Acidified gypsum membrane grinding solution composition
The use of cerium oxide particles and alkoxyacetic acid in a polishing liquid composition addresses the challenges of high-speed and uniform silicon oxide film planarization, improving semiconductor manufacturing efficiency and quality.
Patent Information
- Application Number
- JP2022165767
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-10-14
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2042-10-14
AI Technical Summary
The semiconductor industry faces challenges in achieving high polishing speed and in-plane uniformity during the planarization of silicon oxide films, particularly in the manufacturing of 3D NAND flash memory, due to large surface irregularities and varying polishing speeds across the substrate surface.
A polishing liquid composition comprising cerium oxide particles and alkoxyacetic acid or its salt is used to enhance polishing speed and uniformity, with cerium oxide acting as abrasive grains and alkoxyacetic acid modifying the surface properties to improve fluidity and affinity for water.
The composition achieves both improved polishing speed and in-plane uniformity, enhancing the efficiency and quality of semiconductor substrate manufacturing.
Smart Images

Figure 0007948811000006 
Figure 0007948811000001 
Figure 0007948811000002
Abstract
Description
Technical Field
[0001] The present disclosure relates to a polishing liquid composition for silicon oxide films, a method for manufacturing a semiconductor substrate using the same, and a polishing method.
Background Art
[0002] The chemical mechanical polishing (CMP) technology is a technique in which, while the surface of a substrate to be polished to be processed is in contact with a polishing pad, a polishing liquid is supplied to these contact portions and the substrate to be polished and the polishing pad are moved relative to each other, so that the uneven portions on the surface of the substrate to be polished are chemically reacted and mechanically removed to achieve planarization.
[0003] At present, this CMP technology has become an essential technique for performing processes such as planarization of interlayer insulating films, formation of shallow trench isolation structures, and formation of plugs and embedded metal wirings in the manufacturing process of semiconductor elements. In recent years, the multilayering and high definition of semiconductor elements have advanced dramatically, and further improvements in the yield and throughput of semiconductor elements have been required. Along with this, for the CMP process, polishing that is free from polishing scratches and has a higher speed has been desired.
[0004] For example, Patent Document 1 proposes a method for producing cerium dioxide particles, comprising: a) providing an aqueous reaction mixture comprising a first cerium ion source, a hydroxide ion source, at least one nanoparticle stabilizer, and an oxidizing agent; b) mechanically shearing the mixture, thereby forming a suspension of cerium hydroxide nanoparticles; and c) heating the mixture to a temperature between 50°C and 100°C, thereby forming cerium dioxide nanoparticles, wherein the nanoparticle stabilizer is selected from the group consisting of alkoxy-substituted carboxylic acids, α-hydroxyl carboxylic acids, pyruvic acid, and small organic polyacids. It is described in paragraph 0204 and the like of the same document that the cerium dioxide particles can be used as an abrasive for planarizing semiconductor substrates. Patent Document 2 proposes a polishing solution for polishing the barrier layer of a semiconductor integrated circuit, which contains colloidal silica whose surface exhibits a positive zeta potential, a compound having a carboxyl group, a corrosion inhibitor, and a surfactant, and has a pH of 2.5 to 5.0. [Prior art documents] [Patent Documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 2014-139127 [Patent Document 2] Japanese Patent Publication No. 2008-181954 [Overview of the project] [Problems that the invention aims to solve]
[0006] In recent years, the semiconductor field has seen increasing integration, requiring more complex and miniaturized wiring. Therefore, CMP (Chemical Polishing) attempts to reduce defects by decreasing the particle size of abrasive grains. However, this leads to a decrease in polishing speed, creating a need for improved silicon oxide film polishing speed. In particular, in the planarization process of the interlayer insulating film of 3D NAND flash memory by CMP, there is a problem that planarization by CMP takes a long time because there is a large difference in surface irregularities between the array portion of the film stacked in a step-like manner on the substrate to be polished and its surrounding area. For example, the reference International Conference on Planarization / CMP technology (ICPT), p106 (2016) proposes a method to improve CMP efficiency and shorten polishing time by performing an extra-etching process before CMP, as shown in Figure 1, to refine the protrusions. On the other hand, as the recording capacity increases, the thickness of the array portion increases further, and the difference in surface irregularities becomes even larger. Therefore, there is an increasing need to remove such fine protrusions at high speed. Furthermore, after removing minute protrusions, the entire substrate surface is further polished to flatten it. However, the polishing speed may differ between the center and periphery of the substrate surface, leading to a problem of reduced in-plane uniformity of polishing (global flattening). Therefore, there is a need to improve in-plane uniformity of polishing at a high polishing speed.
[0007] Therefore, this disclosure provides a silicon oxide film polishing liquid composition that can achieve both improved polishing speed and improved in-plane uniformity of polishing, a semiconductor substrate manufacturing method and polishing method using the same, and the like. [Means for solving the problem]
[0008] This disclosure relates, in one embodiment, to a polishing solution composition for silicon oxide films, comprising cerium oxide particles (component A), alkoxyacetic acid represented by the following formula (I) or a salt thereof (component B), and an aqueous medium. [ka] In formula (I) above, R represents an aliphatic hydrocarbon group having 1 to 6 carbon atoms, and M represents a hydrogen atom, an alkali metal, an alkaline earth metal, an organic cation, or ammonium (NH4) + ) indicates.
[0009] This disclosure relates, in one embodiment, to a method for manufacturing a semiconductor substrate, which includes a step of polishing a film to be polished using the silicon oxide film polishing solution composition of this disclosure.
[0010] This disclosure relates in one embodiment to a polishing method, which includes the step of polishing a film to be polished using the polishing solution composition of this disclosure, wherein the film to be polished is a silicon oxide film formed in the manufacturing process of a semiconductor substrate. [Effects of the Invention]
[0011] According to this disclosure, in one embodiment, a polishing liquid composition for silicon oxide films can be provided that can achieve both improved polishing speed and improved in-plane uniformity of polishing. [Brief explanation of the drawing]
[0012] [Figure 1] Figure 1 is a schematic diagram for explaining extra etching before CMP of an interlayer insulating film of a three-dimensional NAND flash memory. [Mode for Carrying Out the Invention]
[0013] As a result of intensive studies by the present inventors, the present invention is based on the finding that by incorporating a specific alkoxyacetic acid or a salt thereof (Component B) into a polishing liquid composition containing cerium oxide particles (Component A), it is possible to achieve both an improvement in the polishing rate of a silicon oxide film and an improvement in in-plane uniformity of polishing.
[0014] That is, in one aspect, the present disclosure relates to a polishing liquid composition for silicon oxide films (hereinafter also referred to as "the polishing liquid composition of the present disclosure"), which contains cerium oxide particles (Component A), an alkoxyacetic acid represented by the following formula (I) or a salt thereof (Component B), and an aqueous medium. [Chemical Formula] In the formula (I), R represents an aliphatic hydrocarbon group having 1 to 6 carbon atoms, and M represents a hydrogen atom, an alkali metal, an alkaline earth metal, an organic cation, or ammonium (NH4 + ).
[0015] According to the polishing liquid composition of the present disclosure, in one or a plurality of embodiments, it is possible to achieve both an improvement in the polishing rate of a silicon oxide film and an improvement in in-plane uniformity of polishing.
[0016] Although the details of the mechanism by which the effects of the present disclosure are exhibited are not clear, it is presumed as follows. To increase the polishing rate, it is important that the chemical agent is sufficiently adsorbed onto cerium oxide to modify the surface properties of cerium oxide. Although the carboxylic acid structure plays the role of adsorption onto cerium oxide, substitution with an alkoxy group improves the adsorptivity to cerium oxide. On the other hand, to improve the in-plane uniformity of polishing, it is considered important to enhance the affinity of the cerium oxide surface for water. If the hydrophobicity is too high, the fluidity of the liquid during polishing will deteriorate. By substituting with an alkoxy group, the affinity for water molecules is improved compared to that of an alkyl group, and as a result, the fluidity of the liquid during polishing is improved, which is considered to enhance the in-plane uniformity. However, the present disclosure should not be construed as being limited to these mechanisms. In the present disclosure, the fluidity of the liquid refers to the flowability of the slurry with respect to the polishing pad. In the present disclosure, the in-plane uniformity refers to the processing uniformity within the wafer surface, and indicates an index of flatness.
[0017] [Film to be polished] In one or more embodiments, the polishing composition of the present disclosure is a polishing composition for polishing a silicon oxide film (film to be polished) (polishing composition for silicon oxide films), and can be used in processes that require polishing of a silicon oxide film. For example, in one or more embodiments, the polishing composition of the present disclosure can be used for polishing a silicon oxide film performed in the step of forming an element isolation structure of a semiconductor substrate, polishing a silicon oxide film performed in the step of forming an interlayer insulating film, polishing a silicon oxide film performed in the step of forming embedded metal wiring, or polishing a silicon oxide film performed in the step of forming an embedded capacitor. In addition, in one or more embodiments, the polishing composition of the present disclosure can be used for manufacturing three-dimensional semiconductor devices such as three-dimensional NAND flash memories. In particular, the polishing liquid composition of this disclosure can be suitably used in one or more embodiments for polishing a substrate (substrate to be polished) having silicon oxide film protrusions (film to be polished). In one or more embodiments, the silicon oxide film protrusions are protrusions of a silicon oxide film on the substrate surface, and examples include protrusions with a width of 10 μm to 500 μm and a height of 4 μm to 10 μm. In one or more embodiments, the silicon oxide film protrusions can be formed by an extra-etching process before CMP of the interlayer insulating film of a three-dimensional NAND flash memory. In one or more embodiments, the silicon oxide film protrusions are silicon oxide film protrusions on the substrate surface after extra etching. In one or more embodiments, the substrate having silicon oxide film protrusions is a substrate that has been extra-etched before CMP of the interlayer insulating film of a three-dimensional NAND flash memory. In one or more embodiments, the polishing liquid composition of this disclosure is for polishing a substrate after extra etching.
[0018] [Cerium oxide particles (component A)] The polishing fluid composition of this disclosure contains cerium oxide (hereinafter also referred to as "ceria") particles (hereinafter simply referred to as "component A") as abrasive grains. Positively charged ceria or negatively charged ceria can be used as component A. The chargeability of component A can be confirmed, for example, by measuring the potential (surface potential) on the surface of the abrasive grains determined by electroacoustic method (ESA method: Electrokinetic Sonic Amplitude). The surface potential can be measured, for example, using a "Zeta Probe" (manufactured by Kyowa Interface Chemical Co., Ltd.), and specifically by the method described in the examples. Component A may be one type or a combination of two or more types. The chargeability of the abrasive grains is not limited, but positively charged ceria is preferred from the viewpoint of improving the polishing speed.
[0019] The manufacturing method, shape, and surface condition of component A are not particularly limited. Examples of component A include colloidal ceria, amorphous ceria, and ceria-coated silica. Colloidal ceria can be obtained by a build-up process, for example, by the methods described in Examples 1 to 4 of Japanese Patent Publication No. 2010-505735. Examples of amorphous ceria include pulverized ceria. One embodiment of pulverized ceria is calcined pulverized ceria obtained by calcining and pulverizing cerium compounds such as cerium carbonate and cerium nitrate. Another embodiment of pulverized ceria is single-crystal pulverized ceria obtained by wet pulverizing ceria particles in the presence of an inorganic acid or an organic acid. Examples of inorganic acids used in wet pulverization include nitric acid, and examples of organic acids include organic acids having a carboxyl group, specifically at least one selected from polycarboxylates such as ammonium polyacrylate, picolinic acid, glutamic acid, aspartic acid, aminobenzoic acid, and p-hydroxybenzoic acid. For example, when at least one selected from picolinic acid, glutamic acid, aspartic acid, aminobenzoic acid, and p-hydroxybenzoic acid is used in wet pulverization, positively charged ceria can be obtained, and when a polycarboxylate such as ammonium polyacrylate is used in wet pulverization, negatively charged ceria can be obtained. Examples of wet grinding methods include wet grinding using a planetary bead mill or the like. Examples of ceria-coated silica include composite particles having a structure in which at least a portion of the surface of silica particles is coated with granular ceria, as described in Examples 1 to 14 of Japanese Patent Publication No. 2015-63451 or Examples 1 to 4 of Japanese Patent Publication No. 2013-119131. These composite particles can be obtained, for example, by depositing ceria onto silica particles.
[0020] Examples of the shape of component A include a roughly spherical, polyhedral, or raspberry-like form.
[0021] The average primary particle size of component A is preferably 5 nm or more, more preferably 10 nm or more, even more preferably 20 nm or more, even more preferably 25 nm or more, even more preferably 30 nm or more, even more preferably 35 nm or more, and even more preferably 40 nm or more, and from the viewpoint of suppressing the occurrence of polishing scratches, it is preferably 300 nm or less, more preferably 200 nm or less, even more preferably 150 nm or less, even more preferably 100 nm or less, even more preferably 75 nm or less, and even more preferably 60 nm or less. In this disclosure, the average primary particle size of component A is calculated using the BET (nitrogen adsorption) method and the BET specific surface area S (m²) 2 It is calculated using ( / g). The BET specific surface area can be measured by the method described in the examples.
[0022] The content of component A in the polishing fluid composition of this disclosure is preferably 0.1% by mass or more, more preferably 0.15% by mass or more, and even more preferably 0.2% by mass or more, from the viewpoint of achieving both improved polishing speed and improved uniformity of polishing in the surface. From the viewpoint of suppressing the occurrence of polishing scratches, it is preferably 10% by mass or less, more preferably 5% by mass or less, even more preferably 1% by mass or less, even more preferably 0.75% by mass or less, and even more preferably 0.5% by mass or less. More specifically, the content of component A in the polishing fluid composition of this disclosure is preferably 0.1% by mass or more and 10% by mass or less, more preferably 0.15% by mass or more and 5% by mass or less, even more preferably 0.2% by mass or more and 1% by mass or less, even more preferably 0.2% by mass or more and 0.75% by mass or less, and even more preferably 0.2% by mass or more and 0.5% by mass or less. When component A is a combination of two or more types, the content of component A refers to the total content of those types.
[0023] [Alkoxyacetic acid represented by formula (I) or its salt (component B)] The polishing liquid composition of this disclosure contains an alkoxyacetic acid represented by the following formula (I) or a salt thereof (hereinafter also simply referred to as "component B"). Component B is a compound that does not have a hydroxyl group. However, the hydroxyl group (-OH) does not include the OH of a carboxyl group (-COOH). Component B may be one type or a combination of two or more types. [ka]
[0024] In formula (I) above, R represents an aliphatic hydrocarbon group having 1 to 6 carbon atoms, and M represents a hydrogen atom, an alkali metal, an alkaline earth metal, an organic cation, or ammonium (NH4) + This shows the following. Examples of organic cations include organic ammonium compounds in one or more embodiments, such as alkylammonium compounds including tetramethylammonium, tetraethylammonium, and tetrabutylammonium. In formula (I) above, R is preferably an alkyl group having 1 to 4 carbon atoms from the viewpoint of achieving both improved polishing speed and improved in-plane uniformity of polishing, and more preferably an alkyl group having 1 to 2 carbon atoms (methyl group or ethyl group) from the viewpoint of water solubility. M is preferably at least one selected from a hydrogen atom, an alkali metal, and an alkaline earth metal from the same viewpoint, and more preferably a hydrogen atom.
[0025] Component B can be, for example, at least one selected from methoxyacetic acid or its salts, and ethoxyacetic acid or its salts. Among these, ethoxyacetic acid or its salts are preferred from the viewpoint of achieving both improved polishing speed of the silicon oxide film and improved in-plane uniformity of polishing.
[0026] The content of component B in the polishing liquid composition of this disclosure is preferably 0.1 mM or more, more preferably 0.2 mM or more, and even more preferably 0.3 mM or more, from the viewpoint of improving polishing speed and uniformity of polishing within the surface, and preferably 10 mM or less, more preferably 5 mM or less, and even more preferably 3 mM or less, from the viewpoint of formulation stability. More specifically, the content of component B in the polishing liquid composition of this disclosure is preferably 0.1 mM or more and 10 mM or less, more preferably 0.2 mM or more and 5 mM or less, and even more preferably 0.3 mM or more and 3 mM or less. When component B is a combination of two or more types, the content of component B refers to the total content of those types.
[0027] [Aqueous medium] Examples of aqueous media included in the polishing fluid composition of this disclosure include water such as distilled water, ion-exchanged water, pure water, and ultrapure water, or a mixed solvent of water and a solvent. Examples of the solvent include solvents that can be mixed with water (for example, alcohols such as ethanol). When the aqueous media is a mixed solvent of water and a solvent, the proportion of water to the total mixed media is not particularly limited as long as the effects of this disclosure are not hindered. From an economic standpoint, for example, 95% by mass or more is preferred, 98% by mass or more is more preferred, and less than 100% by mass is preferred. From the viewpoint of surface cleanliness of the substrate to be polished, water is preferred as the aqueous media, ion-exchanged water and ultrapure water are more preferred, and ultrapure water is even more preferred. The content of the aqueous medium in the polishing fluid composition of this disclosure may be the remainder after excluding component A, component B, and any optional components described later that may be added as needed.
[0028] [Optional ingredients] The polishing liquid composition of this disclosure may further contain any components such as pH adjusters, surfactants, thickeners, dispersants, rust inhibitors, preservatives, basic substances, polishing speed enhancers, silicon nitride film polishing inhibitors, and polysilicon film polishing inhibitors.
[0029] In one or more embodiments, the polishing fluid compositions of the present disclosure substantially do not contain colloidal silica whose surface exhibits a positive zeta potential. For example, the content of colloidal silica in the polishing fluid compositions of the present disclosure is preferably less than 1% by mass, more preferably 0.1% by mass or less, even more preferably 0.01% by mass or less, and even more preferably 0% by mass (i.e., not present). In one or more embodiments, the polishing fluid compositions of the present disclosure are substantially free of corrosion inhibitors. For example, the content of the corrosion inhibitor in the polishing fluid compositions of the present disclosure is preferably less than 0.01% by mass, more preferably 0% by mass (i.e., none). In one or more embodiments, the polishing fluid compositions of the present disclosure are substantially free of cationic surfactants. For example, the amount of the surfactant in the polishing fluid compositions of the present disclosure is preferably less than 0.001 g, more preferably 0 g (i.e., not present) per liter of polishing fluid.
[0030] [Polishing liquid composition] The polishing fluid composition of this disclosure can be manufactured by a manufacturing method comprising the steps of blending component A, component B, an aqueous medium, and optionally any other components in a known manner. For example, the polishing fluid composition of this disclosure may consist of a dispersion (slurry) containing component A and an aqueous medium, a solution containing component B and an aqueous medium, and optionally any other components. In this disclosure, "blending" includes mixing component A, component B, an aqueous medium, and optionally any other components simultaneously or sequentially. The order of mixing is not particularly limited. The blending can be carried out, for example, using a mixer such as a homomixer, homogenizer, ultrasonic disperser, and wet ball mill. The amount of each component blended in the manufacturing method of the polishing fluid composition of this disclosure may be the same as the content of each component in the polishing fluid composition of this disclosure described above.
[0031] Embodiments of the polishing fluid composition of this disclosure may be a so-called one-component type, where all components are pre-mixed and supplied to the market, or a so-called two-component type, where the components are mixed at the time of use. For example, in one or more embodiments, a two-component polishing fluid composition may consist of a first liquid containing component A and a second liquid containing component B, where the first and second liquids are mixed at the time of use. The mixing of the first and second liquids may be performed before supplying them to the surface to be polished, or they may be supplied separately and mixed on the surface of the substrate to be polished. The first and second liquids may each contain the above-mentioned optional components as needed.
[0032] The pH of the polishing liquid composition of this disclosure is preferably greater than 3.5, more preferably 4 or greater, from the viewpoint of achieving both improved polishing speed of the silicon oxide film and improved in-plane uniformity of polishing, and similarly, preferably 7.5 or less, more preferably 6.5 or less, even more preferably 5.5 or less, and still more preferably 5 or less. More specifically, the pH of the polishing liquid composition of this disclosure is preferably greater than 3.5 and 7.5 or less, more preferably 4 or more and 6.5 or less, even more preferably 4 or more and 5.5 or less, and still more preferably 4 or more and 5 or less. In this disclosure, the pH of the polishing liquid composition is the value at 25°C and is the value measured using a pH meter. Specifically, the pH of the polishing liquid composition of this disclosure can be measured by the method described in the examples.
[0033] In this disclosure, "content of each component in the polishing liquid composition" means the content of each component at the time of polishing, that is, at the time when the polishing liquid composition is first used for polishing. The content of each component in the polishing liquid composition of this disclosure can be considered, in one or more embodiments, as the amount of each component blended in the polishing liquid composition of this disclosure. The polishing fluid composition of this disclosure may be stored and supplied in a concentrated state, provided that its stability is not compromised. This is preferable because it reduces manufacturing and transportation costs. This concentrated solution can then be used in the polishing process after being appropriately diluted with the aforementioned aqueous medium as needed. A dilution ratio of 5 to 100 times is preferred.
[0034] [Polishing solution kit] In one embodiment, this disclosure relates to a kit for preparing the polishing fluid composition of this disclosure (hereinafter also referred to as the "polishing fluid kit of this disclosure"). An example of a polishing fluid kit according to this disclosure is a polishing fluid kit (two-component polishing fluid composition) which contains, for example, an abrasive dispersion (first liquid) containing component A and an aqueous medium, and an additive aqueous solution (second liquid) containing component B, in an unmixed state, and which is mixed at the time of use and diluted with an aqueous medium as necessary. The aqueous medium contained in the abrasive dispersion (first liquid) may be the entire amount or a part of the aqueous medium used to prepare the polishing fluid composition. The additive aqueous solution (second liquid) may contain a part of the aqueous medium used to prepare the polishing fluid composition. The abrasive dispersion (first liquid) and the additive aqueous solution (second liquid) may each contain the above-mentioned optional components as necessary. The mixing of the abrasive dispersion (first liquid) and the additive aqueous solution (second liquid) may be performed before supplying them to the surface to be polished, or they may be supplied separately and mixed on the surface of the substrate to be polished. According to the polishing fluid kit of this disclosure, a polishing fluid composition that can achieve both improved polishing speed of silicon oxide film and improved in-plane uniformity of polishing can be obtained.
[0035] [Polishing method] This disclosure relates to a polishing method (hereinafter also referred to as the polishing method of this disclosure) that, in one embodiment, includes the step of polishing a film to be polished using the polishing liquid composition of this disclosure, wherein the film to be polished is a silicon oxide film formed in the manufacturing process of a semiconductor substrate. Examples of the film to be polished include the film to be polished in the polishing liquid composition of this disclosure as described above. For example, in one or more embodiments, the film to be polished in the polishing method of this disclosure is a silicon oxide film protrusion on the substrate surface after extra etching. In one or more embodiments, the polishing method of this disclosure includes the step of polishing a substrate to be polished using the polishing liquid composition of this disclosure. Examples of the substrate to be polished include a substrate after extra etching and a substrate having a silicon oxide film protrusion. By using the polishing method of this disclosure, it is possible to achieve both an improved polishing speed of the silicon oxide film and improved in-plane uniformity of polishing, thereby improving the productivity of high-quality semiconductor substrates. The polishing method and conditions in the polishing method of this disclosure can be the same as those for the semiconductor substrate manufacturing method of this disclosure described later.
[0036] [Manufacturing method for semiconductor substrates] This disclosure relates to a method for manufacturing a semiconductor substrate (hereinafter also referred to as "the semiconductor substrate manufacturing method of this disclosure") which, in one embodiment, includes a step of polishing a film to be polished using the polishing liquid composition of this disclosure (polishing step). Examples of the film to be polished include the film to be polished in the polishing liquid composition of this disclosure as described above. For example, in one or more embodiments, the film to be polished in the semiconductor substrate manufacturing method of this disclosure is the silicon oxide film protrusion on the substrate surface after extra etching. The semiconductor substrate manufacturing method of this disclosure includes, in one or more embodiments, a step of polishing a substrate to be polished using the polishing liquid composition of this disclosure. Examples of the substrate to be polished include, in one or more embodiments, a substrate after extra etching, a substrate having silicon oxide film protrusions, etc. According to the semiconductor substrate manufacturing method of this disclosure, it is possible to achieve both an improvement in the polishing speed of the silicon oxide film and an improvement in the in-plane uniformity of polishing, so that a semiconductor substrate of improved quality can be efficiently manufactured.
[0037] As a specific example of the semiconductor substrate manufacturing method of this disclosure, first, a silicon dioxide film is alternately laminated on a silicon substrate, and then a silicon nitride (Si3N4) film is alternately laminated on the silicon dioxide layer. Subsequently, channels are formed using polysilicon, the laminated films are trimmed, a charge trap layer is formed, and a tungsten (W) gate is formed to create an array. Then, silicon dioxide layers are laminated on the array by CVD (chemical vapor deposition) or the like. The silicon dioxide film thus formed has a large step difference between the array portion and the peripheral portion. Next, the silicon dioxide film in the array portion is polished by CMP until it is the same height as the peripheral portion. As shown in Figure 1, a method has been proposed in which the protrusions are refined, the CMP efficiency is improved, and the polishing time is shortened by performing an extra-etching process before CMP. The polishing liquid compositions of this disclosure can be suitably used in one or more embodiments for polishing substrates having silicon oxide film protrusions after extra etching. In one or more embodiments, the silicon oxide film protrusions are protrusions of the silicon oxide film on the substrate surface, and examples include protrusions with a width of 10 μm to 500 μm and a height of 4 μm to 10 μm.
[0038] In polishing by CMP, the surface of the substrate to be polished and the polishing pad are in contact, and the polishing liquid composition of this disclosure is supplied to these contact areas while the substrate and the polishing pad are moved relative to each other, thereby flattening the uneven surface of the substrate to be polished.
[0039] In the polishing process, the rotation speed of the polishing pad is, for example, 30 to 200 rpm / min, the rotation speed of the substrate to be polished is, for example, 30 to 200 rpm / min, and the polishing load set on the polishing apparatus equipped with the polishing pad is, for example, 20 to 500 g-force / cm². 2 The supply rate of the polishing solution composition can be set to, for example, 10 to 500 mL / min or less. If the polishing solution composition is a two-component polishing solution composition, the polishing speed of the film to be polished can be adjusted by adjusting the supply rate (or supply amount) of the first liquid and the second liquid, respectively.
[0040] In the polishing process described above, the polishing speed of the film to be polished (silicon oxide film) is preferably 50 nm / min or more, more preferably 80 nm / min or more, and even more preferably 90 nm / min or more, from the viewpoint of improving productivity. [Examples]
[0041] The present disclosure will be specifically described below with reference to examples, but the present disclosure is not limited in any way by these examples.
[0042] 1. Preparation of polishing solution composition [Preparation of polishing solution compositions for Examples 1-2 and Comparative Examples 1-3] Abrasive compositions for Examples 1-2 and Comparative Examples 1-3 were obtained by mixing cerium oxide particles (component A), the compounds shown in Table 1 (component B or non-component B), and water. The amount (content) (mass % or mM, effective content) of each component in the abrasive composition is shown in Table 2, and the water content is the residue after removing component A and component B or non-component B. pH adjustment was performed using ammonia or nitric acid.
[0043] The following were used for component A, component B, and non-component B. (Component A) Calcined and ground ceria [Average primary particle size: 45 nm, BET specific surface area: 17 m²] 2 / g, surface potential: 70mV] (Component B) B1: Ethoxyacetic acid (manufactured by Tokyo Chemical Industry Co., Ltd.) [In formula (I), R = C2H5 and M = H.] B2: Methoxyacetic acid (manufactured by Tokyo Chemical Industry Co., Ltd.) [In formula (I), R = CH3 and M = H.] (Non-ingredient B) B3: Acetic acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) B4: Glycolic acid (manufactured by Tokyo Chemical Industry Co., Ltd.) B5: Butyric acid (manufactured by Tokyo Chemical Industry Co., Ltd.)
[0044] [Table 1]
[0045] 2. Measurement methods for various parameters [Average primary particle size of cerium oxide particles (component A)] The average primary particle size (nm) of cerium oxide particles is calculated using the specific surface area S(m²) of the BET (nitrogen adsorption) method. 2 This refers to the particle size (converted to a perfect sphere) calculated using the following formula ( / g), and is calculated using the formula below. In the formula below, the specific surface area S was determined by crushing 10 g of cerium oxide particle slurry in an agate mortar after removing moisture by vacuum drying at 110°C, and then measuring the resulting powder using a flow-type automatic specific surface area measuring device, FlowSorb 2300 (manufactured by Shimadzu Corporation). Average primary particle diameter (nm)=820 / S
[0046] [Surface potential of cerium oxide (component A)] The surface potential (mV) of cerium oxide particles was measured using a surface potential measuring device (Zeta Probe, manufactured by Kyowa Interface Chemical Co., Ltd.). Ultrapure water was used to adjust the cerium oxide concentration to 0.3%, which was then placed in the surface potential measuring device. The surface potential was measured under conditions of a particle density of 7.13 g / ml and a particle dielectric constant of 7. Three measurements were performed, and the average value was used as the measurement result.
[0047] [pH of the polishing solution composition] The pH value of the polishing solution composition at 25°C was measured using a pH meter (Toa Denpa Kogyo Co., Ltd., HM-30G), and the value was obtained 1 minute after immersion of the electrode in the polishing solution composition. The results are shown in Table 2.
[0048] 3. Evaluation of polishing liquid compositions (Examples 1-2 and Comparative Examples 1-3) [Evaluation sample] A silicon wafer with a 2000 nm thick silicon oxide film (blanket film) formed on one side using the TEOS-plasma CVD method was used as the evaluation sample (substrate to be polished).
[0049] [Polishing conditions] Polishing equipment: Single-sided polishing machine [Ebara Corporation, FREX-200] Polishing pad: Hard urethane pad "IC-1000 / Suba400" [manufactured by Nitta Haas Co., Ltd.] Plate rotation speed: 100 rpm Head rotation speed: 107 rpm Grinding load: 280 hPa Polishing liquid supply amount: 200mL / min Polishing time: 1 minute
[0050] [Polishing speed] The evaluation samples were polished under the above polishing conditions using the polishing solution compositions of Examples 1-2 and Comparative Examples 1 and 3. Comparative Example 2 could not be tested due to the aggregation of ceria particles. The thickness of the silicon oxide film before and after polishing was measured using ASET-F5X (manufactured by KLA). The thickness was measured at 4mm intervals from the edge to the center of the wafer, excluding the 3mm portion at the edge, for a total of 47 measurement points. The polishing speed of the silicon oxide film (film to be polished) was calculated as the average of the above 47 points using the following formula, and the results are shown in Table 2. Polishing speed = [Silicon oxide film thickness before polishing (nm) - Silicon oxide film thickness after polishing (nm)] / Polishing time (minutes)
[0051] [In-plane uniformity] WIWNU, an indicator of in-plane uniformity, was calculated using the following formula, and the results are shown in Table 2. WIWNU(%) = [Standard deviation of silicon oxide film polishing rate × 100] / Silicon oxide film polishing rate (nm / min) The results show that the larger the polishing speed deviation at the 47 film thickness measurement points on the wafer surface and the smaller the average polishing speed, the larger the WIWNU value. Conversely, wafers with a small polishing speed deviation and a large average polishing speed have a smaller WIWNU value and superior in-plane uniformity.
[0052] [Table 2]
[0053] As shown in Table 2, the polishing liquid compositions of Examples 1 and 2 were found to achieve both improved polishing speed and improved in-plane uniformity of the silicon oxide film compared to Comparative Examples 1 and 3. The polishing liquid composition of Comparative Example 2 could not be evaluated due to the formation of sediment. [Industrial applicability]
[0054] The polishing liquid composition relating to this disclosure is useful in a method for manufacturing semiconductor devices for high density or high integration.
Claims
1. A polishing liquid composition for polishing a substrate after extra etching, A polishing solution composition for silicon oxide films, comprising cerium oxide particles (component A), at least one selected from methoxyacetic acid or a salt thereof, and ethoxyacetic acid or a salt thereof (component B), and an aqueous medium.
2. The polishing liquid composition according to claim 1, wherein the content of component A is 0.1% by mass or more and 10% by mass or less.
3. The polishing liquid composition according to claim 1 or 2, wherein the content of component B is 0.1 mM or more and 10 mM or less.
4. The polishing liquid composition according to claim 1 or 2, wherein component B is ethoxyacetic acid or a salt thereof.
5. The polishing liquid composition according to claim 1 or 2, wherein component A is amorphous ceria.
6. The polishing liquid composition according to claim 1 or 2, wherein the average primary particle size of component A is 40 nm or more and 60 nm or less.
7. The polishing liquid composition according to claim 1 or 2, wherein the pH of the polishing liquid composition is greater than 3.5 and less than or equal to 7.
5.
8. The process includes polishing a substrate to be polished using the polishing liquid composition described in claim 1 or 2, A method for manufacturing a semiconductor substrate, wherein the substrate to be polished is a substrate after extra etching.
9. A polishing method comprising the step of polishing a substrate to be polished using the polishing liquid composition described in claim 1 or 2, wherein the substrate to be polished is a substrate after extra etching.
Citation Information
Patent Citations
Composition for oxide cmp
JP2001507739A
Polishing solution
JP2008181954A
Polishing solution and polishing method
JP2010067681A
Method for manufacturing cerium dioxide nanoparticles
JP2014139127A
Polishing liquid and substrate polishing method using the same
JP2015008212A