Negative electrode active material for secondary batteries, method for producing same, negative electrode and secondary battery

JPWO2023163012A5Pending Publication Date: 2024-11-05
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024503191
Authority / Receiving Office
JP · JP
Patent Type
Applications
Filing Date
2024-06-27
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Silicon-containing materials for negative electrodes in secondary batteries have high capacity but low conductivity and undergo significant expansion and contraction with lithium ion insertion and release, leading to decreased current collection ability and capacity retention.

Method used

A composite particle structure is developed, where Si-containing particles are connected by a conductive polymer, with a sulfur content less than 0.05% by mass, and a particle size distribution that suppresses expansion, forming a network for improved conductivity and capacity retention.

Benefits of technology

The composite particle structure enhances the conductivity and capacity retention of the negative electrode, maintaining current collection ability and reducing expansion, thereby improving the performance of silicon-containing materials in secondary batteries.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a negative electrode active material for secondary batteries, the negative electrode active material containing composite particles that contain a conductive polymer and Si-containing particles, wherein: a plurality of Si-containing particles are connected by means of the conductive polymer in the composite particles; the particle diameter D50 at the cumulative volume of 50% in the volume-based particle size distribution of the composite particles is 100 µm or less; the composite particles contain elemental sulfur; and the content of the elemental sulfur in the composite particles is less than 0.05% by mass.
Need to check novelty before this filing date? Find Prior Art

Description

Negative electrode active material for secondary battery, method of manufacturing the same, negative electrode and secondary battery

[0001] The present invention relates to a negative electrode active material for a secondary battery, a method for producing the same, a negative electrode, and a secondary battery.

[0002] Silicon (Si)-containing materials are known to be able to store more lithium ions per unit volume than carbonaceous materials such as graphite, and therefore, their use as negative electrode active materials for secondary batteries has been investigated.

[0003] Patent Document 1 proposes organic polymer-silicon composite particles for use as a negative electrode active material in lithium secondary batteries, which are organic polymer-silicon composite particles comprising an organic polymer matrix having free spaces and silicon microparticles, wherein the organic polymer matrix having free spaces is at least one selected from polypyrrole, polyaniline, and polythiophene, silicon microparticles are dispersed within the organic polymer matrix having free spaces, and a metal coating layer is formed on the surface of the organic polymer-silicon composite particles.

[0004] Non-Patent Document 1 proposes a negative electrode in which a conductive organic polymer and silicon particles are combined on a current collector.

[0005] Patent No. 5712439 (Special Publication No. 2013-522820)

[0006] Nat. Commun. 2013, 4, 1943

[0007] Although the Si-containing material has a high capacity, it has a lower electrical conductivity than the carbonaceous material and undergoes a large expansion and contraction due to the absorption and desorption of lithium ions. When the Si-containing material expands, the negative electrode expands, and when the Si-containing material contracts, the current collection ability of the negative electrode decreases.

[0008] In view of the above, one aspect of the present invention relates to a negative electrode active material for a secondary battery, comprising composite particles containing a conductive polymer and a Si-containing particle, wherein a plurality of the Si-containing particles are connected in the composite particle via the conductive polymer, the composite particle has a particle size D50 of 100 μm or less when a cumulative volume of the composite particle is 50% in a volume-based particle size distribution, and the composite particle contains elemental sulfur, and the content of the elemental sulfur in the composite particle is less than 0.05 mass%.

[0009] Another aspect of the present invention relates to a negative electrode for a secondary battery, which includes the above-mentioned negative electrode active material for a secondary battery.

[0010] Yet another aspect of the present invention relates to a secondary battery including a positive electrode, a negative electrode, and a non-aqueous electrolyte, wherein the negative electrode is the above-described negative electrode for a secondary battery.

[0011] Yet another aspect of the present invention relates to a method for producing a negative electrode active material for a secondary battery, the method comprising: a first step of synthesizing a composite comprising a conductive polymer and a Si-containing particle by mixing a monomer that is a raw material of a conductive polymer, a polymerization initiator containing elemental sulfur, and Si-containing particles and polymerizing the monomer; a second step of pulverizing the composite to obtain composite particles having a particle size D50 of 100 μm or less at a cumulative volume of 50% in a volume-based particle size distribution; and a third step of washing the composite particles until the content of the elemental sulfur in the composite particles is less than 0.05 mass%.

[0012] According to the present invention, the expansion of a negative electrode for a secondary battery containing Si-containing particles is suppressed. The novel features of the present invention are set forth in the appended claims, but the present invention, both in terms of structure and content, together with other objects and features of the present invention, will be better understood from the following detailed description taken in conjunction with the drawings.

[0013] 1 is a vertical cross-sectional view showing the configuration of a secondary battery according to one embodiment of the present invention.

[0014] The following describes embodiments of the present disclosure using examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values, materials, etc. may be used as examples. However, other numerical values, materials, etc. may be used as long as the effects of the present disclosure are obtained. Note that components other than those characteristic of the present disclosure may be those of known secondary batteries. In this specification, when a "range between numerical values ​​A and B" is mentioned, the range includes numerical values ​​A and B. The present disclosure also encompasses combinations of features recited in two or more claims arbitrarily selected from the multiple claims recited in the appended claims. In other words, features recited in two or more claims arbitrarily selected from the multiple claims recited in the appended claims may be combined as long as no technical contradiction arises.

[0015] <Negative Electrode Active Material> The negative electrode active material for a secondary battery according to this embodiment includes composite particles, and each composite particle includes a conductive polymer and a Si-containing particle. The negative electrode active material may include a material other than the composite particles. Examples of the material other than the composite particles include a carbonaceous material, a Si-containing material, and a Sn-containing material. One type of negative electrode active material may be used alone, or two or more types may be used in combination.

[0016] <Composite Particles> Composite particles are particles containing a conductive polymer and a Si-containing particle. The particle shape of the composite particle is not particularly limited. In the composite particle, multiple Si-containing particles are connected by the conductive polymer. In other words, multiple Si-containing particles are dispersed in a matrix of the conductive polymer. In the composite particle, for example, at least a portion of the surface of each Si-containing particle is covered with the conductive polymer, and such Si-containing particles aggregate together with the conductive polymer to form the composite particle.

[0017] The content of the composite particles in the negative electrode active material is not particularly limited and may be 100%. However, from the viewpoint of more significantly suppressing expansion of the negative electrode while ensuring high capacity, the content may be 5% by mass to 50% by mass, or 5% by mass to 30% by mass.

[0018] The composite particles have the following properties. First, because the composite particles contain Si-containing particles, they have high capacity and significantly increase the capacity of the negative electrode active material or negative electrode. In particular, when nanosilicon particles are used as the Si-containing particles, the nanosilicon particles are essentially 100% (at least 90% by mass) formed solely of silicon, resulting in composite particles with even higher capacity. Note that conductive polymers can also exhibit capacity through faradaic or non-faradaic reactions.

[0019] Second, by connecting multiple Si-containing particles with a conductive polymer, a good electron-conducting network is formed within each composite particle, thereby enhancing the conductivity of the composite particle. To form a better electron-conducting network, it is desirable to enhance the conductivity of the conductive polymer. For example, the conductivity can be significantly enhanced by doping the conductive polymer with a dopant.

[0020] Third, the composite particles have free volume derived from the conductive polymer. Free volume generally refers to the volume of voids formed within the conductive polymer domain. The free volume absorbs the volume change of the Si-containing particles accompanying the absorption and desorption of lithium ions, or the stress caused by the volume change. Therefore, expansion of the negative electrode due to repeated charge and discharge is suppressed, the current collection ability of the negative electrode is maintained, and the capacity is more easily maintained.

[0021] Fourth, the Si-containing particles are covered with a conductive polymer, which limits contact between the Si-containing particles and the electrolyte and suppresses side reactions. This suppression of side reactions allows the capacity retention rate to be maintained high, and the volume of by-products is reduced, thereby enhancing the effect of suppressing expansion of the negative electrode.

[0022] The content of the Si-containing particles in the composite particles is, for example, 30% by mass or more, 50% by mass or more, 55% by mass or more, or even 60% by mass or more. The higher the content of the Si-containing particles in the composite particles, the higher the capacity of the negative electrode can be obtained. However, from the viewpoint of enhancing the effect of suppressing the expansion of the negative electrode, it is desirable that the content of the Si-containing particles in the composite particles is not excessively high, and may be 90% by mass or less, or 80% by mass or less.

[0023] The remainder of the composite particle other than the Si-containing particle is generally a conductive polymer, and 90% to 100% of the remainder may be a conductive polymer.

[0024] Since the composite particles contain a conductive polymer, the powder resistivity is lower than that of the composite particles containing a non-conductive polymer, for example, 10 3 Ω cm to 10 7 Ω cm. When the composite particles have such a volume resistivity, the internal resistance of the negative electrode is reduced, and the interfacial resistance between the negative electrode mixture layer and the current collector, which will be described later, is also reduced. As a result, the current collecting ability of the negative electrode is maintained at a high level, and the capacity is also likely to be maintained at a high level.

[0025] The powder resistivity of the composite particles is 204 kgf / cm 2 The measurement is carried out by a four-probe method using a powder resistivity measuring device (for example, Loresta SP manufactured by Mitsubishi Chemical Analytic Co., Ltd. (currently Nitto Seiko Analytic Co., Ltd.)) under pressure.

[0026] The particle diameter D50 (hereinafter referred to as "average particle diameter") at which the cumulative volume of the composite particles in the volume-based particle size distribution is 50% may be, for example, 100 μm or less, 50 μm or less, or 30 μm or less. When the average particle diameter of the composite particles has such an upper limit, local volume changes and stress concentrations of the Si-containing particles are less likely to occur, and current collection properties are more easily maintained. Furthermore, such a particle form makes it easier to control the sulfur content in the composite particles to less than 0.05 mass%.

[0027] On the other hand, the average particle size of the composite particles may be, for example, 1 μm or more, 10 μm or more, or 20 μm or more. When the average particle size of the composite particles has such a lower limit, the surface area of ​​the Si-containing particles does not become excessively large, which is effective in suppressing side reactions and makes it easier to ensure a high capacity.

[0028] The volume-based particle size distribution of the composite particles can be measured by a laser diffraction / scattering method using a particle size distribution measuring device (e.g., MT3000II manufactured by Microtrac Co., Ltd.) A dispersion of the composite particles in pure water is used for the measurement.

[0029] The particle diameter D10 at 10% cumulative volume in the volume-based particle size distribution of the composite particles may be 0.5 μm or more (e.g., 0.5 μm to 50 μm). In this case, the proportion of fine composite particles is low, which is effective in suppressing side reactions and also makes it easier to ensure a high capacity.

[0030] The particle diameter D90 at 90% cumulative volume in the volume-based particle size distribution of the composite particles may be 500 μm or less (e.g., 50 μm to 500 μm or 100 μm to 300 μm). In this case, the proportion of excessively large composite particles is low, local volume changes and stress concentrations are less likely to occur, and current collection performance is more easily maintained.

[0031] <Conductive Polymer> A conductive polymer is an organic polymer that exhibits conductivity either alone or by doping with a dopant. A typical example of a conductive polymer is a π-conjugated polymer.

[0032] Examples of π-conjugated polymers include polymers with a basic skeleton such as polypyrrole, polythiophene, polyaniline, polyfuran, polyacetylene, polyphenylene, polyphenylene vinylene, polyacene, and polythiophene vinylene. These polymers also include homopolymers, copolymers of two or more monomers, and derivatives thereof (e.g., substituted products having substituents). For example, polyaniline includes poly(N-methylaniline) in which at least some of the amino groups are substituted with methyl groups. Furthermore, polythiophene includes poly(3,4-ethylenedioxythiophene). However, these are merely specific examples, and conductive polymers are not limited to these specific examples.

[0033] The conductive polymer may be doped with a dopant. Doping with a dopant increases the conductivity of the conductive polymer, reduces the powder resistivity of the composite particles, and makes it easier to maintain current collection. The dopant, for example, donates protons to the conductive polymer to generate anions. When the anions are attached to the protonated conductive polymer, the conductive polymer stably exhibits conductivity.

[0034] The content of the dopant in the composite particles is not particularly limited, but may be, for example, 0.1% by mass to 10% by mass, or 1% by mass to 5% by mass.

[0035] The dopant may be appropriately selected depending on the type of conductive polymer. The dopant may have, for example, an oxo acid group capable of releasing a proton. The dopant may be an oxo acid, an oxo acid ester, or the like capable of releasing a proton. These may be in an ionic (anionic) state.

[0036] Ion-state dopants include sulfate ions, nitrate ions, phosphate ions, borate ions, and halide ions (F - , Cl - ,Br - , I - ), benzenesulfonate ion, naphthalenesulfonate ion, toluenesulfonate ion, methanesulfonate ion (CF3SO3 - ), perchlorate ion (ClO - ), tetrafluoroborate ion (BF4 - ), hexafluorophosphate ion (PF6 - ), fluorosulfate ion (FSO3 - ), bis(fluorosulfonyl)imide ion (N(FSO2)2 - ), bis(trifluoromethanesulfonyl)imide ion (N(CF3SO2)2 - These may be used alone or in combination of two or more.

[0037] The dopant may be a polymer. Examples of the polymer include polyvinyl sulfonic acid, polystyrene sulfonic acid, polyallylsulfonic acid, polyacrylic sulfonic acid, polymethacrylic sulfonic acid, poly(2-acrylamido-2-methylpropanesulfonic acid), polyisoprene sulfonic acid, and polyacrylic acid. These may be homopolymers or copolymers of two or more monomers. These may be in an ionic (anionic) state. These may be used alone or in combination of two or more.

[0038] The dopant may contain phosphorus. More specifically, the dopant may contain phosphoric acid, phosphonic acid, phosphate ester, phosphonate ester, etc. When the conductive polymer contains phosphorus, it may be determined that the conductive polymer contains a dopant containing phosphorus.

[0039] The phosphate ester may be, for example, phytic acid (inositol hexaphosphate ester). In particular, when the conductive polymer contains polyaniline, it is desirable to use phytic acid as a dopant, as it has affinity for both the Si-containing particles and the polyaniline. Phytic acid acts as a proton dopant for the conductive polymer and also forms hydrogen bonds with the hydroxyl groups on the Si surface. This makes it easier for the Si-containing particles to be uniformly coated with the conductive polymer.

[0040] <Polyaniline> Polyaniline is a polyaniline obtained by polymerizing aniline (C 6 H 5 -NH 2 ) as a monomer. As mentioned above, polyaniline includes polyaniline and its derivatives. For example, derivatives in which an alkyl group such as a methyl group is added to at least a portion of the benzene ring, derivatives in which a halogen group or the like is added to at least a portion of the benzene ring, and derivatives in which an alkyl group such as a methyl group is added to at least a portion of the amino group are also included in the polyaniline of the present invention, as long as they are conductive polymers with aniline as the basic skeleton.

[0041] The structure of polyaniline includes (-C 6 H 4 a structural unit capable of forming a benzonoid skeleton of (-NH-) (also called an IP structure), and 6 H 4 ═N—) (also called NP structure) structural units that can form a quinoid skeleton.

[0042] <Si-containing particles> The Si-containing particles are particulate Si-containing materials, and the particle shape is not particularly limited. Examples of the Si-containing material include simple Si, silicon alloys, and silicon compounds.

[0043] The Si-containing particles may be particles containing a lithium ion conductive phase and a silicon phase dispersed in the lithium ion conductive phase. 2 phases, silicate phases (eg, lithium silicate phases), carbon phases, and the like may be used.

[0044] SiO 2 phase and SiO 2 The particles containing the silicon phase dispersed in the SiO x (0.5≦x<2 (e.g., 0.5≦x<1.6)). 2 In the particles containing the lithium silicate phase and the silicon phase dispersed in the lithium silicate phase, the lithium silicate phase is 2z SiO 2+z (0<z<1 (e.g., z=1 / 2)).

[0045] The average particle size of the Si-containing particles is, for example, 10 nm to 500 nm, and may be 30 nm to 50 nm. Nanosilicon particles having such an average particle size may also be used. Nanosilicon particles are easily available. When the average particle size of the Si-containing particles is within the above range, composite particles of an appropriate size are easily synthesized, and the volume change of the composite particles is more significantly suppressed.

[0046] The average particle size of the Si-containing particles is preferably measured before the first charge / discharge, but may also be measured after multiple charge / discharge cycles after the battery is assembled. In this case, it is preferable to measure the average particle size of the Si-containing particles collected from the negative electrode removed from the fully discharged battery.

[0047] The amount of electricity charged when a battery in a fully discharged state (Depth of Discharge: DOD = 100%) is charged to a fully charged state (State of Charge: SOC = 100%, DOD = 0%) corresponds to the rated capacity of the battery. The voltage of a battery in a fully charged state corresponds to the end-of-charge voltage. The voltage of a battery in a fully discharged state corresponds to the end-of-charge voltage.

[0048] The average particle size of the Si-containing particles is measured by observing the cross section of the negative electrode using a SEM or TEM. Specifically, it is determined by averaging the maximum diameters of 100 randomly selected Si-containing particles.

[0049] At least a portion of the surface of the Si-containing particle may be covered with a conductive carbonaceous material. In this case, the conductivity of the Si-containing particle is increased, the current collecting ability of the negative electrode is more easily maintained, and the capacity is more easily maintained. For example, the Si-containing particle and a raw material of the carbonaceous material (pitch, tar, carbon black, etc.) may be mixed and baked at a predetermined temperature to cover at least a portion of the surface of the Si-containing particle with the conductive carbonaceous material.

[0050] <Elemental Sulfur> The composite particles may contain elemental sulfur. The elemental sulfur may be derived from an oxidizing agent used as an initiator when polymerizing the conductive polymer.

[0051] Because elemental sulfur may generate harmful sulfur-based gases through decomposition during charging and discharging, it is desirable that the content of elemental sulfur in the composite particles be low. For example, it is desirable that the content be less than 0.05% by mass, and it may be 0.01% by mass or less. On the other hand, a trace amount of sulfonic acid groups is expected to promote dissociation of lithium salts contained in the electrolyte in the conductive polymer domains, thereby improving lithium ion conductivity. From the viewpoint of achieving such an effect, it is desirable that the content of elemental sulfur in the composite particles be 0.001% by mass or more.

[0052] The sulfur content of the composite particles can be measured, for example, by inductively coupled plasma atomic emission spectroscopy (ICP-AES). Specifically, a sample of the composite particles is dissolved in a heated acid solution (a mixed acid of hydrofluoric acid, nitric acid, and sulfuric acid), the sulfur element is thoroughly extracted, the solution residue is removed by filtration, and the resulting filtrate is then analyzed by ICP-AES to measure the spectral intensity of sulfur. Subsequently, a calibration curve is created using a commercially available standard solution of sulfur element, and the sulfur content is calculated.

[0053] <Nitrogen element> The composite particles may further contain nitrogen element. The nitrogen element may be derived from an oxidizing agent used as an initiator when polymerizing the conductive polymer. The sulfur element and the nitrogen element may be derived from, for example, ammonium persulfate. Ammonium persulfate is suitable as a polymerization initiator when polymerizing aniline to produce polyaniline.

[0054] <Preferred embodiment> In one preferred embodiment of the composite particles, the conductive polymer is polyaniline and the dopant is phytic acid. When ammonium persulfate is used in synthesizing polyaniline, the composite particles may contain elemental sulfur. To control the content of elemental sulfur in the composite particles to a desired range, it is desirable to perform a predetermined washing step.

[0055] <Method for Producing Composite Particles> A method for producing composite particles contained in a negative electrode active material for a secondary battery includes, for example, the following first to third steps.

[0056] (i) First Step The first step is a step of preparing a polymerization liquid and synthesizing a composite. The polymerization liquid is prepared by mixing a monomer, which is a raw material for the conductive polymer, a polymerization initiator containing elemental sulfur, Si-containing particles, and a dopant agent. When synthesizing, for example, polyaniline as the conductive polymer, aniline is used as the monomer. As the polymerization initiator containing elemental sulfur, a peroxide is preferable, and for example, ammonium persulfate is used. As the Si-containing particles, for example, nanoparticles with an average particle size of 10 nm to 500 nm are used.

[0057] When the initiator is dissolved in the polymerization solution, polymerization of the monomer proceeds to produce a conductive polymer. At this time, the conductive polymer grows so as to cover at least a portion of the surface of the Si-containing particle. As a result, a composite containing the conductive polymer and the Si-containing particle and having a structure in which a plurality of Si-containing particles are connected by the conductive polymer is obtained.

[0058] (ii) Second Step: The second step is a step of pulverizing the composite. A pulverizer such as a mixer, mill, or mortar may be used for pulverization. By pulverization, composite particles of a desired size are produced, for example, particles having a particle diameter D50 (average particle diameter) of 100 μm or less at a cumulative volume of 50% in the volume-based particle size distribution. This significantly improves the cleaning effect in the subsequent cleaning step.

[0059] (iii) Step 3 Step 3 is a step of washing the composite particles. It is desirable to wash the composite particles until the sulfur content in the composite particles is less than 0.05% by mass. The washing method is not particularly limited, but may be performed by washing with water. The sulfur element is derived from a polymerization initiator containing sulfur element. If a large amount of polymerization initiator residue remains in the composite particles, it tends to induce side reactions in the battery, which reduces battery performance and may generate harmful sulfur-based gases as the particles decompose. On the other hand, such disadvantages can be prevented by reducing the sulfur content in the composite particles to less than 0.05% by mass through washing.

[0060] The composite may be washed before being pulverized. In this case, washing of the composite particles after pulverization may be omitted, but it is preferable to wash the composite particles after pulverization as well.

[0061] <Negative electrode> The negative electrode comprises a negative electrode mixture layer containing a negative electrode active material and a negative electrode current collector. The negative electrode mixture layer can be formed by applying a negative electrode slurry, in which the components of the negative electrode mixture are dispersed in a dispersion medium, to the surface of the negative electrode current collector and drying the applied layer. The dried coating film may be rolled if necessary.

[0062] The negative electrode mixture includes a negative electrode active material as an essential component, and may include optional components such as a binder, a thickener, and a conductive agent. The negative electrode active material includes the composite particles described above, and may also include materials other than the composite particles. The negative electrode active material may include, for example, a carbonaceous material such as graphite, easily graphitizable carbon (soft carbon), or hardly graphitizable carbon (hard carbon).

[0063] As the binder for the negative electrode, for example, a resin material is used. Examples of the binder include fluororesin, polyolefin resin, polyamide resin, polyimide resin, acrylic resin, vinyl resin, and rubber-like material (for example, styrene butadiene copolymer (SBR)). One type of binder may be used alone, or two or more types may be used in combination.

[0064] Examples of thickeners include cellulose derivatives such as cellulose ether. Examples of cellulose derivatives include carboxymethyl cellulose (CMC) and its modified forms, methyl cellulose, etc. One type of thickener may be used alone, or two or more types may be used in combination.

[0065] Examples of conductive materials include carbon nanotubes (CNTs), carbon fibers other than CNTs, and conductive particles (for example, carbon black and graphite).

[0066] The dispersion medium used in the negative electrode slurry is not particularly limited, but examples thereof include water, alcohol, N-methyl-2-pyrrolidone (NMP), and mixed solvents thereof.

[0067] The negative electrode current collector may be, for example, a metal foil. The negative electrode current collector may be porous. Examples of the material for the negative electrode current collector include stainless steel, nickel, nickel alloy, copper, and copper alloy. The thickness of the negative electrode current collector is not particularly limited, but may be, for example, 1 to 50 μm, or 5 to 30 μm.

[0068] <Positive Electrode> The positive electrode includes a positive electrode active material. The positive electrode typically includes a positive electrode current collector and a layer of positive electrode mixture (hereinafter referred to as a "positive electrode mixture layer") held on the positive electrode current collector. The positive electrode mixture layer can be formed by applying a positive electrode slurry, in which the components of the positive electrode mixture are dispersed in a dispersion medium, to the surface of the positive electrode current collector and drying the slurry. The dried coating may be rolled as necessary. The positive electrode mixture includes a positive electrode active material as an essential component and may include a binder, a thickener, etc. as optional components.

[0069] The positive electrode active material may be any material that can be used as a positive electrode active material for a nonaqueous electrolyte secondary battery (particularly a lithium ion secondary battery), but from the viewpoint of increasing capacity, it contains a lithium transition metal composite oxide (composite oxide N) containing at least nickel as a transition metal. The proportion of the composite oxide N in the positive electrode active material is, for example, 70 mass % or more, or may be 90 mass % or more, or may be 95 mass % or more.

[0070] The composite oxide N may be, for example, a lithium transition metal composite oxide having a layered rock salt structure and containing Ni and at least one selected from the group consisting of Co, Mn, and Al. Hereinafter, a lithium transition metal composite oxide having a layered rock salt structure and containing Ni and at least one selected from the group consisting of Co, Mn, and Al, in which the proportion of Ni among metal elements other than Li is 80 atomic % or more, will also be referred to as a "composite oxide HN." The proportion of the composite oxide HN in the composite oxide N used as the positive electrode active material is, for example, 90 mass % or more, or even 95 mass % or more, or even 100%. The higher the proportion of Ni, the more lithium ions can be extracted from the composite oxide HN during charging, thereby increasing the capacity. Co, Mn, and Al contribute to stabilizing the crystal structure of the composite oxide HN with a high Ni content.

[0071] The composite oxide HN may be, for example, a compound represented by the formula: Li α Ni(1-x1-x2-yz)Co x1 Mn x2 Al y M z O 2+β The element M is an element other than Li, Ni, Co, Mn, Al, and oxygen. Mn contributes to stabilizing the crystal structure of the composite oxide HN, and containing inexpensive Mn in the composite oxide HN is advantageous for cost reduction. Al contributes to stabilizing the crystal structure of the composite oxide HN.

[0072] In the above formula, α, which represents the atomic ratio of lithium, is, for example, 0.95≦α≦1.05. α increases or decreases with charge and discharge. In (2+β), which represents the atomic ratio of oxygen, β satisfies −0.05≦β≦0.05.

[0073] The atomic ratio of Ni, 1-x1-x2-y-z (=v), is, for example, 0.8 or more, or may be 0.85 or more, or 0.90 or more, or 0.95 or more. Furthermore, v may be 0.98 or less, or may be 0.95 or less. The atomic ratio of Co, x1, is, for example, 0.1 or less (0≦x1≦0.1), the atomic ratio of Mn, x2, is, for example, 0.1 or less (0≦x2≦0.1), the atomic ratio of Al, y, is, for example, 0.1 or less (0≦y≦0.1), and the atomic ratio of M, z, is, for example, 0≦z≦0.10.

[0074] The element M may be at least one selected from the group consisting of Ti, Zr, Nb, Mo, W, Fe, Zn, B, Si, Mg, Ca, Sr, Sc, and Y. In particular, when at least one selected from the group consisting of Nb, Sr, and Ca is contained in the composite oxide HN, it is thought that the surface structure of the composite oxide HN is stabilized, the resistance is reduced, and metal elution is further suppressed. It is more effective if the element M is unevenly distributed in the vicinity of the particle surface of the composite oxide HN.

[0075] As the binder for the positive electrode, for example, a resin material is used. Examples of the binder include fluororesin, polyolefin resin, polyamide resin, polyimide resin, acrylic resin, vinyl resin, etc. One type of binder may be used alone, or two or more types may be used in combination.

[0076] Examples of conductive materials include carbon nanotubes (CNTs), carbon fibers other than CNTs, and conductive particles (for example, carbon black and graphite).

[0077] The dispersion medium used in the positive electrode slurry is not particularly limited, but examples thereof include water, alcohol, N-methyl-2-pyrrolidone (NMP), and mixed solvents thereof.

[0078] The positive electrode current collector may be, for example, a metal foil. The positive electrode current collector may be porous. Examples of porous current collectors include nets, punched sheets, and expanded metals. Examples of materials for the positive electrode current collector include stainless steel, aluminum, aluminum alloys, and titanium. The thickness of the positive electrode current collector is not particularly limited, but may be, for example, 1 to 50 μm, or 5 to 30 μm.

[0079] <Electrolyte> The electrolyte may be a liquid electrolyte (electrolytic solution), a gel electrolyte, or a solid electrolyte. The gel electrolyte includes a lithium salt and a matrix polymer, or a lithium salt, a non-aqueous solvent, and a matrix polymer. For example, a polymer material that absorbs a non-aqueous solvent and gels is used as the matrix polymer. Examples of polymer materials include fluororesin, acrylic resin, polyether resin, and polyethylene oxide. The solid electrolyte may be an inorganic solid electrolyte. For example, materials known in all-solid-state lithium-ion secondary batteries (e.g., oxide-based solid electrolytes, sulfide-based solid electrolytes, halide-based solid electrolytes, etc.) are used as the inorganic solid electrolyte. For example, a liquid electrolyte (electrolytic solution) includes a solvent and a solute dissolved in the solvent. The solute is an electrolyte salt that ionically dissociates in the electrolyte. The solute may include, for example, a lithium salt. Components of the electrolyte other than the solvent and solute are additives. The electrolyte may contain various additives.

[0080] The solvent may be an aqueous solvent or a non-aqueous solvent. Examples of non-aqueous solvents that can be used include cyclic carbonates, chain carbonates, cyclic carboxylic acid esters, and chain carboxylic acid esters. Examples of cyclic carbonates include propylene carbonate (PC), ethylene carbonate (EC), and vinylene carbonate (VC). Examples of chain carbonates include diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC). Examples of cyclic carboxylic acid esters include γ-butyrolactone (GBL) and γ-valerolactone (GVL). Examples of chain carboxylic acid esters include methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate (EP). One type of non-aqueous solvent may be used alone, or two or more types may be used in combination.

[0081] Examples of lithium salts include lithium salts of chlorine-containing acids (LiClO4, LiAlCl4, LiB 10 Cl 10 etc.), lithium salts of fluorine-containing acids (LiPF6, LiPF 2 O 2 , LiBF4, LiSbF6, LiAsF6, LiCF3SO3, LiCF3CO2, etc.), lithium salts of fluorine-containing acid imides (LiN(FSO2)2, LiN(CF3SO2)2, LiN(CF3SO2)(CF4F9SO2), LiN(CF5SO2)2, etc.), lithium halides (LiCl, LiBr, LiI, etc.), etc., can be used. One type of lithium salt may be used alone, or two or more types may be used in combination.

[0082] The concentration of the lithium salt in the electrolyte may be 1 mol / L or more and 2 mol / L or less, or may be 1 mol / L or more and 1.5 mol / L or less, but is not limited to the above.

[0083] <Separator> It is desirable to interpose a separator between the positive electrode and the negative electrode. The separator has high ion permeability and adequate mechanical strength and insulating properties. The separator may be made of a microporous thin film, woven fabric, nonwoven fabric, or the like. The separator is preferably made of polyolefin such as polypropylene or polyethylene.

[0084] <Secondary Battery> An example of the structure of a secondary battery is a structure in which an electrode group formed by winding a positive electrode and a negative electrode with a separator interposed therebetween is housed in an exterior body together with an electrolyte solution. However, this is not limited thereto, and other forms of electrode groups may also be applied. For example, a stacked electrode group in which a positive electrode and a negative electrode are stacked with a separator interposed therebetween may also be used. The shape of the secondary battery is also not limited, and may be, for example, a cylindrical type, a prismatic type, a coin type, a button type, a laminate type, or the like. Secondary batteries include nonaqueous electrolyte secondary batteries such as lithium ion secondary batteries containing an electrolyte solution and solid batteries containing a gel electrolyte or a solid electrolyte.

[0085] The structure of the secondary battery will be described below with reference to Fig. 1. Fig. 1 is a longitudinal cross-sectional view of a cylindrical secondary battery 10 that is an example of this embodiment. However, the present disclosure is not limited to the following configuration.

[0086] The secondary battery 10 includes an electrode group 18, an electrolyte (not shown), and a cylindrical battery can 22 with a bottom that accommodates these. A sealing body 11 is crimped to the opening of the battery can 22 via a gasket 21, thereby sealing the battery. The sealing body 11 includes a valve body 12, a metal plate 13, and an annular insulating member 14 interposed between the valve body 12 and the metal plate 13. The valve body 12 and the metal plate 13 are connected to each other at their respective centers. A positive electrode lead 15a extending from the positive electrode 15 is connected to the metal plate 13. Thus, the valve body 12 functions as an external terminal for the positive electrode. A negative electrode lead 16a extending from the negative electrode 16 is connected to the inner bottom surface of the battery can 22. An annular groove 22a is formed near the open end of the battery can 22. A first insulating plate 23 is disposed between one end face of the electrode group 18 and the annular groove 22a. A second insulating plate 24 is disposed between the other end face of the electrode group 18 and the bottom of the battery can 22. The electrode group 18 is formed by winding a positive electrode 15 and a negative electrode 16 with a separator 17 interposed therebetween.

[0087] Hereinafter, the present disclosure will be specifically described based on examples and comparative examples, but the present disclosure is not limited to the following examples.

[0088] Example 1 Synthesis of Composite Particles 2 g of nanosilicon particles (average particle size 40 nm) were dispersed in 60 mL of aqueous solution A containing 100 mM aniline and 30 mM phytic acid. Next, 20 mL of aqueous solution B containing 125 mM ammonium persulfate was poured into aqueous solution A containing the dispersed nanosilicon particles, and the mixture was stirred at room temperature for 3 days to polymerize the aniline, yielding composite A1.

[0089] The composite A1 was separated by suction filtration and then thoroughly washed with distilled water. The washed composite was dried in vacuum at 60°C. The dried composite A1 was pulverized in a mortar and then passed through a sieve with 75 μm openings. The pulverized composite A1 (composite particle A1) was added to 500 mL of pure water and washed with water for 5 hours while stirring. The composite particle A1 was then separated by suction filtration and dried in vacuum at 60°C.

[0090] (Particle Size Distribution) The volume-based particle size distribution of the composite particles was measured by a laser diffraction scattering method. Composite particles A1 had a D50 of 29 μm, a D10 of 1.9 μm, and a D90 of 122 μm.

[0091] (ICP-AES analysis) The content of silicon nanoparticles in Composite Particle A1 was measured by ICP-AES and found to be 67% by mass. The conductive polymer was estimated to be approximately 33% by mass. The content of sulfur element derived from ammonium persulfate in Composite Particle A1 was also measured by ICP-AES and found to be 0.03% by mass.

[0092] (Volume Resistivity) The volume resistivity of the composite particle A1 is 204 kgf / cm 2 When the powder resistivity was measured by the four-probe method using a powder resistivity measuring device (Loresta SP manufactured by Mitsubishi Chemical Analytic Co., Ltd.) under a pressure of 1.6 × 10 6 The value was Ω·cm.

[0093] (FT-IR Analysis) When the conductive polymer (polyaniline) in Composite Particle A1 was analyzed by FT-IR, stretching and vibration absorption attributable to the quinoid structure formed by proton doping were confirmed. In addition, absorption attributable to stretching of the aromatic ring and absorption attributable to N-H stretching were confirmed.

[0094] [Preparation of Negative Electrode] Composite particles A1, sodium salt of carboxymethyl cellulose (CMC-Na), styrene-butadiene rubber (SBR), polyacrylic acid (PAA), and single-walled carbon nanotubes (SWCNT) were mixed in a mass ratio of composite particles A1:CMC-Na:SBR:PAA:SWCNT=100:5:5:5:0.5, water was added, and the mixture was stirred using a mixer (manufactured by Primix, T.K. Hibismix) to prepare a negative electrode slurry. Next, the negative electrode slurry was applied to one side of a copper foil (negative electrode current collector), the coating was dried, and then rolled to form a negative electrode slurry having a density of 0.7 g / cm on one side of the copper foil. 3 The negative electrode mixture layer had a thickness of TA1 at five points. 0-1 ~TA1 0-5 was measured.

[0095] The negative electrode was cut into a 20 mm × 20 mm shape with a 5 mm × 5 mm protrusion, and the negative electrode mixture layer on the protrusion was peeled off to expose the copper foil. A negative electrode tab lead was then connected to the exposed portion of the negative electrode current collector, and a predetermined region on the periphery of the negative electrode tab lead was covered with an insulating film.

[0096] (Resistance of Mixture Layer) The volume resistivity of the negative electrode mixture layer was measured using an electrode resistance measurement system (RM2610 manufactured by Hioki E.E. Corporation) and was found to be 8.3 Ω·cm.

[0097] (Interface Resistance) The interface resistance was measured using an electrode resistance measurement system (RM2610 manufactured by Hioki E.E. Corporation) and found to be 0.35 Ω cm 2 It was.

[0098] [Preparation of Counter Electrode] A counter electrode was prepared by attaching a lithium metal foil having a thickness of 300 μm to one surface of a copper foil.

[0099] The counter electrode was cut into the same shape as the negative electrode, and the lithium metal foil on the protruding portion was peeled off to expose the copper foil. Then, a counter electrode tab lead was connected to the exposed copper foil in the same manner as the negative electrode, and a predetermined area around the periphery of the counter electrode tab lead was covered with an insulating film.

[0100] [Preparation of non-aqueous electrolyte] A mixed solvent of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of EC:EMC:DMC=4:1:15 was added to a non-aqueous electrolyte solution containing lithium hexafluorophosphate (LiPF 6 ) was added in an amount of 1.3 mol / L to prepare a non-aqueous electrolyte.

[0101] [Preparation of Evaluation Cell] A cell with a negative electrode-regulated design capacity of 25 mAh was prepared using the above negative electrode and counter electrode. The negative electrode and counter electrode were placed opposite each other with two aramid-coated polyethylene separators (15 μm thick) interposed between them, with the negative electrode mixture layer and the lithium metal foil overlapping, to obtain an electrode assembly. Next, a rectangular Al laminate film (100 μm thick) was folded in half and the long edge was heat-sealed to form a cylinder. The prepared electrode assembly was then placed into the cylinder from one of the short edges, and the end face of the Al laminate film was aligned with the insulating film of each tab lead and heat-sealed. Next, 0.3 cm of nonaqueous electrolyte was poured into the cylinder from the short edge that was not heat-sealed. 3 The negative electrode mixture layer was impregnated with the nonaqueous electrolyte. The negative electrode mixture layer was then left under a reduced pressure of 0.02 MPa for 3 minutes and then returned to atmospheric pressure. This process was repeated twice to impregnate the negative electrode mixture layer with the nonaqueous electrolyte. Finally, the end face of the Al laminate film on the side where the liquid was injected was heat-sealed to obtain evaluation cell A1. The evaluation cell was fabricated in a dry air atmosphere with a dew point of −60°C or lower.

[0102] [Evaluation] The evaluation cell was clamped between a pair of 10 x 5 cm stainless steel clamps (thickness: 6 mm) and pressurized and fixed at 1 MPa.

[0103] <First cycle> In a thermostatic chamber at 25°C, the negative electrode was charged with lithium at a constant current of 0.1 C (1 C is the current value at which the design capacity is discharged in 1 hour) until the cell voltage reached 0.005 V, after which the battery was allowed to rest for 20 minutes. Next, the negative electrode was charged with lithium at a constant current of 0.01 C until the cell voltage reached 0.005 V, after which the battery was allowed to rest for 20 minutes. Furthermore, the negative electrode was charged with lithium at a constant current of 0.001 C until the cell voltage reached 0.005 V, after which the battery was allowed to rest for 20 minutes.

[0104] Subsequently, lithium was discharged from the negative electrode at a constant current of 0.1 C to a cell voltage of 1.0 V, followed by a 20-minute pause. Next, lithium was discharged from the negative electrode at a constant current of 0.01 C to a cell voltage of 1.0 V, followed by a 20-minute pause. Furthermore, lithium was discharged from the negative electrode at a constant current of 0.001 C to a cell voltage of 1.0 V, followed by a 20-minute pause.

[0105] <Second cycle> The negative electrode was charged with lithium at a constant current of 0.1 C until the cell voltage reached 0.005 V, after which the battery was allowed to rest for 20 minutes. Next, the negative electrode was charged with lithium at a constant current of 0.01 C until the cell voltage reached 0.005 V, after which the battery was allowed to rest for 20 minutes. Furthermore, the negative electrode was charged with lithium at a constant current of 0.001 C until the cell voltage reached 0.005 V, after which the battery was allowed to rest for 20 minutes.

[0106] Next, the cell was disassembled, and the thickness TA1 was measured at five points on the negative electrode mixture layer. 1-1 ~TA1 1-5 Measure the initial thickness TA1 0-n and the expansion thickness TA1 1-n (n = 1, 2, 3, 4, 5), the expansion rate = TA1 1-n / TA1 0-n The average value of these expansion coefficients was found to be 1.43.

[0107] Comparative Example 1 Instead of the composite particles A1, a general-purpose silicon-containing material, SiO x Particles (x=1) (nano Si is SiO 2 An evaluation cell B1 was prepared and evaluated in the same manner as in Example 1, except that the matrix phase (dispersed in the matrix of the matrix phase) was used. 0-n (n = 1, 2, 3, 4, 5) and expansion thickness TB1 1-n (n = 1, 2, 3, 4, 5) Expansion rate = TB1 1-n / TB1 0-n The average value was calculated to be 1.95.

[0108] Comparative Example 2 Composite A1 was synthesized in the same manner as in Example 1, separated by suction filtration, and then vacuum-dried at 60°C without washing with distilled water. The dried composite (hereinafter referred to as composite B2) was pulverized in a mortar. The content of sulfur element derived from ammonium persulfate in the pulverized composite B2 (composite particle B2) was measured by ICP-AES and found to be 0.71% by mass.

[0109] Example 2 Composite A1 was separated by suction filtration and then thoroughly washed with distilled water. After washing, composite A1 was added to 500 mL of pure water and further washed with water for 5 hours while stirring. Composite A1 was then separated by suction filtration and vacuum dried at 60°C. After drying, composite A1 was pulverized in a mortar and passed through a sieve with 75 μm openings. The content of sulfur element derived from ammonium persulfate in the pulverized composite (hereinafter referred to as composite particle A2) was measured by ICP-AES and was found to be 0.05% by mass.

[0110] Example 3 Composite A1 was synthesized in the same manner as in Example 1, separated by suction filtration, and then vacuum-dried at 60°C without washing with distilled water. The dried composite (hereinafter referred to as composite B2) was pulverized in a mortar and passed through a sieve with 75 μm openings. The pulverized composite B2 (composite particle B2) was added to 500 mL of pure water and further washed with water for 5 hours while stirring. Thereafter, composite particles (hereinafter referred to as composite particle A3) were separated by suction filtration and vacuum-dried at 60°C. The content of sulfur element derived from ammonium persulfate in Composite Particle A3 was measured by ICP-AES and was found to be 0.03% by mass. The results are summarized in Table 1.

[0111]

[0112] From Table 1, when composite particles A1 were used, SiO x It can be seen that the expansion rate is significantly lower than when particles are used. It can also be seen that the sulfur content can be significantly reduced by washing the composite with water after crushing.

[0113] Secondary batteries comprising the negative electrode active material according to the present disclosure are suitable for use as main power sources for mobile communication devices, portable electronic devices, and automotive power sources, but are not limited thereto. While the present invention has been described with reference to presently preferred embodiments, such disclosure should not be construed as limiting. Various modifications and alterations will no doubt become apparent to those skilled in the art upon reading the above disclosure. Accordingly, the appended claims should be construed to include all modifications and alterations within the true spirit and scope of the present invention.

[0114] 10: Secondary battery, 11: Sealing body, 12: Valve body, 13: Metal plate, 14: Insulating member, 15: Positive electrode, 15a: Positive electrode lead, 16: Negative electrode, 16a: Negative electrode lead, 17: Separator, 18: Electrode group, 21: Gasket, 22: Battery can, 22a: Groove, 23: First insulating plate, 24: Second insulating plate, 16: Negative electrode

Claims

1. Composite particles including a conductive polymer and a Si-containing particle, In the composite particle, a plurality of the Si-containing particles are connected via the conductive polymer, The composite particle has a particle size D50 of 100 μm or less when the cumulative volume in the volume-based particle size distribution is 50%, The composite particles contain elemental sulfur, The content of the sulfur element in the composite particles is less than 0.05 mass %.

2. The negative electrode active material for a secondary battery according to claim 1 , wherein the composite particles have a free volume.

3. The negative electrode active material for a secondary battery according to claim 1 , wherein the composite particles further contain a nitrogen element.

4. 4. The negative electrode active material for a secondary battery according to claim 1, wherein the conductive polymer contains polyaniline.

5. The particle diameter D10 at 10% cumulative volume in a volume-based particle size distribution of the composite particles is 0.5 μm to 50 μm, and the particle diameter D90 at 90% cumulative volume is 50 μm to 500 μm. The negative electrode active material for secondary batteries according to any one of claims 1 to 3.

6. The powder resistivity of the composite particles is 10 3 Ω cm to 10 7 The negative electrode active material for secondary batteries according to any one of claims 1 to 3, having a resistance of Ω·cm.

7. 4. The negative electrode active material for a secondary battery according to claim 1, wherein the average particle size of the Si-containing particles is 10 nm to 500 nm.

8. 4. The negative electrode active material for a secondary battery according to claim 1, wherein a content of the Si-containing particles in the composite particles is 30% by mass to 90% by mass.

9. 4. The negative electrode active material for a secondary battery according to claim 1, wherein at least a part of the surface of the Si-containing particle is covered with a carbonaceous material having electrical conductivity.

10. A negative electrode for a secondary battery, comprising the negative electrode active material for a secondary battery according to claim 1 .

11. A positive electrode, a negative electrode, and a non-aqueous electrolyte, The negative electrode of claim 10 .

12. a first step of synthesizing a composite including a conductive polymer and a Si-containing particle, the composite including a conductive polymer and a Si-containing particle, and a plurality of the Si-containing particles being linked together by the conductive polymer, by mixing a monomer that is a raw material of the conductive polymer, a polymerization initiator that includes a sulfur element, and a Si-containing particle, and polymerizing the monomer; A second step of pulverizing the composite to obtain composite particles having a particle diameter D50 of 100 μm or less when the cumulative volume in a volume-based particle size distribution is 50%; a third step of washing the composite particles until the content of the sulfur element in the composite particles is less than 0.05% by mass; The method for producing a negative electrode active material for a secondary battery comprises the steps of: