Positive electrode current collector for lead-acid batteries and lead-acid batteries
The positive electrode current collector with a defined width ratio and roughened surface improves adhesion and structural stability, addressing adhesion issues in conventional collectors, thereby enhancing charge acceptance and capacity retention in lead-acid batteries.
Patent Information
- Application Number
- JP2022083174
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-05-20
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2042-05-20
AI Technical Summary
Conventional positive electrode current collectors for lead-acid batteries face issues with adhesion between the electrode material and the collector, leading to decreased capacity retention and charge acceptance performance, particularly in over-discharged states.
A positive electrode current collector with a specific width ratio (0.4 ≤ Y/X ≤ 0.8) and a roughened surface (1.0 μm ≤ Ra ≤ 50 μm) is designed, featuring an inclined surface to enhance adhesion and mitigate expansion/contraction effects, using a lead alloy with a Sn content of 1.1% by mass or more.
The solution improves adhesion between the electrode material and the current collector, enhancing charge acceptance performance and reducing capacity retention loss, especially in over-discharged states, while maintaining structural integrity.
Smart Images

Figure 0007947749000009 
Figure 0007947749000010 
Figure 0007947749000011
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to a positive electrode current collector for a lead-acid battery and a lead-acid battery.
BACKGROUND ART
[0002] Lead-acid batteries are used in various applications including in-vehicle and industrial uses. A lead-acid battery typically includes an electrode plate group in which positive electrode plates and negative electrode plates are alternately stacked with a separator interposed therebetween. The positive electrode plate includes a positive electrode current collector and a positive electrode material held by the positive electrode current collector. Conventionally, various positive electrode current collectors for lead-acid batteries have been proposed.
[0003] Patent Document 1 (Japanese Unexamined Patent Publication No. 2021-170429) discloses "A positive electrode current collector for a lead-acid battery, comprising a frame bone portion and inner bone portions extending inward of the frame bone portion, wherein the positive electrode current collector has an Sn concentration of 1.1 mass% or more, and in a cross section perpendicular to the extending direction of the inner bone portion, a width (Y) in a first direction which is the thickness direction of the positive electrode current collector and a width (X) in a second direction which is perpendicular to the extending direction and the first direction satisfy a relationship of 0.4≦Y / X≦0.8."
[0004] Patent Document 2 (Japanese Unexamined Patent Publication No. 2003-242983) discloses "A foil for a positive electrode current collector of a lead-acid battery, characterized by being made of titanium or a titanium alloy, and having a surface roughness of 0.05<Ra<1.0 and 0.3<Ry<7.0 on at least one surface."
PRIOR ART DOCUMENTS
PATENT DOCUMENTS
[0005]
PATENT DOCUMENT 1
PATENT DOCUMENT 2
SUMMARY OF THE INVENTION
PROBLEMS TO BE SOLVED BY THE INVENTION
[0006] The positive electrode current collector holds the positive electrode material and contributes to the flow of current during charging and discharging. Therefore, the performance of a lead-acid battery changes significantly depending on the relationship between the positive electrode current collector and the positive electrode material. In this context, one of the objectives of the present invention is to provide a positive electrode current collector capable of constructing a lead-acid battery that can exhibit high performance, and a lead-acid battery using the same. [Means for solving the problem]
[0007] One aspect of the present invention relates to a positive electrode current collector for a lead-acid battery. The positive electrode current collector is a positive electrode current collector for a lead-acid battery and includes a frame and an inner frame disposed inside the frame, wherein the width Y in a first direction and the width X in a second direction in a cross section of at least a portion of the inner frame perpendicular to the extension direction of the inner frame satisfy the relationship 0.4 ≤ Y / X ≤ 0.8, the first direction is the thickness direction of the positive electrode current collector, and the second direction is perpendicular to the extension direction and the thickness direction, the surface of at least a portion of the inner frame includes a roughened surface having an arithmetic mean roughness Ra of 1.0 μm or more and 50 μm or less, and the surface of at least a portion of the inner frame has a surface extending along the extension direction and inclined with respect to the thickness direction.
[0008] Another aspect of the present invention relates to a lead-acid battery. The lead-acid battery comprises a positive electrode plate, a negative electrode plate, and an electrolyte, wherein the positive electrode plate comprises a positive electrode current collector for a lead-acid battery according to one aspect of the present invention and a positive electrode material held by the positive electrode current collector. [Effects of the Invention]
[0009] According to the present invention, a high-performance lead-acid battery can be obtained. [Brief explanation of the drawing]
[0010] [Figure 1] This is a schematic top view showing an example of a positive electrode current collector of Embodiment 1. [Figure 2]This figure schematically shows an example of a cross-section along line II-II in Figure 1. [Figure 3] This figure schematically shows another example of a cross-section along line II-II in Figure 1. [Figure 4A] This is a schematic cross-sectional view illustrating one step in an example of a manufacturing method for a positive electrode current collector. [Figure 4B] This is a schematic cross-sectional view showing an example of a step following the step shown in Figure 4A. [Figure 5] This is a schematic top view showing another example of the positive electrode current collector of Embodiment 1. [Figure 6] Figure 2 is a schematic cross-sectional view showing an example of a positive electrode using the positive electrode current collector shown. [Figure 7] This is a schematic exploded perspective view showing an example of a lead-acid battery according to Embodiment 2. [Figure 8] This graph schematically shows an example of the results of the implemented example. [Figure 9] This graph schematically shows another example of the results of the implemented example. [Figure 10] This graph schematically shows another example of the results of the implemented example. [Modes for carrying out the invention]
[0011] The following describes embodiments of the present invention with examples, but the present invention is not limited to the examples described below. In the following description, specific numerical values and materials may be given as examples, but other numerical values and other materials may be applied as long as the present invention can be implemented. In this specification, the description "numerical value A to numerical value B" includes numerical value A and numerical value B, and can be read as "greater than or equal to numerical value A and less than or equal to numerical value B". In the following description, when lower and upper limits of numerical values relating to specific physical properties or conditions are given as examples, either of the given lower limits and either of the given upper limits can be arbitrarily combined, as long as the lower limit is not greater than or equal to the upper limit.
[0012] (Positive electrode current collector for lead-acid batteries) A positive electrode current collector according to one aspect of the present invention is a positive electrode current collector for a lead-acid battery. Hereinafter, the positive electrode current collector according to one aspect of the present invention may be referred to as "positive electrode current collector (C)".
[0013] The positive electrode current collector (C) includes a frame bone and inner bones arranged inside the frame bone. In a cross section of at least a part of the inner bone, the cross section being perpendicular to the extending direction LD of at least a part of the inner bone, the width Y in the first direction D1 and the width X in the second direction D2 satisfy the relationship of 0.4≦Y / X≦0.8. Hereinafter, the at least part of the inner bone that satisfies the relationship of 0.4≦Y / X≦0.8 may be referred to as "part (P)". The first direction D1 is the thickness direction TD of the positive electrode current collector (C). The second direction D2 is a direction perpendicular to the extending direction LD and the thickness direction TD. The surface of the part (P) of the inner bone includes a roughened surface having an arithmetic mean roughness Ra of 1.0 μm or more and 50 μm or less. The part (P) has a surface (sloped surface) that extends along the extending direction LD and is inclined with respect to the thickness direction TD.
[0014] Conventionally, as positive electrode current collectors, grid bodies formed by punching (punching grids), grid bodies formed by expanding processing (expanded grids), grid bodies formed by casting (cast grids), and the like have been used. Among these, the punching grid allows easier control of the grid surface to a specified surface roughness compared to the cast grid. Further, by forming the punching grid through punching of a rolled plate, it is possible to form a punching grid including a plurality of metal structures with different corrosion modes. Thereby, corrosion of the positive electrode current collector can be suppressed. The positive electrode current collector (C) according to the present embodiment is preferably formed by punching processing.
[0015] On the other hand, conventional perforated grids have inferior adhesion between the positive electrode current collector and the positive electrode material compared to cast grids and expanded grids. This is due to differences in grid shape and manufacturing method. The surface of cast grids is roughened by release agents used during casting, resulting in a large contact area with the positive electrode material. In expanded grids, the internal frame is twisted due to the manufacturing method, resulting in good adhesion with the positive electrode material. Furthermore, since expanded grids do not have vertical frame bones, the grid strength in the vertical direction is weak, allowing it to follow the shrinkage of the positive electrode material. Therefore, when using expanded grids, it is possible to suppress the formation of voids between the expanded grid and the positive electrode material.
[0016] On the other hand, while perforated grids can be formed using rolled sheets, similar to expanded grids, perforated grids are formed by punching out the rolled sheets. Therefore, the surface of the inner frame of a perforated grid is smooth, and the adhesion between the grid and the positive electrode material is inferior to that of other grids. Consequently, using a perforated grid as a positive electrode current collector can lead to a decrease in capacity retention and a decrease in charge acceptance performance after being left over-discharged.
[0017] As a result of their investigation, the inventors of this application have newly discovered that the decrease in capacity retention rate can be dramatically suppressed by deforming the perforated grid into a predetermined shape and further roughening its surface within a predetermined range.
[0018] Specifically, the internal bone is formed such that the width Y and width X of at least a portion of the internal bone satisfy the relationship 0.4 ≤ Y / X ≤ 0.8. Furthermore, the surface of at least a portion (P) of the internal bone is made to have a roughened surface with an arithmetic mean roughness Ra of 1.0 μm or more and 50 μm or less. As is common technical knowledge to those skilled in the art, it is expected that the higher the arithmetic mean roughness Ra of the internal bone surface, the better the performance. However, it has recently been found that sufficient effect cannot be obtained when the arithmetic mean roughness Ra exceeds 50 μm. In the range of arithmetic mean roughness Ra from 1.0 to 50 μm, it is thought that when the positive electrode paste is filled, the positive electrode paste penetrates the roughened surface, exhibiting a high anchoring effect and improving the adhesion between the positive electrode current collector and the positive electrode material. On the other hand, when the arithmetic mean roughness Ra exceeds 50 μm, the anchoring effect decreases, and it is thought that the roughening no longer contributes to improving the adhesion between the positive electrode current collector and the positive electrode material.
[0019] When filling a conventional grid (positive electrode current collector) with electrode material, the direction in which the electrode material is compressed is approximately parallel to the wall portion of the grid opening (inside the opening), making it difficult to firmly press the electrode material against the wall portion. Therefore, in conventional grids, the adhesion between the electrode material and the grid was sometimes insufficient. Furthermore, in conventional grids, it was difficult to roughen the surface of the wall portion of the grid opening (inside the opening). Therefore, the inventors of this invention have made at least a portion (P) of the inner bone wider (Y / X ≤ 0.8), and this at least portion (P) has the above-mentioned inclined surface (slope), and the surface of the inner bone has been roughened. As a result, when filling with electrode material, the surface area of the inner bone that is firmly pressed against the electrode material is increased. Furthermore, the adhesion between the electrode material and the inner bone is increased in the roughened portion. Therefore, the adhesion between the electrode material and the positive electrode current collector (C) is greatly improved.
[0020] Furthermore, the presence of the above-mentioned slope on the positive electrode current collector (C) mitigates the effects of expansion and contraction of the positive electrode material, thereby maintaining high adhesion between the positive electrode current collector (C) and the positive electrode material.
[0021] The angle α (acute angle shown in Figure 2) between the slope and the thickness direction TD in a cross section perpendicular to the extension direction LD is not particularly limited. The angle α may be constant or it may vary. That is, the slope may be generally flat or it may be curved. The angle α may be 30° or more, 45° or more, or 60° or more, or 80° or less, 75° or less, or 60° or less. The angle α may be in the range of 30° to 80°, 45° to 80°, or 60° to 80°. In any of these ranges, the upper limit may be 75° or 60°. By setting the angle α to 45° or more (for example, 60° or more), it becomes easier to improve the adhesion between the slope and the electrode material when filling the positive electrode material into the positive electrode current collector. Note that in a cross section perpendicular to the extension direction LD, the angle between the slope and the thickness direction TD at the midpoint of the line segment representing the slope may be within the range exemplified for angle α.
[0022] In the positive electrode current collector (C), when the total length of the internal bones excluding the parts where the internal bones intersect (the length of each internal bone in the extension direction) is taken as the length L, the total length Lp of the parts (P) (the length of the parts (P) in the extension direction) may be 0.5L or more, 0.7L or more, 0.9L or more, or 0.95L or more. The total Lp may be 1.0L or less, 0.95L or less, or 0.9L or less. The total Lp may be in the range of 0.5L to 1.0L, 0.7L to 1.0L, 0.9L to 1.0L, or 0.95L to 1.0L. Within these ranges, the upper limit may be 0.95L or 0.9L, as long as the lower limit does not exceed the upper limit. By making the total length Lp of the parts (P) in the positive electrode current collector (C) 0.5L or more, the effects of the present invention can be fully realized.
[0023] The positive electrode current collector (C) may be made of a lead alloy containing Sn. In that case, the Sn content of the positive electrode current collector (C) may be 1.1% by mass or more, 1.3% by mass or more, or 1.5% by mass or more. The content may be 1.8% by mass or less, 1.5% by mass or less, or 1.3% by mass or less. The content may be in the range of 1.1 to 1.8% by mass, 1.3 to 1.8% by mass, or 1.5 to 1.8% by mass. Within these ranges, the upper limit may be 1.5% by mass or 1.3% by mass, as long as the lower limit does not exceed the upper limit.
[0024] By setting the Sn content of the positive electrode current collector (C) to 1.1% by mass or more, the charge acceptance performance after being left in an over-discharged state can be improved. Generally, increasing the Sn content reduces the adhesion between the positive electrode current collector and the positive electrode material, leading to a decrease in capacity retention. However, by using the positive electrode current collector (C) according to this embodiment, the adhesion between the positive electrode current collector (C) and the positive electrode material can be significantly improved. Therefore, by setting the Sn content to 1.1% by mass or more, the decrease in capacity retention can be particularly suppressed. As a result, it is possible to improve the charge acceptance performance after being left in an over-discharged state while suppressing the decrease in capacity retention. Examples of lead alloys containing Sn will be described later.
[0025] The positive electrode current collector (C) may include vertical frame ribs. The width Wf of the vertical frame ribs may be 0.3 mm or more, 0.5 mm or more, 0.7 mm or more, 1.0 mm or more, 1.3 mm or more, or 1.5 mm or more. The width Wf of the vertical frame ribs may be 2.5 mm or less, 2.0 mm or less, or 1.7 mm or less. The width Wf of the vertical frame ribs may be in the range of 0.5 to 2.0 mm (0.5 mm or more and 2.0 mm or less), 0.7 to 2.0 mm, 1.0 to 2.0 mm, or 1.3 to 2.0 mm. Within these ranges, the upper limit may be 1.7 mm or 1.5 mm.
[0026] By setting the width Wf of the vertical frame ribs to 0.5 mm or more and 2.0 mm or less, the amount of curvature of the positive electrode current collector can be reduced. The reason for this is thought to be as follows: The arithmetic mean roughness Ra of the roughened surface of the inner ribs is 1.0 μm or more and 50 μm or less. A high anchoring effect is achieved on the surface of the inner ribs having such surface roughness. Therefore, when manufacturing the positive electrode plate, the positive electrode paste penetrates into the roughened part of the inner rib surface, improving the adhesion between the inner ribs and the positive electrode material. This adhesion is effective even during overcharging, and even if corrosion of the inner ribs occurs during overcharging, the penetration of sulfuric acid between the inner ribs and the positive electrode material is suppressed. As a result, the elongation of the inner ribs due to corrosion is suppressed.
[0027] When the width Wf of the vertical frame bone is in the range of 0.5 to 2.0 mm, the outward spreading force of the frame bone resists the outward spreading force of the internal bone due to corrosion, thus maintaining balance. When the width Wf is less than 0.5 mm, the spreading force of the internal bone is greater than the spreading force of the frame bone, resulting in greater curvature. When the width Wf is greater than 2.0 mm, the resistance of the vertical frame bone is greater than the spreading force of the internal bone, resulting in greater curvature.
[0028] As described above, by setting the width Wf to a range of 0.5 to 2.0 mm, a balance is achieved between the outward force of the inner frame and the outward force of the frame. Therefore, the elongation and curvature of the positive electrode current collector (C) are suppressed, and as a result, gaps are less likely to form between the positive electrode current collector (C) and the positive electrode material. In addition, because the surface of the inner frame is roughened, the adhesion between the positive electrode current collector (C) and the positive electrode material is improved, further suppressing the elongation and curvature of the positive electrode current collector (C). On the other hand, in the case of a positive electrode current collector that is not roughened, the adhesion between the positive electrode current collector and the positive electrode material is low. In that case, the adverse effects of curvature of the positive electrode current collector become more pronounced. Specifically, curvature makes it easier for gaps to form between the positive electrode current collector and the positive electrode material, so elongation and curvature increase rapidly, further increasing the gap between the positive electrode current collector and the positive electrode material.
[0029] The arithmetic mean roughness Ra of the roughened surface of the endoskeleton is 1.0 μm or more and 50 μm or less. The arithmetic mean roughness Ra may be 2.0 μm or more, 5.0 μm or more, 10 μm or more, or 20 μm or more. The arithmetic mean roughness Ra may be 50 μm or less, 30 μm or less, or 20 μm or less. The arithmetic mean roughness Ra may be in the range of 1.0 to 50 μm, 2.0 to 50 μm, 5.0 to 50 μm, 10 to 50 μm, or 20 to 50 μm. Within these ranges, the upper limit may be 30 μm, 20 μm, or 10 μm, as long as the lower limit does not exceed the upper limit.
[0030] The ratio S1 / S0 of the area S1 of the roughened surface of the inner bone (i.e., the surface with an arithmetic mean roughness Ra of 1.0 μm or more and 50 μm or less) to the area S0 of the inner bone surface may be 0.3 or more, or 0.4 or more, and may be 0.9 or less, 0.8 or less, or 0.6 or less. The ratio S1 / S0 may be in the range of 0.3 to 0.9, or in the range of 0.4 to 0.9. Within these ranges, the upper limit may be 0.8 or 0.6. By setting the ratio S1 / S0 in the range of 0.3 to 0.8 (for example, the range of 0.4 to 0.6), the charge acceptance performance can be particularly improved. Examples of surfaces roughened by press working include the surface facing the main surface of the positive electrode plate (surfaces 120sa and / or surface 120sc in Figures 2 and 3). In a preferred example, the surface facing the main surface of the positive electrode plate in the above part (P) is roughened so that the arithmetic mean roughness Ra is 1.0 μm or more and 50 μm or less.
[0031] The roughened surface described above, and the surface of a portion (P) that is inclined with respect to the thickness direction TD (the sloped surface described above), may be a surface processed by press working.
[0032] The roughening rate, which indicates the proportion of the surface area of the endoskeleton that is roughened, is expressed by the following formula. In the following formula, a roughened surface means a surface that has been roughened so that its arithmetic mean roughness Ra is 1.0 μm or more and 50 μm or less. Roughening rate (%) = 100 × (Area of roughened surface within the endoskeleton surface) / (Area of the endoskeleton surface)
[0033] The surface roughening rate may be 20% or more, 40% or more, or 50% or more. The surface roughening rate may be 80% or less, 60% or less, or 50% or less. The surface roughening rate may be in the range of 20-80%, 40-80%, or 50-80%. In any of these ranges, the upper limit may be 60% or 50%, as long as the lower limit does not exceed the upper limit. From the viewpoint of achieving both high capacity retention and high charge acceptance, the surface roughening rate may be in the range of 40-80% (for example, 40-60%).
[0034] Examples of the configuration of the positive electrode current collector (C) are described below. The positive electrode current collector (C) includes a frame and an inner frame. The positive electrode current collector (C) may also include lugs provided on the frame.
[0035] The positive electrode current collector (C) is preferably formed by further pressing a punched grid obtained by a punching process. The positive electrode current collector (C) may include a frame, ears provided on the frame, and an inner frame inside the frame. A preferred example of the positive electrode current collector (C) is a grid-shaped current collector (grid body). In a grid body, the inner frame portion is grid-shaped (including mesh-like). Using a grid body makes it easier to support the electrode material. The frame is preferably rectangular. The rectangle does not have to be a strict rectangle; the vertices may be slightly rounded, or each side may be slightly bent.
[0036] (frame) The frame structure is formed to surround the outer perimeter of the area where the internal bones are placed. The frame structure has, for example, a rectangular shape. The rectangular shape does not have to be a perfect rectangle; the corners may be slightly rounded, and each side may be slightly curved. When the frame structure is rectangular, it includes an upper element, a lower element, and two lateral elements connecting them. The upper element and the lower element may be referred to as the "horizontal frame structure" below. The two lateral elements may be referred to as the "vertical frame structure" below. The ear portion may be continuous with the upper element.
[0037] There are no particular limitations on the shape of the cross-section of the frame frame (the cross-section perpendicular to the extension direction). The cross-sectional shape of the frame frame may be the same as or different from the cross-sectional shape of the inner frame. The cross-sectional shape of the frame frame may be rectangular or polygonal. If the cross-sectional shape of the frame frame is polygonal, the corners of the polygon may be rounded, and the sides of the polygon may be curved to some extent. The cross-sectional area of the frame frame may be larger than the cross-sectional area of the inner frame. The frame frame has the function of maintaining the shape of the positive electrode current collector (C).
[0038] (Internal bones) The internal bones are located inside the frame bones. There are no particular limitations on the arrangement of the internal bones. In one example, the internal bones are arranged in a grid pattern. The internal bones may include longitudinal bones parallel to the longitudinal frame bones and transverse bones parallel to the upper elements (transverse frame bones). At least a portion of the longitudinal bones may be inclined obliquely with respect to the longitudinal frame bones. At least a portion of the transverse bones may be inclined obliquely with respect to the upper elements. The internal bones may include internal bones extending radially from the ear portion. The internal bones may be straight, curved, or bent.
[0039] As described above, a portion of the endoskeleton (P) has a surface that extends along its extension direction and is inclined with respect to the thickness direction TD (a bevel). The shape of the cross-section of the endoskeleton having such a bevel (a cross-section perpendicular to the extension direction LD) may be quadrangular (e.g., rhombic), hexagonal, or octagonal. If the cross-sectional shape of the endoskeleton is polygonal, the corners of the polygon may be rounded, and the sides of the polygon may be curved to some extent.
[0040] (Manufacturing method for positive electrode current collector (C)) An example of a manufacturing method for the positive electrode current collector (C) is described below. However, the positive electrode current collector (C) may also be manufactured by a manufacturing method other than the one described below.
[0041] This manufacturing method includes steps (i) and (ii) in that order. Step (i) is a step of forming an intermediate lattice body by punching out a metal sheet. The intermediate lattice body includes a frame portion that serves as the frame structure and an intermediate frame that serves as the inner structure. There are no particular limitations on the metal sheet; a sheet made of the metal that constitutes the positive electrode current collector can be used. The metal sheet may also be a rolled sheet.
[0042] Step (ii) is a step in which the intermediate lattice is press-formed in the thickness direction of the intermediate lattice to process the intermediate bones into inner bones. The intermediate bones are deformed by the press-formed process and processed into inner bones having the above-described characteristics. In addition, the surface of the intermediate lattice is roughened by the press-formed process so that the arithmetic mean roughness Ra of the surface of the inner bones is 1.0 μm or more and 50 μm or less. The frame portion may be deformed during the press-formed process. That is, the frame portion formed in step (i) may be deformed and used as frame bones. Alternatively, the frame portion formed in step (i) may be used as frame bones as is.
[0043] Surface roughening by press working can be achieved by roughening the surfaces of the lower and upper dies used in the press working process. Specifically, by roughening the press surfaces of the lower and upper dies that come into contact with the intermediate grid, the surface of the resulting molded product can be roughened. The degree of roughening of the press surface is reflected in the degree of roughening of the molded product's surface. Therefore, by changing the degree of roughening of the press surface, the degree of roughening of the surface of the positive electrode current collector (C) (for example, the surface of the inner bone) can be controlled.
[0044] The current collector obtained in step (ii) can be used as is as the positive electrode current collector (C). Step (ii) may be repeated multiple times if necessary. In this case, the same location may be press-formed in each step (ii), or different locations may be press-formed. Furthermore, if necessary, the current collector obtained in step (ii) may be further processed before being used as the positive electrode current collector (C).
[0045] The surface roughening of the endoskeleton may be performed by methods other than press working. However, press working is preferred because it allows for easy roughening of only a portion of the endoskeleton's surface.
[0046] (lead acid battery) The lead-acid battery according to this embodiment includes a positive electrode plate, a negative electrode plate, and an electrolyte. The positive electrode plate includes a positive electrode current collector (C) (positive electrode current collector for lead-acid battery) according to this embodiment and a positive electrode material held by the positive electrode current collector (C).
[0047] There are no particular limitations on the components other than the positive electrode current collector, and components used in known lead-acid batteries may be used. The lead-acid battery may be an electrolyte lead-acid battery or a valve-regulated lead-acid (VRLA) lead-acid battery. There are no particular limitations on the manufacturing method of the lead-acid battery, except for the manufacturing method of the positive electrode current collector (C), and known manufacturing methods may be applied.
[0048] When lead-acid batteries are installed in vehicles such as automobiles, they are sometimes placed in the engine compartment. In this case, the lead-acid batteries are exposed to high temperatures due to the heat generated by the engine. When the temperature of the lead-acid battery rises, corrosion of the current collector becomes more pronounced, and the impact of corrosion on the lifespan performance becomes significant. The adverse effects of corrosion can be reduced by using a positive electrode current collector (C). For this reason, a positive electrode current collector (C) can be preferably used in lead-acid batteries installed in the engine compartment of a vehicle.
[0049] In this specification, a fully charged lead-acid battery is defined as a state in which, in the case of an electrolyte-type battery, constant current charging is performed in a 25°C water bath at a current of 0.2 times the value indicated for the rated capacity until the voltage reaches 2.5V / cell, and then a further constant current charging is performed for 2 hours at a current of 0.2 times the value indicated for the rated capacity. In the case of a valve-regulated battery, a fully charged state is defined as a state in a 25°C air bath at a constant current and constant voltage of 2.23V / cell at a current of 0.2 times the value indicated for the rated capacity, and charging is terminated when the charging current during constant voltage charging becomes 0.005 times the value indicated for the rated capacity.
[0050] A fully charged lead-acid battery refers to a lead-acid battery that has been fully charged after chemical formation. Full charging of a lead-acid battery can be done immediately after chemical formation, or some time after formation (for example, a lead-acid battery that has been chemically formed and is in use (preferably in the early stages of use) may be fully charged). An early-stage battery refers to a battery that has not been in use for very long and has hardly deteriorated.
[0051] Examples of components of the lead-acid battery according to this embodiment are described below. Known components may be used for components other than those characteristic of this embodiment.
[0052] (Positive plate) The positive electrode plate includes a positive electrode current collector (C) and a positive electrode material held by the positive electrode current collector (C). A Pb-Sn alloy is preferred as the lead alloy used for the positive electrode current collector (C) in terms of corrosion resistance and mechanical strength. The positive electrode current collector (C) may be formed from a lead alloy such as a Pb-Ca alloy or a Pb-Ca-Sn alloy. Alternatively, lead with a purity of 99.9% by mass or higher may be used for the material of the positive electrode current collector (C).
[0053] The positive electrode material contains a positive electrode active material (lead dioxide or lead sulfate) that exhibits capacity through a redox reaction. The positive electrode material may also contain additives as needed.
[0054] The density of the positive electrode material is 3.6 g / cm³. 3 The above may also be acceptable. From the viewpoint of ensuring sufficient initial capacity, the density of the positive electrode material should be 4.8 g / cm³. 3 The following may also apply. Note that the density of the positive electrode material refers to the bulk density of the positive electrode material in a fully charged state.
[0055] Unformed positive electrode plates are obtained by filling a positive electrode current collector with positive electrode paste, followed by maturation and drying. The unformed positive electrode plates are then subjected to chemical formation. The positive electrode paste is prepared by mixing lead powder, additives, water, sulfuric acid, etc.
[0056] (Negative electrode plate) The negative electrode plate includes a negative electrode current collector and a negative electrode material held by the negative electrode current collector. The negative electrode current collector is not particularly limited, and known negative electrode current collectors may be used. The negative electrode current collector may be formed of lead or a lead alloy. Examples of lead alloys used for the negative electrode current collector include Pb-Ca alloys and Pb-Ca-Sn alloys. These lead or lead alloys may further contain at least one element selected from the group consisting of Ba, Ag, Al, Bi, As, Se, and Cu as an additive element. There is no limit to the method of forming the negative electrode current collector; it may be formed by casting lead or a lead alloy, or by processing a sheet of lead or a lead alloy. Examples of processing methods include expansion and punching.
[0057] The shape of the negative electrode current collector may be the same as that of the positive electrode current collector (C). The positive electrode current collector (C) may be used as the negative electrode current collector. Alternatively, a current collector different from the positive electrode current collector (C) may be used as the negative electrode current collector.
[0058] The negative electrode material contains, as an essential component, a negative electrode active material (lead or lead sulfate) that develops capacity through oxidation-reduction reactions. The negative electrode material may also contain additives such as organic shrinkage inhibitors, carbonaceous materials, and barium sulfate. While the charged negative electrode active material is spongy lead, the unformed negative electrode plate is usually made using lead powder. The density of the negative electrode material is 3 g / cm³. 3 The above totals 4.8 g / cm³. 3 The following is also acceptable.
[0059] Organic shrinkage inhibitors may include lignins and / or synthetic organic shrinkage inhibitors. Examples of lignins include lignin, ligninsulfonic acid, or lignin derivatives such as alkali metal salts (such as sodium salts). Synthetic organic shrinkage inhibitors are organic polymers containing sulfur, and generally contain multiple aromatic rings within the molecule, as well as sulfur as a sulfur-containing group. Among sulfur-containing groups, stable forms such as sulfonic acid groups or sulfonyl groups are preferred. Sulfonic acid groups may exist in acid form or in salt form, such as a sodium salt.
[0060] Carbonaceous materials such as carbon black, graphite, hard carbon, and soft carbon can be used as the carbonaceous material included in the negative electrode material. Examples of carbon black include acetylene black, Ketjen black, furnace black, and lamp black. Graphite can be any carbon material containing a graphite-type crystal structure, and may be either artificial graphite or natural graphite.
[0061] In the production of the negative electrode plate, first, an unformed negative electrode plate is produced by filling a negative electrode current collector with negative electrode paste, and then aging and drying it. Subsequently, the negative electrode plate is obtained by forming the unformed negative electrode plate. The negative electrode paste is produced by kneading lead powder and various additives with water and sulfuric acid. In the aging process, the unformed negative electrode plate may be aged at room temperature, or it may be aged at a higher temperature and humidity.
[0062] The chemical conversion can be carried out by immersing the electrode plate group, including the unconverted negative electrode plate, in the sulfuric acid-containing electrolyte in the lead-acid battery case and then charging the electrode plate group. However, the chemical conversion may also be performed before the assembly of the lead-acid battery or the electrode plate group. Spongy lead is produced by the chemical conversion.
[0063] (electrolyte) The electrolyte is an aqueous solution containing sulfuric acid, and may be gelled if necessary. The specific gravity of the electrolyte in a fully charged lead-acid battery at 20°C is preferably, for example, 1.20 or more and 1.35 or less, and 1.25 or more and 1.32 or less.
[0064] (Separator) A separator is typically placed between the negative and positive electrodes. Nonwoven fabrics, microporous membranes, and other materials are used as separators. The thickness and number of separators placed between the negative and positive electrodes should be selected according to the distance between the electrodes.
[0065] Nonwoven fabrics are mats made by intertwining fibers without weaving, and are primarily composed of fibers. For example, nonwoven fabrics are formed of fibers by 60% or more by mass. As fibers, glass fibers, polymer fibers (polyolefin fibers, acrylic fibers, polyester fibers such as polyethylene terephthalate fibers, etc.), pulp fibers, etc., can be used. Among these, glass fibers are preferred. Nonwoven fabrics may also contain components other than fibers, such as acid-resistant inorganic powders and polymers as binders.
[0066] On the other hand, a microporous membrane is a porous sheet mainly composed of materials other than fiber components. For example, it can be obtained by extruding a composition containing a pore-forming agent (such as polymer powder and / or oil) into a sheet, and then removing the pore-forming agent to form pores. Microporous membranes are preferably made of acid-resistant materials, and those mainly composed of polymer components are preferred. Polyolefins such as polyethylene and polypropylene are preferred as polymer components.
[0067] The separator may be composed of, for example, only a nonwoven fabric, or only a microporous membrane. Furthermore, the separator may, as needed, be a laminate of a nonwoven fabric and a microporous membrane, a combination of different or the same type of material, or a combination of different or the same type of material with interlocking protrusions and indentations.
[0068] The separator may be formed in the shape of a bag. In that case, the bag-shaped separator may house either the positive electrode plate or the negative electrode plate. When the bag-shaped separator houses the positive electrode plate, it can suppress a short circuit at the bottom caused by the positive electrode material detaching from the current collector and accumulating at the bottom of the battery case coming into contact with the negative electrode plate. On the other hand, when the bag-shaped separator houses the negative electrode plate, it can suppress a short circuit caused by the positive electrode current collector stretching and penetrating the separator. During overcharging, the stretching of the positive electrode current collector tends to be a problem, so in a preferred example, the bag-shaped separator houses the negative electrode plate.
[0069] (Explanation of terms and measurement methods) (Surface roughness) The arithmetic mean roughness Ra of the roughened surface of the endoskeleton is the arithmetic mean roughness Ra defined in JIS (Japanese Industrial Standards) B0601:2001, and is measured in accordance with that standard. The arithmetic mean roughness Ra can be measured, for example, using the "VK-X100 LASER MICROSCOPE" manufactured by Keyence Corporation.
[0070] The surface roughness of the roughened surface of the inner frame of the positive electrode current collector before the positive electrode material is placed can be measured as is. On the other hand, the surface roughness of the roughened part of the inner frame of the positive electrode current collector after the positive electrode material is placed should be measured after removing the positive electrode material. For example, the positive electrode current collector in a lead-acid battery is measured using the following procedure. First, the lead-acid battery is disassembled and the positive electrode plate is removed. Next, the removed positive electrode plate is treated with an alkaline mannitol solution and then washed with water to obtain a positive electrode current collector from which the positive electrode material has been removed. The obtained positive electrode current collector is then used to measure its surface roughness.
[0071] (Method for measuring width X and width Y) The width Y in the first direction and the width X in the second direction mentioned above are measured as follows. First, the positive electrode current collector is embedded in a thermosetting resin so that the entire positive electrode current collector is covered, and the resin is allowed to harden. Next, the positive electrode current collector embedded in the resin is cut in a cross section perpendicular to the extension direction of the internal bone. Then, the cross section of the internal bone exposed by the cut is photographed with a microscope or the like to obtain an image. Based on the obtained image, the width Y in the first direction and the width X in the second direction are calculated. At this time, the maximum values of width Y and width X in the predetermined image taken are used. In other words, consider a rectangle that circumscribes the internal bone in the photographed image, with each side parallel to the first direction D1 or the second direction D2. The length of the side in the first direction D1 in this rectangle is the width Y, and the length of the side in the second direction D2 is the width X. The ratio Y / X of the width Y in the first direction and the width X in the second direction is obtained from the calculated width Y and width X.
[0072] (Quantitative analysis of Sn in the positive electrode current collector) Before the positive electrode material is retained, a portion of the positive electrode current collector can be taken as a sample and analyzed. For positive electrode current collectors incorporated into lead-acid batteries, a sample for analysis is obtained using the following procedure. First, the positive electrode plate is removed from the lead-acid battery. Next, the positive electrode plate is vibrated to detach the positive electrode material from the positive electrode current collector. Then, a ceramic knife is used to remove any remaining positive electrode material around the positive electrode current collector, and a portion of the metallic-looking part of the positive electrode current collector is taken as a sample. Next, the mass of the collected sample is measured. Next, an aqueous solution is obtained by mixing the sample with tartaric acid and dilute nitric acid. Hydrochloric acid is added to the aqueous solution to precipitate lead chloride, which is then filtered, and the filtrate is collected. Using this filtrate, the Sn content in the positive electrode current collector is determined using the following procedure.
[0073] The quantification of Sn contained in the positive electrode current collector is performed according to the lead-separated inductively coupled plasma emission spectroscopy method described in JIS H2105:1955. More specifically, first, the Sn concentration in the filtrate is analyzed using a calibration curve method with an ICP emission spectrometer. Then, the Sn content in the positive electrode current collector is determined from the obtained concentration and the mass of the collected sample. The ICPS-8000 manufactured by Shimadzu Corporation can be used as the ICP emission spectrometer.
[0074] (Method for measuring the width of frame and vertical frame members) The frame structure is the part that makes up the edge of the current collector, and is provided so as to surround the area where the electrode material of the electrode plate is filled. The vertical frame structure is the frame structure that extends in the approximate vertical direction of the lead-acid battery. The horizontal frame structure is the frame structure that extends in the approximate left-right direction, with the direction perpendicular to the vertical direction being the left-right direction. The vertical frame structure may extend both vertically and diagonally in the left-right direction. The width of the vertical frame structure refers to the maximum length of the vertical frame structure in a direction parallel to the main surface of the positive electrode plate and perpendicular to the direction in which the vertical frame structure extends. The vertical direction of the lead-acid battery will be defined below. The width of the vertical frame structure can be measured using a caliper or the like. The width of the vertical frame structure of the positive electrode current collector incorporated into a lead-acid battery is measured by the following procedure. First, the lead-acid battery is disassembled and the positive electrode plate is removed. Next, the removed positive electrode plate is treated with an alkaline mannitol solution and then washed with water to obtain a positive electrode current collector from which the positive electrode material has been removed. The resulting positive electrode current collector is used to measure the width of the vertical frame ribs.
[0075] (The vertical direction of the lead-acid battery or its components) In this specification, the vertical direction of a lead-acid battery or its components (such as plates, cells, separators, etc.) means the vertical direction of the lead-acid battery in the state in which it is used.
[0076] (electrode material) The negative electrode material and the positive electrode material are usually held by the current collector. The electrode material is the portion of the electrode plate excluding the current collector. The electrode plate may have components such as mats or pasting paper attached to it. Since such components (also called attached components) are used integrally with the electrode plate, they are considered to be included in the electrode plate. When the electrode plate includes attached components (mats, pasting paper, etc.), the electrode material is the portion of the electrode plate excluding the current collector and attached components.
[0077] (Organic shrinkage inhibitor) Organic shrinkage inhibitors are organic compounds that have the function of suppressing the shrinkage of lead, the negative electrode active material, when lead-acid batteries are repeatedly charged and discharged.
[0078] (Fully charged) The fully charged state of an electrolyte lead-acid battery is defined by JIS D 5301:2019. More specifically, a fully charged state is defined as the state in which the lead-acid battery has been charged in a water bath at 25°C ± 2°C at a current (A) equal to 0.2 times the rated capacity (a value in Ah), until the terminal voltage (V) during charging, measured every 15 minutes, or the electrolyte density converted to a temperature of 20°C, shows a constant value with three significant figures for three consecutive times. In the case of a valve-regulated lead-acid battery, a fully charged state is defined as the state in which charging is performed in an air bath at 25°C ± 2°C at a constant current and constant voltage of 2.23V / cell at a current (A) equal to 0.2 times the rated capacity (a value in Ah), and charging is terminated when the charging current during constant voltage charging reaches a value (A) equal to 0.005 times the rated capacity (a value in Ah).
[0079] A fully charged lead-acid battery refers to a lead-acid battery that has been fully charged after chemical formation. Full charging of a lead-acid battery can be done after chemical formation, specifically, immediately after formation or after some time has passed since formation (for example, a lead-acid battery that has been formed and is in use (preferably in the early stages of use) can be fully charged). An early-stage battery refers to a battery that has not been in use for very long and has hardly deteriorated.
[0080] Hereinafter, an example of this embodiment will be specifically described with reference to the drawings. The embodiments described below can be modified based on the above description. Furthermore, the matters described below may be applied to the above embodiments. In addition, matters that are not essential to the invention of this disclosure may be omitted in the embodiments described below.
[0081] (Embodiment 1) Embodiment 1 describes an example of a positive electrode current collector (C). A schematic top view of the positive electrode current collector 100 of Embodiment 1 is shown in Figure 1. The positive electrode current collector 100 has a plate-like shape with numerous through holes formed on its inside. The positive electrode current collector 100 includes a frame frame 110 and an inner frame 120 inside the frame frame 110. The inner frame 120 is connected to the frame frame 110. The frame frame 110 includes an upper element (horizontal frame frame) 111, a lower element (horizontal frame frame) 112 facing the upper element 111, and a pair of side elements (vertical frame frame) 113, 114 connecting the upper element 111 and the lower element 112. An ear portion 130 is connected to the upper element 111. The example of the positive electrode current collector 100 shown in Figure 1 has a lower projection 132 that is continuous with the lower element 112.
[0082] The frame 110 shown in Figure 1 has a rectangular shape. The internal frame 120 includes a plurality of longitudinal ribs 120A and a plurality of transverse ribs 120B. Each of the longitudinal ribs 120A extends parallel to the lateral elements 113 (and lateral elements 114). Each of the transverse ribs 120B extends parallel to the upper elements 111 (and lower elements 112).
[0083] Figure 2 shows a cross-sectional view of the section along line II-II in Figure 1. The section along line II-II in Figure 1 indicates the extension direction LD of the longitudinal rib 120A in the section along line II-II. Figure 2 also shows the thickness direction TD, the first direction D1, and the second direction D2. The thickness direction TD and the first direction D1 are the thickness directions of the positive electrode current collector 100. The second direction D2 is perpendicular to the extension direction LD and the thickness direction TD.
[0084] Figure 2 shows the width Wf of the lateral element (vertical frame) 113. The width Wf is the width of the lateral element 113 in the direction perpendicular to the extension direction and the thickness direction.
[0085] Figure 2 further shows widths X and Y. Width Y is the width in the first direction D1 (thickness direction TD) in a cross section perpendicular to the extension direction LD of the longitudinal bone 120A (internal bone 120). Width X is the width in the second direction D2 in a cross section perpendicular to the extension direction LD of the longitudinal bone 120A (internal bone 120). Widths Y and X satisfy the relationship described above. The arithmetic mean roughness Ra of the roughened surface of the internal bone 120 is within the range described above.
[0086] In the example shown in Figure 2, the cross-section of the vertical bone 120A (internal bone 120) is octagonal, and may also be an octagon with rounded corners. The cross-section of the horizontal bone 120B (internal bone 120) has a similar shape. However, the cross-sectional shapes of the vertical bone 120A and the horizontal bone 120B may be different. Furthermore, the cross-sectional shapes of the vertical bone 120A and / or the horizontal bone 120B may vary depending on the position.
[0087] Referring to Figure 2, the vertical rib 120A (internal rib 120) has four surfaces 120sc that extend along the extension direction LD and are inclined with respect to the thickness direction TD. Furthermore, the vertical rib 120A (internal rib 120) has two surfaces 120sa that are substantially parallel to the main surface of the positive electrode current collector 100, and two surfaces 120sb that are aligned with the thickness direction TD (first direction D1). Note that the main surface of the positive electrode current collector 100 is the main surface when the positive electrode current collector 100 is considered as a single sheet.
[0088] Surfaces 120sa and 120sc are surfaces that are pressed during the press working process. Therefore, at least a portion of these surfaces can be roughened during the press working process. From one perspective, surfaces 120sa and 120sc facing the main surface of the positive electrode current collector 100 are roughened.
[0089] Figure 2 shows an example where the frame frame 110 is not press-formed, but the frame frame 110 may also be press-formed. In that case, the surface of the frame frame 110 may also be roughened in the same way as the surface of the inner frame 120. Furthermore, as mentioned above, the cross-sectional shape of the inner frame 120 may be other shapes. Figure 3 shows a cross-section of an example in which the cross-section of the inner frame 120 is hexagonal. The longitudinal frame 120A (inner frame 120) in the example shown in Figure 3 has four surfaces 120sc that extend along the extension direction LD and are inclined with respect to the thickness direction TD. In addition, the longitudinal frame 120A (inner frame 120) has two surfaces 120sb along the thickness direction TD (first direction D1).
[0090] Figure 2 shows the angle α at which the surface 120sc is inclined with respect to the thickness direction TD in a cross section perpendicular to the stretching direction LD. There are no particular limitations on the angle α, and it may be within the range described above.
[0091] An example of the manufacturing process for the positive electrode current collector 100 shown in Figures 2 and 3 will be explained using the cross-sectional views in Figures 4A and 4B. Note that Figures 4A and 4B only show the cross-sections of the parts corresponding to the parts shown in Figures 2 and 3. First, as shown in Figure 4A, a metal sheet 100x is prepared. The metal sheet 100x is, for example, a rolled sheet formed by rolling. Next, as shown in Figure 4B, the metal sheet 100x is punched out to form an intermediate grid 100y. The intermediate grid 100y includes a frame portion 110y which becomes the frame frame 110 and an intermediate frame 120y which becomes the inner frame 120. Next, the intermediate grid 100y is press-formed. This yields the positive electrode current collector 100 shown in Figure 2 or Figure 3.
[0092] During press working, the internal frame 120 (and the frame frame 110 if necessary) is pressed to achieve a desired cross-sectional shape and to achieve a desired surface roughening. An example of press working is described below. This example of press working is performed using a lower die and an upper die. The press surfaces of the lower die and the upper die are shaped to press and deform the internal frame 120 so that the above-described surface 120sc (slope) is formed. At this time, the portion that will become surface 120sa is also pressed. The surfaces of the press surfaces of the lower die and the upper die are roughened so that surface 120sa and / or surface 120sc are roughened. It is preferable that at least a part or all of surface 120sc (slope) is roughened, and at least a part or all of surface 120sa and surface 120sc may be roughened.
[0093] The arithmetic mean roughness Ra of a roughened surface is greater than the arithmetic mean roughness Ra of the unroughened surface. The arithmetic mean roughness Ra of an unroughened rolled sheet surface is generally less than 1.0 μm.
[0094] As mentioned above, a portion of the vertical rib 120A may be inclined with respect to the side element 113 (or side element 114), and a portion of the horizontal rib 120B may be inclined with respect to the upper element 111 (or lower element 112). Figure 5 schematically shows a top view of an example of a positive electrode current collector 100 in which a portion of the horizontal rib 120B is inclined with respect to the upper element 111 (or lower element 112). In the positive electrode current collector 100 of Figure 5, a portion of the horizontal rib 120B is parallel to the upper element 111 (and lower element 112), and the remaining portion of the horizontal rib 120B is inclined with respect to the upper element 111 (and lower element 112).
[0095] Figure 6 shows a cross-sectional view of an example of a positive electrode plate 3 using the positive electrode current collector 100 shown in Figure 2. Note that Figure 6 shows only the cross-section of the part corresponding to the part shown in Figure 2. As shown in Figure 6, the positive electrode plate 3 includes the positive electrode current collector 100 and the positive electrode material 150 held by the positive electrode current collector 100.
[0096] (Embodiment 2) Embodiment 2 describes an example of the lead-acid battery of this embodiment. Figure 7 shows the external appearance of the lead-acid battery 1 of Embodiment 2.
[0097] The lead-acid battery 1 includes an electrode plate group 11, an electrolyte (not shown), and a battery case 12 that houses them. The battery case 12 is divided into a number of cell chambers 14 by a partition wall 13. Each cell chamber 14 houses one electrode plate group 11. The opening of the battery case 12 is closed with a lid 15 having a negative electrode terminal 16 and a positive electrode terminal 17. The lid 15 is provided with a vent plug 18 for each cell chamber. When replenishing water, the vent plug 18 is removed and the water is supplied. The vent plug 18 may also have a function of venting gas generated in the cell chamber 14 to the outside of the battery.
[0098] Each electrode plate group 11 is constructed by stacking multiple negative electrode plates 2 and positive electrode plates 3 via separators 4. Figure 7 shows an example in which the negative electrode plates 2 are housed in bag-shaped separators 4. In the cell chamber 14 located at one end of the battery case 12, a negative electrode shelf 6, which connects multiple negative electrode plates 2 in parallel, is connected to a through-connector 8, and a positive electrode shelf 5, which connects multiple positive electrode plates 3 in parallel, is connected to a positive electrode column 7. The positive electrode column 7 is connected to a positive electrode terminal 17 on the outside of the lid 15. In the cell chamber 14 located at the other end of the battery case 12, a negative electrode column 9 is connected to the negative electrode shelf 6, and a through-connector 8 is connected to the positive electrode shelf 5. The negative electrode column 9 is connected to a negative electrode terminal 16 on the outside of the lid 15. Each through-connector 8 passes through a through-hole provided in the partition wall 13, connecting the electrode plate groups 11 of adjacent cell chambers 14 in series.
[0099] Figure 7 shows an example of a liquid-type battery (vented battery), but the lead-acid battery may also be a valve-regulated lead-acid battery (VRLA type). In liquid-type batteries, the current collector tends to elongate more significantly than in valve-regulated lead-acid batteries, and the adhesion between the positive electrode current collector and the positive electrode material tends to decrease. By using the positive electrode current collector according to this embodiment, the decrease in adhesion between the positive electrode current collector and the positive electrode material can be suppressed, so the positive electrode current collector according to this embodiment is preferably used in liquid-type batteries.
[0100] Examples of positive electrode current collectors and lead-acid batteries according to the present invention are summarized below. (1) A positive electrode current collector for a lead-acid battery, It includes a frame frame and an inner frame positioned inside the frame frame, In a cross-section of at least a portion of the internal bone, the width Y in the first direction and the width X in the second direction in a cross-section perpendicular to the extension direction of at least a portion of the internal bone satisfy the relationship 0.4 ≤ Y / X ≤ 0.8. The first direction is the thickness direction of the positive electrode current collector, and the second direction is perpendicular to the stretching direction and the thickness direction. The surface of at least a portion of the internal bone includes a roughened surface having an arithmetic mean roughness Ra of 1.0 μm or more and 50 μm or less. A positive electrode current collector for a lead-acid battery, wherein at least a portion of the internal bone has a surface that extends along the extension direction and is inclined with respect to the thickness direction.
[0101] (2) The positive electrode current collector according to (1) above, wherein when the total length of the internal bones excluding the portions where the internal bones intersect is defined as length L, the total length of at least a portion of the internal bones is 0.5L or more.
[0102] (3) A positive electrode current collector as described in (1) or (2) above, wherein the Sn content is 1.1% by mass or more.
[0103] (4) The positive electrode current collector includes a vertical frame, The positive electrode current collector according to any one of (1) to (3) above, wherein the width of the vertical frame ribs is 0.5 mm or more and 2.0 mm or less.
[0104] (5) The positive electrode current collector according to any one of (1) to (4) above, wherein the ratio S1 / S0 of the area S1 of the roughened surface to the area S0 of the surface of the inner bone is 0.3 or more.
[0105] (6) The positive electrode current collector according to any one of (1) to (5) above, wherein the roughened surface and the inclined surface are surfaces processed by press working.
[0106] (7) A lead-acid battery comprising a positive electrode plate, a negative electrode plate, and an electrolyte, A lead-acid battery wherein the positive electrode plate includes a positive electrode current collector for a lead-acid battery as described in any one of (1) to (6) above, and a positive electrode material held by the positive electrode current collector. [Examples]
[0107] The positive electrode current collector and lead-acid battery according to this embodiment will be described in detail below based on examples, but the positive electrode current collector and lead-acid battery according to this embodiment are not limited to the following examples.
[0108] (Experimental Example 1) In Experimental Example 1, multiple lead-acid batteries were fabricated and evaluated using the following procedure.
[0109] (1) Fabrication of the positive electrode current collector First, an intermediate lattice body having a rectangular frame (frame frame) and an intermediate frame positioned inside it was obtained by punching out a rolled sheet of Pb-Ca-Sn alloy. Next, a positive electrode current collector was obtained by press-forming the intermediate lattice body. The cross-sectional shape of the positive electrode current collector was the same as the cross-sectional shape shown in Figure 2. That is, the cross-sectional shape of the inner frame was approximately octagonal. The total length of the parts in which the cross-sectional shape of the inner frame was changed was set to 0.5L or more (L is the length mentioned above). At this time, multiple types of positive electrode current collectors were manufactured by changing the Sn content of the Pb-Ca-Sn alloy, the ratio of the width Y in the first direction to the width X in the second direction Y / X, and the arithmetic mean roughness Ra of the pressed surface of the inner frame to the values in Tables 1 to 5. In this example, the surfaces of the inner frame corresponding to surfaces 120sa and 120sc shown in Figure 2 were roughened.
[0110] (2) Fabrication of the positive electrode plate A positive electrode paste containing lead powder was prepared, and the paste was filled into the grid of the positive electrode current collector. The paste was then aged and dried to produce an unformed positive electrode plate. At this time, the density of the positive electrode material after full charge was 3.6 g / cm³. 3The amount of positive electrode paste filled was adjusted to achieve this result. In this way, multiple types of positive electrode current collectors manufactured in (1) above were used for the positive electrode current collector. In this way, multiple types of positive electrode plates with different positive electrode current collectors were manufactured.
[0111] (3) Fabrication of the negative electrode plate A negative electrode paste was prepared by mixing lead powder, water, dilute sulfuric acid, barium sulfate, carbon black, and an organic shrinkage inhibitor (sodium ligninsulfonate). The negative electrode paste was filled into an expanded grid made of a Pb-Ca-Sn alloy to serve as the negative electrode current collector, and then aged and dried to obtain an unformed negative electrode plate. The density of the negative electrode material after full charge was 3.7 g / cm³. 3 The amount of negative electrode paste filled was adjusted to achieve this result.
[0112] (4) Preparation and evaluation of test batteries The test battery had a voltage of 2V / cell and a 5-hour rate rated capacity of 30Ah. The test battery consisted of six positive electrode plates and seven negative electrode plates sandwiching them. The unformed negative electrode plates were housed in a bag-shaped separator and stacked with the unformed positive electrode plates to form an electrode plate group. The electrode plate group was housed in a polypropylene battery case along with an electrolyte, and the plates were formed inside the case to create a liquid lead-acid battery. As the electrolyte, an aqueous sulfuric acid solution with a specific gravity of 1.28 at 20°C was used. Multiple types of positive electrode plates prepared in (2) above were used. In this way, multiple types of batteries with different positive electrode current collectors were prepared. The following evaluations were performed on the prepared batteries.
[0113] [Evaluation 1: Test of 5-hour rate rated capacity during charge-discharge cycles] The evaluation 1 test was performed on the fabricated batteries in a 25°C water bath as follows: First, the batteries were discharged to 1.75V / cell with a constant current (0.2 times the value indicated for the 5-hour rate rated capacity), and then charged to 135% of the discharged amount with a constant current (0.2 times the value indicated for the 5-hour rate rated capacity). The same cycle was repeated five times. The ratio of the 5-hour rate discharge capacity after the fifth cycle to the initial capacity (5-hour rate discharge capacity) (capacity retention rate) was then calculated.
[0114] Some of the manufacturing conditions for the positive electrode current collector and the evaluation results are shown in Tables 1 to 5. Batteries A1 to A21 are lead-acid batteries (examples) according to this embodiment, and batteries C1 to C24 are comparative examples. The capacity retention rate is expressed as a relative value with the capacity retention rate of battery A10 set to 100%. The amount of charged electricity is the amount of charged electricity obtained in Evaluation 2, and is expressed as a relative value with the amount of charged electricity of battery A10 set to 100%. A higher capacity retention rate indicates less battery degradation due to charging and discharging.
[0115] [Table 1]
[0116] [Table 2]
[0117] [Table 3]
[0118] [Table 4]
[0119] [Table 5]
[0120] Some of the results are shown in Figure 8. As shown in Tables 1 to 5 and Figure 8, the volume retention rate was high when the relationship 0.4 ≤ Y / X ≤ 0.8 was satisfied and the arithmetic mean roughness Ra was between 1.0 μm and 50 μm.
[0121] (Experimental Example 2) Except for changing the manufacturing conditions of the positive electrode current collector, several types of positive electrode current collectors were manufactured using the same method as in Experimental Example 1. The Sn content and the ratio Y / X value in the alloy constituting the positive electrode current collector were changed. In Experimental Example 2, the positive electrode current collectors were manufactured so that the arithmetic mean roughness Ra of the roughened surface was approximately 5 μm. Except for using the manufactured positive electrode current collectors, several lead-acid batteries were manufactured using the same method as in Experimental Example 1. Evaluation 1 above was performed on the manufactured lead-acid batteries in the same manner as in Experimental Example 1, and further evaluation 2 below was performed.
[0122] [Evaluation 2: Amount of electricity charged by constant voltage charging after over-discharge] The following processes (a) to (e) were performed sequentially on a fully charged battery. (a) At room temperature (approximately 25°C), the battery was discharged for 3.5 hours at a current of 1.5A (20-hour rate current). (b) The battery was charged for 24 hours at a constant voltage of 16V (maximum current: 15A) at room temperature (approximately 25°C). (c) A 90Ω resistor was connected to the battery and left for 15 days at room temperature (approximately 25°C). (d) At room temperature (approximately 25°C), a 0.25Ω resistor was connected to the battery and left for 10 days. (e) The battery was charged for 0.5 hours at a constant voltage of 16V (maximum current: 25A) at room temperature (approximately 25°C). The amount of electricity charged by this charge was then calculated.
[0123] Some of the manufacturing conditions for the positive electrode current collector and the evaluation results are shown in Table 6. Note that some of the batteries shown in Table 6 are the same as the batteries shown in Tables 1 to 5, and the results shown in Tables 1 to 5 may be shown in Table 6. Batteries A22 to A36 are lead-acid batteries (examples) according to this embodiment, and batteries C25 to C34 are comparative example batteries. In Table 6, the capacity retention rate is expressed as a relative value with the capacity retention rate of battery A29 set to 100%. In Table 6, the amount of charged electricity (amount of charged electricity in Evaluation 2) is expressed as a relative value with the amount of charged electricity of battery A29 set to 100%. A higher amount of charged electricity (%) indicates higher charge acceptance performance. In the tables below, "-" indicates that it was not measured.
[0124] [Table 6]
[0125] Figure 9 shows the relationship between the Sn content in the alloy and the amount of charged electricity. As shown in Table 6 and Figure 9, increasing the Sn content in the alloy improves the charge acceptance performance, but tends to decrease the capacity retention rate. However, when the ratio Y / X is in the range of 0.4 to 0.8, the decrease in capacity retention rate associated with an increase in Sn content can be suppressed.
[0126] As shown in Figure 9, when the ratio Y / X value is not in the range of 0.4 to 0.8, the charge acceptance is particularly reduced when the Sn content is 1.5 mass% or less. In contrast, when the ratio Y / X value is in the range of 0.4 to 0.8, the reduction in charge acceptance can be minimized even when the Sn content is 1.5 mass% or less.
[0127] (Experimental Example 3) In Experimental Example 3, several types of positive electrode current collectors were fabricated using the same method as in Experimental Example 1. However, the arithmetic mean roughness Ra of the pressed surface of the inner frame and the width Wf of the vertical frame (side elements) were varied as shown in Table 7. The shape of the inner frame of the positive electrode current collector was the same as that of the positive electrode current collector used in Experimental Example 1. A lead-acid battery was fabricated using the fabricated positive electrode current collectors in the following manner. The amount of curvature of the positive electrode current collector after an overcharge test was evaluated for the fabricated lead-acid battery.
[0128] (1) Preparation of test battery Except for changing the positive electrode current collector, the same test batteries (batteries A37-A45 and C35-C43) as those prepared in Experimental Example 1 were assembled.
[0129] (2) Overcharge test An overcharge test was conducted using a test battery. The overcharge test consisted of three 1-week cycles, each consisting of a 5-day overcharge period followed by a 2-day rest period (no charging period). During the overcharge period, the test battery was charged in a 75°C water bath with a constant current of 0.2 C(A) at a 5-hour rate.
[0130] (3) Evaluation of the amount of curvature after the overcharge test The positive electrode current collector was removed from the test battery after the overcharge test was completed. The positive electrode current collector was then placed on a flat stand with the most protruding side of the internal frame facing downwards. At this time, the positive electrode current collector was positioned on the stand so that the distance between the four corners of the rectangular frame and the stand was approximately the same. Next, the distances between the stand and the four corners and four midpoints (midpoints of two adjacent corners) of the frame were measured. The value obtained by arithmetic mean of the eight measured distances was defined as the curvature.
[0131] Table 7 shows some of the manufacturing conditions for the positive electrode current collector and the evaluation results. Batteries A37 to A45 are lead-acid batteries (examples) according to this embodiment, and batteries C35 to C43 are comparative examples.
[0132] [Table 7]
[0133] The results from Table 7 are shown in Figure 10. As shown in Table 7 and Figure 10, the amount of curvature was significantly reduced by setting the width Wf of the vertical frame ribs to a range of 0.5 to 2.0 mm. Therefore, the degradation of battery performance can be particularly suppressed by setting the width Wf of the vertical frame ribs to a range of 0.5 to 2.0 mm.
[0134] (Experimental Example 4) In Experimental Example 4, several types of positive electrode current collectors were fabricated by varying the proportion of the inner bone surface that was roughened. Several types of lead-acid batteries were fabricated in the same manner as in Experimental Example 1, except that the fabricated positive electrode current collectors were used. The obtained lead-acid batteries were evaluated in the same manner as in Evaluation 2 of Experimental Example 2. The roughening rate is expressed by the following formula. Here, a roughened surface refers to a surface that has been roughened so that its arithmetic mean roughness Ra is between 1.0 μm and 50 μm. Roughening rate (%) = 100 × (Area of roughened surface within the endoskeleton surface) / (Area of the endoskeleton surface)
[0135] Table 8 shows the surface roughening rate and some of the evaluation results. In Table 8, the amount of charged electricity (amount of charged electricity for evaluation 2) is expressed as a relative value with the amount of charged electricity of battery C44 set to 100%. Batteries A46 to A48 are lead-acid batteries (examples) according to this embodiment, and battery C44 is a comparative example battery.
[0136] [Table 8]
[0137] In Table 8, the positive electrode current collector with a roughening rate of 0% is a positive electrode current collector that has undergone press processing but has not been roughened. The positive electrode current collectors with roughening rates of 40% and 60% are positive electrode current collectors in which a portion of the surface of the inner bone has been roughened by the press processing described above. The positive electrode current collector with a roughening rate of 100% was formed by roughening a portion of the surface of the inner bone by the press processing described above, and then further roughening the entire surface of the inner bone by the shot peening method.
[0138] As shown in Table 8, the amount of charge decreased significantly when the surface roughening rate was 100%. The reason for this is not clear, but it is thought that if the surface roughening rate is too high, the surface of the rib becomes more susceptible to corrosion, and the adhesion between the rib and the electrode material may decrease due to charging and discharging. On the other hand, by increasing the surface roughening rate, the adhesion between the rib and the positive electrode material can be improved. As a result, the capacity retention rate can be increased as described above. [Industrial applicability]
[0139] The present invention can be used in positive electrode current collectors for lead-acid batteries and in lead-acid batteries themselves. The lead-acid batteries can be applied to valve-regulated and liquid-type lead-acid batteries. The lead-acid batteries can be suitably used as starting power sources for vehicles (automobiles, motorcycles, etc.) and as power sources for industrial energy storage devices such as electric vehicles (forklifts, etc.). The lead-acid batteries are particularly suitable for liquid-type batteries and are especially suitable as starting power sources for vehicles that are prone to being exposed to overcharge conditions. [Explanation of symbols]
[0140] 1:Lead acid battery 2: Negative plate 3: Positive plate 4: Separator 12: Battery case 14: Cell Room 100: Positive electrode current collector 110: Frame 120: Internal bones D1: 1st direction D2 :Second direction LD: Stretching direction TD: Thickness direction
Claims
1. A positive electrode current collector for a lead-acid battery, It includes a frame frame and an inner frame positioned inside the frame frame, In a cross-section of at least a portion of the internal bone, the width Y in the first direction and the width X in the second direction in a cross-section perpendicular to the extension direction of at least a portion of the internal bone satisfy the relationship 0.4 ≤ Y / X ≤ 0.
8. The first direction is the thickness direction of the positive electrode current collector, and the second direction is perpendicular to the stretching direction and the thickness direction. The surface of at least a portion of the internal bone includes a roughened surface having an arithmetic mean roughness Ra of 1.0 μm or more and 50 μm or less. At least a portion of the internal bone has a surface that extends along the extension direction and is inclined with respect to the thickness direction, A positive electrode current collector in which, when the total length of the internal bones excluding the portions where the internal bones intersect is defined as length L, the total length of at least a portion of the internal bones is 0.5L or more.
2. The positive electrode current collector according to claim 1, wherein the Sn content is 1.1% by mass or more.
3. The positive electrode current collector includes a vertical frame structure. The positive electrode current collector according to claim 1, wherein the width of the vertical frame is 0.5 mm or more and 2.0 mm or less.
4. The positive electrode current collector according to claim 1, wherein the ratio S1 / S0 of the area S1 of the roughened surface to the area S0 of the inner bone surface is 0.3 or more.
5. The positive electrode current collector according to claim 4, wherein the roughened surface and the inclined surface are surfaces processed by press working.
6. A lead-acid battery comprising a positive electrode plate, a negative electrode plate, and an electrolyte, The positive electrode plate comprises a positive electrode current collector for a lead-acid battery according to any one of claims 1 to 5, and a positive electrode material held by the positive electrode current collector, in a lead-acid battery.
Citation Information
Patent Citations
Manufacture of grid for lead storage battery
JP1983019868A
Cultivation of plant and breeding of animal
JP1994007038A
Positive electrode collector foil for lead acid storage battery
JP2003242983A
Base plate for lead storage battery, and lead storage battery using the same
JP2004158433A
Method of manufacturing grid for lead acid battery
JP2015213034A