Bonded substrate, and method for manufacturing a bonded substrate

By using silicon oxide intermediate layers with modified layers of 1.8 nm or more on quartz and lithium tantalate or lithium niobate substrates, the bonding strength is improved, addressing void issues and ensuring a stable substrate for surface acoustic wave elements.

JP7948848B2Active Publication Date: 2026-11-11THE JAPAN STEEL WORKS LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023007312
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-01-20
Publication Date
2026-11-11
Estimated Expiration
2043-01-20

AI Technical Summary

Technical Problem

The bonding of quartz and lithium tantalate or lithium niobate substrates in surface acoustic wave elements can result in voids or reduced bonding strength due to varying bonding conditions.

Method used

A bonded substrate is formed by bonding a quartz substrate with a lithium tantalate or lithium niobate substrate using silicon oxide intermediate layers, with modified layers on each substrate surface, where the thickness of these modified layers is set to 1.8 nm or more, achieved through plasma treatment and annealing.

Benefits of technology

This method enhances bonding strength while minimizing void formation, ensuring a stable and robust substrate for surface acoustic wave elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007948848000001
    Figure 0007948848000001
  • Figure 0007948848000002
    Figure 0007948848000002
  • Figure 0007948848000003
    Figure 0007948848000003
Patent Text Reader

Abstract

To provide a bonded substrate with high bonding strength while suppressing void generation.SOLUTION: A bonded substrate 1 in an aspect of the present disclosure is a bonded substrate in which a first substrate 10 and a second substrate 20 are bonded together via a bonding surface 15. The first substrate 10 is a quartz substrate, and the second substrate 20 is a lithium tantalate or lithium niobate substrate. Intermediate layers 11 and 21 made of silicon oxide are formed on the bonding surface 15 side of at least one of the first substrate 10 and the second substrate 20. A first modification layer 12 is formed on the bonding surface 15 side of the first substrate, and the second modification layer 22 is formed on the bonding surface 15 side of the second substrate 20, and a thickness of the modified layers 12 and 22 on the intermediate layers 11 and 21 of the first and second modified layers 12 and 22 is at least 1.8 nm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present disclosure relates to a bonded substrate and a method for manufacturing the bonded substrate.

BACKGROUND ART

[0002] With the evolution of mobile communication devices such as mobile phones, higher performance is also required for Surface Acoustic Wave (SAW) filters. Surface acoustic wave elements constituting SAW filters are required to, for example, achieve a wider bandwidth by improving the electromechanical coupling coefficient, and reduce the absolute value of the Temperature Coefficient of Frequency (TCF). Patent Document 1 discloses a technique related to a surface acoustic wave element.

PRIOR ART DOCUMENTS

PATENT DOCUMENTS

[0003]

PATENT DOCUMENT 1

SUMMARY OF THE INVENTION

PROBLEMS TO BE SOLVED BY THE INVENTION

[0004] For example, when manufacturing a surface acoustic wave element, a bonded substrate obtained by bonding a first substrate made of a quartz substrate and a second substrate made of a lithium tantalate substrate or a lithium niobate substrate is used. However, depending on the bonding conditions of these substrates, voids may be generated at the bonding interface between the first substrate and the second substrate, or the bonding strength between these substrates may be reduced. Other problems and novel features will become apparent from the description of the present specification and the accompanying drawings.

MEANS FOR SOLVING THE PROBLEMS

[0005] A bonded substrate according to one aspect of the present disclosure is a bonded substrate in which a first substrate and a second substrate are bonded via a bonding surface. The first substrate is a quartz substrate, and the second substrate is a lithium tantalate substrate or a lithium niobate substrate. An intermediate layer made of silicon oxide is formed on the bonding surface side of at least one of the first substrate and the second substrate, a first modified layer is formed on the bonding surface side of the first substrate, and a second modified layer is formed on the bonding surface side of the second substrate, and the thickness of the modified layer formed on the intermediate layer among the first modified layer and the second modified layer is 1.8 nm or more.

[0006] A method for manufacturing a bonded substrate according to one aspect of the present disclosure is a method for manufacturing a bonded substrate in which a first substrate, a quartz substrate, and a second substrate, a lithium tantalate substrate or a lithium niobate substrate, are joined via a bonding surface, comprising: a first step of forming an intermediate layer made of silicon oxide on at least one of the bonding surface sides of the first substrate and the second substrate; a second step of plasma treatment of the bonding surface side of the first substrate to form a first modified layer; a third step of plasma treatment of the bonding surface side of the second substrate to form a second modified layer; a fourth step of temporarily bonding the first substrate and the second substrate with the first modified layer and the second modified layer facing each other; and a fifth step of annealing the substrates after temporary bonding to bond the first substrate and the second substrate, wherein the thickness of the modified layer formed on the intermediate layer, among the first modified layer and the second modified layer, is 1.8 nm or more. [Effects of the Invention]

[0007] This disclosure provides a bonded substrate with high bonding strength while suppressing the generation of voids, and a method for manufacturing a bonded substrate. [Brief explanation of the drawing]

[0008] [Figure 1] This is a cross-sectional view showing an example of the configuration of a bonded substrate according to an embodiment. [Figure 2] This is a cross-sectional view showing an example of the configuration of a bonded substrate according to the embodiment (Example 2). [Figure 3]This is a cross-sectional view showing an example of a bonded substrate configuration 3 according to the embodiment. [Figure 4] This is a flowchart illustrating the manufacturing method of the bonded substrate according to the embodiment. [Figure 5] This is a schematic diagram illustrating the manufacturing method of a bonded substrate according to an embodiment. [Figure 6] This is a schematic diagram illustrating the manufacturing method of a bonded substrate according to an embodiment. [Figure 7] This graph shows the relationship between the type of film in the intermediate layer (silicon oxide) and the thickness of the modified layer. [Figure 8] This graph shows the relationship between the type of film in the intermediate layer (silicon oxide) and the bonding strength. [Figure 9] This graph shows the relationship between the thickness of the modified layer and the bonding strength. [Modes for carrying out the invention]

[0009] The embodiments will be described below with reference to the drawings. Figure 1 is a cross-sectional view showing an example of the configuration 1 of a bonded substrate according to an embodiment. In Figure 1, the upper figure shows the substrate before bonding, and the lower figure shows the bonded substrate after bonding. As shown in Figure 1, the bonded substrate 1 according to this embodiment is a bonded substrate in which a first substrate 10 and a second substrate 20 are bonded via a bonding surface 15. Here, the first substrate 10 functions as a support substrate, and the second substrate 20 functions as a piezoelectric element.

[0010] In this embodiment, the first substrate 10 is a quartz substrate. The second substrate 20 is a lithium tantalate substrate or a lithium niobate substrate. By using a quartz substrate as the first substrate 10 (support substrate), the temperature characteristics of the frequency of the surface acoustic wave element can be improved. Furthermore, the lithium tantalate substrate or lithium niobate substrate, which is the second substrate 20, has a high elastic wave propagation speed and a large electromechanical coupling coefficient. Therefore, by using a lithium tantalate substrate or lithium niobate substrate as the second substrate 20 (piezoelectric element), a broadband surface acoustic wave element can be achieved.

[0011] A first intermediate layer 11 and a second intermediate layer 21 are formed as intermediate layers on the bonding surface 15 side of the first substrate 10 and the second substrate 20, respectively. The first intermediate layer 11 and the second intermediate layer 21 are both intermediate layers made of silicon oxide. The first intermediate layer 11 and the second intermediate layer 21 can be formed using, for example, thermal oxidation, sputtering, physical vapor deposition, CVD, etc. In particular, it is preferable to form the first intermediate layer 11 and the second intermediate layer 21 made of silicon oxide using a film formation method that yields a dense film. The thickness of the first intermediate layer 11 and the second intermediate layer 21 can be 50 nm or more and 10 μm or less. In this specification, the first intermediate layer 11 and the second intermediate layer 21 are collectively referred to as intermediate layer 11 and 21.

[0012] Furthermore, the first substrate 10 is provided with a first modified layer 12 on the bonding surface 15 side. The second substrate 20 is provided with a second modified layer 22 on the bonding surface 15 side. That is, the first modified layer 12 is formed on the bonding surface 15 side of the first intermediate layer 11 formed on the first substrate 10. The second modified layer 12 is formed on the bonding surface 15 side of the second intermediate layer 21 formed on the second substrate 20. In this specification, the first modified layer 12 and the second modified layer 22 are collectively referred to as modified layers 12 and 22.

[0013] In this embodiment, the thickness of the first modified layer 12 and the second modified layer 22 is 1.8 nm or more, preferably 1.8 nm to 2.2 nm. In this embodiment, the first modified layer 12 and the second modified layer 22 are amorphous layers produced by modifying the substrate surface, and can be formed by plasma treatment, ion irradiation, etc. In other words, the first modified layer 12 and the second modified layer 22 are amorphous layers mainly composed of silicon oxide that constitutes the first intermediate layer 11 and the second intermediate layer 21. To put it another way, the first modified layer 12 and the second modified layer 22 are layers made of amorphous silicon oxide.

[0014] Here, the thicknesses of the first modified layer 12 and the second modified layer 22 may differ even when conditions such as plasma treatment for forming the modified layers are the same, if the film formation methods for the underlying first intermediate layer 11 and second intermediate layer 21 (in other words, the film qualities of the first intermediate layer 11 and the second intermediate layer 21) are different. For this reason, in the present embodiment, the conditions such as plasma treatment for forming the first modified layer 12 and the second modified layer 22 are respectively modified and optimized in accordance with the film formation methods for the first intermediate layer 11 and the second intermediate layer 21 (in other words, the film qualities of the first intermediate layer 11 and the second intermediate layer 21). Thereby, the thicknesses of the first modified layer 12 and the second modified layer 22 can be set to 1.8 nm or more, preferably 1.8 nm or more and 2.2 nm or less. Accordingly, it is possible to form a bonded substrate with high bonding strength while suppressing the generation of voids.

[0015] Next, Configuration Example 2 of the bonded substrate according to the present embodiment will be described. Figure 2 is a cross-sectional view showing Configuration Example 2 of the bonded substrate according to the embodiment. The bonded substrate 2 according to Configuration Example 2 shown in Figure 2 differs from the bonded substrate 1 according to Configuration Example 1 described with reference to Figure 1 in that the first substrate 10 does not include the first intermediate layer 11. The remaining configuration is the same as that of the bonded substrate 1 according to Configuration Example 1 described with reference to Figure 1.

[0016] As shown in Figure 2, the bonded substrate 2 according to Configuration Example 2 is a bonded substrate in which the first substrate 10 and the second substrate 20 are bonded via a bonding surface 15. A second intermediate layer 21 is formed on the second substrate 20. The first modified layer 12 is formed on the surface of the first substrate 10 on the bonding surface 15 side. The second modified layer 22 is formed on the surface of the second intermediate layer 21 formed on the second substrate 20 on the bonding surface 15 side.

[0017] And in the bonded substrate 2 according to Configuration Example 2, the thickness of the first modified layer 12 formed on the bonding surface 15 side of the first substrate 10 is set to 2.7 nm or more and 3.2 nm or less. Further, the thickness of the second modified layer 22 formed on the second intermediate layer 21 is set to 1.8 nm or more, preferably 1.8 nm or more and 2.2 nm or less.

[0018] Also in the present embodiment, the conditions such as the plasma treatment for forming the second modified layer 22 are respectively changed and optimized according to the film formation method of the second intermediate layer 21 (in other words, the film quality of the second intermediate layer 21). Thereby, the thickness of the second modified layer 22 can be set to 1.8 nm or more, preferably 1.8 nm or more and 2.2 nm or less. In addition, when forming the first modified layer 12 on the bonding surface 15 side of the first substrate 10, the thickness of the first modified layer 12 is set to 2.7 nm or more and 3.2 nm or less by optimizing the conditions such as plasma treatment. Therefore, it is possible to form a bonded substrate with high bonding strength while suppressing the occurrence of voids.

[0019] Next, Configuration Example 3 of the bonded substrate according to the present embodiment will be described. Figure 3 is a cross-sectional view showing Configuration Example 3 of the bonded substrate according to the embodiment. The bonded substrate 3 according to Configuration Example 3 shown in Figure 3 differs from the bonded substrate 1 according to Configuration Example 1 described with reference to Figure 1 in that the second substrate 20 does not include the second intermediate layer 21. The other configurations are the same as those of the bonded substrate 1 according to Configuration Example 1 described with reference to Figure 1.

[0020] As shown in Figure 3, the bonded substrate 3 according to Configuration Example 3 is a bonded substrate in which the first substrate 10 and the second substrate 20 are bonded via the bonding surface 15. A first intermediate layer 11 is formed on the first substrate 10. The first modified layer 12 is formed on the surface of the first intermediate layer 11 formed on the first substrate 10 on the bonding surface 15 side. The second modified layer 22 is formed on the surface of the second substrate 20 on the bonding surface 15 side.

[0021] In the bonded substrate 3 according to Configuration Example 3, the thickness of the first modified layer 12 formed on the first intermediate layer 11 is set to 1.8 nm or more, preferably 1.8 nm or more and 2.2 nm or less. In addition, the thickness of the second modified layer 22 formed on the bonding surface 15 side of the second substrate 20 is set to 2.2 nm or more and 2.7 nm or less.

[0022] In this embodiment as well, the conditions for plasma treatment and other processes when forming the first modified layer 12 are changed and optimized according to the film formation method of the first intermediate layer 11 (in other words, the film quality of the first intermediate layer 11). This makes it possible to set the thickness of the first modified layer 12 to 1.8 nm or more, preferably 1.8 nm to 2.2 nm. Furthermore, when forming the second modified layer 22 on the bonding surface 15 side of the second substrate 20, the thickness of the second modified layer 22 is set to 2.2 nm to 2.7 nm by optimizing the conditions for plasma treatment and other processes. Therefore, it is possible to form a bonded substrate with high bonding strength while suppressing the generation of voids.

[0023] In the bonded substrates 1 to 3 described in the above-mentioned configuration examples 1 to 3, the thickness of the first substrate 10 is 100 μm or more and 1000 μm or less, and the thickness of the second substrate is 10 μm or more and 1000 μm or less. Furthermore, after bonding the first substrate 10 and the second substrate 20, the surface of the second substrate 20 may be polished. For example, the second substrate 20 may be polished so that its thickness is 10 μm or less.

[0024] Next, a method for manufacturing a bonded substrate according to this embodiment will be described. Figure 4 is a flowchart illustrating the method for manufacturing a bonded substrate according to this embodiment. Figures 5 and 6 are schematic diagrams illustrating the method for manufacturing a bonded substrate according to this embodiment. Below, as an example, the manufacturing method for the bonded substrate 1 according to Configuration Example 1 (i.e., a configuration in which both the first substrate 10 and the second substrate 20 are provided with intermediate layers 11 and 21) will be described, but the bonded substrate 2 according to Configuration Example 2 and the bonded substrate 3 according to Configuration Example 3 can also be manufactured using the same manufacturing method.

[0025] When manufacturing the bonded substrate 1 according to this embodiment, first, a first substrate 10 (quartz substrate) is prepared as shown in Figures 4 and 5 (Step S1). For example, the thickness of the first substrate 10 (quartz substrate) is 100 μm or more and 1000 μm or less. Next, a silicon oxide (SiO2) layer, which is the first intermediate layer 11, is deposited on the surface of the first substrate 10 (Step S2). The first intermediate layer 11 can be formed using, for example, thermal oxidation, sputtering, physical vapor deposition, CVD, etc. In particular, it is preferable to form the first intermediate layer 11 using a film deposition method that yields a dense film. The thickness of the first intermediate layer 11 can be 50 nm or more and 10 μm or less. After that, the deposited first intermediate layer 11 is polished (Step S3). By polishing the surface of the first intermediate layer 11 in this way, the surface of the first intermediate layer 11 can be made flat.

[0026] Next, the polished first substrate 10 is cleaned (step S4). For example, the polished first substrate 10 is cleaned using a chemical solution such as APM (Ammonia hydrogen Peroxide Mixture) or SPM (sulfuric acid-hydrogen peroxide mixture). Next, the surface of the first substrate 10 facing the first intermediate layer 11 is plasma treated (step S5). By plasma treating the surface of the first substrate 10 facing the first intermediate layer 11, a first modified layer 12 can be formed on the surface of the first substrate 10 (first intermediate layer 11). The thickness of the first modified layer 12 formed on the surface of the first substrate 10 (first intermediate layer 11) is 1.8 nm or more, preferably 1.8 nm or more and 2.2 nm or less.

[0027] In this embodiment, by performing plasma treatment on the first substrate 10 under conditions where plasma emission is stable (conditions where the variation in plasma emission is small), the variation in the in-plane film thickness of the first modified layer 12 formed on the surface of the first substrate 10 (first intermediate layer 11) can be reduced. The variation in plasma emission can be reduced by adjusting the pressure in the chamber of the plasma processing apparatus and the plasma output (RF output).

[0028] Next, a second substrate 20 (lithium tantalate substrate or lithium niobate substrate) is prepared (step S6). For example, the thickness of the second substrate 20 is 100 μm or more and 1000 μm or less. Next, a silicon oxide (SiO2) layer, which is the second intermediate layer 21, is deposited on the surface of the second substrate 20 (step S7). The second intermediate layer 21 can be formed using, for example, thermal oxidation, sputtering, physical vapor deposition, CVD, etc. In particular, it is preferable to form the second intermediate layer 21 using a deposition method that yields a dense film. The thickness of the second intermediate layer 21 can be 50 nm or more and 10 μm or less. After that, the deposited second intermediate layer 21 is polished (step S8). By polishing the surface of the second intermediate layer 21 in this way, the surface of the second intermediate layer 21 can be made flat.

[0029] Next, the polished second substrate 20 is cleaned (step S9). For example, the polished second substrate 20 is cleaned using a chemical solution such as APM or SPM. Next, the surface of the second substrate 20 facing the second intermediate layer 21 is plasma treated (step S10). By plasma treating the surface of the second substrate 20 facing the second intermediate layer 21, a second modified layer 22 can be formed on the surface of the second substrate 20 (second intermediate layer 21). The thickness of the second modified layer 22 formed on the surface of the second substrate 20 (second intermediate layer 21) is 1.8 nm or more, preferably 1.8 nm or more and 2.2 nm or less.

[0030] In this embodiment, by performing plasma treatment on the second substrate 20 under conditions where plasma emission is stable (conditions where the variation in plasma emission is small), the variation in the in-plane film thickness of the second modified layer 22 formed on the surface of the second substrate 20 (second intermediate layer 21) can be reduced. The variation in plasma emission can be reduced by adjusting the pressure in the chamber of the plasma processing apparatus and the plasma output (RF output).

[0031] Note that the order of the processes in steps S1-S5 and steps S6-S10 may be reversed. In other words, steps S6-S10 may be performed first, followed by steps S1-S5. Also, steps S1-S5 and steps S6-S10 may be performed in parallel (simultaneously).

[0032] Next, with the first modified layer 12 of the first substrate 10 and the second modified layer 22 of the second substrate 20 facing each other, the first substrate 10 and the second substrate 20 are temporarily joined (step S11). For example, after adjusting the in-plane position (horizontal position) of the first substrate 10 and the second substrate 20, the first substrate 10 and the second substrate 20 are moved vertically to temporarily join them.

[0033] Subsequently, as shown in Figures 4 and 6, the substrates after temporary bonding are annealed to bond the first substrate 10 and the second substrate 20 (step S12). Annealing strengthens the bond between the first modified layer 12 of the first substrate 10 and the second modified layer 22 of the second substrate 20, thereby firmly bonding the first substrate 10 and the second substrate 20. For example, the annealing temperature is between 50°C and 300°C. Annealing can be performed, for example, by heating the substrates after temporary bonding in an electric furnace.

[0034] In this embodiment, after joining the first substrate 10 and the second substrate 20, the embodiment may further include a step (step S13) of polishing the surface of the second substrate 20. The polishing step can be carried out, for example, using chemical mechanical polishing (CMP). For example, the second substrate 20 may be polished to a thickness of 10 μm or less.

[0035] By using the manufacturing method (substrate bonding method) described above, the bonded substrate according to this embodiment can be manufactured.

[0036] In this embodiment, the thickness of the first modified layer 12 of the first substrate 10 and the thickness of the second modified layer 22 of the second substrate 20 can be measured using a transmission electron microscope (TEM).

[0037] For example, by measuring the thickness of the first modified layer 12 and the second modified layer 22 using a transmission electron microscope, and changing the plasma treatment conditions according to the measured thickness of the first modified layer 12 and the second modified layer 22, it is possible to form the first modified layer 12 and the second modified layer 22 having the above-mentioned thickness range.

[0038] Furthermore, in this embodiment, the thickness of the first modified layer 12 and the second modified layer 22 of the bonded substrate 1 after bonding can be measured using a transmission electron microscope. In this embodiment, it is assumed that the relationship between the thicknesses of the first modified layer 12 and the second modified layer 22 remains unchanged before and after bonding the first substrate 10 and the second substrate 20.

[0039] When manufacturing the bonded substrate 2 according to Configuration Example 2 (i.e., a configuration in which only the second substrate 20 has an intermediate layer 21), steps S2 and S3 shown in Figures 4 and 5 are omitted. Similarly, when manufacturing the bonded substrate 3 according to Configuration Example 3 (i.e., a configuration in which only the first substrate 10 has an intermediate layer 11), steps S7 and S8 shown in Figures 4 and 5 are omitted. The other manufacturing steps are the same as those for the bonded substrate 1 according to Configuration Example 1.

[0040] Incidentally, the inventors of the present invention have found that the thickness of the first modified layer 12 and the second modified layer 22 differs depending on the type of film formed on the surface of the first substrate 10 and the second substrate 20, respectively. In other words, they have found that even when plasma treatment is performed under the same conditions, the thickness of the first modified layer 12 and the second modified layer 22 differs depending on the type of film formed on the first intermediate layer 11 and the second intermediate layer 21.

[0041] Figure 7 is a graph showing the relationship between the type of intermediate layer (silicon oxide) film and the thickness of the modified layer. Film types A to D shown in Figure 7 were formed using different vapor phase methods. Then, the intermediate layers (silicon oxide) of film types A to D were plasma-treated under the same conditions to form a modified layer, and the thickness of the modified layer was measured. As a result, even when plasma-treated under the same conditions, the thickness of the modified layer differed depending on the type of intermediate layer (silicon oxide). Specifically, the modified layer was thickest with film type D. The modified layer thickness was about the same for film types A and B. The modified layer was thinnest with film type C. There was a large difference of about 1.4 nm in the thickness of the modified layer between film type D and film type C.

[0042] Figure 8 is a graph showing the relationship between the type of intermediate layer (silicon oxide) and the bonding strength. Figure 8 shows the bonding strength when there is no intermediate layer (silicon oxide), when intermediate layer (silicon oxide) is of type B, when intermediate layer (silicon oxide) is of type C, and when intermediate layer (silicon oxide) is of type D. As shown in Figure 8, the bonding strength differs for the case without an intermediate layer (silicon oxide) and for each of the cases where intermediate layers (silicon oxide) are of types B to D.

[0043] Figure 9 is a graph showing the relationship between the thickness of the modified layer and the bonding strength. Figure 9 shows the relationship between the thickness of the modified layer formed in the intermediate layer of film types B to D and the bonding strength. As shown in Figure 9, there was a positive correlation between the thickness of the modified layer and the bonding strength. As shown in Figure 9, it was found that to obtain a bonding strength greater than 0.50, the thickness of the modified layer needs to be 1.8 nm or more.

[0044] In the bonded substrate according to this embodiment, by setting the thickness of the modified layer formed on the surface of the intermediate layer (silicon oxide) to 1.8 nm or more, it is possible to obtain a bonded substrate with high bonding strength while suppressing the generation of voids. Furthermore, by increasing the bonding strength of the bonded substrate, it is possible to suppress the delamination of the bonded substrate during the polishing process.

[0045] Specifically, in the bonded substrate 1 according to Configuration Example 1 shown in Figure 1, a first intermediate layer 11 and a second intermediate layer 21 are provided on both the first substrate 10 and the second substrate 20, respectively. Therefore, by setting the thickness of the first modified layer 12 and the second modified layer 22 formed on the surfaces of the first intermediate layer 11 and the second intermediate layer 21 to 1.8 nm or more, the bonding strength of the bonded substrate can be increased while suppressing the occurrence of voids. In other words, in the bonded substrate 1 according to Configuration Example 1 shown in Figure 1, intermediate layers (silicon oxide) 11 and 21 are formed on both the first substrate 10 and the second substrate 20, so the film thickness of the modified layers 12 and 22 formed on the surfaces of the intermediate layers (silicon oxide) 11 and 21 is set to 1.8 nm or more.

[0046] Furthermore, in the bonded substrate 2 according to Configuration Example 2 shown in Figure 2, a second intermediate layer 21 is provided on the second substrate 20. Therefore, by making the thickness of the second modified layer 22 formed on the surface of the second intermediate layer 21 1.8 nm or more, the bonding strength of the bonded substrate can be increased while suppressing the occurrence of voids. In other words, in the bonded substrate 2 according to Configuration Example 2 shown in Figure 2, since the intermediate layer (silicon oxide) 21 is formed only on the second substrate 20, the thickness of the modified layer 22 formed on the surface of the intermediate layer (silicon oxide) 21 of the second substrate 20 is set to 1.8 nm or more. At this time, the thickness of the first modified layer 12 formed on the bonding surface 15 side of the first substrate 10 is set to 2.7 nm or more and 3.2 nm or less.

[0047] Furthermore, in the bonded substrate 3 according to configuration example 3 shown in Figure 3, a first intermediate layer 11 is provided on the first substrate 10. Therefore, by making the thickness of the first modified layer 12 formed on the surface of the first intermediate layer 11 1.8 nm or more, the bonding strength of the bonded substrate can be increased while suppressing the occurrence of voids. In other words, in the bonded substrate 3 according to configuration example 3 shown in Figure 3, since the intermediate layer (silicon oxide) 11 is formed only on the first substrate 10, the thickness of the modified layer 12 formed on the surface of the intermediate layer (silicon oxide) 11 of the first substrate 10 is set to 1.8 nm or more. At this time, the thickness of the second modified layer 22 formed on the bonding surface 15 side of the second substrate 20 is set to 2.2 nm or more and 2.7 nm or less.

[0048] Furthermore, the film thickness of the modified layers 12 and 22 can be adjusted by changing the plasma treatment and other conditions according to the film type of the intermediate layers 11 and 21.

[0049] Furthermore, in this embodiment, by forming intermediate layers 11 and 21 on at least one surface of the first substrate 10 and the second substrate 20, the influence of the first substrate 10 and the second substrate 20, that is, the influence of the first substrate 10 and the second substrate 20 on the modified layers 12 and 22, can be canceled out. Therefore, the options for the first substrate 10 and the second substrate 20 can be expanded. In addition, by changing the conditions such as plasma treatment according to the film type of the intermediate layers 11 and 21, the film thickness of the modified layers 12 and 22 can be adjusted, making it easier to determine the conditions for obtaining the desired modified layers 12 and 22. [Examples]

[0050] Next, we will describe some examples.

[0051] <Sample Preparation> Each sample was fabricated using the method described in Figures 4 to 6. Specifically, a bonded substrate 2 according to Configuration Example 2 shown in Figure 2 (i.e., a configuration in which only the second substrate 20 has an intermediate layer 21) was fabricated. When fabricating the bonded substrate 2 according to Configuration Example 2, steps S2 and S3 shown in Figures 4 and 5 were omitted.

[0052] First, a quartz substrate with a thickness of 400 μm was prepared as the first substrate 10. Next, the quartz substrate was cleaned by immersing it in APM solution and washing it for 10 minutes.

[0053] Next, a quartz substrate was plasma-treated to form a modified layer with a thickness of 3.0 nm on its surface. The plasma treatment was performed by generating a capacitively coupled plasma under a reduced pressure atmosphere. The plasma treatment conditions were set to an RF output of 100 W, and the treatment time was adjusted to achieve a modified layer thickness of 3.0 nm.

[0054] Furthermore, a lithium tantalate substrate (LT substrate) with a thickness of 200 μm was prepared as the second substrate 20. Next, a silicon oxide (SiO2) layer, which is the intermediate layer (second intermediate layer), was deposited on the surface of the lithium tantalate substrate. Four different types of intermediate layers were formed. Film types A to D were formed using different vapor phase methods. Each sample with a different film type will be referred to as sample A to D from now on. The thickness of each intermediate layer was set to 800 nm. After that, the deposited intermediate layers were polished.

[0055] Next, the polished lithium tantalate substrate was cleaned by immersing it in an APM solution for 10 minutes. Then, the lithium tantalate substrate was plasma-treated to form a modified layer on the surface of the intermediate layer of the lithium tantalate substrate. The plasma treatment was performed by generating a capacitively coupled plasma under a reduced pressure atmosphere. The plasma treatment conditions were set to an RF output of 100W. The plasma treatment conditions were the same for samples A to D.

[0056] Next, the modified layers of the quartz substrate and the lithium tantalate substrate were brought into contact with each other while the modified layers of the quartz substrate and the lithium tantalate substrate were facing each other, thereby performing a preliminary bonding. After that, the substrates after the preliminary bonding were annealed at 150°C to bond the quartz substrate and the lithium tantalate substrate, forming a bonded substrate.

[0057] In addition, a sample without an intermediate layer (without an intermediate layer) was prepared separately on the surface of the lithium tantalate substrate.

[0058] <Sample Evaluation> After forming a modified layer on the surface of the intermediate layer of a lithium tantalate substrate, the thickness of the modified layer for samples A to D was measured. The thickness of the modified layer was measured using a transmission electron microscope. Figure 7 is a graph showing the relationship between the intermediate layer (silicon oxide) film types A to D and the thickness of the modified layer. As shown in Figure 7, even when plasma treatment was performed under the same conditions, the thickness of the modified layer differed depending on the intermediate layer (silicon oxide) film types A to D. Specifically, the modified layer thickness was thickest for film type D. The thickness of the modified layer was about the same for film types A and B. The thickness of the modified layer was thinnest for film type C. There was a large difference of about 1.4 nm in the thickness of the modified layer between film type D and film type C.

[0059] Furthermore, the bonding strength of samples A to D, prepared as described above, and the sample without the intermediate layer (SiO2 film) was investigated. Bonding strength was measured using the blade method. The evaluation method for the blade method was the same as that described in the reference (Materials Science and Engineering R25 (1999) p. 1-88).

[0060] Figure 8 shows the bonding strength of the sample without the intermediate layer (SiO2 film) and the bonding strength of samples B to D. As shown in Figure 8, the bonding strength differed for the sample without the intermediate layer (SiO2 film) and for each of samples B to D.

[0061] Figure 9 is a graph showing the relationship between the thickness of the modified layer and the bonding strength for samples B to D. As shown in Figure 9, there was a positive correlation between the thickness of the modified layer and the bonding strength. As shown in Figure 9, it was found that in order to obtain a bonding strength greater than 0.50, the thickness of the modified layer needed to be 1.8 nm or more.

[0062] Furthermore, the presence or absence of voids was investigated for samples A to D prepared as described above. The presence or absence of voids was investigated using a differential interference contrast microscope. As a result, the occurrence of voids in samples A to D was below the standard value, indicating that void formation was suppressed.

[0063] Based on the above results, in sample D, where the modified layer thickness was 1.8 nm or more, it was possible to suppress the generation of voids while achieving a bonding strength above the standard value.

[0064] Although the present invention has been specifically described above based on embodiments, it goes without saying that the present invention is not limited to the above embodiments and can be modified in various ways without departing from its essence. [Explanation of Symbols]

[0065] 1, 2, 3 Bonded substrate 10. First board 11. First Meso-Place 12. First Modified Layer 15 Joint surface 20 Second board 21. Second Meso-Marginal Layer 22 Second Reformed Layer

Claims

1. A bonded substrate in which a first substrate and a second substrate are joined via a bonding surface, The first substrate is a quartz substrate, The second substrate is a lithium tantalate substrate or a lithium niobate substrate. A first intermediate layer and a second intermediate layer made of silicon oxide are formed on the bonding surface side of each of the first and second substrates, respectively. A first modified layer is formed on the bonding surface side of the first intermediate layer formed on the first substrate, A second modified layer is formed on the bonding surface side of the second intermediate layer formed on the second substrate, The thickness of the first modified layer formed on the first intermediate layer is 1.8 nm or more and 2.2 nm or less. The thickness of the second modified layer formed on the second intermediate layer is 1.8 nm or more and 2.2 nm or less. Bonded substrate.

2. A bonded substrate in which a first substrate and a second substrate are joined via a bonding surface, The first substrate is a quartz substrate, The second substrate is a lithium tantalate substrate or a lithium niobate substrate. A second intermediate layer made of silicon oxide is formed on the bonding surface side of the second substrate. A first modified layer is formed on the surface of the first substrate that is on the bonding surface side. A second modified layer is formed on the bonding surface side of the second intermediate layer formed on the second substrate, The thickness of the first modified layer formed on the bonding surface side of the first substrate is 2.7 nm or more and 3.2 nm or less. The thickness of the second modified layer formed on the second intermediate layer is 1.8 nm or more and 2.2 nm or less. Bonded substrate.

3. A bonded substrate in which a first substrate and a second substrate are joined via a bonding surface, The first substrate is a quartz substrate, The second substrate is a lithium tantalate substrate or a lithium niobate substrate. A first intermediate layer made of silicon oxide is formed on the bonding surface side of the first substrate. A first modified layer is formed on the bonding surface side of the first intermediate layer formed on the first substrate, A second modified layer is formed on the surface of the second substrate that is on the bonding surface side. The thickness of the first modified layer formed on the first intermediate layer is 1.8 nm or more and 2.2 nm or less. The thickness of the second modified layer formed on the bonding surface side of the second substrate is 2.2 nm or more and 2.7 nm or less. Bonded substrate.

4. The bonded substrate according to claim 1 or 3, wherein the thickness of the first intermediate layer is 50 nm or more and 10 μm or less.

5. The bonding substrate according to claim 1 or 2, wherein the thickness of the second intermediate layer is 50 nm or more and 10 μm or less.

6. The thickness of the first substrate is 100 μm or more and 1000 μm or less. The thickness of the second substrate is 10 μm or more and 1000 μm or less. A bonded substrate according to any one of claims 1 to 3.

7. A method for manufacturing a bonded substrate in which a first substrate, a quartz substrate, and a second substrate, a lithium tantalate substrate or a lithium niobate substrate, are joined via a bonding surface, A first step is to form a first intermediate layer and a second intermediate layer made of silicon oxide on the bonding surface side of each of the first and second substrates, A second step involves plasma treatment of the bonding surface side of the first intermediate layer formed on the first substrate to form a first modified layer, A third step involves plasma treatment of the bonding surface side of the second intermediate layer formed on the second substrate to form a second modified layer, A fourth step involves temporarily joining the first substrate and the second substrate with the first modified layer and the second modified layer facing each other, The process includes a fifth step of annealing the substrate after the temporary bonding to bond the first substrate and the second substrate, The thickness of the first modified layer formed on the first intermediate layer is set to 1.8 nm or more and 2.2 nm or less. The thickness of the second modified layer formed on the second intermediate layer is set to 1.8 nm or more and 2.2 nm or less. A method for manufacturing bonded substrates.

8. A method for manufacturing a bonded substrate in which a first substrate, a quartz substrate, and a second substrate, a lithium tantalate substrate or a lithium niobate substrate, are joined via a bonding surface, A first step is to form a second intermediate layer made of silicon oxide on the bonding surface side of the second substrate, A second step involves plasma treatment of the surface of the first substrate on the bonding surface side to form a first modified layer, A third step involves plasma treatment of the bonding surface side of the second intermediate layer formed on the second substrate to form a second modified layer, A fourth step involves temporarily joining the first substrate and the second substrate with the first modified layer and the second modified layer facing each other, The process includes a fifth step of annealing the substrate after the temporary bonding to bond the first substrate and the second substrate, The thickness of the first modified layer formed on the bonding surface side of the first substrate is set to 2.7 nm or more and 3.2 nm or less. The thickness of the second modified layer formed on the second intermediate layer is set to 1.8 nm or more and 2.2 nm or less. A method for manufacturing bonded substrates.

9. A method for manufacturing a bonded substrate in which a first substrate, a quartz substrate, and a second substrate, a lithium tantalate substrate or a lithium niobate substrate, are joined via a bonding surface, A first step is to form a first intermediate layer made of silicon oxide on the bonding surface side of the first substrate, A second step involves plasma treatment of the bonding surface side of the first intermediate layer formed on the first substrate to form a first modified layer, A third step involves plasma treatment of the surface of the second substrate on the bonding surface side to form a second modified layer, A fourth step involves temporarily joining the first substrate and the second substrate with the first modified layer and the second modified layer facing each other, The process includes a fifth step of annealing the substrate after the temporary bonding to bond the first substrate and the second substrate, The thickness of the first modified layer formed on the first intermediate layer is set to 1.8 nm or more and 2.2 nm or less. The thickness of the second modified layer formed on the bonding surface side of the second substrate is set to 2.2 nm or more and 2.7 nm or less. A method for manufacturing bonded substrates.

10. A method for manufacturing a bonded substrate according to claim 7 or 9, further comprising the step of polishing the bonding surface side of the first intermediate layer after forming the first intermediate layer.

11. The method for manufacturing a bonded substrate according to claim 7 or 8, further comprising the step of polishing the bonding surface side of the second intermediate layer after forming the second intermediate layer.

12. The method for manufacturing a bonded substrate according to claim 10, wherein the first intermediate layer is polished so that its thickness is 50 nm or more and 10 μm or less.

13. The method for manufacturing a bonded substrate according to claim 11, wherein the second intermediate layer is polished to a thickness of 50 nm or more and 10 μm or less.

14. A method for manufacturing a bonded substrate according to any one of claims 7 to 9, wherein the temperature of the annealing treatment is 50°C or more and 300°C or less.

15. The thickness of the first substrate is 100 μm or more and 1000 μm or less. The thickness of the second substrate is 10 μm or more and 1000 μm or less. A method for manufacturing a bonded substrate according to any one of claims 7 to 9.

16. A method for manufacturing a bonded substrate according to any one of claims 7 to 9, further comprising the step of polishing the side of the second substrate opposite to the side on which the second modified layer is formed, after bonding the first substrate and the second substrate.

17. The method for manufacturing a bonded substrate according to claim 16, wherein the second substrate is polished so that its thickness is 10 μm or less.

Citation Information

Patent Citations

  • Acoustic wave resonator, filter, and multiplexer

    JP2020043403A

  • Bonded substrate, surface acoustic wave element, surface acoustic wave element device, and manufacturing method of bonded substrate

    JP2021158666A

  • Composite substrate, elastic wave element, and production method for composite substrate

    WO2020250490A1