Electrode manufacturing method
A three-step drying process with controlled dew points and pressures in consecutive furnaces addresses electrode strain issues, improving energy efficiency and productivity in electrode manufacturing.
Patent Information
- Application Number
- JP2023148874
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-09-14
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2043-09-14
AI Technical Summary
Conventional electrode manufacturing methods involve temperature fluctuations that cause electrode strain due to linear expansion differences, leading to poor energy efficiency and reduced productivity.
A method involving a three-step drying process with controlled dew points and pressures in consecutive furnaces, eliminating the need for intermediate cooling and directly connecting coating and baking steps, enhancing energy efficiency and productivity.
Improves productivity by eliminating intermediate cooling steps and maintaining consistent temperature, thus enhancing energy efficiency in electrode manufacturing.
Smart Images

Figure 0007948114000001
Abstract
Description
[Technical Field]
[0001] This disclosure relates to a method for manufacturing electrodes. [Background technology]
[0002] Various techniques have been proposed regarding the manufacturing method of electrodes, such as the one disclosed in Patent Document 1. [Prior art documents] [Patent Documents]
[0003] [Patent Document 1] Japanese Patent Publication No. 2020-145034 [Overview of the Initiative] [Problems that the invention aims to solve]
[0004] Conventional technology involves coating and drying, pressing, and baking (absolute drying) in order to suppress electrode springback, where residual stress during press working is released over time, increasing the electrode thickness. However, if the workpiece temperature is high after the coating and drying process, electrode strain occurs due to the difference in linear expansion between the electrode composite and the current collector. Therefore, it is necessary to lower the temperature once before pressing. Therefore, even though the temperature is raised during the coating and drying process, it is necessary to lower the temperature once and then raise it again during the baking process, resulting in poor energy efficiency (low productivity).
[0005] This disclosure is made in view of the above circumstances and primarily aims to provide a method for manufacturing electrodes that can improve productivity. [Means for solving the problem]
[0006] In a first embodiment of this disclosure, a method for manufacturing an electrode is described, A coating process in which an electrode slurry is applied to a substrate, The process includes a drying step for drying the electrode slurry, The aforementioned drying process is After the coating process, a first step is to dry the electrode slurry at a constant rate below a first dew point, After the first step, a second step is performed in which the electrode slurry is reduced-rate dried below the second dew point, The process includes a third step of drying the electrode slurry at a reduced dew point after the second step, The second dew point is lower than the first dew point. The third dew point is lower than the second dew point, providing a method for manufacturing electrodes.
[0007] In a second embodiment of this disclosure, in the first embodiment, the pressure in the first furnace in the first step is smaller than the pressure in the second furnace in the second step. The pressure in the second furnace during the second step may be less than the pressure in the third furnace during the third step.
[0008] In a third embodiment of this disclosure, in the second embodiment, the temperature in the third furnace in the third step may be 65°C or higher.
[0009] In a fourth embodiment of this disclosure, in the second embodiment, the volume of the first furnace may be greater than the volumes of the second and third furnaces.
[0010] In a fifth embodiment of this disclosure, in the first embodiment, the third dew point may be -20°C or lower. [Effects of the Invention]
[0011] The electrode manufacturing method of this disclosure can improve productivity. [Brief explanation of the drawing]
[0012] [Figure 1] This is a schematic diagram illustrating an example of the drying process in this disclosure. [Modes for carrying out the invention]
[0013] Hereinafter, embodiments according to the present disclosure will be described. Matters other than those specifically mentioned in the present specification that are necessary for implementing the present disclosure (for example, general configurations and manufacturing processes of electrodes that do not characterize the present disclosure) can be grasped as design matters of a person skilled in the art based on conventional techniques in the relevant field. The present disclosure can be implemented based on the content disclosed in the present specification and common general technical knowledge in the relevant field. In addition, the dimensional relationships (length, width, thickness, etc.) in the drawings do not reflect actual dimensional relationships.
[0014] The present disclosure provides a method for manufacturing an electrode, comprising: a coating step of coating an electrode slurry on a substrate; and a drying step of drying the electrode slurry, wherein the drying step includes: a first step of subjecting the electrode slurry to constant-rate drying under a first dew point after the coating step; a second step of subjecting the electrode slurry to falling-rate drying under a second dew point after the first step; and a third step of subjecting the electrode slurry to falling-rate drying under a third dew point after the second step, wherein the second dew point is lower than the first dew point, and the third dew point is lower than the second dew point.
[0015] Conventionally, in the coating and drying step, the temperature was raised to about 100°C, then cooled to room temperature in the subsequent pressing step to suppress the occurrence of electrode distortion, and the temperature was raised again to about 200°C in the baking (absolute drying) step (absolute drying of the electrode before liquid injection). In the present disclosure, by preventing the vapor of the electrode slurry from being brought into the baking step, the conventional coating and drying step and the baking step in reel-to-reel conveyance are directly connected, so that cooling in the pressing step is no longer required, energy efficiency is improved, and productivity can be enhanced.
[0016] (1) Coating Step The coating step is a step of coating the electrode slurry on the substrate.
[0017] The base material may be a current collector or the like. The current collector may be a negative electrode current collector, a positive electrode current collector, a bipolar current collector, etc. Examples of materials for the current collector include metals such as aluminum, copper, stainless steel, and nickel. The thickness of the current collector is, for example, 0.1 μm or more and 100 μm or less. The shape of the current collector may be sheet-like or the like.
[0018] The electrode slurry is applied to the first surface of the substrate. The electrode slurry may be applied only to the first surface of the current collector, or it may be applied to the first surface of the current collector and the second surface which is the back surface of the first surface. Electrode slurry can be prepared by mixing electrode materials, including active material, binder, conductive material, electrolyte, thickener, etc., with a solvent. The electrode slurry may be a positive electrode slurry or a negative electrode slurry. The electrode slurry may contain water at a concentration of approximately 10,000 ppm or less.
[0019] The active material may also be the positive electrode active material. Examples of positive electrode active materials include oxide active materials. Examples of oxide active materials include LiCoO2, LiMnO2, LiNiO2, LiVO2, and LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 Rock salt layered active materials such as O2, LiMn2O4, Li(Ni 0.5 Mn 1.5 Examples include spinel-type active materials such as O4, and olivine-type active materials such as LiFePO4, LiMnPO4, LiNiPO4, and LiCuPO4.
[0020] The active material may also be the negative electrode active material. Examples of negative electrode active materials include carbon active materials, oxide active materials, and metal active materials. Examples of carbon active materials include mesocarbon microbeads (MCMB), highly oriented graphite (HOPG), hard carbon, and soft carbon. Examples of oxide active materials include Nb2O5 and Li4Ti5O 12 Examples of metal active materials include SiO. Examples of metal active materials include In, Al, Si, and Sn.
[0021] Examples of the binder include fluorine-containing binders such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE), rubber-based binders such as butadiene rubber, and acrylic binders.
[0022] Examples of the conductive material include carbon materials, metal particles, conductive polymers, and the like. Examples of the carbon material include particulate carbon materials such as acetylene black (AB) and Ketjen black (KB); and fibrous carbon materials such as carbon fibers, carbon nanotubes (CNT), and carbon nanofibers (CNF).
[0023] Examples of the thickener include polysaccharides such as carboxymethyl cellulose and methyl cellulose.
[0024] Examples of the electrolyte include solid electrolytes such as sulfide solid electrolytes and oxide solid electrolytes. Examples of the sulfide solid electrolyte include solid electrolytes containing Li element, element X (X is at least one selected from P, As, Sb, Si, Ge, Sn, B, Al, Ga, and In), and S element. The sulfide solid electrolyte may further contain at least one of O element and halogen element. Examples of the halogen element include F element, Cl element, Br element, and I element.
[0025] Examples of the oxide solid electrolyte include Li2O-B2O3-P2O5, Li2O-SiO2, Li2O-B2O3, Li 1.3 Al 0.3 Ti 0.7 (PO4)3, Li5La3Ta2O 12 , Li7La3Zr2O 12 , Li6BaLa2Ta2O 12 , Li 3.6 Si 0.6 P 0.4 O4, Li4SiO4, Li3PO4, Li3PO 4-3 / 2x N x (x≦1), and the like.
[0026] Examples of solvents include aqueous solvents and organic solvents. An aqueous solvent refers to water or a mixed solvent containing water and a polar organic solvent. For example, a suitable dispersion medium can be selected depending on the type of active material, binder, etc. As an aqueous solvent, water is preferably used due to its ease of handling. Examples of polar organic solvents that can be used as a mixed solvent include alcohols such as methanol, ethanol, and isopropyl alcohol, ketones such as acetone, and ethers such as tetrahydrofuran. Examples of organic solvents include N-methyl-2-pyrrolidone (NMP).
[0027] (2) Drying process The drying process is a process of drying the electrode slurry. Typically, a drying device is used in the drying process to dry the electrode slurry. The drying device can be any conventionally known device capable of drying the electrode slurry, such as a hot air device, a laser device, or an IR (infrared) device. In the drying process, the electrode slurry may be completely dried until the moisture content is several hundred ppm or less. The electrode slurry becomes an electrode layer through a drying process.
[0028] The drying process includes a first step, a second step, and a third step. The first step is to dry the electrode slurry at a constant rate below the first dew point after the coating step. The second step is to reduce the rate of drying the electrode slurry below the second dew point after the first step. The third step is to reduce the rate of drying the electrode slurry below the third dew point after the second step. In the first step, the electrode slurry may be dried in the first furnace; in the second step, the electrode slurry may be dried in the second furnace; and in the third step, the electrode slurry may be dried in the third furnace. In the drying step, the workpiece containing the substrate and the electrode slurry coated on the substrate may be placed on a conveyor and transported in the order of the first furnace, the second furnace, and the third furnace. Alternatively, the workpiece may be placed on a conveyor and transported in the order of the coating step and the drying step. The transport speed may be, for example, 30 m / min or more.
[0029] The second dew point is lower than the first dew point, and the third dew point is lower than the second dew point. The first dew point may be -20°C or higher, or -10°C or higher. The second dew point may be lower than the first dew point and higher than the third dew point, for example, -10°C or lower. The third dew point may be -20°C or lower.
[0030] The pressure in the first furnace during the first process may be lower than the pressure in the second furnace during the second process, and the pressure in the second furnace during the second process may be lower than the pressure in the third furnace during the third process. This suppresses the generation of airflow from the first furnace to the second furnace, and suppresses the generation of airflow from the second furnace to the third furnace, and makes it possible to maintain a state in which the dew points of the second and third furnaces are lower than the dew point of the first furnace. The pressure inside the first furnace in the first process may be negative relative to the outside of the drying process system, and may also be negative relative to the pressure inside the second furnace in the second process. The pressure in the second furnace during the second process may be positive relative to the pressure in the first furnace during the first process, and negative relative to the pressure in the third furnace during the third process. The pressure inside the third furnace in the third process may be negative relative to the outside of the drying process system, and positive relative to the pressure inside the second furnace in the second process.
[0031] The volume of the first furnace may be larger than the volumes of the second and third furnaces. By making the volumes of the second and third furnaces smaller than the volume of the first furnace, the dew point of the air can be lowered from the second process onward. The volumes of the second and third furnaces may be the same or different.
[0032] In the first step, the electrode slurry may be heated using a hot air device, laser device, IR device, etc. In the first step, outside air may be supplied into the first furnace, or hot air with a dew point of -20°C to 25°C and a temperature of 65°C or higher may be supplied to raise the temperature inside the first furnace to 65°C or higher. In the first step, taking advantage of the fact that the pressure inside the first furnace is lower than the pressure inside the second furnace, hot air may be supplied into the second furnace, an airflow may be generated so that the hot air flows from the second furnace to the first furnace, and the hot air supplied to the second furnace may be supplied into the first furnace. This can suppress the rise in the dew point inside the second furnace. Radiant heat may also be used in the first step. In the first step, the electrode slurry may be heated to the maximum temperature required for drying the electrode slurry, and the heating temperature of the electrode slurry may be between 100°C and 200°C. The drying time of the electrode slurry in the first step is not particularly limited as long as it is within the constant-rate drying period of the electrode slurry. The constant-rate drying period is the period during which the surface and core temperatures of the material are kept the same and the water content decreases linearly with time. The drying time of the electrode slurry in the first step can be set appropriately according to the dew point and temperature in the first furnace, the heating temperature of the electrode slurry, etc. In the first step, the electrode slurry may be dried using a laser and IR at a temperature of 100°C to 200°C for 10 to 15 seconds.
[0033] In the second step, hot air, for example, with a dew point of -10°C or lower and a temperature of 65°C or higher, may be supplied to the second furnace to raise the temperature inside the second furnace to 65°C or higher. In the second step, hot air may be supplied to the third furnace by taking advantage of the fact that the pressure inside the first furnace is lower than the pressure inside the second furnace, and the pressure inside the second furnace is lower than the pressure inside the third furnace, generating an airflow so that the hot air flows from the third furnace to the second furnace and the first furnace, and the hot air supplied to the third furnace may also be supplied to the second furnace and the first furnace. This can suppress the rise in the dew point inside the third furnace. In the second step, by providing the second furnace, the first furnace and the third furnace can be isolated, and the inside of the third furnace can be maintained at a low dew point. The drying time of the electrode slurry in the second step is not particularly limited as long as it is within the decay drying period of the electrode slurry. The decay drying period is the period until the surface temperature begins to rise rapidly, the core temperature follows suit, and the surface temperature and core temperature of the material approach the heat source temperature.
[0034] In the third step, hot air with a dew point of -20°C or lower and a temperature of 65°C or higher may be supplied to the third furnace to raise the temperature inside the third furnace to 65°C or higher. In the third step, the electrode slurry may be heated using a hot air device, laser device, IR device, etc. In the third step, radiant heat may be utilized. The heating temperature of the electrode slurry in the third step may be 100°C to 200°C. The temperature of the hot air supplied to the third furnace in the third process may be the same as or higher than the temperature of the hot air supplied to the first furnace in the first process, and may also be higher than the temperature reached by the electrode slurry, from the viewpoint of suppressing a decrease in the temperature of the electrode slurry. The drying time of the electrode slurry in the third step is not particularly limited as long as it is within the decay drying period of the electrode slurry. In the third step, the electrode slurry may be dried using a laser or IR at a temperature of 100°C to 200°C for 10 to 15 seconds.
[0035] The dew point at the outlet of the third furnace in the third step may be -20°C or lower. The area on the outlet side after leaving the third furnace may be a dry air atmosphere. In the third step, moisture is removed from the electrode slurry to a level of several hundred ppm or less, for example, 500 ppm or less, and an electrode layer is formed on the substrate. After the third step, the electrode, including the substrate and the electrode layer, may be pressed.
[0036] The dew point fluctuates when outside air flows into the furnace or when the moisture in the electrode slurry itself dries. Therefore, in the drying process, a dew point meter may be installed, and in an environment where hot air is supplied, the dew point of the air, the amount of hot air supplied, and the temperature of the hot air may be adjusted as appropriate according to the measured dew point. Specifically, the dew point meter may be installed in the exhaust piping of the third reactor. The dew point of the exhaust piping may then be fed back to the supply air side, and the dew point of the air, the amount of hot air supplied, and the temperature of the hot air may be adjusted so that the dew point value reaches a predetermined dew point. Even if the internal furnace environment fluctuates due to the evaporation of moisture in the electrode slurry, the dew point, hot air supply rate, hot air temperature, etc., can be adjusted to follow these changes, allowing for stable drying of the electrode slurry. Instead of adjusting the dew point, hot air supply rate, and hot air temperature for all three furnaces (1st to 3rd), the most efficient way to completely dry the electrode slurry is to observe and control the dew point of the final zone, the 3rd furnace. To adjust the amount of hot air supplied, an auto damper or the like, which can control opening and closing and the degree of opening according to the dew point, may be used.
[0037] Figure 1 is a schematic diagram showing an example of the drying process of this disclosure. In the drying process shown in Figure 1, the workpiece 1 is transported in the transport direction, in the first step the workpiece 1 is heated in the first furnace 10 by a laser device 11, in the second step hot air 50 is supplied to the second furnace 20 by a hot air device 21, and in the third step hot air 50 is supplied to the third furnace 30 by a hot air device 32, and the workpiece 1 is heated in the third furnace 30 by a laser device 31. In the first step, hot air 50 may also be supplied into the first furnace 10 by a hot air device. In the first step, a hot air device, an IR device, etc. may be used instead of the laser device 11. In the second step, a partition may be provided to separate the first furnace 10 and the third furnace 30. In the second step, the hot air 50 supplied from the hot air device 21 may have a dew point of -10°C or lower and a temperature of 65°C or higher. In the third step, the hot air 50 supplied from the hot air device 32 may have a dew point of -20°C or lower and a temperature of 65°C or higher. The volumes of the second furnace 20 and the third furnace 30 are smaller than the volume of the first furnace 10. Because the pressure inside the first furnace 10 is lower than the pressure inside the second furnace 20, the hot air 50 supplied to the second furnace 20 generates an airflow that flows from the second furnace 20 into the first furnace 10, and the second dew point inside the second furnace 20 is maintained to be lower than the first dew point inside the first furnace 10. Because the pressure inside the second furnace 20 is lower than the pressure inside the third furnace 30, the hot air 50 supplied to the third furnace 30 generates an airflow that flows from the third furnace 30 into the second furnace 20, and the third dew point inside the third furnace 30 is maintained to be lower than the second dew point inside the second furnace 20. The area on the outlet side of the third furnace 30 after the third process may be under a dry air atmosphere. After the third step, workpiece 1 is subjected to a pressing process.
[0038] The electrode obtained by the manufacturing method of this disclosure comprises an electrode layer and a current collector. The electrode layer may be either a positive electrode layer or a negative electrode layer. The electrode layer may also contain a positive electrode active material and a negative electrode active material, as well as a binder, conductive material, electrolyte, etc. These materials are as described above. The current collector may be a negative electrode current collector, a positive electrode current collector, a bipolar current collector, etc. The material, thickness, and shape of the current collector are as described above.
[0039] The electrodes of this disclosure are typically used in the manufacture of batteries. The electrodes may be positive or negative electrodes. The type of battery using electrodes is not particularly limited, but lithium-ion secondary batteries are an example. The battery may be a liquid-type battery using an electrolyte solution, or a solid-state battery using a solid electrolyte solution. Applications of the battery include, for example, powering vehicles such as hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), battery electric vehicles (BEVs), gasoline cars, and diesel cars. In particular, it may be used as a power source for hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), or electric vehicles (BEVs). The battery may also be used as a power source for mobile devices other than vehicles (e.g., trains, ships, aircraft), or as a power source for electrical products such as information processing devices. [Explanation of symbols]
[0040] 1. Work 10.First furnace 11. Laser device 20.Second Furnace 21.Hot air device 30. No. 3 furnace 31. Laser device 32.Hot air equipment 50. Hot air
Claims
1. A method for manufacturing electrodes, A coating process in which an electrode slurry is applied to a substrate, A drying step in which the electrode slurry is dried until the moisture content is 500 ppm or less, and an electrode layer is formed on the substrate, The process includes a pressing step in which the substrate and the electrode layer are pressed after the drying step, The aforementioned drying process is After the coating process, a first step is to dry the electrode slurry at a constant rate below a first dew point, After the first step, a second step is performed in which the electrode slurry is reduced-rate dried below the second dew point, The process includes a third step of drying the electrode slurry at a reduced dew point after the second step, The second dew point is lower than the first dew point. The third dew point is lower than the second dew point. The pressure inside the first furnace in the first step is less than the pressure inside the second furnace in the second step. The pressure in the second furnace during the second step is less than the pressure in the third furnace during the third step. The temperatures inside the first furnace, the second furnace, and the third furnace are 65°C or higher. A method for manufacturing an electrode, wherein the second dew point is -10°C or lower, and the third dew point is -20°C or lower.
2. The method for manufacturing an electrode according to claim 1, wherein the volume of the first furnace is greater than the volumes of the second and third furnaces.
Citation Information
Patent Citations
Manufacture of sheet-form electrode plate
JP1996111222A
Manufacture of nonaqueous secondary battery
JP1997283120A
Manufacturing method of electrode plate and electrode plate
JP2006107780A
Method and apparatus of manufacturing electrode for electrochemical element
JP2007227831A
Method for manufacturing electrode for nonaqueous electrolyte secondary battery and manufacturing device