Method for producing releasable buckled crimped yarn cake, apparatus for producing the same, and releasable buckled crimped yarn cake
Patent Information
- Application Number
- JP2025520520
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Priority Date
- 2023-05-18
- Filing Date
- 2024-05-07
- Publication Date
- 2024-11-21
AI Technical Summary
Conventional methods for producing buckled crimped yarn require complex processes involving high-speed winding, rewinding, and crimping, leading to high equipment costs, safety concerns, and difficulties in achieving both bulkiness and compactness, with limited versatility and dimensional stability.
A method and apparatus for directly forming a buckled crimped yarn cake by spinning fiber-forming fluid into fibers with buckling crimps, using a pressurized gas chamber or suction gun, and compressing them into a cake shape without high-speed rotating bodies, allowing for easy unwinding and division into small packages.
The method produces yarn with excellent bulkiness, crimp fastness, and dimensional stability, suitable for small-lot, high-mix production, while maintaining fiber versatility, without the need for high-speed equipment and with reduced costs and safety risks.
Abstract
Description
Method for producing unreelable buckled crimped yarn cake, manufacturing device therefor, and unreelable buckled crimped yarn cake
[0001] The present invention relates to a method and apparatus for producing a cake of buckled-crimped yarn (also known as forced-crimped yarn), as well as a releasable buckled-crimped yarn cake obtained by the method. "Releasable" here means that the yarn can be continuously peeled from the cake by pulling the yarn ends apart while adjusting the tension, with or without a guide. The production method of the present invention can simultaneously achieve fiberization of a fiber-forming fluid, imparting buckled crimps, and compressing the yarn into cakes. Because the buckled-crimped yarn is caked in a split state, the unwound yarn is spread and extremely bulky. Furthermore, the cake of the present invention is cylindrical and can be divided perpendicular to its axis, eliminating the need for rewinding when dividing into smaller packages; thus, extremely small packages can be easily produced. Furthermore, because no high-speed rotor is used during packaging, conditions can be easily changed independently for each batch, making it suitable for small-lot, high-mix production. The fibers obtained by the present invention do not undergo an independent drawing process (using rollers), so although they are not high in strength, they do not recover when relaxed and have excellent dimensional stability. Although flat yarns cannot be obtained by the method of the present invention, the versatility of the fibers is not impaired by the inherent crimp, as is the case with wool or cotton yarns.
[0002] Currently, a method is known in which a winder is used to spin fibers at high speeds, for example, at 5,000 m / min or higher, to obtain fibers that do not require additional drawing. Furthermore, it is not difficult to eject the spun fibers through a pressurized gas chamber at 6,000 m / min or higher, as described in Patent Documents 1 and 2, or to use a suction gun (as described in Patent Document 3) to index the fibers at 5,000 m / min or higher. (In this specification, a suction gun refers to a device capable of indexing fibers in an atmospheric pressure environment. In other words, the suction gun method does not include the pressurized gas chamber method described above.) In either case, however, directly packaging such spun fibers requires a high-speed winder, which requires significant safety considerations and requires significant equipment costs. Furthermore, high-speed winding directly connected to spinning produces flat yarns, and if crimping is to be performed midway, a significant speed reduction is unavoidable. On the other hand, if crimping is to be performed on the flat yarn obtained by high-speed winding, rewinding is required, which inevitably increases costs.
[0003] In contrast, other known methods include a pressurized gas chamber method in which fibers are first spun into the atmosphere and then compressed into a cake-like package (Patent Document 4), and a method in which fibers are buckled and crimped by the pressurized gas chamber method directly after spinning to form a buckled and crimped fiber column (Patent Document 5), and then these buckled and crimped fiber columns are stored in a spiral shape to form a package (Patent Document 6). However, the former method (Patent Document 4) lacks a buckling and crimping process, resulting in a low crimpability of the resulting fiber, and the compression device has an unsimple structure, making it impractical. The latter method (Patent Document 5) has the disadvantage that the package easily collapses, making it difficult to achieve high density. The present invention overcomes these problems of the prior art and enables the production of a compressed package of buckled and crimped fibers directly after spinning using a simple method and device.
[0004] US Patent No. 3,707,593 British Patent No. 1574464 JP 1-117179 JP 52-96222 JP 54-46924 JP 55-98061
[0005] The present invention provides a highly bulky buckled crimped yarn cake, an inexpensive and safe method for producing the same, and an apparatus for producing the same.
[0006] Conventional technologies require tedious processes, including spinning, winding, unwinding, buckling crimping (also known as forced crimping), and rewinding, to obtain buckling-crimped yarn from spun raw materials. This requires a high-speed winder and an automatic package changeover device for winding, making it difficult to develop inexpensive and safe equipment, nor to develop equipment that is flexible enough for small-lot, high-mix production. Furthermore, in terms of yarn quality, fibers that undergo a roller-drawing process undergo a process in which their structure is temporarily fixed as a flat yarn. Even if they are subsequently buckling-crimped, the final product tends to recall its crystalline structure (i.e., tends to return to its pre-processing state), making it difficult to obtain a fiber with robust buckling crimp. Furthermore, conventional spool-type packaging makes it difficult to achieve both compactness in the package and bulkiness in the released yarn.
[0007] In other words, while a winder was typically used to produce fiber packages from spun raw materials, high-speed rotors were used at high winding speeds that eliminated the need for additional drawing, requiring significant safety considerations and high equipment costs. Furthermore, the resulting yarn was typically flat. On the other hand, it is possible to wind partially oriented yarns such as POY (Partially Oriented Yarn) and then crimp the yarn while drawing it further, but the rewinding process is costly. In consideration of these problems, the present invention produces unwindable buckled-crimped yarn cakes by directly depositing high-speed spun yarn. Because the buckled-crimped yarns are caked in a split state, the unwound yarns are spread and extremely bulky. Furthermore, the cakes of the present invention are cylindrical and can be split perpendicular to their axes, eliminating the need for rewinding when splitting the package for use. Furthermore, because no high-speed rotors are used for caking, independent conditions can be easily set for each strand, making the present invention suitable for small-lot, high-mix production.
[0008] A fiber-forming fluid is spun from a nozzle and sprayed together with pressurized gas from orifices located at the opposing end of the nozzle to form fiber columns with buckled crimps in the crimp-imparting section located at the tip of the orifice, and the fiber columns are fed into a compression chamber consisting of an inverted funnel-shaped section and a cylindrical section, where they are piled up and formed into cakes while being vibrated and compressed from the downstream side of the compression chamber to produce a releasable buckled crimped yarn cake.
[0009] The method of the present invention does not require a high-speed rotating body during packaging, so it does not require large-scale equipment, and the risks associated with high speeds are minimal. It makes it possible to produce unreelable buckled-crimped yarn cakes directly from spun materials at high speeds. On the other hand, since it is easy to change the production conditions for each spindle, it is suitable for small-lot, high-mix production. Furthermore, the fibers obtained by the present invention have excellent dimensional stability, with strong buckled crimps and compression indentations. While they differ from flat yarns and false-twist textured yarns, this does not impair their versatility as fibers, as is the case with wool or cotton yarns.
[0010] In the present invention, a spinning solution suitable for melt spinning or dry-wet spinning is used as the fiber-forming fluid. However, since the spinning solution must be solidified while being withdrawn together with the high-speed fluid, a melt-spinning solution is advantageous because it can be rapidly solidified by rapid cooling or indexing and there is little exchange of solvents between the spinning solution and the high-speed fluid. Examples of melt-spinning solutions include thermoplastic resin fibers such as polyolefin resins, polyamide resins, polyester resins, polyether ketones, polyether ether ketones, polyether sulfones, polyphenylene sulfides, thermoplastic polyetherimides, and thermoplastic fluorine-based resins. Specifically, the material is preferably polyester, polypropylene, polyamide, polyethylene, or a combination thereof. Particularly preferred polyester materials include polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate, and polyamide materials such as nylon 6 and nylon 66. Such combinations include composite spinning and blend spinning, but the preferred combinations are limited because the materials are prone to yarn breakage when taken up at high speed.
[0011] As a method for taking up the spinning solution while solidifying it together with the high-speed fluid, there is a method in which the spinning solution is ejected from the spinneret into a pressurized gas chamber together with the pressurized gas from a fine hole provided at the opposing part of the spinning spinneret, and a method in which the spinning solution is once spun into the open air, the solidified fibers are sucked into a fine hole with a suction gun, and then ejected from the opposing part together with the pressurized gas.
[0012] The method using a pressurized gas chamber is suitable for high-speed take-up, and because a strong traction force acts in a pressurized fluid atmosphere, it is easy to obtain highly oriented, low-elongation fibers in one go. For example, even with polyethylene terephthalate, which is relatively difficult to orient, it is not difficult to achieve a spinning speed of around 6,000 m per minute and a fiber elongation of about 40% at an air pressure of 2 to 3 atmospheres. Furthermore, it is possible to achieve a spinning speed of 8,000 m per minute or more. Furthermore, this method allows the spun fiber to be buckled and crimped while maintaining a relatively high temperature, making it easy to obtain highly processed fibers.
[0013] On the other hand, even with a high-performance suction gun, additional stretching is not required for polyethylene terephthalate, and it is possible to take up, for example, 5,000 m per minute or more. Suction guns can be operated in the atmosphere, so there is a great degree of freedom in measures against thread breakage, and there is an advantage that the air flow around the nozzle is less affected by the outer wall, making it easier to reduce thread sway and thread breakage.
[0014] On the other hand, if direct spinning is not an issue, any fiber that has been wound up by a traditional method can be used as the raw material, and then it can be ejected from small holes using a suction gun together with pressurized gas, and then similarly formed into a cake. In this case, although there will be differences in quality and cost, a wide range of materials that are not suitable for direct spinning can be used.
[0015] For economical and safe reasons, pressurized air is generally used as the high-velocity fluid after adjusting the temperature to a moderate level. Heated steam can also be used alone or mixed with air, but measures to prevent condensation mist are required and it can be difficult to use with materials that have a low freezing point.
[0016] For the sake of simplicity, the following description will be given by way of example, using the reference numerals in the drawings, of a pressurized gas chamber method using air as the gas and a melt-spinnable polymer as the spinning dope. However, the technical concept of the method of the present invention can be applied to both existing fibers and the suction gun method, and the following description of the examples does not in any way limit the interpretation of the claims of the present invention.
[0017] The pressurized gas chamber (3) smoothly converges at the opposing end of the spinneret (1) and connects to the orifice (6), and the spun fibers are ejected at high speed together with the pressurized air from the open end of the orifice (6). The orifice desirably has a smooth wall surface, and its diameter is preferably 2 to 5 mm, preferably 2.5 to 4 mm, more preferably 2.5 to 3.5 mm, and its length is about 50 to 500 mm, preferably 70 to 300 mm, more preferably 100 to 200 mm.
[0018] If the pore diameter is less than 2 mm, there is a risk of pore clogging in the event of yarn breakage. On the other hand, if the diameter is 5 mm or more, not only does the effect of increasing the take-up speed saturate, but the amount of compressed air becomes excessive, which is uneconomical, increases noise, and the air flow in the compressed air chamber becomes easily disturbed, which can easily cause yarn breakage. Depending on the thickness of the spun fiber, a pore diameter of 2.5 to 4 mm is appropriate for producing an average filament yarn of approximately 50 to 500 denier. With a pore diameter of 2.5 mm or more, even if sudden fusion or yarn breakage of the spun fiber occurs, as long as it is partial, the spun fiber can continue to be taken up. Of course, such fusion or yarn breakage can cause fatal problems such as dye spots in clothing, but it is not necessarily fatal for bulky yarns used for wadding and bulky sheets.
[0019] Even if the length of the pores is 50 mm or less, it is possible to significantly increase the take-up speed, but considering that even greater speeds are possible with lengths longer than that, there is little benefit to actively adopting lengths of 50 mm or less. On the other hand, if the length exceeds 500 mm, the effect of increasing the take-up speed will saturate, so there is little point in actively adopting lengths. However, even if lengths exceed 500 mm, such as 1000 mm or 2000 mm, are used, there are often no fatal problems with regard to the take-up speed, so it is possible to significantly change the position of the jet or, for example, by adopting smoothly curved pores, it becomes possible to significantly change the direction of the jet.
[0020] A gauge pressure of about 1 to 5 atmospheres is often used for the pressure chamber (3). It is easier to maintain a high take-up speed if the solidification point of the spinning dope is as downstream as possible, i.e., near the entrance of the fine holes; therefore, a pressure of 2 to 4 atmospheres is often used for this purpose. However, this pressure shifts to a lower pressure side if the spinning length (the distance from the spinneret (1) to the entrance of the fine holes (6)) is longer, or if the discharge rate of the dope is reduced, or if the air temperature is lower. However, even at a pressure of 1 atmosphere or less, it is not difficult to maintain a take-up speed of about 4,000 m per minute, and depending on the type of polymer and the application of the spun fiber, this can still be sufficient to achieve the intended purpose. On the other hand, a pressure exceeding 5 atmospheres does not necessarily increase the take-up speed, but may be preferable in cases where materials require rapid cooling or high discharge rates are used.
[0021] Here, the solidification point of the spun fibers means the position at which the spun fibers can be taken up and inter-fiber fusion can be avoided during the buckling and crimping process. Therefore, in the present invention, the solidification point of the spinning solution being near the entrance of the pores (6) means that the spinning solution solidifies in that vicinity, and the constituent fibers in the obtained package are not in a fused state but are dispersed as single fibers. Since fusion often remains at or below the melting point of the material but above the second-order transition point, it is not easy to accurately define the temperature of the solidification point. However, the conditions under which the constituent fibers in the obtained package are dispersed as single fibers rather than in a parallel bundle state can be easily grasped as appropriate.
[0022] The pressurized gas chamber (3), being a pressure-resistant vessel, is preferably cylindrical, with one end formed by the nozzle (1) and the other end converged into a funnel shape and connected to the fine hole (6). Its length (from the nozzle (1) to the entrance of the fine hole (6), i.e., corresponding to the spinning length) must be equal to or longer than the length from the nozzle (1) to the solidification point of the spun fiber in order to prevent fusion of the spun fiber. The length from the nozzle (1) to the entrance of the fine hole (6) is typically 300 mm to 5,000 mm, and preferably 500 mm to 2,000 mm. However, since it is easier to increase the take-up speed by positioning the solidification point of the spun fiber at the downstream end of the pressurized gas chamber (3), i.e., near the entrance of the fine hole (6), it is desirable to make the length of the pressurized gas chamber (3) as short as possible within a range that does not cause fusion of the spun fiber. On the other hand, the solidification point of the spun fiber varies greatly depending on the discharge rate of the spinning dope, the solidification temperature, the air pressure, etc., and the spinning length also varies greatly depending on these factors. That is, if the discharge rate is large, or if the solidification temperature of the material is low, or if the air pressure is low, it becomes necessary to increase the spinning length. For example, when attempting to obtain polyester or polyamide filaments of about 150D-48F, a length of 500 to 1000 mm is often adopted for the pressurized gas chamber (3).
[0023] In the pressurized gas chamber (3), to prevent the spinning fluid from shaking or breaking, the compressed air and the spinning fluid must be guided to the pores (6) while flowing together in an orderly manner. To achieve this, it is desirable for the cross section of the compressed air chamber to be large, but there are limits to this. Therefore, the compressed air must be pre-straightened before being guided to the pressurized gas chamber (3). Specifically, a compressed air supply chamber is provided on the outer periphery of the pressurized gas chamber (3), and an annular air dispersion member is provided between the two. The compressed air is uniformly dispersed in the compressed air supply chamber before being supplied to the pressurized gas chamber (3). The air dispersion member is a member that can impart minimal resistance to the passage of compressed air, and examples thereof include a porous metal plate, a metal plate perforated with numerous fine holes, and a laminate of fine wire mesh.
[0024] Empirically, it is preferable to locate the air dispersion member as downstream as possible from the pressurized gas chamber, as this reduces yarn breakage. If it is located upstream, the spinneret is likely to be affected by the compressed air temperature, and the flow pattern of the spinning fluid is likely to be disturbed because the high-speed compressed air comes into contact with the low-speed spinning fluid flow.
[0025] Furthermore, it is desirable for the air dispersion member to have a large air dispersion area in order to maximize its rectifying effect. Since the member is an annular member that constitutes part of the wall of the pressurized air chamber (3) and its diameter cannot be changed significantly, increasing the air dispersion area requires increasing its height. Specifically, in consideration of the strength and processing precision of the member, it is often desirable for the height to be 100 mm rather than 50 mm, and 200 mm rather than 100 mm. This enhances the air dispersion effect and ensures a natural air supply to the upper part of the compressed air chamber.
[0026] The buckling and crimping of the fibers ejected from the perforations is achieved by guiding the ejected fibers through perforations (6) into a permeable narrow path. The narrow path is located on the extension axis of the perforations and is a cylindrical path with a diameter equal to or slightly larger than that of the perforations (6). The path is designed to reduce the coefficient of friction in the axial direction. For example, if the perforations have a diameter of 3 mm, multiple slits parallel to the axis can be provided downstream of the narrow path to achieve an inscribed diameter of 3 to 5 mm, or multiple piano wires approximately 1 to 2 mm in diameter x 100 mm in diameter can be arranged in a cylindrical shape. The piano wires are preferably matte-plated to reduce friction, and gaps of approximately 0.1 to 0.5 mm are provided between them to allow for ventilation.
[0027] The fibers ejected from the pores (6) are opened and dispersed immediately after ejection, and come into contact with the wall of the narrow passage, where they accumulate in a columnar shape due to friction with the wall (i.e., undergo buckling and crimping). However, due to the pressure of the ejected gas, they are continuously ejected from the narrow passage while maintaining the shape of the buckled and crimped fiber column. During buckling and crimping, the microstructure of the fibers has not yet been fixed, and the temperature is high, so there is more plasticity than expected, and the fibers are firmly fixed in their shape. The buckled and crimped fiber column follows the inscribed shape of the narrow passage and takes on a caterpillar-like shape with numerous fluffs at the slit portion. The numerous fluffy fibers are generated by the gas being ejected and discharged. Meanwhile, the ejected gas is continuously ejected and discharged from the gaps in the narrow passage in a direction perpendicular to the axis. Furthermore, by providing a path between the narrow hole and the narrow passage with a diameter 1.5 to 3 times that of the narrow hole, the acceleration force of the spun fiber bundle can be reduced, the fiber bundle can be split, and the buckling crimping process due to contact resistance with the narrow passage wall can be facilitated. In this case, the narrow passage should have a diameter equal to or slightly larger than that of the path. The narrow passage diameter is the dominant factor that determines the crimp period, so the path diameter is also important in this sense.
[0028] The force that continuously pushes out the buckled-crimped fiber pillars is the pressure of the ejected air. When the fiber pillars are formed, the pressure in the compressed air chamber (3) increases by about 10 to 50 kPaG compared to before formation (hereinafter referred to as back pressure), and it can be seen that this pressure functions as an ejection force for the buckled-crimped fiber pillars. If the gap between the compressed air ejection end of the pore and the upper end of the buckled-crimped fiber pillar narrows, the back pressure, i.e., the ejection force, increases; if it widens, it decreases; therefore, a stable balance is reached when the gap is an appropriate value within a few mm.
[0029] On the other hand, if the discharge rate of the buckled-crimped fiber pillars is artificially increased using rollers or the like, the gap increases and the back pressure decreases; if it is decreased, the gap decreases and the back pressure increases. For example, the back pressure can be controlled by feeding the buckled-crimped fiber pillars using rollers arranged on the outer periphery of the narrow path while gripping the fuzz of the buckled-crimped fiber pillars that have been ejected outside the narrow path. Controlling the back pressure contributes to stabilizing operations. Materials for the feed rollers include rubber and metal, and surface shapes such as mirror finish, matte finish, and streaky irregularities are selected depending on the required friction coefficient. Furthermore, an oil can be applied to the buckled-crimped fiber pillars via the feed rollers.
[0030] The buckled and crimped fiber columns are continuously forced into a compression chamber. The compression chamber is composed of an inverted funnel-shaped section (10), a cylindrical section (16), and, for example, a piston (13) located at the opposite end of the inverted funnel-shaped section (10) and inscribed in the cylindrical section. The fiber columns meander while inscribed in the inverted funnel-shaped section (10), expanding radially and spreading throughout the entire cylindrical section (16), where they are layered and compressed to form a compressed fiber mass. By maintaining an appropriate funnel angle (e.g., 20 to 120 degrees) and smoothing the connections between the narrow passages and the cylindrical section, it is possible to prevent the stacking order of the buckled and crimped fiber columns from being reversed. A preferred angle is 25 to 90 degrees, and a more preferred angle is 30 to 60 degrees.
[0031] The piston (13) gradually retracts axially as the compressed fiber mass grows, allowing for continuous production of compressed fiber mass. To increase the density of the fiber mass, the temperature of the fiber in the compression chamber must be maintained above its second-order transition point, and the compression force of the piston must be kept as high as possible. For example, if the back pressure is 20 kPaG and the cross-sectional area of the compressed fiber mass is 100 cm², the compression force can be increased to nearly 20 kg / cm² due to the back pressure.
[0032] Furthermore, by applying vibrations ranging from low frequencies to ultrasonic frequencies in the axial direction of the compressed fiber agglomerates via the piston (13), it is possible to apply dramatically high repeated impact loads without significantly affecting the feeding of the buckled and crimped fiber column at the entrance of the compression chamber. That is, if large voids remain in the compressed fiber agglomerates and the temperature is above the second-order transition point, the compressed fiber agglomerates have strong plasticity, so the vibrations rapidly attenuate within them and hardly propagate to the entrance of the compression chamber. That is, the vibrations significantly increase the apparent density of the compressed fiber agglomerates without inhibiting their axial growth, and can even cake the compressed fiber agglomerates. Acceleration proportional to the square of the frequency is transmitted from the piston as vibration stress, further compressing the compressed fiber agglomerates into cake-like shapes. For example, it is not particularly difficult to apply instantaneous compressive forces of 100 kg / cm or more through vibration compression. Furthermore, the application of high-frequency vibrations improves the lubrication at the interface between the compression chamber wall and the compressed fiber agglomerates, reducing friction and enabling smooth movement of the fiber cakes.
[0033] When the discharge speed of the buckled and crimped fiber columns is artificially controlled using rollers (14) or the like, the back pressure can be adjusted by the feed speed of the rollers (14) and the cake density can be adjusted by the retreat speed of the piston (13). If the retreat speed of the piston (13) is too low, it becomes difficult for the rollers (14) to smoothly feed the buckled and crimped fiber columns, but it is easy to experimentally adjust the retreat speed of the piston (13) so as to maximize the cake density without causing this problem.
[0034] On the other hand, the cake growth rate can be controlled without using the piston (13) by adjusting the cross-sectional area or shape of the downstream side of the compression chamber to provide an appropriate discharge resistance. In this case, the piston movement required for attaching and detaching the package is not required, so an endless cake can be produced and cut to any length. The discharge resistance can be adjusted by providing a resistance member at the discharge section of the compression chamber or by adjusting the shape of the compression chamber, and the shape can also be adjusted externally if the compression chamber is given flexibility. However, if vibration compression by the piston (13) is not used, it will be difficult to increase the cake density.
[0035] However, if the friction between the compressed fiber mass and the compression chamber is too great to allow smooth feeding, it is effective to slightly widen the cylindrical portion (16) of the compression chamber. The degree of widening can be easily determined experimentally, but is usually 5 degrees or less, preferably 3 degrees or less. If widening of the cylindrical portion (16) is to be avoided in order to maintain uniformity of the apparent density within the cake, the amount of oil or lubricity can be adjusted to promote the movement of the compressed fiber mass.
[0036] The density of the fiber cake is uniquely determined by the feed rate of the buckled and crimped fiber columns and the retraction rate of the piston (13). If the retraction rate of the piston (13) is increased, the density of the fiber cake decreases, and if it is decreased, the density increases. However, if the retraction rate is too slow, it becomes difficult to feed the buckled and crimped fiber columns. Therefore, the fiber cake is produced at as low a retraction rate as possible while checking the feed rate of the buckled and crimped fiber columns and the retraction rate of the piston.
[0037] If the fiber material can be maintained above its second-order transition temperature in the compression chamber and maintain its plasticity as a fiber mass, it will be possible to mold it into a cake with a high apparent density. Therefore, it is desirable to provide a heater or jacket for temperature control in part or all of the area surrounding the compression chamber. For example, the melting point of polyethylene terephthalate fiber is around 260°C, but its second-order transition temperature is around 80°C, so the temperature inside the compression chamber should be around 80 to 160°C. By feeding an appropriate amount of oil near the entrance of the compression chamber via a roller or injection, the moist heat state of the fibers and the slippage between the fibers are ensured, further increasing the apparent density of the fiber cake. Moist heat also has an important effect on the fiber transition temperature. Of course, the oil also improves the cake's reelability.
[0038] It is important not to allow the spun fibers an opportunity to cool below the second-order transition point before buckling and crimping them and compressing them into a cake. If cooling is allowed along the way, the crystalline structure of the fibers will be fixed during the cooling process, and even if the processed yarn is subsequently buckling and crimped, it will retain the structure it had at the time of cooling and will attempt to return to its original structure in response to physical and chemical stimuli during subsequent processing and use. The crimped and compressed yarn of the present invention is crimped and compressed at a high plasticity stage before cooling, and does not return to its original structure as described above, making it different from traditional buckling and crimped yarn.
[0039] Furthermore, in the present invention, numerous indentations may occur on the fiber surface during the compression baking process. This is also because the fibers are compressed into cakes in a highly plastic state. Although the indentations are not noticeable in the form of single fibers, they have the effect of reducing the inorganic gloss when the fibers are made into, for example, filament woven fabrics.
[0040] The inner surface of the compression chamber is preferably a low-friction surface, at least in the axial direction, such as a mirror finish or a matte finish. Furthermore, to facilitate the feeding of the cake, at least a portion of the cylindrical portion (16) may be made to have a gently diverging structure.
[0041] The compression chamber preferably has a structure in which at least two detachable cylindrical containers are connected in series. When the downstream cylinder becomes full of cake, it can be separated as a fiber package and replaced with an empty cylinder.
[0042] The cross section of the cylindrical compression chamber may be approximately circular or approximately polygonal. A circle is the simplest, but a triangular, square, or hexagonal polygon has the advantage of allowing for tighter packing when packaging. Of course, the upstream inverted funnel portion (10) should be smoothly connected (i.e., the fibers do not get caught) regardless of the shape of the cylindrical portion (16). Depending on the compression conditions, dyeing irregularities may occur in the buckled crimped yarn at the corners of the approximately polygonal shape. However, intentional use of this can impart irregularities to the yarn, resulting in a shapeless, non-periodic irregularity without fineness variations. Achieving such irregularities while maintaining high fiber productivity is extremely difficult with winder-based yarn reeling technology. Naturally, such irregularities are small in a hexagonal shape and large in a triangular shape. The approximately polygonal shape does not necessarily apply to the entire compression chamber; only the separable portion of the package can be used, and other variations are also possible. Various shapes, such as an ellipse, are also possible. The key is to have a structure that does not hinder the smooth feeding of the cake.
[0043] In a preferred embodiment of the present invention, a high-frequency impact is applied from the downstream side of the package to the upstream side by a piston (13). This impact is similar in quality to the impact commonly used in impact tools, for example. The impact is absorbed by the plasticity of the cake (usually 200 mm or more in major diameter) and the friction between the cake and the compression chamber wall. Furthermore, the piston (13) moves slowly downstream while applying the impact, corresponding to the cake's growth, so it does not impede cake growth. For example, if a cake is continuously impacted with a force of 1 kg / cm², an amplitude of 1 mm, and 10 impacts per second while still in a highly plastic state, the apparent specific gravity will be approximately 0.3 to 0.6. This value translates to a package weight of approximately 700 to 1400 g (100 mm diameter x 300 mm), which is fully practical. In fact, it is exceptionally compact for a package of buckling-crimped yarn.
[0044] The cross-sectional area of the cylindrical portion (16) is determined according to the size of the package required for use. Because it is easy to change, small packages can be easily produced. For example, if the cake has a diameter of 5 cm, a length of 10 cm, and an apparent density of 0.4 g / cm3, the package weight will be 78.5 g, which is equivalent to a length of about 7 km of 100D filament yarn. If it is folded in half, it will become 3.5 km. It is estimated that there are many needs for such end products. However, it is not difficult to make the diameter larger than 10 cm if necessary.
[0045] The fibers obtained by the present invention exhibit significant characteristics of high-speed spinning. For example, polyester fibers exhibit high overall crystallinity, low amorphous orientation, and high crystalline orientation. Tenacity is 3-4 g / d and elongation is approximately 30-50%, which is insufficient for some industrial applications requiring high strength, but sufficient strength for clothing and batting applications. Low amorphous orientation enhances dyeability, while high crystalline orientation affects fiber dimensional stability. On the other hand, fibers produced by traditional methods, which require slow spinning speeds and separate drawing, tend to achieve high strength and a high initial modulus, but when relaxed during subsequent processing, they exhibit an undesirable primary yield point around 1 g / d on the SS curve, leading to dimensional stability problems. In the present invention, the solidification and buckling-crimping of the spun fibers occur almost simultaneously, presumably resulting in buckling-crimping during the process of fixing the fiber structure, making it ideal for improving crimp fastness. Furthermore, the significant formation of indentations on the fiber surface during the compression cake stage is presumably closely related to the fact that the fiber structure is still in the process of being fixed at the time of indentation formation. The indentations on the fiber surface impart a subtle matte effect to the final product. As mentioned above, the crimped compressed yarn of the present invention is crimped and compressed at a stage of high plasticity before cooling, and is therefore different from traditional buckled-crimped yarn, which is buckled and crimped after cooling.
[0046] The above effects are basically common to both the pressurized gas chamber method and the suction gun method. However, in the suction gun method, the spun fiber is taken up while in contact with the inner wall of the suction gun after solidification, whereas in the pressurized gas method, the spun fiber is usually taken up without contact with the inner wall of the pores, which has the advantage that the buckling crimp processing can be carried out in a less solidified state. This means that a higher temperature can be maintained during the fiber processing cycle, and higher crimp fastness can be achieved.
[0047] Spinning material: Polyethylene terephthalate IV 0.68; Die temperature: 300°C; Die (1): 0.25φ, 48H; Discharge rate: 120G / min; Size of the cylindrical part of the compressed air chamber: 150φ x 1.5m, with a 150φ x 100mm porous metal placed at the bottom of the cylindrical part (16); Angle of the funnel-shaped part (10) of the compressed air chamber: 60 degrees; Compressed air: 300kPaG, 30°C; Slit (6): Connects a 3φ x 300mm path and a 7φ x 70mm path; Narrow path: Twelve chrome-plated piano wires, 1φ x 60mm, with a matte finish, are installed downstream, coaxially with the slit (6), so that the inscribed circle is 8mm; Inverted funnel-shaped part (10) The angle is 60 degrees, and the upper end is an 11mmφ cylinder that circumscribes the lower 5mm of the narrow piano wire, then connects to an inverted funnel shape via a 30R curve, and the inner surface of the lower end connects to the cylindrical part of the compression container (16) via a 30R curve. There are two 0.5φ oil supply holes at opposite points 20mm from the upstream end. The cylindrical part of the compression container has an inner diameter of 100φ x 400mm and is detachable 200mm from the upstream side. The connecting surfaces of the upstream and downstream parts are funnel-shaped surfaces that are angled 60° downward to prevent fibers from getting caught. The striking piston is cylindrical with a diameter of 99.5φ, and the compression container side has a flat surface perpendicular to its axis. Impact strength, stroke, and period: 80kg, 2mm, 10 c / sec Temperature inside the compression container: 110°C
[0048] The take-up speed reached approximately 6,000 m. Continuous operation was possible by replacing the downstream compression vessel when a 150 mm cake was filled. It was possible to continuously unwind the buckled crimped yarn from the fiber cake.
[0049] Figure 1 shows an example of an apparatus for spinning, take-up, buckling and crimping, and compression, and the state of the apparatus. Figure 2 shows the state in which the take-up yarn becomes a buckling and crimped fiber column and is sent to the compression chamber. Figure 3 shows the state in which the feed rate of the buckling and crimped fiber column is adjusted with a roller. Figure 4 shows the state in which the feed rate of the buckling and crimped fiber column is adjusted with a roller. Figure 5 shows the state in which the downstream side of the serially connected cylindrical containers is separated into a package. Figure 6 shows the state in which the crimped yarn is unwound from the cake through a guide.
[0050] The method of the present invention allows for the inexpensive and safe production of buckled crimped yarn cakes that can be unwound in one go from spun raw materials. Because the crimped yarns of the present invention are caked in a buckled state, the unwound yarns have excellent bulk and crimp fastness, making them suitable for the production of bulky sheets. Because the cakes of the present invention can be divided axially, rewinding is not required for division; that is, extremely small packages can be easily produced. Because the packaging equipment of the present invention is simple, it is suitable for the production of a wide variety of products in small quantities. Because the fibers obtained by the present invention do not undergo a roller drawing process, they do not have high strength, but they do not recover upon relaxation and have excellent dimensional stability. Although flat yarns cannot be obtained by the method of the present invention, the inherent crimping of the fibers, as is the case with wool or cotton yarns, does not impair the versatility of the fibers.
[0051] REFERENCE SIGNS LIST 1 Spinneret 2 Spun yarn 3 Pressurized gas chamber 4 Pressurized chamber cylinder 5 Pressurized gas distribution chamber 6, 6' Micropores 7, 7', 7'', 7''' Crimping section 8, 8', 8'', 8''' Buckled crimped fiber column 9, 9' Oil distribution chamber 10, 10' Inverted funnel-shaped section of compression chamber 11, 11' Heating medium chamber 12, 12', 12'', 12''' Crimped compressed fiber mass 13 Piston 14, 14' Feed roller 15 Cylindrical section 16 Connecting section 17, 17' Detachable cylindrical section 18 Unwound yarn 19 Guide
Claims
1. A method for producing a releasable buckled crimped yarn cake, comprising: spinning a fiber-forming fluid through a spinneret, spraying it together with pressurized gas from fine holes located at the opposing parts of the spinneret, forming a fiber column having buckled crimps in the crimp-imparting section located at the tip of the fine holes, sending the fiber column into a compression chamber consisting of an inverted funnel-shaped section and a cylindrical section, and stacking the fiber column in the compression chamber while compressing it into a cake.
2. A method for producing a releasable buckled crimped yarn cake according to claim 1, wherein said fiber-forming fluid is spun from a spinneret into a pressurized gas chamber and fiberized in the pressurized gas chamber.
3. A method for producing a releasable buckled crimped yarn cake according to claim 1, wherein the fiber-forming fluid is spun into the atmosphere from a nozzle and then sprayed together with pressurized gas from a small hole located at the opposite side of the nozzle by a suction gun.
4. A method for producing a releasable buckled crimped yarn cake according to claim 1, wherein said compressing method comprises vibrating and compressing the cake from the downstream side of said compression chamber.
5. A method for producing a releasable buckled crimped yarn cake according to claim 1, wherein the means for spinning said fiber-forming fluid from a spinneret into a pressurized gas chamber is melt spinning.
6. A method for producing a releasable buckled crimped yarn cake according to claim 1, wherein said fiber column is compressed in a compression chamber above the second order transition point.
7. The method of producing a releasable buckled crimped yarn cake according to claim 1, further comprising using a feed roller to feed said fiber column into said compression chamber.
8. The method for producing a releasable buckled crimped yarn cake according to claim 3, wherein said fibers are polyester-based, polypropylene-based, polyamide-based, polyethylene-based or combinations thereof.
9. A method for producing a releasable buckled crimped yarn cake according to claim 1, wherein the cross section of said tubular portion is substantially circular.
10. A method for producing a releasable buckled crimped yarn cake according to claim 1, wherein at least the downstream side of the cross section of said tubular portion is approximately polygonal.
11. A method for producing a releasable buckled crimped yarn cake according to claim 1, wherein said tubular portion has a detachable connecting portion in series.
12. A method for producing a releasable buckled crimped yarn cake, comprising: ejecting fibers together with pressurized gas, forming a fiber column having buckled crimps in a crimping section provided at the tip of the fine hole, feeding the fiber column into a compression chamber consisting of an inverted funnel-shaped section and a cylindrical section, and stacking the fiber column in the compression chamber while compressing it into a cake.
13. An apparatus for producing a releasable buckled and crimped yarn cake, comprising: a member for ejecting fibers from a fine hole together with a high-velocity fluid; a buckling and crimping section provided at the tip of the fine hole; and a compression chamber provided at the tip of the buckling and crimping section, the compression chamber consisting of an inverted funnel-shaped section with its upper end circumscribing and a cylindrical section.
14. The apparatus for producing a releasable buckled crimped yarn cake according to claim 13, further comprising an axially movable compression member disposed downstream of said compression chamber.
15. An apparatus for producing a releasable buckled crimped yarn cake as claimed in claim 13, wherein said compression member is a vibrating compression member.
16. An apparatus for producing a releasable buckled crimped yarn cake as described in claim 13, wherein the member for ejecting the fibers from the pores together with the high-velocity fluid comprises a nozzle for spinning a fiber-forming fluid into a pressurized gas chamber, a pressurized gas chamber, and pores located opposite the nozzle.
17. The apparatus for producing a releasable buckled crimped yarn cake according to claim 13, wherein the member for ejecting the fibers from the fine holes together with the high-velocity fluid is a suction gun.
18. The apparatus for producing a releasable buckled crimped yarn cake according to claim 13, wherein said vibrating compression member is a piston inscribed in said compression chamber and gradually movable downstream.
19. The apparatus for producing a releasable buckled crimped yarn cake according to claim 13, wherein said tubular portion is provided with detachable connecting portions in series.
20. A releasable buckled-crimped yarn cake formed by compressing a fiber column of buckled-crimped yarn in a meandering stack.
21. The releasable buckled crimped yarn cake of claim 20, wherein said crimped yarn is polyester-based, polypropylene-based, polyamide-based, polyethylene-based, or a combination thereof.