Photocurable composition, three-dimensional shaped object, and tool to be fit inside oral cavity

JPWO2023189780A5Active Publication Date: 2024-11-28MITSUI CHEMICALS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024511848
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-17
Filing Date
2023-03-17
Publication Date
2024-11-28
Estimated Expiration
2043-03-17

AI Technical Summary

Technical Problem

Three-dimensional objects manufactured by stereolithography for dental applications, such as dentures and appliances, often lack sufficient toughness after cleaning with isopropyl alcohol, which compromises their performance in the oral cavity.

Method used

A photocurable composition comprising (meth)acrylic monomers with specific structures and a photopolymerization initiator, which forms a cured product with high toughness even after isopropyl alcohol cleaning, utilizing a combination of (meth)acrylic monomers A and B with urethane bonds and (meth)acryloyl groups, and a photopolymerization initiator, optimized for stereolithography.

Benefits of technology

The composition ensures that the three-dimensional objects exhibit enhanced bending strength, elastic modulus, and toughness, making them suitable for use in the oral cavity as durable dental appliances.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2023189780000001
    Figure 2023189780000001
  • Figure 2023189780000002
    Figure 2023189780000002
  • Figure 2023189780000003
    Figure 2023189780000003
Patent Text Reader

Abstract

Provided is a photocurable composition comprising: a (meth)acrylic monomer (A) that has two urethane bonds and two (meth)acryloyl groups, each of the two (meth)acryloyl groups being joined to each of the two urethane bonds via a C4-10 alkylene group having bonded thereto an oxygen atom or a nitrogen atom; a (meth)acrylic monomer (B) having one (meth)acryloyl group; and a photopolymerization initiator.
Need to check novelty before this filing date? Find Prior Art

Description

Photocurable composition, three-dimensional object, and appliance to be worn in the oral cavity

[0001] The present disclosure relates to a photocurable composition, a three-dimensionally shaped object, and an appliance to be worn in the oral cavity.

[0002] In recent years, dental products such as dental prostheses and instruments used in the oral cavity have been studied. For example, from the viewpoint of the efficiency of forming these dental products, a method for producing three-dimensional objects such as dental products by stereolithography using a 3D printer is known (see, for example, Patent Document 1).

[0003] Patent No. 4160311

[0004] When a three-dimensional object produced by stereolithography using a photocurable composition is used for an intraoral appliance such as a denture base or a splint, it is required to have a certain level of toughness in addition to a certain level of bending strength and bending modulus. Furthermore, a three-dimensional object produced by stereolithography is sometimes washed with isopropyl alcohol after fabrication, but this washing can reduce the toughness of the three-dimensional object, and in some cases, sufficient toughness cannot be obtained.

[0005] An object of one aspect of the present disclosure is to provide a photocurable composition capable of producing a three-dimensional object that has high toughness even after being washed with isopropyl alcohol, as well as a three-dimensional object obtained from the photocurable composition, and an appliance to be worn in the oral cavity.

[0006] Means for solving the above problems include the following aspects. <1> A photocurable composition comprising: a (meth)acrylic monomer (A) having two urethane bonds and two (meth)acryloyl groups, each of which is linked to the two urethane bonds via an alkylene group having 4 to 10 carbon atoms and an oxygen atom or a nitrogen atom bonded thereto; a (meth)acrylic monomer (B) having one (meth)acryloyl group; and a photopolymerization initiator. <2> The photocurable composition according to <1>, wherein the (meth)acrylic monomer (A) is a compound represented by the following general formula (A-1):

[0007]

[0008] (In formula (A-1), R 1A is a divalent hydrocarbon group, and R 2A and R 3A are each independently an alkylene group having 4 to 10 carbon atoms, and R 4A and R 5A are each independently a methyl group or a hydrogen atom. 1A <4> The photocurable composition according to <2>, wherein R in the general formula (A-1) is a divalent hydrocarbon group having 5 to 20 carbon atoms. 1A is a group represented by any one of the following general formulas (a-1) to (a-7):

[0009]

[0010] (In formulas (a-1) to (a-7), * indicates a bonding position.) <5> The photocurable composition according to any one of <1> to <4>, wherein the (meth)acrylic monomer (B) is at least one of a compound represented by the following general formula (B-1) and a compound represented by the following general formula (B-2):

[0011]

[0012] (In formula (B-1), R 1B1 is a monovalent organic group having one or more groups selected from the group consisting of an aromatic ring, a hydroxy group, and a carboxy group, and R 2B1 is a methyl group or a hydrogen atom. 1B2 and R 2B2 are each independently a monovalent organic group, and R 1B2 and R 2B2 may be bonded to each other to form a ring, R 3B2represents a methyl group or a hydrogen atom.) <6> The photocurable composition according to any one of <1> to <5>, wherein the (meth)acrylic monomer (A) has a molecular weight of 440 to 650. <7> The photocurable composition according to any one of <1> to <6>, wherein the (meth)acrylic monomer (B) has a molecular weight of 125 to 300. <8> The photocurable composition according to any one of <1> to <7>, wherein the content of the (meth)acrylic monomer (A) is 300 to 950 parts by mass per 1000 parts by mass of the (meth)acrylic monomer component contained in the photocurable composition. <9> The photocurable composition according to any one of <1> to <8>, wherein the content of the (meth)acrylic monomer (B) is 50 to 700 parts by mass per 1000 parts by mass of the (meth)acrylic monomer component contained in the photocurable composition. <10> The photocurable composition according to any one of <1> to <9>, which has a viscosity of 5 mPa·s to 6,000 mPa·s as measured at 25°C and 50 rpm using an E-type viscometer. <11> The photocurable composition is irradiated with visible light having a wavelength of 405 nm at an irradiation dose of 11 mJ / cm. 2 The cured layers A1 were laminated in the thickness direction to form a rectangular plate-shaped object A1 having a length of 64 mm, a width of 10 mm, and a thickness of 3.3 mm. The object A1 was then irradiated with ultraviolet light having a wavelength of 365 nm at an irradiation dose of 10 J / cm. 2 When a rectangular plate-shaped test piece A1 having a length of 64 mm, a width of 10 mm, and a thickness of 3.3 mm was prepared by irradiating the photocurable composition with visible light having a wavelength of 405 nm, the test piece A1 had a bending strength of 50 MPa or more and a bending modulus of elasticity of 1500 MPa or more, and the irradiation dose of visible light having a wavelength of 405 nm to the photocurable composition was 11 mJ / cm. 2 The cured layers A2 were laminated in the thickness direction to form a rectangular plate-shaped object A2 having a length of 39 mm, a width of 8 mm, and a thickness of 4 mm. The object A2 was then irradiated with ultraviolet light having a wavelength of 365 nm at an irradiation dose of 10 J / cm. 2 When a rectangular plate-shaped test piece A2 having a length of 39 mm, a width of 8 mm, and a thickness of 4 mm was prepared by irradiating the test piece A2, the total work of fracture of the test piece A2 was 500 J / m 2The photocurable composition according to any one of <1> to <10>, which is above. <12> The photocurable composition according to any one of <1> to <11>, which is used for stereolithography. <13> The photocurable composition according to any one of <1> to <12>, which is used for manufacturing an appliance to be worn in the oral cavity by stereolithography. <14> A three-dimensionally shaped object comprising a cured product of the photocurable composition according to any one of <1> to <13>. <15> An appliance to be worn in the oral cavity, which comprises the three-dimensionally shaped object according to <14>.

[0013] According to one aspect of the present disclosure, there are provided a photocurable composition capable of producing a three-dimensional object that has high toughness even after being washed with isopropyl alcohol, as well as a three-dimensional object obtained from the photocurable composition and an appliance to be worn in the oral cavity.

[0014] In the present disclosure, a numerical range expressed using "to" means a range that includes the numerical values ​​written before and after "to" as the lower and upper limits. In the present disclosure, when a composition contains multiple substances corresponding to each component, the amount of each component contained in the composition means the total amount of the multiple substances present in the composition, unless otherwise specified. In the numerical ranges described in stages in the present disclosure, the upper or lower limit described in one numerical range may be replaced with the upper or lower limit of another numerical range described in stages. Furthermore, in the numerical ranges described in the present disclosure, the upper or lower limit of that numerical range may be replaced with a value shown in the examples. In the present disclosure, "light" is a concept that includes active energy rays such as ultraviolet rays and visible light.

[0015] In this disclosure, "(meth)acrylate" means acrylate or methacrylate, "(meth)acryloyl" means acryloyl or methacryloyl, and "(meth)acrylic" means acrylic or methacrylic.

[0016] [Photocurable Composition] The photocurable composition of the present disclosure includes a (meth)acrylic monomer (A) (hereinafter also referred to as "(meth)acrylic monomer (A)") having two urethane bonds and two (meth)acryloyl groups, each of which is linked to the two urethane bonds via an alkylene group having 4 to 10 carbon atoms and to which an oxygen atom or a nitrogen atom is bonded, a (meth)acrylic monomer (B) (hereinafter also referred to as "(meth)acrylic monomer (B)") having one (meth)acryloyl group, and a photopolymerization initiator. The photocurable composition of the present disclosure, by combining the (meth)acrylic monomer (A) and the (meth)acrylic monomer (B), enables the production of a three-dimensionally shaped object that has high toughness even after washing with isopropyl alcohol.

[0017] The photocurable composition of the present disclosure is a composition that cures upon irradiation with light, and a cured product is obtained by curing this composition. A preferred method for producing a cured product using the photocurable composition of the present disclosure is stereolithography. The photocurable composition of the present disclosure is preferably a photocurable composition for stereolithography, and in other words, a cured product produced using the photocurable composition of the present disclosure is preferably a stereolithography product (i.e., a cured product obtained by stereolithography).

[0018] Stereolithography is a method of repeatedly irradiating a photocurable composition with light to form cured layers, thereby laminating the cured layers and obtaining a cured product (i.e., a stereolithography product). Stereolithography may be inkjet-type stereolithography or liquid-vat-type stereolithography (i.e., stereolithography using a liquid vat).

[0019] In inkjet stereolithography, droplets of a photocurable composition are ejected from an inkjet nozzle onto a substrate, and the droplets attached to the substrate are irradiated with light to obtain a cured product. In one example of inkjet stereolithography, for example, a head equipped with an inkjet nozzle and a light source is scanned within a plane while the photocurable composition is ejected from the inkjet nozzle onto the substrate, and the ejected photocurable composition is irradiated with light to form a cured layer. These operations are repeated to sequentially stack cured layers to obtain a cured product (i.e., a stereolithography product).

[0020] In liquid tank-type stereolithography, a portion of a photocurable composition (i.e., an uncured photocurable composition in a liquid state; the same applies hereinafter) contained in a liquid tank is cured by irradiating it with light to form a cured layer, and this operation is repeated to stack cured layers and obtain a cured product (i.e., a stereolithography product). Liquid tank-type stereolithography differs from inkjet-type stereolithography in that a liquid tank is used. Examples of liquid tank-type stereolithography include DLP (Digital Light Processing) stereolithography and SLA (Stereolithography) stereolithography. In the DLP method, planar light is irradiated onto the photocurable composition in the liquid tank. In the SLA method, laser light is scanned onto the photocurable composition in the liquid tank. From the viewpoint of more effectively achieving the effects of the photocurable composition of the present disclosure, DLP-type stereolithography is preferred as liquid tank-type stereolithography.

[0021] An example of DLP-based stereolithography uses a 3D printer (e.g., Kulzer's "Cara Print 4.0," Asiga's "Max UV," etc.) equipped with: a build table movable in the vertical direction; a tray (i.e., liquid tank) arranged below the build table (on the gravity side; the same applies below) that includes a light-transmitting portion and contains a photocurable composition; and a light source (e.g., an LED light source) arranged below the tray for irradiating the photocurable composition in the tray with planar light through the light-transmitting portion of the tray. In this example, first, a gap of one layer is formed between the build table and the tray, and this gap is filled with photocurable composition. Next, planar light is irradiated from below through the light-transmitting portion of the tray onto the photocurable composition filled in the gap, curing the irradiated area to form a first cured layer. Next, the gap between the build table and the tray is widened by the next layer, and the resulting space is filled with photocurable composition. Next, the photocurable composition filling the space is irradiated with light in the same manner as for curing the first layer, forming a second cured layer. By repeating the above operations, cured layers are stacked to produce a three-dimensional object. In this example, the three-dimensional object may be further cured by further irradiating the produced three-dimensional object with light. For details on DLP-based stereolithography, see, for example, Japanese Patent Publication No. 5111880 and Japanese Patent Publication No. 5235056.

[0022] <Applications> The application of the photocurable composition of the present disclosure is not particularly limited. The photocurable composition of the present disclosure may be a photocurable composition used in the production of dental products. Dental products produced using the photocurable composition have high toughness even after being washed with isopropyl alcohol. Examples of dental products include dental prostheses, appliances worn in the oral cavity, dental models, and models for lost-beam casting. Examples of dental prostheses include inlays, crowns, bridges, temporary crowns, and temporary bridges. Examples of appliances worn in the oral cavity include dentures (e.g., complete dentures, partial dentures, etc.), mouthpieces, mouthguards, orthodontic appliances, splints such as occlusal splints and splints for treating temporomandibular disorders, impression trays, and surgical guides. Examples of dental models include tooth and jaw models.

[0023] The photocurable composition of the present disclosure is preferably a photocurable composition used for stereolithography, more preferably a photocurable composition used for producing dental products by stereolithography, and even more preferably a photocurable composition used for producing appliances to be worn in the oral cavity by stereolithography.

[0024] <(Meth)acrylic Monomer (A)> The photocurable composition of the present disclosure includes a (meth)acrylic monomer (A) having two urethane bonds and two (meth)acryloyl groups, each of which is linked to the two urethane bonds via an alkylene group having 4 to 10 carbon atoms and an oxygen atom or a nitrogen atom bonded thereto. One type of (meth)acrylic monomer (A) may be used alone, or two or more types may be used in combination.

[0025] The (meth)acrylic monomer (A) is a compound having two urethane bonds, and each of the two (meth)acryloyl groups is linked to each of the two urethane bonds via an alkylene group having 4 to 10 carbon atoms and an oxygen atom or a nitrogen atom bonded thereto. Each of the two (meth)acryloyl groups in the (meth)acrylic monomer (A) is bonded to an oxygen atom or a nitrogen atom bonded to the alkylene group having 4 to 10 carbon atoms, preferably to an oxygen atom or a nitrogen atom bonded to an alkylene group having 4 to 8 carbon atoms, and more preferably to an oxygen atom or a nitrogen atom bonded to an alkylene group having 4 carbon atoms. The use of this (meth)acrylic monomer (A) makes it possible to obtain a three-dimensionally shaped object having excellent flexural modulus, flexural strength, and toughness.

[0026] The (meth)acrylic monomer (A) is preferably a compound having two urethane bonds, in which each of the two (meth)acryloyl groups is linked to each of the two urethane bonds via an alkylene group having 4 to 10 carbon atoms and having an oxygen atom bonded thereto, and more preferably a compound represented by the following general formula (A-1):

[0027]

[0028] In formula (A-1), R 1A is a divalent hydrocarbon group, and R 2A and R 3A are each independently an alkylene group having 4 to 10 carbon atoms, and R 4A and R 5A are each independently a methyl group or a hydrogen atom.

[0029] R in general formula (A-1) 1A is preferably a divalent hydrocarbon group having 5 to 20 carbon atoms, more preferably a divalent chain hydrocarbon group having 5 to 10 carbon atoms or a divalent hydrocarbon group having 6 to 18 carbon atoms and a cyclic structure, and even more preferably a divalent hydrocarbon group having 8 to 16 carbon atoms and a cyclic structure.

[0030] Examples of the divalent chain hydrocarbon group having 5 to 10 carbon atoms include a pentylene group, a hexylene group, a heptylene group, an octylene group, a nonylene group, and a decylene group.

[0031] Examples of the cyclic structure include an aromatic ring structure, an alicyclic structure, etc. The cyclic structure also includes a combination of an aromatic ring structure and another linking group (for example, a divalent hydrocarbon group), such as a bisphenol A structure.

[0032] Examples of the aromatic ring structure include a benzene ring, a naphthalene ring, a bisphenol A structure, a phenylphenol structure, a phenoxybenzyl structure, a phenylalkylene structure, and an α-hydroxyphenyl structure.

[0033] Examples of the alicyclic structure include a cyclopropylene group, a cyclobutylene group, a cyclopentylene group, a cyclohexylene group, a cyclohexenylene group, a cycloheptylene group, a cyclooctylene group, a cyclononylene group, a cyclodecylene group, a cycloundecylene group, a cyclododecylene group, a cyclotridecylene group, a cyclotetradecylene group, a cyclopentadecylene group, a cyclooctadecylene group, a cycloicosylene group, a bicyclohexylene group, a norbornylene group, an isobornylene group, and an adamantylene group. Of these, a norbornylene group and an isobornylene group are preferred.

[0034] R in general formula (A-1) 1A is preferably a group represented by any one of the following general formulas (a-1) to (a-7), and more preferably a group represented by any one of the following general formulas (a-1) to (a-4).

[0035]

[0036] In formulas (a-1) to (a-7), * indicates a bonding position.

[0037] R 2A and R 3Aare each independently an alkylene group having 4 to 10 carbon atoms, preferably an alkylene group having 4 to 8 carbon atoms, and more preferably an alkylene group having 4 carbon atoms. Examples of alkylene groups having 4 to 10 carbon atoms include a 1,4-butanediyl group, a 1,2-dimethyl-1,2-ethanediyl group, a 2-methyl-1,3-propanediyl group, a 1,5-pentanediyl group, a 1,6-hexanediyl group, a 1,7-heptanediyl group, a 1,8-octanediyl group, a 1,9-nonanediyl group, a 1,10-decanediyl group, and a 2,4,4-trimethylhexylene group. 2A and R 3A and are preferably both 1,4-butanediyl groups.

[0038] The molecular weight of the (meth)acrylic monomer (A) is preferably 440 to 750, more preferably 440 to 650, even more preferably 450 to 600, and particularly preferably 470 to 550.

[0039] From the viewpoint of obtaining a three-dimensionally shaped article excellent in flexural modulus, flexural strength, and toughness, the content of the (meth)acrylic monomer (A) is preferably 300 parts by mass to 950 parts by mass, more preferably 350 parts by mass to 900 parts by mass, and even more preferably 400 parts by mass to 900 parts by mass, relative to 1000 parts by mass of the (meth)acrylic monomer component contained in the photocurable composition.

[0040] <(Meth)acrylic Monomer (B)> The photocurable composition of the present disclosure contains a (meth)acrylic monomer (B) having one (meth)acryloyl group. The (meth)acrylic monomer (B) may be used alone or in combination of two or more.

[0041] By combining this (meth)acrylic monomer (B) having one (meth)acryloyl group with the above-mentioned (meth)acrylic monomer (A), it becomes possible to produce a three-dimensional object that has high toughness even after washing with isopropyl alcohol.

[0042] The (meth)acrylic monomer (B) of the present disclosure is preferably at least one of a compound represented by the following general formula (B-1) and a compound represented by the following general formula (B-2).

[0043]

[0044] In formula (B-1), R 1B1 is a monovalent organic group having one or more groups selected from the group consisting of an aromatic ring, a hydroxy group, and a carboxy group, and R 2B1 is a methyl group or a hydrogen atom. 1B1 The monovalent organic group in formula (B-2) is preferably a monovalent organic group having 2 to 30 carbon atoms, and more preferably a monovalent organic group having 4 to 20 carbon atoms. 1B2 and R 2B2 are each independently a monovalent organic group, and R 1B2 and R 2B2 may be bonded to each other to form a ring, R 3B2 is a methyl group or a hydrogen atom. 1B2 and R 2B2 The monovalent organic group in R is preferably a monovalent organic group having 2 to 10 carbon atoms, and more preferably a monovalent organic group having 2 to 5 carbon atoms. 1B2 and R 2B2 When R are bonded to each other to form a ring, the ring may be a ring consisting of a nitrogen atom and a carbon atom, or may be a ring consisting of a nitrogen atom, a heteroatom other than a nitrogen atom (for example, an oxygen atom), and a carbon atom. 1B2 and R 2B2 When they are bonded to each other to form a ring, the ring may be a 4-membered to 8-membered ring, or may be a 5-membered or 6-membered ring.

[0045] The (meth)acrylic monomer (B) of the present disclosure may contain two or more compounds represented by general formula (B-1), may contain two or more compounds represented by general formula (B-2), or may contain a combination of one or more compounds represented by general formula (B-1) and one or more compounds represented by general formula (B-2).

[0046] R 1B1is preferably a monovalent organic group having an aromatic ring, a monovalent organic group having a hydroxy group, or a monovalent organic group having a carboxy group. Note that a monovalent organic group having an aromatic ring and a hydroxy group, and a monovalent organic group having an aromatic ring and a carboxy group are classified as a monovalent organic group having an aromatic ring. 1B1 When R is a monovalent organic group having a hydroxy group or a monovalent organic group having a carboxy group, the flexibility of the three-dimensionally shaped object tends to be improved. The monovalent organic group having an aromatic ring may be a monovalent organic group having an aromatic ring and a hydroxy group.

[0047] The monovalent organic group having an aromatic ring may have the aromatic ring structure shown below: In the aromatic ring structure shown below, * indicates the bonding position.

[0048]

[0049] The molecular weight of the (meth)acrylic monomer (B) is preferably 125 to 300, more preferably 130 to 280, and even more preferably 130 to 270.

[0050] From the viewpoint of obtaining a three-dimensionally shaped object having excellent flexural modulus, flexural strength, and toughness, the content of the (meth)acrylic monomer (B) is preferably 50 parts by mass to 700 parts by mass, more preferably 100 parts by mass to 650 parts by mass, and even more preferably 100 parts by mass to 600 parts by mass, relative to 1000 parts by mass of the (meth)acrylic monomer component contained in the photocurable composition.

[0051] From the viewpoint of obtaining a three-dimensionally shaped article excellent in flexural modulus, flexural strength, and toughness, the ratio of the contents of the (meth)acrylic monomer (A) and the (meth)acrylic monomer (B) ((meth)acrylic monomer (A):(meth)acrylic monomer (B)) may be 40:60 to 95:5 or 45:55 to 90:10.

[0052] The photocurable composition of the present disclosure may contain photopolymerizable components other than the (meth)acrylic monomer (A) and the (meth)acrylic monomer (B) (hereinafter referred to as "other photopolymerizable components"). Examples of other photopolymerizable components include compounds containing an ethylenic double bond. Examples of compounds containing an ethylenic double bond include (meth)acrylic monomers other than the (meth)acrylic monomer (A) and the (meth)acrylic monomer (B), styrene, styrene derivatives, (meth)acrylonitrile, and the like. Hereinafter, the (meth)acrylic monomer (A), the (meth)acrylic monomer (B), and other photopolymerizable components used as needed will also be referred to as photopolymerizable components.

[0053] From the viewpoint of mechanical strength of the three-dimensional object, the content of the photopolymerizable component relative to the total amount of the photocurable composition of the present disclosure is preferably 60% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. The upper limit of the content of the photopolymerizable component relative to the total amount of the photocurable composition of the present disclosure is not particularly limited, and may be less than 100% by mass, for example, 99.9% by mass or less.

[0054] From the viewpoint of obtaining a three-dimensional object having excellent flexural modulus, flexural strength, and toughness, the total content of the (meth)acrylic monomer (A) and the (meth)acrylic monomer (B) is preferably 50% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, based on the total mass of the photopolymerizable components. The upper limit of the total content of the (meth)acrylic monomer (A) and the (meth)acrylic monomer (B) is not particularly limited, and may be 100% by mass or less, based on the total mass of the photopolymerizable components.

[0055] The (meth)acrylic monomer as another photopolymerizable component may contain a (meth)acrylic monomer (C) represented by the general formula (C-1).

[0056]

[0057] In formula (C-1), R 1C is a divalent hydrocarbon group, and R 2C and R 3Care each independently an alkylene group having 2 or 3 carbon atoms, and R 4C and R 5C are each independently a methyl group or a hydrogen atom. 1C A preferred structure of R in the above formula (A-1) is 1A This is the same as the preferred configuration of R. 2C and R 3C are each independently an alkylene group having 2 or 3 carbon atoms. Examples of the alkylene group having 2 or 3 carbon atoms include an ethylene group, a propylene group, and a methylethylene group. 2C and R 3C and are preferably both ethylene groups.

[0058] Other (meth)acrylic monomers that are photopolymerizable components include (meth)acrylic monomers having two (meth)acryloyl groups and no urethane bond, and (meth)acrylic monomers having three or more (meth)acryloyl groups.

[0059] The content of the other photopolymerizable component (preferably the (meth)acrylic monomer (C)) is preferably 50% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less, based on the total mass of the photopolymerizable component. The lower limit of the content of the other photopolymerizable component (preferably the (meth)acrylic monomer (C)) is not particularly limited, and may be 0% by mass or more based on the total mass of the photopolymerizable component.

[0060] <Photopolymerization Initiator> The photocurable composition of the present disclosure contains a photopolymerization initiator. The photopolymerization initiator is not particularly limited as long as it generates radicals upon irradiation with light, and is preferably one that generates radicals at the wavelength of light used during stereolithography. The wavelength of light used during stereolithography is generally 365 nm to 500 nm, but in practice, it is preferably 365 nm to 430 nm, and more preferably 365 nm to 420 nm. Examples of photopolymerization initiators include acylphosphine oxide-based compounds, alkyl benzoylformate compounds, alkylphenone-based compounds, titanocene-based compounds, oxime ester-based compounds, benzoin-based compounds, acetophenone-based compounds, benzophenone-based compounds, thioxanthone-based compounds, α-acyloxime ester-based compounds, phenylglyoxylate-based compounds, benzyl-based compounds, azo-based compounds, diphenyl sulfide-based compounds, organic dye-based compounds, iron-phthalocyanine-based compounds, benzoin ether-based compounds, and anthraquinone-based compounds. The photopolymerization initiator may be contained in one kind or in a combination of two or more kinds.

[0061] As the photopolymerization initiator, from the viewpoint of reactivity, an acylphosphine oxide-based compound and an alkylphenone-based compound are more preferable, and as the photopolymerization initiator, it is more preferable to use one or more acylphosphine oxide-based compounds, or to use one or more acylphosphine oxide-based compounds and one or more alkylphenone-based compounds in combination.

[0062] Examples of the acylphosphine oxide compounds include 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 2,6-dimethoxybenzoyldiphenylphosphine oxide, and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide.

[0063] An example of the alkylphenone compound is 1-hydroxy-cyclohexyl-phenyl-ketone.

[0064] The total content of the photopolymerization initiators in the photocurable composition of the present disclosure is preferably 0.1% by mass to 10% by mass, more preferably 0.3% by mass to 8% by mass, and even more preferably 0.5% by mass to 5% by mass, relative to the total amount of the photocurable composition.

[0065] <Other Components> The photocurable composition of the present disclosure may contain one or more other components other than the above-described components, as necessary. When the photocurable composition contains other components, the total mass of the (meth)acrylic monomer (A), the (meth)acrylic monomer (B), and the photopolymerization initiator is preferably 30% by mass or more, more preferably 50% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, and even more preferably 90% by mass or more, based on the total amount of the photocurable composition.

[0066] Examples of other components include monomers other than the (meth)acrylic monomer (A) and the (meth)acrylic monomer (B) (for example, the above-mentioned (meth)acrylic monomer (C)). When the photocurable composition contains a monomer other than the (meth)acrylic monomer (A) and the (meth)acrylic monomer (B) as other components, the content of the monomer as the other component is preferably 50% by mass or less, more preferably 30% by mass or less, even more preferably 20% by mass or less, and particularly preferably 10% by mass or less, based on the total mass of the (meth)acrylic monomer (A) and the (meth)acrylic monomer (B).

[0067] Examples of other components include colorants, coupling agents such as silane coupling agents (e.g., 3-acryloxypropyltrimethoxysilane), additives such as rubber agents, ion trapping agents, ion exchange agents, leveling agents, plasticizers, and antifoaming agents, and thermal polymerization initiators. When the photocurable composition of the present disclosure contains a thermal polymerization initiator, photocuring and thermal curing can be performed in combination. Examples of thermal polymerization initiators include thermal radical generators and amine compounds.

[0068] However, from the viewpoint of further improving the molding accuracy of the cured product, the photocurable composition of the present disclosure does not contain an inorganic filler (e.g., silica, barium borosilicate glass, etc.; the same applies hereinafter), or if it contains an inorganic filler, the content of the inorganic filler relative to the total amount of the photocurable composition is preferably 60% by mass or less (more preferably 40% by mass or less, even more preferably 20% by mass or less, and particularly preferably 10% by mass or less).

[0069] The method for preparing the photocurable composition of the present disclosure is not particularly limited. Examples of methods for preparing the photocurable composition of the present disclosure include a method of mixing (meth)acrylic monomer (A), (meth)acrylic monomer (B), a photopolymerization initiator, and, if necessary, other components. The means for mixing the components is not particularly limited, and includes, for example, ultrasonic dissolution, a twin-arm mixer, a roll mixer, a twin-screw extruder, a ball mill mixer, and a planetary mixer. The photocurable composition of the present embodiment may be prepared by mixing the components, filtering the mixture through a filter to remove impurities, and then subjecting the mixture to a vacuum degassing treatment.

[0070] <Preferred Viscosity of Photocurable Composition> The photocurable composition of the present disclosure preferably has a viscosity (hereinafter also simply referred to as "viscosity") measured at 25°C and 50 rpm using an E-type viscometer of 5 mPa·s to 6000 mPa·s. Here, rpm means revolutions per minute (revolutions per minute). When the viscosity is 5 mPa·s to 6000 mPa·s, the photocurable composition exhibits excellent handleability when producing a cured product (particularly a stereolithography product). The viscosity is more preferably 10 mPa·s to 5000 mPa·s, even more preferably 20 mPa·s to 5000 mPa·s, and even more preferably 100 mPa·s to 4500 mPa·s.

[0071] In the photocurable composition of the present disclosure, the photocurable composition is irradiated with visible light having a wavelength of 405 nm at an irradiation dose of 11 mJ / cm 2The cured layers A1 were laminated in the thickness direction to form a rectangular plate-shaped object A1 having a length of 64 mm, a width of 10 mm, and a thickness of 3.3 mm. The object A1 was then irradiated with ultraviolet light having a wavelength of 365 nm at an irradiation dose of 10 J / cm. 2 When a rectangular plate-shaped test piece A1 having a length of 64 mm, a width of 10 mm, and a thickness of 3.3 mm is prepared by irradiating the material, it is preferable that the bending strength of the test piece A1 is 50 MPa or more and the bending modulus of elasticity is 1500 MPa or more.

[0072] In the photocurable composition of the present disclosure, the photocurable composition is irradiated with visible light having a wavelength of 405 nm at an irradiation dose of 11 mJ / cm 2 The cured layers A2 were laminated in the thickness direction to form a rectangular plate-shaped object A2 having a length of 39 mm, a width of 8 mm, and a thickness of 4 mm. The object A2 was then irradiated with ultraviolet light having a wavelength of 365 nm at an irradiation dose of 10 J / cm. 2 When a rectangular plate-shaped test piece A2 having a length of 39 mm, a width of 8 mm, and a thickness of 4 mm was prepared by irradiating the test piece A2, the total work of fracture of the test piece A2 was 500 J / m 2 It is preferable that this is equal to or greater than this.

[0073] The upper limit of the bending strength of the test piece A1 is not particularly limited, and may be, for example, 90 MPa or less. The upper limit of the bending modulus of the test piece A1 is not particularly limited, and may be, for example, 3000 MPa or less. The upper limit of the total work of fracture of the test piece A2 is not particularly limited, and may be 2000 J / m 2 It may be the following:

[0074] For test piece A1 cleaned with IPA, the bending strength and bending modulus of test piece A1 may satisfy the above-mentioned numerical conditions. For test piece A2 cleaned with IPA, the total work of fracture of test piece A2 may satisfy the above-mentioned numerical conditions. Examples of cleaning methods using IPA include the methods described in the Examples below.

[0075] If the test piece A1 obtained from the photocurable composition of the present disclosure satisfies the above-mentioned conditions for flexural strength and flexural modulus, an oral appliance having excellent mechanical strength will tend to be obtained. If the test piece A2 obtained from the photocurable composition of the present disclosure satisfies the above-mentioned conditions for total work of fracture, an oral appliance having excellent toughness will tend to be obtained.

[0076] [Three-dimensionally shaped object] The three-dimensionally shaped object of the present disclosure includes a cured product of the photocurable composition of the present disclosure. Therefore, the three-dimensionally shaped object of the present disclosure has high toughness even after being washed with isopropyl alcohol. The three-dimensionally shaped object of the present disclosure preferably includes a cured product obtained by stereolithography (i.e., a stereolithography object). The method for producing the cured product (e.g., a stereolithography object) is as described above.

[0077] [Intraoral appliances] The intraoral appliances of the present disclosure include the three-dimensionally shaped articles described above. Therefore, the intraoral appliances of the present disclosure have high toughness even after cleaning with isopropyl alcohol. Specific examples of intraoral appliances are as described above, such as dentures and splints.

[0078] Examples of the present disclosure will be described below, but the present disclosure is not limited to the following examples.

[0079] Examples 1 to 19, Comparative Examples 1 to 3 <Preparation of Photocurable Compositions> The components shown in Tables 1 to 4 below were mixed to obtain photocurable compositions.

[0080] <Measurements and Evaluations> The photocurable compositions obtained were subjected to the following measurements and evaluations. The results are shown in Tables 1 to 4.

[0081] (IPA cleaning method) Using a 3D printer (Kulzer, Cara Print 4.0), the obtained photocurable composition was irradiated with visible light having a wavelength of 405 nm at an irradiation dose of 11 mJ / cm. 2The cured layers A1 were then stacked in the thickness direction to obtain a 64 mm long, 10 mm wide, and 3.3 mm thick object A1. The resulting object A1 was immersed in isopropyl alcohol (IPA) and cleaned for 5 minutes using an ultrasonic cleaner with an output of 60 W. The cleaned object A1 was then dried using an air blower, and then irradiated with ultraviolet light having a wavelength of 365 nm at a dose of 10 J / cm. 2 Similarly, a 3D printer (Kulzer, Cara Print 4.0) was used to irradiate the photocurable composition with visible light at a wavelength of 405 nm at an irradiation dose of 11 mJ / cm. 2 The cured layer A2 was formed to a thickness of 50 μm, and the cured layer A2 was then shaped to a length of 39 mm, a width of 8 mm, and a thickness of 4 mm to obtain a molded object A2. The molded object A2 was immersed in isopropyl alcohol and cleaned for 5 minutes using an ultrasonic cleaner with an output of 60 W. The cleaned molded object A2 was then dried with an air blower, and then irradiated with ultraviolet light having a wavelength of 365 nm at a dose of 10 J / cm. 2 A rectangular plate-shaped test piece A2 with a length of 39 mm, a width of 8 mm, and a thickness of 4 mm was obtained by stereolithography under the condition of irradiation with ultraviolet light at a wavelength of 365 nm. For the test pieces without IPA cleaning, test pieces A1 and A2 were obtained by irradiating ultraviolet light at a wavelength of 365 nm without undergoing the aforementioned isopropyl alcohol immersion process. Note that the above cleaning method using IPA is only an example, and the cleaning method using IPA is not limited to the method described in the Examples. Furthermore, for each of Examples 1 to 3 and Comparative Examples 1 to 3, a comparison of the cases with IPA cleaning (Examples 1B to 3B, Comparative Examples 1B to 3B) and without IPA cleaning (Examples 1A to 3A, Comparative Examples 1A to 3A) is shown in Tables 1 to 4. For Examples 4 to 19, only the cases with IPA cleaning (Examples 4B to 19B) are shown.

[0082] (Viscosity of Photocurable Composition) The viscosity of the photocurable composition was measured using an E-type viscometer at 25° C. and 50 rpm.

[0083] (Bending Strength and Bending Modulus of Stereolithography) The obtained test piece A1 (hereinafter referred to as "test piece") was stored in a constant temperature water bath at 37±1°C for 50±2 hours. Thereafter, the test piece was removed from the constant temperature water bath, and the bending strength and bending modulus of the removed test piece were measured in accordance with ISO20795-1:2008. These measurements were performed using a tensile testing device (manufactured by Intesco Corporation) at a tensile speed of 5±1 mm / min.

[0084] (Total Work of Fracture in Fracture Toughness Test by Bending Test) The obtained test piece A2 (hereinafter referred to as "test piece") was notched in accordance with ISO20795-1:2008 and stored in a constant temperature water bath at 37±1°C for 7 days±2 hours. Thereafter, the test piece was removed from the constant temperature water bath, and the removed test piece was subjected to a fracture toughness test by bending test in accordance with ISO20795-1:2008 to measure the total work of fracture (J / m 2 The fracture toughness test by bending test (i.e., measurement of total work of fracture) was carried out using a tensile testing machine (manufactured by Intesco Co., Ltd.) at a pushing speed of 1.0±0.2 mm / min.

[0085]

[0086]

[0087]

[0088]

[0089] In Tables 1 to 4, the numbers in the "Composition" column for each Example and Comparative Example mean parts by mass, and blank spaces mean that the corresponding component is not contained.

[0090] <(Meth)acrylic Monomer (A)> In Tables 1 to 4, the compounds classified as (meth)acrylic monomer (A) having two urethane bonds and two (meth)acryloyl groups, each of which is linked to the two urethane bonds via an alkylene group having 4 to 10 carbon atoms and an oxygen atom or a nitrogen atom, are specifically UDA1 to UDA4 shown below.

[0091] UDA1: Compound prepared in Preparation Example 1 UDA2: Compound prepared in Preparation Example 2 UDA3: Compound prepared in Preparation Example 3 UDA4: Compound prepared in Preparation Example 4

[0092]

[0093] <(Meth)acrylic Monomer (B)> In Tables 1 to 4, the compounds classified as the (meth)acrylic monomer (B) having one (meth)acryloyl group are specifically the following compounds.

[0094] BZA: Benzyl acrylate, manufactured by Osaka Organic Chemical Industry Co., Ltd. PO-A: Phenoxyethyl acrylate, manufactured by Kyoeisha Chemical Co., Ltd. 4-HBA: 4-Hydroxybutyl acrylate, manufactured by Osaka Organic Chemical Industry Co., Ltd. POB-A: m-Phenoxybenzyl acrylate, manufactured by Kyoeisha Chemical Co., Ltd. A-LEN-10: Ethoxylated-o-phenylphenol acrylate, manufactured by Shin-Nakamura Chemical Co., Ltd. ACMO: 4-Acryloylmorpholine, manufactured by KJ Chemicals M5700: 2-Hydroxy-3-phenoxypropyl acrylate, manufactured by Toagosei Co., Ltd. HOMS: 2-Methacryloyloxyethyl succinate, manufactured by Kyoeisha Chemical Co., Ltd. HEMA: 2-Hydroxyethyl acrylate, manufactured by Kyoeisha Chemical Co., Ltd. PO: Phenoxyethyl methacrylate, manufactured by Kyoeisha Chemical Co., Ltd.

[0095]

[0096] <(Meth)acrylic Monomer (C)> In Tables 1 to 4, the compounds classified as the (meth)acrylic monomer (C) represented by the above-mentioned general formula (C-1) are specifically UDA5 to UDA7 shown below.

[0097] UDA5: Compound prepared in Production Example 5 UDA6: Compound prepared in Production Example 6 UDA7: Compound prepared in Production Example 7

[0098]

[0099] <Photopolymerization Initiators> In Tables 1 to 4, the compounds classified as photopolymerization initiators are specifically the following photopolymerization initiators 1 to 4.

[0100] Omnirad 819: acylphosphine oxide compound (manufactured by IGM Resins B.V.) Omnirad 184: alkylphenone compound (manufactured by IGM Resins B.V.) Omnirad TPO: acylphosphine oxide compound (manufactured by IGM Resins B.V.)

[0101]

[0102] Production Examples 1 to 7 are explained below. The abbreviations used in the production examples are as follows: HEA: 2-hydroxyethyl acrylate 2-HPA: 2-hydroxypropyl acrylate 4-HBA: 4-hydroxybutyl acrylate DBTDL: dibutyltin dilaurate MEHQ: 4-methoxyphenol TMXDI: 1,3-tetramethylxylylene diisocyanate XDI: m-xylylene diisocyanate NBDI: norbornane-2,6-diylbis(methylene)diisocyanate H6XDI: 1,3-bis(isocyanatomethyl)cyclohexane

[0103] (Production Example 1: Production of UDA1) 288 g (2.00 mol) of 4-HBA, 0.48 g (0.1% by mass relative to the total mass of 4-HBA and XDI), and 0.24 g (0.05% by mass relative to the total mass of 4-HBA and XDI) of MEHQ were added to a 1-liter four-neck flask equipped with a thoroughly dried stirring blade and a thermometer, and the mixture was stirred until homogeneous, after which the temperature was raised to 60°C. Subsequently, 188 g (1.00 mol) of XDI was added dropwise over 1 hour. During the dropwise addition, the internal temperature rose due to the heat of reaction, so the amount added was controlled so that the temperature remained below 80°C. After the entire amount was added dropwise, the reaction temperature was maintained at 80°C, and the reaction was carried out for 10 hours. During this time, the progress of the reaction was monitored by HPLC analysis, and the end point of the reaction was confirmed. The product was discharged from the reactor, yielding 445 g of urethane acrylate (UDA1). The viscosity at 65°C was 430 mPa·s.

[0104] (Production Example 2: Production of UDA2) 288 g (2.00 mol) of 4-HBA, 0.48 g (0.1% by mass relative to the total mass of 4-HBA and TMXDI), and 0.24 g (0.05% by mass relative to the total mass of 4-HBA and TMXDI) of MEHQ were added to a 1-liter four-neck flask equipped with a thoroughly dried stirring blade and a thermometer, and the mixture was stirred until homogeneous, and then heated to 60°C. Subsequently, 244 g (1.00 mol) of TMXDI was added dropwise over 1 hour. During the dropwise addition, the internal temperature rose due to the heat of reaction, so the amount added was controlled so that the temperature remained below 80°C. After the entire amount was added dropwise, the reaction temperature was maintained at 80°C, and the reaction was carried out for 10 hours. During this time, the progress of the reaction was monitored by HPLC analysis, and the end point of the reaction was confirmed. The product was discharged from the reactor to obtain 510 g of urethane acrylate (UDA2), which had a viscosity of 1600 mPa·s at 65° C.

[0105] (Production Example 3: Production of UDA3) 390 g (2.70 mol) of 4-HBA, 0.67 g (0.1% by mass relative to the total mass of 4-HBA and NBDI), and 0.34 g (0.05% by mass relative to the total mass of 4-HBA and NBDI) of MEHQ were added to a 1-liter four-neck flask equipped with a thoroughly dried stirring blade and a thermometer, and the mixture was stirred until homogeneous. The mixture was then heated to 60°C. Subsequently, 278 g (1.35 mol) of NBDI was added dropwise over 1 hour. During the dropwise addition, the internal temperature rose due to the heat of reaction, so the amount added was controlled to maintain the temperature at 80°C or below. After the entire amount was added dropwise, the reaction temperature was maintained at 80°C, and the reaction was carried out for 10 hours. The progress of the reaction was monitored by HPLC analysis, and the end point of the reaction was confirmed. The product was discharged from the reactor, yielding 630 g of urethane acrylate (UDA3). The viscosity at 65°C was 360 mPa·s.

[0106] (Production Example 4: Production of UDA4) 288 g (2.00 mol) of 4-HBA, 0.48 g (0.1% by mass relative to the total mass of 4-HBA and H6XDI), and 0.24 g (0.05% by mass relative to the total mass of 4-HBA and H6XDI) of MEHQ were added to a 1-liter four-neck flask equipped with a thoroughly dried stirring blade and a thermometer, and the mixture was stirred until homogeneous, after which the temperature was raised to 60°C. Subsequently, 194 g (1.00 mol) of H6XDI was added dropwise over 1 hour. During the dropwise addition, the internal temperature rose due to the heat of reaction, so the amount added was controlled so that the temperature remained below 80°C. After the entire amount was added dropwise, the reaction temperature was maintained at 80°C, and the reaction was carried out for 10 hours. During this time, the progress of the reaction was monitored by HPLC analysis, and the end point of the reaction was confirmed. The product was discharged from the reactor to obtain 450 g of urethane acrylate (UDA4), which had a viscosity of 340 mPa·s at 65° C.

[0107] (Production Example 5: Production of UDA5) 232 g (2.00 mol) of HEA, 0.48 g (0.1% by mass relative to the total mass of HEA and TMXDI), and 0.24 g (0.05% by mass relative to the total mass of HEA and TMXDI) of MEHQ were added to a 1-liter four-neck flask equipped with a thoroughly dried stirring blade and a thermometer, and the mixture was stirred until homogeneous. The mixture was then heated to 60°C. Subsequently, 244 g (1.00 mol) of TMXDI was added dropwise over 1 hour. During the dropwise addition, the internal temperature rose due to the heat of reaction, so the amount added was controlled to keep the temperature below 80°C. After the entire amount was added dropwise, the reaction temperature was maintained at 80°C and the reaction was carried out for 10 hours. The progress of the reaction was monitored by HPLC analysis to confirm the end point of the reaction. The product was discharged from the reactor to obtain 455 g of urethane acrylate (UDA5). The viscosity at 65°C was 2200 mPa·s.

[0108] (Production Example 6: Production of UDA6) 418 g (3.21 mol) of 2HPA, 0.72 g (0.1% by mass relative to the total mass of 2-HPA and XDI), and 0.36 g (0.05% by mass relative to the total mass of 2-HPA and XDI) of MEHQ were added to a 1-liter four-neck flask equipped with a thoroughly dried stirring blade and a thermometer, and the mixture was stirred until homogeneous, after which the temperature was raised to 60°C. Subsequently, 303 g (1.61 mol) of XDI was added dropwise over 1 hour. Since the internal temperature rose due to the heat of reaction during the dropwise addition, the amount added was controlled so that the temperature remained below 80°C. After the entire amount was added dropwise, the reaction temperature was maintained at 80°C, and the reaction was carried out for 10 hours. At this time, the progress of the reaction was monitored by HPLC analysis, and the end point of the reaction was confirmed. The product was discharged from the reactor, yielding 690 g of urethane acrylate (UDA7). The viscosity at 65°C was 570 mPa·s.

[0109] (Production Example 7: Production of UDA7) 372 g (3.20 mol) of HEA, 0.70 g of DBTDL (0.1% by mass relative to the total mass of HEA and NBDI), and 0.35 g of MEHQ (0.05% by mass relative to the total mass of HEA and NBDI) were added to a 1-liter four-neck flask equipped with a thoroughly dried stirring blade and a thermometer, and the mixture was stirred until homogeneous. The mixture was then heated to 60°C. Subsequently, 330 g (1.60 mol) of NBDI was added dropwise over 1 hour. During the addition, the internal temperature rose due to the heat of reaction, so the amount added was controlled to keep the temperature below 80°C. After the entire amount was added dropwise, the reaction temperature was maintained at 80°C and the reaction was carried out for 10 hours. The progress of the reaction was monitored by HPLC analysis to confirm the end point of the reaction. The product was discharged from the reactor to obtain 670 g of urethane acrylate (UDA7). The viscosity at 65°C was 930 mPa·s.

[0110] As shown in Table 1, when the photocurable compositions of Examples 1 to 3 were used, no significant change in the total work of fracture in the fracture toughness test by bending test was observed before and after IPA cleaning. On the other hand, as shown in Table 4, when the photocurable compositions of Comparative Examples 1 to 3 were used, a significant decrease in the total work of fracture in the fracture toughness test by bending test was confirmed after IPA cleaning. These results demonstrate that the use of the photocurable compositions of Examples 1 to 3 enabled the production of three-dimensional objects with high toughness even after cleaning with isopropyl alcohol. For each of Examples 4 to 19, after IPA cleaning, the total work of fracture in the fracture toughness test by bending test was comparable to that obtained using the photocurable compositions of Examples 1 to 3. Furthermore, after IPA cleaning, the total work of fracture in the fracture toughness test by bending test was significantly greater than that obtained using the photocurable compositions of Comparative Examples 1 to 3. Therefore, the use of the photocurable compositions of Examples 4 to 19 enabled the production of three-dimensional objects with high toughness even after cleaning with isopropyl alcohol.

[0111] The disclosure of Japanese Patent Application No. 2022-054222, filed on March 29, 2022, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.

Claims

1. a (meth)acrylic monomer (A) having two urethane bonds and two (meth)acryloyl groups, each of the two (meth)acryloyl groups being linked to each of the two urethane bonds via an alkylene group having 4 to 10 carbon atoms and having an oxygen atom or a nitrogen atom bonded thereto; A (meth)acrylic monomer (B) having one (meth)acryloyl group; A photocurable composition comprising:

2. The photocurable composition according to claim 1, wherein the (meth)acrylic monomer (A) is a compound represented by the following general formula (A-1): 【Chemistry 1】 (In formula (A-1), R 1A is a divalent hydrocarbon group, R 2A and R 3A are each independently an alkylene group having 4 to 10 carbon atoms; R 4A and R 5A are each independently a methyl group or a hydrogen atom.

3. R in the general formula (A-1) 1A The photocurable composition according to claim 2, wherein is a divalent hydrocarbon group having 5 to 20 carbon atoms.

4. R in the general formula (A-1) 1A is a group represented by any one of the following general formulas (a-1) to (a-7): 【Chemistry 2】 (In formulas (a-1) to (a-7), * indicates a bonding position.)

5. The (meth)acrylic monomer (B) is a compound represented by the following general formula (B-1): The photocurable composition according to any one of claims 1 to 4, which is at least one compound represented by the following general formula (B-2): 【Chemistry 3】 (In formula (B-1), R 1B1 is a monovalent organic group having one or more groups selected from the group consisting of an aromatic ring, a hydroxy group, and a carboxy group; R 2B1 is a methyl group or a hydrogen atom. 1B2 and R 2B2 are each independently a monovalent organic group; R 1B2 and R 2B2 may be bonded to each other to form a ring, R 3B2 is a methyl group or a hydrogen atom.

6. The photocurable composition according to any one of claims 1 to 4, wherein the (meth)acrylic monomer (A) has a molecular weight of 440 to 650.

7. The photocurable composition according to any one of claims 1 to 4, wherein the (meth)acrylic monomer (B) has a molecular weight of 125 to 300.

8. The photocurable composition according to any one of claims 1 to 4, wherein a content of the (meth)acrylic monomer (A) is 300 parts by mass to 950 parts by mass per 1000 parts by mass of the (meth)acrylic monomer component contained in the photocurable composition.

9. The photocurable composition according to any one of claims 1 to 4, wherein the content of the (meth)acrylic monomer (B) is 50 parts by mass to 700 parts by mass relative to 1000 parts by mass of the (meth)acrylic monomer component contained in the photocurable composition.

10. 5. The photocurable composition according to claim 1, having a viscosity of 5 mPa·s to 6000 mPa·s as measured with an E-type viscometer at 25° C. and 50 rpm.

11. The photocurable composition was irradiated with visible light having a wavelength of 405 nm at a dose of 11 mJ / cm 2 The cured layers A1 are laminated in the thickness direction to form a rectangular plate-shaped object A1 having a length of 64 mm, a width of 10 mm, and a thickness of 3.3 mm. The object A1 is irradiated with ultraviolet light having a wavelength of 365 nm at a dose of 10 J / cm. 2 When a rectangular plate-shaped test piece A1 having a length of 64 mm, a width of 10 mm, and a thickness of 3.3 mm is prepared by irradiating the test piece A1, the bending strength of the test piece A1 is 50 MPa or more, the bending modulus of elasticity is 1500 MPa or more, and The photocurable composition was irradiated with visible light having a wavelength of 405 nm at a dose of 11 mJ / cm 2 The cured layers A2 are laminated in the thickness direction to form a rectangular plate-shaped object A2 having a length of 39 mm, a width of 8 mm, and a thickness of 4 mm. The object A2 is irradiated with ultraviolet light having a wavelength of 365 nm at a dose of 10 J / cm. 2 When a rectangular plate-shaped test piece A2 having a length of 39 mm, a width of 8 mm, and a thickness of 4 mm was prepared by irradiating the test piece A2, the total work of fracture of the test piece A2 was 500 J / m 2 The photocurable composition according to any one of claims 1 to 4, wherein

12. The photocurable composition according to any one of claims 1 to 4, which is used for stereolithography.

13. The photocurable composition according to any one of claims 1 to 4, which is used for producing an appliance to be worn in the oral cavity by stereolithography.

14. A three-dimensional object comprising a cured product of the photocurable composition according to any one of claims 1 to 4.

15. An appliance to be fitted in an oral cavity, comprising the three-dimensional object according to claim 14.