Fiber molded articles, fibrous binders, and their applications
A fibrillated fibrous binder addresses the strength and dispersibility issues of recycled fibers in FRP, enabling the production of high-strength composite materials using recycled and various fibers, suitable for applications in FRP.
Patent Information
- Application Number
- JP2024553126
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-10-27
- Filing Date
- 2023-10-26
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2043-10-26
AI Technical Summary
Existing fiber-reinforced plastics (FRP) face challenges in maintaining the strength of recycled carbon fibers and other fiber materials due to impaired entanglement and poor dispersibility, leading to fragmented and weaker recycled fibers, and there is a need for a binder that enhances the strength and performance of composite materials using various types of fibers.
The use of a fibrillated fibrous binder, such as fibrillated cellulose fiber, with specific ratios and properties, to create a fibrous molded article that maintains strength and allows for the production of composite materials with recycled and various types of fibers.
The fibrous molded article achieves sufficient strength and performance characteristics, enabling the production of high-strength composite materials even with recycled fibers, and can be processed into forms like FRP with improved properties.
Smart Images

Figure 0007949052000001 
Figure 0007949052000002 
Figure 0007949052000003
Abstract
Description
[Technical Field]
[0001] This invention relates to fibrous molded articles, fibrous binders used therein, and applications thereof. [Background technology]
[0002] Fiber-reinforced plastics (FRP) are reinforced plastic materials that use epoxy resin or phenolic resin as a matrix and combine it with fibrous materials such as glass fibers or carbon fibers to improve various functions. Among these, carbon fiber is a material that is lightweight yet has excellent strength and elastic modulus, and carbon fiber-reinforced plastics (CFRP) using carbon fibers are used in an extremely wide range of fields, including automotive parts, ship parts, aircraft parts, spacecraft parts, drone parts, civil engineering and construction materials, sporting goods, and electronic and electrical appliance parts such as personal computers.
[0003] Generally, FRP (fiber-reinforced plastic) is manufactured by impregnating a sheet-like fibrous material with a resin component that serves as the base material. While there are many technological developments aimed at improving the performance of FRP, one important factor in manufacturing such composite materials using fibrous materials is that the fibrous molded body itself has sufficient strength before being impregnated with the base material.
[0004] Nonwoven fabrics are typical sheet-like fibrous materials used in FRP (Fiber Reinforced Plastics). Various methods for producing nonwoven fabrics from fibrous materials have already been developed, not only in the field of FRP. Furthermore, research and development have also progressed on the production of nonwoven fabrics specifically for use in FRP, as described above.
[0005] For example, in fiber-reinforced plastic molded articles that use thermoplastic resin as a binder for carbon fibers, if the thermoplastic resin melts at high temperatures such as thermal melting, the fixation of the entanglement points between carbon fibers is impaired. As a result, the three-dimensional structure of the carbon fibers collapses, the carbon fibers become more likely to orient in a specific direction, and the strength may decrease. To solve this problem, a method has been disclosed in which a papermaking sheet before resin impregnation is subjected to the papermaking process using a mixed dispersion of carbon fibers and water-swelled fillyric fibers (for example, Patent Document 1).
[0006] Furthermore, when inorganic fibers such as carbon fibers, glass fibers, and metal fibers are processed into nonwoven fabrics by the wet papermaking method, the dispersibility in water is poor because inorganic fibers are hydrophobic. As a result, it has been difficult to obtain inorganic fiber sheets with good form. To overcome this problem, a technique has been disclosed that uses a dispersant containing a predetermined surfactant or resin (for example, Patent Document 2).
[0007] Incidentally, in recent years, promoting sustainable development has become a global consensus, and as the use of composite materials composed of fibers such as carbon fiber and matrix materials increases, as mentioned above, the development of their reuse is also required. [Prior art documents] [Patent Documents]
[0008] [Patent Document 1] International Publication No. 2014 / 021366 [Patent Document 2] Japanese Patent Publication No. 2017-57511 [Overview of the Initiative] [Problems that the invention aims to solve]
[0009] As described above, one strategy to take advantage of the superior properties of the fibers incorporated into FRP is to ensure that the strength of the fiber molded body itself is excellent before impregnation with the base material. However, when fibrous components such as carbon fibers are separated from molded products such as CFRP for reuse, the recycled carbon fibers obtained differ significantly from the unused fibrous state, and in many cases become fragmented and shorter compared to the unused ones. Even when attempting to process recycled carbon fibers again into fiber molded sheets, it is often impossible to process them into a sheet form, or even if they can be processed into a sheet form, it is difficult to obtain the strength, resistance, and other performance characteristics required for FRP materials.
[0010] Therefore, one possible strategy for producing fiber-molded sheets using recycled fibers is to increase the amount of binder used. However, from the perspective of producing FRP with desired performance, it was necessary to minimize the amount of binder in order to better utilize the properties of the main fiber material. Furthermore, there was a need for a binder suitable for producing molded products using various types of fiber materials, not just carbon fibers.
[0011] In light of the above circumstances, one of the challenges we aim to solve is to provide a fiber molded article with sufficient strength and a composite material using the same. Another challenge we aim to address is to provide a fibrous molded article with sufficient strength using recycled carbon fibers, as well as a composite material using the same. Another challenge we aim to address is to provide fiber molded articles and composite materials using the same that possess sufficient strength, using various types of fiber materials. [Means for solving the problem]
[0012] Through diligent research, the inventors have discovered that by using a fibrillated fibrous binder, it is possible to form a fibrous molded article with a predetermined strength, suitable for the manufacture of FRP and other applications. This disclosure is based on this finding.
[0013] The invention presented in this disclosure can be understood in multiple aspects and forms, and may include, for example, the following embodiments as means for solving the problem. In this disclosure, the invention presented in this disclosure is also referred to simply as "the present invention," either conceptually or according to each individual form.
[0014] [1] A fiber molded article, The aforementioned fibrous molded body comprises a main fibrous material and a fibrous binder. The ratio of the main fiber material to the fibrous binder is 1 to 20 parts by weight of the fibrous binder per 100 parts by weight of the main fiber material. The krill ratio of the fibrous binder is 1.25 to 3.00. Fiber molded body. [2] The fibrous molded article according to [1] above, wherein the average fiber length of the fibrous binder is 0.30 to 2.50 mm. [3] The fiber molded article according to [1] or [2] above, wherein the main fiber material is one or more selected from the group consisting of carbon fiber, glass fiber, metal fiber, natural fiber, cellulosic fiber, regenerated fiber, semi-synthetic fiber, and synthetic fiber. [4] The fiber molded article according to [1] or [2] above, wherein the main fiber material is one or more selected from the group consisting of carbon fiber, glass fiber, PET fiber, and aramid fiber. [5] The fiber molded article according to [1] or [2] above, wherein the main fiber material is carbon fiber. [6] The fiber molded article according to any one of the above items [3] to [5], wherein the carbon fiber is a first-use carbon fiber, a recycled carbon fiber, or a mixture thereof. [7] The fibrous molded article according to any one of the above items [1] to [6], wherein the fibrous binder is fibrillated cellulose fiber. [8] The fibrous molded article according to any one of the above items [1] to [7], wherein the fineness of the fibrous binder is 95% or less. [9] A fiber-reinforced resin molded article comprising the fiber molded article according to any one of the above [1] to [8], and a resin component impregnated into the fiber molded article.
[10] A fibrillated cellulose fiber, wherein the curl ratio of the fibrillated cellulose fiber is 1.25 to 3.00, and the fine ratio of the fibrillated cellulose fiber is 95% or less, which is a fibrous binder for fiber molded articles. [Effects of the Invention]
[0015] According to one or more aspects of the invention presented in the present disclosure, a fiber molded article having sufficient strength can be provided. Further, according to one or more aspects of the invention presented in the present disclosure, a fiber molded article having sufficient strength can be provided using recycled carbon fibers. Further, according to one or more aspects of the invention presented in the present disclosure, a fiber molded article having sufficient strength can be provided using various types of fiber materials. Furthermore, according to one or more aspects of the invention presented in the present disclosure, various excellent composite materials can be provided using the fiber molded article as described above. [Mode for Carrying Out the Invention]
[0016] The present disclosure is based on an international application under the Patent Cooperation Treaty, and the original language of the application is Japanese. The present disclosure is scheduled to be translated into the language required by each country upon entry into the designated States and elected States. In the present disclosure, unless otherwise specified, Japanese nouns may be either singular or plural depending on the full text or context of the present disclosure. In addition, when translated into a language that has distinctions between countable and uncountable nouns, and between singular and plural forms for countable nouns, such as English, unless otherwise specified, the singular reference includes the plural case, and the plural reference includes the singular case, depending on the full text or context of the present disclosure.
[0017] Hereinafter, embodiments of the present invention will be described. In this disclosure, the term "one embodiment" in relation to the present invention refers to any one embodiment used to describe the present invention in detail, unless otherwise specified, and does not negate or limit the existence of other or more embodiments. As shown below, the present invention may have multiple embodiments that fall within its scope. These multiple embodiments may also be provided as modified forms, for example, by various combinations of the components (or technical features) shown in this disclosure. Furthermore, in this disclosure, where the term "embodiment" is used, it includes one or more embodiments unless otherwise specified.
[0018] In this disclosure, unless otherwise specified, the notation "AA~BB" in relation to a numerical range means "AA or greater and BB or less" (where "AA" and "BB" represent any numerical value). Furthermore, unless otherwise specified, the units for both the lower and upper limits are the same as the unit immediately following the latter (i.e., "BB" in this case). In this disclosure, the combination of the lower and upper limits of a numerical range can be any combination of numerical values selected from the set of lower or upper limits provided as examples of preferred values. Also, the expression "X and / or Y" means both X and Y, or either one of them.
[0019] 1. Fibrous binder The fibrous binder of this disclosure can be suitably used as a binder for bonding the main fibrous materials that constitute the body of the fibrous molded article described in detail below.
[0020] Preferably, the fibrous binder is, for example, fibrillated cellulose fiber. In this disclosure, "fibrillation" refers to the process by which a fiber becomes fuzzy or rough due to friction or beating. In other words, it can also be said to be the process of making small fibers (i.e., fibrils) fuzzy from the fiber body by friction or beating. In this disclosure, "fibrillated cellulose fiber" refers to a cellulose fiber that has been fibrillated and has small fibers (fibrils) fuzzy on its surface.
[0021] Cellulose fibers include, for example, natural cellulose fibers, chemically modified cellulose fibers, and regenerated cellulose fibers. Examples of natural cellulose fibers include wood pulp such as coniferous pulp and hardwood pulp, and herbaceous pulp such as straw pulp, bamboo pulp, linter pulp, hemp pulp, and kenaf pulp. Examples of chemically modified cellulose fibers include cellulose fibers that have been oxidized, etherified, cationized, or esterified. Examples of regenerated cellulose fibers include rayon, cupro, and lyocell.
[0022] In other words, fibrillated cellulose can be obtained by subjecting cellulose fibers to friction or beating treatment using, for example, a single-disc refiner (SDR), a double-disc refiner (DDR), a beater, a mixer, a mill, or a grinding device, thereby loosening and fluffing the surface of the fibers. Alternatively, a suspension or slurry of cellulose fibers may be prepared and subjected to high-speed, high-pressure treatment using a homogenizer.
[0023] The fibrous binder preferably satisfies at least one of the following property indicators, or any two or more indicators.
[0024] <Freeness> In this disclosure, "freeness" is one of the indicators of fibrillation of fibers, and is determined by measuring how much water is removed when the target test product (in this disclosure, for example, a fibrous binder) is prepared as a slurry and water is rapidly removed through a predetermined filter. More specifically, the value of freeness in this disclosure can be determined by the measurement method used in the examples below. A higher freeness value indicates that water is easily removed and less fluffing is observed, while a lower value indicates that water is difficult to remove and more fluffing is observed. Freeness is also referred to as beatenness or freeness.
[0025] The filtration rate of the fibrous binder, when measured according to the specific test methods performed for the examples described in detail below, is preferably 0 to 100 ml. Having a filtration rate within this range contributes to forming a fibrous molded body with sufficient strength. From the perspective of further pursuing the strength of the fibrous molded body, the lower limit of the filtration rate of the fibrous binder is theoretically most preferably 0, but practically it may be 5 ml or more. On the other hand, the upper limit of the filtration rate of the fibrous binder may more preferably be 50 ml or less, and even more preferably 40, 30, or 20 ml or less.
[0026] <Average fiber length of fibrous binder> The average fiber length of the fibrous binder is preferably 0.30 to 2.50 mm. Having the average fiber length within this range contributes to forming a fibrous molded body with sufficient strength. To further pursue the strength of the fibrous molded body, more preferable lower and upper limits may be as follows: The lower limit of the average fiber length of the fibrous binder is more preferably 0.35 mm or more, and even more preferably 0.40, 0.45, or 0.50 mm or more. The upper limit of the average fiber length of the fibrous binder may more preferably be 2.00, 1.75, or 1.50 mm or less, and even more preferably 1.25 mm or less.
[0027] <Average fiber diameter of fibrous binders> The average fiber diameter of the fibrous binder is preferably 10.0 to 40.0 μm. Having the average fiber diameter within this range contributes to forming a fibrous molded article with sufficient strength. From the viewpoint of further pursuing the strength of the fibrous molded article, the more preferable lower and upper limits are as follows. The lower limit of the average fiber diameter of the fibrous binder may be more preferably 15.0 μm or more, and even more preferably 20.0 μm or more. The upper limit of the average fiber diameter of the fibrous binder may more preferably be 38.0 μm or less, and even more preferably 35.0 μm or less.
[0028] <Krill ratio of fibrous binder> In this disclosure, the "krill ratio" is the ratio of the reductions in the ultraviolet and infrared regions of transmitted light when light is incident on a slurry of a fibrous binder. Fibrils, which are formed when the fiber walls are detached from the fiber (the fiber body or main trunk) by processes such as friction or beating, and have a diameter of about 1 / 100th of the fiber, scatter and absorb mainly ultraviolet light, whether they remain attached to the fiber or float detached. Therefore, the transmitted ultraviolet light is reduced relative to the incident light, and the amount of reduction correlates with the total surface area of the fibrils. On the other hand, non-fibril fibers scatter and absorb mainly infrared light. Therefore, the transmitted infrared light is reduced relative to the incident light, and the amount of reduction correlates with the total surface area of the non-fibril fibers. Thus, the krill ratio serves as an indicator of the degree of fibrilization of the fibrous binder. The krill ratio value in this disclosure can be determined by the measurement methods used in the following examples.
[0029] The krill ratio of the fibrous binder is preferably 1.25 to 3.00. Having a krill ratio within this range contributes to forming a fibrous molded article with sufficient strength. From the viewpoint of further pursuing the strength of the fibrous molded article, the lower limit of the krill ratio can be more preferably 1.30 or higher, and even more preferably 1.35 or higher. The upper limit of the krill ratio may more preferably be 2.80, 2.60, or 2.40 or less.
[0030] <Fineness ratio of fibrous binder (%)> In this disclosure, the fineness ratio is an index indicating the proportion of fine fibers with a fiber length of less than 0.2 mm. The value of the fineness ratio in this disclosure can be determined by the measurement method used in the following examples. In the process of fibrillation of fibers, fibers that are excessively ground down to a length of less than 0.2 mm are considered to have a low contribution to the binding effect on the fiber molded article.
[0031] The fineness ratio of the fibrous binder is preferably 10 to 95%. More specifically, it is as follows: The upper limit of the fineness ratio of the fibrous binder is preferably 95% or less. Having the fineness ratio within this range contributes to forming a fibrous molded article with sufficient strength. From the viewpoint of further pursuing the strength of the fibrous molded article, the upper limit of the fineness ratio of the fibrous binder may more preferably be 90% or less, and even more preferably 85%, 80%, 75%, or 70% or less. The lower limit of the fineness ratio of the fibrous binder can be set arbitrarily from the viewpoint of further pursuing the strength of the fibrous molded article, but it is usually preferably 10%, 20%, 30%, or 40% or more.
[0032] 2. Fiber molded body The fibrous molded article of this disclosure is a molded article comprising a main fibrous material and a fibrous binder as constituent materials. The shape of the molded article is not particularly limited, but preferred shapes include sheet-like or plate-like shapes. As the fibrous binder, the fibrous binder of this disclosure described above can be suitably used.
[0033] The main fiber material is the main material of the molded article. The ratio of the main fiber material to the fiber binder is preferably 1 to 20 parts by weight of fibrous binder per 100 parts by weight of main fiber material.
[0034] Generally, in FRP (fiber-reinforced plastic) obtained by impregnating a nonwoven fabric (fiber molded body) with a resin component that serves as the matrix and then curing it, there has often been a demand to minimize the amount of binder component in the nonwoven fabric. This is presumably because, from the perspective of making the most of the inherent properties of the main fiber material, the binder has been considered an unnecessary component. However, it is difficult to produce fiber molded bodies such as nonwoven fabrics with sufficient strength using only the main fiber material without using any binder, and therefore, in the production of fiber molded bodies such as nonwoven fabrics, the amount of binder has been added as little as possible out of necessity.
[0035] In contrast, the fibrous molded articles of this disclosure use a predetermined fibrous binder as described above, thereby enabling sufficient strength in the fibrous molded articles. Moreover, it has been found that such fibrous molded articles exhibit superior strength and other properties even when further processed into forms such as FRP.
[0036] As described above, the amount of fibrous binder added to 100 parts by weight of the main fiber material can preferably be any value between 1 and 20 parts by weight. More specifically, the amount of fibrous binder added may be 20, 19, 18, 17, 16, 15, 14, 13, 12, 11, 10, 9, 8, 7, 6, 5, 4, 3, 2, or 1 part by weight per 100 parts by weight of the main fiber material. Expressed as a numerical range, the upper limit of the amount of fibrous binder is more preferably 18 parts by weight or less, and even more preferably 15, 13, or 10 parts by weight or less, per 100 parts by weight of the main fiber material. On the other hand, the lower limit of the amount of fibrous binder is more preferably 2, 3, or 4 parts by weight or more, per 100 parts by weight of the main fiber material.
[0037] To mix the main fiber material and the fibrous binder, for example, a liquid such as water can be used as a medium, and the two materials can be added to the liquid and mixed by stirring. When mixing the main fiber material and the fibrous binder, other additives, such as dispersants and viscous agents, may also be added.
[0038] By using a dispersant, hydrophilicity can be imparted to the hydrophobic main fiber material, or secondary aggregation can be reduced by promoting repulsion between fibers. Examples of dispersants include polyoxyalkylene monophenyl ether, polyether-based urethane resin, and polyoxyethylene polyoxypropylene stearyl ether. The amount of dispersant added may be preferably 1 to 20 parts by weight, more preferably 3 to 10 parts by weight, per 100 parts by weight of the main fiber material.
[0039] Furthermore, by using a viscous agent, viscosity can be imparted to the slurry, reducing secondary aggregation of the hydrophobic main fiber material. Examples of viscous agents include polyethylene oxide and sodium polyacrylate. The amount of viscous agent added may be preferably 1 to 50 parts by weight, more preferably 5 to 30 parts by weight, per 100 parts by weight of the main fiber material.
[0040] <Main fiber material> The main fiber material is not particularly limited as long as it is a fiber material that can be formed into woven fabrics, knitted fabrics, nonwoven fabrics, etc. The main fiber material may be inorganic or organic fiber. Examples of inorganic fibers include carbon fiber, glass fiber, and metal fiber. Examples of organic fibers include "natural fibers" such as cotton, hemp, and animal hair, "synthetic fibers" made from petroleum, etc., cellulose fibers derived from wood, or "semi-synthetic fibers" or "regenerated fibers" made from natural materials by various treatments. Examples of "synthetic fibers" include polyamide fibers, polyester fibers, polyurethane fibers, polyvinyl alcohol fibers, pitch fibers, polyacrylonitrile (PAN) fibers, phenolic fibers, polyphenylene sulfide fibers, polyvinyl chloride fibers, polypropylene fibers, polyethylene fibers, and polystyrene fibers. Examples of "regenerated fibers" obtained from natural materials include rayon, cupro, and lyocell.
[0041] Preferably, the main fiber material includes, for example, carbon fiber, glass fiber, metal fiber, cellulosic fiber, regenerated fiber, semi-synthetic fiber, and synthetic fiber. More specifically, examples of inorganic fibers include carbon fiber, glass fiber, and metal fiber, and examples of organic fibers include cellulosic fiber, pitch fiber, PAN fiber, phenol fiber, PET fiber, aramid fiber, and polyphenylene sulfide fiber. Among these, carbon fiber, glass fiber, PET fiber, and aramid fiber are more preferably used as the main fiber material, and carbon fiber is even more preferably used. Examples of carbon fiber include rayon-based carbon fiber, pitch-based carbon fiber, PAN-based carbon fiber, and phenol-based carbon fiber, and activated carbon fiber may also be used. The main fiber material may be used alone or two or more types may be used.
[0042] The carbon fibers may be first-use carbon fibers, recycled carbon fibers (recycled carbon fibers), or a mixture of these. In this disclosure, "first-use" (or "unused") carbon fibers are used in contrast to the term "recycled," and refer to pristine fibers that are used for the first time after being manufactured, not recycled fibers, such as so-called virgin fibers. In this disclosure, "recycled" carbon fibers refer to fibers recovered from in-process scraps generated during the production process and used CFRP products (materials that have been used for some purpose as carbon fibers) that are discharged as waste, using these materials as raw materials for recycling and undergoing recycling processing. Furthermore, in this disclosure, "recycled carbon fibers" are also referred to as "recycled carbon fibers," "recovered carbon fibers," or, as commonly called, "recycled carbon fibers" (in English, they are also commonly called Recycled Carbon Fiber (abbreviation: rCF)).
[0043] <Average fiber length of the main fiber material> The average fiber length of the main fiber material is preferably 1 to 100 mm. Having the average fiber length within this range contributes to forming a fibrous molded body with sufficient strength. To further pursue the strength of the fibrous molded body, more preferable lower and upper limits may be as follows: The lower limit of the average fiber length of the main fiber material may more preferably be 2, 3, or 4, and even more preferably 5 mm or more. The upper limit of the average fiber length of the main fiber material may more preferably be 80, 60, 50, 40, or 30 mm or less, and even more preferably 20 mm or less.
[0044] <Average fiber diameter of the main fiber material> The average fiber diameter of the main fiber material is preferably 1.0 to 50.0 μm. Having the average fiber diameter within this range contributes to forming a fibrous molded article with sufficient strength. From the viewpoint of further pursuing the strength of the fibrous molded article, the more preferable lower and upper limits are as follows. The lower limit of the average fiber diameter of the main fiber material may more preferably be 2.0, 3.0, 4.0, or 5.0 μm or more, and even more preferably 6.0 μm or more. The upper limit of the average fiber diameter of the fibrous binder may more preferably be 40.0, 30.0, 20.0, or 15.0 μm or less, and even more preferably 10.0 μm or less.
[0045] In one preferred embodiment of this disclosure, recycled carbon fiber (rCF), obtained by separating and recovering carbon fibers contained in FRP or the like, can be suitably used. Such recycled carbon fibers are usually shorter in length than their original fiber length before being processed into FRP or the like, and their surface is rough, making it difficult to obtain sufficient strength when processed into a nonwoven fabric. However, by using the fibrous binder described above in this disclosure, a nonwoven fabric using such recycled carbon fibers as a fiber material can be made to have sufficient strength. In another preferred embodiment, recycled carbon fiber and newly produced carbon fiber (unused carbon fiber) may be mixed and used as the main fiber material.
[0046] There are no particular restrictions on the method of forming fibrous articles such as nonwoven fabrics, and conventional methods can be used. For example, as a method for manufacturing nonwoven fabrics, a fibrous sheet can be obtained using a wet process with main fiber material cut to an appropriate length as the raw material.
[0047] The molded articles of this disclosure may use other types of binders and other materials in addition to the fibrous binder and main fiber material described above. Examples of such materials include painters that can be used in papermaking, such as starch, SBR, polyvinyl alcohol-based aqueous solutions, unsaturated polyester-based aqueous solutions, and acrylic-based aqueous solutions. Furthermore, composite fibers such as polyvinyl alcohol-based fibrous binders, core-sheath fibers, parallel fibers, and radially divided fibers can also be used as moist heat bonding types. Specifically, examples include combinations of polypropylene (core) and polyethylene (sheath), polypropylene (core) and ethylene vinyl alcohol (sheath), high-melting-point polyester (core) and low-melting-point polyester (sheath), and high-melting-point polyester (core) and polyethylene (sheath). In addition, fibers composed solely of polyethylene or polypropylene can be used as fully melted types. Various fibrillated fibrous binders can also be used. They can be widely used regardless of whether they are synthetic or natural products. Examples of such fibrillated fibrous binders may include acrylic fibers, polyethylene fibers, polypropylene fibers, polyacrylonitrile fibers, nylon fibers, aramid fibers, and the like.
[0048] A preferred embodiment of the fiber molded article of this disclosure may be molded in the form of a sheet. In the case of a sheet molded article, the basis weight is preferably 20 to 200 g / m². 2 It is possible. Setting the lower limit of the basis weight to be equal to or greater than the above preferred value helps prevent insufficient tensile strength of the sheet-like molded product. From the viewpoint of preventing insufficient tensile strength of the sheet-like molded product, the lower limit of the basis weight is more preferably 30 g / m². 2 More preferably 40 g / m 2 It is possible. On the other hand, by setting the upper limit of the basis weight to the above preferred value or less, it is possible to easily remove moisture and perform drying in the production process. From the viewpoint of ease of drying treatment, the upper limit of the basis weight is more preferably 190, 180, or 170 g / m 2 , still more preferably 160 or 150 g / m 2 .
[0049] The density of the fiber molded body of the present disclosure is preferably 0.05 to 0.20 g / cm 3 . By setting the lower limit of the density to the above preferred value or more, it contributes to achieving a good composite balance with the resin when processing into FRP or the like. From the viewpoint of such a composite balance with the resin, the lower limit of the density is more preferably 0.06 or 0.07 g / cm 3 or more, still more preferably 0.08 or 0.09 g / cm 3 or more. On the other hand, by setting the upper limit of the density to the above preferred value or less, the impregnation of the resin can be performed more easily when processing into FRP or the like. From the viewpoint of resin impregnation property, the upper limit of the density is more preferably 0.19 or 0.18 g / cm 3 , still more preferably 0.17 or 0.16 g / cm 3 .
[0050] The fiber molded body of the present disclosure can be adjusted to have favorable tensile strength. The tensile strength of the fiber molded body of the present disclosure can be appropriately adjusted according to needs. Although there may be several means for adjusting the tensile strength, for example, it can also be adjusted by the blending amount of the fibrous binder and the like. When measured according to the specific test method (using a test piece with a width of 15 mm and a length of 150 mm) implemented for Examples and the like described in detail below, the tensile strength of the fiber molded body of the present disclosure can be adjusted to, for example, at least 0.06 or 0.07 kN / mm or more. For even higher tensile strength, it can be adjusted to, for example, 0.10, 0.15, 0.19, 0.21, or 0.22 kN / mm or more, and further 0.23, 0.25, 0.30, or 0.40 kN / mm or more.
[0051] 3. Applications of fiber molded products (3.1) The fiber molded articles of this disclosure can be applied to an extremely wide range of applications. For example, various FRPs can be obtained by impregnating a sheet of the fiber molded article of this disclosure (also called a fiber molded article sheet) with a base resin and curing it. Examples of FRPs include glass fiber reinforced plastics, carbon fiber reinforced plastics, boron fiber reinforced plastics, and aramid fiber reinforced plastics.
[0052] (3.2) When activated carbon fibers are used as the main material of the fiber molded article in this disclosure, it can be used as an adsorbent for liquid and gas phases. Suitable applications for the adsorbent include, for example, water purification and chemical filters for semiconductor manufacturing cleanrooms. [Examples]
[0053] The present invention will be described in more detail below with reference to examples, but the technical scope (or technical reach) of the invention presented in this disclosure is not limited to the following examples. Furthermore, the measurement methods, calculation methods, and evaluation methods shown below can be used as methods for determining numerical values when the invention presented in this disclosure is specified using numerical values.
[0054] <Example FB1 (Fibrous Binder)> (1) Preparation of pulp slurry 300g of unbeaten LBKP (bleached hardwood pulp) (manufactured by Nippon Paper Industries Ltd.) was disintegrated to obtain a 3.0% (W / V) slurry. (2) Fibrillation The obtained pulp slurry was fibrillated by 11 passes using a single disc refiner, and then diluted with water to obtain a 0.5% (W / V) slurry with a filtration rate of 32 ml, an average fiber length of 0.78 mm, an average fiber diameter of 20.8 μm, an krill ratio of 1.37, and a fineness of 48.4%.
[0055] <Example FB2 (Fibrous Binder)> (1) Preparation of pulp slurry 300g of unbeaten NBKP (bleached softwood pulp) (manufactured by Nippon Paper Industries Co., Ltd.) was disintegrated to obtain a 3.0% (W / V) slurry. (2) Fibrillation The obtained pulp slurry was fibrillated by circulating it through a single disc refiner for four passes, and then diluted with water to obtain a 0.5% (W / V) slurry with a filtration rate of 15 ml, an average fiber length of 1.03 mm, an average fiber diameter of 28.8 μm, an krill ratio of 1.63, and a fineness of 49.9%.
[0056] <Example FB3 (Fibrous Binder)> (1) Preparation of pulp slurry A 3.0% (W / V) slurry was obtained in the same manner as in Example FB2(1). (2) Fibrillation The obtained pulp slurry was fibrillated by 10 passes using a single disc refiner, and then diluted with water to obtain a 0.5% (W / V) slurry with a filtration rate of 0 ml, an average fiber length of 0.56 mm, an average fiber diameter of 25.6 μm, an acrylic ratio of 2.14, and a fineness of 59.3%.
[0057] <Comparative Example FB1 (Fibrous Binder)> (1) Preparation of chemically modified pulp 40 kg of unbeaten NBKP (manufactured by Nippon Paper Industries Co., Ltd.) was added to 4000 L of an aqueous solution containing 312 g of TEMPO (manufactured by Sigma Aldrich) (0.05 mmol per 1 g of oven-dried cellulose) and 4112 g of sodium bromide (1.0 mmol per 1 g of oven-dried cellulose), and the mixture was stirred. Then, an aqueous sodium hypochlorite solution was added until the sodium hypochlorite concentration reached 5.5 mmol / g, and the oxidation reaction was started at room temperature. To correct the decrease in pH during the reaction, a 3 M aqueous sodium hydroxide solution was added sequentially to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH in the system no longer changed. After adjusting the pH of the reaction mixture to 2 by adding hydrochloric acid, the pulp was thoroughly washed with water by repeated dehydration and dilution with water, and dehydration was continued until the pulp solids concentration was 20% by weight to obtain chemically modified pulp with a carboxyl group content of 1.4 mmol / g.
[0058] (2) Fibrillation The obtained chemically modified pulp was dispersed in water, and sodium hydroxide was added and stirred to obtain a 1.1% (W / V) slurry at pH 7.7. 4300 kg of the obtained slurry was subjected to fibrillation by 20 passes in a monoflow double disc refiner at a circulation rate of 80%. After dilution with water, a 0.5% (W / V) slurry was obtained with a filtration rate of 0 ml, an average fiber length of 0.29 mm, an average fiber diameter of 30.3 μm, a krill ratio of 3.33, and a fineness of 99.8%.
[0059] <Comparative Example FB2 (Fibrous Binder)> (1) Preparation of pulp slurry A 3.0% (W / V) slurry was obtained in the same manner as in Example FB1(1). (2) Dilution The obtained pulp slurry was diluted with water to obtain a 0.5% (W / V) slurry with a filtration rate of 620 ml, an average fiber length of 0.94 mm, an average fiber diameter of 19.8 μm, an krill ratio of 0.83, and a fineness of 30.7%.
[0060] <Comparative Example FB3 (Fibrous Binder)> (1) Preparation of pulp slurry A 3.0% (W / V) slurry was obtained in the same manner as in Example FB1(1). (2) Fibrillation The obtained pulp slurry was fibrillated by circulating it five times using a single disc refiner, and then diluted with water to obtain a 0.5% (W / V) slurry with a filtration rate of 78 ml, an average fiber length of 0.83 mm, an average fiber diameter of 20.2 μm, an krill ratio of 1.22, and a fineness of 42.6%.
[0061] <Comparative Example FB4 (Fibrous Binder)> (1) Preparation of pulp slurry A 3.0% (W / V) slurry was obtained in the same manner as in Example FB2(1). (2) Dilution The obtained pulp slurry was diluted with water to obtain a 0.5% (W / V) slurry with a filtration rate of 650 ml, an average fiber length of 2.11 mm, an average fiber diameter of 28.0 μm, an krill ratio of 0.98, and a fineness of 13.5%.
[0062] <Comparative Example FB5 (Fibrous Binder)> (1) Preparation of pulp slurry A 3.0% (W / V) slurry was obtained in the same manner as in Example FB2(1). (2) Fibrillation The obtained pulp slurry was fibrillated by circulating it twice using a single disc refiner, and then diluted with water to obtain a 0.5% (W / V) slurry with a filtration rate of 362 ml, an average fiber length of 1.80 mm, an average fiber diameter of 27.6 μm, an krill ratio of 1.20, and a fineness of 25.7%.
[0063] <Example S1 (Fiber molded sheet)> Composition (1): 94% recycled carbon fiber (w / w), 6% fibrous binder (w / w) At room temperature, using a commercial mixer with a power of 2800W and a capacity of 3.9L, 0.08g of a dispersant (aqueous solution of polyether-based polyurethane resin, manufactured by Meisei Chemical Co., Ltd., model number Pulset HA) and 140g of a 0.1% (W / W) aqueous solution of a viscous agent (polyethylene oxide, manufactured by Meisei Chemical Co., Ltd., model number Alcox SK) were added to 700ml of water and mixed uniformly. Then, 1.33g of recycled carbon fiber (manufactured by Carbon Fiber Recycle Industry Co., Ltd., 9mm sieved product obtained by secondary heating of Toray Industries model number T800SC scraps, average fiber diameter 7μm, average fiber length 10mm, water content 1.4%) and 16.8g of the fibrous binder from Example FB1 were added as the main fiber material, and the mixture was stirred at a rotation speed of 15000rpm for 6 minutes to obtain a slurry. The slurry was hand-formed using a round (16 mm diameter) hand-formed sheet machine (manufactured by Tozai Seiki Co., Ltd.), and then subjected to primary (5 min) and secondary (2 min) pressing at a standard press pressure of 410 ± 10 kPa in accordance with JIS P8222:2015 using an AUTOMATIC SHEET PRESS (Kumagai Riki Kogyo Co., Ltd.). After that, it was dried in a dryer at 50°C for 30 minutes to obtain the fiber molded sheet of Example S1(1).
[0064] Composition (2): 94% carbon fiber (w / w), 6% fibrous binder (w / w) Except for using 1.33 g of carbon fiber (Toray Industries, Ltd., model number T700SC-12K-50C, average fiber diameter 7 μm, average fiber length 12 mm, moisture content 1.0%) as the main fiber material, the same procedure as in formulation (1) was used to obtain the fiber molded sheet of Example S1(2).
[0065] Composition (3): Glass fiber 94% (W / W), fibrous binder 6% (W / W) Except for using 1.40 g of glass fiber (PFG Fiber Glass Corporation, model number E225, average fiber diameter 7 μm, average fiber length 5 mm, moisture content 6.0%) as the main fiber material, the same procedure as in formulation (1) was used to obtain the fiber molded sheet of Example S1(3).
[0066] Composition (4): PET fiber 94% (W / W), fibrous binder 6% (W / W) Except for using 1.40 g of PET fiber (manufactured by Teijin, model number TA04N SD 0.6×5, average fiber diameter 7 μm, average fiber length 5 mm, moisture content 5.9%) as the main fiber material, the same procedure as in formulation (1) was used to obtain the fiber molded sheet of Example S1(4).
[0067] Composition (5): 94% aramid fiber (W / W), 6% fibrous binder (W / W) Example S1 was prepared in the same manner as in formulation (1), except that 1.43 g of aramid fiber (Toray DuPont Ltd., Kevlar® aramid fiber staple, 1.7 dtex, average fiber diameter 15 μm, average fiber length 6 mm, moisture content 8.2%) was used as the main fiber material. (5) A fibrous molded sheet was obtained.
[0068] Composition (6): 97% recycled carbon fiber (w / w), 3% fibrous binder (w / w) Example S1 was prepared in the same manner as in Formula (1), except that 1.38 g of recycled carbon fiber from Formula (1) and 8.4 g of fibrous binder from Example FB1 were used as the main fiber material. (6) A fibrous molded sheet was obtained.
[0069] <Example S2 (Fiber molded sheet)> Except for using the fibrous binder of Example FB2, the procedure was the same as in Examples S1(1) to S1(6). 6 types Fiber molded sheets were obtained in Examples S2(1), S2(2), S2(3), S2(4), S2(5), and S2(6). Composition (1): 94% recycled carbon fiber (w / w), 6% fibrous binder (w / w) Composition (2): 94% carbon fiber (w / w), 6% fibrous binder (w / w) Composition (3): Glass fiber 94% (W / W), fibrous binder 6% (W / W) Composition (4): PET fiber 94% (W / W), fibrous binder 6% (W / W) Composition (5): 94% aramid fiber (W / W), 6% fibrous binder (W / W) Composition (6): 97% recycled carbon fiber (w / w), 3% fibrous binder (w / w)
[0070] <Example S3 (Fiber molded sheet)> Except for using the fibrous binder of Example FB3, the procedure was the same as in Examples S1(1) to S1(6). 6 types Fiber molded sheets were obtained as Examples S3(1), S3(2), S3(3), S3(4), S3(5), and S3(6). Composition (1): 94% recycled carbon fiber (w / w), 6% fibrous binder (w / w) Composition (2): 94% carbon fiber (w / w), 6% fibrous binder (w / w) Composition (3): Glass fiber 94% (W / W), fibrous binder 6% (W / W) Composition (4): PET fiber 94% (W / W), fibrous binder 6% (W / W) Composition (5): 94% aramid fiber (W / W), 6% fibrous binder (W / W) Composition (6): 97% recycled carbon fiber (w / w), 3% fibrous binder (w / w)
[0071] <Comparative Example S1 (Fiber Molded Sheet)> Except for using the fibrous binder of Comparative Example FB1, the procedure was the same as in Examples S1(1) to S1(6). 6 types Fiber molded sheets: Comparative Examples S1(1), S1(2), S1(3), S1(4), S1(5), and S1(6) were obtained. Composition (1): 94% recycled carbon fiber (w / w), 6% fibrous binder (w / w) Composition (2): 94% carbon fiber (w / w), 6% fibrous binder (w / w) Composition (3): Glass fiber 94% (W / W), fibrous binder 6% (W / W) Composition (4): PET fiber 94% (W / W), fibrous binder 6% (W / W) Composition (5): 94% aramid fiber (W / W), 6% fibrous binder (W / W) Composition (6): 97% recycled carbon fiber (w / w), 3% fibrous binder (w / w)
[0072] <Comparative Example S2 (Fiber Molded Sheet)> Except for using the fibrous binder of Comparative Example FB2, the procedure was the same as in Examples S1(1) to S1(6). 6 types Fiber molded sheets were obtained: Comparative Examples S2(1), S2(2), S2(3), S2(4), S2(5), and S2(6). Composition (1): 94% recycled carbon fiber (w / w), 6% fibrous binder (w / w) Composition (2): 94% carbon fiber (w / w), 6% fibrous binder (w / w) Composition (3): Glass fiber 94% (W / W), fibrous binder 6% (W / W) Composition (4): PET fiber 94% (W / W), fibrous binder 6% (W / W) Composition (5): 94% aramid fiber (W / W), 6% fibrous binder (W / W) Composition (6): 97% recycled carbon fiber (w / w), 3% fibrous binder (w / w)
[0073] <Comparative Example S3 (Fiber Molded Sheet)> Except for using the fibrous binder of Comparative Example FB3, the procedure was the same as in Examples S1(1) to S1(6). 6 types Fiber molded sheets were obtained as Comparative Examples S3(1), S3(2), S3(3), S3(4), S3(5), and S3(6). Composition (1): 94% recycled carbon fiber (w / w), 6% fibrous binder (w / w) Composition (2): 94% carbon fiber (w / w), 6% fibrous binder (w / w) Composition (3): Glass fiber 94% (W / W), fibrous binder 6% (W / W) Composition (4): PET fiber 94% (W / W), fibrous binder 6% (W / W) Composition (5): 94% aramid fiber (W / W), 6% fibrous binder (W / W) Composition (6): 97% recycled carbon fiber (w / w), 3% fibrous binder (w / w)
[0074] <Comparative Example S4 (Fiber Molded Sheet)> Except for using the fibrous binder of Comparative Example FB4, the procedure was the same as in Examples S1(1) to S1(6). 6 types Fiber molded sheets: Comparative Examples S4(1), S4(2), S4(3), S4(4), S3(5), and S3(6) were obtained. Composition (1): 94% recycled carbon fiber (w / w), 6% fibrous binder (w / w) Composition (2): 94% carbon fiber (w / w), 6% fibrous binder (w / w) Composition (3): Glass fiber 94% (W / W), fibrous binder 6% (W / W) Composition (4): PET fiber 94% (W / W), fibrous binder 6% (W / W) Composition (5): 94% aramid fiber (W / W), 6% fibrous binder (W / W) Composition (6): 97% recycled carbon fiber (w / w), 3% fibrous binder (w / w)
[0075] <Comparative Example S5 (Fiber Molded Sheet)> Except for using the fibrous binder of Comparative Example FB5, the procedure was the same as in Examples S1(1) to S1(6). 6 types Comparative Examples S5(1), S5(2), S5(3), S5(4), S5(5), and S5(6) of the fiber molded sheet were obtained. Composition (1): 94% recycled carbon fiber (w / w), 6% fibrous binder (w / w) Composition (2): 94% carbon fiber (w / w), 6% fibrous binder (w / w) Composition (3): Glass fiber 94% (W / W), fibrous binder 6% (W / W) Composition (4): PET fiber 94% (W / W), fibrous binder 6% (W / W) Composition (5): 94% aramid fiber (W / W), 6% fibrous binder (W / W) Composition (6): 97% recycled carbon fiber (w / w), 3% fibrous binder (w / w)
[0076] The shape, physical properties, and other characteristics and various performance parameters of the fibrous binder, main fiber material, and fibrous molded articles were measured and evaluated using the methods described below. The numerical values and evaluations related to the various shapes, physical properties, and performance parameters shown in this disclosure can be obtained using the following measurement and evaluation methods.
[0077] <Drainage of fibrous binders> The filtration efficiency of the fibrous binder was measured using a Canadian Standard Freeness Tester (manufactured by Tozai Seiki Co., Ltd.). Note that the term "filtration efficiency" is also referred to as "freeness" or "beating efficiency."
[0078] <Method for evaluating the physical properties of fibers> For the fibrous binder, the average fiber length (mm), average fiber diameter (μm), krill ratio, and fineness (%) were measured as follows. Furthermore, for the main fiber material, the average fiber length (mm), average fiber diameter (μm), and water content (%) were determined as follows.
[0079] <Average fiber length> (1) Fiber length of the fibrous binder Except for fibers with a length of less than 0.2 mm, fibers with a length of 0.2 mm or more were diluted to a solid content of 0.1 g and a slurry volume of 300 cc, and measured using an L&W Fiber Tester Plus Code912 (Lorenzen & Bettley). (2) Fiber length of the main fiber material (recycled carbon fiber) Considering the large variability in recycled carbon fibers, 20 fiber bundles were randomly selected, and each fiber bundle was measured using calipers. The average value was then calculated. (3) Fiber length of the main fiber material (other than recycled carbon fiber) We adopted the average fiber length (or cut size) value provided by the supplier.
[0080] <Average fiber diameter> (1) Average fiber diameter of fibrous binder Except for fibers with a length of less than 0.2 mm, fibers with a length of 0.2 mm or more were diluted to a solid content of 0.1 g and a slurry volume of 300 cc, and measured using an L&W Fiber Tester Plus Code912 (Lorenzen & Bettley). (2) Average fiber diameter of the main fiber material The fiber diameter of the main fiber material was determined by measuring 10 fibers randomly selected from a 500x magnified image using a Schottky emission electron microscope JSM-7900F (manufactured by JEOL Ltd.), and then calculating the average value.
[0081] <Moisture content of main fiber material> The moisture content of the main fiber material was determined using a halogen moisture meter HB43 (manufactured by Mettler-Toledo Co., Ltd.).
[0082] <Krill ratio> Ultraviolet or infrared light was incident on a slurry of fibrous binder, and the reduction in transmitted light from the incident light was determined for each case of ultraviolet or infrared light source. The krill ratio was calculated using the ultraviolet and infrared reduction amounts based on Equation 1 below. The slurry used in the test was prepared by diluting the fibrous binder to a solid content of 0.1 g and a slurry volume of 300 cc. An L&W Fiber Tester Plus Code912 (Lorenzen & Bettley) was used as the measuring instrument.
[0083] <Expression 1> (CR) = (UVR) / (IRR) In Equation 1, CR, UVR, and IRR are defined as follows: CR: Krill ratio UVR: UV reduction amount IRR: Infrared Reduction
[0084] <Foil ratio> The ratio of fine fibers (fibers with a length of less than 0.2 mm), i.e., the fineness ratio, was calculated using the following formula 2.
[0085] <Expression 2> (FR) = (FFL) / (WFL) × 100 (%) In Equation 2, FR, FFL, and WFL are defined as follows: FR: Fine Rate FFL: Total length of fine fibers (fibers with a length of less than 0.2 mm) WFL: Total length of all fibers (fibers less than 0.2 mm in length + fibers 0.2 mm or longer)
[0086] The above FFL and WFL values were obtained by diluting the fibrous binder to a solid content of 0.1 g and slurry to 300 cc, and measuring them using an L&W Fiber Tester Plus Code 912 (Lorenzen & Bettley).
[0087] <Dimensions and weight of the fiber molded product> The dimensions of the fiber molded body were determined by measuring them using a ruler or similar tool as follows. The fiber molded body samples used for measurement were conditioned overnight in an atmosphere of 23°C and 50% RH. The weight of the conditioned fiber molded body was measured using an electronic balance. Using the obtained measurements, the basis weight and density of the fiber molded body were calculated as follows.
[0088] <Thickness of the fiber molded body> For sheet-shaped fiber molded materials, the sheet thickness (in μm) was measured using a thickness tester TM600 (manufactured by Kumagai Riki Kogyo Co., Ltd.) at a surface pressure of 100 kPa.
[0089] <Basis weight of fiber molded product> For sheet-like fiber molded products, the basis weight (unit: g / m²) can be calculated from its weight and area. 2 ) was sought.
[0090] <Density of fiber molded material> Density of fiber molded material (unit: g / cm³) 3 ) is the basis weight (unit: g / m²) of the fiber molded product.2 The basis weight was calculated by dividing the basis weight by the sheet thickness (unit: μm) of the fiber molded product. The basis weight and sheet thickness of the fiber molded product were calculated from the measurement results obtained by the above method.
[0091] <Tensile strength of fiber molded articles> A sheet-like fibrous material was conditioned at 23°C and 50% humidity for 12 hours. Under these conditions, a test specimen (15 mm wide, 150 mm long) was cut, and its tensile strength (kN / m) was measured using an L&W Tensile Tester Code 066 (Laurentzen & Bettley).
[0092] Table 1-1 shows the measurement results for the fibrous binder used as the binding component. Table 1-2 shows the measurement results for the sheet-like recycled carbon fiber molded product of formulation (1) (94% recycled carbon fiber, 6% binding component). Table 1-3 shows the measurement results for the sheet-like carbon fiber molded product of formulation (2) (94% carbon fiber, 6% binding component). Table 1-4 shows the measurement results for the sheet-like glass fiber molded product of formulation (3) (94% glass fiber, 6% binding component). Table 1-5 shows the measurement results for the sheet-like PET fiber molded product of formulation (4) (94% PET fiber, 6% binding component). Table 1-6 shows the measurement results for the sheet-like aramid fiber molded product of formulation (5) (94% aramid fiber, 6% binding component). Table 1-7 shows the measurement results for the sheet-like recycled carbon fiber molded product of formulation (6) (94% recycled carbon fiber, 6% binding component).
[0093] [Table 1-1]
[0094] [Table 1-2]
[0095] [Table 1-3]
[0096] Table 1-4
[0097] Table 1-5
[0098] Table 1-6
[0099] Table 1-7
Claims
1. A fiber molded body, The aforementioned fibrous molded body comprises a main fibrous material and a fibrous binder. The ratio of the main fiber material to the fibrous binder is 1 to 20 parts by weight of the fibrous binder per 100 parts by weight of the main fiber material. The aforementioned main fiber material is carbon fiber. The krill ratio of the fibrous binder is 1.25 to 3.
00. Fiber molded body.
2. The fibrous molded article according to claim 1, wherein the average fiber length of the fibrous binder is 0.30 to 2.50 mm.
3. The fiber molded article according to claim 1, wherein the carbon fibers are first-use carbon fibers, recycled carbon fibers, or a mixture thereof.
4. The fibrous molded article according to claim 1, wherein the fibrous binder is fibrillated cellulose fiber.
5. The fibrous molded article according to claim 1, wherein the fineness of the fibrous binder is 95% or less.
6. A fiber-reinforced resin molded article comprising a fiber molded article according to any one of claims 1 to 5 and a resin component impregnated in the fiber molded article.
Citation Information
Patent Citations
Fiber sheet containing hydrophobicized microfibrous cellulose
JP2008248441A
Lithium ion secondary battery separator and lithium ion secondary battery arranged by use thereof
JP2016171048A
Dispersant for wet type paper, dispersion composition for wet type paper and fiber sheet
JP2017057511A
Wet nonwoven fabric of short carbon fiber, and carbon fiber reinforced resin
JP2020158912A
Carbon fiber-containing wet type unwoven fabric
JP2022070291A