Aqueous poly(hydroxyalkanoic acid) suspension and production method therefor
Patent Information
- Application Number
- JP2024509861
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-29
AI Technical Summary
Polyhydroxyalkanoic acid (PHA) aqueous suspensions face challenges with odor and mold formation over time, and molecular weight reduction during storage and heating, limiting their stability and usability in producing high-quality laminates.
Adding hydrogen peroxide to a PHA aqueous suspension with a pH of 5 or less, maintaining a hydrogen peroxide concentration of 0.05 to 1.5% by weight, which stabilizes the suspension and suppresses bacterial growth and molecular weight decrease.
The method enhances storage stability, prevents odor and mold formation, and minimizes molecular weight loss during heating, allowing for the production of high-quality PHA laminates with potential antibacterial or sterilizing properties.
Abstract
Description
Aqueous polyhydroxyalkanoic acid suspension and method for producing the same
[0001] The present invention relates to an aqueous suspension of polyhydroxyalkanoic acid and a method for producing the same, as well as a laminate using the polyhydroxyalkanoic acid and a method for producing the same.
[0002] Polyhydroxyalkanoic acid (hereinafter sometimes abbreviated as "PHA") is known to be biodegradable. PHA produced by microorganisms accumulates within the microbial cells. Therefore, in order to use PHA as a plastic, a process of separating and purifying PHA from the microbial cells is required. In the process of separating and purifying PHA, the microbial cells are disrupted, and then cell-derived components other than PHA are solubilized. PHA can be separated by performing separation procedures such as centrifugation, filtration, and drying.
[0003] In the process of producing PHA, impurities derived from bacterial cells are removed to decolorize and deodorize the PHA. For example, Patent Document 1 describes that decolorization or deodorization is achieved by contacting PHA-containing bacterial cells or impurities in partially purified PHA with ozone. It also describes that the ozone treatment is preferably carried out on a polymer suspension exhibiting a nearly neutral pH.
[0004] Furthermore, Patent Document 2 describes a purification method for obtaining highly pure PHA that is free from yellowing and unpleasant odors in high yield, in which a PHA-containing solution separated from a microorganism is treated with hydrogen peroxide while adding an alkali to the PHA-containing solution to control the pH between 7 and 13. It also describes that in order to enhance the purification effect, the treatment with hydrogen peroxide is preferably carried out at a temperature of 50° C. or higher for 10 minutes to 10 hours.
[0005] JP-A No. 2002-510747
[0006] As described above, Patent Documents 1 and 2 disclose methods for sufficiently purifying PHA to obtain deodorized and decolorized PHA.
[0007] On the other hand, a laminate including a PHA layer can be produced by coating a substrate such as paper with PHA, and in this case, an aqueous suspension of PHA can be coated on the substrate and then dried.
[0008] However, it has been found that even if the aqueous PHA suspension contains PHA that has been subjected to a purification treatment as described in Patent Documents 1 and 2 and that has been deodorized and decolorized, when the aqueous suspension is stored for a long period of time or at high temperatures, there is a problem that odor and mold will develop over time due to bacterial growth, etc. Furthermore, when the aqueous PHA suspension or the PHA obtained therefrom is subjected to a heating and / or drying treatment, the molecular weight of the PHA tends to decrease, and it is also necessary to suppress such decrease.
[0009] In view of the above-mentioned current situation, the present invention aims to provide a method for producing an aqueous polyhydroxyalkanoic acid suspension that can suppress the generation of odor and mold over time in the aqueous polyhydroxyalkanoic acid suspension and can also suppress a decrease in the molecular weight of the polyhydroxyalkanoic acid.
[0010] As a result of intensive research to solve the above-mentioned problems, the inventors discovered that the above-mentioned problems can be solved by adding hydrogen peroxide to an aqueous suspension of polyhydroxyalkanoic acid having a pH below a specific value, and thus completed the present invention.
[0011] That is, the present invention relates to a method for producing an aqueous polyhydroxyalkanoic acid suspension, which includes a step of adding hydrogen peroxide to an aqueous polyhydroxyalkanoic acid suspension having a pH of 5 or less. The present invention also relates to an aqueous polyhydroxyalkanoic acid suspension, the aqueous suspension having a pH of 5 or less and containing 0.05 to 1.5 wt % hydrogen peroxide based on the solid content including the polyhydroxyalkanoic acid. The present invention also relates to a method for producing a laminate having a resin layer containing polyhydroxyalkanoic acid, which includes a step of coating a substrate with the aqueous suspension to form a coating film, and a step of drying the coating film. The present invention also relates to a laminate having a substrate and a resin layer containing polyhydroxyalkanoic acid produced using an aqueous polyhydroxyalkanoic acid suspension having a pH of 5 or less, wherein the hydrogen peroxide concentration in the resin layer is 30 to 200 ppm, and to a molded article including the laminate.
[0012] According to the present invention, it is possible to provide a method for producing an aqueous polyhydroxyalkanoic acid suspension, which can suppress the generation of odor and mold over time in the aqueous polyhydroxyalkanoic acid suspension and can also suppress a decrease in the molecular weight of the polyhydroxyalkanoic acid.
[0013] The aqueous suspension of polyhydroxyalkanoic acid obtained by the present invention has excellent storage stability and handleability, and is less likely to develop odor or mold even when stored for a long period of time or at high temperatures. Furthermore, the polyhydroxyalkanoic acid obtained from the suspension undergoes relatively little molecular weight reduction upon heating and / or drying.
[0014] Furthermore, by coating a substrate with the aqueous suspension of polyhydroxyalkanoic acid obtained by the present invention and drying it, a laminate having a resin layer containing polyhydroxyalkanoic acid can be produced. The resin layer of such a laminate can contain hydrogen peroxide, and therefore can be expected to exhibit disinfecting, antibacterial or sterilizing, or antiviral effects.
[0015] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to the following embodiments.
[0016] The method for producing a polyhydroxyalkanoic acid aqueous suspension according to this embodiment includes a step of adding hydrogen peroxide to a polyhydroxyalkanoic acid aqueous suspension having a pH of 5 or less. Hereinafter, polyhydroxyalkanoic acid may be abbreviated as "PHA." The PHA aqueous suspension before the addition of hydrogen peroxide is referred to as PHA aqueous suspension (A), and the PHA aqueous suspension after the addition of hydrogen peroxide is referred to as PHA aqueous suspension (B).
[0017] <PHA> "PHA" is a general term for polymers with hydroxyalkanoic acid as a monomer unit. Specific examples include polyglycolic acid, polylactic acid, poly-3-hydroxyalkanoate (hereinafter abbreviated as P3HA), and poly-4-hydroxyalkanoate. Of these, P3HA is preferred.
[0018] The P3HA has the formula: [—CHR—CH 2 —CO—O—] (wherein R is C n H 2n+1 where n is an alkyl group represented by the formula (I), and n is an integer of 1 or more and 15 or less. The copolymerization method is not particularly limited, and may be random copolymerization, alternating copolymerization, block copolymerization, graft copolymerization, etc., but random copolymerization is preferred because it is easily available. The P3HA may be a copolymer containing the repeating unit represented by the formula (I) and other repeating units.
[0019] Among the repeating units represented by the above formula, it is preferable to contain a 3-hydroxybutyrate unit. The P3HA may be a homopolymer of a 3-hydroxybutyrate unit, but is particularly preferably a copolymer containing a 3-hydroxybutyrate unit and another hydroxyalkanoate unit.
[0020] Specific examples of P3HA include poly(3-hydroxybutyrate) (P3HB), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (P3HB3HH), poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (P3HB3HV), poly(3-hydroxybutyrate-co-4-hydroxybutyrate) (P3HB4HB), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate) (P3HB3HO), poly(3-hydroxybutyrate-co-3-hydroxyoctadecanoate) (P3HB3HOD), poly(3-hydroxybutyrate-co-3-hydroxydecanoate) (P3HB3HD), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate) (P3HB3HV3HH), and the like. Among these, P3HB, P3HB3HH, P3HB3HV, and P3HB4HB are preferred because they are easy to produce industrially.
[0021] By changing the composition ratio of the repeating units in P3HA, the melting point or crystallinity of PHA can be changed, and as a result, physical properties such as Young's modulus and heat resistance can be changed. In addition, it is possible to impart physical properties between those of polypropylene and polyethylene. From the viewpoints of ease of industrial production and being a physically useful plastic, P3HB3HH, which is a copolymer of 3-hydroxybutyric acid and 3-hydroxyhexanoic acid, is more preferred.
[0022] From the viewpoint of the balance between flexibility and strength, the composition ratio of the repeating units in P3HA is preferably 80 / 20 to 99 / 1 (mol / mol) in terms of the composition ratio of 3-hydroxybutyrate units to other hydroxyalkanoate units, and more preferably 83 / 17 to 97 / 3 (mol / mol). When the composition ratio of 3-hydroxybutyrate units to other hydroxyalkanoate units is 99 / 1 (mol / mol) or less, good flexibility is obtained, and when it is 80 / 20 (mol / mol) or more, high hardness can be obtained.
[0023] The weight-average molecular weight of the PHA is not particularly limited, but from the viewpoint of mechanical strength, it is preferably 100,000 or more, more preferably 150,000 or more, and even more preferably 200,000 or more. From the viewpoint of processability of the PHA, the weight-average molecular weight is preferably 700,000 or less, more preferably 600,000 or less, and even more preferably 550,000 or less.
[0024] The weight-average molecular weight of PHA can be determined as a polystyrene-equivalent molecular weight by gel permeation chromatography (GPC) (Shodex GPC-101 manufactured by Showa Denko K.K.) using a polystyrene gel (Shodex K-804 manufactured by Showa Denko K.K.) as a column and chloroform as a mobile phase.
[0025] <PHA aqueous suspension (A)> The "PHA aqueous suspension" is a dispersion of PHA particles in an aqueous medium. The aqueous medium may be water alone or a mixed solvent of water and a water-compatible organic solvent. In the mixed solvent, the concentration of the water-compatible organic solvent is not particularly limited as long as it is equal to or lower than the solubility of the organic solvent used in water.
[0026] The organic solvent is not particularly limited, but examples thereof include alcohols such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, isobutanol, pentanol, hexanol, and heptanol; ketones such as acetone and methyl ethyl ketone; ethers such as tetrahydrofuran and dioxane; nitriles such as acetonitrile and propionitrile; amides such as dimethylformamide and acetamide; dimethyl sulfoxide, pyridine, and piperidine. Among these, methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, isobutanol, acetone, methyl ethyl ketone, tetrahydrofuran, dioxane, acetonitrile, and propionitrile are preferred because they are easily removable. Furthermore, methanol, ethanol, 1-propanol, 2-propanol, butanol, and acetone are more preferred because they are easily available. Furthermore, methanol, ethanol, and acetone are particularly preferred.
[0027] The aqueous medium constituting the PHA aqueous suspension (A) preferably contains water. The content of water in the entire aqueous medium is preferably 5 to 100% by weight, more preferably 10% by weight or more, more preferably 30% by weight or more, even more preferably 50% by weight or more, and particularly preferably 70% by weight or more. It may also be 90% by weight or more, or 95% by weight or more.
[0028] The solids concentration in the PHA aqueous suspension (A) is not particularly limited, but may be a concentration suitable for coating applications or spray drying, which will be described later. For example, the concentration of the solids including PHA in the PHA aqueous suspension (A) may be 20 to 60% by weight. The lower limit is preferably 25% by weight or more, more preferably 30% by weight or more, and even more preferably 35% by weight or more. The upper limit may be 55% by weight or less.
[0029] The purity of the PHA contained in the PHA aqueous suspension (A) is not particularly limited. However, since the PHA aqueous suspension (A) is preferably one obtained after decomposition or removal of cell-derived components other than PHA by a purification treatment as described below, in this case, the PHA contained in the PHA aqueous suspension (A) can be of high purity. Specifically, the ratio of the PHA contained in the PHA aqueous suspension (A) to the total solid content contained in the PHA aqueous suspension (A) is preferably 95 wt% or more, more preferably 97 wt% or more, even more preferably 99 wt% or more, and particularly preferably 99.5 wt% or more.
[0030] From the same viewpoint, it is preferable that the protein content in the PHA aqueous suspension (A) is low. Specifically, the amount of protein is preferably 30,000 ppm or less, more preferably 15,000 ppm or less, even more preferably 10,000 ppm or less, and particularly preferably 7,500 ppm or less, based on the total solid content in the PHA aqueous suspension (A).
[0031] <Method for Preparing PHA Aqueous Suspension (A)> The method for preparing the PHA aqueous suspension (A) is not particularly limited. The PHA aqueous suspension (A) may be prepared by mixing a PHA powder with an aqueous medium, but the following method is a suitable preparation method. Microorganisms capable of producing PHA are cultured to accumulate PHA within the microbial cells, and then the cells are disrupted to obtain a cell lysate. Subsequently, the resulting solution is dehydrated by filtration, centrifugation, or the like, as needed, and then purified to decompose and / or remove cell-derived components other than the PHA. The resulting PHA is washed with water or the like as needed, and the concentration is adjusted by adding or removing an aqueous medium containing water as needed, thereby obtaining the PHA aqueous suspension (A). This method is described in detail below.
[0032] The microorganism is not particularly limited as long as it is a microorganism that synthesizes PHA, and may be a naturally occurring microorganism, a microorganism deposited in a strain depository (e.g., IFO, ATCC, etc.), or a mutant or transformant that can be prepared from such a microorganism.
[0033] Examples of the genera of the microorganisms include bacteria of the genera Cupriavidus, Alcaligenes, Ralstonia, Pseudomonas, Bacillus, Azotobacter, Nocardia, and Aeromonas. Particularly preferred are strains of Alcaligenes lipolytica, Alcaligenes latus, Aeromonas caviae, Aeromonas hydrophila, and C. necator. Furthermore, when a microorganism does not inherently have the ability to produce PHA or when the amount of PHA produced is low, a transformant obtained by introducing a target PHA synthase gene and / or a mutant thereof into the microorganism can also be used. The PHA synthase gene used to prepare such a transformant is not particularly limited, but a PHA synthase gene derived from Aeromonas caviae is preferred.
[0034] By culturing such PHA-producing microorganisms under appropriate conditions, it is possible to obtain microbial cells that have accumulated PHA within the cells. The culturing method is not particularly limited, but for example, the method described in JP-A-05-93049 can be used.
[0035] After PHA is accumulated within microbial cells by culturing the microorganisms, the PHA-containing cells are preferably disrupted by physical, chemical, or biological treatment. The disruption method is not particularly limited, and conventional methods utilizing fluid shear force, solid shear force, or grinding, such as a French press, homogenizer, X-press, ball mill, colloid mill, DYNO mill, or ultrasonic homogenizer, can be used. Other methods that can be used include those using chemicals such as acids, alkalis, surfactants, organic solvents, and cell wall synthesis inhibitors; methods using enzymes such as lysozyme, pectinase, cellulase, and zymolyase; methods using supercritical fluids; osmotic disruption, freezing, and dry grinding. Another example is an autolysis method that utilizes the action of proteases and esterases contained in the cells themselves. These disruption methods can be used alone or in combination. Furthermore, batch processing or continuous processing can be used.
[0036] The cell lysate obtained by disrupting cells contains, in addition to PHA, cell-derived components such as proteins, nucleic acids, lipids, and sugar components in the cells, as well as culture substrate residues. Therefore, after cell disruption, it is preferable to carry out a dehydration step to separate water containing water-soluble components such as these cell-derived components and culture substrate residues. This reduces the content of impurities. Dehydration methods are not particularly limited, but include filtration, centrifugation, sedimentation, electrophoresis, etc.
[0037] Next, it is preferable to carry out a purification treatment to decompose and / or remove impurities such as cell-derived components other than PHA. One example of the purification treatment is a method using an enzyme. Usable enzymes are not particularly limited as long as they have the activity of decomposing cell-derived components, and examples include proteolytic enzymes, lipolytic enzymes, cell wall-decomposing enzymes, and nucleolytic enzymes. In addition, commercially available enzyme laundry detergents and enzyme compositions containing enzymes and enzyme stabilizers, anti-redeposition agents, etc. can also be used. These may be used alone or in combination of two or more types.
[0038] The time required for the enzyme treatment can be appropriately set in consideration of the desired degree of purification, and may be, for example, 0.5 to 2 hours. The amount of enzyme used depends on the type and activity of the enzyme and is not particularly limited, but may be, for example, about 0.001 to 10 parts by weight per 100 parts by weight of PHA, and from the viewpoint of cost, 0.01 to 5 parts by weight is preferred.
[0039] Other examples of the purification treatment include a method using hypochlorous acid and a method using hydrogen peroxide.
[0040] The treatment using hypochlorous acid may be carried out under conditions in which the pH of the PHA dispersion is in the alkaline region and contact with heat, light, and metals is suppressed. The pH is preferably 8 or higher, more preferably 10 or higher, and even more preferably 12 or higher. The temperature during the treatment is preferably 40° C. or lower, more preferably 20° C. or lower.
[0041] In the purification treatment using hydrogen peroxide, in order to enhance the purification effect in a short time, it is preferable to heat the PHA dispersion after adding hydrogen peroxide to the dispersion. The temperature is preferably 50°C or higher, more preferably 70°C or higher. The upper limit of the temperature is preferably the boiling point of the dispersion or lower. In the purification treatment, it is preferable to hold the dispersion under heating for, for example, about 10 minutes to 10 hours, more preferably 30 minutes to 5 hours, and even more preferably 1 to 3 hours.
[0042] In order to suppress a decrease in the molecular weight of the PHA due to the purification treatment using hydrogen peroxide, it is preferable to carry out the purification treatment while controlling the pH of the PHA dispersion to 7 to 13 by continuously or intermittently adding an alkali to the PHA dispersion. The alkali is not particularly limited, but examples thereof include sodium hydroxide, sodium carbonate, and potassium hydroxide. For details of pH control, see the description in Patent Document 2. The purification treatment using hydrogen peroxide described above is carried out in the process of preparing the PHA aqueous suspension (A), and is a treatment different from the addition of hydrogen peroxide to the PHA aqueous suspension (A).
[0043] The various purification treatments described above may be carried out either alone or in combination of two or more.
[0044] After the purification treatment described above, dehydration is carried out as necessary, and the obtained PHA can be washed with water or the like as necessary to further increase the degree of purification of the PHA. For washing, an organic solvent may be used, or a mixture of water and an organic solvent may be used. The pH of the water may also be adjusted. The organic solvent used as the washing solvent is preferably a hydrophilic solvent, and specific examples include methanol, ethanol, acetone, acetonitrile, tetrahydrofuran, ketones, and amines. Two or more of these organic solvents may be mixed and used. Furthermore, a surfactant or the like may be added to the water.
[0045] If necessary, water and / or the above-mentioned water-compatible organic solvent may be added to the PHA obtained after washing, or the water and / or organic solvent used for washing may be removed to obtain a PHA aqueous suspension (A) adjusted to a desired concentration.
[0046] A step of applying mechanical shear to the PHA aqueous suspension (A) to separate the partially aggregated PHA particles from each other may be carried out. Applying mechanical shear is preferable in that it can substantially eliminate aggregates and obtain an aqueous PHA suspension (A) containing PHA particles of uniform particle size. The step of applying mechanical shear can be carried out using, for example, a stirrer, a homogenizer, ultrasonic waves, etc.
[0047] <pH of PHA aqueous suspension (A)> According to this embodiment, the pH of the PHA aqueous suspension (A) is set to 5 or less. This makes it possible to suppress a decrease in the molecular weight of the PHA, which may occur during heating and / or drying. The PHA aqueous suspension (A) obtained through the above-described purification step often has a pH of more than 7. Therefore, it is preferable to adjust the pH of the PHA aqueous suspension (A) to 5 or less by adding an acid to the PHA aqueous suspension (A).
[0048] The acid that can be used to adjust the pH is not particularly limited, and may be either an organic acid or an inorganic acid, regardless of whether it is volatile. Specific examples of the acid include sulfuric acid, hydrochloric acid, phosphoric acid, and acetic acid. Alternatively, the pH may be adjusted to 5 or less by adding an organic salt or an inorganic salt instead of or together with the acid.
[0049] The pH of the PHA aqueous suspension (A) may be 5 or less, preferably 4.5 or less. From the viewpoint of the acid resistance of the container, the lower limit of the pH is preferably 1 or more, more preferably 2 or more, and even more preferably 3 or more.
[0050] <Addition of Hydrogen Peroxide to PHA Aqueous Suspension (A)> According to this embodiment, hydrogen peroxide is added to PHA aqueous suspension (A) having a pH of 5 or less to obtain PHA aqueous suspension (B). This makes it possible to suppress a decrease in molecular weight of the PHA obtained from PHA aqueous suspension (B) during heating and / or drying, and to suppress the generation of odor and mold that may occur over time during storage of PHA aqueous suspension (B). The form of hydrogen peroxide to be added is not particularly limited, but it is preferable to add aqueous hydrogen peroxide because of its ease of availability.
[0051] The amount of hydrogen peroxide added can be set as appropriate, but is preferably within the range of 0.05 to 1.5% by weight based on the solid content including PHA contained in the PHA aqueous suspension (A). The amount of hydrogen peroxide added is the amount added converted into the pure content of hydrogen peroxide.
[0052] In order to obtain a better effect of suppressing odor and mold generation, the lower limit of the amount of hydrogen peroxide added is preferably 0.08% by weight or more, more preferably 0.1% by weight or more, and may also be 0.2% by weight or more, or 0.3% by weight or more.
[0053] On the other hand, if the amount of hydrogen peroxide added is large, foaming may occur in the PHA aqueous suspension (B) due to the addition of hydrogen peroxide, so the upper limit of the amount added is preferably 1.2% by weight or less, more preferably 1% by weight or less. It may also be 0.8% by weight or less, or 0.5% by weight or less. Foaming in the PHA aqueous suspension (B) not only results in a poor appearance, but also makes it difficult to accurately measure the PHA aqueous suspension (B) or to store the PHA aqueous suspension (B) in a container and close the lid.
[0054] The temperature of the PHA aqueous suspension (A) when hydrogen peroxide is added is not particularly limited, and although it may be heated, heating is not necessary and the temperature may be room temperature (for example, about 10 to 30° C.). After adding hydrogen peroxide to the PHA aqueous suspension (A), the resulting PHA aqueous suspension (B) does not need to be maintained under heating and may be maintained at room temperature.
[0055] In order to disperse the hydrogen peroxide uniformly, it is preferable to stir the PHA aqueous suspension (B) while adding the hydrogen peroxide or after adding the hydrogen peroxide.
[0056] The resulting PHA aqueous suspension (B) can be directly poured into a sealable container and sealed without the need for subsequent washing, dilution, etc. Alternatively, hydrogen peroxide may be added to the PHA aqueous suspension (A) already filled in a sealable container to form the PHA aqueous suspension (B), which may then be sealed.
[0057] <PHA aqueous suspension (B)> The PHA aqueous suspension (B) obtained by adding hydrogen peroxide has a pH of 5 or less, similar to the PHA aqueous suspension (A). The pH is preferably 4.5 or less. From the viewpoint of the acid resistance of the container, the lower limit of the pH is preferably 1 or more, more preferably 2 or more, and even more preferably 3 or more.
[0058] The content of hydrogen peroxide in the PHA aqueous suspension (B) is preferably within a range of 0.05 to 1.5% by weight, based on the solid content, including PHA, contained in the PHA aqueous suspension (B). From the viewpoint of further suppressing odor and mold generation, the lower limit of the content is preferably 0.08% by weight or more, and more preferably 0.1% by weight or more. It may be 0.2% by weight or more, or 0.3% by weight or more. Furthermore, from the viewpoint of suppressing foaming in the PHA aqueous suspension (B), the upper limit of the content is preferably 1.2% by weight or less, and more preferably 1% by weight or less. It may be 0.8% by weight or less, or 0.5% by weight or less.
[0059] The solids concentration in the PHA aqueous suspension (B) is not particularly limited, but may be approximately the same as the solids concentration in the PHA aqueous suspension (A), for example, 20 to 60% by weight. Generally, the higher the concentration of the PHA aqueous suspension, the more likely it is that mold and odor will develop over time. However, the PHA aqueous suspension containing hydrogen peroxide according to this embodiment can suppress the development of mold and odor over time, even if the solids concentration is high. The lower limit of the solids concentration in the PHA aqueous suspension (B) is preferably 25% by weight or more, more preferably 30% by weight or more, and even more preferably 35% by weight or more. The upper limit may be 55% by weight or less.
[0060] The protein content in the PHA aqueous suspension (B) is not particularly limited, but may be approximately the same as the protein content in the PHA aqueous suspension (A), and is preferably 30,000 ppm or less, more preferably 15,000 ppm or less, even more preferably 10,000 ppm or less, and particularly preferably 7,500 ppm or less, based on the total solid content contained in the PHA aqueous suspension (B).
[0061] The average particle size of the PHA particles in the PHA aqueous suspension (B) is not particularly limited and can be set appropriately. When the PHA aqueous suspension (B) is used for coating applications described later, the average particle size may be, for example, 0.1 to 50 μm, preferably 0.5 to 30 μm, and more preferably 0.8 to 20 μm, from the viewpoint of achieving both PHA productivity and uniformity during coating.
[0062] The average particle size of the PHA particles in the PHA aqueous suspension (B) can be calculated by adjusting the aqueous suspension containing PHA to a predetermined concentration using a general-purpose particle size meter such as a Microtrac particle size meter (manufactured by Nikkiso, FRA), and by calculating the particle size corresponding to 50% of the total particle accumulation amount in a normal distribution.
[0063] The PHA aqueous suspension (B) does not need to contain a dispersant, but it is preferable to contain a dispersant to stabilize the PHA aqueous suspension (B). Examples of dispersants include anionic surfactants such as sodium lauryl sulfate and sodium oleate; cationic surfactants such as lauryl trimethylammonium chloride; nonionic surfactants such as glycerin fatty acid esters, sorbitan fatty acid esters, sucrose fatty acid esters, polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, and polyoxyethylene polyoxypropylene glycol; and water-soluble polymers such as polyvinyl alcohol, ethylene-modified polyvinyl alcohol, polyvinylpyrrolidone, and methylcellulose. These dispersants may be used alone or in combination of two or more.
[0064] When a dispersant is used, the amount thereof to be added is not particularly limited, but may be, for example, 0.1 to 10% by weight, and preferably 0.5 to 5% by weight, based on the total solid content contained in the PHA aqueous suspension (B). The dispersant may be added before or after the addition of hydrogen peroxide.
[0065] The number of bacteria in the PHA aqueous suspension (B) is not particularly limited, but from the viewpoint of suppressing the generation of odor and mold over time in the PHA aqueous suspension (B), it is set to 1×10 5 It is preferable that the number of particles is less than 1×10 4 More preferably, 1×10 3 More preferably, 4×10 2 The number of bacteria in the PHA aqueous suspension (B) can be measured by the method described in the Examples section.
[0066] The PHA aqueous suspension (B) may be filled in a sealable container and sealed. Since the PHA aqueous suspension (B) is inhibited from generating odors and mold over time, it is suitable for storage and / or transportation in the container.
[0067] <Uses of PHA aqueous suspension (B)> The uses of the PHA aqueous suspension (B) are not particularly limited, and the PHA aqueous suspension (B) can also be used to obtain PHA powder by drying the PHA aqueous suspension (B). Examples of the drying method in this case include heat drying and spray drying.
[0068] According to a preferred embodiment, the PHA aqueous suspension (B) can be used to obtain a laminate by applying the PHA aqueous suspension (B) as a coating liquid to a substrate and drying it. This embodiment will be described in detail below.
[0069] When the PHA aqueous suspension (B) is used as a coating liquid, additives and the like are added to the PHA aqueous suspension (B) as needed, and then the PHA aqueous suspension (B) is coated on one or both sides of a substrate to form a coating film. The coating can be carried out using a general coating machine.
[0070] The substrate is not particularly limited, and substrates made of various materials can be used. However, from the viewpoint of enhancing the biodegradability of the entire laminate obtained, it is preferable that the substrate is biodegradable.
[0071] The biodegradable substrate is not particularly limited, but examples thereof include paper (mainly composed of cellulose), cellophane, cellulose ester; polyvinyl alcohol, polyamino acid, polyglycolic acid, pullulan, etc. Paper or cellophane is preferred, and paper is particularly preferred, because it has excellent heat resistance and is inexpensive. The type of paper is also not particularly limited, and examples thereof include cup base paper, kraft paper, fine paper, coated paper, tissue paper, glassine paper, and paperboard. The paper may contain additives such as water-resistant agents, water-repellents, and inorganic substances, as needed.
[0072] The substrate may be previously subjected to a surface treatment such as corona treatment, flame treatment, anchor coating treatment, etc. These surface treatments may be performed alone or in combination.
[0073] Next, the coating film formed on one or both sides of the substrate is dried to convert the coating film into a resin layer, thereby obtaining a laminate including the substrate and the resin layer. The heating temperature during drying of the coating film is not particularly limited, but is preferably 100°C or higher, and more preferably 120°C or higher. The upper limit of the heating temperature is preferably 200°C or lower in order to suppress thermal decomposition of the PHA. The heating time can be set appropriately, but may be, for example, about 1 second to 5 minutes. After heating, it is desirable to appropriately cool the laminate.
[0074] The above-mentioned coating and drying steps may be carried out batchwise or continuously while transporting the film-like substrate between a plurality of rolls.
[0075] By the method described above, a laminate including a substrate and a PHA-containing resin layer can be obtained, and this laminate also constitutes one aspect of the present invention.
[0076] The PHA-containing resin layer may contain hydrogen peroxide because it is formed by applying the PHA aqueous suspension (B) containing hydrogen peroxide to a substrate. Specifically, the hydrogen peroxide concentration in the PHA-containing resin layer may be in the range of 30 to 200 ppm, preferably 40 to 150 ppm, more preferably 50 to 110 ppm, and even more preferably 60 to 100 ppm.
[0077] In addition, when the above-mentioned conventional purification treatment using hydrogen peroxide is performed in the stage of producing the PHA aqueous suspension (A), the hydrogen peroxide resulting from the purification treatment may be contained in the PHA-containing resin layer. However, since dehydration and washing treatments are usually performed after the purification treatment using hydrogen peroxide, the amount of hydrogen peroxide contained in the PHA-containing resin layer resulting from the purification treatment is extremely small, and if hydrogen peroxide is not added to the PHA aqueous suspension (A), the above-mentioned hydrogen peroxide concentration in the PHA-containing resin layer cannot be reached (see Comparative Example 1 described later).
[0078] The PHA-containing resin layer may contain one or more resins other than PHA. Examples of such other resins include aliphatic polyester resins such as polybutylene succinate, polycaprolactone, and polylactic acid, and aliphatic aromatic polyester resins such as polybutylene adipate terephthalate, polybutylene sebatate terephthalate, and polybutylene azelate terephthalate. To ensure the biodegradability of the resin layer, the amount of these resins added is preferably 20 parts by weight or less, more preferably 10 parts by weight or less, even more preferably 5 parts by weight or less, and particularly preferably 1 part by weight or less, relative to 100 parts by weight of PHA. The PHA-containing resin layer does not necessarily contain any resin other than PHA.
[0079] The PHA-containing resin layer may contain additives commonly used in the art, as long as the effects of the invention are achieved. Examples of such additives include inorganic fillers such as talc, calcium carbonate, mica, silica, titanium oxide, and alumina; organic fillers such as rice husk, wood flour, and recycled paper such as newspaper; various starches and cellulose; colorants such as pigments and dyes; odor absorbers such as activated carbon and zeolite; fragrances such as vanillin and dextrin; plasticizers; antioxidants; weather resistance improvers; UV absorbers; nucleating agents; lubricants; release agents; water repellents; antibacterial agents; sliding property improvers; tackifiers; fillers; and chemicals. Only one type of additive may be contained, or two or more types may be contained. The content of these additives can be appropriately determined by those skilled in the art depending on the intended use.
[0080] The weight per unit of PHA in the PHA-containing resin layer (basis weight) is, for example, 5 to 100 g / m 2 and 10 to 50 g / m 2 is preferred, and 15 to 40 g / m 2 When the weight per unit of PHA in the PHA-containing resin layer is within the above range, defects such as pinholes can be prevented, the PHA-containing resin layer can have a strength sufficient for use, and functions such as water resistance can be efficiently exhibited.
[0081] The thickness of the PHA-containing resin layer is not particularly limited, but is preferably 5 to 100 μm, more preferably 10 to 50 μm, from the viewpoint of preventing water absorption and ensuring flexibility.
[0082] The laminate according to this embodiment includes at least a substrate and a PHA-containing resin layer. It may be composed of only these layers, or may include other layers in addition to these layers. Examples of such other layers include a gas barrier layer, a printed layer, and other resin layers. The gas barrier layer may be a known layer, such as a metal foil, a metal vapor deposition film, a metal oxide vapor deposition film, a silicon oxide vapor deposition film, a polyvinyl alcohol film, or an ethylene-vinyl alcohol copolymer film. The gas barrier layer may be bonded to the substrate via an adhesive layer.
[0083] The laminate according to this embodiment can be subjected to secondary processing to produce various molded articles. Examples of such molded articles include tubes, plates, rods, packaging materials (e.g., bags), containers (e.g., bottle containers), and parts. In particular, the molded articles can be suitably used as various packaging container materials such as shopping bags, various bags, food and confectionery packaging materials, cups, trays, and cartons (in other words, in various fields such as food, cosmetics, electronics, medicine, and pharmaceuticals). Furthermore, since the molded articles have a PHA-containing resin layer formed on one side of the paper substrate, which has high adhesion to the substrate and good heat resistance, they can be particularly suitably used as containers for liquids, particularly containers for hot contents, such as cups for food and beverages such as instant noodles, instant soup, and coffee, trays for prepared meals, bento boxes, and microwaveable foods.
[0084] The secondary processing can be carried out by any method known in the technical field, for example, using various bag-making machines, filling and packaging machines, etc. Processing can also be carried out using devices such as paper cup forming machines, punching machines, and box-making machines. In these processing machines, known techniques can be used to bond the laminate, for example, heat sealing, impulse sealing, ultrasonic sealing, high-frequency sealing, hot air sealing, and frame sealing. In particular, it is preferable that the molded body is one that has been secondary processed using a heat sealing method. The heat sealing may be carried out between the substrate layer and the PHA-containing resin layer, or may be carried out between the PHA-containing resin layers.
[0085] In order to improve the physical properties of the molded article, the molded article can be composited with another molded article made of a material different from the molded article (for example, fiber, thread, rope, woven fabric, knitted fabric, nonwoven fabric, paper, film, sheet, tube, plate, rod, container, bag, part, foam, etc.). These materials are also preferably biodegradable.
[0086] The following items list preferred embodiments of the present disclosure, but the present invention is not limited to them. [Item 1] A method for producing an aqueous polyhydroxyalkanoic acid suspension, comprising the step of adding hydrogen peroxide to an aqueous polyhydroxyalkanoic acid suspension having a pH of 5 or less. [Item 2] The production method according to Item 1, wherein the amount of hydrogen peroxide added is 0.1 to 1 wt % based on the solid content containing the polyhydroxyalkanoic acid. [Item 3] A method for producing an aqueous polyhydroxyalkanoic acid suspension, comprising the step of adding hydrogen peroxide to an aqueous polyhydroxyalkanoic acid suspension having a pH of 5 or less. [Item 4] A method for producing an aqueous polyhydroxyalkanoic acid suspension, wherein the amount of hydrogen peroxide added is 0.1 to 1 wt % based on the solid content containing the polyhydroxyalkanoic acid. [Item 5] A method for producing an aqueous polyhydroxyalkanoic acid suspension, wherein the number of bacteria in the aqueous suspension after the addition of hydrogen peroxide is 4 x 10 2Item 4: The method according to any one of items 1 to 3, wherein the concentration of solids containing the polyhydroxyalkanoic acid in the aqueous suspension is 20 to 60% by weight. Item 5: The method according to any one of items 1 to 4, wherein the polyhydroxyalkanoic acid is a copolymer containing 3-hydroxybutyrate units and other hydroxyalkanoate units. Item 6: The method according to item 5, wherein the other hydroxyalkanoate units are 3-hydroxyhexanoate units. Item 7: An aqueous suspension of polyhydroxyalkanoic acid, wherein the pH of the aqueous suspension is 5 or less, and wherein the aqueous suspension contains 0.05 to 1.5% by weight of hydrogen peroxide relative to the solids containing the polyhydroxyalkanoic acid. Item 8: A method for producing a laminate having a resin layer containing polyhydroxyalkanoic acid, comprising the steps of: coating a substrate with the aqueous suspension according to item 7 to form a coating film; and drying the coating film. [Item 9] A laminate having a substrate and a resin layer containing a polyhydroxyalkanoic acid produced using an aqueous suspension of polyhydroxyalkanoic acid having a pH of 5 or less, wherein the resin layer has a hydrogen peroxide concentration of 30 to 200 ppm. [Item 10] A molded article comprising the laminate according to item 9.
[0087] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0088] (Method for measuring pH of aqueous suspension) Measurement was carried out using a JIS type I glass electrode pH meter (LAQUAact / manufactured by HORIBA).
[0089] (Method for measuring solid content concentration of aqueous suspension) An aqueous suspension of a polymer placed in an ointment can was heated in an oven at 105°C for 30 minutes, and the solid content concentration in the aqueous suspension was determined from the weight before and after heating.
[0090] (Method for evaluating foaming due to incorporation of hydrogen peroxide) The foaming of the aqueous suspension after incorporation of hydrogen peroxide was evaluated according to the following criteria: No foaming after incorporation of hydrogen peroxide: Good; Foaming after incorporation of hydrogen peroxide, but the foam disappeared after one day: Fair; Foaming after incorporation of hydrogen peroxide, and the foam remained after one day: Bad.
[0091] (Method for measuring bacterial count) The aqueous suspension stored at room temperature for 14 days was diluted with sterilized water and placed in a Petri dish, and dissolved Waxman agar medium was poured into it, mixed, solidified into a sheet, and cultured for 2 days in an incubator set at 32°C (pour plate culture method). After culture, the number of microbial colonies that appeared on the sheet was counted using a colony counter to determine the number of bacteria in the aqueous suspension.
[0092] (Method for Evaluating Odor of Aqueous Suspension) The odor of the aqueous suspension stored at room temperature for 14 days was evaluated according to the following criteria: No unpleasant odor: ○ Slightly unpleasant fermentation odor: △ Extremely unpleasant fermentation odor: ×
[0093] (Method for calculating molecular weight retention of polymer after heating) The water content in the aqueous suspension was dried to obtain a powder, which was then measured for molecular weight using gel permeation chromatography. The powder was then preheated at 160°C for 2 minutes, and then heated at the same temperature for 20 minutes. The molecular weight was then measured again under the same conditions. The ratio (%) of the molecular weight after heating to the molecular weight before heating was calculated, and this was defined as the molecular weight retention.
[0094] (Method for measuring hydrogen peroxide content in coating film of coated paper) Coated paper cut into 1 cm squares was immersed in chloroform kept at 40°C and stirred for 3 hours, and water was added to the filtrate, followed by separation and extraction. Potassium permanganate was added dropwise to the separated aqueous layer, and the point at which the added solution turned reddish purple was set as the endpoint. The hydrogen peroxide content (ppm) was calculated from the amount of potassium permanganate added up to the endpoint.
[0095] (Preparation of Aqueous Suspension Containing PHBH Isolated from Microorganisms) First, Ralstonia eutropha (formerly Alcaligenes eutrophus AC32 (Deposit No. FERM BP-6038)) into which Aeromonas caviae-derived 3-hydroxyalkanoic acid copolymer synthase group genes had been introduced was cultured by the method described in J. Bacteriol., 179, pp. 4821-4830 (1997), to obtain bacterial cells containing approximately 67% by weight of PHBH. In the PHBH, the composition ratio of PHA repeating units (composition ratio of 3-hydroxybutyrate unit / 3-hydroxyhexanoate unit) was 89 / 11 (mol / mol). Next, paste-like bacterial cells were separated from the culture broth by centrifugation (5000 rpm, 10 min). Water was added to the bacterial cells to prepare a suspension of 75 g dry bacterial cells / L, and aqueous sodium hydroxide solution was added as an alkali to maintain the pH at 11.7. The bacterial constituents other than PHBH were solubilized by stirring and physical disruption, and the mixture was centrifuged (3,000 rpm, 10 min) to obtain a precipitate. The precipitate was further washed with water to separate PHBH with a weight-average molecular weight of approximately 260,000, a 3HH molar fraction of 11%, and a purity of 91 wt%, yielding a suspension containing 75 g / L of PHBH. The suspension was placed in a stirring tank equipped with a pH electrode and maintained at 70°C. The pH electrode was connected to a Marubishi Bioengine Lab Controller Model MDL-6C, and was set so that when the pH fell below the set value, a peristaltic pump would operate and sodium hydroxide aqueous solution would enter the suspension until the set value was reached. The pH of the lab controller was set to 10, and 30% aqueous hydrogen peroxide was added to the suspension so that the hydrogen peroxide concentration was 5 wt% relative to the polymer weight (0.375 wt% relative to the suspension weight), followed by stirring for 1 hour. The suspension was then washed twice with water by centrifugation, and then washed twice with methanol. This yielded an aqueous suspension (A) with a PHA concentration of 52 wt%. The protein content of the aqueous suspension was 1,500 ppm based on the solids, and the PHA purity was 99.8 wt% or more.
[0096] Example 1 Sulfuric acid was added to the prepared aqueous suspension (A) to adjust the pH to 4.6. Then, 30% aqueous hydrogen peroxide was added to the aqueous suspension so that the hydrogen peroxide concentration was 0.1 wt % relative to the solid content (PHA) of the aqueous suspension. This resulted in an aqueous suspension (B). The solid content of this aqueous suspension (B) and the presence or absence of foaming due to the addition of hydrogen peroxide were evaluated, and the molecular weight retention rate of the PHA separated from the aqueous suspension (B) upon heating was measured. Furthermore, the bacterial count and odor of the aqueous suspension (B) were measured 14 days after the addition of hydrogen peroxide.
[0097] Furthermore, PVA resin (partially saponified product (saponification degree 88%), Kuraray Poval 5-88, manufactured by Kuraray Trading Co., Ltd.) was blended into the aqueous suspension (B) in an amount of 3% by weight based on the solid content of the aqueous suspension (B) to prepare a coating material. 2 The coating material was applied so that the coating was as follows: the coating material was dried at 105°C for 2 minutes to evaporate the water, and then the coating material was heated at 160°C for 2 minutes to obtain coated paper.
[0098] The resulting coated paper was subjected to potassium permanganate titration to measure the hydrogen peroxide content in the coating film. The results are shown in Table 1.
[0099] Example 2 The same procedure as in Example 1 was carried out, except that the hydrogen peroxide solution was added so that the concentration of hydrogen peroxide relative to the solid content of the aqueous suspension was 0.5% by weight. The results are shown in Table 1.
[0100] Example 3 The same procedure as in Example 1 was carried out, except that the hydrogen peroxide solution was added so that the hydrogen peroxide concentration relative to the solid content of the aqueous suspension was 1.0 wt %. The results are shown in Table 1.
[0101] Example 4 The same procedure as in Example 1 was carried out, except that the hydrogen peroxide solution was added so that the hydrogen peroxide concentration relative to the solid content of the aqueous suspension was 0.05% by weight. The results are shown in Table 1.
[0102] Example 5 The same procedure as in Example 1 was carried out, except that the hydrogen peroxide solution was mixed so that the hydrogen peroxide concentration relative to the solid content of the aqueous suspension was 1.5 wt %. The results are shown in Table 1.
[0103] Comparative Example 1 The same procedure as in Example 1 was carried out, except that sulfuric acid was added to adjust the pH to 4.6, and hydrogen peroxide was not added. The results are shown in Table 1.
[0104] Comparative Example 2 The same procedure as in Example 1 was carried out, except that sulfuric acid was not added to the aqueous suspension. The results are shown in Table 1.
[0105]
[0106] Table 1 shows that in Examples 1 to 5, in which hydrogen peroxide was added to a PHA aqueous suspension having a pH of 5 or less, the bacterial count after storage of the aqueous suspension was relatively low and the odor was relatively suppressed. It also shows that the molecular weight retention rate of the polymer after heating was relatively high. On the other hand, in Comparative Example 1, in which hydrogen peroxide was not added to the PHA aqueous suspension, the bacterial count after storage of the aqueous suspension increased and a significantly unpleasant fermentation odor was also observed. Furthermore, in Comparative Example 2, in which hydrogen peroxide was added to an aqueous suspension having a pH greater than 5, the molecular weight of the PHA obtained from the aqueous suspension was significantly reduced by heating.
Claims
1. The method includes a step of adding hydrogen peroxide to an aqueous suspension (A) of polyhydroxyalkanoic acid having a pH of 5 or less, A method for producing an aqueous polyhydroxyalkanoic acid suspension, wherein the protein content in the aqueous polyhydroxyalkanoic acid suspension (A) is 30,000 ppm or less based on the total solid content in the aqueous polyhydroxyalkanoic acid suspension (A).
2. 2. The method according to claim 1, wherein the amount of hydrogen peroxide added is 0.1 to 1% by weight based on the solid content containing the polyhydroxyalkanoic acid.
3. The number of bacteria in the aqueous suspension after the addition of hydrogen peroxide was 4 x 10 2 The method according to claim 1 or 2, wherein the concentration of the nucleophilic substance is less than or equal to 1 / ml.
4. The method according to claim 1 or 2, wherein the concentration of solids containing the polyhydroxyalkanoic acid in the aqueous suspension (A) is 20 to 60% by weight.
5. 3. The method according to claim 1, wherein the polyhydroxyalkanoic acid is a copolymer containing 3-hydroxybutyrate units and other hydroxyalkanoate units.
6. The method according to claim 5, wherein the other hydroxyalkanoate units are 3-hydroxyhexanoate units.
7. 1. An aqueous suspension of polyhydroxyalkanoic acid comprising: The pH of the aqueous suspension is 5 or less, the aqueous suspension contains hydrogen peroxide in an amount of 0.05 to 1.5% by weight based on the solid content including the polyhydroxyalkanoic acid; A polyhydroxyalkanoic acid aqueous suspension, in which the protein content contained in the aqueous suspension is 30,000 ppm or less based on the total solid content contained in the aqueous suspension.
8. The method includes a step of coating the aqueous suspension according to claim 7 on a substrate to form a coating film, and a step of drying the coating film. A method for producing a laminate having a resin layer containing a polyhydroxyalkanoic acid.
9. A substrate; A resin layer containing polyhydroxyalkanoic acid produced using an aqueous suspension of polyhydroxyalkanoic acid having a pH of 5 or less, The laminate, wherein the hydrogen peroxide concentration in the resin layer is 30 to 200 ppm.
10. A molded article comprising the laminate according to claim 9.
11. A process for disrupting microbial cells that have accumulated polyhydroxyalkanoic acid; and The method according to claim 1 or 2, further comprising a step of performing a purification treatment for decomposing and / or removing cell-derived components other than polyhydroxyalkanoic acid to reduce the protein content, and further adjusting the pH to 5 or less to obtain an aqueous suspension of polyhydroxyalkanoic acid (A).
12. The manufacturing method described in claim 11, wherein the purification treatment is carried out using at least one member selected from the group consisting of enzymes, hypochlorous acid, and hydrogen peroxide.
13. The method of claim 12, wherein the purification treatment is carried out while controlling the pH of the polyhydroxyalkanoic acid dispersion to 7 to 13 using hydrogen peroxide.