Fiber adhesive

The use of paramylon nanofibers with a low hydration rate addresses the issues of allergenicity and inadequate heat and water resistance in conventional adhesives, offering a safe and effective bonding solution for food-grade non-woven bags.

KR1020260161628APending Publication Date: 2026-11-09가부시키가이샤 유글리드
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
KR1020267033806
Authority / Receiving Office
KR · KR
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-03-15
Filing Date
2025-03-14
Publication Date
2026-11-09

AI Technical Summary

Technical Problem

Existing adhesives for food-grade non-woven bags, such as tea bags and soup bags, face challenges in terms of food safety, allergenicity, and inadequate heat and water resistance, particularly when exposed to hot or boiling water, due to the use of conventional natural polymers like starch paste and agar.

Method used

A fiber adhesive comprising paramylon nanofibers derived from Euglena, with a hydration rate of 15% or less, which are non-allergenic and exhibit excellent heat and water resistance, achieved through a specific defibrillation process involving alkaline dissolution and high shear force.

Benefits of technology

The adhesive provides strong, durable bonding suitable for food-grade non-woven bags, maintaining adhesion in hot or boiling water conditions and ensuring food safety by avoiding chemical modification, thus preserving the natural properties of paramylon.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCT00004_ABST
    Figure PCT00004_ABST
Patent Text Reader

Abstract

The present invention relates to a fiber adhesive comprising paramylon nanofibers, which are fibrous β-1,3-glucans obtained from paramylon particles derived from Euglena, characterized in that the dehydration rate of the paramylon nanofibers is 15% or less. According to the present invention, it is possible to provide a fiber adhesive that is non-allergic, contains natural polymer compounds not derived from animals, and has excellent heat and water resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to an adhesive for fibers, and more particularly to an adhesive useful for bonding non-woven food bags, such as tea bags for holding tea leaves like black tea or green tea, or soup bags for holding ingredients for soup such as skipjack tuna kezuribushi, mackerel kezuribushi, or kelp. Background Technology

[0002] Food-grade nonwoven bags, such as tea bags and soup bags, are formed by folding a rectangular nonwoven sheet and bonding appropriate locations to form a bag shape. Conventionally, bonding of nonwoven sheets has been performed by a hot melt method in which a sealant containing a thermoplastic plastic such as polypropylene, polyester, polyurethane, or vinyl ethylene acetate is applied to the bonding area and heat-pressed (Patent Document 1).

[0003] However, from a food safety perspective, it is undesirable to use plastic for bonding food-grade non-woven bags, such as tea bags or soup bags. In particular, in the European Union (EU), where regulations on food additives are strict, there is a growing demand to use compostable materials for items such as tea bags (see the European Commission’s proposed regulations on packaging and packaging waste). Furthermore, as environmental pollution caused by microplastics resulting from the fine shredding of plastic waste has recently become a concern, there is a demand to use adhesives made primarily of natural materials for bonding non-woven bags as well. Prior art literature

[0004] Patent Document 1: Japanese Patent Publication No. 2024-016460 Patent Document 2: Japanese Patent Publication No. 2018-154723 The problem to be solved

[0005] Natural materials used in adhesives include starch paste, pullulan, agar, gelatin, gluten, and animal glue. Among these, gluten, which is a protein, is an allergenic substance, and animal glue and gelatin, which are natural polymer compounds derived from animals, are extracted from cows and pigs, so their use is sometimes restricted for religious reasons. For this reason, gluten, animal glue, and gelatin cannot be used for bonding non-woven bags containing food, such as tea bags or soup bags.

[0006] Meanwhile, starch paste and agar are both non-allergenic and are natural polymer compounds not derived from animals, so they do not have the problems described above. However, starch paste and agar have low heat resistance, and if a nonwoven sheet coated with starch paste and agar is placed in water and heated to about 105°C, the coating of starch paste and agar detaches from the nonwoven sheet. Since tea bags and broth bags are used in hot water, adhesives made primarily of starch paste and agar are unsuitable as adhesives for tea bags and broth bags.

[0007] The problem that the present invention aims to solve is to provide a fiber adhesive that is non-allergenic and contains a natural polymer compound not of animal origin, and has excellent heat and water resistance. means of solving the problem

[0008] The fiber adhesive according to the present invention is a fiber adhesive comprising paramylon nanofibers, which are fibrous β-1,3-glucans obtained from paramylon particles derived from Euglena, wherein

[0009] The above paramylon nanofiber is characterized by having a dehydration rate of 15% or less.

[0010] The inventors, while seeking a non-allergic and non-animal-derived natural polymer compound capable of acting as an adhesive, discovered that paramylon nanofibers, which are fibrous materials of paramylon, a polysaccharide derived from Euglena, a type of microalgae, are useful as materials for fiber adhesives.

[0011] Euglena is a species of microalgae that accumulates paramylon particles as photosynthetic products within its cells. Paramylon particles are elliptical particles with a major axis of 3–5 μm and a minor axis of 2–3 μm, and fibers called paramylon nanofibers (PNF) exist densely within these particles. Within the paramylon particles, single-stranded PNF self-organizes to form a triple helix structure, and the fibrous material entangles with one another to form fibers with a diameter of about 20 nm. Single-stranded PNF is a linear (string-like) polysaccharide (β-1,3-glucan) in which about 2,000 glucose molecules are β-1,3-linked, and it has the chemical structure shown in Fig. 1.

[0012] It was reported by the EFSA (European Food Safety Authority) in 2023 that paramylon is safe for humans to ingest at a dose of 5,000 mg / kg. Therefore, the fiber adhesive of the present invention containing PNF can be considered safe for food hygiene.

[0013] However, conventional adhesives made of general PNF were insufficient as adhesives for objects used by immersing them in water (including hot and warm water), such as nonwoven food bags or soup bags, because the objects would peel off at the bonding site during use. As a result of further investigation, the fiber adhesive according to the present invention was developed. That is, while the hydration rate of conventional general PNF is about 18%, the PNF included in the fiber adhesive of the present invention has a hydration rate of 15% or less.

[0014] Such PNF is obtained by dissolving paramylon particles under alkaline conditions and simultaneously neutralizing and applying a disintegration treatment using high shear force. The PNF obtained in this manner possesses homogeneous dispersibility and aggregated dispersibility, and has the property of dispersing in liquids containing water. Since the PNF included in the fiber adhesive according to the present invention possesses the above properties, it is uniformly dispersed within the adhesive, allowing the fiber adhesive to be uniformly applied to the bonding portion of an object. The method for obtaining PNF from paramylon particles in the present invention will be explained in detail in the section [Forms for Carrying Out the Invention] below.

[0015] Until now, adhesives containing paramylon (β-1,3-glucan) extracted from Euglena have been proposed, but the mainstream approach involved increasing the adhesive ability of paramylon by chemically modifying it, such as by introducing an acyl group to the β-1,3-glucan (Patent Document 2). However, chemically modifying paramylon may alter its properties, thereby reducing its safety as a food. In contrast, the PNF included in the fiber adhesive according to the present invention is not chemically modified, and in this respect, the fiber adhesive according to the present invention is highly safe. Furthermore, by not performing chemical modification of the PNF, it is possible to reduce the cost and shorten the manufacturing time associated with the production of the adhesive.

[0016] The PNF included in the fiber adhesive according to the present invention exhibits adhesiveness, water resistance, and heat resistance by heat pressing. Here, in this specification, "water resistance" refers to the property of maintaining adhesive ability for a long period even after being immersed in water at room temperature, and "heat resistance" refers to the property of maintaining adhesive ability even after being immersed in water at a temperature of 100°C or higher. Accordingly, the fiber adhesive according to the present invention can be suitably used as an adhesive for food nonwoven bags, such as tea bags or soup bags, which are used by immersing them in hot water or boiling water.

[0017] The objects to be bonded with the fiber adhesive of the present invention are not limited to nonwoven fabrics, and gauze, threads, etc., can also be bonded. In addition, any object composed of intertwined fibers and having a non-smooth surface can be bonded to the fiber adhesive of the present invention. The bonded objects may be formed from natural fibers, synthetic fibers, or mixed fibers, or may be formed from regenerated fibers. Furthermore, the fiber adhesive of the present invention can be used to bond two objects made of different fiber materials. Effects of the invention

[0018] The fiber adhesive according to the present invention contains PNF, which is a non-allergic and non-animal-derived natural polymer compound, and has excellent heat and water resistance, so it can be suitably used as an adhesive for food nonwoven bags, such as tea bags or soup bags, which are used by immersing them in hot water or boiling water. Brief explanation of the drawing

[0019] [Fig. 1] Chemical structure of paramylon (β-1,3-glucan) [Fig. 2] Scanning electron microscope image of paramylon particles (X1000). [Fig. 3] Enlarged image of a portion of the scanning electron microscope image of Fig. 2 (X20000). [Fig. 4] Scanning electron microscope image (X30000) of low yield paramylon nanofiber (PNF). [Fig. 5] Scanning electron microscope image of low yield PNF (enlarged view of Fig. 4 (X100000)). [Fig. 6] Scanning electron microscope image of low yield PNF (X30000). [Fig. 7] Scanning electron microscope image of low yield PNF (enlarged view of Fig. 6 (X100000)). [Fig. 8] Congo-Red absorption spectrum of PNF. [Fig. 9] A photograph showing the appearance of a 2% dispersion of PNF obtained by conventional defibrillation treatment and a 2% dispersion of low-yield PNF after standing for 2 weeks. [Fig. 10] Optical microscope image (X100) of a location where a 2% dispersion of low-yield PNF was applied to a cotton nonwoven fabric. [Fig. 11] Optical microscope image of a location where a 2% dispersion of low-yield PNF was applied to a cotton nonwoven fabric (enlarged view of Fig. 9 (X200)). [Fig. 12] Optical microscope image of cotton nonwoven fabric (X100). [Fig. 13] Optical microscope image of cotton nonwoven fabric (enlarged view of Fig. 11 (X200)). [Fig. 14] Graph showing the results of the tensile test (1). [Fig. 15] Graph showing the results of the tensile test (2). [Fig. 16] Graph showing the results of the tensile test (3). [Fig. 17] Photograph of the test specimen used in the tensile test (3). [Fig. 18] Graph showing the results of the tensile test (4). [Fig. 19] Photograph of the test specimen used in the tensile test (4). [Fig. 20] Photograph showing the relationship between heating temperature and the coloration of PNF. Specific details for implementing the invention

[0020] The fiber adhesive according to the present invention is an adhesive comprising paramylon nanofibers (PNF), which are fibrous β-1,3-glucans extracted from paramylon particles derived from Euglena gracilis, wherein the saturation rate of the PNF is 15% or less, preferably 10% or less, and more preferably 5% or less. The PNF included in the fiber adhesive according to the present invention can be obtained by applying a characteristic defibrillation treatment to the PNF generated from paramylon particles.

[0021] Paramylon consists of β-1,3-glucan, in which glucose is linked by β-1,3 bonds (see Fig. 1). Conventional general paramylon nanofibers are in an aggregated state due to hydrogen bonding of the hydroxyl side chains of β-1,3-glucan, and have a yield of about 18%. In contrast, the PNF included in the fiber adhesive according to the present invention has a state in which the hydroxyl side chains appropriately surround water molecules, and thus the yield is 15% or less. In the following description, to distinguish it from conventional general PNF, the PNF included in the fiber adhesive according to the present invention will be referred to as "low yield PNF."

[0022] Example 1

[0023] (1) Extraction of paramylon particles

[0024] After washing Euglena, the cell membrane of Euglena is dissolved with a 0.1 M sodium hydroxide (NaOH) solution to obtain a lysate. This lysate is washed with water multiple times (e.g., four times) and then suspended in a 1% sodium dodecyl sulfate (SDS) solution. Subsequently, the suspension is washed thoroughly to obtain paramylon particles. Figures 2 and 3 show electron microscope images of the obtained paramylon particles. These paramylon particles were elliptical disc-shaped with a major axis of 3–5 μm and a minor axis of 2–3 μm.

[0025] (2) Purification of low-yield PNF

[0026] Paramylon particles were dissolved in a 1 M NaOH solution, diluted twice with water to make a 0.5 M NaOH solution, and then neutralized with malic acid to obtain a paramylon solution. The neutralization of the paramylon solution was performed by passing equal amounts of the paramylon solution and malic acid through a fine nozzle and mixing them while applying shear force. By this method, the paramylon particles in the paramylon solution were defibrated to become low-yield PNF, and a slurry (PNF slurry) containing the above PNF was obtained. In this embodiment, neutralization was performed using malic acid, an organic acid that does not have metal corrosive properties, but in addition to malic acid, organic acids such as formic acid and citric acid, or inorganic acids such as hydrochloric acid and sulfuric acid may be used.

[0027] (3) Cleaning of low-yield PNF and preparation of low-yield PNF dispersion

[0028] The PNF slurry was centrifuged at 5,000 g for 10 minutes to obtain a precipitate excluding the supernatant. Water was added to this precipitate to suspend it sufficiently, and the operation of centrifuging this suspension at 5,000 g for 10 minutes to obtain a precipitate by excluding the supernatant was repeated four times to wash the low-yield PNF. Water was added to the precipitate obtained from the final washing operation, and the concentration of low-yield PNF contained therein was measured using a heat-drying moisture meter (MF-50, manufactured by A.N.D.), and a low-yield PNF dispersion was prepared such that the concentration of the PNF was 2 to 5% (preferably 2%). Furthermore, unless specifically stated otherwise in this specification, "%" indicates mass-volume percentage (w / v%).

[0029] (4) Confirmation of low-yield PNF

[0030] Figures 4 to 7 are micrographs of low yield PNF obtained by the above procedure, Figures 4 and 5 are scanning electron microscope images of one example of low yield PNF, and Figures 6 and 7 are scanning electron microscope images of another example of low yield PNF.

[0031] The molecular weight (Mw) of the single strand of low-yield PNF was measured by GPC (gel filtration chromatography), and the molecular weight (Mw) was 100,000 to 270,000. In addition, the single strand PNF and the low-yield PNF were each mixed with a Congo-Red aqueous solution, and the absorption spectrum of the mixture was measured using a visible light absorption spectrophotometer. The measurement results are shown in Figure 8. As can be seen from this figure, the maximum absorption spectrum of the single strand PNF was 488 nm, whereas the maximum absorption spectrum of the low-yield PNF was 513 nm. From these results, it was confirmed that the low-yield PNF is a state in which multiple nanofibers with a triple helix structure are aggregated.

[0032] Conventional general PNF is obtained by a defibrillation process in which equal amounts of paramylon solution and malic acid are mixed, that is, a conventional defibrillation process performed without passing through a fine nozzle. In contrast, low-yield PNF is obtained by passing the paramylon solution through a fine nozzle simultaneously with neutralization and applying a defibrillation process while applying high shear force to the paramylon particles. Through such a defibrillation process, the low-yield PNF is in a state where the hydroxyl side chains appropriately encircle water molecules, resulting in a lower yield than conventional PNF and exhibiting homogeneous dispersibility in water.

[0033] For a paramylon solution obtained from the same Euglena, a 2% dispersion of PNF was prepared by applying a conventional defibrillation treatment and the defibrillation treatment of the present example, respectively, and the yield of each PNF was determined. As a result, while the yield of the conventional defibrillation treatment was approximately 18%, the yield of the defibrillation treatment of the present example was 1-15%, indicating a lower yield. Figure 9 is a photograph showing the appearance of a 2% dispersion of PNF obtained by the conventional defibrillation treatment (yield of approximately 18%) (right) and a 2% dispersion of PNF obtained by the defibrillation treatment of the present example (yield of approximately 2%) after standing for two weeks. Looking at these photographs, in the 2% dispersion of PNF obtained by the conventional defibrillation treatment, the PNF is precipitated, whereas in the 2% dispersion of PNF obtained by the defibrillation treatment of the present example, the PNF is widely dispersed, proving that the yield is low.

[0034] Example 2

[0035] (1) Preparation of adhesive

[0036] As an adhesive for fibers according to the present invention, a 2% dispersion of low-yield PNF prepared in Example 1 (hereinafter referred to as 2% PNF dispersion) was used. In this example, low-yield PNF with a molecular weight (Mw) of 270,000 was used.

[0037] In addition, adhesives of Comparative Examples 1 to 10 below were prepared.

[0038] 1: A 2% dispersion of low molecular weight PNF (molecular weight (Mw) = 32,000) (hereinafter referred to as 2% low molecular weight PNF dispersion),

[0039] 2: A 2% dispersion of paramylon particles (hereinafter referred to as the 2% paramylon particle dispersion),

[0040] 3: 0.5% dispersion of strong alkaline PNF (hereinafter referred to as 0.5% strong alkaline PNF dispersion),

[0041] 4: A 2% aqueous solution of carboxymethyl cellulose sodium salt (CMC) (hereinafter referred to as 2% CMC aqueous solution),

[0042] 5: 2% cellulose nanofiber dispersion (hereinafter referred to as 2% CNF dispersion),

[0043] 6: 2% curdran dispersion (hereinafter, 2% curdran β-glucan),

[0044] 7: A 2% or 5% dispersion of β-1,3-glucan derived from bread yeast (hereinafter, 2% or 5% bread yeast β-glucan),

[0045] 8: A 2% or 5% dispersion of β-1,3-glucan derived from barley (hereinafter, 2% or 5% barley β-glucan),

[0046] 9: A 2% aqueous solution of agar (agarose, agaropectin), a natural polymer compound (hereinafter referred to as 2% agar solution),

[0047] 10: 2% starch paste

[0048] prepared.

[0049] The low molecular weight PNF is a PNF obtained by hydrolyzing the low yield PNF obtained in Example 1 using 1 to 6% hydrochloric acid at a temperature of 80°C for 5 hours. In hydrolysis using 1 to 6% hydrochloric acid, a low molecular weight PNF with a molecular weight (Mw) of 32,000 to 64,000 is obtained, but here, one with a molecular weight (Mw) of 32,000 was used.

[0050] Paramylon particles were used that were obtained by extracting paramylon particles from Euglena with 0.1 M sodium hydroxide and then deproteinizing them, in the same manner as in Example 1.

[0051] Strong alkaline PNF is PNF obtained by treating the PNF obtained in Example 1 with a 1 M sodium hydroxide solution.

[0052] The cellulose nanofiber used was "Leocrista I-2SX" (Leocrista is a registered trademark), a product of Daiichigogyo Seiyaku Co., Ltd. "Leocrista I-2SX" is a product in which carboxyl groups are introduced into cellulose fibers by oxidizing natural cellulose nanofibers (CNF) using the TEMPO (2,2,6,6-tetramethylpiperidine-1-oxyl radical) oxidation method.

[0053] The 2% starch paste was purchased from Fuekinori Kogyo Co., Ltd., the agar from Nakaraitetsu Co., Ltd., the curd β-1,3-glucan from Fujifilm Wako Junyaku Co., Ltd., the bread yeast β-1,3-glucan from Ortas Co., Ltd., the barley β-1,3-glucan from ADEKA Co., Ltd., and the CMC from Marugo Corporation.

[0054] (2) Preparation of nonwoven fabric

[0055] To confirm the adhesive strength of the adhesive according to the present embodiment and the adhesive of the comparative example, the basis weight (g / m²) 2 Three types of cotton nonwoven fabrics with different weights and thicknesses (mm) (Product names: Benly (registered trademark) SC194, SH25G, SE103, manufactured by Asahi Kasei Co., Ltd.), and one type of rayon nonwoven fabric (spun lace (basis weight 30g / m²)). 2 Prepared the Marukoseishi Kabushiki Kaisha.

[0056] Basis weight (g / m²) of 3 types of cotton nonwoven fabrics 2 The thickness (mm) is as follows.

[0057] SC194: 18.5 g / m 2 , 0.25 mm

[0058] SH25G: 25 g / m 2 , 0.16 mm

[0059] SE103: 100 g / m 2 , 0.54 mm

[0060] (3) Heat pressing test

[0061] Three types of cotton nonwoven fabrics and one type of rayon nonwoven fabric were each prepared and formed into a short sheet shape (length 65 mm, width 20 mm). Then, the end of the short sheet nonwoven fabric (length 14 mm, width 20 mm (area 280 mm) 2 Regarding )), the adhesives of the examples and comparative examples were applied such that the amount of PNF, etc., was 6 mg. Then, another single-layer nonwoven fabric was superimposed on it, and after heat pressing by applying a pressure of 4500 Pa for 45 seconds to 60 seconds at a temperature range of 85°C to 160°C, it was investigated whether or not adhesion occurred.

[0062] As a result of heat pressing, the three types of cotton nonwoven fabrics, rayon nonwoven fabrics, and cotton and rayon nonwoven fabrics were all bonded by the 2% PNF dispersion. From this, it was thought that nonwoven fabrics with a non-smooth surface could be bonded by the 2% PNF dispersion regardless of material or thickness.

[0063] Meanwhile, 2% CNF dispersion, 2% agar solution, and starch paste were able to bond three types of cotton nonwoven fabrics together, rayon nonwoven fabrics together, and cotton nonwoven fabrics and rayon nonwoven fabrics together, but other comparative examples did not show bonding ability.

[0064] The results of the heat pressing test are summarized in Table 1 below. In the table, “○” indicates that it adhered, and “Х” indicates that it did not adhere or peeled off.

[0065] splice 105℃, 20 min 121℃, 20 min 2% PNF dispersion ○ ○ ○ 2% low molecular weight PNF dispersion × - - 2% Paramylon particles × - - 0.5% strong alkaline PNF dispersion × - - 2% CMC aqueous solution × - - 2% CNF dispersion ○ ○ ○ 2% Curdran β-glucan × - - 5% bread yeast β-glucan × - - 5% Barley β-glucan × - - 2% agar solution ○ × × 2% starch paste ○ × ×

[0066] When the molecular weight (Mw) of PNF is reduced by hydrolysis using hydrochloric acid, the viscosity is lowered, and the concentration of PNF in the dispersion can be increased; however, in low molecular weight PNF with a molecular weight (Mw) of 100,000 or less, the adhesive ability was lost. In addition, PNF obtained by mechanical disintegration using a homogenizer, such as 0.5% strong alkali PNF, also did not exhibit adhesive ability for the same reason as low molecular weight PNF.

[0067] Bread yeast β-glucan has a structure in which it has short side chains of β-1,6 bonds branched from β-1,3 bonds, and it is thought that these branched side chains cause the loss of adhesive ability. Barley β-glucan is composed of β-1,3 and β-1,4 bonds, and it is thought that this structure is the cause of the loss of adhesive ability. Curdran β-glucan is a straight-chain β-1,3-glucan similar to PNF, but its molecular weight is approximately 1,200,000, which is about four times larger than that of PNF. In addition, curdran β-glucan exhibits a unique thermal property not seen in PNF, which is that it gels upon heating. It is thought that these properties are the reason why it did not exhibit adhesive ability. However, if curdran β-glucan is hydrolyzed until it reaches a molecular weight equivalent to that of the PNF in this example, gelation upon heating is suppressed, and there is a possibility that it can be used as an adhesive.

[0068] (3-1) Mechanism of Adhesion

[0069] A 2% PNF dispersion was applied to a cotton nonwoven fabric and the bonded portion was observed under an optical microscope. As shown in Figures 10 and 11, a PNF film was observed to be formed between the nonwoven fabrics that are the bonded materials.

[0070] The above-described film is an aggregate of PNF, but this PNF consists of multiple triple-helix nanofibers. It is believed that the reason the PNF possesses such a structure is that when extracting the PNF from the paramylon particles, the alkaline solution of the paramylon particles is passed through a narrow nozzle and neutralized while applying shear force. In other words, by neutralizing the paramylon particle solution while passing it through a narrow nozzle and applying shear force, the nanofibers constituting the paramylon particles align along their length and contract. This results in the formation of a PNF containing high-aspect-ratio fiber aggregates arranged in random protrusion shapes. When a dispersion of such PNF is applied to a nonwoven fabric serving as the substrate, the PNF within the dispersion diffuses between the fibers of the nonwoven fabric, and the protrusions of the fiber aggregates fit into the gaps of the fabric. In this state, two nonwoven fabrics are overlapped and heat-pressed, causing the hydration reaction of PNF to proceed and further shrinkage to occur, and moisture evaporates to form a heat-irreversible film, thereby completing the adhesion of the two nonwoven fabrics. On the other hand, when a dispersion that does not contain PNF is applied to the nonwoven fabric and heat-pressed, as shown in FIGS. 12 and 13, gaps exist between the fibers of the nonwoven fabric and adhesion does not occur.

[0071] Based on this principle of adhesion, adhesion does not occur in paramilon particles where PNF is tightly wound.

[0072] (4) Hot water resistance test

[0073] A heat resistance test was performed using a 2% PNF dispersion, a 2% CNF dispersion, a 2% agar solution, and a 2% starch paste, which indicate the adhesive ability of the nonwoven fabric through a heat pressing test. Specifically, 300 μL (6 mg as the amount of PNF, etc.) of a 2% PNF dispersion, a 2% CNF dispersion, a 2% agar solution, or a 2% starch paste was applied to the end (length 14 mm, width 20 mm) of a single-piece cotton nonwoven fabric (Benly SH25G) (length 65 mm, width 20 mm), and then another single-piece cotton nonwoven fabric was overlapped and heat-pressed with an iron at 144°C for 120 seconds to produce a test specimen. Then, the above test specimen was placed in an autoclave at 105°C or 121°C and heated for 20 minutes. Afterward, the test specimen removed from the water was dried to investigate whether the adhesive surface peeled off. The results are shown in Table 1.

[0074] As can be seen from Table 1, the test specimens bonded with 2% starch paste and 2% agar solution were easily delaminated by being placed in hot water at 105°C and 121°C. On the other hand, the test specimens bonded with 2% PNF dispersion did not delaminate when placed in hot water at either 105°C or 121°C. In addition, the test specimens bonded with 2% CNF dispersion did not delaminate when placed in hot water at either 105°C or 121°C, but the adhesive strength decreased by 50% compared to before being placed in hot water.

[0075] (5) Dissolution test

[0076] 300 μL (6 mg) of a 2% PNF dispersion was applied between the ends (length 14 mm, width 20 mm) of two single-sheet cotton nonwoven fabrics (Benly SH25G) (length 65 mm, width 20 mm), and the two were bonded by heating and pressing with an iron at 144°C for 120 seconds to prepare a test specimen. Then, a PNF leaching test from the test specimen was performed according to the following procedure.

[0077] First, a test specimen was placed in 100 mL of water and heated in an autoclave at 105°C or 121°C for 20 minutes. Then, the amount of glucose was calculated by measuring the β-1,3-glucan (refer to the structural formula in Fig. 1) eluted into the water using the high-sensitivity phenol sulfate method. Additionally, two sheets of single-piece cotton nonwoven fabric were placed in 100 mL of water and heated in an autoclave at 105°C or 121°C for 20 minutes; the amount of glucose was calculated by measuring the fiber components eluted into the water using the same high-sensitivity phenol sulfate method. This amount of glucose was used as the background.

[0078] Table 2 shows the calculated glucose amount. In Table 2, "cont" represents the glucose amount leached from the untreated cotton nonwoven fabric, and "PNF" represents the glucose amount leached from the test specimen. Additionally, "PNF-cont" in Table 2 is the amount of glucose leached from the test specimen minus the glucose leached from the untreated cotton nonwoven fabric. When heated to 105°C, no glucose leaching was confirmed from the test specimen, but when heated to 121°C, the glucose leaching amount from the test specimen was 0.22 mg. The ratio of the leaching amount (0.22 mg) to the PNF coating amount (45 mg) on ​​the test specimen (leaching rate (%)) is 0.49%, which is approximately 0.045 mg when converted to the amount of PNF used for the adhesive of the tea bag. The EFSA (European Food Safety Authority) reports that it is safe for humans to consume up to 5,000 mg / kg, which translates to 250,000 mg for a person weighing 50 kg. The figure of 0.045 mg is less than 1 / 50,000,000 of this value, indicating that it is an amount that poses no safety issues.

[0079] Glucose (mg) PNF cont Dissolution rate (%) cont 105℃ 0.86 PNF 105℃ 0.86 0 0 cont 121℃ 1.60 PNF 121℃ 1.82 0.22 0.49

[0080] (6) Water resistance test

[0081] Two sheets of single-layer cotton nonwoven fabric (Benly SH25G) (length 65 mm, width 20 mm) were overlapped, a 2% PNF dispersion was applied between each end (length 14 mm, width 20 mm), and the two were bonded using caulking (kashime). Then, the bonded area was heat-pressed at 85°C or 144°C for 2 minutes to produce test specimens, after which the test specimens were left in water at room temperature for 1 to 21 days. The results are shown in Table 3.

[0082] As can be seen from Table 3, the test specimens compressed at a low temperature (85℃) showed water resistance without peeling for up to 14 days, and the test specimens compressed at a high temperature (144℃) showed water resistance without peeling for up to 21 days.

[0083] In addition, although not shown in Table 3, a water resistance test was performed using 2% starch paste and 2% agar solution, similar to the 2% PNF dispersion. Unlike water-insoluble PNF, starch paste and agar are water-soluble; therefore, when the test specimens were left in water at room temperature, they all leached out of the test specimens, and the test specimens peeled off after 1 hour.

[0084] Water resistance test Days of flooding cold pressing High temperature pressing 1 ○ ○ 2 ○ ○ 3 ○ ○ 5 ○ ○ 7 ○ ○ 14 ○ ○ 21 △ ○

[0085] (7) Tensile test (1)

[0086] Two single-piece cotton nonwoven fabrics (Benly SH25G, length 65 mm, width 20 mm) were laid out in the longitudinal direction so that their respective ends (length 14 mm, width 20 mm) overlapped, and 1, 2, 4, 6, and 8 mg of PNF were placed between the ends of the two cotton nonwoven fabrics. The ends were then heat-pressed with an iron at 144°C for 2 minutes to laminate them, thereby producing a test specimen. The test specimen was attached to a tensile testing machine (product name "Tensilon Universal Material Testing Machine RTG-1210", manufactured by A. AND D Co., Ltd.), and the specimen was tensile in the longitudinal direction (machine direction (MD)) under conditions of a chuck distance of 30 mm and a tensile speed of 10 mm / min, and the maximum tensile strength (N) was determined.

[0087] The results of determining the maximum tensile strength and calculating the average for four test specimens (n=4) are shown in Fig. 14 and Table 4. As shown in Fig. 14 and Table 4, the tensile strengths of the test specimens coated with 4 mg, 6 mg, and 8 mg of PNF are nearly equivalent, and 4–4.5 N / 280 mm 2 ...was. Regarding this, the maximum tensile strength of test specimens coated with 1 mg and 2 mg of PNF was 2.0–2.2 N / 280 mm 2 ...was halved.

[0088] Maximum load (N) / 280 mm 2 PNF mg / 280 mm 2 Average STDEV 8 4.60 0.42 6 4.35 0.74 4 4.40 0.74 2 2.25 0.72 1 1.99 0.63

[0089] (8) Tensile test (2)

[0090] Two sheets of single-piece cotton nonwoven fabric (Benly SH25G) (length 65 mm, width 20 mm) were laid out in the longitudinal direction so that their respective ends (length 14 mm, width 20 mm) overlapped, and 6 mg of PNF was placed between the ends. The ends were then heat-pressed with an iron at 144°C for 2 minutes to produce a test specimen. Then, the test specimen was placed in water and heat-treated in an autoclave at 105°C and 121°C for 20 minutes, and the maximum tensile strength was measured in the same manner as in the tensile test (1). In addition, as a comparative example, the maximum tensile strength was determined in the same manner for the test specimen that was not immersed in water, and for the single-piece cotton nonwoven fabric used as a test specimen that was heat-treated in an autoclave at 105°C and 121°C for 20 minutes.

[0091] The results of determining the maximum tensile strength and calculating the average for four test specimens (n=4) are shown in FIG. 15 and Table 5. As shown in FIG. 15 and Table 5, the maximum tensile strength of the unheated test specimen is 4.35 N / 280 mm 2 In comparison, the maximum tensile strength of the test specimen heated in 105℃ water was 3.8 N / 280mm2 The maximum tensile strength of the test specimen heated in 121℃ water is 4.2 N / 280mm 2 ...as such, the maximum tensile strength of the heated specimens was slightly lower than that of the unheated specimens, but did not decrease significantly, ranging from 87.3% to 96.5% of the tensile strength of the unheated specimens. In addition, the maximum tensile strength of the specimens heated to 105°C and 121°C was approximately 98% and 95% of the maximum tensile strength of the cotton nonwoven fabric heated to 105°C and 121°C, respectively, and there was no significant difference from the maximum tensile strength of the cotton nonwoven fabric itself.

[0092] Maximum load (N) / 280 mm 2 PNF mg Heating temperature Average STDEV 6 - 4.35 0.74 6 121℃ 4.20 0.41 6 105℃ 3.80 0.45 Non-woven fabric only 121℃ 4.42 0.73 Non-woven fabric only 105℃ 3.88 0.42

[0093] (9) Tensile test (3)

[0094] The end (280 mm) of two sheets of single-sheet cotton nonwoven fabric (Benly SH25G, length 65 mm, width 20 mm) 2 Except for applying 300 μL (PNF: 6 mg) of a 2% PNF dispersion between the ends and changing the heating temperature to 131°C, 160°C, and the heating time to 60 seconds, 90 seconds, and 120 seconds when heat-pressing the ends, test specimens were prepared in the same manner as in the tensile test (1), and the maximum tensile strength was measured in the same manner. The results are shown in FIG. 16 and Table 6. In this experimental example as well, the maximum tensile strength was measured for four test specimens for each temperature and time condition.

[0095] 2% PNF Maximum tensile strength (N) Heating temperature (°C) Heating time (sec) Average STDEV 131 60 4.75 1.30 90 4.39 0.38 120 3.56 0.58 160 60 3.91 0.86 90 3.08 0.89 120 3.92 0.22

[0096] As can be seen from Figure 16 and Table 6, the maximum tensile strength of the specimen heated at 131°C for 60 seconds or 90 seconds was approximately the same as the maximum tensile strength of the specimen heated at 121°C for 20 minutes (see Figure 15 and Table 5), but the specimen heated at 131°C for 120 seconds, and the specimen heated at 160°C for 60 seconds, 90 seconds, or 120 seconds had a lower maximum tensile strength than the specimen heated at 121°C for 20 minutes.

[0097] Figure 17 is a photograph showing the appearance of test specimens prepared at heating temperatures of 131°C and 160°C and heating times of 60 seconds, 90 seconds, and 120 seconds. In the test specimens heated at 131°C for 60 seconds or 90 seconds (the two specimens on the left), the applied 2% PNF dispersion was in a less dry state, and wrinkles appeared after natural drying.

[0098] (10) Tensile test (4)

[0099] The end (280 mm) of two sheets of single-sheet cotton nonwoven fabric (Benly SH25G, length 65 mm, width 20 mm) 2 120 μL (PNF: 6 mg) of a 5% PNF dispersion was applied between the ends, and test specimens were prepared by setting the heating temperature to 160°C and the heating times to 60, 30, and 20 seconds when heat-pressing the ends, and also by setting the heating temperature to 178°C and the heating time to 15 seconds. Additionally, the ends (280 mm) of two single-sheet Cupro nonwoven fabrics (length 65 mm, width 14 mm) were prepared. 2 120 μL (PNF: 6 mg) of a 5% PNF dispersion was applied between the layers, and test specimens were prepared by setting the heating temperature to 178°C and the heating time to 15 seconds when heat-pressing the ends. The Cupro nonwoven fabric had a thickness of 0.16 mm and a basis weight of 18 g / m². 2 The above was used. For these test specimens, the maximum tensile strength was measured in the same way as in the tensile test (1). The results are shown in FIG. 18 and Table 7.

[0100] 5% PNF Maximum tensile strength (N) Heating temperature (°C) Heating time (sec) Average STDEV Cotton non-woven fabric 160 60 4.72 0.99 30 5.58 0.43 20 4.88 0.84 178 15 5.00 0.22 Cupro nonwoven fabric 178 15 2.41 0.63

[0101] As can be seen from the comparison of the results shown in FIG. 18 and Table 7 with the results of the tensile test (3), the side of the test specimen formed by bonding cotton nonwoven fabric using a 5% PNF dispersion had a greater overall maximum tensile strength than the side of the test specimen formed by bonding cotton nonwoven fabric using a 2% PNF dispersion. In addition, when comparing the test specimen formed by bonding cotton nonwoven fabric with the test specimen formed by bonding cupro nonwoven fabric, the side of the test specimen formed by bonding cotton nonwoven fabric had a greater maximum tensile strength. Furthermore, the cupro nonwoven fabric had a large bend when the 5% PNF dispersion was applied, making it difficult to bond.

[0102] Figure 19 is a photograph showing the appearance immediately after heat pressing of a cotton nonwoven fabric prepared by heat pressing a 5% PNF dispersion under conditions of a heating temperature of 160°C and heating times of 60 seconds, 30 seconds, and 20 seconds, and a 5% PNF dispersion prepared by heat pressing a cotton nonwoven fabric under conditions of a heating temperature of 178°C and a heating time of 15 seconds (2 pieces each, totaling 8 pieces). As can be seen from the figure, wrinkles occurred in all pieces except the one heat-pressed at 160°C for 60 seconds.

[0103] (11) Heating temperature and coloring of PNF

[0104] FIG. 20 is a photograph of the appearance of cotton nonwoven fabrics when 300 μL (PNF: 6 mg) of a 2% PNF dispersion is applied between two cotton nonwoven fabrics (Benly SH25G) and heat-pressed at temperatures of 131°C, 158°C, 184°C, and 200°C or higher for 60 seconds, 30 seconds, 60 seconds, and 15 seconds, respectively. From this photograph, it can be seen that when heated to 184°C and 200°C, the area where the 2% PNF dispersion was applied turns brown. Although the maximum tensile strength tends to increase when the heat-pressing temperature is raised, the discoloration is noticeable and undesirable when bonding white cotton nonwoven fabrics as shown in the photograph of FIG. 20, as the PNF turns brown.

[0105] (12) Review of pressure required for heat pressing of nonwoven fabric using PNF dispersion

[0106] Two sheets of nonwoven fabric coated with a 2% PNF dispersion were overlapped and compressed by caulking while applying a pressure of 0.5 to 0.6 MPa with an air cylinder. When compressed at a heating temperature of 144°C, the nonwoven fabric bonded with sufficient strength after 60 seconds of heat compression, but when compressed at a heating temperature of 85°C, it took more than 120 seconds for the nonwoven fabric to bond, and furthermore, wrinkles were prone to occur in the nonwoven fabric during heat compression, and water resistance was low.

[0107] (13) Heating and pressing device

[0108] When bonding two nonwoven fabrics, the PNF dispersion may be applied to the entire surface of the nonwoven fabric, but it is also possible to apply it using a spot stamp to prevent the occurrence of wrinkles. By doing this, the amount of PNF used can be reduced to about 30-40% compared to when the PNF is applied to the entire surface, and furthermore, the same degree of bonding effect is obtained. When applying the PNF dispersion using a spot stamp, the amount of liquid per drop should be 20μL to 100μL, preferably 20μL to 50μL, and the spacing between spots should be about 7 mm.

[0109] When two nonwoven fabrics are joined by multiple caulkings, the multiple caulkings may be arranged in parallel or in a cross shape. A combination of an upper caulking and a lower flat plate is also effective to prevent wrinkles.

[0110] [sun]

[0111] (Clause 1) The present invention is a fiber adhesive comprising paramylon nanofibers, which are fibrous β-1,3-glucans obtained from paramylon particles derived from Euglena, wherein

[0112] The yield of the above paramylon nanofiber is 15% or less.

[0113] (Paragraph 2) The fiber adhesive described in Paragraph 2 is, in the fiber adhesive described in Paragraph 1,

[0114] The yield of the above paramylon nanofiber is 10% or less.

[0115] (Paragraph 3) The fiber adhesive described in Paragraph 3 is, in the fiber adhesive described in Paragraph 2,

[0116] The yield of the above paramylon nanofiber is 1% or more and 5% or less.

[0117] (Paragraph 4) The fiber adhesive described in Paragraph 4 is, in any one of Paragraphs 1 to 3, a fiber adhesive,

[0118] The water resistance maintenance time measured by the water resistance test shown below is 22 days or less.

[0119] Water resistance test: Two sheets of single-piece nonwoven fabric (length 65 mm, width 20 mm) are laid out in the longitudinal direction so that their respective ends (length 14 mm, width 20 mm) overlap, and a fiber adhesive is placed between the ends such that the amount of paramylon nanofiber is 6 mg. The ends are then laminated by heat pressing at 144°C for 2 minutes to produce a test specimen. The test specimen is immersed in water, and the water resistance retention time, which is the time until the test specimen peels off, is measured.

[0120] (Clause 5) The fiber adhesive described in Clause 5 is, in any one of Clauses 1 to 4, a fiber adhesive,

[0121] The heat resistance maintenance time measured by the heat resistance test shown below is 21 days or less.

[0122] Heat and water resistance test: Two single-piece nonwoven fabrics (length 65 mm, width 20 mm) are laid out in the longitudinal direction so that their respective ends (length 14 mm, width 20 mm) overlap, and a fiber adhesive is placed between the ends so that the amount of paramylon nanofiber is 6 mg. The ends are then laminated by heat pressing at 115°C for 2 minutes to produce a test specimen. The test specimen is immersed in water at 105°C to 121°C for 20 minutes, and then the time until the test specimen peels off in water is measured.

[0123] In addition, the water resistance retention time and heat resistance retention time of the fiber adhesive according to the present invention may be determined according to the usage conditions of the substrate bonded with the adhesive. For example, in the case of a substrate used by being immersed in water or hot water for a few minutes to several hours, such as non-woven tea bags or soup bags, the water resistance retention time and heat resistance retention time of the fiber adhesive is sufficient to be 1 hour to 24 hours.

[0124] (Clause 6) The fiber adhesive described in Clause 6 is, in any one of Clauses 1 to 5, a fiber adhesive,

[0125] The maximum tensile strength measured by the tensile test shown below is 4 N or more.

[0126] Tensile test: Two nonwoven fabrics (length 65 mm, width 20 mm) are laid out in the longitudinal direction so that their respective ends (length 14 mm, width 20 mm) overlap, and a fiber adhesive is placed between the ends so that the amount of paramylon nanofiber is 6 mg, and the ends are laminated by heat pressing at 115°C for 1 minute to produce a test specimen. The test specimen is attached to a tensile testing machine and tensile in the longitudinal direction of the test specimen under conditions of a chuck distance of 30 mm and a tensile speed of 10 mm / min to determine the maximum tensile strength (N).

[0127] (Clause 7) The fiber adhesive described in Clause 7 is a fiber adhesive described in any one of Clauses 1 to 6, wherein the content of paramylon nanofiber is 2% or more and 5% or less.

[0128] (Clause 8) The method for producing paramylon nanofibers described in Clause 8 is,

[0129] A paramylon solution is prepared by adding paramylon particles to a basic solution, and

[0130] A method for producing paramylon nanofibers by adding an acidic solution to the paramylon solution to neutralize the paramylon solution,

[0131] The paramylon solution is neutralized by passing equal amounts of the paramylon solution and the acidic solution through a capillary tube.

Claims

Claim 1 A fiber adhesive comprising paramylon nanofibers, which are fibrous β-1,3-glucans obtained from paramylon particles derived from Euglena, wherein the dehydration rate of the paramylon nanofibers is 15% or less. Claim 2 A fiber adhesive according to claim 1, wherein the dehydration rate of the paramylon nanofiber is 10% or less. Claim 3 A fiber adhesive according to claim 2, wherein the dehydration rate of the paramylon nanofiber is 1% or more and 5% or less. Claim 4 An adhesive for fibers according to any one of claims 1 to 3, wherein the water resistance retention time measured by the water resistance test described below is 22 days or less. Water resistance test: Two sheets of single-piece nonwoven fabric (length 65 mm, width 20 mm) are laid out in the longitudinal direction so that their respective ends (length 14 mm, width 20 mm) overlap, and the adhesive for fibers is placed between the ends such that the amount of paramylon nanofiber is 6 mg, and the ends are laminated by heat pressing at 144°C for 2 minutes to produce a test specimen. The test specimen is immersed in water, and the water resistance retention time, which is the time until the test specimen peels off, is measured. Claim 5 An adhesive for fibers according to any one of claims 1 to 3, wherein the time of maintaining heat and water resistance measured by the heat and water resistance test described below is 21 days or less. Heat and water resistance test: Two sheets of single-piece nonwoven fabric (length 65 mm, width 20 mm) are laid out in the longitudinal direction so that their respective ends (length 14 mm, width 20 mm) overlap, and the adhesive for fibers is placed between the ends such that the amount of paramylon nanofiber is 6 mg, and the ends are laminated by heat pressing under conditions of 115°C for 2 minutes to produce a test specimen. The test specimen is immersed in water at 105°C to 121°C, and the time until the test specimen peels off is measured. Claim 6 A fiber adhesive according to any one of claims 1 to 3, wherein the maximum tensile strength measured by the tensile test described below is 4 N or more. Tensile test: Two nonwoven fabrics (length 65 mm, width 20 mm) are laid out in the longitudinal direction so that their respective ends (length 14 mm, width 20 mm) overlap, the fiber adhesive is placed between the ends so that the amount of paramylon nanofiber is 6 mg, and the ends are laminated by heat pressing at 115°C for 1 minute to produce a test specimen. The test specimen is attached to a tensile testing machine and tensile in the longitudinal direction of the test specimen under conditions of a chuck distance of 30 mm and a tensile speed of 10 mm / min, and the maximum tensile strength (N) is determined. Claim 7 An adhesive for fibers according to any one of claims 1 to 3, wherein the paramylon nanofiber content is 2% or more and 5% or less. Claim 8 A method for producing paramylon nanofibers by adding paramylon particles to a basic solution to prepare a paramylon solution, and adding an acidic solution to the paramylon solution to neutralize the paramylon solution, wherein the paramylon solution and the acidic solution are passed through a capillary tube in equal amounts to neutralize the paramylon solution.