Electrolytic electrodes and methods for manufacturing electrolytic electrodes
The electrolytic electrode with a ruthenium and metal element (A) coating achieves low voltage electrolysis, addressing voltage maintenance issues and enabling efficient chlorine gas production.
Patent Information
- Application Number
- JP2023045039
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2043-03-22
Smart Images

Figure 0007948047000005 
Figure 0007948047000006 
Figure 0007948047000007
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to an electrode for electrolysis and a method for producing the electrode for electrolysis.
BACKGROUND ART
[0002] In the ion-exchange membrane brine electrolysis process, there is a demand for a technology capable of maintaining a low electrolysis voltage over a long period of time in order to reduce power consumption. When the breakdown of the electrolysis voltage is analyzed in detail, in addition to the theoretically required voltage, voltages caused by the resistance of the ion-exchange membrane and the structural resistance of the electrolytic cell, the overpotentials of the anode and the cathode, the voltage caused by the distance between the anode and the cathode, and the like can be cited. Furthermore, if electrolysis is continued over a long period of time, voltage rise and the like based on impurities in the brine and various other causes may also occur. Among the above-mentioned electrolysis voltages, various studies have been conducted to lower the overpotential of the anode. For example, Patent Document 1 discloses an invention of an insoluble anode in which a coating of a platinum group oxide such as ruthenium is provided on a titanium base material. This anode is called DSA (Dimension Stable Anode). In addition, Patent Documents 2 to 6 also disclose electrodes for electrolysis.
PRIOR ART DOCUMENTS
PATENT DOCUMENTS
[0003]
PATENT DOCUMENT 1
PATENT DOCUMENT 2
PATENT DOCUMENT 3
PATENT DOCUMENT 4
PATENT DOCUMENT 5
PATENT DOCUMENT 6
SUMMARY OF THE INVENTION
PROBLEMS TO BE SOLVED BY THE INVENTION
[0004] Therefore, an object of the present invention is to provide an electrolytic electrode that produces a low voltage during electrolysis. Another object of the present invention is to provide a method for manufacturing an electrolytic electrode that produces a low voltage during electrolysis. [Means for solving the problem]
[0005] The present invention relates to an electrolytic electrode comprising a conductive substrate, a first coating layer covering the conductive substrate, and a second coating layer covering the first coating layer. The above-mentioned first coating layer contains the first catalyst, The above-mentioned second coating layer contains a second catalyst comprising ruthenium and a metal element (A) capable of forming a rutile structure when an oxide is formed, and the molar ratio of the ruthenium and metal element (A) in the second catalyst is such that the interplanar spacing of the Miller index (10¹) plane in the spectrum obtained by X-ray diffraction of the second catalyst is 99.6 to 100% of the peak value.
[0006] The above metal element (A) is preferably titanium and / or tin.
[0007] The above molar ratio [ruthenium element / metal element (A)] is preferably greater than 50 / 50 and less than or equal to 90 / 10.
[0008] The electrolytic electrode described above is preferably for electrolysis of saline solution.
[0009] The electrolytic electrode described above is preferably an anode.
[0010] Furthermore, the present invention relates to a method for manufacturing an electrolytic electrode comprising a conductive substrate, a first coating layer covering the conductive substrate, and a second coating layer covering the first coating layer. The above-mentioned first coating layer contains the first catalyst, A process of mixing ruthenium and a metallic element (A) that can form a rutile structure when an oxide is formed, and then performing X-ray diffraction. a step of plotting, for each mixing molar ratio, the crystal plane spacing calculated by the Bragg equation for the Miller index (101) plane in the spectrum obtained by X-ray diffraction, a step of selecting a molar ratio at which the value is 99.6 to 100% of the peak value of the crystal plane spacing, a step of mixing the ruthenium element and the metal element (A) at the selected molar ratio to prepare a catalyst for the second coating layer, and a step of coating the surface of the first coating layer with the catalyst for the second coating layer to form the second coating layer. A method for producing an electrode for electrolysis is provided, comprising these steps.
[0011] The metal element (A) is preferably a titanium element and / or a tin element.
[0012] The electrode for electrolysis is preferably for electrolysis of saline solution.
[0013] The electrode for electrolysis is preferably an anode.
[0014] Furthermore, the present invention provides a method for producing chlorine gas, comprising electrolyzing a saline solution using the electrode for electrolysis to generate chlorine gas.
Effects of the Invention
[0015] By using the electrode for electrolysis of the present invention, electrolysis can be performed at a low voltage. Furthermore, according to the method for producing an electrode for electrolysis of the present invention, an electrode for electrolysis that allows electrolysis to be performed at a low voltage can be easily produced.
Brief Description of the Drawings
[0016] [Figure 1] It is a cross-sectional view showing one embodiment of the electrode for electrolysis of the present invention. [Figure 2] It is a graph showing the relationship between the molar ratio of the ruthenium element and the titanium element in Example 1 and the crystal plane spacing calculated by the Bragg equation for the Miller index (101) plane. [Figure 3]This is a graph showing the relationship between the molar ratio of ruthenium element and tin element in Example 2 and the crystal plane spacing calculated by the Bragg equation for the Miller index (101) plane. [Figure 4] The linear sweep voltammogram in the Examples is shown. [Mode for Carrying Out the Invention]
[0017] [Electrode for Electrolysis] The electrode for electrolysis of the present invention includes a conductive substrate, a first coating layer covering the conductive substrate, and a second coating layer covering the first coating layer. Figure 1 is a cross-sectional view showing one embodiment of the electrode for electrolysis of the present invention. The electrode 1 for electrolysis shown in Figure 1 includes a conductive substrate 2, a layer (first coating layer) 3 covering the conductive substrate 2, and a layer (second coating layer) 4 covering the first coating layer 3.
[0018] The first coating layer 3 covers the entire outer periphery of the cylindrical conductive substrate 2 and is in contact with the conductive substrate 2. The second coating layer 4 covers the entire outer periphery of the first coating layer 3 and is in contact with the first coating layer 3. Although the electrode 1 for electrolysis is composed of the conductive substrate 2, the first coating layer 3, and the second coating layer 4, it may include other layers besides these.
[0019] (Conductive Substrate) The conductive substrate is not particularly limited as long as it is composed of a material having electrical conductivity. When the electrode for electrolysis of the present invention is used for electrolysis of saline solution, the electrode for electrolysis of the present invention is used in a high-concentration saline solution near saturation in a chlorine gas generation atmosphere, so the material of the conductive substrate is preferably a corrosion-resistant valve metal. Examples of the valve metal include titanium, tantalum, niobium, zirconium and the like, and titanium is preferred from the viewpoints of economic efficiency and excellent affinity with the first coating layer.
[0020] The shape of the conductive substrate is not particularly limited, and an appropriate shape can be selected according to the purpose, and for example, an expanded shape, a perforated plate, a wire mesh and the like are preferable. In addition, the thickness of the conductive substrate is preferably 0.1 to 2 mm.
[0021] It is preferable that the conductive substrate and the first coating layer are in contact. The conductive metal surface (especially the contact surface with the first coating layer) is preferably subjected to a surface area increasing treatment from the viewpoint of excellent adhesion with the first coating layer. Examples of methods for increasing the surface area include blasting using cut wire, steel grid, alumina grid, etc., and acid treatment using sulfuric acid or hydrochloric acid. Multiple treatments may be combined to perform the surface area increasing treatment. In particular, it is preferable to combine blasting and acid treatment. It is preferable to form irregularities on the surface of the conductive substrate by blasting, and then perform acid treatment.
[0022] (first coating layer) The first coating layer contains a catalyst (first catalyst) for promoting at least one reaction of the electrolytic reaction. Examples of metal elements that the first catalyst may contain include ruthenium, titanium, iridium, tantalum, niobium, tin, cobalt, manganese, molybdenum, lanthanum, zirconium, and platinum. The first catalyst may contain the above metal elements as elemental metals or as metal compounds such as metal oxides. The first catalyst may contain only one of the above metal elements or two or more. The above metal elements preferably contain ruthenium, and more preferably contain one or more selected from the group consisting of titanium, iridium, and platinum.
[0023] The thickness of the first coating layer is preferably 0.1 to 7 μm, and more preferably 0.5 to 3 μm. A thickness of 0.1 μm or more in the first coating layer makes it easier to maintain high initial electrolytic performance. A thickness of 5 μm or less is economically advantageous.
[0024] (Second coating layer) The second coating layer contains a catalyst (second catalyst) for promoting at least one of the electrolytic reactions. The first and second catalysts have different compositions. It is preferable that the first and second coating layers are in contact. The second catalyst contains at least a ruthenium element and a metal element that can form a rutile structure when an oxide is formed. In this specification, the metal element that can form a rutile structure when an oxide is formed may be referred to as "metal element (A)". Examples of metal element (A) include titanium, tin, vanadium, manganese, cesium, germanium, silver, copper, lead, and iridium. Among these, titanium and / or tin are preferred as metal element (A). Only one metal element (A) may be used, or two or more may be used.
[0025] Examples of rutile oxides that a metal element (A) can adopt include vanadium oxide such as VO2, manganese oxide such as β-MnO2, cesium oxide such as CsO2, germanium oxide such as GeO2, silver oxide such as AgO2, copper oxide such as CuO2, lead oxide such as PbO2, and iridium oxide such as IrO2.
[0026] The second catalyst may contain ruthenium and other metallic elements besides metallic element (A). Examples of these other metallic elements include platinum. Only one of these other metallic elements may be used, or two or more may be used.
[0027] The second catalyst may contain the ruthenium element, metal element (A), and the other metal elements as elemental metals, or as metal compounds such as metal oxides. In particular, it is preferable to contain them as metal oxides.
[0028] The molar ratio of the ruthenium element to the metal element (A) in the second catalyst is the value at which the interplanar spacing calculated by the Braggs equation for the Miller index (10¹) plane in the spectrum obtained by X-ray diffraction of the second catalyst reaches 99.6-100% of its peak value. As a result, no correlation was found between the crystallite size calculated from the Sherrer equation and the Halder-Wagner method and the cell voltage, whereas a correlation was observed between the interplanar spacing calculated by the Braggs equation for the Miller index (10¹) plane and the cell voltage. When the interplanar spacing is 99.6% or higher of its peak value, the cell voltage is significantly reduced, and the amount of by-products such as oxygen is low.
[0029] The above-mentioned interplane spacing is 99.6% or more of the peak value, preferably 99.7% or more, more preferably 99.8% or more, and even more preferably 99.9% or more. In particular, when metal element (A) is titanium, it is preferably 99.7% or more, more preferably 99.8% or more, and even more preferably 99.9% or more. When metal element (A) is tin, it is preferably 99.9% or more.
[0030] The molar ratio [ruthenium element / metal element (A)] of the ruthenium element to the metal element (A) in the second catalyst described above is, for example, 20 / 80 to 90 / 10. In one embodiment, the molar ratio is preferably greater than 50 / 50 (for example, greater than 50 / 50 and 90 / 10 or less), more preferably 55 / 45 to 80 / 20, and is particularly preferred when metal element (A) is titanium. In another embodiment, the molar ratio is preferably 35 / 65 or greater (for example, 35 / 65 to 90 / 10), more preferably 35 / 65 to 80 / 10, and even more preferably 36 / 64 to 65 / 35, and is particularly preferred when metal element (A) is tin.
[0031] The total proportion of ruthenium and metal elements (A) (particularly titanium and / or tin) in the second catalyst is preferably 80 mol% or more, more preferably 90 mol% or more, even more preferably 95 mol% or more, and especially preferably 97 mol% or more, and may be 98 mol% or more, 99 mol% or more, or 99.5 mol% or more, based on the total amount of all metal elements in the second catalyst (100 mol%).
[0032] The proportion of iridium elements in the second catalyst is preferably 5 mol% or less, more preferably 1 mol% or less, even more preferably 0.1 mol% or less, and particularly preferably 0.01 mol% or less, relative to the total amount of all metal elements in the second catalyst (100 mol%). A lower proportion results in less by-product generation, such as oxygen.
[0033] The thickness of the second coating layer is preferably 0.1 to 1.0 μm, and more preferably 0.3 to 0.5 μm. A thickness of 0.1 μm or more in the second coating layer makes it easier to maintain high initial electrolytic performance. A thickness of 0.5 μm or less is economically advantageous.
[0034] The total amount of metal elements in the second catalyst in the second coating layer is preferably 5 to 100 moles, and more preferably 10 to 65 moles, relative to 100 moles of the total amount of metal elements in the first catalyst in the first coating layer.
[0035] The electrolytic electrode of the present invention has a current density value of 0.80 mA / cm² at 1.0 V vs. Ag / AgCl, as measured by linear sweep voltammetry (LSV). 2 Preferably, it is 0.90 mA / cm² or higher, and more preferably 0.90 mA / cm². 2 More preferably 0.95 mA / cm² 2 That concludes the explanation. The above current density value is 0.80 mA / cm². 2The above conditions allow for a lower voltage during electrolysis. The above LSV was measured using a three-electrode cell with a platinum mesh as the control electrode, Ag / AgCl as the reference electrode, and 200 g / L NaCl as the electrolyte, with a sweep rate of 10 mV / s, specifically measured by the method described in the examples.
[0036] The electrolytic electrode of the present invention is preferably an anode. Furthermore, the electrolytic electrode is preferably for electrolysis of an alkaline chloride aqueous solution, and particularly preferably for electrolysis of a saline solution. When the electrolytic electrode of the present invention is used as such an electrode, the voltage during electrolysis is particularly low.
[0037] The electrolytic electrode of the present invention can be manufactured by the method for manufacturing the electrolytic electrode of the present invention described later, but is not limited to such a method and can also be manufactured by known or conventional methods.
[0038] [Method for manufacturing electrolytic electrodes] The electrolytic electrode of the present invention can be manufactured by the method for manufacturing an electrolytic electrode of the present invention. The method for manufacturing an electrolytic electrode of the present invention is a method for manufacturing an electrolytic electrode comprising the conductive substrate, the first coating layer covering the conductive substrate, and the second coating layer covering the first coating layer. The manufacturing method comprises at least the steps of: mixing ruthenium and a metal element (metal element (A)) that can take on a rutile structure when an oxide is formed and performing X-ray diffraction (X-ray diffraction step); plotting the interplanar spacing of the Miller index (101) plane in the spectrum obtained by X-ray diffraction for each mixing molar ratio (interplanar spacing plotting step); selecting a molar ratio that is 99.6 to 100% of the peak value of the interplanar spacing (molar ratio selection step); mixing ruthenium and metal element (A) at the selected molar ratio to produce a catalyst for the second coating layer (catalyst production step); and coating the surface of the first coating layer with the catalyst for the second coating layer to form a second coating layer (second coating layer formation step).
[0039] (First coating layer formation step) The above manufacturing method may include a step of forming the first coating layer on the surface of a conductive substrate (first coating layer formation step). The method for forming the first coating layer can be a known or conventional method. For example, the first coating layer can be formed by applying a coating solution of a metal element or metal compound that forms the first catalyst to the surface of a conductive substrate, and then firing the resulting coating film in an oxygen-containing atmosphere. By firing the coating solution in an oxygen-containing atmosphere, the components in the coating solution are thermally decomposed, and the first coating layer, which is the catalyst layer, can be formed. Through the above thermal decomposition, the precursor metal compound, etc., is decomposed into a metal oxide or metal element and a gaseous substance by firing in an oxygen-containing atmosphere. Fired in an oxidizing atmosphere is conducive to the formation of metal oxides.
[0040] The above metal compounds are not particularly limited, but examples include metal salts such as chloride salts, nitrates, sulfates, and metal alkoxides. The solvent used in the coating solution can be selected according to the type of elemental metal or metal compound, and can be water, alcohols such as butanol, etc. The metal concentration in the coating solution is not particularly limited, but from the viewpoint of appropriately controlling the thickness of the first coating layer, 10 to 150 g / L is preferred.
[0041] Methods for applying the coating solution to the surface of a conductive substrate include a dipping method in which the conductive substrate is immersed in the coating solution, a method of applying the coating solution to the surface of the conductive substrate with a brush, a roll method in which the conductive substrate is passed through a sponge-like roll impregnated with the coating solution, and an electrostatic coating method in which the conductive substrate and the coating solution are charged to opposite charges and sprayed. Among these, the roll method and the electrostatic coating method are preferred from the viewpoint of superior industrial productivity.
[0042] It is preferable to dry the above coating film. This allows the coating film to be formed more firmly on the surface of the conductive substrate. The drying conditions can be appropriately selected depending on the composition of the coating liquid and the type of solvent, and it is preferable to dry it at a temperature of 10 to 90°C for 1 to 20 minutes, for example.
[0043] The firing temperature when firing the above coating film in an oxygen-containing atmosphere can be appropriately selected depending on the composition of the coating solution and the type of solvent, but 300 to 650°C is preferred. A longer firing time is preferable, but from the viewpoint of electrode productivity, a thermal decomposition time of 5 to 60 minutes per cycle is preferred. If necessary, the coating, drying, and firing cycle of the above coating solution can be repeated to increase the thickness of the first coating layer. Furthermore, after the formation of the first coating layer, firing for a longer period of time can be performed as needed to improve the stabilization of the first coating layer.
[0044] (X-ray diffraction process) In the above X-ray diffraction process, ruthenium and metal element (A) are mixed and X-ray diffraction is performed. In the above X-ray diffraction process, X-ray diffraction analysis is performed on multiple mixtures with different mixing ratios of ruthenium and metal element (A). The number of types of mixtures to be subjected to X-ray diffraction is three or more, preferably four or more, in order to obtain a peak for interplane spacing, and if a peak value is not obtained, the process is continued until one is obtained. The mixing ratio (molar ratio) of ruthenium and metal element (A) in the above mixture [ruthenium:metal element (A)] is preferably selected from the range of 1:9 to 9:1, such that the total is an integer ratio of 10, and more preferably includes 3:7, 4:6, and 6:4. The above mixture may be calcined before performing X-ray diffraction. The calcination temperature is, for example, 300 to 600°C.
[0045] The ruthenium element and metal element (A) to be mixed may be the elemental metals themselves or metal compounds such as oxides. It is preferable to mix the elemental metals and metal compounds in powder form.
[0046] (Plotting of interplanar spacing) In the above crystal plane spacing plotting step, the crystal plane spacing calculated by the Braggs equation for the Miller index (10¹) plane in the spectrum obtained by X-ray diffraction is plotted for each mixed molar ratio. That is, first, a graph is created by X-ray analysis with the x-axis representing the proportion (mol%) of ruthenium or metallic element (A) and the y-axis representing the crystal plane spacing calculated by the Braggs equation for the Miller index (10¹) plane.
[0047] (Molar ratio selection process) In the molar ratio selection step described above, the peak value of the interplane spacing is determined from the graph created in the interplane spacing plotting step described above, and the molar ratio of ruthenium and metal element (A) is selected to be 99.6 to 100% of the peak value of the interplane spacing. If the mixing ratio is selected from the range of 1:9 to 9:1, where the sum is an integer ratio of 10, the peak value may be selected from these mixing ratios. The ratio to the peak value is preferably as described above.
[0048] (Catalyst preparation process) In the catalyst preparation process described above, a catalyst for the second coating layer is prepared by mixing ruthenium and metal element (A) in the molar ratio selected in the molar ratio selection process described above. The ruthenium and metal element (A) may be either elemental metals or metal compounds. Examples of ruthenium compounds and metal element (A) compounds are those described and explained above as metal compounds that may be included in the second coating layer. After mixing, treatments such as calcination may be performed.
[0049] (Second coating layer formation step) In the second coating layer formation step described above, the catalyst for the second coating layer is applied to the surface of the first coating layer to form the second coating layer. The method for forming the second coating layer can be a known or conventional method. For example, a coating film can be formed by applying a coating solution containing the catalyst for the second coating layer to the surface of the first coating layer, and then firing the resulting film in an oxygen-containing atmosphere to produce the second catalyst and form the second coating layer. By firing the coating solution in an oxygen-containing atmosphere, the components in the coating solution are thermally decomposed, and the second coating layer, which is the catalyst layer, can be formed. Through this thermal decomposition, precursor metal compounds, etc., are decomposed into metal oxides or elemental metals and gaseous substances by firing in an oxygen-containing atmosphere. Fired in an oxidizing atmosphere is conducive to the formation of metal oxides.
[0050] The solvent used in the above coating solution can be selected according to the type of elemental metal or metal compound, and can be water, alcohols such as butanol, etc. The metal concentration in the above coating solution is not particularly limited, but from the viewpoint of appropriately controlling the thickness of the second coating layer, 10 to 150 g / L is preferred.
[0051] Methods for applying the coating liquid to the surface of the first coating layer include a dipping method in which the conductive substrate on which the first coating layer is formed is immersed in the coating liquid, a method of applying the coating liquid to the surface of the first coating layer with a brush, a roll method in which the conductive substrate on which the first coating layer is formed is passed through a sponge-like roll impregnated with the coating liquid, and an electrostatic coating method in which the surface of the first coating layer of the conductive substrate and the coating liquid are charged to opposite charges and sprayed. Among these, the roll method and the electrostatic coating method are preferred from the viewpoint of being superior in industrial productivity.
[0052] It is preferable to dry the above coating film. This allows the coating film to be formed more firmly on the surface of the first coating layer. The drying conditions can be appropriately selected depending on the composition of the coating liquid and the type of solvent, and it is preferable to dry it at a temperature of 10 to 200°C for 1 to 20 minutes, for example.
[0053] The firing temperature when firing the above coating film in an oxygen-containing atmosphere can be appropriately selected depending on the composition of the coating solution and the type of solvent, but is preferably 300 to 650°C, and more preferably 350 to 500°C. A longer firing time is preferable, but from the viewpoint of electrode productivity, a thermal decomposition time of 5 to 60 minutes per cycle is preferable. It is preferable that the firing temperature of the second coating layer be lower than the firing temperature of the first coating layer. By lowering the firing temperature of the second coating layer, a lower overpotential can be achieved from the initial stage of electrolysis.
[0054] Furthermore, if necessary, the coating, drying, and firing cycle of the above coating solution can be repeated to increase the thickness of the second coating layer. In addition, after the second coating layer is formed, if necessary, it can be fired for a longer period to improve the stability of the second coating layer.
[0055] When electrolysis is performed using the electrolytic electrode of the present invention, electrolysis can be carried out at a low voltage. Furthermore, the method for manufacturing the electrolytic electrode of the present invention makes it possible to easily manufacture an electrolytic electrode that can be used for electrolysis at a low voltage. For this reason, the electrolytic electrode of the present invention can be used for various electrolysis applications. In particular, it is preferable to use it as an anode for chlorine gas generation, and more preferably as an anode for sodium chloride electrolysis (specifically, an anode for sodium chloride electrolysis using the ion exchange membrane method). By using the electrolytic electrode of the present invention as an anode for sodium chloride electrolysis, sodium hydroxide and chlorine gas can be produced by electrolyzing saline solution.
[0056] [Electrolytic cell] An electrolytic cell can be provided using the electrolytic electrode of the present invention. The electrolytic cell comprises at least an anode, a cathode, and a cation exchange membrane disposed between the anode and the cathode. It is preferable to use the electrolytic electrode of the present invention as the anode. The electrolytic cell can be used for various electrolysis processes, and a typical example will be described below in the case of use in the electrolysis of an alkaline chloride aqueous solution.
[0057] The above electrolysis is not particularly limited and can be carried out under known or conventional conditions. For example, a 2.5 to 5.5 N alkali chloride aqueous solution is supplied to the anode chamber, and water or a diluted alkali hydroxide aqueous solution is supplied to the cathode chamber. The electrolysis temperature is 50 to 120°C and the current density is 5 to 100 A / dm². 2 Electrolysis can be performed under these conditions.
[0058] The configuration of the electrolytic cell described above is not particularly limited, and may be unipolar or bipolar, for example. The materials used to make up the electrolytic cell are not particularly limited, but for example, titanium, which is resistant to alkali chloride and chlorine, is preferred as the material for the anode chamber. Nickel, which is resistant to alkali hydroxide and hydrogen, is preferred as the material for the cathode chamber. The electrodes may be arranged with an appropriate gap between the cation exchange membrane and the anode, but it can also be used without problems even if the anode and the cation exchange membrane are in contact. In addition, although the cathode is generally arranged with an appropriate gap between it and the cation exchange membrane, a contact-type electrolytic cell (zero-gap electrolytic cell) without this gap can also be used without problems.
[0059] As the cathode, known materials can be used, such as a cathode made by coating a nickel substrate with nickel, nickel oxide, a nickel-tin alloy, activated carbon and oxide, ruthenium oxide, platinum, etc. [Examples]
[0060] An embodiment of this disclosure will be described in more detail below based on examples.
[0061] Example 1 (X-ray diffraction measurement) Four catalyst mixtures were prepared by mixing ruthenium oxide and titanium oxide powders in molar ratios [ruthenium:titanium] of 30:70, 40:60, 60:40, and 70:30, respectively, and firing them at 450°C for 20 minutes. X-ray diffraction measurements were performed on each catalyst mixture to obtain XRD spectra, and the interplanar spacing of the Miller index (10¹) planes was calculated using Braggs' equation with analysis software. The x-axis represented the percentage of ruthenium (mol%), and the y-axis represented the interplanar spacing (Å). The resulting graph is shown in Figure 2. The conditions for the X-ray diffraction measurements and analysis software are as follows. As shown in Figure 2, the catalyst mixture with a molar ratio of 60:40 showed a peak in interplanar spacing. Table 1 shows the interplanar spacing and the percentage of the peak value for each catalyst mixture. [X-ray diffraction] Equipment: Rigaku Corporation's "Ultima IV" horizontal sample type multi-purpose X-ray diffractometer Measurement conditions X-ray source: CuKα ray Tube current: 40KV Tube voltage: 40mA Scan speed: 3° / min. [Analysis software] Qualitative analysis: PDXL Database: ICDD
[0062] [Table 1]
[0063] Example 2 (X-ray diffraction measurement) Three catalyst mixtures were prepared by mixing ruthenium oxide and tin oxide powders in molar ratios [ruthenium:tin] of 30:70, 40:60, and 60:40, respectively, and calcining them at 450°C for 10 minutes. X-ray diffraction measurements were performed on each catalyst mixture to obtain XRD spectra, and the interplanar spacing of the Miller index (10¹) planes was calculated using Braggs' equation with analysis software. The x-axis represented the percentage of ruthenium (mol%), and the y-axis represented the interplanar spacing (Å). The resulting graph is shown in Figure 3. The X-ray diffraction measurement and analysis software conditions were the same as in Example 1. As shown in Figure 3, the catalyst mixture with a molar ratio of 40:60 showed a peak in interplanar spacing. Table 2 shows the interplanar spacing and the percentage of the peak value for each catalyst mixture.
[0064] [Table 2]
[0065] Example 3 (Fabrication of electrolytic electrodes) The catalyst mixtures prepared in Examples 1 and 2 were dissolved in butanol to a concentration of 7.0% by mass to prepare a catalyst solution. The catalyst solution was applied to the surface of a first coating layer (material: Pt-IrO2-RuO2-TiO2, thickness: 5-10 μm) formed on the surface of a conductive substrate, valve metal (titanium) (thickness: 1-3 mm), dried at 120°C to form a coating film, and then fired at 400°C or 450°C to form a second coating layer (thickness: 0.5 μm) to prepare an electrolytic electrode.
[0066] <Rating> The electrolytic electrodes obtained in Example 3 were evaluated as follows.
[0067] (1) Measurement of cell voltage Using a two-chamber sodium chloride electrolytic cell incorporating ion exchange, the electrolytic electrode prepared in Example 3 was used as the anode, and a Ni mesh coated with a precious metal catalyst was used as the cathode. The ion exchange membrane was "N2030WX" (manufactured by Chemours), and the electrolyte was 200 g / L NaCl. The temperature was 80°C and the current density was 4 kA / m². 2 Electrolysis was performed under the specified conditions, and the cell voltage was measured. The results are shown in Table 3. The cell voltage was measured by using a tester to measure the lead wires welded to the positive and negative electrodes.
[0068] [Table 3]
[0069] As shown in Tables 1-3, electrodes using mixed catalysts with high peaks in interplane spacing resulted in lower cell voltages.
[0070] (2) LSV (Linear Sweep Voltammetry) A three-electrode cell was used, with a platinum mesh as the control electrode and Ag / AgCl as the reference electrode. The electrolytic electrode obtained in Example 3 was used as the working electrode. 200 g / L NaCl was used as the electrolyte. The sweep rate was set to 10 mV / s. Figure 4 shows the linear sweep voltammogram, and Table 4 shows the current density values at 1.0 V vs. Ag / AgCl.
[0071] [Table 4]
[0072] As shown in Table 4 and Figure 4, electrodes using mixed catalysts with a high peak in interplane spacing exhibited high current values, suggesting that electrolysis was possible at low voltages.
[0073] The following describes variations of the invention relating to this disclosure. [Note 1] An electrolytic electrode comprising a conductive substrate, a first coating layer covering the conductive substrate, and a second coating layer covering the first coating layer, The first coating layer includes the first catalyst, The second coating layer contains a second catalyst comprising ruthenium and a metal element (A) capable of forming a rutile structure when an oxide is formed, wherein the molar ratio of ruthenium to metal element (A) in the second catalyst is such that the interplanar spacing of the Miller index (10¹) plane in the spectrum obtained by X-ray diffraction of the second catalyst is 99.6-100% of the peak value, for use as an electrolytic electrode. [Note 2] The electrolytic electrode described in Note 1, wherein the metal element (A) is titanium and / or tin. [Note 3] The electrolytic electrode described in Note 1 or 2, wherein the molar ratio [ruthenium element / metal element (A)] is greater than 50 / 50 and 90 / 10 or less. [Note 4] An electrolytic electrode described in any one of Notes 1 to 3, for use in the electrolysis of saline solution. [Note 5] An electrolytic electrode that is the anode, as described in any one of Notes 1 to 4. [Note 6] A method for manufacturing an electrolytic electrode comprising a conductive substrate, a first coating layer covering the conductive substrate, and a second coating layer covering the first coating layer, The first coating layer includes the first catalyst, A process of mixing ruthenium and a metallic element (A) that can form a rutile structure when an oxide is formed, and then performing X-ray diffraction. A step of plotting the interplanar spacing of the Miller index (10¹) plane in the spectrum obtained by X-ray diffraction, calculated by the Braggs equation, for each molar ratio of the mixture. A step of selecting a molar ratio of a value that is 99.6 to 100% of the peak value of the interplanar spacing. A step of preparing a catalyst for a second coating layer by mixing ruthenium element and the metal element (A) in the selected molar ratio, and A method for manufacturing an electrolytic electrode, comprising the step of coating the surface of the first coating layer with the catalyst for the second coating layer to form a second coating layer. [Note 7] The method for manufacturing an electrolytic electrode according to Note 6, wherein the metal element (A) is titanium and / or tin. [Note 8] The method for manufacturing an electrolytic electrode according to Note 6 or 7, wherein the electrolytic electrode is for electrolysis of saline solution. [Note 9] The method for manufacturing an electrolytic electrode according to any one of Notes 6 to 8, wherein the electrolytic electrode is an anode. [Note 10] A method for producing chlorine gas, comprising electrolyzing saline solution using an electrolytic electrode described in any one of Notes 1 to 5 to generate chlorine gas. [Explanation of Symbols]
[0074] 1 Electrode for electrolysis 2 Conductive base material 3 First coating layer 4 Second coating layer
Claims
1. An electrolytic electrode comprising a conductive substrate, a first coating layer covering the conductive substrate, and a second coating layer covering the first coating layer, The first coating layer includes the first catalyst, The second coating layer contains a second catalyst comprising ruthenium and a metal element (A) that can adopt a rutile structure when an oxide is formed. The molar ratio of the ruthenium element to the metal element (A) in the second catalyst is such that the interplanar spacing of the Miller index (101) plane in the spectrum obtained by X-ray diffraction of the second catalyst is 99.6 to 100% of the peak value, calculated by the Braggs equation. The aforementioned metallic element (A) is at least one element selected from the group consisting of titanium, tin, vanadium, manganese, cesium, germanium, silver, copper, lead, and iridium. An electrolytic electrode used as an anode for generating chlorine gas.
2. The electrolytic electrode according to claim 1, wherein the metal element (A) is titanium and / or tin.
3. The electrolytic electrode according to claim 1, wherein the molar ratio [ruthenium element / metal element (A)] is greater than 50 / 50 and less than or equal to 90 / 10.
4. An electrolytic electrode according to any one of claims 1 to 3, for use in the electrolysis of saline solution.
5. The device comprises a conductive substrate, a first coating layer covering the conductive substrate, and a second coating layer covering the first coating layer. This is a method for manufacturing an electrolytic electrode used as an anode for generating chlorine gas. The first coating layer includes the first catalyst, A process of mixing ruthenium and a metallic element (A) that can form a rutile structure when an oxide is formed, and then performing X-ray diffraction. A step of plotting the interplanar spacing of the Miller index (10¹) plane in the spectrum obtained by X-ray diffraction, calculated by the Braggs equation, for each mixed molar ratio. A step of selecting a molar ratio that is 99.6 to 100% of the peak value of the interplanar spacing. A step of preparing a catalyst for a second coating layer by mixing ruthenium element and the metal element (A) in the selected molar ratio, and The process includes a step of forming a second coating layer by coating the surface of the first coating layer with the catalyst for the second coating layer, A method for manufacturing an electrolytic electrode, wherein the metal element (A) is at least one element selected from the group consisting of titanium, tin, vanadium, manganese, cesium, germanium, silver, copper, lead, and iridium.
6. The method for manufacturing an electrolytic electrode according to claim 5, wherein the metal element (A) is titanium and / or tin.
7. The method for manufacturing an electrolytic electrode according to claim 5 or 6, wherein the electrolytic electrode is for electrolysis of saline solution.
8. A method for producing chlorine gas, comprising electrolyzing saline solution using the electrolytic electrode described in claim 4 to generate chlorine gas.
Citation Information
Patent Citations
Nanocrystal metal oxide composite electrode and method for preparing same
CN101532147A
Electrolysis electrodes, their preparation methods, and electrolytic cells
CN104562078B
JP1971021884Y1
Anode for electrolysis
JP1987243790A
Insoluble electrode and electrochemical liquid treatment apparatus
JP2009142733A