Energy storage element and negative electrode for energy storage element
The use of solid and hollow graphite particles with fibrous carbon in the negative electrode active material layer addresses the performance issues of solid graphite, enhancing charge-discharge cycle and output performance in energy storage devices.
Patent Information
- Application Number
- JP2022578256
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-01-26
- Filing Date
- 2022-01-18
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2042-01-18
AI Technical Summary
Solid graphite particles exhibit lower input/output performance compared to hollow graphite due to fewer reactive active sites and reduced discharge capacity when particle size is reduced, leading to decreased charge-discharge cycle performance in energy storage devices.
A negative electrode active material layer comprising solid graphite particles with a small median diameter, hollow graphite particles with a larger median diameter, and fibrous carbon as a conductive agent, optimizing the resistance difference and electronic conductivity for improved charge-discharge cycle and output performance.
The combination of solid and hollow graphite particles with fibrous carbon enhances current distribution and maintains excellent electronic conductivity, resulting in superior charge-discharge cycle and output performance of energy storage elements.
Smart Images

Figure 0007947990000002 
Figure 0007947990000003 
Figure 0007947990000001
Abstract
Description
Technical Field
[0001] The present invention relates to an electricity storage device and a negative electrode for an electricity storage device.
Background Art
[0002] Non-aqueous electrolyte secondary batteries, typified by lithium-ion non-aqueous electrolyte secondary batteries, are widely used in electronic devices such as personal computers and communication terminals, automobiles, and the like due to their high energy density. The non-aqueous electrolyte secondary battery generally includes an electrode body having a pair of electrodes electrically isolated by a separator, and a non-aqueous electrolyte interposed between the electrodes, and is configured to perform charging and discharging by transferring ions between the two electrodes. In addition, capacitors such as lithium ion capacitors and electric double layer capacitors are also widely used as electricity storage devices other than non-aqueous electrolyte secondary batteries.
[0003] For the purpose of increasing the energy density and improving the charge-discharge efficiency of such electricity storage devices, carbon materials including graphite are used as the negative electrode active material of the electricity storage devices (see Patent Document 1).
Prior Art Documents
Patent Documents
[0004]
Patent Document 1
Summary of the Invention
Problems to be Solved by the Invention
[0005] According to the inventors' findings, among carbon materials, solid graphite tends to have lower input / output performance compared to hollow graphite because it does not have voids within its particles. On the other hand, solid graphite has relatively few reactive active sites and excellent durability. To improve the input / output performance of solid graphite, reducing its particle size is effective, but reducing the particle size of solid graphite may reduce its discharge capacity. For this reason, the inventors have been considering using a mixture of small-particle solid graphite and hollow graphite as a negative electrode active material. However, when electrode plates using a negative electrode active material made by mixing small-particle solid graphite and hollow graphite were press-formed, instances of reduced charge-discharge cycle performance were observed.
[0006] This invention has been made in view of the above circumstances, and its main objective is to provide an energy storage element that has excellent charge-discharge cycle performance and excellent output performance. [Means for solving the problem]
[0007] A power storage element according to one aspect of the present invention comprises a negative electrode having a negative electrode substrate and a negative electrode active material layer directly or indirectly laminated on at least one surface of the negative electrode substrate, wherein the negative electrode active material layer contains solid graphite particles having a median diameter D1, hollow graphite particles having a median diameter D2 larger than that of the solid graphite particles, and a conductive agent, the conductive agent being fibrous carbon. [Effects of the Invention]
[0008] According to one aspect of the present invention, the energy storage element exhibits excellent charge-discharge cycle performance and superior output performance. [Brief explanation of the drawing]
[0009] [Figure 1] Figure 1 is a perspective view showing one embodiment of an energy storage element. [Figure 2] Figure 2 is a schematic diagram showing one embodiment of an energy storage device configured by assembling multiple energy storage elements. [Modes for carrying out the invention]
[0010] First, an overview of the energy storage element and the negative electrode for the energy storage element disclosed herein will be described.
[0011] A power storage element according to one aspect of the present invention comprises a negative electrode having a negative electrode substrate and a negative electrode active material layer directly or indirectly laminated on at least one surface of the negative electrode substrate, wherein the negative electrode active material layer contains solid graphite particles having a median diameter D1, hollow graphite particles having a median diameter D2 larger than that of the solid graphite particles, and a conductive agent, the conductive agent being fibrous carbon.
[0012] The energy storage element exhibits excellent charge-discharge cycle performance and output performance because its negative electrode active material layer contains solid graphite particles with a median diameter D1, hollow graphite particles with a larger median diameter D2 than the solid graphite particles, and fibrous carbon as a conductive agent. The reason for this is not entirely clear, but it is thought to be as follows: The negative electrode of the energy storage element contains solid graphite particles with a small median diameter and hollow graphite particles with a larger median diameter than the solid graphite particles, which reduces the resistance difference between the hollow graphite particles and the solid graphite particles. As a result, the current distribution during charging and discharging in the energy storage element becomes smaller, and the difference in degradation progression between the hollow graphite particles with a large median diameter and the solid graphite particles with a small median diameter becomes smaller. In addition, the negative electrode of the energy storage element contains fibrous carbon as a conductive agent, resulting in excellent electronic conductivity due to the bonding between solid graphite particles with a small median diameter, hollow graphite particles with a large median diameter, and the fibrous carbon. Furthermore, this excellent electronic conductivity is maintained over a long period even after charge-discharge cycles. These factors are believed to contribute to improvements in charge-discharge cycle performance and output performance.
[0013] In one preferred embodiment of the energy storage element disclosed herein, the relationship between the median diameter D1 of the solid graphite particles and the median diameter D2 of the hollow graphite particles satisfies 1 < (D2 / D1) ≤ 10. By using a combination of solid graphite particles and hollow graphite particles to achieve the above-mentioned specific median diameter ratio, an energy storage element with superior charge-discharge cycle performance and superior output performance can be obtained.
[0014] In one preferred embodiment of the energy storage element disclosed herein, the median diameter D1 of the solid graphite particles is 1 μm or more and less than 5 μm. Furthermore, the median diameter D2 of the hollow graphite particles is 5 μm or more and 20 μm or less. By having the median diameters D1 of the solid graphite particles and D2 of the hollow graphite particles within these ranges, an energy storage element with superior charge-discharge cycle performance and superior output performance can be suitably obtained.
[0015] In one preferred embodiment of the energy storage element disclosed herein, the average aspect ratio of the fibrous carbon is 50 or more and 100 or less. By using fibrous carbon with an average aspect ratio within the above range, the effects of this embodiment can be more favorably exhibited.
[0016] A negative electrode for an energy storage element according to another aspect of the present invention comprises a negative electrode substrate and a negative electrode active material layer directly or indirectly laminated on at least one surface of the negative electrode substrate, wherein the negative electrode active material layer contains solid graphite particles having a median diameter D1, hollow graphite particles having a larger median diameter D2 than the solid graphite particles, and a conductive agent, the conductive agent being fibrous carbon. By including solid graphite particles with a small median diameter and hollow graphite particles with a larger median diameter than the solid graphite particles, the resistance difference between the hollow graphite particles and the solid graphite particles is reduced. As a result, the current distribution during charging and discharging in the energy storage element becomes smaller, and the difference in degradation progression between hollow graphite particles with a large median diameter and solid graphite particles with a small median diameter becomes smaller. In addition, the negative electrode contains fibrous carbon as a conductive agent, resulting in excellent electronic conductivity due to the bonding between solid graphite particles with a small median diameter, hollow graphite particles with a large median diameter, and the fibrous carbon. Furthermore, this excellent electronic conductivity is maintained over a long period even after charge-discharge cycles. These factors are believed to contribute to improving the charge-discharge cycle performance and output performance of energy storage elements using this negative electrode.
[0017] The following describes in detail a negative electrode for an energy storage element and an energy storage element according to one embodiment of the present invention, as well as other embodiments. Note that the names of the components (each element) used in each embodiment may differ from the names of the components (each element) used in the background art.
[0018] <Negative electrode for energy storage element> A negative electrode for an energy storage element according to one embodiment of the present invention comprises a negative electrode substrate and a negative electrode active material layer disposed directly on at least one surface of the negative electrode substrate or via an intermediate layer.
[0019] (Negative electrode substrate) The negative electrode substrate is conductive. Whether or not it is conductive is determined by the volume resistivity measured in accordance with JIS-H-0505 (1975) if it is 10 7 The determination is made using Ω·cm as the threshold. The negative electrode substrate material can be metals such as copper, nickel, stainless steel, nickel-plated steel, or their alloys, or carbonaceous materials. Among these, copper or copper alloys are preferred. Examples of negative electrode substrates include foil, vapor-deposited film, mesh, and porous materials, with foil being preferred from a cost standpoint. Therefore, copper foil or copper alloy foil is preferred as the negative electrode substrate. Examples of copper foil include rolled copper foil and electrolytic copper foil.
[0020] The average thickness of the negative electrode substrate is preferably 2 μm to 35 μm, more preferably 3 μm to 30 μm, even more preferably 4 μm to 25 μm, and particularly preferably 5 μm to 20 μm. By setting the average thickness of the negative electrode substrate within the above range, it is possible to increase the strength of the negative electrode substrate while increasing the energy density per unit volume of the energy storage element.
[0021] The intermediate layer is a layer placed between the negative electrode substrate and the negative electrode active material layer. The intermediate layer contains a conductive agent such as carbon particles to reduce the contact resistance between the negative electrode substrate and the negative electrode active material layer. The composition of the intermediate layer is not particularly limited and may include, for example, a binder and a conductive agent.
[0022] (Negative electrode active material layer) The negative electrode active material layer contains solid graphite particles having a median diameter D1, hollow graphite particles having a larger median diameter D2 than the solid graphite particles, and a conductive agent. The negative electrode active material layer also contains optional components such as binders, thickeners, and fillers as needed.
[0023] In this specification, "graphite" means the average lattice plane spacing (d) of the (002) plane as measured by X-ray diffraction before charging or discharging or in the discharge state. 002 ) is a carbon material with a wavelength of less than 0.34 nm.
[0024] Here, "discharge state" refers to a state in which sufficient lithium ions that can be absorbed and released during charging and discharging are released from the carbon material, which is the negative electrode active material. For example, in a half-cell using a negative electrode containing a carbon material as the negative electrode active material as the working electrode and metallic Li as the counter electrode, this is the state in which the open-circuit voltage is 0.7V or higher.
[0025] In this specification, “solid” means that the inside of the particle is filled and there are substantially no voids. More specifically, in this specification, “solid” means that, in a cross-section of the particle observed in an SEM image obtained using a scanning electron microscope (SEM), the area ratio of the area excluding voids within the particle to the total area of the particle is 95% or more. In a preferred embodiment, the area ratio of a solid graphite particle may be 97% or more (e.g., 99% or more). “Hollow” means that, in a cross-section of the particle observed in an SEM image obtained using a SEM, the area ratio of the area excluding voids within the particle to the total area of the particle is less than 95%. In a preferred embodiment, the area ratio of a hollow graphite particle may be 92% or less (e.g., 90% or less).
[0026] The area ratio R, which is the total area of a graphite particle excluding the voids within the particle, can be determined by the following procedure. (1) Preparation of the sample for measurement The graphite particle powder to be measured is fixed with a thermosetting resin. The cross-section of the resin-fixed graphite particle is exposed using a cross-section polisher to prepare a sample for measurement. The graphite particle to be measured is prepared according to the following procedure. If graphite particles can be prepared before the assembly of the energy storage element, they are used as is. If the sample is prepared from an assembled energy storage element, the energy storage element is discharged with a constant current of 0.1C to the discharge termination voltage during normal use, and then discharged. The energy storage element in this discharged state is disassembled, the negative electrode is removed, thoroughly washed with dimethyl carbonate, and then dried under reduced pressure at room temperature, and graphite particles are collected from the negative electrode. The work from disassembling the energy storage element to preparing the graphite particle to be measured is carried out in a dry air atmosphere with a dew point of -40°C or lower. Here, "normal use" refers to using the energy storage element under the recommended or specified charge and discharge conditions, and, if a charger for the energy storage element is available, using the energy storage element with that charger. (2) Acquisition of SEM images A JSM-7001F scanning electron microscope (manufactured by JEOL Ltd.) is used to acquire SEM images. Secondary electron images will be observed. The acceleration voltage will be 15kV. The observation magnification will be set so that 3 to 15 graphite particles appear in one field of view. The obtained SEM images will be saved as image files. Other conditions such as spot diameter, working distance, irradiation current, brightness, and focus will be set appropriately so that the outlines of the graphite particles are clear. (3) Cutting out the outline of graphite particles The outlines of graphite particles are extracted from the acquired SEM image using the image cropping function of Adobe Photoshop Elements 11. This outline cropping is done by selecting the area outside the outline of the active material particles using the Quick Selection Tool and editing everything except the graphite particles into a black background. If fewer than three graphite particles have had their outlines cropped, the SEM image is acquired again and the process is repeated until three or more graphite particles have had their outlines cropped. (4) Binarization process For the image of the first graphite particle among the extracted graphite particles, the image analysis software PopImaging 6.00 is used to perform binarization, setting the threshold to a concentration 20% lower than the concentration where the intensity is maximum. By performing binarization, the area of the lower concentration side is calculated and defined as "Area S1 excluding voids within the particle". Next, the same first graphite particle image as before is subjected to binarization with a threshold of 10. By performing binarization, the outer edge of the graphite particle is determined, and the area inside that outer edge is calculated to be the "total area S0 of the particle". Using the S1 and S0 calculated above, the "area ratio R1, which is the total area of the particle excluding the voids within the particle, relative to the total area of the particle" for the first graphite particle is calculated by calculating S1(S1 / S0) relative to S0. For the images of the second and subsequent graphite particles from the cut-out graphite particles, the same binarization process described above is performed on each to calculate the areas S1 and S0. Based on these calculated areas S1 and S0, the area ratios R2, R3, ... for each graphite particle are calculated. (5) Determination of area ratio R By calculating the average value of all area ratios R1, R2, R3, ... calculated through binarization, the "area ratio R of the graphite particle, excluding the voids within the particle, relative to the total area of the particle" is determined.
[0027] (Median diameter) The median diameter D2 of the hollow graphite particles is not particularly limited, as long as it is greater than the median diameter D1 of the solid graphite particles (i.e., D2 > D1). D2 is, for example, 5 μm or more, typically 6 μm or more. D2 is preferably 7 μm or more, more preferably 7.5 μm or more. In some embodiments, D2 may be 8 μm or more, or 10 μm or more (e.g., 12 μm or more). Furthermore, from the viewpoint of improving output performance, hollow graphite particles with a D2 of 20 μm or less can be preferably used. For example, D2 is preferably 18 μm or less, more preferably 16 μm or less. In some embodiments, D2 may be 14 μm or less, or 12 μm or less (e.g., 10 μm or less). The techniques disclosed herein can preferably be implemented in which the median diameter D2 of the hollow graphite particles is 5 μm or more and 20 μm or less (more specifically 6 μm or more and 16 μm or less, and particularly 8 μm or more and 14 μm or less).
[0028] On the other hand, the median diameter D1 of the solid graphite particles is not particularly limited, as long as it is smaller than D2. From the viewpoint of improving output performance, solid graphite particles with a D1 of less than 5 μm can be preferably used. For example, D1 is preferably 4.5 μm or less, more preferably 4 μm or less. In some embodiments, D1 may be 3.6 μm or less, or 3.4 μm or less (e.g., 3.2 μm or less). Also, from the viewpoint of ease of handling during manufacturing or manufacturing cost, D1 is usually 0.5 μm or more, preferably 1 μm or more, more preferably 1.5 μm or more, and even more preferably 2 μm or more. For example, solid graphite particles with a D1 of 2.5 μm or more (e.g., 2.8 μm or more) may be used. From the viewpoint of achieving both the above output performance and ease of manufacturing, solid graphite particles with a D1 of 0.5 μm or more and less than 8 μm are preferred, solid graphite particles with a D1 of 1.5 μm or more and 5 μm or less are more preferred, and those with a D1 of 2 μm or more and 4 μm or less are particularly preferred.
[0029] From the viewpoint of better demonstrating the effects of using the above-mentioned hollow graphite particles and solid graphite particles in combination, it is preferable that the relationship between D1 and D2 satisfies 1 < (D2 / D1) ≤ 10. By using the above-mentioned hollow graphite particles and solid graphite particles in combination to achieve a specific median diameter ratio, excellent charge-discharge cycle performance and output performance can be obtained. The technology disclosed herein can be preferably implemented, for example, in a manner in which the relationship between D1 and D2 is 1.5 ≤ (D2 / D1) ≤ 8, more preferably 1.8 ≤ (D2 / D1) ≤ 6, even more preferably 2 ≤ (D2 / D1) ≤ 5.2, and particularly preferably 2.5 ≤ (D2 / D1) ≤ 4.8. In some embodiments, for example, (D2 / D1) ≤ 4 may also be the case, and typically (D2 / D1) ≤ 3.5 (for example, (D2 / D1) ≤ 3).
[0030] The value obtained by subtracting D1 from D2 (i.e., D2-D1) is preferably 2 μm or more, more preferably 4 μm or more. Furthermore, D2-D1 is preferably 18 μm or less, more preferably 15 μm or less, and even more preferably 12 μm or less. For example, D2-D1 may be 10 μm or less, or 6 μm or less.
[0031] In this specification, "median diameter" refers to the value (D50) at which the volume-based cumulative distribution calculated in accordance with JIS-Z8819-2(2001) reaches 50%. Specifically, it can be measured using the following method. The measurement is performed using a laser diffraction particle size distribution analyzer (Shimadzu Corporation's "SALD-2200") as the measuring device and Wing SALD-2200 as the measurement control software. A scattering measurement mode is adopted, and laser light is irradiated onto a wet cell through which a dispersion liquid in which the sample to be measured is dispersed in a dispersion solvent is circulated, and the scattered light distribution is obtained from the sample to be measured. The scattered light distribution is then approximated by a log-normal distribution, and the particle size corresponding to a cumulative degree of 50% is defined as the median diameter (D50). It has been confirmed that the median diameter based on the above measurement is in close agreement with the median diameter obtained by extracting 100 particles from SEM images, avoiding extremely large and extremely small particles. In this SEM image, the diameter of each particle is defined as the Ferret diameter, and the volume of each particle is calculated as a sphere with the Ferret diameter as its diameter.
[0032] (Types of graphite particles) Hollow graphite particles and solid graphite particles can be appropriately selected from various known graphite particles, each having a suitable median diameter and shape. Examples of such known graphite particles include natural graphite particles and artificial graphite particles. Here, natural graphite is a general term for graphite obtained from natural minerals, and artificial graphite is a general term for graphite manufactured artificially.
[0033] Specific examples of graphite particles that can be preferably employed as hollow graphite particles include natural graphite particles. Such natural graphite particles have high crystallinity and can effectively contribute to the improvement of the discharge capacity per volume of the negative electrode active material layer of the electricity storage device. Specific examples of the natural graphite particles include massive graphite (flaky graphite) and earthy graphite. As the solid graphite particles, natural graphite particles having a median diameter smaller than that of the hollow graphite particles may be used, or artificial graphite particles may be used. Such solid graphite particles have no voids inside, and can contribute to an increase in the bulk density of the negative electrode active material layer by being filled in the gaps between the hollow graphite particles. The hollow graphite particles and the solid graphite particles may be composite particles in which the graphite particles and particles made of another material (for example, another carbon material or a Si compound) are bonded to form a composite, or may be non-composite particles that are not composited. The hollow graphite particles and solid graphite particles disclosed herein can be preferably used in the form of non-composite particles in which the graphite particles are not bonded to particles made of another material. The hollow graphite particles and the solid graphite particles may be graphite particles having a coat (for example, an amorphous carbon coat) on the surface.
[0034] In a preferred embodiment, the hollow graphite particles and the solid graphite particles can be selected such that the R value (R1) of the hollow graphite particles is smaller than the R value (R2) of the solid graphite particles (that is, R1<R2). Here, the "R value" refers to the peak intensity (I G1 ) of the D band relative to the peak intensity (I of the G band in the Raman spectrum D1 ) (I D1 / I G1). For example, the hollow graphite particles and the solid graphite particles can be selected such that the relationship between the R value (R2) of the solid graphite particles and the R value (R1) of the hollow graphite particles satisfies 1<(R2 / R1)≦4, more preferably 1.2≦(R2 / R1)≦3, even more preferably 1.3≦(R2 / R1)≦2.5, for example 1.4≦(R2 / R1)≦2.2. In an electricity storage device provided with hollow graphite particles and solid graphite particles having such R values (R1, R2) in the negative electrode active material layer, the application effect of this embodiment can be exhibited more favorably. For example, when natural graphite particles are used as the hollow graphite particles, various types of artificial graphite particles can be preferably employed as the solid graphite particles.
[0035] The R value (R1) of the hollow graphite particles is suitably approximately less than 0.25 (for example, 0.05 or more and less than 0.25), preferably 0.23 or less (for example, 0.10 or more and 0.23 or less), more preferably 0.22 or less (for example, 0.12 or more and 0.22 or less), and even more preferably 0.21 or less. In some embodiments, R1 of the hollow graphite particles may be 0.20 or less, or may be 0.18 or less. The R value (R2) of the solid graphite particles can be approximately 0.25 or more (for example, 0.25 or more and 0.80 or less), for example 0.28 or more (for example, 0.28 or more and 0.70 or less), typically 0.30 or more (for example, 0.30 or more and 0.60 or less). In some embodiments, R2 of the solid graphite particles may be 0.50 or less, or may be 0.40 or less.
[0036] Here, the "Raman spectrum" shall be obtained by performing Raman spectroscopic measurement using "HR Revolution" manufactured by HORIBA, Ltd. under the conditions of a laser wavelength of 532 nm (YAG laser), a grating of 600 g / mm, and a measurement magnification of 100 times. Specifically, first, 200 cm -1 to 4000 cm -1 Raman spectroscopic measurement is performed in the range, and the obtained Raman spectrum data is processed at 4000 cm -1The Raman intensity at [location] is used as the base intensity, and normalized by the maximum Raman intensity within the above measurement range (e.g., the intensity of the G band). Next, the obtained normalized Raman spectrum is fitted using the Lorentz function, and 1580 cm⁻¹ is set. -1 Nearby G-band and 1350cm -1 The intensity of each nearby D band is calculated, and the peak intensity of the G band in the Raman spectrum (I G1 ) and "Peak intensity of the D band (I D1 )"
[0037] Hollow graphite particles and solid graphite particles may be spherical or non-spherical. Specific examples of non-spherical particles include spindle-shaped (e.g., elliptical, oval), flake-shaped, and plate-shaped particles. Spindle-shaped solid graphite particles are particularly preferred. Hollow graphite particles and solid graphite particles may have irregularities on their surface. Hollow graphite particles and solid graphite particles may also contain particles formed by the aggregation of multiple graphite particles.
[0038] The proportion of hollow graphite particles to the total content of hollow graphite particles and solid graphite particles is not particularly limited. The upper limit of the proportion is preferably 90% by mass, preferably 80% by mass, and more preferably 75% by mass. On the other hand, the lower limit of the proportion of hollow graphite particles is preferably 10% by mass, preferably 20% by mass, and more preferably 30% by mass (e.g., 40% by mass). The technology disclosed herein can preferably be implemented in a manner in which the proportion of hollow graphite particles to the total content of hollow graphite particles and solid graphite particles is 10% by mass or more and 80% by mass or less (more preferably 25% by mass or more and 65% by mass or less, and particularly 50% by mass or more and 70% by mass or less). By having the proportion of hollow graphite particles to the total content of hollow graphite particles and solid graphite particles within the above range, the discharge capacity per unit volume of the negative electrode active material layer can be further increased. The proportion of hollow graphite particles to the total content of hollow graphite particles and solid graphite particles can be determined, for example, from the area ratio of each graphite particle in an SEM image or from the mass change of the sample in a predetermined atmosphere (e.g., a water vapor atmosphere) using a thermogravimetric (TG) instrument.
[0039] (Other negative electrode active materials) The negative electrode active material layer disclosed herein may contain other graphite particles (hereinafter referred to as "third graphite particles") other than the hollow graphite particles and solid graphite particles described above, to the extent that the effects of the present invention are not impaired. The third graphite particles can be appropriately selected and used from among various known graphite particles. The shape of the third graphite particles is not particularly limited, but it is preferable that they be spherical or spindle-shaped with an aspect ratio of 2 to 5. When third graphite particles are included, it is appropriate that the total mass of the hollow graphite particles and solid graphite particles in the negative electrode active material layer be 70% by mass or more, preferably 80% by mass or more, and more preferably 90% by mass or more. In particular, a storage element in which 100% by mass of the graphite particles contained in the negative electrode active material layer are hollow graphite particles and solid graphite particles is preferred. By using graphite particles that are substantially composed of only these two types—hollow graphite particles and solid graphite particles—the advantages of using hollow graphite particles and solid graphite particles, respectively, can be utilized while more effectively achieving the aforementioned effects. The number of different types of graphite particles contained in the negative electrode active material layer can usually be roughly determined based on the differences in the external shapes of these multiple types of graphite particles. These differences in external shape may include, for example, differences in average particle diameter, differences in average aspect ratio, differences in particle surface shape (e.g., presence and degree of surface irregularities, presence and degree of surface coating), or differences in the density and rarefaction shape within the particles, among others. The external shape of graphite particles can be determined, for example, from SEM images.
[0040] The negative electrode active material layer disclosed herein may contain carbonaceous active materials other than the hollow graphite particles, solid graphite particles, and the third graphite particles (hereinafter referred to as "non-graphitized carbonaceous active materials"), to the extent that the effects of the present invention are not impaired. Examples of non-graphitized carbonaceous active materials include non-graphitizable carbon and easily graphitizable carbon. Here, "non-graphitizable carbon" refers to the average lattice plane spacing (d) of the (002) plane measured by X-ray diffraction before charging / discharging or in the discharge state. 002 ) refers to carbon materials with a wavelength of 0.36 nm or more and 0.42 nm or less. "Easily graphitizable carbon" refers to the above (d 002) refers to a carbon material with a diameter of 0.34 nm or more and less than 0.36 nm. When a non-graphitized carbonaceous active material is included, it is appropriate that the total mass of the hollow graphite particles and the solid graphite particles in the total mass of the carbonaceous active material contained in the negative electrode active material layer be 70% by mass or more, preferably 80% by mass or more, and more preferably 90% by mass or more. Among these, a storage element in which 100% by mass of the carbonaceous active material contained in the negative electrode active material layer is the hollow graphite particles and the solid graphite particles is preferred.
[0041] The negative electrode active material layer disclosed herein may contain negative electrode active material made of a material other than carbonaceous active material (hereinafter referred to as non-carbonaceous active material) to the extent that it does not impair the effects of the present invention. Examples of such non-carbonaceous active material include metalloids such as Si, metals such as Sn, oxides of these metals, or composites of these metals and carbon materials. The content of the above non-carbonaceous active material is appropriately, for example, 30% by mass or less of the total mass of negative electrode active material contained in the negative electrode active material layer, preferably 20% by mass or less, and more preferably 10% by mass or less. The technology disclosed herein can preferably be implemented in a manner in which the total proportion of carbonaceous active material in the total mass of negative electrode active material contained in the negative electrode active material layer is greater than 90% by mass. The proportion of carbonaceous active material is more preferably 95% by mass or more, even more preferably 98% by mass or more, and particularly preferably 99% by mass or more. Among these, energy storage elements in which 100% by mass of the negative electrode active material contained in the negative electrode active material layer is carbonaceous active material are preferred.
[0042] (Fibrous carbon) The solid graphite particles and hollow graphite particles described above are also conductive, but they contain fibrous carbon as a conductive agent. The fibrous carbon is a component that functions as a conductive agent in the negative electrode active material layer. The fibrous carbon is not particularly limited as long as it is a fibrous carbon material. Examples of fibrous carbon include carbon nanofibers, pitch-based carbon fibers, vapor-grown carbon fibers, and carbon nanotubes (CNTs), but graphene-based carbon CNTs can be suitably used. Examples of CNTs include single-wall carbon nanotubes (SWCNTs) formed by one layer of graphene, and multi-wall carbon nanotubes (MWCNTs) formed by two or more layers (e.g., 2 to 20 layers, typically 2 to 60 layers) of graphene. CNTs may also contain SWCNTs and MWCNTs in any ratio (for example, a mass ratio of SWCNTs to MWCNTs of 100:0 to 50:50, preferably 100:0 to 80:20). Those consisting substantially of only SWCNTs are particularly preferred. The structure of the graphene-based carbon is not particularly limited and may be chiral, zigzag, or armchair type. It may also contain catalyst metals used in the synthesis of CNTs (e.g., Fe, Co, and platinum group elements (Ru, Rh, Pd, Os, Ir, Pt)).
[0043] There are no particular restrictions on the aspect ratio (average length L relative to average diameter D) of the fibrous carbon, but for example, it is 20 or more. From the viewpoint of exhibiting better conductivity, the aspect ratio of the fibrous carbon is preferably 30 or more, more preferably 40 or more, even more preferably 50 or more, and particularly preferably 70 or more. There is no particular upper limit to the aspect ratio of the fibrous carbon, but from the viewpoint of handling and ease of manufacture, it is appropriate to keep it at approximately 2000 or less, preferably 1000 or less, more preferably 500 or less, even more preferably 200 or less, and particularly preferably 100 or less. For example, fibrous carbon with an average aspect ratio of 50 or more and 200 or less (even more preferably 50 or more and 100 or less, and particularly preferably 70 or more and 100 or less) is suitable.
[0044] The average diameter (fiber diameter) D of the fibrous carbon is, for example, 1 nm or more. From the viewpoint of exhibiting better conductivity, the average diameter D of the fibrous carbon is preferably 3 nm or more, more preferably 5 nm or more, even more preferably 7 nm or more, and particularly preferably 9 nm or more. There is no particular upper limit to the average diameter D of the fibrous carbon, but it is appropriate to keep it generally 100 nm or less, preferably 80 nm or less, more preferably 50 nm or less, even more preferably 30 nm or less, and particularly preferably 15 nm or less. For example, fibrous carbon with an average diameter D of 1 nm or more and 100 nm or less (for example, 5 nm or more and 80 nm or less, typically 10 nm or more and 60 nm or less) is suitable. By using fibrous carbon of the above size, the affinity between solid graphite particles and hollow graphite particles and fibrous carbon is more effectively increased. Therefore, the application effects of the technology disclosed herein can be better realized.
[0045] The average length L of the fibrous carbon is, for example, 0.5 μm or more. The average diameter L of the fibrous carbon is preferably 0.8 μm or more, more preferably 1 μm or more, even more preferably 2 μm or more, and particularly preferably 5 μm or more, from the viewpoint of exhibiting better conductivity. There is no particular upper limit to the average length L of the fibrous carbon, but it is appropriate to keep it generally 50 μm or less, preferably 30 μm or less, more preferably 20 μm or less, even more preferably 15 μm or less, and particularly preferably 10 μm or less. For example, fibrous carbon with an average length L of 1 μm or more and 20 μm or less (for example, 2 μm or more and 10 μm or less, typically 2 μm or more and 6 μm or less) is preferred.
[0046] In a preferred embodiment, the average length L of the fibrous carbon is greater than the median diameter D1 of the solid graphite particles and smaller than the median diameter D2 of the hollow graphite particles (i.e., D1 / L < 1 and D2 / L > 1). By using fibrous carbon of this size, the affinity between the fibrous carbon and the small-sized solid graphite particles and the large-sized hollow graphite particles is more effectively enhanced. Therefore, the application effects of the technology disclosed herein can be better realized.
[0047] The ratio (D1 / L) of the median diameter D1 of the solid graphite particles to the average length L of the fibrous carbon is not particularly limited, but may be less than 1 (i.e., D1 / L < 1). The ratio (D1 / L) is preferably 0.9 or less, more preferably 0.8 or less, and even more preferably 0.7 or less. The lower limit of the ratio (D1 / L) of the median diameter D1 of the solid graphite particles to the average length L of the fibrous carbon is not particularly limited, but may be, for example, 0.1 or more. The ratio (D1 / L) is preferably 0.2 or more, more preferably 0.3 or more, and even more preferably 0.4 or more.
[0048] The ratio (D2 / L) of the median diameter D2 of the hollow graphite particles to the average length L of the fibrous carbon is not particularly limited, but can be greater than 1 (i.e., D2 / L > 1). The ratio (D2 / L) is preferably 1.2 or more, more preferably 1.3 or more, and even more preferably 1.5 or more. The upper limit of the ratio (D2 / L) of the median diameter D2 of the hollow graphite particles to the average length L of the fibrous carbon is not particularly limited, but can be, for example, 5 or less. The ratio (D2 / L) is preferably 4 or less, more preferably 3.5 or less, and even more preferably 3 or less. In some embodiments, the ratio (D2 / L) may be 2.5 or less, or 2 or less.
[0049] Preferable examples of the fibrous carbon disclosed herein include those in which the aspect ratio of the fibrous carbon is 20 to 2000 and the above ratio values satisfy 0.1≦D1 / L<1 and 1<D2 / L≦5; those in which the aspect ratio of the fibrous carbon is 30 to 500 and the above ratio values satisfy 0.1≦D1 / L≦0.9 and 1.1≦D2 / L≦4; those in which the aspect ratio of the fibrous carbon is 50 to 300 and the above ratio values satisfy 0.2≦D1 / L≦0.8 and 1.2≦D2 / L≦3; and those in which the aspect ratio of the fibrous carbon is 70 to 100 and the above ratio values satisfy 0.3≦D1 / L≦0.7 and 1.5≦D2 / L≦2.5; and the like. By using the fibrous carbon having the aspect ratio and average length L within such predetermined ranges, the affinity between the small-particle-diameter solid graphite particles, the large-particle-diameter hollow graphite particles, and the fibrous carbon is more effectively enhanced. Therefore, it is possible to construct an electricity storage device that has excellent charge-discharge cycle performance and excellent output performance, which could not be obtained conventionally.
[0050] The above-mentioned average diameter and average length are defined as the average values of any 10 fibrous carbon pieces observed with an electron microscope.
[0051] The average lattice spacing (d of the (002) plane of fibrous carbon determined by X-ray diffractometry 002 ) is preferably less than 0.340 nm. When the average lattice spacing (d of the fibrous carbon 002 ) is small and the crystallinity is high in this way, the electrical conductivity is further enhanced. The lower limit of the average lattice spacing (d of this fibrous carbon 002 ) can be set to, for example, 0.330 nm. In addition, the half-value width (002) of the peak corresponding to the (002) plane of fibrous carbon by X-ray diffractometry is, for example, 0.5° or more. The half-value width (002) of the fibrous carbon is preferably less than 0.7°.
[0052] Fibrous carbon can be obtained by methods such as spinning to form fibers from a polymer and then heat-treating them in an inert atmosphere, or by vapor phase growth, in which organic compounds are reacted at high temperatures in the presence of a catalyst. Fibrous carbon obtained by vapor phase growth (vapor phase growth fibrous carbon) is preferred. Commercially available fibrous carbon can also be used.
[0053] The fibrous carbon content in the negative electrode active material layer may be, for example, 0.05% by mass or more and 20% by mass or less, but is preferably 0.1% by mass or more and 10% by mass or less, and more preferably 0.5% by mass or more and 5% by mass or less. In some cases, the fibrous carbon content in the negative electrode active material layer may be even more preferably 3% by mass or less (for example, 2% by mass or less, typically 1% by mass or less). By setting the fibrous carbon content above the lower limit, the conductivity can be further increased. On the other hand, by setting the fibrous carbon content below the upper limit, the content of solid graphite particles and hollow graphite particles can be relatively increased, thereby increasing the energy density.
[0054] The negative electrode active material layer may contain conductive agents other than fibrous carbon. Examples of other conductive agents include carbonaceous materials other than fibrous carbon, metals, conductive ceramics, etc. Examples of carbonaceous materials include ungraphitized carbon and graphene-based carbon. Examples of ungraphitized carbon include carbon black. Examples of carbon black include furnace black, acetylene black, and Ketjen black. Examples of graphene-based carbon include graphene and fullerene. However, the content of other conductive agents in the negative electrode active material layer is preferably less than 1% by mass, more preferably less than 0.1% by mass, and even more preferably substantially 0% by mass. By using substantially only fibrous carbon as the conductive agent and reducing the content of the conductive agent in this way, the energy density can be further increased.
[0055] (Any other ingredients) Examples of binders include thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, polyacrylic, and polyimide; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), and fluororubber; and polysaccharide polymers.
[0056] The binder content in the negative electrode active material layer is preferably 1% by mass or more and 10% by mass or less, and more preferably 3% by mass or more and 9% by mass or less. By keeping the binder content within the above range, the active material can be stably maintained.
[0057] Examples of thickening agents include polysaccharide polymers such as carboxymethylcellulose (CMC) and methylcellulose. If the thickening agent has a functional group that reacts with lithium or the like, this functional group may be deactivated beforehand by methylation or the like.
[0058] The filler is not particularly limited. Examples of fillers include polyolefins such as polypropylene and polyethylene, inorganic oxides such as silicon dioxide, alumina, titanium dioxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicates, hydroxides such as magnesium hydroxide, calcium hydroxide, and aluminum hydroxide, carbonates such as calcium carbonate, sparingly soluble ionic crystals such as calcium fluoride, barium fluoride, and barium sulfate, nitrides such as aluminum nitride and silicon nitride, mineral resource-derived materials such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, or artificial products thereof.
[0059] The negative electrode active material layer may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, and I, typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba, and transition metallic elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Ta, Hf, Nb, and W as components other than the negative electrode active material, conductive agent, binder, thickener, and filler.
[0060] The upper limit of Q2 / Q1, which is the ratio of the surface roughness Q2 of the region of the negative electrode substrate where the negative electrode active material layer is not laminated to the surface roughness Q1 of the region where the negative electrode active material layer is laminated in the negative electrode substrate, is preferably 0.94, and more preferably 0.92. As pressure is applied to the negative electrode substrate, the surface roughness of the region where the negative electrode active material layer is formed increases, and therefore Q2 / Q1 decreases. In other words, when no pressure is applied to the negative electrode substrate, the surface roughness of the region where the negative electrode active material layer is laminated and the region where the negative electrode active material layer is not laminated (the so-called exposed region of the negative electrode substrate) are almost the same. That is, Q2 / Q1 approaches 1. In this energy storage element, if Q2 / Q1 exceeds 0.92, the pressure applied to the negative electrode active material layer is absent or small. Therefore, the density of the negative electrode active material becomes relatively low, and the energy density of the energy storage element may decrease. On the other hand, the lower limit of the surface roughness ratio Q2 / Q1 is preferably 0.70, and more preferably 0.75. When Q2 / Q1 is above the lower limit, a negative electrode with high active material density can be obtained, and it can become an energy storage element with high lifetime characteristics.
[0061] The "surface roughness" mentioned above refers to the centerline roughness Ra of the substrate surface (or, in the case of areas where an active material layer is laminated, the surface after the active material layer has been removed), measured using a laser microscope in accordance with JIS-B0601 (2013). Specifically, the surface roughness Q2 of the portion of the negative electrode where the negative electrode substrate is exposed is measured in accordance with JIS-B0601 (2013) using a commercially available laser microscope (Keyence Corporation, model name "VK-8510"). The measurement conditions are as follows: the measurement area is 149 μm × 112 μm (16688 μm). 2Next, the negative electrode is ultrasonically cleaned to remove the negative electrode active material layer, and the surface roughness Q1 of the region where the negative electrode active material layer was laminated is measured in the same way as the surface roughness of the exposed portion of the negative electrode substrate.
[0062] The lower limit of the density of the negative electrode active material layer is 1.40 g / cm³. 3 Preferably, 1.5 g / cm³ 3 More preferably, 1.51 g / cm³ 3 This is even more preferable. In some embodiments, the density of the negative electrode active material layer is 1.53 g / cm³. 3 It may be greater than or equal to 1.55 g / cm³. 3 The density may be greater than or equal to the above range. Having the density of the negative electrode active material layer within the above range allows for a high energy density energy storage element. On the other hand, if a negative electrode pressed to the above density of the negative electrode active material layer is used, the good electronic conductivity due to the bonding of small-particle solid graphite particles, large-particle hollow graphite particles, and the conductive agent may be impaired by pressing, potentially leading to a decrease in charge-discharge cycle performance. However, according to this embodiment, by including fibrous carbon as the conductive agent, the good electronic conductivity due to the above bonding is maintained for a long period of time even after pressing and after charge-discharge cycles. The upper limit for the density of the negative electrode active material layer is 1.7 g / cm³. 3 Preferably, 1.65 g / cm³ 3 More preferably, 1.6 g / cm³ 3 This is even more preferable. Within such a range of negative electrode active material layer densities, a higher level of compatibility between high energy density and good charge-discharge cycle performance can be achieved.
[0063] <Energy storage element> An energy storage element according to one embodiment of the present invention has a positive electrode, a negative electrode, and a non-aqueous electrolyte. Hereinafter, a non-aqueous electrolyte secondary battery (hereinafter also simply referred to as a "secondary battery") will be described as an example of an energy storage element. The positive electrode and the negative electrode usually form an electrode body that is alternately superimposed by lamination or winding with a separator in between. This electrode body is housed in a container, and the non-aqueous electrolyte is filled into this container. The non-aqueous electrolyte is interposed between the positive electrode and the negative electrode. Furthermore, as the container, a known metal container, a resin container, etc., that are normally used as containers for secondary batteries can be used.
[0064] [Negative electrode] The negative electrode in the secondary battery is the negative electrode according to the embodiment of the present invention described above. Because the energy storage element is equipped with this negative electrode, a higher level of compatibility between charge / discharge cycle performance and output performance can be achieved.
[0065] [Positive electrode] The positive electrode comprises a positive electrode substrate and a positive electrode active material layer disposed directly on the positive electrode substrate or via an intermediate layer. The configuration of the intermediate layer is not particularly limited and can be selected from, for example, the configurations exemplified in the negative electrode.
[0066] The positive electrode substrate is electrically conductive. The positive electrode substrate can be made from metals such as aluminum, titanium, tantalum, or stainless steel, or alloys thereof. Among these, aluminum or aluminum alloys are preferred from the viewpoint of high potential resistance, high conductivity, and cost. Examples of positive electrode substrates include foil, vapor-deposited film, mesh, and porous materials, with foil being preferred from the viewpoint of cost. Therefore, aluminum foil or aluminum alloy foil is preferred as the positive electrode substrate. Examples of aluminum or aluminum alloys include A1085, A3003, and A1N30 as specified in JIS-H-4000 (2014) or JIS-H4160 (2006).
[0067] The average thickness of the positive electrode substrate is preferably 3 μm to 50 μm, more preferably 5 μm to 40 μm, even more preferably 8 μm to 30 μm, and particularly preferably 10 μm to 25 μm. By setting the average thickness of the positive electrode substrate within the above range, it is possible to increase the strength of the positive electrode substrate while increasing the energy density per unit volume of the secondary battery.
[0068] The positive electrode active material layer contains a positive electrode active material. The positive electrode active material layer may contain optional components such as a conductive agent, binder, thickener, and filler, as needed. The optional components such as the conductive agent, binder, thickener, and filler can be selected from the materials exemplified above for the negative electrode.
[0069] The positive electrode active material can be appropriately selected from known positive electrode active materials. For lithium-ion secondary batteries, materials capable of intercalating and releasing lithium ions are typically used as positive electrode active materials. Examples of positive electrode active materials include lithium transition metal composite oxides having an α-NaFeO2 crystal structure, lithium transition metal composite oxides having a spinel crystal structure, polyanionic compounds, chalcogen compounds, and sulfur. Examples of lithium transition metal composite oxides having an α-NaFeO2 crystal structure include Li[Li x Ni (1-x) ]O2(0≦x<0.5), Li[Li x Ni γ Co (1-x-γ) ]O2(0≦x<0.5, 0<γ<1), Li[Li x Co (1-x) ]O2(0≦x<0.5), Li[Li x Ni γ Mn (1-x-γ) ]O2(0≦x<0.5, 0<γ<1), Li[Li x Ni γ Mn β Co (1-x-γ-β) ]O2(0≦x<0.5, 0<γ, 0<β, 0.5<γ+β<1), Li[Li x Ni γ Co β Al (1-x-γ-β)Examples include ]O2 (0≦x<0.5, 0<γ, 0<β, 0.5<γ+β<1). As a lithium transition metal composite oxide having a spinel-type crystal structure, Li x Mn2O4, Li x Ni γ Mn (2-γ) Examples include O4. Examples of polyanion compounds include LiFePO4, LiMnPO4, LiNiPO4, LiCoPO4, Li3V2(PO4)3, Li2MnSiO4, Li2CoPO4F, etc. Examples of chalcogen compounds include titanium disulfide, molybdenum disulfide, molybdenum dioxide, etc. Some atoms or polyanions in these materials may be substituted with atoms or anions of other elements. The surfaces of these materials may be coated with other materials. In the positive electrode active material layer, one of these materials may be used alone, or two or more may be used in mixture form.
[0070] The positive electrode active material is usually in the form of particles (powder). The average particle size of the positive electrode active material is preferably, for example, 0.1 μm or more and 20 μm or less. Setting the average particle size of the positive electrode active material above the lower limit makes it easier to manufacture or handle the positive electrode active material. Setting the average particle size of the positive electrode active material below the upper limit improves the electronic conductivity of the positive electrode active material layer. When a composite material of the positive electrode active material and other materials is used, the average particle size of the composite material is used as the average particle size of the positive electrode active material. "Average particle size" refers to the value at which the volume-based integrated distribution calculated in accordance with JIS-Z-8819-2 (2001), based on the particle size distribution measured by laser diffraction / scattering method on a dilution of particles diluted with a solvent, in accordance with JIS-Z-8825 (2013), becomes 50%.
[0071] To obtain powder with a predetermined particle size, grinders and classifiers are used. Examples of grinding methods include using mortars, ball mills, sand mills, vibrating ball mills, planetary ball mills, jet mills, counter-jet mills, swirling airflow jet mills, or sieves. Wet grinding, which involves the coexistence of water or organic solvents such as hexane, can also be used during grinding. For classification, sieves and wind classifiers are used as needed, both dry and wet.
[0072] The content of the positive electrode active material in the positive electrode active material layer is preferably 50% to 99% by mass, more preferably 70% to 98% by mass, and even more preferably 80% to 95% by mass. By setting the content of the positive electrode active material within the above range, it is possible to achieve both high energy density and manufacturability in the positive electrode active material layer.
[0073] The conductive agent is not particularly limited as long as it is a conductive material. Examples of such conductive agents include carbonaceous materials, metals, and conductive ceramics. Examples of carbonaceous materials include graphitized carbon, non-graphitized carbon, and graphene-based carbon. Examples of non-graphitized carbon include carbon nanofibers, pitch-based carbon fibers, and carbon black. Examples of carbon black include furnace black, acetylene black, and Ketjen black. Examples of graphene-based carbon include graphene, carbon nanotubes (CNTs), and fullerenes. The conductive agent can take the form of powder or fiber. One of these materials may be used alone as the conductive agent, or two or more may be used in mixture form. These materials may also be used in composite form. For example, a composite material of carbon black and CNTs may be used. Among these, carbon black is preferred from the viewpoint of electronic conductivity and coating properties, and acetylene black is particularly preferred.
[0074] The content of the conductive agent in the positive electrode active material layer is preferably 1% by mass or more and 10% by mass or less, and more preferably 3% by mass or more and 9% by mass or less. By setting the content of the conductive agent within the above range, the energy density of the secondary battery can be increased.
[0075] Optional components such as binders, thickeners, and fillers can be selected from the materials exemplified above for the negative electrode.
[0076] The positive electrode active material layer may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, and I, typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba, and transition metal elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Nb, and W as components other than the positive electrode active material, conductive agent, binder, thickener, and filler.
[0077] [Separator] The separator can be appropriately selected from known separators. Examples of separators include separators consisting only of a substrate, and separators having a heat-resistant layer containing heat-resistant particles and a binder formed on one or both sides of the substrate. Examples of materials for the separator substrate include woven fabrics, nonwoven fabrics, and porous resin films. Among these materials, porous resin films are preferred from the viewpoint of strength, and nonwoven fabrics are preferred from the viewpoint of liquid retention of non-aqueous electrolytes. From the viewpoint of shutdown function, polyolefins such as polyethylene and polypropylene are preferred for the separator substrate material, and from the viewpoint of oxidative degradation resistance, polyimide and aramid are preferred. Composite materials of these resins may also be used as the separator substrate.
[0078] The heat-resistant particles contained in the heat-resistant layer preferably have a mass loss of 5% or less when heated from room temperature to 500°C in an air atmosphere of 1 atmosphere, and more preferably have a mass loss of 5% or less when heated from room temperature to 800°C. Inorganic compounds are examples of materials with a mass loss of less than the specified amount. Examples of inorganic compounds include oxides such as iron oxide, silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, calcium oxide, strontium oxide, barium oxide, magnesium oxide, and aluminosilicates; nitrides such as aluminum nitride and silicon nitride; carbonates such as calcium carbonate; sulfates such as barium sulfate; sparingly soluble ionic crystals such as calcium fluoride, barium fluoride, and barium titanate; covalent crystals such as silicon and diamond; mineral resource-derived materials such as talc, montmorillonite, boehmite, zeolite, apatite, kaolin, mullite, spinel, olivine, sericite, bentonite, and mica, or artificial products thereof. These inorganic compounds may be used individually or in combination, or two or more may be used as a mixture. Among these inorganic compounds, silicon dioxide, aluminum oxide, or aluminosilicates are preferred from the viewpoint of safety for energy storage elements.
[0079] The porosity of the separator is preferably 80 volume% or less from the viewpoint of strength, and preferably 20 volume% or more from the viewpoint of discharge performance. Here, "porosity" refers to a volume-based value and means the measurement value obtained using a mercury porosimeter.
[0080] A polymer gel composed of a polymer and a non-aqueous electrolyte may be used as a separator. Examples of polymers include polyacrylonitrile, polyethylene oxide, polypropylene oxide, polymethyl methacrylate, polyvinyl acetate, polyvinylpyrrolidone, and polyvinylidene fluoride. Using a polymer gel has the effect of suppressing leakage. A polymer gel may also be used in combination with a porous resin film or nonwoven fabric as described above as a separator.
[0081] (Non-aqueous electrolytes) As the non-aqueous electrolyte, it can be appropriately selected from known non-aqueous electrolytes. A non-aqueous electrolyte solution may be used as the non-aqueous electrolyte. The non-aqueous electrolyte solution contains a non-aqueous solvent and an electrolyte salt dissolved in this non-aqueous solvent.
[0082] As the non-aqueous solvent, it can be appropriately selected from known non-aqueous solvents. Examples of non-aqueous solvents include cyclic carbonates, linear carbonates, carboxylic acid esters, phosphate esters, sulfonic acid esters, ethers, amides, and nitriles. As the non-aqueous solvent, compounds in which some of the hydrogen atoms contained in these compounds are substituted with halogens may also be used.
[0083] Examples of cyclic carbonates include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylene carbonate (VC), vinylethylene carbonate (VEC), chloroethylene carbonate, fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), styrene carbonate, 1-phenylvinylene carbonate, and 1,2-diphenylvinylene carbonate. Among these, EC is preferred.
[0084] Examples of linear carbonates include diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diphenyl carbonate, trifluoroethyl methyl carbonate, and bis(trifluoroethyl) carbonate. Among these, EMC is preferred.
[0085] It is preferable to use a cyclic carbonate or a linear carbonate as the non-aqueous solvent, and it is more preferable to use a cyclic carbonate and a linear carbonate in combination. Using a cyclic carbonate can promote the dissociation of the electrolyte salt and improve the ionic conductivity of the non-aqueous electrolyte. Using a linear carbonate can keep the viscosity of the non-aqueous electrolyte low. When using a cyclic carbonate and a linear carbonate in combination, the volume ratio of the cyclic carbonate to the linear carbonate (cyclic carbonate:linear carbonate) is preferably in the range of 5:95 to 50:50.
[0086] The electrolyte salt can be appropriately selected from known electrolyte salts. Examples of electrolyte salts include lithium salts, sodium salts, potassium salts, magnesium salts, and onium salts. Among these, lithium salts are preferred.
[0087] Examples of lithium salts include inorganic lithium salts such as LiPF6, LiPO2F2, LiBF4, LiClO4, and LiN(SO2F)2; lithium oxalate salts such as lithium bis(oxalate)borate (LiBOB), lithium difluorooxalate borate (LiFOB), and lithium bis(oxalate)difluorophosphate (LiFOP); and lithium salts having halogenated hydrocarbon groups such as LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9), LiC(SO2CF3)3, and LiC(SO2C2F5)3. Among these, inorganic lithium salts are preferred, and LiPF6 is more preferred.
[0088] The electrolyte salt content in the non-aqueous electrolyte is 0.1 mol / dm³ at 20°C and 1 atm. 3 More than 2.5mol / dm 3 Preferably, it is 0.3 mol / dm³ 3 More than 2.0mol / dm 3 It is more preferable that it be less than or equal to 0.5 mol / dm 3 More than 1.7mol / dm 3 It is even more preferable that the following is the case: 0.7 mol / dm 3More than 1.5mol / dm 3 The following is particularly preferable. By setting the electrolyte salt content within the above range, the ionic conductivity of the non-aqueous electrolyte can be increased.
[0089] Non-aqueous electrolytes may contain additives in addition to the non-aqueous solvent and electrolyte salt. Examples of additives include halogenated carbonate esters such as fluoroethylene carbonate (FEC) and difluoroethylene carbonate (DFEC); oxalates such as lithium bis(oxalate) borate (LiBOB), lithium difluorooxalate borate (LiFOB), and lithium bis(oxalate) difluorophosphate (LiFOP); imide salts such as lithium bis(fluorosulfonyl)imide (LiFSI); aromatic compounds such as biphenyl, alkylbiphenyl, terphenyl, partially hydrogenated terphenyl, cyclohexylbenzene, t-butylbenzene, t-amylbenzene, diphenyl ether, and dibenzofuran; partially halogenated compounds of the above aromatic compounds such as 2-fluorobiphenyl, o-cyclohexylfluorobenzene, and p-cyclohexylfluorobenzene; halogenated anisole compounds such as 2,4-difluoroanisole, 2,5-difluoroanisole, 2,6-difluoroanisole, and 3,5-difluoroanisole; vinylene carbonate, methylvinylene carbonate, and ethyl vinylene carbonate. - Bonate, succinic anhydride, glutaric anhydride, maleic anhydride, citraconic anhydride, glutaconic anhydride, itaconic anhydride, cyclohexanedicarboxylic acid anhydride; ethylene sulfite, propylene sulfite, dimethyl sulfite, methyl methanesulfonate, busulfan, methyl toluenesulfonate, dimethyl sulfate, ethylene sulfate, sulfolane, dimethyl sulfone, diethyl sulfone, dimethyl sulfoxide, diethyl sulfoxide, tetramethylene sulfoxide, diphenyl sulfide, 4,4'-bis(2,2-dioxo-1) Examples include 3,2-dioxathiolane, 4-methylsulfonyloxymethyl-2,2-dioxo-1,3,2-dioxathiolane, thioanisole, diphenyl disulfide, dipyridinium disulfide, 1,3-propensultone, 1,3-propanesultone, 1,4-butanesultone, 1,4-butensultone, perfluorooctane, tristrimethylsilyl borate, tristrimethylsilyl phosphate, tetrakithtrimethylsilyl titanate, lithium monofluorophosphate, lithium difluorophosphate, etc. These additives may be used individually or in combination of two or more.
[0090] The additive content in the non-aqueous electrolyte is preferably 0.01% to 10% by mass relative to the total mass of the non-aqueous electrolyte, more preferably 0.1% to 7% by mass, even more preferably 0.2% to 5% by mass, and particularly preferably 0.3% to 3% by mass. By setting the additive content within the above range, it is possible to improve the capacity retention performance or cycle performance after high-temperature storage, and to further improve safety.
[0091] For the non-aqueous electrolyte, a solid electrolyte may be used, or a non-aqueous electrolyte and a solid electrolyte may be used in combination.
[0092] The solid electrolyte can be selected from any material that has ionic conductivity, such as lithium, sodium, and calcium, and is solid at room temperature (e.g., 15°C to 25°C). Examples of solid electrolytes include sulfide solid electrolytes, oxide solid electrolytes, oxynitride solid electrolytes, and polymer solid electrolytes.
[0093] Examples of sulfide solid electrolytes in lithium-ion secondary batteries include Li2S-P2S5, LiI-Li2S-P2S5, and Li 10 Ge-P2S 12 These are some examples.
[0094] <Configuration of the energy storage device> The shape of the energy storage element in this embodiment is not particularly limited, and examples include cylindrical batteries, prismatic batteries, flat batteries, coin-type batteries, button-type batteries, and the like.
[0095] Figure 1 shows an example of a rectangular battery, specifically an energy storage element 1. The figure is a transparent view of the inside of the container. An electrode body 2, having a positive electrode and a negative electrode wound around a separator, is housed in a rectangular container 3. The positive electrode is electrically connected to the positive electrode terminal 4 via a positive electrode lead 41. The negative electrode is electrically connected to the negative electrode terminal 5 via a negative electrode lead 51.
[0096] The energy storage element of this embodiment can be mounted as an energy storage unit (battery module) composed of multiple energy storage elements 1 in power supplies for vehicles such as electric vehicles (EVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs), power supplies for electronic devices such as personal computers and communication terminals, or power storage power supplies. In this case, it is sufficient that the technology of the present invention is applied to at least one of the energy storage elements included in the energy storage unit. Figure 2 shows an example of a power storage device 30 which is formed by further assembling power storage units 20, each of which is an assembly of two or more electrically connected power storage elements 1. The power storage device 30 may include busbars (not shown) that electrically connect two or more power storage elements 1, busbars (not shown) that electrically connect two or more power storage units 20, etc. The power storage unit 20 or the power storage device 30 may include a condition monitoring device (not shown) that monitors the state of one or more power storage elements 1.
[0097] <Manufacturing method for energy storage elements> The method for manufacturing the energy storage element of this embodiment can be appropriately selected from known methods. The manufacturing method includes, for example, preparing an electrode body, preparing a non-aqueous electrolyte, and housing the electrode body and the non-aqueous electrolyte in a container. Preparing the electrode body includes preparing a positive electrode and a negative electrode, and forming the electrode body by stacking or winding the positive electrode and the negative electrode via a separator. In the method for manufacturing the energy storage element of this embodiment, in the step of preparing the negative electrode, a negative electrode active material containing hollow graphite particles having a median diameter D2 and solid graphite particles having a median diameter D1 smaller than the hollow graphite particles, and fibrous carbon as a conductive agent are used.
[0098] In the process of preparing the negative electrode, a negative electrode active material layer containing hollow graphite particles and solid graphite particles is laminated along at least one surface of the negative electrode substrate by, for example, coating the negative electrode mixture paste onto the negative electrode substrate. Specifically, the negative electrode active material layer is laminated by, for example, coating the negative electrode mixture paste onto the negative electrode substrate and drying it. After drying, the negative electrode active material layer is pressed in the direction of its average thickness. In one preferred embodiment, the density of the negative electrode active material layer is 1.40 g / cm³. 3More than 1.70g / cm 3 The following (preferably 1.50 g / cm³): 3 More than 1.65g / cm 3 The negative electrode active material layer is pressed to the following conditions. The pressure (linear pressure) during this pressing is not particularly limited, but is generally preferably 10 kgf / mm or more and 100 kgf / mm or less, and more preferably 20 kgf / mm or more and 80 kgf / mm or less.
[0099] The method for housing the non-aqueous electrolyte in a container can be appropriately selected from known methods. For example, when using a non-aqueous electrolyte solution, the non-aqueous electrolyte solution can be injected through an inlet formed in the container, and then the inlet can be sealed. The energy storage element obtained in this way may have excellent battery performance. For example, the energy storage element may satisfy at least one (preferably all) of the following: excellent charge-discharge cycle performance, good output performance, and high energy density.
[0100] <Other Embodiments> Furthermore, the energy storage element of the present invention is not limited to the embodiments described above, and various modifications may be made without departing from the spirit of the present invention. For example, the configuration of one embodiment may be added to the configuration of another embodiment, and a part of the configuration of one embodiment may be replaced with the configuration of another embodiment or with well-known technology. In addition, a part of the configuration of one embodiment may be deleted. Also, well-known technology may be added to the configuration of one embodiment.
[0101] In the above embodiment, the case in which the energy storage element is used as a rechargeable non-aqueous electrolyte secondary battery (e.g., a lithium-ion secondary battery) has been described, but the type, shape, dimensions, capacity, etc. of the energy storage element are arbitrary. The present invention can also be applied to various secondary batteries, electric double-layer capacitors, or capacitors such as lithium-ion capacitors.
[0102] In the above embodiment, an electrode body in which a positive electrode and a negative electrode are stacked with a separator in between has been described, but the electrode body does not need to have a separator. For example, the positive electrode and the negative electrode may be in direct contact with each other, with a non-conductive layer formed on the active material layer of either the positive electrode or the negative electrode. [Examples]
[0103] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the following examples.
[0104] [Fabrication of the negative electrode in Example 1] A negative electrode mixture paste was prepared containing the negative electrode active material with the composition shown in Table 1 (percentage of content relative to the total content of solid and hollow graphite particles), styrene-butadiene rubber as a binder, carboxymethylcellulose as a thickener, and carbon nanotubes as a conductive agent, with water as the dispersion medium. The ratio of negative electrode active material, binder, thickener, and conductive agent was 96.8:1.0:1.2:1.0 by mass ratio of solid content. The negative electrode mixture paste was coated on both sides of a negative electrode substrate (surface roughness 0.74 μm) made of 8 μm thick copper foil, and dried to form a negative electrode active material layer. The amount of negative electrode mixture (obtained by evaporating the dispersion medium from the negative electrode mixture paste) applied per unit area on one side after drying was 0.98 g / 100 cm². 2 This was done. Then, a roll press was used to press the material to a pressure (linear pressure) of 20 kgf / mm or more. As for the carbon nanotubes, those with an aspect ratio of 83, an average length of 5 μm, and an average diameter of 60 nm were used. In this way, the negative electrode of Example 1 was obtained.
[0105] [Negative electrode preparation for Example 2, Comparative Example 10, Comparative Example 12, and Comparative Example 14] The negative electrodes for Example 2, Comparative Example 10, Comparative Example 12, and Comparative Example 14 were prepared using the same procedure as in Example 1, except that the negative electrode active material had the composition shown in Table 1.
[0106] [Negative electrode preparation for Comparative Example 1, Comparative Example 4, Comparative Example 7, Comparative Example 11, and Comparative Example 13] The negative electrodes for Comparative Examples 1, 4, 7, 11, and 13 were prepared using the same procedure as in Example 1, except that the negative electrode active material had the composition shown in Table 1 and no conductive agent was used. The ratio of the negative electrode active material, binder, and thickener in each example was 97.8:1.0:1.2 by mass ratio of solid content.
[0107] [Negative electrode preparation for Comparative Example 2, Comparative Example 5, and Comparative Example 8] The negative electrodes for Comparative Examples 2, 5, and 8 were prepared using the same procedure as in Example 1, except that the negative electrode active material had the composition shown in Table 1, and flake graphite was used as the conductive agent instead of carbon nanotubes. The ratio of the negative electrode active material, binder, thickener, and conductive agent in each example was 96.8:1.0:1.2:1.0 in terms of solid content by mass ratio.
[0108] [Negative electrode preparation for Comparative Examples 3, 6, and 9] The negative electrodes for Comparative Examples 3, 6, and 9 were prepared using the same procedure as in Example 1, except that the negative electrode active material had the composition shown in Table 1, and acetylene black was used as the conductive agent instead of carbon nanotubes. The ratio of the negative electrode active material, binder, thickener, and conductive agent in each example was 96.8:1.0:1.2:1.0 by mass ratio of solid content.
[0109] Table 1 shows the materials (negative electrode active material, conductive agent) and physical properties of the negative electrode for each example.
[0110] [Fabrication of energy storage elements] The energy storage elements of Examples 1, 2, and Comparative Examples 1 to 14 were fabricated by winding together the negative electrode shown in Table 1, the positive electrode described later, and a polyethylene separator with a thickness of 14 μm in a laminated state. The positive electrode was made of LiNi as the positive electrode active material. 0.6 Mn 0.2 Co 0.2A positive electrode mixture paste was prepared containing O2, polyvinylidene fluoride (PVDF) as a binder, and acetylene black as a conductive agent, with N-methyl-2-pyrrolidone (NMP) as the dispersion medium. The ratio of positive electrode active material, binder, and conductive agent was 94.5:4.0:1.5 by mass ratio of solid content. The positive electrode mixture paste was coated onto both sides of a positive electrode substrate made of 15 μm thick aluminum foil, pressed, and dried to form a positive electrode active material layer. The amount of positive electrode mixture (obtained by evaporating the dispersion medium from the positive electrode mixture paste) applied per unit area on one side after drying was 1.7 g / 100 cm². 2 I made it so that it would be like that. Next, 1.2 mol / dm³ of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) were mixed in a non-aqueous solvent in a volume ratio of EC:DMC:EMC = 30:35:35. 3 A non-aqueous electrolyte was obtained by dissolving LiPF6. Then, the positive electrode and the negative electrode were stacked with a separator made of polyethylene microporous membrane to fabricate an electrode body. This electrode body was placed in an aluminum rectangular battery case and positive electrode terminals and negative electrode terminals were attached. After pouring the non-aqueous electrolyte into the container (rectangular battery case), it was sealed to obtain the energy storage elements of the example and comparative example.
[0111] [evaluation] (Ratio of surface roughness of negative electrode substrate) As described above, the surface roughness Q1 of the region where the negative electrode active material layer was laminated and the surface roughness Q2 of the portion of the negative electrode where the negative electrode substrate was exposed were measured using a laser microscope. Subsequently, the ratio of the surface roughness of the negative electrode substrate (Q2 / Q1) was calculated using the measured Q1 and Q2. Here, when measuring the surface roughness Q1 of the region where the negative electrode active material layer was laminated, the negative electrode active material layer was removed by ultrasonic cleaning using a Branson 2510J-DTH tabletop ultrasonic cleaner for 3 minutes in water and 1 minute in ethanol.
[0112] (Density of the negative electrode active material layer) The density of the negative electrode active material layer is determined by the amount of negative electrode mixture applied (W(g / 100cm)). 2), the thickness of the negative electrode active material layer before charging and discharging, as described later, was denoted as T (cm), and calculated using the following formula. Density of the negative electrode active material layer (g / cm³) 3 ) = W / (T × 100)
[0113] (DCR and capacity retention rate after charge-discharge cycles) (1)Initial discharge capacity In a constant temperature bath at 25°C, constant current constant voltage (CCCV) charging was performed under conditions of a charging current of 15.0A and a charging termination voltage of 4.25V until the charging current fell to 0.5A or less, followed by a 20-minute rest period. Subsequently, constant current (CC) discharge was performed with a discharge current of 45.0A and a discharge termination voltage of 2.75V. The discharge capacity at this time was defined as the "initial discharge capacity". (2) DCR after initial discharge capacity measurement The DC resistance (DCR) of the energy storage elements after the initial discharge capacity measurement described above was evaluated. The energy storage elements, after the initial discharge capacity measurement, were charged with a constant current of 15.0A in a constant temperature bath at 25°C to an amount of charge equivalent to 50% of the state of charge (SOC) of the discharge capacity measured under the same conditions as the discharge capacity measurement method described above. After the SOC of the batteries was set to 50% under the above conditions, they were discharged for 10 seconds at current values of 45.0A, 90.0A, 135.0A, and 300.0A, respectively. The DCR value, which corresponds to the slope, was obtained from the current-voltage performance graph obtained by plotting the voltage 10 seconds after the start of discharge on the vertical axis and the discharge current value on the horizontal axis. Table 1 shows the ratio [%] of the DCR value of each test example to the DCR value of Comparative Example 1 (relative ratio [%] with Comparative Example 1). The evaluation was based on the following three levels. An evaluation of A indicates a good effect. A: The relative ratio with Comparative Example 1 is less than 107%. B: The relative ratio with Comparative Example 1 is between 107% and 109%. C: The relative ratio with Comparative Example 1 is over 109%. (3) Capacity retention rate after charge-discharge cycles For each energy storage element after measuring the "initial discharge capacity," constant current constant voltage (CCCV) charging was performed in a 45°C constant temperature bath under the conditions of a charging current of 15.0A and a charging termination voltage of 4.25V until the charging current fell to 0.5A or less, followed by a 10-minute rest period. Subsequently, constant current (CC) discharge was performed with a discharge current of 45.0A and a discharge termination voltage of 2.75V, followed by a 10-minute rest period. This charge-discharge cycle was performed 300 times. After 300 cycles, the discharge capacity was measured under the same conditions as the "initial discharge capacity" measurement test, and this discharge capacity was defined as the "discharge capacity after 300 cycles." The "discharge capacity after 300 cycles" relative to the "initial discharge capacity" was defined as the capacity retention rate after the charge-discharge cycle. The evaluation was based on the following three levels. An evaluation of A indicates a good effect. A: The capacity retention rate after charge-discharge cycles is over 89%. B: The capacity retention rate after charge-discharge cycles is 85% or more and 89% or less. C: The capacity retention rate after charge-discharge cycles is less than 85%.
[0114] Table 1 shows the evaluation results for the negative electrodes of Example 1, Example 2, and Comparative Examples 1 through 14.
[0115] [Table 1]
[0116] As shown in Table 1, Examples 1 and 2, in which the negative electrode active material layer contained solid graphite particles having a median diameter D1, hollow graphite particles having a larger median diameter D2 than the solid graphite particles, and fibrous carbon as a conductive agent, exhibited good capacity retention after charge-discharge cycles while keeping the initial resistance low.
[0117] On the other hand, when the median diameter D2 of hollow graphite particles was smaller than that of solid graphite particles, the initial resistance was higher. Also, when fibrous carbon was not included as a conductive agent, the effect of suppressing the decrease in capacity retention rate after charge-discharge cycles was poor. When neither solid graphite particles nor hollow graphite particles were included as the negative electrode active material, either or both of the effect of suppressing low resistance and the decrease in capacity retention rate after charge-discharge cycles were poor.
[0118] As described above, the energy storage element demonstrated excellent charge-discharge cycle performance and superior output performance. [Explanation of symbols]
[0119] 1. Energy storage element 2 Electrode body 3 containers 4 Positive terminal 41 Positive lead 5 Negative terminal 51 Negative lead 20 Energy storage units 30 Energy storage devices
Claims
1. The negative electrode comprises a negative electrode substrate and a negative electrode active material layer directly or indirectly laminated on at least one surface of the negative electrode substrate. The above-mentioned negative electrode active material layer contains solid graphite particles having a median diameter D1, hollow graphite particles having a median diameter D2, and a conductive material. The median diameter D1 of the above solid graphite particles is 1 μm or more and less than 5 μm. The median diameter D2 of the above hollow graphite particles is 5 μm or more and 20 μm or less. The conductive material is fibrous carbon, The average length of the above fibrous carbon is 5 μm or more and 50 μm or less. An energy storage element in which the content ratio of the hollow graphite particles to the total content of the solid graphite particles and the hollow graphite particles is 10% by mass or more and 90% by mass or less.
2. The relationship between the median diameter D1 of the solid graphite and the median diameter D2 of the hollow graphite particles is The energy storage element according to claim 1, satisfying 1 < (D2 / D1) ≤ 10.
3. The energy storage element according to claim 1 or claim 2, wherein the average aspect ratio of the fibrous carbon is 50 or more and 100 or less.
4. The device comprises a negative electrode substrate and a negative electrode active material layer directly or indirectly laminated on at least one surface of the negative electrode substrate. The above negative electrode active material layer consists of solid graphite particles having a median diameter D1, It contains hollow graphite particles having a median diameter D2 and a conductive material. The median diameter D1 of the above solid graphite particles is 1 μm or more and less than 5 μm. The median diameter D2 of the above hollow graphite particles is 5 μm or more and 20 μm or less. The conductive material is fibrous carbon, The average length of the above fibrous carbon is 5 μm or more and 50 μm or less. A negative electrode for an energy storage element, wherein the content ratio of the hollow graphite particles to the total content of the solid graphite particles and hollow graphite particles is 10% by mass or more and 90% by mass or less.
Citation Information
Patent Citations
Negative electrode active material for lithium secondary battery, negative electrode containing same for lithium secondary battery, and lithium secondary battery
EP3719883A1
Non-aqueous electrolyte secondary battery
JP2004146292A
Negative electrode active material for lithium secondary battery, process of manufacturing the same, and lithium secondary battery containing the same
JP2014232728A
Nonaqueous electrolyte and nonaqueous electrolytic secondary battery using the same
JP2018014319A
Negative electrode active material and negative electrode for secondary battery comprising the same