at 15° C. or higher and 50° C. or lower to produce a silicon oxide compound-containing liquid.
[0130] Examples of the organic nitrogen compound include primary amines, secondary amines, tertiary amines, and quaternary ammonium salts. The organic nitrogen compound preferably includes at least one of primary amines, secondary amines, and quaternary ammonium salts, and specific examples include methylamine, ethylamine, dimethylamine, diethylamine, and tetramethylammonium hydroxide. A solution containing an organic acid, rather than an organic nitrogen compound, may be added to the mixture containing the precursor of the silicon compound.
[0131] The amount of the organic nitrogen compound added to the mixture containing the precursor of the silicon compound is preferably such that the molar ratio of amine / Si is 0.5 or more and 15 or less, more preferably 1 or more and 10 or less, and even more preferably 1.5 or more and 5 or less. In addition, the amount of the organic nitrogen compound added to the mixture containing the precursor of the silicon compound is preferably such that the molar ratio of amine / Si is 1.7 or more, more preferably 1.3 or more, and even more preferably 1.3 or more, from the viewpoint of generating a silicon compound that dissolves in the organic nitrogen compound. On the other hand, in terms of reducing costs, the molar ratio of amine / Si is preferably 1.5 or less, more preferably 1.2 or less, and even more preferably 1 or less.
[0132] The time for adding the organic nitrogen compound to the mixed solution containing the precursor of the silicon compound is preferably within 60 minutes, more preferably within 30 minutes, and even more preferably within 10 minutes.
[0133] In the stirring step, after the solution containing the organic nitrogen compound is added to the mixed solution containing the precursor of the silicon compound, the liquid temperature during stirring is preferably 15° C. to 50° C., more preferably 20° C. to 45° C., and even more preferably 25° C. to 40° C. If the liquid temperature during stirring exceeds 50° C., the organic nitrogen compound and the like evaporate, making it difficult for the precursor of the silicon compound to dissolve, and increasing the possibility that the precursor of the silicon compound remains.
[0134] Furthermore, in the stirring step, after adding the solution containing the organic nitrogen compound to the mixed solution containing the precursor of the silicon compound, the stirring time is preferably from 10 minutes to 24 hours, more preferably from 30 minutes to 20 hours, and even more preferably from 1 hour to 15 hours.
[0135] In this way, a solution containing an organic nitrogen compound can be added to a mixed solution containing a silicon compound precursor, and the mixture is stirred at 15° C. to 50° C. to produce a silicon oxide compound-containing liquid. As described above, it is presumed that the silicon compound precursor contains many Si-OH structures, which makes it easier to dissolve the silicon oxide in water.
[0136] A method for producing a molybdic acid compound-containing liquid, which is a metallic acid compound-containing liquid of the present invention, will be described below. Note that the description of the same points as those of the above-mentioned method for producing a tantalic acid compound-containing liquid will be omitted.
[0137] First, molybdenum or molybdenum oxide is reacted with hydrofluoric acid (HF), such as an aqueous solution of hydrofluoric acid, to produce molybdenum fluoride (H 2 MoF 6 ) and dissolving it in water to obtain an aqueous solution of molybdenum fluoride, which is an acidic metal solution.
[0138] Here, the molybdenum fluoride aqueous solution is prepared by adding water (e.g., pure water) to convert molybdenum into MoO 3 It is preferable to adjust the molybdenum content to 1 to 100 g / L in terms of molybdenum content. 3 When the molybdenum content is 1 g / L or more in terms of the molybdenum content, it is preferable because the molybdenum compound hydrate is easily soluble in water, and when productivity is taken into consideration, it is more preferable that the molybdenum content is 10 g / L or more, and even more preferable that the molybdenum content is 20 g / L or more. 3 A molybdic acid compound hydrate having a concentration of 100 g / L or less in terms of total solubility in water is preferable, and in order to more reliably synthesize a molybdic acid compound hydrate having a high water solubility, a concentration of 90 g / L or less is more preferable, a concentration of 80 g / L or less is even more preferable, and a concentration of 70 g / L or less is particularly preferable. From the viewpoint of completely dissolving molybdenum or molybdenum oxide, the pH of the aqueous molybdenum fluoride solution is preferably 2 or less, and more preferably 1 or less.
[0139] Next, the molybdenum fluoride aqueous solution is neutralized with an alkaline aqueous solution to obtain a fluorine-containing molybdenum hydrate cake. The alkaline aqueous solution used to neutralize the molybdenum fluoride aqueous solution is preferably 10% by mass to 30% by mass ammonia water.
[0140] In the above neutralization reaction, the amount of NH 3 The molar ratio of NH / Mo is preferably 95 to 500, more preferably 100 to 450, and even more preferably 110 to 400. The amount of addition is determined based on the NH 3 The molar ratio of NH / HF is preferably 3.0 or more, more preferably 4.0 or more, and even more preferably 5.0 or more. 3 The molar ratio of / HF is preferably 100 or less, more preferably 50 or less, and even more preferably 40 or less.
[0141] The addition time in the above-mentioned neutralization reaction is preferably within 10 minutes, more preferably within 8 minutes, and even more preferably within 5 minutes.
[0142] The fluorine-containing molybdenum hydrate cake obtained by the above-mentioned neutralization reaction is decanted with dilute ammonia water using a centrifuge, and washing is repeated until the amount of liberated fluoride ions becomes 100 mg / L or less, thereby removing the fluoride ions from the fluorine-containing molybdenum hydrate cake and obtaining a molybdenum-containing precipitate. The fluorine-containing molybdenum hydrate cake obtained by the above-mentioned neutralization reaction contains fluorine compounds such as ammonium fluoride as impurities, so it is preferable to remove these. The washing liquid used to remove the fluoride ions is preferably dilute ammonia water.
[0143] The molybdenum content of the obtained molybdenum-containing precipitate was measured by taking a portion of the molybdenum-containing precipitate, drying it at 110 °C for 24 hours, and then calcining it at 1000 °C for 4 hours to obtain MoO3 The MoO 3 The weight of the precipitate is measured, and the molybdenum content of the molybdenum-containing precipitate can be calculated from the weight.
[0144] A tertiary amine compound and pure water are added to the obtained molybdenum-containing precipitate and stirred for 10 minutes to obtain a molybdenum-containing mixed liquid. After that, 35% by mass of hydrogen peroxide is added to the molybdenum-containing mixed liquid and stirred for 30 minutes to obtain a molybdic acid compound-containing liquid.
[0145] The tertiary amine compound is preferably mixed so that the content of the tertiary amine compound in the molybdenum-containing mixed liquid is 0.1% by mass or more and 30% by mass or less, and the tertiary amine compound is preferably one or more selected from the group consisting of trimethylamine, triethylamine, and tri-n-propylamine.
[0146] The hydrogen peroxide content of the hydrogen peroxide solution is preferably 0.5% by mass to 35% by mass. The hydrogen peroxide is preferably mixed with molybdenum in a molar ratio of H 2 O 2 It is preferable to add hydrogen peroxide so that the ratio of / Mo is 0.6 or more and 1.5 or less, and since there is a possibility that hydrogen peroxide may decompose during mixing, it is more preferable that the ratio is 0.7 or more and 1.2 or less.
[0147] As in the above-mentioned method for producing a tantalic acid compound-containing liquid, it is preferable to have a step of removing hydrogen peroxide from the obtained molybdic acid compound-containing liquid.
[0148] A method for producing a tungstic acid compound-containing liquid, which is a metallic acid compound-containing liquid of the present invention, will be described below. Note that the description of the same points as those of the above-mentioned method for producing a tantalic acid compound-containing liquid will be omitted.
[0149] First, tungsten or tungsten oxide is reacted with hydrofluoric acid (HF), such as an aqueous solution of hydrofluoric acid, to produce tungsten fluoride (H 2 MoF 6) and dissolving it in water to obtain an acidic metal aqueous solution, that is, an aqueous tungsten fluoride solution.
[0150] Here, the tungsten fluoride aqueous solution is prepared by adding water (e.g., pure water) to convert tungsten into WO 3 It is preferable to adjust the tungsten content to 1 to 100 g / L in terms of WO 3 When the tungsten content is 1 g / L or more, it is preferable because the tungsten acid compound hydrate is easily soluble in water, and when productivity is taken into consideration, it is more preferable that the tungsten content is 10 g / L or more, and even more preferable that the tungsten content is 20 g / L or more. 3 If the converted amount is 100g / L or less, it is preferable because the tungstic acid compound hydrate is easily soluble in water, and in order to more reliably synthesize the tungstic acid compound hydrate that is easily soluble in water, it is more preferable that the converted amount is 90g / L or less, further more preferable that the converted amount is 80g / L or less, and particularly preferable that the converted amount is 70g / L or less. Note that, in terms of completely dissolving tungsten or tungsten oxide, the pH of the tungsten fluoride aqueous solution is preferably 2 or less, more preferably 1 or less.
[0151] Next, the tungsten fluoride aqueous solution is neutralized with an alkaline aqueous solution to obtain a fluorine-containing tungsten hydrate cake. Here, the alkaline aqueous solution used to neutralize the tungsten fluoride aqueous solution is preferably 10% by mass to 30% by mass ammonia water.
[0152] In the above neutralization reaction, the amount of NH 3 The molar ratio of NH 3 / W is preferably 95 to 500, more preferably 100 to 450, and even more preferably 110 to 400. The amount of addition is determined based on the amount of NH 3 / W, from the viewpoint of the formation of a tungstic acid compound that dissolves in amines or diluted ammonia water. 3 The molar ratio of NH / HF is preferably 3.0 or more, more preferably 4.0 or more, and even more preferably 5.0 or more. 3The molar ratio of / HF is preferably 100 or less, more preferably 50 or less, and even more preferably 40 or less.
[0153] The addition time in the above-mentioned neutralization reaction is preferably within 10 minutes, more preferably within 8 minutes, and even more preferably within 5 minutes.
[0154] The fluorine-containing tungsten hydrate cake obtained by the above-mentioned neutralization reaction is decanted with dilute ammonia water using a centrifuge, and washing is repeated until the amount of liberated fluoride ions becomes 100 mg / L or less, thereby removing the fluoride ions from the fluorine-containing tungsten hydrate cake and obtaining a tungsten-containing precipitate. The fluorine-containing tungsten hydrate cake obtained by the above-mentioned neutralization reaction contains fluorine compounds such as ammonium fluoride as impurities, so it is preferable to remove these. It is preferable that the washing liquid used to remove the fluoride ions is dilute ammonia water.
[0155] The tungsten content of the obtained tungsten-containing precipitate was measured by taking a part of the tungsten-containing precipitate, drying it at 110°C for 24 hours, and then calcining it at 1000°C for 4 hours to obtain WO 3 The WO generated in this way 3 The weight of the precipitate is measured, and the tungsten content of the tungsten-containing precipitate can be calculated from the weight.
[0156] A tertiary amine compound and pure water are added to the resulting tungsten-containing precipitate and stirred for 10 minutes to obtain a tungsten-containing mixed liquid. Then, 35% by mass of hydrogen peroxide is added to the tungsten-containing mixed liquid and stirred for 30 minutes to obtain a tungsten acid compound-containing liquid.
[0157] The tertiary amine compound is preferably mixed so that the content of the tertiary amine compound in the tungsten-containing mixed liquid is 0.1% by mass or more and 30% by mass or less. The tertiary amine compound is preferably one or more selected from the group consisting of trimethylamine, triethylamine, and tri-n-propylamine.
[0158] The hydrogen peroxide content of the hydrogen peroxide solution is preferably 0.5% by mass to 35% by mass. The hydrogen peroxide is preferably in a molar ratio of hydrogen peroxide to tungsten H 2 O 2 It is preferable to add hydrogen peroxide so that the ratio of hydrogen peroxide to water is 0.6 to 1.5, and since there is a possibility that hydrogen peroxide may decompose during mixing, it is more preferable that the ratio of hydrogen peroxide to water is 0.7 to 1.2.
[0159] As in the above-mentioned method for producing a tantalic acid compound-containing liquid, it is preferable to have a step of removing hydrogen peroxide from the obtained tungstic acid compound-containing liquid.
[0160] A method for producing a hafnium acid compound-containing liquid, which is a metal acid compound-containing liquid of the present invention, will be described below. Note that the description of the same points as those of the above-mentioned method for producing a tantalic acid compound-containing liquid will be omitted.
[0161] First, hafnium or hafnium oxide is reacted with hydrofluoric acid (HF), such as an aqueous solution of hydrofluoric acid, to produce hafnium fluoride (H 2 HfF 6 ) and dissolving it in water to obtain an acidic metal aqueous solution, that is, an aqueous hafnium fluoride solution.
[0162] Here, the hafnium fluoride solution is prepared by adding water (e.g., pure water) to convert hafnium to HfO 2 It is preferable to adjust the hafnium content to 1 to 100 g / L in terms of HfO 2 A hafnium content of 1 g / L or more in terms of the hafnium oxide compound hydrate is preferably soluble in water, and from the viewpoint of productivity, a hafnium content of 10 g / L or more is more preferable, and a hafnium content of 20 g / L or more is even more preferable.2 A conversion of 100 g / L or less is preferable because it results in a hafnium oxide hydrate that is easily soluble in water, and in order to more reliably synthesize a hafnium oxide hydrate that is easily soluble in water, a conversion of 90 g / L or less is more preferable, a conversion of 80 g / L or less is even more preferable, and a conversion of 70 g / L or less is particularly preferable. Note that, from the viewpoint of completely dissolving hafnium or hafnium oxide, the pH of the hafnium fluoride aqueous solution is preferably 2 or less, and more preferably 1 or less.
[0163] Next, the hafnium fluoride aqueous solution is neutralized with an alkaline aqueous solution to obtain a fluorine-containing hafnium hydrate cake. Here, the alkaline aqueous solution used to neutralize the hafnium fluoride aqueous solution is preferably 10% by mass to 30% by mass ammonia water.
[0164] In the above neutralization reaction, the amount of NH 3 The molar ratio of NH / Hf is preferably 95 to 500, more preferably 100 to 450, and even more preferably 110 to 400. The amount of addition is adjusted to NH 3 The molar ratio of NH / HF is preferably 3.0 or more, more preferably 4.0 or more, and even more preferably 5.0 or more. 3 The molar ratio of / HF is preferably 100 or less, more preferably 50 or less, and even more preferably 40 or less.
[0165] The addition time in the above-mentioned neutralization reaction is preferably within 10 minutes, more preferably within 8 minutes, and even more preferably within 5 minutes.
[0166] The fluorine-containing hafnium hydrate cake obtained by the above-mentioned neutralization reaction is decanted with dilute ammonia water using a centrifuge, and washing is repeated until the amount of liberated fluoride ions is 100 mg / L or less, thereby removing the fluoride ions from the fluorine-containing hafnium hydrate cake and obtaining a hafnium-containing precipitate. The fluorine-containing hafnium hydrate cake obtained by the above-mentioned neutralization reaction contains fluorine compounds such as ammonium fluoride as impurities, so it is preferable to remove these. It is preferable that the washing liquid used to remove the fluoride ions is dilute ammonia water.
[0167] The hafnium content of the obtained hafnium-containing precipitate was measured by taking a part of the hafnium-containing precipitate, drying it at 110°C for 24 hours, and then calcining it at 1000°C for 4 hours to obtain HfO 2 The HfO 2 The weight of the precipitate is measured, and the hafnium content of the precipitate containing hafnium can be calculated from the weight.
[0168] A tertiary amine compound and pure water are added to the obtained hafnium-containing precipitate and stirred for 10 minutes to obtain a hafnium-containing mixed liquid. After that, 35% by mass hydrogen peroxide is added to the hafnium-containing mixed liquid and stirred for 30 minutes to obtain a hafnium acid compound-containing liquid.
[0169] The tertiary amine compound is preferably mixed so that the content of the tertiary amine compound in the hafnium-containing mixed solution is 0.1% by mass or more and 30% by mass or less. The tertiary amine compound is preferably one or more selected from the group consisting of trimethylamine, triethylamine, and tri-n-propylamine.
[0170] The hydrogen peroxide content of the hydrogen peroxide solution is preferably 0.5% by mass to 35% by mass. The hydrogen peroxide is preferably in a molar ratio of hydrogen peroxide to hafnium H 2 O 2It is preferable to add hydrogen peroxide so that / Hf is 0.6 or more and 1.5 or less, and since there is a possibility that hydrogen peroxide may decompose during mixing, it is more preferable that the ratio is 0.7 or more and 1.2 or less.
[0171] As in the above-mentioned method for producing a tantalic acid compound-containing liquid, it is preferable to have a step of removing hydrogen peroxide from the obtained hafnic acid compound-containing liquid.
[0172] A method for producing a rare earth element acid compound-containing liquid, which is a metallic acid compound-containing liquid of the present invention, will be described below. Note that the description of the same points as those of the above-mentioned method for producing a tantalic acid compound-containing liquid will be omitted.
[0173] First, a rare earth element or a rare earth oxide is reacted with hydrofluoric acid (HF), such as an aqueous solution of hydrofluoric acid, to form a rare earth fluoride, which is then dissolved in water to obtain an aqueous solution of rare earth fluoride, which is an acidic metal solution.
[0174] Here, it is preferable to adjust the rare earth fluoride aqueous solution to contain 1 to 100 g / L of rare earth element in terms of rare earth oxide by adding water (e.g., pure water). In this case, it is preferable that the rare earth element content is 1 g / L or more in terms of rare earth oxide, since it becomes a rare earth element acid compound hydrate that is easily soluble in water, and in consideration of productivity, it is more preferable that it is 10 g / L or more, and even more preferable that it is 20 g / L or more. On the other hand, it is preferable that the rare earth element content is 100 g / L or less in terms of rare earth oxide, since it becomes a rare earth element acid compound hydrate that is easily soluble in water, and in order to synthesize a rare earth element acid compound hydrate that is easily soluble in water more reliably, it is more preferable that it is 90 g / L or less, even more preferable that it is 80 g / L or less, and particularly preferable that it is 70 g / L or less. In addition, the pH of the rare earth fluoride aqueous solution is preferably 2 or less, more preferably 1 or less, from the viewpoint of completely dissolving the rare earth element or rare earth element oxide.
[0175] Next, the aqueous solution of rare earth fluoride is neutralized with an aqueous alkaline solution to obtain a fluorine-containing rare earth hydrate cake. The aqueous alkaline solution used to neutralize the aqueous solution of rare earth fluoride is preferably 10% by mass to 30% by mass ammonia water.
[0176] In the above neutralization reaction, the amount of NH 3 The molar ratio of NH to rare earth element is preferably 95 to 500, more preferably 100 to 450, and even more preferably 110 to 400. The amount of addition is determined based on the NH 3 The molar ratio of NH / HF is preferably 3.0 or more, more preferably 4.0 or more, and even more preferably 5.0 or more. 3 The molar ratio of / HF is preferably 100 or less, more preferably 50 or less, and even more preferably 40 or less.
[0177] The addition time in the above-mentioned neutralization reaction is preferably within 10 minutes, more preferably within 8 minutes, and even more preferably within 5 minutes.
[0178] The fluorine-containing rare earth element hydrate cake obtained by the above-mentioned neutralization reaction is decanted with dilute ammonia water using a centrifuge, and washing is repeated until the amount of liberated fluoride ions becomes 100 mg / L or less, thereby removing the fluoride ions from the fluorine-containing rare earth element hydrate cake and obtaining a rare earth element-containing precipitate. The fluorine-containing rare earth element hydrate cake obtained by the above-mentioned neutralization reaction contains fluorine compounds such as ammonium fluoride as impurities, so it is preferable to remove these. The washing liquid used to remove the fluoride ions is preferably dilute ammonia water.
[0179] The rare earth element content of the rare earth element-containing precipitate is determined by taking a portion of the rare earth element-containing precipitate, drying it at 110° C. for 24 hours, and then calcining it at 1000° C. for 4 hours to produce a rare earth element oxide. The weight of the rare earth element oxide thus produced can be measured, and the rare earth element content of the rare earth element-containing precipitate can be calculated from the weight.
[0180] A tertiary amine compound and pure water are added to the rare earth element-containing precipitate obtained, and the mixture is stirred for 10 minutes to obtain a rare earth element-containing mixed liquid. After that, 35% by mass of hydrogen peroxide is added to the rare earth element-containing mixed liquid, and the mixture is stirred for 30 minutes to obtain a rare earth element acid compound-containing liquid.
[0181] The tertiary amine compound is preferably mixed so that the content of the tertiary amine compound in the rare earth element-containing mixed liquid is 0.1% by mass or more and 30% by mass or less, and the tertiary amine compound is preferably one or more selected from the group consisting of trimethylamine, triethylamine, and tri-n-propylamine.
[0182] The hydrogen peroxide content of the hydrogen peroxide solution is preferably 0.5% by mass to 35% by mass. The hydrogen peroxide is preferably in a molar ratio H 2 O 2 It is preferable to add hydrogen peroxide so that / Hf is 0.6 or more and 1.5 or less, and since there is a possibility that hydrogen peroxide may decompose during mixing, it is more preferable that the ratio is 0.7 or more and 1.2 or less.
[0183] As in the above-mentioned method for producing a tantalic acid compound-containing liquid, it is preferable to have a step of removing hydrogen peroxide from the obtained rare earth acid compound-containing liquid.
[0184] The method for producing a metal acid compound-containing film of the present invention includes the steps of applying the metal acid compound-containing liquid of the present invention to a substrate, and drying and / or firing the liquid. The metal acid compound-containing liquid of the present invention used in the method for producing a metal acid compound-containing film of the present invention may be one produced by the method for producing a metal acid compound-containing liquid of the present invention described above.
[0185] Of the metal acid compound-containing films of the present invention, the method for producing the metal acid compound-containing dry film of the present invention includes a coating step of coating the metal acid compound-containing liquid of the present invention onto the surface of a substrate, and a film drying step of drying the metal acid compound-containing liquid coated on the surface of the substrate to obtain a dry film.
[0186] Specifically, the metal acid compound-containing liquid obtained by the above-mentioned method for producing a metal acid compound-containing liquid of the present invention is dropped onto the surface of a substrate using a syringe while being filtered, for example, with a filter having a pore size of 2 μm, as necessary, and then applied by spin coating (700 rpm, 10 seconds, then 1500 rpm, 15 seconds). Next, the substrate is dried at 110° C. for 30 minutes to form a metal acid compound-containing dry film on the surface of the substrate.
[0187] Of the metal acid compound-containing films of the present invention, the method for producing the metal acid compound-containing fired film of the present invention includes a coating step of coating the metal acid compound-containing liquid of the present invention onto the surface of a substrate, a film drying step of drying the metal acid compound-containing liquid coated on the surface of the substrate to obtain a dried film, and a film firing step of firing the dried film in the atmosphere at a firing temperature of 300°C or higher and 1,200°C or lower for a firing time of 1 hour or higher and 12 hours or lower to obtain a fired film.
[0188] Specifically, as described above, the metal acid compound-containing liquid of the present invention is applied to the surface of a substrate, and the substrate is dried to form a metal acid compound-containing dried film of the present invention. The substrate is then placed in a static furnace and baked in air at a baking temperature of 300°C or higher and 1,200°C or lower for a baking time of 1 hour or higher and 12 hours or lower, thereby forming a metal acid compound-containing baked film of the present invention on the surface of the substrate.
[0189] The method for producing a complex metal acid compound-containing liquid of the present invention includes the steps of neutralizing an acidic metal aqueous solution containing a metal and / or metalloid element with an alkaline aqueous solution to produce a precipitate containing the metal and / or metalloid element, adding a tertiary amine compound and hydrogen peroxide to the precipitate to produce a complex metal acid compound-containing liquid, and then mixing the complex metal acid compound-containing liquid with Li, Na, M, or Zn.g and at least one element A selected from the group consisting of Al, K, Ca, V, Mn, Fe, Co, Ni, Cu, Zn, Sn, Sr, and Ba, to produce a liquid containing a complex metal acid compound.
[0190] Specifically, the metal acid compound-containing liquid of the present invention produced by the above-mentioned method for producing a metal acid compound-containing liquid of the present invention and Li, Na, M g The composite metal acid compound-containing liquid of the present invention can be obtained by mixing the element A with at least one element A selected from the group consisting of Al, K, Ca, V, Mn, Fe, Co, Ni, Cu, Zn, Sn, Sr, and Ba, and maintaining the liquid temperature at an appropriate temperature for a predetermined period of time while stirring. The element A may be in various forms such as an oxide, hydroxide, metal complex, or salt made of a polyoxometalate or a peroxo complex.
[0191] As in the above-mentioned method for producing a tantalic acid compound-containing liquid, it is preferable to have a step of removing hydrogen peroxide from the resulting complex metal acid compound-containing liquid.
[0192] The method for producing a double metal acid compound-containing film of the present invention includes the steps of applying the double metal acid compound-containing liquid of the present invention to a substrate, and drying and / or firing the same. The complex metal acid compound-containing liquid of the present invention used in the method for producing a complex metal acid compound-containing film of the present invention may be one produced by the method for producing a complex metal acid compound-containing liquid of the present invention described above.
[0193] Of the complex metal acid compound-containing films of the present invention, the method for producing the complex metal acid compound-containing dry film of the present invention, like the method for producing the metal acid compound-containing dry film of the present invention, has a coating step of applying the complex metal acid compound-containing liquid of the present invention to the surface of a substrate, and a film drying step of drying the complex metal acid compound-containing liquid applied to the surface of the substrate to obtain a dry film.
[0194] Of the complex metal acid compound-containing films of the present invention, the method for producing the complex metal acid compound-containing fired film of the present invention, like the method for producing the metal acid compound-containing fired film of the present invention, includes an application step of applying the complex metal acid compound-containing liquid of the present invention to the surface of a substrate, a film drying step of drying the complex metal acid compound-containing liquid applied to the surface of the substrate to obtain a dried film, and a film firing step of firing the dried film in air at a firing temperature of 300°C or higher and 1,200°C or lower for a firing time of 1 hour or higher and 12 hours or lower to obtain a fired film.
[0195] In this specification, when "X to Y" (X and Y are any numbers) is expressed, unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably greater than X" or "preferably smaller than Y". In addition, when "X or more" (X is any number) or "Y or less" (Y is any number), it also includes the meaning of "preferably greater than X" or "preferably less than Y". Effect of the Invention
[0196] The metal acid compound-containing liquid and the method for producing the same of the present invention have a low environmental impact and excellent dispersibility. [Brief description of the drawings]
[0197] [Figure 1] 1 is a table listing physical property values and measurement results of metal acid compound-containing liquids according to Examples 1 to 8 of the present invention and Comparative Examples 1 to 9. [Diagram 2] 1 is a table listing physical property values and measurement results of metal acid compound-containing liquids according to Examples 9 and 10 of the present invention and Comparative Examples 10 to 12. BEST MODE FOR CARRYING OUT THEINVENTION
[0198] The metal acid compound-containing liquid according to the embodiment of the present invention will be further described below with reference to the following examples. Here, the metal acid compound-containing liquids according to Examples 1 to 8 and Comparative Examples 1 to 9 are tantalic acid compound-containing liquids. Moreover, the metal acid compound-containing liquids according to Examples 9 and 10 and Comparative Examples 10 to 12 are niobic acid compound-containing liquids. However, the following examples do not limit the present invention.
[0199] Example 1 100g of tantalum hydroxide (Ta 2 O 5 A tantalum fluoride aqueous solution (Ta 2 O 5 A concentration of 33.3% by weight was obtained.
[0200] 100 g of this tantalum fluoride solution was mixed with ammonia water (NH 3 A fluorine-containing tantalum hydrate cake was obtained by adding 1,000 mL of the aqueous solution (concentration: 25 mass%).
[0201] Next, this fluorine-containing tantalum hydrate cake was decanted using a centrifuge and washed with dilute ammonia water until the amount of liberated fluoride ions was 100 mg / L or less, thereby obtaining a tantalum-containing precipitate from which the fluoride ions had been removed. At this time, ammonia water was used as the washing liquid.
[0202] Here, the tantalum content of the obtained tantalum-containing precipitate was measured by taking a part of the tantalum-containing precipitate, drying it at 110°C for 24 hours, and then firing it at 1000°C for 4 hours. 2 O 5 The Ta generated in this way 2 O 5 The weight of the tantalum-containing precipitate was measured, and the Ta 2 O 5 The tantalum oxide content (in terms of oxide) was 50 mass %. The Ta content (in terms of tantalum, metal) of the tantalum-containing precipitate was calculated to be 40.9 mass %.
[0203] Then, 50 g of 10 mass% triethylamine and 317 g of pure water were added to the obtained tantalum-containing precipitate, and the mixture was stirred for 10 minutes to obtain a tantalum-containing mixed solution. 2 O 5 83 g of 35 mass% hydrogen peroxide was added to the tantalum-containing mixed solution so that the hydrogen peroxide content was 5 mass% in terms of Ta, 4.1 mass% in terms of metal (Ta), and the final hydrogen peroxide content was 6.8 mass%, and the mixture was stirred for 30 minutes to obtain a tantalic acid compound-containing solution according to Example 1. No precipitate or sediment was observed in the tantalic acid compound-containing solution according to Example 1. The pH of the tantalic acid compound-containing solution according to Example 1 was 11.0.
[0204] Example 2 In Example 2, the final tantalum content was calculated as an oxide (Ta 2 O 5 A similar production method to that of Example 1 was carried out, except that 35 mass% hydrogen peroxide was added to the tantalum-containing mixed solution so that the total concentration was 7.5 mass% in terms of Ta equivalent and 6.1 mass% in terms of Ta metal equivalent, to obtain a tantalic acid compound-containing solution of Example 2. No precipitate or sediment was observed in the tantalic acid compound-containing solution of Example 2. The pH of the tantalic acid compound-containing solution of Example 2 was 11.1.
[0205] Example 3 In Example 3, the same manufacturing method as in Example 1 was carried out, except that 15 mass% triethylamine was added to the tantalum-containing precipitate, to obtain a tantalic acid compound-containing liquid according to Example 3. No precipitate or sediment was observed in the tantalic acid compound-containing liquid according to Example 3. The pH of the tantalic acid compound-containing liquid according to Example 3 was 11.3.
[0206] Example 4 In Example 4, the same manufacturing method as in Example 1 was carried out, except that 5 mass% of triethylamine was added to the tantalum-containing precipitate, to obtain a tantalic acid compound-containing liquid according to Example 4. No precipitate or sediment was observed in the tantalic acid compound-containing liquid according to Example 4. The pH of the tantalic acid compound-containing liquid according to Example 4 was 10.9.
[0207] Example 5 In Example 5, the same manufacturing method as in Example 1 was carried out, except that 15 mass% triethylamine was added to the tantalum-containing precipitate, and 35 mass% hydrogen peroxide was added to the tantalum-containing mixed solution so that the final hydrogen peroxide content was 13.4 mass%, to obtain a tantalic acid compound-containing solution according to Example 5. No precipitate or sediment was observed in the tantalic acid compound-containing solution according to Example 5. The pH of the tantalic acid compound-containing solution according to Example 5 was 10.7.
[0208] Example 6 In Example 6, the same manufacturing method as in Example 1 was carried out, except that 15 mass% triethylamine was added to the tantalum-containing precipitate, and 35 mass% hydrogen peroxide was added to the tantalum-containing mixed solution so that the final hydrogen peroxide content was 5 mass%, to obtain a tantalic acid compound-containing solution according to Example 6. No precipitate or sediment was observed in the tantalic acid compound-containing solution according to Example 6. The pH of the tantalic acid compound-containing solution according to Example 6 was 10.7.
[0209] Example 7 In Example 7, the same manufacturing method as in Example 1 was carried out, except that 15 mass% trimethylamine was added to the tantalum-containing precipitate, to obtain a tantalic acid compound-containing liquid according to Example 7. No precipitate or sediment was observed in the tantalic acid compound-containing liquid according to Example 7. The pH of the tantalic acid compound-containing liquid according to Example 7 was 11.0.
[0210] Example 8 In Example 8, the same manufacturing method as in Example 1 was carried out, except that 10 mass% trimethylamine was added to the tantalum-containing precipitate, to obtain a tantalic acid compound-containing liquid according to Example 8. No precipitate or sediment was observed in the tantalic acid compound-containing liquid according to Example 8. The pH of the tantalic acid compound-containing liquid according to Example 8 was 10.6.
[0211] Comparative Example 1 In Comparative Example 1, a manufacturing method similar to that of Example 1 was carried out, except that 10 mass% of methylamine was added to the tantalum-containing precipitate, to obtain a tantalic acid compound-containing liquid according to Comparative Example 1. A white precipitate was observed in the tantalic acid compound-containing liquid according to Comparative Example 1. The pH of the tantalic acid compound-containing liquid according to Comparative Example 1 was 10.5.
[0212] Comparative Example 2 In Comparative Example 2, the same manufacturing method as in Example 1 was carried out except that 10 mass% dimethylamine was added to the tantalum-containing precipitate, to obtain a tantalic acid compound-containing liquid according to Comparative Example 2. A white precipitate was observed in the tantalic acid compound-containing liquid according to Comparative Example 2. The pH of the tantalic acid compound-containing liquid according to Comparative Example 2 was 10.2.
[0213] Comparative Example 3 In Comparative Example 3, the same manufacturing method as in Example 1 was carried out except that 10 mass % TMAH was added to the tantalum-containing precipitate, to obtain a tantalic acid compound-containing liquid according to Comparative Example 3. A white precipitate was observed in the tantalic acid compound-containing liquid according to Comparative Example 3. The pH of the tantalic acid compound-containing liquid according to Comparative Example 3 was 10.1.
[0214] Comparative Example 4 In Comparative Example 4, the same manufacturing method as in Example 1 was carried out, except that 5 mass% of methylamine was added to the tantalum-containing precipitate, to obtain a tantalic acid compound-containing liquid according to Comparative Example 4. A white precipitate was observed in the tantalic acid compound-containing liquid according to Comparative Example 4. The pH of the tantalic acid compound-containing liquid according to Comparative Example 4 was 10.3.
[0215] Comparative Example 5 In Comparative Example 5, the same manufacturing method as in Example 1 was carried out except that 5 mass% dimethylamine was added to the tantalum-containing precipitate, to obtain a tantalic acid compound-containing liquid according to Comparative Example 5. A white precipitate was observed in the tantalic acid compound-containing liquid according to Comparative Example 5. The pH of the tantalic acid compound-containing liquid according to Comparative Example 5 was 10.3.
[0216] Comparative Example 6 In Comparative Example 6, the same manufacturing method as in Example 1 was carried out except that 5 mass% TMAH was added to the tantalum-containing precipitate, to obtain a tantalic acid compound-containing liquid according to Comparative Example 6. A white precipitate was observed in the tantalic acid compound-containing liquid according to Comparative Example 6. The pH of the tantalic acid compound-containing liquid according to Comparative Example 3 was 10.5.
[0217] Comparative Example 7 In Comparative Example 7, the same manufacturing method as in Example 1 was carried out except that 15 mass% methylamine was added to the tantalum-containing precipitate, to obtain a tantalic acid compound-containing liquid according to Comparative Example 7. A white precipitate was observed in the tantalic acid compound-containing liquid according to Comparative Example 7. The pH of the tantalic acid compound-containing liquid according to Comparative Example 7 was 10.3.
[0218] Comparative Example 8 In Comparative Example 8, the same production method as in Example 1 was carried out except that 15 mass% dimethylamine was added to the tantalum-containing precipitate, to obtain a tantalic acid compound-containing liquid according to Comparative Example 8. A white precipitate was observed in the tantalic acid compound-containing liquid according to Comparative Example 8. The pH of the tantalic acid compound-containing liquid according to Comparative Example 8 was 10.4.
[0219] Comparative Example 9 In Comparative Example 9, the same manufacturing method as in Example 1 was carried out except that 15 mass % TMAH was added to the tantalum-containing precipitate, to obtain a tantalic acid compound-containing liquid according to Comparative Example 9. A white precipitate was observed in the tantalic acid compound-containing liquid according to Comparative Example 9. The pH of the tantalic acid compound-containing liquid according to Comparative Example 9 was 10.7.
[0220] Example 9 Niobium hydroxide 100g (Nb 2 O 5 Niobium fluoride (Nb fluoride) aqueous solution was prepared by dissolving niobium fluoride (Nb fluoride) in 100 g of 55% hydrofluoric acid aqueous solution and adding 100 mL of ion-exchanged water. 2 O 5 A concentration of 33.3% by weight was obtained.
[0221] 100 g of this niobium fluoride solution was mixed with ammonia water (NH 3 A fluorine-containing niobium hydrate cake was obtained by adding 1,000 mL of a 25% concentration aqueous solution of niobium hydrate.
[0222] Next, this fluorine-containing niobium hydrate cake was decanted using a centrifuge with dilute ammonia water and washed until the amount of liberated fluoride ions was 100 mg / L or less, to obtain a niobium-containing precipitate from which the fluoride ions had been removed. At this time, ammonia water was used as the washing liquid.
[0223] Here, the niobium content of the obtained niobium-containing precipitate was determined by taking a part of the tantalum-containing precipitate, drying it at 110°C for 24 hours, and then calcining it at 1000°C for 4 hours to obtain the Ta content. 2 O 5 The resulting Nb 2 O 5 The weight of the niobium-containing precipitate was measured, and the Nb 2 O 5 The niobium oxide content (in terms of oxide) was 50 mass %. The Nb content (in terms of niobium metal) of the niobium-containing precipitate was calculated to be 35 mass %.
[0224] Then, 50 g of 10 mass% triethylamine and 317 g of pure water were added to the obtained niobium-containing precipitate, and the mixture was stirred for 10 minutes to obtain a niobium-containing mixed liquid. 2 O 583 g of 35 mass% hydrogen peroxide was added to the tantalum-containing mixed liquid so that the hydrogen peroxide content was 5 mass% in terms of Nb conversion, 3.5 mass% in terms of metal conversion (Nb conversion), and the final hydrogen peroxide content was 6.8 mass%, and the mixture was stirred for 30 minutes to obtain a niobic acid compound-containing liquid according to Example 9. No precipitate or sediment was observed in the niobic acid compound-containing liquid according to Example 9. The pH of the niobic acid compound-containing liquid according to Example 9 was 10.4.
[0225] Example 10 In Example 10, the same manufacturing method as in Example 9 was carried out except that 10 mass% trimethylamine was added to the niobium-containing precipitate, to obtain a niobic acid compound-containing liquid according to Example 10. No precipitate or sediment was observed in the niobic acid compound-containing liquid according to Example 10. The pH of the niobic acid compound-containing liquid according to Example 10 was 10.7.
[0226] Comparative Example 10 In Comparative Example 10, the same manufacturing method as in Example 9 was carried out except that 10 mass% of methylamine was added to the niobium-containing precipitate, to obtain a niobic acid compound-containing liquid according to Comparative Example 10. A white precipitate was observed in the niobic acid compound-containing liquid according to Comparative Example 10. The pH of the niobic acid compound-containing liquid according to Comparative Example 10 was 10.3.
[0227] Comparative Example 11 In Comparative Example 11, the same manufacturing method as in Example 9 was carried out except that 10 mass% dimethylamine was added to the niobium-containing precipitate, to obtain a niobic acid compound-containing liquid according to Comparative Example 11. A white precipitate was observed in the niobic acid compound-containing liquid according to Comparative Example 11. The pH of the niobic acid compound-containing liquid according to Comparative Example 11 was 10.2.
[0228] Comparative Example 12 In Comparative Example 12, the same manufacturing method as in Example 9 was carried out except that 10 mass% TMAH was added to the niobium-containing precipitate, to obtain a niobic acid compound-containing liquid according to Comparative Example 12. A white precipitate was observed in the niobic acid compound-containing liquid according to Comparative Example 12. The pH of the niobic acid compound-containing liquid according to Comparative Example 12 was 10.1.
[0229] The following physical properties were measured for the metal acid compound-containing liquids obtained in Examples 1 to 10 and Comparative Examples 1 to 12. The measured physical properties and the methods for measuring the physical properties are shown below, and the measurement results for the metal acid compound-containing liquids of Examples 1 to 8 and Comparative Examples 1 to 9 are shown in Figure 1, and the measurement results for the metal acid compound-containing liquids of Examples 9 and 10 and Comparative Examples 10 to 12 are shown in Figure 2.
[0230] <Elemental analysis> If necessary, the sample was appropriately diluted with dilute hydrochloric acid, and the Ta was measured using an ICP emission spectrometer (Agilent Technologies: AG-5110) in accordance with JIS K0116:2014. 2 O 5 Weight fraction of Ta converted to Nb 2 O 5 Converted Nb weight fraction, TiO 2 Converted Ti weight fraction, MoO 3 Mo weight fraction converted to WO 3 Converted W weight fraction, ZrO 2 Zr weight fraction of HfO 2 Converted Hf weight fraction, SiO 2 The weight fraction of silicon converted into rare earth metal equivalent, or the weight fraction of rare earth element converted into rare earth metal equivalent, was measured.
[0231] Dynamic Light Scattering The particle size distribution was evaluated using a zeta potential, particle size, and molecular weight measurement system (Otsuka Electronics Co., Ltd.: ELSZ-2000) in accordance with JIS Z 8828:2019 "Particle size analysis - dynamic light scattering method". In addition, to remove dust and other particles from the solution to be measured immediately before the measurement, the solution was filtered with a filter with a pore size of 2 μm, and ultrasonic treatment was performed for 3 minutes at 28 kHz using an ultrasonic cleaner (As One Co., Ltd.: VS-100III). The particle size (D50) refers to the median diameter (D50), which is the particle size that shows the 50% cumulative value of the cumulative distribution curve.
[0232] The initial particle diameter (D50) of particles in the metal acid compound-containing liquid obtained in Examples 1 to 10 and Comparative Examples 1 to 12 and the particle diameter over time (D50) of particles in the metal acid compound-containing liquid after standing for 20 days in an incubator set at room temperature of 25°C were calculated. The above-mentioned filtering was performed when measuring the "initial particle diameter D50 (nm)", but was not performed when measuring the "particle diameter over time D50 (nm)", and only ultrasonic treatment was performed. The metal acid compound-containing liquids according to Comparative Examples 1 to 12 were not measured for the "initial particle diameter D50 (nm)" and "particle diameter over time D50 (nm)" because precipitates were deposited.
[0233] <Transmittance measurement> 4 ml of the metal acid compound-containing liquid obtained in Examples 1 to 10 and Comparative Examples 1 to 12 was placed in a quartz cell with an optical path length of 5.0 mm, and the transmittance in the wavelength region of 550 nm to 700 nm (specifically, the transmittance at wavelengths of 550 nm, 600 nm, 650 nm, and 700 nm) of the metal acid compound-containing liquid according to Examples 1 to 10 and Comparative Examples 1 to 12 was measured using a spectrophotometer according to the transmittance measurement conditions described above. The "initial transmittance" in Figs. 1 and 2 refers to the transmittance of the metal acid compound-containing liquid adjusted to a liquid temperature of 25°C immediately after production. In addition, the "tempered transmittance" in Figs. 1 and 2 refers to the transmittance of the metal acid compound-containing liquid after being left to stand for one month in an incubator set at room temperature of 25°C. Note that the metal acid compound-containing liquids according to Comparative Examples 1 to 12 were not measured for the "initial transmittance" and "tempered transmittance" because precipitates were deposited.
[0234] <pH measurement> The pH of the metal acid compound-containing liquid obtained in Examples 1 to 10 and Comparative Examples 1 to 12 was measured using an electrode (HORIBA: Standard ToupH electrode 9615S-10D) of a pH meter (HORIBA: Glass electrode type hydrogen ion concentration indicator D-51) after confirming that the liquid temperature had stabilized at 25°C. The "initial pH" in Figures 1 and 2 refers to the pH of the metal acid compound-containing liquid whose temperature was adjusted to 25°C immediately after production. Furthermore, the "pH over time" in Figures 1 and 2 refers to the pH of the metal acid compound-containing liquid after it was left to stand for one month in an incubator set at room temperature of 25°C.
[0235] <Film uniformity test> The appearance of the coating film formed on the surface of the glass substrate, which is a substitute for the current collector plate, was evaluated by observing it with an optical microscope. The metal acid compound-containing liquid obtained in Examples 1 to 10 and Comparative Examples 1 to 12 was filtered with a filter having a pore size of 2 μm, and dropped onto a 50 mm×50 mm glass substrate that had been degreased and washed with acetone and then dried using a syringe, and applied by spin coating (1,500 rpm, 15 seconds). The applied portion was then naturally dried to form a coating film on the glass substrate. The glass substrate was observed with an optical microscope (magnification: 40 times) in a central area of 15 mm×15 mm of the coating film formed. If no air bubbles, coating unevenness, or cracks were observed, the coating uniformity was evaluated as excellent and the glass substrate was evaluated as “○ (GOOD)”, and if even one was observed, the coating uniformity was evaluated as not excellent and the glass substrate was evaluated as “× (BAD)”.
[0236] As shown in Figures 1 and 2, the metal acid compound-containing liquids of Examples 1 to 10 contain a metal and / or metalloid element and a tertiary amine compound, and when the content of the metal and / or metalloid element in the metal acid compound-containing liquid is 0.1 mass% or more and less than 30% in terms of the metal and / or metalloid element, and the particle diameter (D50) of the particles in the metal acid compound-containing liquid is 1000 nm or less as measured by dynamic light scattering, the liquid has high dispersibility and excellent liquid stability.
[0237] Furthermore, the metal acid compound-containing liquids of Examples 1 to 10 contained a metal and / or metalloid element and a tertiary amine compound, and when the content of the metal and / or metalloid element in the metal acid compound-containing liquid was 0.1 mass% or more and less than 30% in terms of the metal of the metal and / or metalloid element, and the maximum transmittance of the metal acid compound-containing liquid in the wavelength range of 550 nm to 700 nm was 70%T or more, the liquid had high dispersibility and excellent liquid stability.
[0238] Furthermore, the metal acid compound-containing liquids of Examples 1 to 10 had high dispersibility and excellent liquid stability when the metal and / or metalloid elements contained in the metal acid compound-containing liquid were one or more selected from Ta, Nb, Ti, Zr, Mo, W, Hf, Si, and rare earth elements.
[0239] In addition, the metal acid compound-containing liquids of Examples 1 to 10 had reduced environmental impact when the tertiary amine compound contained in the metal acid compound-containing liquid was one or more selected from trimethylamine, triethylamine, and tri-n-propylamine.
[0240] The inventions disclosed in this specification include, in addition to the configurations of each invention or embodiment, those that are specified by changing these partial configurations to other configurations disclosed in this specification, to the extent applicable, or those that are specified by adding other configurations disclosed in this specification to these configurations, or those that are specified as higher-level concepts by deleting these partial configurations to the extent that partial action and effects are obtained. [Industrial Applicability]
[0241] The metal acid compound-containing liquid according to the present invention and its manufacturing method are suitable for forming a uniform metal acid compound coating film on the surface of a substrate, etc., because of their low environmental impact and high dispersibility. In addition, the metal acid compound-containing liquid according to the present invention and its manufacturing method have excellent storage stability, and the occurrence rate of defective products due to the occurrence of precipitation due to changes over time can be suppressed, so that waste can be reduced and the energy cost for waste disposal can be reduced. In particular, the use of amines can be reduced, so that the environmental impact can be reduced. Reduction of waste can reduce the occurrence rate of defective products, leading to the sustainable management and efficient benefits of natural resources, as well as the achievement of decarbonization (carbon neutrality).
Claims
1. A metal acid compound-containing liquid containing a metal and / or metalloid element, a tertiary amine compound, and hydrogen peroxide, The metal and / or metalloid element includes at least Ta and / or Nb among one or more selected from Ta, Nb, Ti, Zr, Mo, W, Hf, Si, and rare earth elements; A metal acid compound-containing liquid, wherein the particle diameter (D50) of particles in the metal acid compound-containing liquid as measured by dynamic light scattering is 1000 nm or less.
2. A metal acid compound-containing liquid containing a metal and / or metalloid element, a tertiary amine compound, and hydrogen peroxide, The metal and / or metalloid element includes at least Ta and / or Nb among one or more selected from Ta, Nb, Ti, Zr, Mo, W, Hf, Si, and rare earth elements; A metal acid compound-containing liquid, characterized in that the maximum transmittance of the metal acid compound-containing liquid in the wavelength region of 550 nm to 700 nm is 70% T or more.
3. The metal acid compound-containing liquid according to claim 1 or 2, characterized in that the content of the metal and / or metalloid elements in the metal acid compound-containing liquid is more than 0 mass% and less than 30% in terms of metal equivalent of the metal and / or metalloid elements.
4. 3. The metal acid compound-containing liquid according to claim 1, wherein the tertiary amine compound is at least one selected from the group consisting of trimethylamine, triethylamine, and tri-n-propylamine.
5. A complex metal acid compound-containing liquid comprising the metal acid compound-containing liquid according to claim 1 or 2, and at least one element A selected from the group consisting of Li, Na, Mg, Al, K, Ca, V, Mn, Fe, Co, Ni, Cu, Zn, Sn, Sr, and Ba.
6. neutralizing an acidic metal aqueous solution containing a metal and / or metalloid element with an alkaline aqueous solution to produce a precipitate containing the metal and / or metalloid element; adding a tertiary amine compound and hydrogen peroxide to the precipitate to generate a metal acid compound-containing liquid; having A method for producing a metal acid compound-containing liquid, characterized in that the metal and / or metalloid element contains at least Ta and / or Nb, among one or more selected from Ta, Nb, Ti, Zr, Mo, W, Hf, Si, and rare earth elements.
7. 7. The method for producing a metal acid compound-containing liquid according to claim 6, further comprising a step of removing the hydrogen peroxide.
8. 3. A method for producing a metal acid compound-containing film, comprising applying the metal acid compound-containing liquid according to claim 1 or 2 to a substrate, and drying and / or baking the coating.
9. A method for producing a metal acid compound-containing film, comprising applying a metal acid compound-containing liquid produced by the method for producing a metal acid compound-containing liquid according to claim 6 or 7 to a substrate, and drying and / or firing the substrate.
10. neutralizing an acidic metal aqueous solution containing a metal and / or metalloid element with an alkaline aqueous solution to produce a precipitate containing the metal and / or metalloid element; adding a tertiary amine compound and hydrogen peroxide to the precipitate to generate a metal acid compound-containing liquid; mixing the metal acid compound-containing liquid with at least one element A selected from the group consisting of Li, Na, Mg, Al, K, Ca, V, Mn, Fe, Co, Ni, Cu, Zn, Sn, Sr, and Ba to produce a composite metal acid compound-containing liquid; having A method for producing a liquid containing a complex metal acid compound, characterized in that the metal and / or semimetal element contains at least Ta and / or Nb, among one or more selected from Ta, Nb, Ti, Zr, Mo, W, Hf, Si, and rare earth elements.
11. 11. The method for producing a complex metal acid compound-containing liquid according to claim 10, further comprising a step of removing the hydrogen peroxide.
12. A method for producing a complex metal acid compound-containing film, comprising applying the complex metal acid compound-containing liquid according to claim 5 to a substrate, and drying and / or firing the same.
13. A method for producing a complex metal acid compound-containing film, comprising applying a complex metal acid compound-containing liquid produced by the method for producing a complex metal acid compound-containing liquid according to claim 10 or 11 to a substrate, and drying and / or firing the substrate.
Citation Information
Patent Citations
Precipitation of tantalum or niobium compound
JP1982003717A
Organotantalum aqueous solution and method for producing tantalum lactate peroxy compound crystal
JP2006182714A
Ferroelectric substance, its manufacturing method and ferroelectric device using the method
JP2007005161A
Hydrothermal method for manufacturing NANO to micrometer-scale particle
JP2008044833A
Niobic acid organosol and process for producing the same
JP2018127392A