Surface treatment member
A protective layer of SiO2 and Zn/Al carbonate-type layered double hydroxide on steel surfaces addresses the challenge of corrosion resistance in soil, effectively trapping anions and enhancing protection against chloride ions.
Patent Information
- Application Number
- KR1020267033789
- Authority / Receiving Office
- KR · KR
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-03-28
- Filing Date
- 2025-02-18
- Publication Date
- 2026-11-09
AI Technical Summary
Existing steel components buried in soil face challenges in maintaining corrosion resistance, particularly at depths of several centimeters from the soil surface, where conventional treatments are inadequate.
A protective layer composed of SiO2 and a zinc-containing compound, including Zn/Al carbonate-type layered double hydroxide, is applied to the steel surface to enhance corrosion resistance by trapping anions and providing sacrificial protection.
The surface treatment member exhibits excellent corrosion resistance even in the harsh environment of the soil surface layer, preventing chloride ions from penetrating and causing localized corrosion.
Smart Images

Figure PCT00024_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a surface treatment member. Background Technology
[0002] Steel is widely used as a material for various structures. After being processed into various shapes, steel is joined together as needed using fastening components such as screws, bolts, and rivets, or through joining processes using various welding methods, to become components with desired shapes (e.g., various steel structures).
[0003] It is believed that steel components (steel members) as described above are exposed to various environments depending on their application, leading to surface contamination or corrosion. For this reason, various studies have been conducted in the past regarding technologies to improve the antifouling and corrosion resistance of steel.
[0004] For example, the following patent document 1 discloses a technology for improving the antifouling properties (particularly, resistance to contamination by algae) of coated steel by providing a coating layer on the surface of various steel plates that includes a pyrithione compound, at least one of a silicate-based compound and its cured product, and a hydrotalcite, and does not contain a resin paint.
[0005] In addition, Patent Document 2 below discloses a repair method for improving the corrosion resistance of a steel structure, comprising: a surface conditioning process for obtaining a surface conditioning surface by performing a treatment to increase the surface exposure area ratio of the corroded steel structure surface to 30% or more; a corrosion inhibition process for applying a corrosion inhibitor containing hydrocalmite and / or hydrotalcite to the surface; a grinding process for grinding or polishing the surface to which the corrosion inhibitor has been applied; a paint application process for applying a zinc powder-containing paint to the surface after the grinding process; and a painting process for further applying a paint to the surface after applying the zinc powder-containing paint. Prior art literature
[0006] Japanese Patent Publication No. 2017-109417 and Japanese Patent Publication No. 2017-213557 The problem to be solved
[0007] Here, it is presumed that when various steel components are installed at desired locations, at least a portion of them are often buried in the soil. For parts of the steel components exposed to the atmosphere, it is easy to assess the corrosion status by visually inspecting the exposed areas. However, for parts buried in the soil, unlike those exposed to the atmosphere, it is difficult to visually inspect the corrosion status, and maintenance of corroded sections is also challenging. Therefore, high corrosion resistance is required for steel components used in soil.
[0008] The inventors examined the corrosion conditions of steel members in soil. As a result, as described below, they discovered that the corrosion behavior of steel members in soil with a depth of 1 m or more from the soil surface and the corrosion behavior of steel members in soil with a depth of several centimeters from the soil surface are significantly different. Subsequently, they found that in such soil with a depth of several centimeters from the soil surface, even if a steel member is manufactured by applying the technology disclosed in Patent Document 1 and Patent Document 2, there is room for improvement in its corrosion resistance.
[0009] Therefore, the present invention has been made in consideration of the above problem, and the objective of the present invention is to provide a surface-treated member made of steel that is capable of exhibiting excellent corrosion resistance even in soil at a depth of several centimeters from the soil surface. means of solving the problem
[0010] In order to solve the above problem, the inventors carefully examined the matter and devised a method to provide a protective layer with high barrier properties, mainly composed of SiO2, on the surface of a steel member used as a substrate to suppress corrosion in soil at a depth of several centimeters from the surface. On the other hand, since SiO2, which is the main component of the protective layer, is a hard material, there was a concern that micro-level fine defects might occur in the protective layer when the steel member with the protective layer is processed into a desired shape. If micro-level defects exist in the protective layer, corrosion agents (in particular, chloride ions (Cl)) can enter through these defects - Anions such as ) can reach the surface of the steel, potentially leading to localized corrosion.
[0011] Based on the above findings, the inventors conceived of providing a protective layer containing SiO2 and a zinc-containing compound containing a zinc element having sacrificial corrosion protection capabilities. Furthermore, as such a zinc-containing compound, they conceived of using a Zn / Al carbonate-type layered double hydroxide (i.e., Zn / Al hydrotalcite) which is a compound capable of trapping corrosion factors including anions, in a specific amount.
[0012] The gist of the present invention, completed based on these findings, is as follows.
[0013] (1) A surface treatment member comprising a steel material and a protective layer positioned on the surface of the steel material, wherein the protective layer has a Zn concentration of 1.00 mass% or more and less than 30.00 mass%, a Si concentration of 1.00 mass% or more and less than 25.00 mass%, and also contains SiO2 and a Zn / Al carbonate-type layered double hydroxide.
[0014] (2) A surface treatment member described in (1), wherein the thickness of the protective layer is 0.1㎛ or more and 50.0㎛ or less.
[0015] (3) A surface treatment member described in (1) or (2), wherein, in the measurement result of measuring the surface of the protective layer by X-ray diffraction (XRD), the peak intensity of the peak attributable to the Zn / Al carbonate-type layered double hydroxide is 1000 cps or more and 150000 cps or less.
[0016] (4) The protective layer has an Mg concentration of 0.10 mass% or more and 5.00 mass% or less, and further contains a Mg / Al carbonate-type layered double hydroxide, a surface treatment member as described in (1) or (2).
[0017] (5) A surface treatment member described in (4), wherein, in the measurement result of measuring the surface of the protective layer by X-ray diffraction (XRD), the peak intensity of the peak attributable to the Mg / Al carbonate-type layered double hydroxide is 1000 cps or more and 150000 cps or less.
[0018] (6)
[0019] A surface treatment member described in (1) or (2), wherein, in the measurement result obtained by measuring the surface of the protective layer by X-ray diffraction (XRD), the peak intensity of the peak attributed to SiO2 is 500 cps or more and 100,000 cps or less.
[0020] (7) A surface treatment member described in (1) or (2), wherein, when looking at the distribution of Si concentration in the thickness direction of the protective layer, the Si concentration at half thickness on the surface side of the protective layer is 1.3 times or more than the Si concentration at half thickness on the steel side of the protective layer.
[0021] (8) The protective layer is a surface treatment member described in (1) or (2) containing SiO2 particles having a particle size of 0.1 to 1.0 μm as the SiO2.
[0022] (9) A surface treatment member described in (1) or (2), further comprising a second protective layer positioned on the protective layer, wherein the second protective layer contains SiO2 particles having a particle size of 1.0 to 30.0 μm.
[0023] (10) The surface treatment member described in (9), wherein the thickness of the second protective layer is 1 μm or more and 100 μm or less.
[0024] (11) A surface treatment member described in (1) or (2), having a zinc-based plating layer between the steel and the protective layer.
[0025] (12) The zinc-based plating layer has an Al concentration of 0.10 mass% or more and less than 40.00 mass%, and also has a Zn concentration of 60.00 mass% or more, and is a surface treatment member as described in (11).
[0026] (13) The zinc-based plating layer has an Mg concentration of 0.10 mass% or more and less than 15.00 mass%, and is a surface treatment member as described in (12).
[0027] (14) A surface treatment member described in (11), wherein the thickness of the zinc-based plating layer is 1 μm or more and 200 μm or less. Effects of the invention
[0028] As described above, according to the present invention, a surface-treated member made of steel can be provided that exhibits excellent corrosion resistance even in soil at a depth of several centimeters from the soil surface. Brief explanation of the drawing
[0029] Figure 1 is a schematic diagram illustrating a structure installed on the surface of soil. FIG. 2 is a schematic diagram illustrating the structure of a surface treatment member according to an embodiment of the present invention. FIG. 3a is a schematic diagram illustrating an example of the structure of a surface treatment member according to the same embodiment. FIG. 3b is a schematic diagram illustrating an example of the structure of a surface treatment member according to the same embodiment. FIG. 4a is a schematic diagram illustrating another example of the structure of a surface-treated member according to the same embodiment. FIG. 4b is a schematic diagram illustrating another example of the structure of a surface-treated member according to the same embodiment. FIG. 5 is a schematic diagram for explaining the protective layer of a surface treatment member according to the same embodiment. Specific details for implementing the invention
[0030] Suitable embodiments of the present invention will be described in detail below with reference to the attached drawings. Additionally, components having substantially the same functional configuration in this specification and drawings are given the same reference numerals to avoid redundant descriptions.
[0031] (Humidity behavior in soil at a depth of several centimeters from the soil surface)
[0032] Before describing the surface treatment member according to an embodiment of the present invention, the corrosion behavior in soil at a depth of several centimeters from the soil surface, as discovered by the inventors, will be described with reference to FIG. 1. FIG. 1 is a schematic diagram for describing a structure installed on the soil surface. In addition, for convenience, "soil at a depth of several centimeters from the soil surface" may be referred to as the "soil surface layer" below.
[0033] As schematically illustrated in FIG. 1, various structures, such as a frame loaded with solar power generation panels, road signs, guardrails, and traffic signals, are installed on the soil surface. In order to install the structures more stably on the soil surface, a part of the structure (e.g., the area near the bottom of a support, enclosed by a dashed line in FIG. 1) is often buried in the soil, as shown in FIG. 1.
[0034] Various structures often utilize different types of steel as materials, for example, from the perspective of production costs. When parts of structures made of various steel are buried in the soil, there is a concern regarding the corrosion of the steel material.
[0035] Two effects of soil on the corrosion of steel can be identified: the retention of moisture, a corrosion factor, and the inhibition of oxygen diffusion, also a corrosion factor. The retention of moisture acts to increase the corrosion rate, while the inhibition of oxygen diffusion acts to decrease the corrosion rate. In soil, compared to the atmosphere, a humid environment (i.e., moisture) is maintained for a long time, such as after rainfall. On the other hand, because the infiltration and diffusion of oxygen from the atmosphere are inhibited by the soil, the corrosion rate decreases. The actual corrosion rate in soil is determined by the interaction of both of these two effects, which have a trade-off relationship as described above. Generally, since the effect of inhibiting oxygen diffusion is greater than the effect of retaining moisture, the corrosion rate in soil is inhibited compared to the atmosphere.
[0036] On the other hand, the situation is significantly different in soil at a depth of several centimeters from the surface (soil surface layer). Even in the soil surface layer, moisture is difficult to evaporate due to the soil, so the steel remains in contact with moisture for a longer period compared to the atmosphere. Meanwhile, in the soil surface layer, the distance from the atmosphere is short, and oxygen supply from the atmosphere is rapid, so the effect of inhibiting oxygen diffusion by the soil is small. Therefore, along with the effect of moisture retention, it is thought that almost no corrosion inhibition effect by the soil can be obtained in the soil surface layer. As such, the soil surface layer conceived by the inventors can be described as an extremely harsh corrosive environment compared to soil at a depth of 1 meter or more from the surface. Therefore, it can be said that extremely high corrosion resistance is required for steel installed in the soil surface layer.
[0037] In order to achieve such extremely high corrosion resistance, the inventors conceived of providing a protective layer with high barrier properties, primarily composed of SiO2, on the surface of the steel substrate. Meanwhile, since SiO2, which is the main component of the protective layer, is a hard material, there was concern that micro-level defects might occur in the protective layer when the steel substrate with the protective layer is processed into a desired shape. If micro-level defects exist in the protective layer, corrosion agents (in particular, chloride ions (Cl₂)) can penetrate through these defects. - Anions such as ) can reach the surface of the steel, potentially leading to localized corrosion.
[0038] Based on the findings above, the inventors conceived of providing a protective layer containing SiO2 and a zinc-containing compound comprising a zinc element having sacrificial corrosion protection. By further including a zinc-containing compound having sacrificial corrosion protection in a protective layer with high barrier properties containing SiO2, further improvement in corrosion resistance is realized, even if a corrosive agent reaches the protective layer.
[0039] Furthermore, the inventors have also conceived of using a specific amount of a Zn / Al carbonate-type layered double hydroxide (i.e., Zn / Al-type hydrotalcite), which is a compound capable of trapping corrosion agents including anions, as a zinc-containing compound as described above. As can be inferred from the description "layered," the carbonate-type layered double hydroxide is a compound having a so-called layered structure in which plate-like structures are stacked with predetermined spacing, and between the layers Cl - It can trap anions, including ions. Accordingly, in addition to the sacrificial protection ability exhibited by the zinc element, the carbonate-type layered double hydroxide itself can trap anions that are corrosion agents. As a result, even if a corrosion agent reaches the protective layer, it becomes possible to further prevent the corrosion agent from reaching the steel, thereby realizing further improvement in corrosion resistance.
[0040] Accordingly, even if a surface-treated member made of steel is installed in the surface layer of the soil, it is possible to improve the corrosion resistance of the steel.
[0041] Based on the findings described above, the inventors conducted further investigations and, as a result, produced a surface treatment member according to an embodiment of the present invention as described in detail below.
[0042] (Regarding surface-treated members)
[0043] Hereinafter, a surface treatment member according to an embodiment of the present invention will be described in detail with reference to FIGS. 2 to 4b. FIGS. 2 to 4b are schematic diagrams for explaining the structure of a surface treatment member according to the present embodiment. In addition, for convenience, FIGS. 2 to 4b will be described using the coordinate axes shown in the drawings.
[0044] The surface treatment member according to the present embodiment is constructed using various steel materials as the material, as described in detail below. Here, the specific structure of the surface treatment member according to the present embodiment is not particularly limited. The specific structure of the surface treatment member according to the present embodiment may be, for example, box-shaped, or plate-shaped using plate-shaped steel, such as the roof or wall of a building. Furthermore, the specific structure of the surface treatment member according to the present embodiment may be a molded body or a joined body using various structural steel, such as a solar power generation panel frame, for example, a molded body or a joined body using various H-shaped steel or prismatic steel, such as the framework of a structure, or a molded body or joined body using various steel pipes, such as various supports, signs, signal lights, guardrails, etc. Such a surface treatment member is used, for example, by burying at least a portion of the surface treatment member in the soil.
[0045] FIG. 2 schematically shows a portion of a surface-treated member (1) according to the present embodiment when viewed in a planar view from above the surface (in the Z-axis direction in the drawing). As schematically shown in FIG. 2, the surface-treated member (1) according to the present embodiment is made of a surface-treated steel material (10) in which a protective layer (13) containing a specific component is provided on the surface of the steel material (11) as described below.
[0046] FIGS. 3a to 4b schematically show a cross-section when the surface treatment member (1) shown in FIG. 2 is cut along the AA cutting line in the Z-axis direction. The cross-sectional view shown in FIGS. 3a to 4b corresponds to cutting the surface treatment member (1) according to the present embodiment in the thickness direction of the surface treatment steel material (10) that is the material of the surface treatment member (1).
[0047] As schematically illustrated in FIG. 3a, the surface treatment member (1) according to the present embodiment is composed of a steel material (11) as the base material and a surface treatment steel material (10) having a protective layer (13) located on the surface of the steel material (11). In addition, as schematically illustrated in FIG. 3b, the surface treatment steel material (10) may further have a zinc-based plating layer (15) between the steel material (11) and the protective layer (13).
[0048] Below, the steel material (11), protective layer (13), and zinc-based plating layer (15) are first described.
[0049] <Regarding steel (11)>
[0050] The steel material (11) used as the substrate for the surface-treated steel material (10) according to the present embodiment is not particularly limited, and various steel materials may be used depending on the mechanical strength (e.g., tensile strength) required for the surface-treated member (1). Examples of such steel materials (11) include various types of Al-killed steel, ultra-low carbon steel containing Ti, Nb, etc., high-strength steel containing reinforcing elements such as P, Si, Mn in addition to ultra-low carbon steel, and various steel materials containing other various components (Cr, N, Cu, B, Ni, Mg, Ca, V, Co, Zn, As, Y, Zr, Mo, Sn, Sb, Ta, W, Pb, Bi, REM, etc.).
[0051] In addition, as shown in FIG. 3b, a zinc-based plating layer (15) as described later may be placed on the surface of the steel material (11), but a pre-plating layer may be provided on the surface of the steel material (11) before performing zinc plating to form the zinc-based plating layer (15). Examples of metals that can be used for the pre-plating layer include Ni, Sn, or alloys combining these elements. If a pre-plated steel material is used in which these platings have been pre-plated in advance, unplated areas (areas where the plated metal bounces off due to an oxide film, etc.) can be eliminated. This is presumed to be because when the pre-plated steel material is immersed in a molten plating bath, the metal elements of the molten plating bath react with the pre-plating layer to form Ni(Sn)-Al-Fe-Zn. The adhesion amount of the pre-plating layer per side is 0.2 to 2.0 g / m² 2 It is desirable that it be within the range. The adhesion amount of the pre-plating layer is 0.2 g / m² 2 By doing so, it is possible to reliably achieve the effect of suppressing incomplete plating by the pre-plating as described above. In addition, the adhesion amount of the pre-plating layer is 2.0 g / m² 2By doing this, it is possible to achieve the above-mentioned anti-plating effect while preventing the dissolution of Fe by the pre-plating layer, thereby preventing the formation of Fe-Zn-based composite oxides.
[0052] In addition, the thickness of the steel (11) is not specifically limited and can be appropriately set according to the mechanical strength, etc. required for the surface treatment member (1).
[0053] <Regarding the protective layer (13)>
[0054] The protective layer (13) is a layer located on the surface of the steel material (11) (Fig. 3a) or on the surface of the zinc-based plating layer (15) (Fig. 3b), and has a Zn concentration of 5 mass% or more and less than 30 mass%, a Si concentration of 5 mass% or more and less than 25 mass%, and also contains SiO2 and Zn / Al-based carbonate-type layered double hydroxide. The surface treatment member (1) according to the present embodiment exhibits excellent corrosion resistance even when at least a portion is installed in the surface layer of the soil by having the protective layer (13) as described above.
[0055] The detailed composition of this protective layer (13) will be explained in detail below.
[0056] <Regarding the zinc-based plating layer (15)>
[0057] Between the steel material (11) and the protective layer (13) as described above, a zinc-based plating layer (15) may be positioned as shown in FIG. 3b. This zinc-based plating layer (15) is not particularly limited as long as it contains at least zinc (Zn), and various known zinc-based platings can be applied.
[0058] Examples of such zinc-based plating include zinc plating represented by, for instance, hot-dip galvanizing or alloyed hot-dip galvanizing, zinc-nickel plating, zinc-iron plating, zinc-chromium plating, zinc-aluminum plating, zinc-titanium plating, zinc-magnesium plating, zinc-manganese plating, zinc-aluminum-magnesium plating, and zinc-aluminum-magnesium-silicon plating. Additionally, as a zinc-based plating, it may be used that contains a small amount of dissimilar metal elements or impurities such as cobalt, molybdenum, tungsten, nickel, titanium, chromium, aluminum, manganese, iron, magnesium, lead, bismuth, antimony, tin, copper, cadmium, arsenic, etc., during the plating process, or that disperses inorganic materials such as silica, alumina, and titania. The plating method is not particularly limited, and various known plating methods such as electroplating, hot-dip plating, deposition plating, dispersion plating, and vacuum plating may be used.
[0059] Among the various zinc-based platings as described above, the zinc-based plating layer (15) according to the present embodiment is more preferably a zinc-based plating layer having a chemical composition as described below, for example. By using a zinc-based plating layer (15) having a chemical composition as described below, it becomes possible to further improve various properties, including corrosion resistance, of the surface treatment member (1) according to the present embodiment. Below, a more preferred chemical composition of the zinc-based plating layer (15) as described above will be explained in detail.
[0060] Regarding the chemical composition of the zinc-based plating layer (15)
[0061] The chemical composition of the zinc-based plating layer (15) according to the present embodiment has, in some aspects, a chemical composition in which Al: 0.10% or more and less than 40.00% by mass, and the remainder is composed of Zn and impurities of 60.00% or more by mass.
[0062] In addition, in the chemical composition of any embodiment of the zinc-based plating layer (15) according to the present embodiment, it is more preferable that the chemical composition of the zinc-based plating layer (15) further contains Mg: 0.10% or more and less than 15.00% in place of some of the remainder of Zn.
[0063] In addition, according to another embodiment, the chemical composition of the zinc-based plating layer (15) according to the present embodiment contains, in mass%, Al: 0.10% or more and less than 40.00% and Mg: 0.10% or more and less than 15.00%, and further contains one or more types selected from the group consisting of the following element group A, element group B, element group C, element group D, element group E and element group F, and the remainder consists of Zn and impurities.
[0064] [Element Group A]: One or two types selected from the group consisting of Si: 2.50% or less and Fe: 5.00% or less
[0065] [Element Group B]: One or more selected from the group consisting of Sb: less than 0.50%, Pb: less than 0.50%, and Sr: less than 0.50%.
[0066] [Element Group C]: One or more selected from the group consisting of Cu: less than 0.25%, Ti: less than 0.25%, Cr: less than 0.25%, Nb: less than 0.25%, Ni: less than 0.25%, Mn: less than 0.25%, Co: less than 0.25%, and V: less than 0.25%.
[0067] [Element Group D]: One or more elements selected from the group consisting of Sn: 2.00% or less, Bi: less than 0.50%, and In: less than 2.00%.
[0068] [Element Group E]: One or more selected from the group consisting of Ca: 3.00% or less, La: less than 0.50%, Ce: less than 0.50%, and Y: 0.50% or less.
[0069] [Element Group F]: B: Less than 0.50%
[0070] [Al: 0.10 mass% or more, less than 40.00 mass%]
[0071] Al is an element necessary to form the main metal structure (Zn-Al metal structure) in a preferred embodiment of the zinc-based plating layer (15) according to the present embodiment. Therefore, it is desirable that Al be contained in an amount greater than a predetermined amount to ensure corrosion resistance as a plated steel. If the Al content in the zinc-based plating layer (15) is less than 0.10 mass%, there is a possibility that such corrosion resistance cannot be guaranteed. Therefore, in the zinc-based plating layer (15) according to the present embodiment, it is desirable that the Al content be 0.10 mass% or more. The Al content is preferably 3.00 mass% or more, more preferably 4.00 mass% or more, and even more preferably 6.00 mass% or more. By having the Al content within the above range, it becomes possible to ensure corrosion resistance as a plated steel.
[0072] Meanwhile, if the Al content of the zinc-based plating layer (15) is 40.00 mass% or more, the Al phase that functions as a cathode when placed in a corrosive environment increases excessively, making it easier for the steel (11) to corrode, and thus there is a possibility that the corrosion resistance of the plated steel cannot be guaranteed. Therefore, in the zinc-based plating layer (15) according to the present embodiment, it is preferable that the Al content be less than 40.00 mass%. The Al content is preferably 25.00 mass% or less, more preferably less than 25.00 mass%, and even more preferably 20.00 mass% or less.
[0073] In the zinc-based plating layer (15) according to the present embodiment, the remainder of the Al is Zn and impurities.
[0074] Zn is an element necessary to form the main metal structure (Zn-Al metal structure) in a preferred embodiment of the zinc-based plating layer (15) according to the present embodiment, and is an important element for improving corrosion resistance as a plated steel. In addition, by the zinc-based plating layer (15) containing the above Al within the above range and further containing Zn, it becomes possible to secure the corrosion resistance required for plated steel.
[0075] [Mg: 0.10 mass% or more, less than 15.00 mass%]
[0076] Mg is an important element for forming the main metal structure (Zn-Al-Mg metal structure) in a more preferred embodiment of the zinc-based plating layer (15) according to the present embodiment. Therefore, it is more preferable that Mg be contained in an amount greater than a predetermined amount to ensure corrosion resistance as a plated steel. If the Mg content of the zinc-based plating layer (15) is less than 0.10 mass%, there is a possibility that such corrosion resistance cannot be guaranteed. Therefore, in the zinc-based plating layer (15) according to the present embodiment, it is preferable that the Mg content be 0.10 mass% or more. The Mg content is preferably 0.30 mass% or more, and more preferably 3.00 mass% or more. By having the Mg content within the above range, it becomes possible to ensure corrosion resistance as a plated steel.
[0077] Meanwhile, if the Mg content of the zinc-based plating layer (15) is 15.00 mass% or more, the anode dissolution of the zinc-based plating layer is likely to proceed when placed in a corrosive environment, so there is a possibility that corrosion resistance as a plated steel material cannot be guaranteed. Therefore, in the zinc-based plating layer (15) according to the present embodiment, it is preferable that the Mg content be less than 15.00 mass%. The Mg content is preferably less than 12.50 mass%, and more preferably 12.00 mass% or less. By having the Mg content within the above range, it becomes possible to guarantee corrosion resistance as a plated steel material.
[0078] Next, regarding a preferred response to a zinc-based plating layer (15) according to another aspect of the present embodiment, the element groups A to F that the chemical composition of such zinc-based plating layer (15) may have will be described in detail.
[0079] In addition, in the zinc-based plating layer (15) according to another aspect of the present embodiment, when at least one of the elements belonging to the following element groups A to F is included, it is preferable to include at least one of the elements belonging to the following element groups A to F within the range of the following content and with a total content of 60.00 mass% or less.
[0080] By making the total content of elements belonging to element groups A to F 60.00 mass% or less, it becomes possible to enjoy the effects exhibited by the addition of each element, as described in detail below, without damaging each other. The total content of elements belonging to element groups A to F is preferably 50.00 mass% or less, and more preferably 40.00 mass% or less.
[0081] ◇ Elemental Group A
[0082] In another aspect of the zinc-based plating layer (15) according to the present embodiment, a group of elements A that the zinc-based plating layer (15) may contain is described. At least one of the elements in the group of elements A shown below is an element that may be contained in the zinc-based plating layer (15) in place of a portion of the remainder of Zn.
[0083] [Element Group A]: One or two types selected from the group consisting of Si: 2.50% or less and Fe: 5.00% or less
[0084] [Si: 0 to 2.50 mass%]
[0085] In other aspects of the zinc-based plating layer (15) according to the present embodiment, since it is conceivable that it does not contain Si, the lower limit of the content is 0 mass%. Meanwhile, Si is an element that can further improve the adhesion between the zinc-based plating layer (15) and the steel (11) by suppressing the excessive growth of the Fe-Al metal structure formed at the interface between the zinc-based plating layer (15) and the steel (11). When Si is included in the zinc-based plating layer (15), in order to suppress the excessive growth of the Fe-Al metal structure, the Si content is preferably 0.05 mass% or more, and more preferably 0.20 mass% or more. On the other hand, if the Si content exceeds 2.50 mass%, it may form an excessive amount of Mg and high-melting-point intermetallic compounds, thereby potentially hindering the formation of Al-Mg oxides that have the effect of suppressing Zn evaporation during welding.
[0086] In addition, if the Si content in the plating bath for manufacturing the zinc-based plating layer (15) is excessively high, the viscosity of the plating bath increases more than necessary, and there is a possibility that the operability during the manufacture of the plated steel (hereinafter referred to as "plating operability") may decrease. Therefore, the Si content in the plating bath is adjusted from the perspective of plating operability. The Si content in the zinc-based plating layer (15) is preferably 1.50 mass% or less, and more preferably 1.00 mass% or less.
[0087] [Fe: 0 to 5.00 mass%]
[0088] In the zinc-based plating layer (15), elements constituting the steel material from the base steel material (11) may be incorporated. In particular, in the molten plating method, elements constituting the steel material (11) are easily incorporated into the zinc-based plating layer (15) due to mutual diffusion of elements caused by the solid-liquid reaction between the steel material (11) and the zinc-based plating layer (15). Due to this incorporation of elements, a predetermined amount of Fe is often contained in the zinc-based plating layer (15), and the content is often 0.01 mass% or more. When the above mutual diffusion is promoted, the adhesion between the steel material (11) and the zinc-based plating layer (15) is improved. From the perspective of improving the adhesion between the steel material (11) and the zinc-based plating layer (15), it is preferable that the Fe content in the zinc-based plating layer (15) be 0.20 mass% or more.
[0089] In addition, Fe may be intentionally added to the plating bath used when manufacturing the zinc-based plating layer (15) within a range that does not impair the effects of the present invention. However, if the Fe content in the plating bath increases, high-melting-point intermetallic compounds of Fe and Al are formed in the plating bath. In this case, it is undesirable because these high-melting-point intermetallic compounds tend to adhere to the zinc-based plating layer (15) as dross, significantly lowering the appearance quality. In this regard, the Fe content in the plating bath is adjusted. It is preferable that the Fe content in the zinc-based plating layer (15) be 5.00 mass% or less. More preferably, the Fe content in the zinc-based plating layer (15) is 3.00 mass% or less, and even more preferably 2.00 mass% or less, 1.00 mass% or less, or 0.50 mass% or less.
[0090] ◇ Element Group B
[0091] In another aspect of the zinc-based plating layer (15) according to the present embodiment, a group of elements B that the zinc-based plating layer (15) may contain is described. At least one of the elements in the group of elements B described below is an element that may be contained in the zinc-based plating layer (15) in place of a portion of the remainder of Zn.
[0092] [Element Group B]: One or more selected from the group consisting of Sb: less than 0.50%, Pb: less than 0.50%, and Sr: less than 0.50%.
[0093] [Sb: 0 to 0.50 mass%]
[0094] [Pb: 0 to 0.50 mass%]
[0095] [Sr: 0 to 0.50 mass%]
[0096] In other aspects of the zinc-based plating layer (15) according to the present embodiment, since it is conceivable that it does not contain Sb, Pb, or Sr, the lower limit of the content of these elements is 0 mass%. Meanwhile, if at least one of Sb, Pb, or Sr is contained in the zinc-based plating layer (15), spangles are formed on the surface of the zinc-based plating layer (13), making it possible to improve the metallic luster. Therefore, from the perspective of further improving the decorative properties of the plated steel, it is preferable that at least one of Sb, Pb, or Sr be contained in the zinc-based plating layer (15). This effect of improving decorative properties is manifested when the content of at least one of Sb, Pb, or Sr is 0.05 mass% or more. Therefore, when at least one of Sb, Pb, or Sr is contained in the zinc-based plating layer (15), it is preferable that the content of each of these elements be independently 0.05 mass% or more.
[0097] Meanwhile, if a zinc-based plating layer (15) is formed in which any of the contents of Sb, Pb, and Sr exceeds 0.50 mass%, the amount of dross generated in the plating bath used to form the zinc-based plating layer (15) increases, and there is a possibility that a plated steel material with good plating properties cannot be manufactured. Therefore, it is preferable that the contents of Sb, Pb, and Sr in the zinc-based plating layer (15) are each independently 0.50 mass% or less. The contents of Sb, Pb, and Sr are each independently, preferably 0.20 mass% or less.
[0098] ◇ Elemental Group C
[0099] In another aspect of the zinc-based plating layer (15) according to the present embodiment, the group of elements C that the zinc-based plating layer (15) may contain is described. At least one of the elements in the group of elements C shown below is an element that may be contained in the zinc-based plating layer (15) in place of a portion of the remainder of Zn.
[0100] [Element Group C]: One or more selected from the group consisting of Cu: less than 0.25%, Ti: less than 0.25%, Cr: less than 0.25%, Nb: less than 0.25%, Ni: less than 0.25%, Mn: less than 0.25%, Co: less than 0.25%, and V: less than 0.25%.
[0101] [Cu: 0 mass% or more, less than 0.25 mass%]
[0102] [Ti: 0 mass% or more, less than 0.25 mass%]
[0103] [Cr: 0 mass% or more, less than 0.25 mass%]
[0104] [Nb: 0 mass% or more, less than 0.25 mass%]
[0105] [Ni: 0 mass% or more, less than 0.25 mass%]
[0106] [Mn: 0 mass% or more, less than 0.25 mass%]
[0107] [Co: 0 mass% or more, less than 0.25 mass%]
[0108] [V: 0 mass% or more, less than 0.25 mass%]
[0109] In other aspects of the zinc-based plating layer (15) according to the present embodiment, since it is conceivable that it does not contain Cu, Ti, Cr, Nb, Ni, Mn, Co, and V, the lower limit of the content of these elements is 0 mass%. Meanwhile, if at least one of Cu, Ti, Cr, Nb, Ni, Mn, Co, and V is contained in the zinc-based plating layer (15), when the plated steel is welded, these elements are introduced into the Fe-Al metal structure created by welding, making it possible to further improve the corrosion resistance of the formed weldment. This effect of improving the corrosion resistance of the weldment is manifested when the content of at least one of Cu, Ti, Cr, Nb, Ni, Mn, Co, and V in the zinc-based plating layer (13) becomes 0.05 mass% or more. Therefore, when at least one of Cu, Ti, Cr, Nb, Ni, Mn, Co, and V is included in the zinc-based plating layer (15), it is preferable that the content of each of these elements be at least 0.05 mass% independently.
[0110] Meanwhile, when forming a zinc-based plating layer (15) in which any of the contents of Cu, Ti, Cr, Nb, Ni, Mn, Co, and V is 0.25 mass% or more, these elements may form various intermetallic compounds in the plating bath for forming the zinc-based plating layer (15), causing an increase in the viscosity of the plating bath, and thus making it impossible to manufacture a plated steel material with good plating properties. Therefore, it is preferable that the contents of Cu, Ti, Cr, Nb, Ni, Mn, Co, and V in the zinc-based plating layer (15) be each independently less than 0.25 mass%. The contents of Cu, Ti, Cr, Nb, Ni, Mn, Co, and V are each independently, preferably 0.20 mass% or less.
[0111] ◇ Elemental Group D
[0112] In another aspect of the zinc-based plating layer (15) according to the present embodiment, the group of elements D that the zinc-based plating layer (13) may contain is described. At least one of the elements in the group of elements D shown below is an element that may be contained in the zinc-based plating layer (13) in place of a portion of the remaining Zn.
[0113] [Element Group D]: One or more elements selected from the group consisting of Sn: 20.00% or less, Bi: less than 5.00%, and In: less than 2.00%.
[0114] [Sn: 0 mass% or more 2.00 mass%]
[0115] [Bi: 0 mass% or more, less than 0.50 mass%]
[0116] [In: 0 mass% or more, less than 2.00 mass%]
[0117] In other embodiments of the zinc-based plating layer (15) according to the present embodiment, since it is conceivable that it does not contain Sn, Bi, or In, the lower limit of the content of these elements is 0 mass%. Meanwhile, Sn, Bi, and In form intermetallic compounds with Mg in the zinc-based plating layer (15), thereby making it possible to improve the weldability of the zinc-based plating layer (13). Furthermore, since all of these intermetallic compounds have high melting points, when the plated steel is welded, they do not evaporate after welding and remain as intermetallic compounds. The presence of these elements makes it possible to improve corrosion resistance and corrosion resistance, and also makes it possible to improve the corrosion resistance of the welded part during welding. This effect of improving corrosion resistance is manifested when the content of at least one of Sn, Bi, and In in the zinc-based plating layer (15) is 0.05 mass% or more. Therefore, when at least one of Sn, Bi, and In is included in the zinc-based plating layer (15), it is preferable that the content of each of these elements be independently 0.05 mass% or more.
[0118] Meanwhile, excessive addition of Sn may increase the amount of intermetallic compounds formed, potentially lowering the corrosion resistance of the zinc-based plating layer (15) after welding. In addition, excessive addition of Bi and In may embrittle the zinc-based plating layer (15), making it prone to peeling, and may also lower the corrosion resistance of the zinc-based plating layer (15) after welding. These phenomena become pronounced when the Sn content exceeds 2.00 mass%, when the Bi content is 0.50 mass% or more, or when the In content is 2.00 mass% or more. Therefore, it is preferable that the Sn content be 2.00 mass% or less, the Bi content be less than 0.50 mass%, and the In content be less than 2.00 mass%. It is more preferable that the Sn content be 1.00 mass% or less, the Bi content be 0.30 mass% or less, and the In content be 1.00 mass% or less.
[0119] ◇ Elemental Group E
[0120] In another aspect of the zinc-based plating layer (15) according to the present embodiment, the group of elements E that the zinc-based plating layer (15) may contain is described. At least one of the elements in the group of elements E shown below is an element that may be contained in the zinc-based plating layer (15) in place of a portion of the remainder of Zn.
[0121] [Element Group E]: One or more selected from the group consisting of Ca: 3.00% or less, La: less than 0.50%, Ce: less than 0.50%, and Y: 0.50% or less.
[0122] [Ca: 0 to 3.00 mass%]
[0123] In other embodiments of the zinc-based plating layer (15) according to the present embodiment, since it is possible to conceive of a case in which it does not contain Ca, the lower limit of the content is 0 mass%. Meanwhile, if Ca is contained in the plating bath for manufacturing the zinc-based plating layer (15), the dross generated along with an increase in Mg concentration during plating operation can be reduced, thereby improving plating operability.
[0124] In addition, when Ca is contained in the zinc-based plating layer (15), it forms intermetallic compounds with Al and Zn. Also, when Si is contained along with Ca in the zinc-based plating layer (15), Ca forms intermetallic compounds with Si. Since these intermetallic compounds have a high melting point and a stable structure, it becomes possible to suppress Liquid Metal Embrittlement (LME) when the plated steel is welded. When Ca is contained in the zinc-based plating layer (15), the effect of improving plating operability and the effect of suppressing LME during welding are manifested by making the Ca content 0.01 mass% or more. More preferably, the Ca content in the zinc-based plating layer (15) is 0.05 mass% or more.
[0125] Meanwhile, if the Ca content in the zinc-based plating layer (15) exceeds 3.00 mass%, there is a possibility that the corrosion resistance of the plated steel may decrease. In this regard, it is preferable that the Ca content in the zinc-based plating layer (15) be 3.00 mass% or less. The Ca content in the zinc-based plating layer (15) is preferably 2.00 mass% or less, and more preferably 1.00 mass% or less.
[0126] [La: 0 mass% or more, less than 0.50 mass%]
[0127] [Ce: 0 mass% or more, less than 0.50 mass%]
[0128] [Y: 0 mass% or more, 0.50 mass% or less]
[0129] In other aspects of the zinc-based plating layer (15) according to the present embodiment, since it is conceivable that it does not contain La, Ce, and Y, the lower limit of the content of these elements is 0 mass%. Meanwhile, La, Ce, and Y are elements that exhibit an effect almost equivalent to that of Ca. This is due to the fact that the atomic radius of each element is close to the atomic radius of Ca, and when these elements are contained in the zinc-based plating layer (15), they substitute for the Ca position.
[0130] These effects of improving plating workability and suppressing LME during welding are achieved by making the content of each of these elements independently 0.01 mass% or more. Therefore, when at least one of La, Ce, and Y is included, it is preferable that the content of each of these elements independently be 0.01 mass% or more. The content of La, Ce, and Y in the zinc-based plating layer (15) is independently, more preferably 0.05 mass% or more.
[0131] Meanwhile, if the content of La, Ce, and Y in the plating bath for manufacturing the zinc-based plating layer (15) is excessively high, the viscosity of the plating bath may increase more than necessary, potentially leading to a decrease in plating operability. Therefore, the content of La, Ce, and Y in the plating bath is adjusted from the perspective of plating operability. It is preferable that the content of La, Ce, and Y be independently less than 0.50 mass%, less than 0.50 mass%, and 0.50 mass% or less, respectively. The content of La, Ce, and Y is independently, preferably 0.10 mass% or less.
[0132] ◇ Element group F
[0133] In another aspect of the zinc-based plating layer (15) according to the present embodiment, the group of elements F that the zinc-based plating layer (15) may contain is described. The elements of the group of elements F shown below are elements that may be contained in the zinc-based plating layer (13) in place of a portion of the remaining Zn.
[0134] [Element Group F]: B: Less than 0.50%
[0135] [B: 0 mass% or more and less than 0.50 mass%]
[0136] In other embodiments of the zinc-based plating layer (15) according to the present embodiment, since a case in which B is not contained can be conceived, the lower limit of the content is 0 mass%. Meanwhile, when B is contained in the zinc-based plating layer (15), it has the effect of further suppressing LME. This is presumed to be because when B is contained in the zinc-based plating layer (15), it combines with any of Zn, Al, Mg, and Ca to form various intermetallic compounds. Furthermore, it is thought that because B is present in the zinc-based plating layer (13), B diffuses from the zinc-based plating layer (15) to the steel (11), and through grain boundary strengthening, has the effect of further suppressing LME of the steel (11). In addition, since the various intermetallic compounds formed with respect to B have extremely high melting points, it is presumed to also act to suppress Zn evaporation during welding. These improvement effects are manifested by containing B at a rate of 0.05 mass% or more. Therefore, when B is included, it is desirable that the content of B be 0.05 mass% or more.
[0137] Meanwhile, in order to include B in the zinc-based plating layer (15), if B is included in excess in the plating bath, it causes a rapid increase in the plating melting point, which lowers plating workability and may result in the inability to manufacture a plated steel with excellent plating properties. Since this lowering of plating workability becomes significant when the B content is 0.50 mass% or more, it is preferable that the B content be less than 0.50 mass%. More preferably, the B content is 0.10 mass% or less.
[0138] [Method for Measuring Chemical Components]
[0139] The chemical composition of the above zinc-based plating layer (15) can be measured using ICP-AES (Inductively Coupled Plasma Atomic Emission Spectrometry) or ICP-MS (Inductively Coupled Plasma Mass Spectrometry). Additionally, ICP-AES is used when analyzing chemical composition down to 0.1 mass%, and ICP-MS is used when analyzing trace amounts of chemical composition less than 0.1 mass%. A plated steel material is immersed in a 10% HCl aqueous solution containing an inhibitor for about 1 minute to peel off the zinc-based plating layer portion, and a solution is prepared in which the zinc-based plating layer is dissolved. The obtained solution is analyzed using ICP-AES or ICP-MS to obtain the chemical composition as the overall average of the zinc-based plating layer.
[0140] Regarding the thickness of the zinc-based plating layer (15)
[0141] The thickness of the zinc-based plating layer (15) as described above (thickness d in FIG. 3b) p The thickness of the zinc-based plating layer (15) is preferably, for example, 1 μm or more, and more preferably 3 μm or more. In addition, the thickness of the zinc-based plating layer (15) is preferably, for example, 200 μm or less, and more preferably 50 μm or less. By making the thickness of the zinc-based plating layer (15) within the above range, the surface treatment member (1) according to the present embodiment can exhibit sufficient corrosion resistance.
[0142] In addition, the thickness of the zinc-based plating layer (15) can be measured by direct observation from the cross-section. Specifically, a cross-sectional sample containing the zinc-based plating layer (15) is obtained by cutting at any location of the surface treatment member (1) in the thickness direction of the surface treatment member (1). Then, the obtained cross-sectional sample is embedded in a room-temperature drying epoxy resin so that the cross-section can be observed, and after mechanically polishing the embedded surface, it is observed with an SEM. In this SEM observation, a person skilled in the art can easily distinguish the steel (11), the zinc-based plating layer (15), and the protective layer (13) from the appearance. The thickness of the zinc-based plating layer (15) is measured at any five locations, and the average value of the thicknesses obtained at the five points is taken as the thickness of the zinc-based plating layer (15).
[0143] <Regarding the second protective layer (17)>
[0144] FIGS. 4a and 4b schematically illustrate another example of the structure of a surface treatment member (1) according to the present embodiment. As schematically illustrated in FIGS. 4a and 4b, the surface treatment member (1) according to the present embodiment may further have a second protective layer (17) on top of the protective layer (13).
[0145] In addition, the detailed composition of this second protective layer (17) will be explained in detail below.
[0146] <Detailed composition of the protective layer (13)>
[0147] Next, the detailed configuration of the protective layer (13) of the surface treatment member (1) according to the present embodiment will be described.
[0148] As previously mentioned, the protective layer (13) according to the present embodiment has a Zn concentration of 1 mass% or more and less than 30 mass%, a Si concentration of 1 mass% or more and less than 25 mass%, and also contains SiO2 and a Zn / Al carbonate-type layered double hydroxide.
[0149] 《SiO2》
[0150] As mentioned above, the protective layer (13) according to the present embodiment contains SiO2, thereby exhibiting excellent barrier properties due to SiO2, and it is possible to improve the corrosion resistance of the surface treatment member (1) according to the present embodiment.
[0151] Such SiO2 is not specifically limited, and various known SiO2s can be used. Examples of such SiO2s include silica sand, colloidal silica, fumed silica, water-dispersible silica, precipitated silica, silica gel, etc.
[0152] Here, whether the protective layer (13) of the surface treatment member (1) contains SiO2 can be determined by measuring the surface of the protective layer (13) by X-ray diffraction (XRD) and whether a peak attributable to SiO2 exists in the obtained measurement result.
[0153] Here, a peak attributed to SiO2 can be cited, for example, as the peak observed at 2θ = 26.65 ± 0.50. Here, XRD measurements can be performed, for example, by the following method.
[0154] ◇ Method for measuring the XRD pattern of the protective layer (13)
[0155] First, a sample is cut from a surface-treated member (1) having a protective layer (13). The dimensions of this sample are, for example, 20 mm × 20 mm when viewed from a direction perpendicular to the surface of the surface-treated member (1). Next, the XRD pattern of the sample is measured using an X-ray diffraction device (for example, RINT-TTR III manufactured by Rigaku Co., Ltd.). Examples of the conditions for measuring the XRD pattern at this time are given below.
[0156] XRD pattern measurement conditions:
[0157] X-ray output: 50kV, 300mA
[0158] X-ray tube: Cu
[0159] Measurement range: Start angle 5°, End angle 100°
[0160] Scan speed: 2deg / min
[0161] Step width: 0.01deg
[0162] Scan Axis: 2Theta / Theta
[0163] Solar slit: 5°
[0164] Diverging slit: 1 / 2°
[0165] Divergence vertical limit slit: 10mm
[0166] Scattering slit: Open (Full open)
[0167] Light receiving slit: Open (fully open)
[0168] Goniometer radius: 285mm
[0169] Detector: 1D detector D / tex Ultra-HE, monochromator installed in front of the detector
[0170] For the measurement result data obtained under the above measurement conditions, the background can be removed using an application such as PDXL2 manufactured by Rigaku Co., Ltd. (e.g., PDXL2) mounted on an X-ray diffraction device, and then the peak attributed to SiO2 can be identified.
[0171] In addition, in the protective layer (13) according to the present embodiment, it is preferable that the peak intensity of the peak attributed to SiO2, measured as described above, is 500 cps or more and 100,000 cps or less. Since the peak intensity is within the above range, it can be determined that the protective layer (13) contains a sufficient amount of SiO2 to exert a barrier effect against corrosion factors. More preferably, the peak intensity of the peak attributed to SiO2 is 1,000 cps or more.
[0172] In addition, the protective layer (13) according to the present embodiment preferably contains SiO2 particles having a particle size of 0.10 to 1.00 μm as the SiO2. In addition, the average particle size of the SiO2 particles is preferably 0.10 to 1.00 μm. Here, the SiO2 particles according to the present embodiment are particles comprising element Si and element O, wherein the sum of the mass% of Si and the mass% of O is 95 mass% or more, and (the number of moles of Si / the sum of the number of moles of Si and the number of moles of O) is 0.25 or more and 0.50 or less. By containing SiO2 particles having such an average particle size, the density of the protective layer (13) can be improved, and consequently, the barrier properties of the protective layer (13) can be further improved. The average particle size of the SiO2 particles is preferably 0.50 μm or less.
[0173] The proportion of SiO2 particles having the above-mentioned particle size (0.10 to 1.00 μm) among the total SiO2 particles is preferably 70 to 100% of the total number of SiO2 particles contained in the protective layer (13) according to the present embodiment. By containing SiO2 particles having the above-mentioned particle size in the above amount, the density of the protective layer (13) and furthermore the barrier properties of the protective layer (13) can be further improved. The proportion of SiO2 particles having the above-mentioned particle size is more preferably 80% or more of the total number of SiO2 particles contained in the protective layer (13).
[0174] Here, the particle size of the SiO2 particles as described above, and the proportion of SiO2 particles having the particle size as described above (0.10 to 1.00 μm) that account for the total of the SiO2 particles, can be measured by direct observation from a cross-section. In addition, in this embodiment, the particle size of the SiO2 particles determined by such cross-sectional observation is defined as the particle size of the SiO2 particles in the protective layer (13).
[0175] The method for measuring the particle size of SiO2 particles is specifically as follows.
[0176] First, an arbitrary location of the surface treatment member (1) of interest is cut in the thickness direction of the surface treatment member (1) (i.e., a direction perpendicular to the surface of the surface treatment member (1)) to obtain a cross-sectional sample of the protective layer (13). Then, the obtained cross-sectional sample is embedded in a room-temperature drying epoxy resin so that the cross-section can be observed, and after the embedded surface is mechanically polished, it is observed with an SEM. In addition, in this embodiment, particles with a measured particle size of 0.05 μm or more are defined as "SiO2 particles." Particles with a particle size of less than 0.05 μm are not treated as "SiO2 particles" in this embodiment because only the ends of the SiO2 particles are observed, or the particles themselves are too fine and have little influence on the barrier effect of the protective layer (13).
[0177] In addition, the field of view during SEM observation is set to 200 µm × 300 µm. In any 5 fields of view, the particle size and number of "all SiO2 particles with a particle size of 0.05 µm or more" present in the field of view are measured. Among them, the number of SiO2 particles with a particle size of 0.10 to 1.00 µm is calculated. By doing so, the "number of SiO2 particles with a particle size of 0.10 to 1.00 µm" / "number of SiO2 particles with a particle size of 0.05 µm or more" can be calculated.
[0178] In addition, the average particle size of SiO2 particles can be calculated by calculating the average value of the particle sizes of all SiO2 particles with a particle size of 0.05 μm or more present in the field of view (sum of the particle sizes of all particles / number of all particles).
[0179] Furthermore, a person skilled in the art can easily recognize SiO2 particles in the cross-sectional observation described above. In addition, even if the surface-treated member is already buried in the soil, it is possible to perform the cross-sectional observation described above by collecting a measurement sample from the buried surface-treated member.
[0180] Zn / Al-based layered carbonate double hydroxide
[0181] As previously mentioned, the protective layer (13) according to the present embodiment contains a Zn / Al carbonate-type layered double hydroxide, thereby trapping anions as corrosion agents that have penetrated into the protective layer (13). By doing so, it is possible to improve the corrosion resistance of the surface-treated member (1) according to the present embodiment.
[0182] Zn / Al layered double hydroxide (hydrotalcite) is a compound having the general formula as shown in (1) below.
[0183] [Zn 1-X Al X( OH)2] X+ [A n- X / n ·mH2O] X- … (1)
[0184] Here, A in the above general formula (1) n- is OH - , F - , Cl - , Br - , NO 2- , CO3 2- , SO4 2- , Fe(CN)3 3- , CH3COO - ...represents n-valent anions such as oxalate ions, salicylate ions, etc. Additionally, X represents a value greater than 0 and less than or equal to 0.33. Among these Zn / Al layered double hydroxides, A n- As carbonate ions (CO3 2- A Zn / Al carbonate-type layered double hydroxide having ) is a Zn / Al-based carbonate-type layered double hydroxide.
[0185] Among the Zn / Al-based carbonate-type layered double hydroxides mentioned above, zinc-aluminum-hydroxide-carbonate-hydrate (Zn6Al2(OH)2), which is a particularly stable material 16 It is more desirable to use CO3·4H2O.
[0186] Mg / Al-based layered double hydroxide of the carbonate type
[0187] The protective layer (13) according to the present embodiment preferably contains Mg / Al carbonate layered double hydroxide in addition to the above SiO2 and Zn / Al carbonate layered double hydroxide. Mg / Al carbonate layered double hydroxide is a compound having a layered structure similar to Zn / Al carbonate layered double hydroxide and can trap anions between the layers. Here, since the interlayer length of Mg / Al carbonate layered double hydroxide is different from that of Zn / Al carbonate layered double hydroxide, it can trap a different type of corrosion factor than Zn / Al carbonate layered double hydroxide. Therefore, by the protective layer (13) according to the present embodiment further containing Mg / Al carbonate layered double hydroxide in addition to Zn / Al carbonate layered double hydroxide, it becomes possible to further improve the corrosion resistance of the surface treatment member (1).
[0188] Zn / Al layered double hydroxides (hydrotalcites) are compounds having the general formula as shown in (2) below.
[0189] [Mg 1-X Al X (OH)2] X+ [A n- X / n ·mH2O] X- … (1)
[0190] Here, A in the above general formula (1) n- is OH - , F - , Cl - , Br - , NO 2- , CO3 2- , SO4 2- , Fe(CN)3 3- , CH3COO - ...represents n-valent anions such as oxalate ions, salicylate ions, etc. Additionally, X represents a value greater than 0 and less than or equal to 0.33. Among these Mg / Al-based layered double hydroxides, A n- As carbonate ions (CO32- A layered double hydroxide of the carbonate type having ) is a Mg / Al-based carbonate type.
[0191] Among the Mg / Al-based carbonate-type layered double hydroxides mentioned above, magnesium aluminum hydroxide carbonate hydrate (Mg6Al2(OH)2), which is a particularly stable material 16 It is more desirable to use CO3·4H2O.
[0192] Method for Identifying Layered Double Hydroxides of the Carbonate Type
[0193] Here, whether the protective layer (13) of the surface treatment member (1) contains Zn / Al carbonate-type layered double hydroxide or Mg / Al carbonate-type layered double hydroxide as described above can be determined by measuring the surface of the protective layer (13) by XRD and determining whether there is a peak attributable to Zn / Al carbonate-type layered double hydroxide or a peak attributable to Mg / Al carbonate-type layered double hydroxide in the measurement result obtained.
[0194] Here, for example, the peak observed at 2θ = 11.64 ± 0.50 can be cited as a peak attributed to the Zn / Al carbonate-type layered double hydroxide. Also, for example, the peak observed at 2θ = 11.71 ± 0.50 can be cited as a peak attributed to the Mg / Al carbonate-type layered double hydroxide. Here, since the XRD measurement conditions are the same as above, a detailed explanation is omitted below.
[0195] In addition, in the protective layer (13) according to the present embodiment, it is preferable that the peak intensity of the peak attributed to the Zn / Al carbonate-type layered double hydroxide, measured as above, be 1000 cps or more and 150000 cps or less. Since the peak intensity is within the above range, it can be determined that the protective layer (13) contains Zn / Al carbonate-type layered double hydroxide sufficient to trap anions, which are corrosion agents. More preferably, the peak intensity of the peak attributed to the Zn / Al carbonate-type layered double hydroxide is 5000 cps or more.
[0196] In addition, when the protective layer (13) according to the present embodiment contains Mg / Al carbonate-type layered double hydroxide, it is preferable that the peak intensity of the peak attributed to the Mg / Al carbonate-type layered double hydroxide, measured as above, be 1000 cps or more and 150000 cps or less. Since the peak intensity is within the above range, it can be determined that the protective layer (13) contains Mg / Al carbonate-type layered double hydroxide sufficient to sufficiently trap anions, which are corrosion agents. More preferably, the peak intensity of the peak attributed to the Mg / Al carbonate-type layered double hydroxide is 5000 cps or more.
[0197] Regarding other ingredients
[0198] The protective layer (13) according to the present embodiment may contain various Si-containing compounds, Zn-containing compounds, Al-containing compounds, Mg-containing compounds, etc., in addition to the components mentioned above.
[0199] ◇ Si-containing compounds
[0200] Examples of Si-containing compounds that can be contained in the protective layer (13) according to the present embodiment include various silicate-based compounds and their cured products. Examples of such silicate compounds include, for instance, 3-(2-aminoethyl)aminopropyltrimethoxysilane, 3-(2-aminoethyl)aminopropylmethyldimethoxysilane, 3-(2-aminoethyl)aminopropyltriethoxysilane, 3-(2-aminoethyl)aminopropylmethyldiethoxysilane, 3-(2-aminoethyl)aminopropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, N-2-(N-vinylbenzylaminoethyl)-3-aminopropyltrimethoxysilane, N-2-(N-vinylbenzylaminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(N-vinylbenzylaminoethyl)-3-aminopropyltriethoxysilane, N-2-(N-vinylbenzylaminoethyl)-3-aminopropylmethyldiethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldiethoxysilane, methyltrimethoxysilane, dimethyldimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, vinyltriacetoxysilane, 3-chloropropyltrimethoxysilane, 3-chloropropylmethyldimethoxysilane, 3-chloropropyltriethoxysilane, 3-chloropropylmethyldiethoxysilane, 3-anilinopropyltrimethoxysilane, 3-anilinopropylmethyldimethoxysilane, Examples include 3-anilinopropyltriethoxysilane, 3-anilinopropylmethyldiethoxysilane, vinyltrimethoxysilane, vinylmethyldimethoxysilane, vinyltriethoxysilane, vinylmethyldiethoxysilane, octadecyldimethyl[3-(trimethoxysilyl)propyl]ammonium chloride, octadecyldimethyl[3-(methyldimethoxysilyl)propyl]ammonium chloride, octadecyldimethyl[3-(triethoxysilyl)propyl]ammonium chloride, octadecyldimethyl[3-(methyldiethoxysilyl)propyl]ammonium chloride, 3-chloropropylmethyldimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, methyltrichlorosilane, dimethyldichlorosilane, trimethylchlorosilane, etc.
[0201] ◇ Zn-containing compounds
[0202] Examples of Zn-containing compounds that may be contained in the protective layer (13) according to the present embodiment include ZnO, Zn(OH)2, Zn5(OH)8Cl2·H2O, Zn5(CO3)2(OH)6, Zn2Al(OH)6Cl·1.8H2O, etc.
[0203] ◇ Al-containing compounds
[0204] Examples of Al-containing compounds that may be contained in the protective layer (13) according to the present embodiment include Al2O3, Al(OH)3, etc.
[0205] ◇ Mg-containing compounds
[0206] Examples of Mg-containing compounds that may be contained in the protective layer (13) according to the present embodiment include MgZn2.
[0207] ◇ Organic resins
[0208] In addition, the protective layer (13) according to the present embodiment may contain various organic resins as film components. By further containing organic resins in the protective layer (13) according to the present embodiment, it becomes possible to further improve the corrosion resistance of the protective layer (13).
[0209] As such organic resins, known organic resins such as polyester resin, polyurethane resin, epoxy resin, phenolic resin, acrylic resin, polyolefin resin, fluoropolymer resin, etc., may be used. In addition, it is also possible to use film-forming resin components, such as modified resins of these resins, that have been crosslinked with butylated melamine resin, methylated melamine resin, butylmethyl mixed melamine resin, urea resin, isocyanate resin, or a crosslinking agent component of a mixed system of these resins. Furthermore, electron beam curing resins or UV-curing resins may be used as organic resins. To further increase adhesion to the steel (11) or zinc-based plating layer (15), it is preferable to use at least one of the resins having a steel portion or polar functional groups in the molecular chain (polyester resin, urethane resin, epoxy resin, acrylic resin, etc.). These organic resins may be used alone or two or more may be used in combination.
[0210] ◇ Other ingredients
[0211] The protective layer (13) according to the present embodiment may contain zirconium compounds, fluoride, vanadium compounds, tannins, or tannic acid in addition to the various components mentioned above.
[0212] In addition, the protective layer (13) according to the present embodiment may further include various anti-corrosion pigments in addition to the various components mentioned above. As such anti-corrosion pigments, any of the following may be used: for example, calcium ion exchange silica (which is sometimes referred to as calcium silicate), magnesium oxide, calcium molybdate, aluminum molybdate, barium molybdate, etc.
[0213] In addition, the protective layer (13) according to the present embodiment may additionally contain extender pigments such as precipitated barium sulfate or clay, or coloring pigments such as titanium oxide, as needed. In addition, the protective layer (13) according to the present embodiment may also contain additives such as coloring agents, viscosity modifiers, leveling agents, defoaming agents, and ultraviolet absorbers as needed, in addition to the anti-corrosion pigments, extender pigments, and coloring pigments as described above.
[0214] Regarding the elemental concentration of the protective layer (13)
[0215] The protective layer (13) according to the present embodiment containing the above-mentioned components has a Zn concentration of 5.00 mass% or more and less than 30.00 mass%, and a Si concentration of 5.00 mass% or more and less than 25.00 mass%. Additionally, the protective layer (13) according to the present embodiment preferably has an Al concentration of 0.01 mass% or more and 10.00 mass% or less.
[0216] [Zn: 1.00 mass% or more, less than 30.00 mass%]
[0217] If the Zn concentration is less than 1.00 mass%, the content of the Zn / Al carbonate-type layered double hydroxide in the protective layer (13) according to the present embodiment is insufficient, and sufficient corrosion resistance cannot be obtained. By making the Zn concentration 1.00 mass% or more, it becomes possible to exhibit sufficient corrosion resistance even when the surface treatment member (1) is installed in the surface layer of the soil. In the protective layer (13) according to the present embodiment, the Zn concentration is preferably 10.00 mass% or more, and more preferably 15.00 mass% or more.
[0218] Meanwhile, if the Zn concentration is 30.00 mass% or higher, the content of Zn / Al carbonate-type layered double hydroxide in the protective layer (13) according to the present embodiment is excessively high, and the content of SiO2 becomes insufficient. By making the Zn concentration less than 30.00 mass%, it becomes possible to secure the SiO2 content while exhibiting sufficient corrosion resistance even when the surface treatment member (1) is installed on the surface layer of the soil. In the protective layer (13) according to the present embodiment, the Zn concentration is preferably 25.00 mass% or lower, and more preferably 20.00 mass% or lower.
[0219] [Si: 1.00 mass% or more, less than 25.00 mass%]
[0220] If the Si concentration is less than 1.00 mass%, the SiO2 content in the protective layer (13) according to the present embodiment is insufficient, and sufficient corrosion resistance cannot be obtained. By making the Si concentration 1.00 mass% or more, it becomes possible to exhibit sufficient corrosion resistance even when the surface treatment member (1) is installed in the surface layer of the soil. In the protective layer (13) according to the present embodiment, the Si concentration is preferably 10.00 mass% or more, and more preferably 15.00 mass% or more.
[0221] Meanwhile, if the Si concentration is 25.00 mass% or higher, the SiO2 content in the protective layer (13) according to the present embodiment is excessively high, and the content of Zn / Al carbonate-type layered double hydroxide becomes insufficient. By making the Si concentration less than 25.00 mass%, it becomes possible to secure the content of Zn / Al carbonate-type layered double hydroxide while exhibiting sufficient corrosion resistance even when the surface treatment member (1) is installed on the surface layer of the soil. In the protective layer (13) according to the present embodiment, the Si concentration is preferably 20.00 mass% or lower, and more preferably 15.00 mass% or lower.
[0222] [Mg: 0.10 mass% or more, 5.00 mass% or less]
[0223] In the case where the protective layer (13) according to the present embodiment contains an Mg-containing compound including an Mg / Al carbonate-type layered double hydroxide, it is preferable that the Mg concentration of the protective layer (13) be 0.10 mass% or more and 5.00 mass% or less.
[0224] By making the Mg concentration of the protective layer (13) 0.10 mass% or more, the protective layer (13) according to the present embodiment has a layered double hydroxide of the Mg / Al carbonate type sufficient to trap anions, which are corrosion agents, and exhibits superior corrosion resistance. The Mg concentration of the protective layer (13) is more preferably 0.50 mass% or more, and even more preferably 1.00 mass% or more.
[0225] Meanwhile, by making the Mg concentration of the protective layer (13) 5.00 mass% or less, the protective layer (13) according to the present embodiment suppresses the insufficient content of Zn / Al-based carbonate-type layered double hydroxide, thereby enabling each of the Zn / Al-based and Mg / Al-based carbonate-type layered double hydroxides to trap various corrosion factors in a balanced manner and exhibit superior corrosion resistance. The Mg concentration of the protective layer (13) is more preferably 4.00 mass% or less, and even more preferably 3.00 mass% or less.
[0226] Here, the above Zn concentration, Si concentration, and Mg concentration can be measured as follows.
[0227] First, an arbitrary location of the surface treatment member (1) of interest is cut in the thickness direction of the surface treatment member (1) (i.e., a direction perpendicular to the surface of the surface treatment member (1)) to obtain a cross-sectional sample of the protective layer (13). From an arbitrary location on the surface of the protective layer (13) of this cross-sectional sample, the location of the interface with the zinc-based plating layer (15) or the location of the interface with the steel material (11) along the thickness direction of the protective layer (13) (e.g., the Z-axis direction in FIG. 3a) is analyzed by an energy dispersive X-ray spectroscopy (EDS) analysis device equipped in a scanning electron microscope (SEM, e.g., JEOL JSM-7000F, etc.), and the obtained analysis results are mapped. Here, the elements of interest during the analysis are Zn, Si, Al, Mg, and C. The observation conditions for the SEM-EDS at this time can be, for example, acceleration voltage: 15 kV, irradiation current: 4.91 nA, number of sweeps: 10, and observation magnification: 500x.
[0228] The range corresponding to the protective layer (13) can be easily determined from the SEM image by a person skilled in the art. However, in this embodiment, the portion where the Zn concentration and Si concentration correspond to the above range in the depth profile of each element obtained as described above is treated as the region of the protective layer (13). Next, the average concentration of Zn, Si, and Mg elements in the region of the protective layer (13) is calculated from the depth profile of the obtained Zn, Si, and Mg elements.
[0229] The above measurements are similarly performed at any five locations of the obtained cross-sectional sample, and the average value of the obtained average concentration of each element at the number of measurement locations is treated as the Zn, Si, and Mg concentrations in the protective layer (13).
[0230] Regarding the distribution of Si elements in the protective layer (13)
[0231] Next, the distribution state of Si elements in the thickness direction of the protective layer (13) according to the present embodiment will be explained in detail with reference to FIG. 5. FIG. 5 is an explanatory diagram for explaining the distribution state of Si elements in the protective layer (13) according to the present embodiment.
[0232] As schematically illustrated in FIG. 5, the area from the surface side of the protective layer (13) (the Z-axis forward side in FIG. 5) toward the steel material (11) to the center of the thickness of the protective layer (13) is referred to as “Area a” for convenience. Likewise, the location from the center of the thickness of the protective layer (13) toward the steel material (11) to the interface with the steel material (11) (or the interface with the zinc plating layer (15) if the zinc plating layer (15) is present) is referred to as “Area b” for convenience.
[0233] In the same manner as the above method for measuring Si concentration, the depth profile for region a and the depth profile for region b are measured for the Si element, and the Si concentrations of regions a and b are calculated in the same manner as above. The Si concentration of region a obtained in this way is [Si] a denoted as, and the Si concentration in region b is [Si] b It is decided to write it as follows.
[0234] At this time, the protective layer (13) according to the present embodiment has a Si concentration (i.e., [Si] at half thickness on the surface side of the protective layer (13) a ) is the Si concentration (i.e., [Si] at 1 / 2 thickness on the steel (11) side of the protective layer (13). b ) at least 1.3 times (i.e., [Si] a ≥1.3×[Si] b It is desirable that the relationship holds.
[0235] [Si] a ≥1.3×[Si] bWhen the relationship is established, it means that the Si element in the protective layer (13) is distributed more in region a than in region b. It is thought that the corrosion agent penetrates from the surface side region of the protective layer (13) (i.e., region a) toward the steel material (11). Therefore, by distributing the Si element in region a, it becomes possible to more effectively prevent the penetration of the corrosion agent and further improve the corrosion resistance of the protective layer (13).
[0236] Si concentration in region a [Si] a is the Si concentration in region b [Si] b Regarding , it is more preferably 1.4 times or more, and even more preferably 1.5 times or more. Meanwhile, this magnification ([Si] a / [Si] b The larger ) is, the better, and although there is no upper limit specified, in practice, the upper limit is about 2.0 times.
[0237] Regarding the thickness of the protective layer (13)
[0238] The thickness of the protective layer (13) according to the present embodiment having the above configuration (thickness d1 in FIG. 3a to 4b) is preferably 0.1 μm or more and 50.0 μm or less. By making the thickness d1 of the protective layer (13) 0.1 μm or more, the surface treatment member (1) according to the present embodiment exhibits superior corrosion resistance. More preferably, the thickness d1 of the protective layer (13) is 1.0 μm or more.
[0239] Meanwhile, as the thickness d1 of the protective layer (13) becomes 50.0 μm or less, the surface treatment member (1) ensures the adhesion of the protective layer (13) and exhibits superior corrosion resistance. More preferably, the thickness d1 of the protective layer (13) is 30.0 μm or less.
[0240] In addition, the thickness of this protective layer (13) can be measured by direct observation from a cross-section. Specifically, a cross-sectional sample containing the protective layer (13) is obtained by cutting at any location of the surface treatment member (1) in the thickness direction of the surface treatment member (1). Then, the obtained cross-sectional sample is embedded in a room-temperature drying epoxy resin so that the cross-section can be observed, and after mechanically polishing the embedded surface, it is observed with an SEM. In this SEM observation, a person skilled in the art can easily distinguish the steel (11), the zinc-based plating layer (15), and the protective layer (13) from the appearance. The thickness of the protective layer (13) is measured at any five locations, and the average value of the thicknesses obtained at the five points is taken as the thickness of the protective layer (13).
[0241] Above, the detailed configuration of the protective layer (13) according to the present embodiment has been described.
[0242] <Detailed composition of the second protective layer (17)>
[0243] As schematically illustrated in FIGS. 4a and 4b, in the surface treatment member (1) according to the present embodiment, it is preferable that a second protective layer (17) is further positioned on the protective layer (13).
[0244] This second protective layer (17) contains SiO2 particles (19) as schematically shown in FIGS. 4a and 4b. These SiO2 particles (19) have an average particle size of 1.00 to 30.00 μm. Since the average particle size of the SiO2 particles (19) contained in the second protective layer (17) is 1.00 to 30.00 μm, the second protective layer (17) becomes a barrier layer, and the corrosion resistance as a surface treatment member (1) is further improved. Here, the average particle size of the SiO2 particles (19) is more preferably 10.00 μm or more. Also, the average particle size of the SiO2 particles (19) is more preferably 15.00 μm or less.
[0245] In addition, the average particle size of the SiO2 particles (19) of the second protective layer (17) can be measured in the same way as the average particle size of the SiO2 particles of the protective layer (13).
[0246] In the second protective layer (17) according to the present embodiment, the ratio of SiO2 particles (19) with a particle size of 1.00 to 30.00 μm ("number of SiO2 particles with a particle size of 1.00 to 30.00 μm" / "number of SiO2 particles with a particle size of 0.05 μm or more") is preferably 10 to 80%. By making the ratio of SiO2 particles (19) with a particle size of 1.00 to 30.00 μm 10% or more, it is possible to further improve the corrosion resistance of the surface treatment member (1). More preferably, the ratio of SiO2 particles (19) with a particle size of 1.00 to 30.00 μm is 30% or more.
[0247] Meanwhile, by making the ratio of SiO2 particles (19) with a particle size of 1.00 to 30.00 μm 80% or less, it is possible to further improve the corrosion resistance of the surface treatment member (1) while maintaining the adhesion of the second protective layer (19). More preferably, the ratio of SiO2 particles (19) is 70% or less.
[0248] Here, the particle size and number of SiO2 particles in the second protective layer (17) can be measured in the same way as the method for measuring the SiO2 content of the protective layer (13).
[0249] In addition, the second protective layer (17) according to the present embodiment may contain, in addition to the SiO2 particles (19) as described above, various compounds containing elements such as Zn, Al, Mg, and C (e.g., oxides or carbonate compounds containing at least one of these elements).
[0250] The thickness of the second protective layer (19) according to the present embodiment (thickness d2 in FIG. 4a and 4b) is preferably 1.0 μm or more and 100.0 μm or less. By making the thickness d2 of the second protective layer (19) 1.0 μm or more, the surface-treated member (1) according to the present embodiment exhibits superior corrosion resistance. More preferably, the thickness d2 of the second protective layer (19) is 10.0 μm or more.
[0251] Meanwhile, as the thickness d2 of the second protective layer (19) becomes 100.0 μm or less, the surface treatment member (1) ensures the adhesion of the second protective layer (19) and exhibits superior corrosion resistance. More preferably, the thickness d2 of the second protective layer (19) is 50.0 μm or less.
[0252] In addition, the thickness d2 of the second protective layer (19) can be measured in the same way as the thickness d1 of the protective layer (13) described above.
[0253] Here, the range corresponding to the protective layer (13) and the range corresponding to the second protective layer (19) can be easily determined from the SEM image by a person skilled in the art, but the region containing particles located on the upper side (opposite side to the steel material (11) side) of the region determined as the region of the protective layer (13) in the depth profile of each element by the SEM-EDS described above is treated as the region of the second protective layer (17).
[0254] Above, the detailed configuration of the second protective layer (19) according to the present embodiment has been described.
[0255] (Regarding the method of manufacturing a surface-treated member)
[0256] Hereinafter, an example of a method for manufacturing a surface treatment member (1) according to the present embodiment will be described.
[0257] <Method for manufacturing surface-treated steel material (10)>
[0258] The surface-treated steel (10) used as the material for the surface-treated member (1) according to the present embodiment is manufactured by using the steel (11) as a base material, forming a zinc-based plating layer (15) on the surface of the steel (11), applying a treatment agent for forming a protective layer to the surface of the zinc-based plating layer (15), and storing the surface after applying the treatment agent in a specific atmosphere for a predetermined time.
[0259] Method for forming a zinc-based plating layer (15)
[0260] Here, in addition to the molten plating method, thermal spraying, cold spraying, sputtering, deposition, and electroplating methods can be applied to form the zinc-based plating layer (15). However, the molten plating method is the most desirable in terms of cost.
[0261] Hereinafter, an example of a manufacturing method for obtaining a zinc-based plating layer (15) according to the present embodiment using a molten plating method will be described in detail.
[0262] In the manufacturing process of such a zinc-based plating layer (15), a steel plate, which is an example of a steel material (11) used as a substrate, is first rolled by the Zenzimir method to a desired plate thickness, then wound into a coil shape and installed in a molten plating line.
[0263] In the hot-dip galvanizing line, steel sheets are continuously passed through while being ejected from the coil. At this time, the steel sheets are heated and reduced at 800°C in an N2-5% H2 gas atmosphere under an environment where oxidation is unlikely to occur, for example, with an oxygen concentration of 20 ppm or less, by means of an annealing facility provided on the line, and then air-cooled with N2 gas to approximately the bath temperature of the subsequent plating bath + 20°C, and then immersed in the plating bath.
[0264] Here, a plating alloy in a molten state having the chemical composition as described above is prepared in the plating bath. The temperature of the plating bath is set above the melting point of the plating alloy (for example, about 460 to 660°C).
[0265] When preparing the material for the plating alloy, it is preferable to use a pure metal (purity of 99% or higher) as the alloy material. First, a predetermined amount of alloy metal is mixed to obtain the composition of the plating layer as described above, and then completely melted using a high-frequency induction furnace or an arc furnace under vacuum or inert gas exchange conditions to form an alloy. In addition, the molten material obtained by melting the alloy mixed with the predetermined components (composition of the plating layer) in the atmosphere is used as a plating bath.
[0266] Furthermore, there is no specific restriction requiring the use of pure metals in the production of the plating alloys described above; existing Zn, Mg, and Al alloys may be melted and used. In this case, there is no problem as long as only alloys of a specified composition with low impurity levels are used.
[0267] After immersing the steel plate in the plating bath as described above, it is lifted at a predetermined speed. At this time, the amount of plating deposited is controlled, for example, by N2 wiping gas, so that the zinc-based plating layer formed reaches a desired thickness. Here, regarding conditions other than the bath temperature, general plating operation conditions can be applied, and no special equipment or conditions are required.
[0268] In addition, various heat treatments may be performed on the molten plating alloy located on the steel plate as needed.
[0269] Method for forming the protective layer (13) and the second protective layer (17)
[0270] The protective layer (13) and the second protective layer (17) in the surface-treated steel material (10) according to the present embodiment are formed by applying a treatment agent for forming a protective layer to the surface of the zinc-based plating layer (15) formed as described above, and then storing the surface after applying the treatment agent in a specific atmosphere for a predetermined time.
[0271] ◇ Preparation of treatment agent for forming a protective layer
[0272] A treatment agent for forming a protective layer is prepared by mixing a component to be contained in the protective layer (more specifically, a SiO2 component and components of various carbonate-type layered double hydroxides such as Zn / Al or Mg / Al systems) with water as a solvent.
[0273] Here, as the SiO2 component contained in the treatment agent, various types of SiO2 as previously mentioned are used. At this time, it is more preferable to use a mixture of SiO2 particles having multiple types of average particle sizes (hereinafter also simply referred to as "SiO2 mixture") as the SiO2.
[0274] For example, by using SiO2 particles with an average particle size of 0.1 to 1.0 μm as a SiO2 mixture, a treatment agent for forming a protective layer (13) can be obtained. Here, it is preferable that the content of SiO2 particles with an average particle size of 0.1 to 1.0 μm be, for example, 50 to 75 mass% with respect to the total mass of the SiO2 mixture.
[0275] Likewise, by using SiO2 particles with an average particle size of 1.0 to 30.0 μm as the SiO2 mixture, a treatment agent for forming the second protective layer (17) can be obtained. Here, it is preferable that the content of SiO2 particles with an average particle size of 1.0 to 30.0 μm be, for example, 10 to 20 mass% with respect to the total mass of the SiO2 mixture.
[0276] Here, it is desirable to set the amount of water in each treatment agent (i.e., the water content of the treatment agent) such that the volume ratio of water with respect to the vacancies of the SiO2 mixture is 50% or more and 80% or less. Here, the vacancies of the SiO2 mixture can be determined in advance based on the vacancies ratio {1-(B / A)} obtained from the specific gravity “A” of the SiO2 used and the apparent specific gravity “B” of the SiO2 mixture before adding water.
[0277] In addition, it is preferable that the pH of the water used as a solvent for each treatment agent be within the range of 4 to 9. By doing so, it is possible to make the reactivity of the treatment agent more desirable. By doing so, it is possible to easily extract plating components (particularly components such as Zn) from the zinc-based plating layer (15). As a result, in the storage process described later, the components of the zinc-based plating layer (15) that has already been formed and the components of the treatment agent for forming a protective layer or the treatment agent for forming a second protective layer react appropriately, thereby forming a protective layer (13) or a second protective layer (17) according to the present embodiment.
[0278] ◇ Application of treatment agent
[0279] The treatment agent for forming a protective layer prepared as above can be applied to the surface of the zinc-based plating layer (15) to a thickness of 0.5 mm or more and 3.0 mm or less. Here, the application of the treatment agent as above can be carried out by a generally known application method, such as roll coating, curtain flow coating, air spray, airless spray, immersion, bar coating, brush coating, etc.
[0280] ◇ Storage of steel materials after treatment agent application
[0281] As described above, the steel material (steel material (11) having a zinc-based plating layer (15)) coated with a treatment agent is stored in an atmosphere with a temperature of 10 to 40°C and a relative humidity of 80% or more. By doing so, the components of the zinc-based plating layer (15) that has already been formed and the components of the treatment agent for forming a protective layer react appropriately, thereby forming a protective layer (13) according to the present embodiment.
[0282] Here, it is preferable that the storage time of the steel material as described above be 240 hours or more. By doing so, it is possible to form a protective layer (13) having the surface-treated steel material (10) according to the present embodiment. Meanwhile, although the upper limit of the storage time of the steel material is not specifically stipulated, practically, it is about 1440 hours. In particular, by making the storage time of the steel material 360 hours or more and 720 hours or less, it is possible to form a protective layer (13) having a more desirable thickness.
[0283] In addition, when forming a second protective layer (17) as an upper layer of the protective layer (13) formed as described above, a portion of the protective layer (13) formed as described above may be removed as necessary, then a treatment agent for forming the second protective layer is applied to the protective layer (13), and the structure is stored in the same manner as described above.
[0284] Here, since the application and storage conditions of the treatment agent for forming the second protective layer are the same as those for forming the protective layer, a detailed explanation is omitted below.
[0285] Additionally, the zinc-based plating layer (15) formed on the surface of the steel (11) may disappear from the surface of the steel (11) as a result of reacting with all the components of the treatment agent through this storage process. Also, depending on the storage time, the zinc-based plating layer (15) may remain between the steel (11) and the formed protective layer (13).
[0286] In addition, in the treatment agent for forming the protective layer, the pH of the water used as a solvent is set to 4 to 5 to make it easier to elute the plating components, and the temperature in the storage process is set to 30 to 40°C, thereby making it possible to concentrate elemental Si on the surface side of the protective layer (13).
[0287] By undergoing the process described above, a surface-treated steel material (10) that serves as the material for the surface-treated member (1) according to the present embodiment can be manufactured. Above, an example of a method for manufacturing a surface-treated steel material (10) according to the present embodiment has been described in detail.
[0288] Method for manufacturing a surface-treated member
[0289] A surface-treated steel material (10) obtained as described above is used as a material to manufacture a surface-treated member (1) according to the present embodiment. Here, in obtaining the part for manufacturing the surface-treated member (1) from the surface-treated steel material (10), it is possible to use various shape processing treatments, such as various forming processing treatments, fastening members such as bolts or rivets, or joining treatments by welding. By appropriately combining these treatments, a surface-treated member (1) having a desired shape can be manufactured from the surface-treated steel material (10).
[0290] Above, an example of a method for manufacturing a surface-treated member (1) according to the present embodiment has been briefly described.
[0291] Examples
[0292] Hereinafter, the surface treatment member according to the present invention will be described in detail while presenting examples and comparative examples. Furthermore, the examples presented below are merely examples of the surface treatment member according to the present invention, and the surface treatment member according to the present invention is not limited to the following examples.
[0293] Preparation of galvanized steel
[0294] In the test described below, cold-rolled steel sheets and Ni-plated cold-rolled steel sheets (both manufactured by Nippon Seitetsu Co., Ltd.) as shown in Table 1 below were prepared as plating substrates and cut to a size of 60 mm × 60 mm. Plating was performed using a batch-type hot-dip galvanizing test apparatus manufactured in-house, and multiple plated steel materials having the plating layer composition shown in Table 2 below were produced for each level. In addition, the plating thickness per side at each level is shown in Table 4 below.
[0295] [Table 1]
[0296]
[0297] [Table 2]
[0298]
[0299] <Preparation of Treatment Agent for Forming a Protective Layer>
[0300] Using commercially available SiO2 with various average particle sizes (Silica Flower series manufactured by Masuoka Yokyo Genryo Co., Ltd.), a treatment agent for forming a protective layer containing the components shown at each level in Tables 4-1 to 4-6 below was prepared. In addition, when preparing the treatment agent for forming a protective layer, a pH adjuster shown in Table 3 below was used as needed.
[0301] [Table 3]
[0302]
[0303] The prepared treatment agent was applied to the surface of the plated steel and storage treatment was performed under the conditions shown in Tables 4-1 to 4-6 below to form a protective layer and a second protective layer. Afterward, SiO2 that did not contribute to the formation of the protective layer was removed by washing with water, and then air-dried to obtain a surface-treated steel. In addition, multiple such surface-treated steels were produced for each level. For each surface-treated steel obtained in this way, various measurements of the protective layer, the second protective layer, and the plating layer were performed based on the above method. The results obtained are summarized in Tables 5-1 to 5-6 below.
[0304] [Table 4-1]
[0305]
[0306] [Table 4-2]
[0307]
[0308] [Table 4-3]
[0309]
[0310] [Table 4-4]
[0311]
[0312] [Table 4-5]
[0313]
[0314] [Table 4-6]
[0315]
[0316] [Table 5-1]
[0317]
[0318] [Table 5-2]
[0319]
[0320] [Table 5-3]
[0321]
[0322] [Table 5-4]
[0323]
[0324] [Table 5-5]
[0325]
[0326] [Table 5-6]
[0327]
[0328] In addition, for each surface-treated steel obtained in this way, corrosion resistance in soil was evaluated based on the following method.
[0329] Corrosion Resistance Evaluation Method
[0330] The corrosion resistance of the surface-treated steel of each obtained level was evaluated by burying it in soil simulating the surface layer of the soil. Silica sand with an average particle size of 200 μm (Flattery 40H manufactured by Yamakawa Sangyo Co., Ltd.) was used as the soil. The coating thickness of each surface-treated steel was set to 50 mm. After burying each surface-treated steel in this manner, ion-exchanged water containing 0.3 mass% NaCl and 0.1 mass% Na2SO4 was added dropwise to the soil to adjust the moisture content to 100%. Subsequently, the drying and wetting processes described below were repeated. Samples with 20, 40, and 100 repetitions were prepared and evaluated, respectively.
[0331] Drying process: Store at 30℃ for 7 days.
[0332] Wetting process: Dropping ion-exchanged water is added to adjust the moisture content to 100%.
[0333] After conducting the above test, the surface-treated steel was pickled with hydrochloric acid to remove the second protective layer, the protective layer, the plating layer existing beneath the protective layer, and the corrosion products of the steel. Subsequently, the mass of the steel was measured, and the corrosion loss was measured by comparing it with the mass of the test material (before plating). The evaluation criteria were as follows, and scores of “A,” “B,” and “C” were considered passing. The results obtained are summarized in Tables 6-1 to 6-6 below.
[0334] <Evaluation Criteria>
[0335] Rating A: Corrosion loss 1 g / m 2 below
[0336] B: Corrosion loss is 1 g / m 2 Exceeding 5g / m 2 below
[0337] C: Corrosion loss is 5g / m 2 Exceeding 15g / m² 2 below
[0338] D: Corrosion loss is 15g / m 2 Exceeding 200g / m² 2 below
[0339] E: Corrosion loss is 200g / m 2 over
[0340] [Table 6-1]
[0341]
[0342] [Table 6-2]
[0343]
[0344] [Table 6-3]
[0345]
[0346] [Table 6-4]
[0347]
[0348] [Table 6-5]
[0349]
[0350] [Table 6-6]
[0351]
[0352] As is evident from Tables 4-1 to 6-6 above, the embodiments corresponding to the present invention exhibit excellent corrosion resistance, whereas the comparative examples corresponding to the present invention exhibit insufficient corrosion resistance.
[0353] Although suitable embodiments of the present invention have been described in detail above with reference to the accompanying drawings, the present invention is not limited to these examples. It is evident to those skilled in the art that various modifications or alterations can be made within the scope of the technical concept described in the claims, and these are naturally understood to fall within the technical scope of the present invention.
[0354] The embodiments disclosed herein are illustrative in all respects and are not restrictive. The above embodiments may be omitted, substituted, or modified in various forms without departing from the appended claims, the configurations falling within the technical scope of the present invention as described below, and the spirit thereof. For example, the constituent elements of the above embodiments may be combined arbitrarily within the scope that does not impair their effects. Furthermore, from any such combination, the operation and effect of each constituent element regarding the combination are naturally obtained, and other operations and other effects are obtained that are obvious to those skilled in the art from the description in this specification.
[0355] Furthermore, the effects described in this specification are merely illustrative or exemplary and are not limiting. That is, the technology relating to the present invention may exhibit other effects that are obvious to those skilled in the art from the description in this specification, either together with or in lieu of the above effects.
[0356] In addition, the following configurations also fall within the technical scope of the present invention.
[0357] (1)
[0358] The steel material and,
[0359] A protective layer located on the surface of the above steel material
[0360] Equipped with,
[0361] The above protective layer
[0362] The Zn concentration is 1.00 mass% or more and less than 30.00 mass%, and the Si concentration is 1.00 mass% or more and less than 25.00 mass%, and also
[0363] A surface-treated member containing SiO2 and Zn / Al carbonate-type layered double hydroxide.
[0364] (2)
[0365] A surface treatment member described in (1), wherein the thickness of the protective layer is 0.1㎛ or more and 50.0㎛ or less.
[0366] (3)
[0367] A surface treatment member described in (1) or (2), wherein, in the measurement result obtained by X-ray diffraction (XRD) of the surface of the protective layer, the peak intensity of the peak attributed to the Zn / Al carbonate-type layered double hydroxide is 1000 cps or more and 150000 cps or less.
[0368] (4)
[0369] The above protective layer has an Mg concentration of 0.10 mass% or more and 5.00 mass% or less, and further contains a Mg / Al carbonate-type layered double hydroxide, a surface treatment member described in any one of (1) to (3).
[0370] (5)
[0371] A surface treatment member described in (4), wherein, in the measurement result obtained by X-ray diffraction (XRD) of the surface of the protective layer, the peak intensity of the peak attributed to the Mg / Al carbonate-type layered double hydroxide is 1000 cps or more and 150000 cps or less.
[0372] (6)
[0373] A surface treatment member described in any one of (1) to (5), wherein, in the measurement result of measuring the surface of the protective layer by X-ray diffraction (XRD), the peak intensity of the peak attributed to SiO2 is 500 cps or more and 100,000 cps or less.
[0374] (7)
[0375] A surface treatment member described in any one of (1) to (6), wherein, when looking at the distribution of Si concentration in the thickness direction of the protective layer, the Si concentration at half thickness on the surface side of the protective layer is at least 1.3 times the Si concentration at half thickness on the steel side of the protective layer.
[0376] (8)
[0377] The above protective layer is a surface treatment member described in any one of (1) to (7), containing SiO2 particles having a particle size of 0.1 to 1.0 μm as the SiO2.
[0378] (9)
[0379] A second protective layer located on the above protective layer is further provided,
[0380] The second protective layer is a surface treatment member described in any one of (1) to (8), containing SiO2 particles with a particle size of 1.0 to 30.0 μm.
[0381] (10)
[0382] The surface treatment member described in (9), wherein the thickness of the second protective layer is 1 μm or more and 100 μm or less.
[0383] (11)
[0384] A surface treatment member described in any one of (1) to (10), further comprising a zinc-based plating layer between the above steel material and the above protective layer.
[0385] (12)
[0386] The above zinc-based plating layer has an Al concentration of 0.10 mass% or more and less than 40.00 mass%, and also has a Zn concentration of 60.00 mass% or more, and is a surface treatment member as described in (11).
[0387] (13)
[0388] The above zinc-based plating layer is a surface treatment member described in (11) or (12) having an Mg concentration of 0.10 mass% or more and less than 15.00 mass%.
[0389] (14)
[0390] A surface treatment member described in any one of (11) to (13), wherein the thickness of the zinc-based plating layer is 1 μm or more and 200 μm or less. Explanation of the symbols
[0391] 1: Surface-treated member 10: Surface-treated steel 11: Steel 13: Protection layer 15: Zinc-based plating layer 17: Second protective layer 19: SiO2 particles
Claims
Claim 1 A surface-treated member comprising a steel material and a protective layer positioned on the surface of the steel material, wherein the protective layer has a Zn concentration of 1.00 mass% or more and less than 30.00 mass%, a Si concentration of 1.00 mass% or more and less than 25.00 mass%, and also contains SiO2 and a Zn / Al carbonate-type layered double hydroxide. Claim 2 A surface-treated member according to claim 1, wherein the thickness of the protective layer is 0.1㎛ or more and 50.0㎛ or less. Claim 3 A surface-treated member according to claim 1 or 2, wherein, in the measurement result obtained by measuring the surface of the protective layer by X-ray diffraction (XRD), the peak intensity of the peak attributed to the Zn / Al carbonate-type layered double hydroxide is 1,000 cps or more and 150,000 cps or less. Claim 4 A surface-treated member according to claim 1 or 2, wherein the protective layer has an Mg concentration of 0.10 mass% or more and 5.00 mass% or less, and further contains an Mg / Al-based carbonate-type layered double hydroxide. Claim 5 A surface-treated member according to claim 4, wherein, in the measurement result obtained by measuring the surface of the protective layer by X-ray diffraction (XRD), the peak intensity of the peak attributed to the Mg / Al carbonate-type layered double hydroxide is 1,000 cps or more and 150,000 cps or less. Claim 6 A surface-treated member according to claim 1 or 2, wherein, in the measurement result obtained by measuring the surface of the protective layer by X-ray diffraction (XRD), the peak intensity of the peak attributed to SiO2 is 500 cps or more and 100,000 cps or less. Claim 7 A surface-treated member according to claim 1 or 2, wherein, when observing the distribution of Si concentration in the thickness direction of the protective layer, the Si concentration at half the thickness on the surface side of the protective layer is at least 1.3 times the Si concentration at half the thickness on the steel side of the protective layer. Claim 8 A surface treatment member according to claim 1 or 2, wherein the protective layer contains SiO2 particles having a particle size of 0.1 to 1.0 μm as the SiO2. Claim 9 A surface treatment member according to claim 1 or 2, further comprising a second protective layer positioned on the protective layer, wherein the second protective layer contains SiO2 particles having a particle size of 1.0 to 30.0 μm. Claim 10 A surface-treated member according to claim 9, wherein the thickness of the second protective layer is 1 μm or more and 100 μm or less. Claim 11 A surface treatment member according to claim 1 or 2, further comprising a zinc-based plating layer between the steel material and the protective layer. Claim 12 A surface-treated member according to claim 11, wherein the zinc-based plating layer has an Al concentration of 0.10 mass% or more and less than 40.00 mass%, and also has a Zn concentration of 60.00 mass% or more. Claim 13 In claim 12, the zinc-based plating layer is a surface-treated member having an Mg concentration of 0.10 mass% or more and less than 15.00 mass%. Claim 14 A surface-treated member according to claim 11, wherein the thickness of the zinc-based plating layer is 1 μm or more and 200 μm or less.