Glass cloth, surface-treated glass cloth, prepreg, and printed circuit boards
By controlling fiber opening coefficients and using surface-treated glass cloths, the issue of microvoids in prepregs is resolved, leading to high-yield, fast signal transmission printed circuit boards.
Patent Information
- Application Number
- JP2024085949
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-06-05
- Filing Date
- 2024-05-28
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2044-05-28
AI Technical Summary
Glass cloths with non-uniform fiber opening lead to microvoids in prepregs, causing volume expansion and contraction during printed circuit board manufacturing, resulting in warping and low yield rates.
A glass cloth with controlled average unit area fiber opening coefficient (SD) of 0.35 to 0.75, average unit area uniformity coefficient (RA) of 0.10 to 0.40, and RA/SD value of 0.10 to 1.10, treated with aminosilane or alkenylsilane coupling agents, is used to produce prepregs with good fiber opening uniformity and no microvoids.
The solution results in prepregs with a good appearance and high yield rate, and printed circuit boards with fast signal transmission speed.
Smart Images

Figure 0007948680000014 
Figure 0007948680000001 
Figure 0007948680000002
Abstract
Description
[Technical Field]
[0001] This invention relates to textile fabrics, and more particularly to glass cloth and its applications. [Background technology]
[0002] As electronic products become more multifunctional, faster, lighter, and smaller, the glass cloth used in the manufacture of printed circuit boards (PCBs) is being developed to be thinner.
[0003] To make glass cloth thinner, it is common to manufacture it by weaving glass fiber yarns with a short average filament diameter as both warp and weft threads. However, this increases the proportion of yarn window area (i.e., the gap between warp and weft threads in the glass cloth) within the cloth.
[0004] When the proportion of the thread window area increases, the fiber weave effect is more likely to occur when signals pass through printed circuit boards made of such glass cloth, negatively impacting the signal transmission speed.
[0005] To address the above issues, it is common practice to increase the degree of fiber opening (or fiber splitting) of the glass cloth. Fiber opening is a technique that increases the surface area of the glass fiber yarn and reduces the yarn window by uniformly dispersing the multiple filaments that make up the glass fiber yarn in a flattened shape.
[0006] For example, Patent Documents 1 and 2 disclose glass cloth having a specific degree of fiber opening. [Prior art documents] [Patent Documents]
[0007] [Patent Document 1] Taiwan Patent No. I720996 [Patent Document 2] Taiwan Patent No. I723117 Publication [Overview of the Initiative] [Problems that the invention aims to solve]
[0008] However, if the glass cloth only meets a specific degree of fiber opening and has poor fiber opening uniformity, that is, if the difference in the size of each thread window within the glass cloth is too large, then microvoids will be present in the prepreg manufactured using that glass cloth. This leads to problems such as excessive expansion and contraction of the prepreg's volume during the printed circuit board manufacturing process, causing warping in the manufactured printed circuit boards and resulting in a low yield rate for printed circuit boards.
[0009] Therefore, the object of the present invention is to provide a glass cloth having a good degree of fiber opening and good fiber opening uniformity, a surface-treated glass cloth, a prepreg, and a printed circuit board. [Means for solving the problem]
[0010] To achieve the above objective, the present invention provides a glass cloth, which is a woven fabric made of multiple warp threads and multiple weft threads made of glass fiber yarn. The glass cloth has an average unit area fiber opening coefficient SD within the range of 0.35 to 0.75, an average unit area uniformity coefficient RA within the range of 0.10 to 0.40, and an RA / SD value within the range of 0.10 to 1.10. The aforementioned SD and RA are determined by the following equations 1 and 2:
[0011]
number
[0012] Further, the present invention is a surface-treated glass cloth which is a surface-treated product of the above glass cloth obtained using a treatment liquid, wherein the treatment liquid contains a treatment agent selected from the group consisting of aminosilane coupling agents, alkenylsilane coupling agents, acryloyloxysilane coupling agents, and combinations thereof. The present invention provides a surface-treated glass cloth characterized by the above features.
[0013] Further, the present invention provides a prepreg characterized by comprising a partially cured resin and the above surface-treated glass cloth.
[0014] Further, the present invention provides a printed wiring board characterized by being formed from the above prepreg. [Effects of the Invention]
[0015] For the glass cloth of the present invention, the inventors designed SD and RA in consideration of the average width, average weaving density, and width range of the plurality of warp yarns and the plurality of weft yarns, and limited SD to be within the range of 0.35 to 0.75, RA to be within the range of 0.10 to 0.40, and the RA / SD value to be within the range of 0.10 to 1.10, so that the glass cloth has a good fiber opening degree and good fiber opening uniformity. The surface-treated glass cloth of the present invention produced from the glass cloth of the present invention also has a good fiber opening degree and good fiber opening uniformity, whereby the prepreg of the present invention produced from the surface-treated glass cloth of the present invention has a good appearance and no microvoids, and the printed wiring board of the present invention produced from the prepreg of the present invention has the advantages of a high yield rate and fast signal transmission speed. Brief Description of the Drawings
[0016] [Figure 1] It is a diagram showing a part of one embodiment of the glass cloth of the present invention. Modes for Carrying Out the Invention
[0017] In order to more clearly describe the objectives, technical solutions and advantages of the embodiments of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the accompanying drawings of the embodiments of the present invention. It is obvious that the described embodiments are part, not all, of the embodiments of the present invention. Typically, the components of the embodiments of the present invention illustrated and depicted in the accompanying drawings may be arranged and designed in a variety of different configurations. Accordingly, the following detailed description of the embodiments of the present invention provided in the accompanying drawings does not constitute any limitation on the protection scope of the present invention, and merely illustrates selected embodiments of the present invention.
[0018] In the description of the present invention, terms indicating orientation or positional relationship such as "upper", "lower", "inner", "outer", "left", "right", "front", and "rear" are based on the orientation or positional relationship shown in the drawings, or the orientation or positional relationship conventionally placed when using the product of the present invention, for the purpose of simpler and clearer description, and do not teach or imply that the corresponding apparatus or device must have a specific orientation, structure or operation in a specific orientation, and are not limitations on the present invention.
[0019] <Glass Cloth> The glass cloth of the present invention is a glass cloth which is a woven fabric composed of a plurality of warps that are glass fiber yarns and a plurality of wefts that are glass fiber yarns. That is, the glass cloth of the present invention is a glass cloth produced by weaving using a plurality of warps that are glass fiber yarns and a plurality of wefts that are the glass fiber yarns.
[0020] In this embodiment, the glass fiber yarns used for the warps and the wefts are the same type of glass fiber yarn.
[0021] The glass cloth has an average unit area fiber opening coefficient SD within the range of 0.35 to 0.75, an average unit area uniformity coefficient RA within the range of 0.10 to 0.40, and an RA / SD value within the range of 0.10 to 1.10.
[0022] SD and RA are determined by the following equations 1 and 2.
[0023]
number
[0024] The average unit area fiber opening coefficient (SD) represents the "degree of fiber opening" of the glass cloth.
[0025] Furthermore, W×F represents the average area of the region where multiple warp threads and multiple weft threads overlap.
[0026] 25400 is a unit of weave density (threads / 25.4 mm = threads / 25400 μm), representing the maximum width allocated to each warp and weft thread. Therefore,
[0027]
number
[0028] The maximum area includes the area where each warp and weft thread overlaps (i.e., the area of area A shown in Figure 1), the area where each warp thread does not overlap with each weft thread (i.e., the area of area B shown in Figure 1), the area where each weft thread does not overlap with each warp thread (i.e., the area of area C shown in Figure 1), and the area of each thread window (i.e., the area of area D shown in Figure 1).
[0029] The average unit area uniformity coefficient RA represents the "fiber opening uniformity" of the glass cloth.
[0030]
number
[0031]
number
[0032]
number
[0033] By controlling the values of SD, RA, and RA / SD to be within the above range, the glass cloth has a good degree of fiber opening and good fiber opening uniformity, that is, the proportion occupied by the yarn window area is low and the difference in size between each yarn window in the glass cloth is small. As a result, the surface-treated glass cloth of the present invention manufactured using this glass cloth (i.e., the glass cloth of the present invention) also has a good degree of fiber opening and good fiber opening uniformity. As a result, the prepreg of the present invention manufactured using the surface-treated glass cloth of the present invention has a good appearance and is free of microvoids, and the printed circuit board of the present invention manufactured using the prepreg of the present invention has the advantages of a high yield rate and a fast signal transmission speed.
[0034] When the SD falls below 0.35, the degree of fiber opening in the glass cloth decreases, meaning that the proportion of the yarn window area increases. When signals pass through printed circuit boards manufactured using such glass cloth, a fiber weaving effect is more likely to occur, negatively impacting the signal transmission speed.
[0035] Generally, to improve the degree of fiber opening in glass cloth, the water pressure used for opening during manufacturing is sometimes increased. When the SD exceeds 0.75, the degree of fiber opening in glass cloth increases. However, because the water pressure used for opening is too high, the filaments of the multiple warp and weft threads in the glass cloth may break. As a result, the surface of the manufactured glass cloth has the disadvantage of having fuzz. Prepregs manufactured using such glass cloth have the disadvantage of having colloidal particles, and printed circuit boards manufactured using such prepregs have the disadvantage of having protrusions.
[0036] When the RA exceeds 0.40, the uniformity of the fiber opening of the glass cloth is poor, meaning there is a large difference in the size of each thread window within the glass cloth. As a result, prepregs manufactured using such glass cloth contain microvoids, and the volume of the prepreg expands and contracts too much during the printed circuit board manufacturing process. This causes warping in the manufactured printed circuit boards and reduces the yield rate of the printed circuit boards.
[0037] If the RA / SD value exceeds 1.10, even if SD is within the range of 0.35 to 0.75 and RA is within the range of 0.10 to 0.40, prepregs manufactured using such glass cloth will have a poor appearance and contain microvoids, resulting in a low yield rate for printed circuit boards manufactured using such prepregs.
[0038] In order to give the prepreg a superior appearance, in some embodiments the RA / SD value is in the range of 0.20 to 1.00, and in some embodiments the RA / SD value is in the range of 0.20 to 0.90.
[0039] In some embodiments, each warp thread is composed of multiple filaments, each weft thread is composed of multiple filaments, each warp thread has an average filament diameter in the range of 3.0 μm to 5.0 μm and an average number of filaments in the range of 30 to 200, and each weft thread has an average filament diameter in the range of 3.0 μm to 5.0 μm and an average number of filaments in the range of 30 to 200.
[0040] Each filament is manufactured by spinning glass raw materials, which include, for example, glass raw materials for general electronic components (e.g., E-glass), low dielectric constant (low K) glass raw materials, low thermal expansion coefficient (low CTE) glass raw materials, or glass raw materials that combine low dielectric constant and low thermal expansion coefficient.
[0041] In some embodiments, the average thickness of the glass cloth is in the range of 10.0 μm to 50.0 μm, and the average basis weight of the glass cloth is 10.0 g / m 2 ~50.0 g / m 2 is within the range.
[0042] In some embodiments, based on the calculated average area of the glass cloth, the average weaving density of the plurality of warp yarns is in the range of 50 threads / 25.4mm to 100 threads / 25.4mm, and the average weaving density of the plurality of weft yarns is in the range of 50 threads / 25.4mm to 100 threads / 25.4mm.
[0043] The glass cloth of the present invention is produced by treating an unopened glass cloth (i.e., a glass cloth that has not been subjected to opening treatment) through a process including an opening treatment. As long as the produced glass cloth has an SD in the range of 0.35 to 0.75, an RA in the range of 0.10 to 0.40, and an RA / SD value in the range of 0.10 to 1.10, all existing operation methods and equipment for opening treatment are suitable for producing the glass cloth of the present invention, and there is no need to limit the specific operation method and equipment of the opening treatment.
[0044] In some embodiments, the opening treatment is performed by applying tension to the unopened glass cloth in conjunction with spraying a high-pressure water column flow onto the unopened glass cloth using an opening device. The tension is, for example, in the range of 50 N to 300 N but is not limited thereto, and the water pressure of the high-pressure water column flow is, for example, in the range of 20 kg to 80 kg but is not limited thereto.
[0045] <Surface-treated glass cloth> The surface-treated glass cloth of the present invention is a surface-treated product of the above-mentioned glass cloth of the present invention obtained with a treatment liquid. That is, the surface-treated glass cloth of the present invention is produced by subjecting the above glass cloth to surface treatment, and the surface treatment includes reacting the glass cloth with a treatment liquid to change the properties of the glass cloth, so that the surface-treated glass cloth can interact with a resin in a subsequent process.
[0046] Since the glass cloth of the present invention has the advantage of having a good degree of fiber opening and good fiber opening uniformity, the surface-treated glass cloth of the present invention also has the advantage of having a good degree of fiber opening and good fiber opening uniformity.
[0047] In some embodiments, the treatment solution comprises a treatment agent selected from the group consisting of aminosilane coupling agents (amino group-containing silane coupling agents), alkenylsilane coupling agents (alkenyl group-containing silane coupling agents), acryloyloxysilane coupling agents (acryloyloxy group-containing silane coupling agents), and combinations thereof. That is, the treatment solution is manufactured by containing a treatment agent.
[0048] Aminosilane coupling agents include, for example, 3-aminopropyltriethoxysilane These are some examples, but are not limited to these.
[0049] Examples of alkenylsilane coupling agents include, but are not limited to, vinyltrimethoxysilane.
[0050] Examples of acryloyloxysilane coupling agents include, but are not limited to, 3-(trimethoxysilyl)propyl methacrylate.
[0051] In some embodiments, the aminosilane coupling agent is 3-aminopropyltriethoxysilane The alkenylsilane coupling agent is vinyltrimethoxysilane, and the acryloyloxysilane coupling agent is 3-(trimethoxysilyl)propyl methacrylate.
[0052] <Prepreg> The prepreg of the present invention comprises a partially solidified resin and the surface-treated glass cloth of the present invention described above. That is, the prepreg of the present invention is formed by partially solidifying an impregnated cloth containing the resin and the surface-treated glass cloth of the present invention described above.
[0053] Specifically, the manufacturing of the prepreg involves impregnating the surface-treated glass cloth of the present invention, which serves as both a reinforcement and insulation material, with a resin to obtain an impregnated cloth, and then partially solidifying the impregnated cloth to reach the B-stage.
[0054] The surface-treated glass cloth of the present invention has the advantage of having a good degree of fiber opening and good fiber opening uniformity. Specifically, the proportion of the yarn window area in the surface-treated glass cloth is low and the difference in size between each yarn window in the surface-treated glass cloth is small, so the area filled with resin in the surface-treated glass cloth is relatively small, and the appearance of the prepreg of the present invention using the surface-treated glass cloth of the present invention is good and free of microvoids.
[0055] Examples of resins include, but are not limited to, thermosetting resins or UV-curable resins.
[0056] In some embodiments, the resin is a thermosetting resin.
[0057] Thermosetting resins include, for example, polyphenylene ether resin, phenolic resin, epoxy resin, and urea resin. Examples include, but are not limited to, formaldehyde resin, unsaturated polyester resin, melamine resin, fluororesin, or bismaleimide triazine resin (abbreviated as BT resin).
[0058] Examples of UV-curing resins include, but are not limited to, UV-curing polyurethane or UV-curing acrylic resin.
[0059] In some embodiments, the thermosetting resin is selected from the group consisting of, for example, epoxy resins, polyphenylene ether resins, phenolic resins, and bismaleimidotriazine resins.
[0060] An example of a downstream application of the prepreg of the present invention is to manufacture a laminate by stacking multiple prepregs and then adding a copper foil layer to at least one side, and then manufacturing a copper clad laminate (CCL) by thermocompression bonding the laminate.
[0061] In some embodiments, the production of the prepreg further includes the addition of an inorganic filler to produce an impregnated cloth, thereby the prepreg formed by the partial solidification of the impregnated cloth further includes the inorganic filler. By adding an inorganic filler, properties such as thermal conductivity, laser drilling property, and thermal expansion of a copper-clad laminate produced using the prepreg can be adjusted, and thus the printed circuit board produced using the copper-clad laminate has good reliability.
[0062] <Printed circuit board> The printed circuit board of the present invention is made of the above-described prepreg of the present invention. That is, the printed circuit board of the present invention is manufactured using the above-described prepreg of the present invention.
[0063] Specifically, an example of a downstream application of the prepreg is the manufacture of printed circuit boards by drilling, plating with gold or a gold-containing alloy, and etching circuit patterns onto a copper-clad laminate.
[0064] Since the prepreg of the present invention has a good appearance and does not contain microvoids, the printed circuit boards of the present invention manufactured using the prepreg of the present invention do not suffer from the problem of low yield.
[0065] The following describes embodiments of the present invention. It should be understood that these embodiments are illustrative and descriptive, and should not be construed as limiting the present invention.
[0066] <Example 1> Manufacturing of glass cloth: A weaver's beam was obtained by sequentially warping and sizing multiple glass fiber threads as warp threads and then beaming them. This weaver's beam was then installed in an air-jet loom (manufacturer: Toyota Industries Corporation, model number: JAT710) and woven together with multiple glass fiber threads as weft threads to create an unopened glass cloth. Finally, the unopened glass cloth was sequentially desizing and opening processes were performed to produce the glass cloth.
[0067] Table 1 shows the specifications of the raw silk (gray yarn) for each warp and weft thread (i.e., average filament diameter and average number of filaments), the tension applied during the fiber opening process, and the water pressure of the high-pressure water column.
[0068] Manufacturing of surface-treated glass cloth: The glass cloth was immersed in a treatment solution for 30 seconds, and then dried at 150°C to produce surface-treated glass cloth.
[0069] The treatment solution was produced by hydrolyzing an aminosilane coupling agent and an aqueous acetic acid solution for 30 minutes under conditions where the pH value was within the range of 3.5 to 5.5. Assuming the total amount of the aminosilane coupling agent and the aqueous acetic acid solution is 100 wt%, the amount of aminosilane coupling agent used was 0.08 wt%.
[0070] Prepreg manufacturing method: The surface-treated glass cloth was impregnated in a resin solution to obtain an impregnated cloth, and then the impregnated cloth was solidified at 210°C for 6 minutes to produce a partially solidified prepreg.
[0071] The resin solution was obtained by mixing a resin (specifically, bismaleimide triazine resin, manufacturer: Prior Company Limited, Taiwan, model number: BT-0001) with a solvent (specifically, methyl ethyl ketone). The total volume of the resin solution was 100 wt%, and the amount of resin used was 50 wt%.
[0072] <Examples 2-13 and Comparative Examples 1-7> The differences between Examples 2 to 13 and Comparative Examples 1 to 7 and Example 1 are shown in Tables 1 to 3. In each example, warp and weft threads with different raw silk specifications were used to produce glass cloths with different degrees of opening and different opening uniformity, according to different opening processing conditions.
[0073] In the resin solutions used in Examples 2 to 13 and Comparative Examples 1 to 7, the resin was epoxy resin (Manufacturer: Nan Ya Plastics Corporation, Taiwan; Model number: NPEB475) In the case of K70), the solvent was 1-methoxy-2-propanol, and the total amount of resin solution was 100 wt%, with 60 wt% of the resin used. The impregnated cloth was then solidified at 190°C for 6 minutes.
[0074] In the resin solutions used in Examples 2 to 13 and Comparative Examples 1 to 7, when the resin is polyphenylene ether resin (manufacturer: SABIC, Saudi Arabia, model number: NORYL SA9000), The solvent used was methyl ethyl ketone, and the total amount of resin solution was 100 wt%, with 65 wt% of the resin used. The impregnated cloth was then solidified at 180°C for 4 minutes.
[0075] <Evaluation Criteria> The following describes the standard measurement methods for glass cloth in Examples 1 to 13 and Comparative Examples 1 to 7, as well as the standard measurement methods and appearance evaluation methods for prepregs, using Example 1 as an example. The measurement results and appearance evaluation results are shown in Tables 1 to 3.
[0076] Average weave density of warp threads (D w ), average weft density (D f ) Measurement: A digital weave density measuring instrument (manufacturer: Textest Instruments, Switzerland, model number: FX3250) was used to measure the surface of the glass cloth in Example 1 to obtain the average weave density of multiple warp threads and the average weave density of multiple weft threads in the glass cloth in Example 1.
[0077] Measurement of the average width of the warp threads (W) and the average width of the weft threads (F): A 30cm length of glass cloth from Example 1 was cut, and the cut glass cloth was evenly divided into five measurement areas along its width. The cut glass cloth was then placed in a microscope (Manufacturer: NIKON, Model: ME600, Magnification: 5x), and five photographs were obtained of each measurement area. These photographs were then taken using image dimension measurement software (TS-Link, TOTAL-SMART). Using a device manufactured by TECHNOLOGY CO., LTD., the width of each warp thread and each weft thread in each photograph was measured, the average value of multiple warp threads and the average value of multiple weft threads in each photograph were calculated, and finally the average value of the average width data measured in each measurement area (i.e., the average data of the widths of five warp threads and the average data of the widths of five weft threads) was calculated to obtain the average width of multiple warp threads and the average width of multiple weft threads in the glass cloth of Example 1.
[0078] Warp thread width range (R w ), range of weft width (R f How to calculate ): R w = This is the difference between the maximum and minimum widths within multiple warp threads. R f = This is the difference between the maximum and minimum widths within multiple weft threads.
[0079] Measurement of the average thickness of glass cloth: The glass cloth of Example 1, which was 30 cm long and divided into five measurement areas, was placed on a digital micrometer (manufacturer: TESA, Switzerland; model number: MICROMASTER IP54; minimum scale: 0.001 mm) and the thickness of each measurement area was measured. Finally, the average value of the thickness data measured in each measurement area (i.e., the data for the five thicknesses) was calculated to obtain the average thickness of the glass cloth of Example 1.
[0080] Measurement of the average basis weight of glass cloth: The glass cloth from Example 1 was cut into three equal parts, and each part of the glass cloth was further cut into samples measuring 30 cm x 30 cm. The weight of each sample was then measured using an electronic balance (manufacturer: OHAUS, USA, model number: PR224, minimum scale division: 0.0001 g), and the basis weight of each sample was calculated using the following formula 3.
[0081] Equation 3: Basis weight of sample = Weight of sample / Area of sample Finally, the average basis weight of each sample (i.e., the data for the three basis weights) was calculated to obtain the average basis weight of the glass cloth in Example 1.
[0082] Measurement of resin content in prepreg: Based on the standard measurement method for "Resin Content of Prepreg Material (Treated Weight)" in IPC-TM-650 2.3.16.1 (1994 edition), the glass cloth and prepreg of Example 1 were each cut into 20cm x 20cm samples, and the weight of each sample was measured using the electronic balance described above. The resin content in the prepreg of Example 1 was then calculated using Equation 4 below.
[0083] Equation 4: Resin content in prepreg = (1 - weight of glass cloth sample / weight of prepreg sample) × 100% Measuring the average thickness of the prepreg: A 30cm length of prepreg from Example 1 was cut, and the cut prepreg was evenly divided into five measurement areas along its width. The cut prepreg was then placed on the digital micrometer described above, and the thickness of each measurement area was measured. Finally, the average value of the thickness data measured in each measurement area (i.e., the data for the five thicknesses) was calculated to obtain the average thickness of the prepreg from Example 1.
[0084] Measurement of the number of microvoids in the prepreg and evaluation of the appearance of the prepreg: The prepreg from Example 1 was cut into 5cm x 5cm samples, and then observed under the microscope described above. If there were pinhole-sized holes on the surface of the sample, they were considered microvoids, and the number of pinhole-sized microvoids on the surface of the sample was calculated.
[0085] If the number of microvoids in the prepreg was 0, the appearance of the prepreg was evaluated as "good." If the number of microvoids in the prepreg was between 1 and 100, the appearance of the prepreg was evaluated as "having a few pinholes." If the number of microvoids in the prepreg was 101 or more, the appearance of the prepreg was evaluated as "having obvious pinholes."
[0086] [Table 1-1]
[0087] [Table 1-2]
[0088] [Table 2-1]
[0089] [Table 2-2]
[0090] [Table 3-1]
[0091] [Table 3-2] According to Tables 1 to 3, the glass cloths of Examples 1 to 13 satisfy all requirements for SD within the range of 0.35 to 0.75, RA within the range of 0.10 to 0.40, and RA / SD value within the range of 0.10 to 1.10, and the prepregs of Examples 1 to 13 have a good appearance without microvoids on the surface.
[0092] In contrast, the glass cloths of Comparative Examples 1 to 7 do not meet all the requirements for an SD in the range of 0.35 to 0.75, an RA in the range of 0.10 to 0.40, and an RA / SD value in the range of 0.10 to 1.10, and the prepregs of Comparative Examples 1 to 7 have microvoids on their surface.
[0093] Therefore, the glass cloths of Examples 1 to 13 satisfy all the requirements of an SD in the range of 0.35 to 0.75, an RA in the range of 0.10 to 0.40, and an RA / SD value in the range of 0.10 to 1.10, thus demonstrating that the absence of microvoids on the surface of the prepregs of Examples 1 to 13 can be achieved.
[0094] According to the above, the glass cloth of the present invention is characterized by calculating SD and RA based on the average width, average weave density, and width range of multiple warp and weft threads, and by limiting the SD to be within the range of 0.35 to 0.75, the RA to be within the range of 0.10 to 0.40, and the RA / SD value to be within the range of 0.10 to 1.10. As a result, the glass cloth of the present invention is characterized by a good degree of fiber opening and good fiber opening uniformity, and the surface-treated glass cloth of the present invention manufactured using the glass cloth of the present invention also has a good degree of fiber opening and good fiber opening uniformity. Consequently, the prepreg of the present invention manufactured using the surface-treated glass cloth of the present invention has a good appearance and is free of microvoids, and the printed circuit board of the present invention manufactured using the prepreg of the present invention has the advantages of a high yield rate and a fast signal transmission speed. Therefore, the objectives of the present invention can be reliably achieved.
[0095] While the present invention has been described in relation to what may be considered exemplary embodiments, it is understood that the invention is not limited to the disclosed embodiments and is intended to cover a variety of configurations that fall within the broadest spirit and scope of interpretation to encompass all such modifications and equivalent configurations.
[0096] The above embodiments are illustrative in illustrating the principles and effects of the present invention and do not limit it. A person skilled in the art can make some modifications and alterations to the above embodiments, provided that they do not deviate from the spirit and scope of the invention. Therefore, all modifications and alterations made by a person skilled in the art, provided that they do not deviate from the spirit of the invention, should also be considered to fall within the scope of protection of the present invention. [Industrial applicability]
[0097] The glass cloth of this invention is suitable for use in electronic products. [Explanation of Symbols]
[0098] A. Area of the part where each warp thread and each weft thread overlap. B. Area of the portion of each warp thread that does not overlap with each weft thread. C. Area of the portion of each weft thread that does not overlap with each warp thread. D Area of each thread window
Claims
1. Glass cloth is a fabric made of multiple warp threads and multiple weft threads made of glass fiber yarn. The glass cloth has an average unit area fiber opening coefficient SD in the range of 0.35 to 0.75, an average unit area uniformity coefficient RA in the range of 0.10 to 0.40, and a value of RA / SD in the range of 0.10 to 1.
10. The SD and RA are determined by the following formulas 1 and 2: [Math 1] In the formula, W is the average width of the plurality of warp threads, F is the average width of the aforementioned multiple weft threads, D w This is the average weave density of the multiple warp threads, D f This is the average weave density of the multiple weft threads, R w This is the range of widths of the aforementioned multiple warp threads, R f A glass cloth characterized in that is a range of widths of the plurality of weft threads.
2. The glass cloth according to claim 1, characterized in that the RA / SD value is within the range of 0.20 to 1.
00.
3. The glass cloth according to claim 2, characterized in that the RA / SD value is within the range of 0.20 to 0.
90.
4. Each of the aforementioned warp threads is composed of multiple filaments, Each of the aforementioned weft threads is composed of multiple filaments, Each of the warp threads has an average filament diameter in the range of 3.0 μm to 5.0 μm, and an average number of filaments in the range of 30 to 200. The glass cloth according to claim 1, characterized in that each of the aforementioned weft threads has an average filament diameter in the range of 3.0 μm to 5.0 μm and an average number of filaments in the range of 30 to 200.
5. The average thickness of the aforementioned glass cloth is within the range of 10.0 μm to 50.0 μm. The average basis weight of the aforementioned glass cloth is 10.0 g / m². 2 ~50.0 g / m 2 It is within the range, The glass cloth according to claim 1, characterized in that, using the average area of the glass cloth as a calculation basis, the average weaving density of the plurality of warp threads is in the range of 50 threads / 25.4 mm to 100 threads / 25.4 mm, and the average weaving density of the plurality of weft threads is in the range of 50 threads / 25.4 mm to 100 threads / 25.4 mm.
6. The surface-treated glass cloth is a surface-treated product of the glass cloth described in claim 1, which is a surface-treated glass cloth using a processing liquid. The surface-treated glass cloth is characterized in that the treatment solution comprises a treatment agent selected from the group consisting of aminosilane coupling agents, alkenylsilane coupling agents, acryloyloxysilane coupling agents, and combinations thereof.
7. A prepreg characterized by comprising a partially solidified resin and the surface-treated glass cloth described in claim 6.
8. The prepreg according to claim 7, characterized in that the resin is a thermosetting resin.
9. The prepreg according to claim 8, characterized in that the thermosetting resin is selected from the group consisting of epoxy resin, polyphenylene ether resin, and bismaleimidotriazine resin.
10. A printed circuit board characterized by being made of a prepreg as described in any one of claims 7 to 9.
Citation Information
Patent Citations
Glass cloth
JP2017043873A
Glass cloth
JP2018021274A
Glass cloth manufacturing method and glass yarn
JP2020105683A
Glass cloth and glass yarn
JP2022181738A
JPP7029033B