Adhesive sheet
The adhesive sheet with a gas generating layer and adhesive layer deforms upon laser irradiation to enable precise peeling of small electronic components, addressing inconsistent peeling issues in conventional adhesive sheets.
Patent Information
- Application Number
- KR1020267035003
- Authority / Receiving Office
- KR · KR
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-07-01
- Filing Date
- 2020-11-30
- Publication Date
- 2026-11-09
AI Technical Summary
Conventional adhesive sheets struggle to effectively fix and peel small electronic components due to variations in thermally expandable microsphere size, leading to inconsistent peeling performance.
An adhesive sheet comprising a gas generating layer that deforms upon laser irradiation, allowing precise peeling by generating gas within a controlled area, with a gas generating layer and adhesive layer configured to ensure selective peeling of small electronic components.
The adhesive sheet enables precise and controlled peeling of small electronic components, preventing unnecessary detachment and minimizing adhesive residue, while maintaining positional accuracy and preventing damage.
Smart Images

Figure PAT00008_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to an adhesive sheet. Background Technology
[0002] Conventionally, when processing electronic components, there are cases where an operation is performed in which a workpiece is temporarily fixed on an adhesive sheet during processing and then peeled off from the adhesive sheet after processing. As an adhesive sheet used for such operations, an adhesive sheet is sometimes used that has a predetermined adhesive strength during processing and can reduce its adhesive strength after processing. As one such adhesive sheet, an adhesive sheet composed of containing thermally expandable microspheres within an adhesive layer has been proposed (e.g., Patent Document 1). An adhesive sheet containing thermally expandable microspheres has the characteristic that, while having a predetermined adhesive strength, the adhesive strength is reduced or lost by expanding the thermally expandable microspheres by heating, thereby forming irregularities on the adhesive surface and reducing the contact area. Such an adhesive sheet has the advantage of being able to easily peel off a workpiece without external stress.
[0003] However, in recent years, accompanied by the trend of lightweighting and increasing the number of various devices, electronic components have become miniaturized, creating a need to temporarily fix electronic components that have been miniaturized to a size comparable to the aforementioned thermally expandable microspheres. When processing miniaturized electronic components by temporarily fixing them, the influence of areas where large-sized thermally expandable microspheres exist or areas where such microspheres do not exist becomes significant due to variations in particle size, and consequently, there are cases where good peeling cannot be performed in such areas. Prior art literature
[0004] Japanese Patent Publication No. 2001-131507 The problem to be solved
[0005] The present invention is made to solve the above-mentioned conventional problems, and the purpose is to provide an adhesive sheet that can effectively temporarily fix small electronic components (e.g., chips with a size of 100 μm or less) and also effectively peel them off. means of solving the problem
[0006] The adhesive sheet of the present invention is an adhesive sheet comprising a gas generating layer and at least one adhesive layer disposed on one side of the gas generating layer, wherein the adhesive layer is a layer whose surface is deformed by laser light irradiation on the adhesive sheet.
[0007] In one embodiment, the gas generating layer is a layer capable of absorbing ultraviolet rays.
[0008] In one embodiment, the gas generating layer includes an ultraviolet absorber.
[0009] In one embodiment, the thickness of the gas generating layer is 0.1㎛ to 50㎛.
[0010] In one embodiment, the gas generating layer is a layer that generates hydrocarbon gas.
[0011] In one embodiment, the gasification initiation temperature of the gas generating layer is 150°C to 500°C.
[0012] In one embodiment, the elastic modulus Er(gas) [unit: MPa] and thickness h(gas) [unit: μm] of the gas generating layer by nanoindentation method satisfy the following formula (1).
[0013] Log(Er(gas)×10 6 )≥8.01×h(gas) -0.116 … (1)
[0014] In one embodiment, the thickness of the adhesive layer is 0.1 μm to 50 μm.
[0015] In one embodiment, the amount of deformation of the surface of the adhesive layer caused by laser light irradiation on the adhesive sheet is 0.6 μm or more in vertical displacement of the adhesive layer.
[0016] In one embodiment, the adhesive sheet has an ultraviolet transmittance of 30% or less at a wavelength of 360 nm.
[0017] In one embodiment, the adhesive sheet has a 10% weight reduction temperature of 200°C to 500°C.
[0018] In one embodiment, the adhesive sheet has a water vapor permeability of 5000 g / (m²·day) or less.
[0019] According to another aspect of the present invention, a method for processing an electronic component is provided. The method for processing an electronic component comprises bonding the electronic component onto the adhesive sheet and irradiating the adhesive sheet with a laser light to peel the electronic component off from the adhesive sheet.
[0020] In one embodiment, the peeling of the electronic component is performed selectively at a specific location.
[0021] In one embodiment, after attaching the electronic component to the adhesive sheet, a predetermined treatment is performed on the electronic component before peeling the electronic component from the adhesive sheet.
[0022] In one embodiment, the treatment is grinding, dicing, die bonding, wire bonding, etching, deposition, molding, circuit formation, inspection, quality inspection, cleaning, transfer, arrangement, repair, or protection of the device surface.
[0023] In one embodiment, the method for processing the electronic component includes peeling the electronic component from the adhesive sheet and then placing the electronic component on another sheet. Effects of the invention
[0024] According to the present invention, an adhesive sheet can be provided that can effectively temporarily fix a small electronic component (e.g., a chip with a size of 100 μm or less) and also effectively peel it off. Brief explanation of the drawing
[0025] FIG. 1 is a schematic cross-sectional view of an adhesive sheet according to one embodiment of the present invention. FIG. 2 is a schematic cross-sectional view of an adhesive sheet according to another embodiment of the present invention. Figure 3 is a schematic diagram illustrating the method for measuring piercing strength. Specific details for implementing the invention
[0026] A. Overview of Adhesive Sheets
[0027] FIG. 1 is a schematic cross-sectional view of an adhesive sheet according to a preferred embodiment of the present invention. The adhesive sheet (100) comprises a gas generating layer (10) and at least one adhesive layer (20) disposed on one side of the gas generating layer (10). The gas generating layer (10) generates gas by irradiating with laser light. More specifically, the gas generating layer (10) is a layer that generates gas by gasifying its components by irradiating with laser light. The surface of the adhesive layer (20) can be deformed by irradiating laser light onto the adhesive sheet (substantially the gas generating layer). In one embodiment, the deformation is caused by gas generated from the gas generating layer (10) and may occur on the side of the adhesive layer (20) opposite to the gas generating layer (10). As the laser light, UV laser light is typically used.
[0028] The adhesive sheet of the present invention can be used by adhering a workpiece, such as an electronic component, to the adhesive layer. The adhesive sheet of the present invention is provided with a gas generating layer and partially generates gas within a minute range by irradiating with laser light. As described above, deformation occurs in the adhesive layer due to the gas generation, and as a result, peelability is exhibited in the part irradiated with laser light. Typically, the laser light is irradiated from the side opposite to the adhesive layer of the gas generating layer. According to the present invention, since deformation can be generated within a minute range in this manner, the small electronic component can be effectively peeled even when processing (processing) an extremely fine small electronic component. Furthermore, even when a small electronic component requiring peeling and a small electronic component not requiring peeling are temporarily fixed adjacent to each other, peeling can be performed at the location to be peeled and not at locations other than the location to be peeled; that is, only the small electronic component requiring peeling can be peeled, and unnecessary detachment of the small electronic component can be prevented. In order to ensure good deformation of the adhesive layer, it is desirable that at least a portion of the generated gas be barrierd so as not to escape from the adhesive sheet, and the adhesive layer can function as a gas barrier layer. Furthermore, the adhesive sheet is advantageous in that it has excellent directionality during peeling, allows peeling only at desired locations, prevents damage, and leaves minimal adhesive residue. Additionally, directionality during peeling is an indicator representing the positional accuracy when a substrate, such as a small electronic component, is peeled from the adhesive sheet and injection molded at a location spaced at a certain distance; excellent directionality prevents the substrate from flying off in an unexpected direction during peeling.
[0029] Deformation of the adhesive layer refers to displacement occurring in the normal direction (thickness direction) and the horizontal direction (direction orthogonal to the thickness direction) of the adhesive layer. Deformation of the adhesive layer is generated by generating gas from the gas generation layer by pulse scanning with a UV laser light having a wavelength of 355 nm and a beam diameter of approximately 20 μmφ, at an output of 0.80 mW and a frequency of 40 kHz. The shape after deformation is observed, for example, by measuring an arbitrary single spot pulse-scanned with a confocal laser microscope or a non-contact interference microscope (WYKO) one minute after laser light irradiation. The shape may be a foam (convex), a through hole (irregularity), or a depression (concave), and peelability may occur due to these deformations. To efficiently peel electronic components in the normal direction, it is preferable for the change in displacement in the normal direction before and after laser light irradiation to be large, and it is particularly suitable to form a foam shape. The foam (convexity) is defined based on the surface of the adhesive sheet in the un-irradiated portion, with the highest point defined as vertical displacement Y and the half-length total width defined as horizontal displacement X (diameter). Regarding through holes (irregularities) and indentations (concave areas) formed after laser irradiation, the difference between the highest point and the lowest point is defined as vertical displacement Y, and the diameter of the hole is defined as horizontal displacement X. Hereinafter, the portion deformed by laser irradiation is also referred to as the "deformed portion." The vertical displacement of the adhesive layer is preferably 0.6 μm or more, more preferably 0.7 μm or more, and even more preferably 1.0 μm or more. Within this range, peelability is excellent, and the directionality during peeling is excellent. Furthermore, peeling can be performed with high precision in the desired direction, and as a result, adhesive residue, damage, etc., can be prevented. The upper limit of the said vertical displacement is, for example, 10 μm (preferably 20 μm). The horizontal displacement of the adhesive layer is preferably 80 μm or less, more preferably 50 μm or less, and even more preferably 40 μm or less. Within this range, peeling can be preferably performed only at desired locations for small adherents.In addition, the same effect can be expected even when the adherends are arranged at narrow intervals. The lower limit of the horizontal displacement is, for example, 3 μm (preferably 4 μm).
[0030] FIG. 2 is a schematic cross-sectional view of an adhesive sheet according to another embodiment of the present invention. The adhesive sheet (200) further comprises an intermediate layer (30) between the gas generating layer (10) and the adhesive layer (20). By providing an intermediate layer, the deformation of the adhesive layer can be easily controlled (details will be described later). In addition, the intermediate layer can function as a gas barrier layer in cooperation with the adhesive layer. Therefore, by providing an intermediate layer, gas barrier properties are improved, and an adhesive sheet with a more preferably deformed adhesive layer can be obtained. The intermediate layer may be a single layer or a multilayer layer.
[0031] Although not described, the adhesive sheet may further comprise other layers. For example, a substrate, another adhesive layer, etc. may be provided on the side opposite to the adhesive layer of the gas generating layer. As the substrate, for example, a film formed of any suitable resin is used.
[0032] The adhesive strength of the adhesive layer SUS430 of the adhesive sheet of the present invention is preferably 0.1 N / 20 mm or more, more preferably 0.2 N / 20 mm to 50 N / 20 mm, even more preferably 0.5 N / 20 mm to 40 N / 20 mm, particularly preferably 0.7 N / 20 mm to 20 N / 20 mm, and most preferably 1 N / 20 mm to 10 N / 20 mm. Within this range, an adhesive sheet exhibiting good adhesiveness can be obtained, for example, as a temporary fixing sheet used in the manufacture of electronic components. In this specification, adhesive strength refers to the adhesive strength measured by a method conforming to JIS Z 0237:2000 (bonding conditions: 1 reciprocating of a 2 kg roller, tensile speed: 300 mm / min, peel angle 180°) under an environment of 23°C.
[0033] In one embodiment, the gas generating layer has a predetermined adhesive strength. The adhesive strength of the gas generating layer of the adhesive sheet of the present invention on SUS430 is preferably 0.1 N / 20 mm or more, more preferably 0.5 N / 20 mm to 50 N / 20 mm, even more preferably 1 N / 20 mm to 40 N / 20 mm, particularly preferably 1.5 N / 20 mm to 30 N / 20 mm, and most preferably 2 N / 20 mm to 20 N / 20 mm. Within this range, an adhesive sheet exhibiting good adhesiveness can be obtained, for example, as a temporary fixing sheet used in the manufacture of electronic components.
[0034] The thickness of the adhesive sheet of the present invention is preferably 2㎛ to 200㎛, more preferably 3㎛ to 150㎛, and even more preferably 5㎛ to 120㎛.
[0035] The haze value of the adhesive sheet of the present invention is preferably 50% or less, more preferably 0.1% to 40%, and even more preferably 0.5% to 30%. Within this range, it becomes possible to see the substrate (e.g., a stand for temporarily fixing electronic components) through the adhesive sheet, and, for example, an adhesive sheet with excellent visibility of a marking provided on a stand to indicate the temporary fixing position of an electronic component can be obtained. Since the adhesive sheet of the present invention can be constructed without containing insoluble fillers in each layer provided by the adhesive sheet, it can be made into an adhesive sheet with a low haze value and excellent visibility of the substrate as described above. This effect is an excellent effect that is not obtained in adhesive sheets containing insoluble fillers (e.g., thermally expandable microspheres).
[0036] The water vapor permeability of the adhesive sheet of the present invention is preferably 5000 g / (m²·day) or less, more preferably 4800 g / (m²·day) or less, even more preferably 4500 g / (m²·day) or less, and even more preferably 4200 g / (m²·day) or less. In an adhesive sheet having a water vapor permeability within this range, the release of gas generated by laser light irradiation is prevented, and a deformation portion with an excellent shape is formed in the adhesive layer. By using such an adhesive sheet, small substrates (e.g., electronic components) can be peeled off with high precision. It is preferable that the water vapor permeability of the adhesive sheet of the present invention be as low as possible, but the lower limit is, for example, 0.1 g / (m²·day). The water vapor permeability can be measured by a measurement method conforming to JIS K7129B under an atmosphere of 30°C and 90% RH.
[0037] The water vapor permeability of the laminate comprising the adhesive layer and the intermediate layer is preferably 10,000 g / (m²·day) or less, more preferably 7,000 g / (m²·day) or less, even more preferably 5,000 g / (m²·day) or less, even more preferably 4,800 g / (m²·day) or less, even more preferably 4,500 g / (m²·day) or less, and particularly preferably 4,200 g / (m²·day) or less. Within this range, the laminate comprising the adhesive layer and the intermediate layer functions well as a gas barrier layer, and the adhesive layer forms a deformation portion with an excellent shape. By using such an adhesive sheet, small substrates (e.g., electronic components) can be peeled off with high precision. Although it is preferable for the water vapor permeability of the laminate comprising the adhesive layer and the intermediate layer to be as low as possible, the lower limit is, for example, 1 g / (m²·day).
[0038] The piercing strength of the laminate comprising the adhesive layer and the intermediate layer is preferably 10 mN to 5000 mN, more preferably 30 mN to 4000 mN, even more preferably 50 mN to 3000 mN, and particularly preferably 100 mN to 2000 mN. Within this range, the laminate comprising the adhesive layer and the intermediate layer functions well as a gas barrier layer, and shape changes due to gas generation occur preferably, and as a result, the adhesive layer forms a deformation portion with an excellent shape. By using such an adhesive sheet, small adherents (e.g., electronic components) can be peeled off with high precision. The piercing strength is measured by using a compression tester 6 (manufactured by Kato Tech Co., Ltd., product name "KES-G5") as shown in FIG. 3, by inserting and supporting sample 4 (e.g., the laminate) in a sample holder (5A, 5B) having a circular opening with a diameter of 11.28 mm. More specifically, at a measurement temperature of 23°C, a piercing needle (radius of curvature: 1 mm) is pierced into the sample at the center of the circular opening (piercing speed: 0.1 mm / s), and the maximum load at the point of failure can be defined as the piercing strength.
[0039] The ultraviolet transmittance of the laminate composed of the adhesive layer and the intermediate layer at a wavelength of 360 nm is preferably 50% to 100%, and more preferably 60% to 95%.
[0040] The ultraviolet transmittance of the adhesive sheet at a wavelength of 360 nm is preferably 30% or less, more preferably 20% or less, even more preferably 15% or less, particularly preferably 10% or less, and most preferably 5% or less. The lower limit of the ultraviolet transmittance of the adhesive sheet at a wavelength of 360 nm is, for example, 0% (preferably 0.05%, more preferably 0.1%).
[0041] The 10% weight loss temperature of the adhesive sheet is preferably 200°C to 500°C, more preferably 220°C to 450°C, even more preferably 250°C to 400°C, and particularly preferably 270°C to 370°C. Within this range, an adhesive sheet capable of forming a better deformation portion can be obtained by laser light irradiation. The 10% weight loss temperature of the adhesive sheet refers to the temperature at the point in time when the weight of the adhesive sheet has decreased by 10% by weight relative to the weight before heating (i.e., the weight of the adhesive sheet has become 90% of the weight before irradiation) in the TGA analysis when the adhesive sheet is heated.
[0042] B. Gas generation layer
[0043] The gas generating layer may be a layer capable of absorbing ultraviolet rays. In one embodiment, the gas generating layer comprises an ultraviolet absorber. By including an ultraviolet absorber, a gas generating layer capable of absorbing laser light and generating gas can be formed. Typically, the gas generating layer comprises an ultraviolet absorber and adhesive A. Preferably, the ultraviolet absorber is dissolved in adhesive A. When the ultraviolet absorber is dissolved in adhesive A, a deformed portion (e.g., an uneven portion) can be generated at any location in the adhesive layer, and an adhesive sheet with minimal variation in the shape of the deformed portion (e.g., an uneven portion) can be obtained. By using such an adhesive sheet, a deformed portion (e.g., an uneven portion) can be generated at a desired location with high precision, and the effects of the present invention become significant. Furthermore, in this specification, the state of "dissolved in the adhesive" means that the ultraviolet absorber is not present in the gas generating layer as a particle. More specifically, it is preferable that the gas generating layer does not contain ultraviolet absorbers with a particle size of 10 μm or more when measuring the particle distribution within the cross-section of the gas generating layer by X-ray CT. Additionally, the gas generating layer may or may not contain components insoluble in the adhesive. In one embodiment, the presence or absence and content of insoluble components in the gas generating layer are evaluated by the haze value of the gas generating layer, and the lower the haze value, the lower the content of insoluble components in the gas generating layer is evaluated. Preferably, the gas generating layer does not substantially contain components insoluble in the adhesive.
[0044] The elastic modulus of the cross-section of the gas generating layer by the nanoindentation method is preferably 0.01 MPa to 1000 MPa, and more preferably 0.05 MPa to 800 MPa. Within this range, a change in the shape of the gas generating layer due to gas generation occurs in a desirable manner, and as a result, a deformation portion of the adhesive layer with an excellent shape is formed. The elastic modulus by the nanoindentation method refers to the elastic modulus obtained from the load-indentation depth curve obtained by continuously measuring the load and indentation depth of the indenter during loading and unloading when the indenter is pressed into the sample (e.g., adhesive surface). The elastic modulus by the nanoindentation method is obtained by numerically processing the displacement-load hysteresis curve obtained by pressing a diamond Berkovich-type (triangular pyramidal) probe perpendicularly onto the cross-section of the layer to be measured in the software (triboscan) of the measuring device. In this specification, the elastic modulus by the nanoindentation method of a cross-section is the elastic modulus measured using a nanoindenter (Triboindenter TI-950 manufactured by Hysitron Inc.) by a single indentation method at a predetermined temperature (25°C) under measurement conditions of an indentation speed of approximately 500 nm / sec, a drawing speed of approximately 500 nm / sec, and an indentation depth of approximately 1500 nm. Furthermore, the elastic modulus of the gas generating layer can be adjusted by the type of material included in the corresponding layer, the structure of the base polymer constituting the material, and the type and amount of additives added to the corresponding layer. Additionally, in this specification, when the term "elastic modulus by the nanoindentation method" is used without referring to a cross-section or a surface, the said elastic modulus refers to the elastic modulus by the nanoindentation method of a cross-section.
[0045] The elastic modulus of the surface of the gas generating layer by the nanoindentation method is preferably 0.01 MPa to 1000 MPa, and more preferably 0.05 MPa to 800 MPa. Within this range, a change in the shape of the gas generating layer due to gas generation occurs in a desirable manner, and as a result, a deformation portion of the adhesive layer with an excellent shape is formed. The elastic modulus by the nanoindentation method refers to the elastic modulus obtained from the load-indentation depth curve obtained by continuously measuring the load and indentation depth of the indenter during loading and unloading when the indenter is pressed into the sample (e.g., adhesive surface). The elastic modulus by the nanoindentation method is obtained by numerically processing the displacement-load hysteresis curve obtained by pressing a diamond Berkovich-type (triangular pyramidal) probe perpendicularly into the target layer for measurement in the software (triboscan) of the measuring device. In this specification, the elastic modulus by the nanoindentation method of the surface is the elastic modulus measured by a single indentation method at a predetermined temperature (25°C) using a nanoindenter (Triboindenter TI-950 manufactured by Hysitron Inc.) under measurement conditions of an indentation speed of about 500 nm / sec, a drawing speed of about 500 nm / sec, and an indentation depth of about 3000 nm. In addition, the elastic modulus of the gas generating layer can be adjusted by the type of material included in the corresponding layer, the structure of the base polymer constituting the material, and the type and amount of additives added to the corresponding layer. In the present invention, there is no significant difference between the elastic modulus by the nanoindentation method measured by the above method with the cross-section as the measurement surface and the elastic modulus by the nanoindentation method measured by the above method with the surface as the measurement surface, and in cases where measurement from the cross-section is difficult, the value measured from the surface can be adopted as the value measured from the cross-section.
[0046] The gasification initiation temperature of the above gas generation layer is preferably 150°C to 500°C, more preferably 170°C to 450°C, even more preferably 190°C to 420°C, and particularly preferably 200°C to 400°C. Within this range, an adhesive sheet capable of forming a better deformation portion can be obtained by laser light irradiation. Furthermore, in this specification, the gasification initiation temperature of the gas generation layer refers to the gas generation rise temperature calculated from EGA analysis when the adhesive sheet is heated. The gas generation rise temperature is defined as the temperature at which half of the maximum gas generation peak of the EGA / MS spectrum obtained from EGA analysis is reached. The lower the gasification initiation temperature, the lower the temperature at which gas begins to be generated when laser light is irradiated, so that a sufficient amount of gas is generated even when laser light is irradiated at a lower output. In one embodiment, the gasification initiation temperature of the gas generation layer corresponds to the gasification initiation temperature of the ultraviolet absorber.
[0047] The 10% weight reduction temperature of the gas generating layer is preferably 150°C to 500°C, more preferably 170°C to 450°C, and even more preferably 200°C to 400°C. Within this range, an adhesive sheet capable of forming a better deformation portion can be obtained by laser light irradiation. The 10% weight reduction temperature of the gas generating layer refers to the temperature at the point in time when the weight of the gas generating layer decreases by 10% relative to the weight before heating (i.e., the weight of the gas generating layer becomes 90% relative to the weight before heating) in the TGA analysis when the adhesive sheet is heated (e.g., heated by laser light irradiation).
[0048] The thickness of the gas generating layer is preferably 0.1 μm to 50 μm, more preferably 1 μm to 40 μm, even more preferably 2 μm to 30 μm, and particularly preferably 5 μm to 20 μm. Within this range, an adhesive sheet capable of forming a better deformation portion can be obtained by laser light irradiation.
[0049] The above gas generating layer satisfies the following equation (1) with elastic modulus Er(gas) [unit: MPa] and thickness h(gas) [unit: μm] by nanoindentation method.
[0050] Log(Er(gas)×10 6 )≥8.01×h(gas) -0.116 … (1)
[0051] In the present invention, the gas generating layer is configured to satisfy the above equation (1), thereby preventing excessive deformation caused by the gas generated from the gas generating layer, and the adhesive sheet is deformed well by laser light irradiation. By forming such a gas generating layer, surface deformation within a minute range can be generated without placing a thick barrier layer (adhesive layer) as a layer to prevent excessive deformation, and the adhesive layer (gas barrier layer) can be flexibly configured.
[0052] In one embodiment, the elastic modulus Er(gas) [unit: MPa] and thickness h(gas) [unit: μm] obtained by the nanoindentation method satisfy the following formula (2). In one embodiment, the elastic modulus Er(gas) [unit: MPa] and thickness h(gas) [unit: μm] obtained by the nanoindentation method satisfy the following formula (3).
[0053] Log(Er(gas)×10 6 )≥7.66×h(gas) -0.092 … (2)
[0054] Log(Er(gas)×10 6 )≥7.52×h(gas) -0.081 … (3)
[0055] If it is within this range, the above effect becomes more pronounced.
[0056] In one embodiment, the elastic modulus Er(gas) [unit: MPa] and thickness h(gas) [unit: μm] by the nanoindentation method further satisfy the following formula (4).
[0057] Log(Er(gas)×10 6 )≤ 47.675×h(gas) -0.519 … (4)
[0058] The ultraviolet transmittance of the gas generating layer at a wavelength of 360 nm is preferably 30% or less, more preferably 20% or less, even more preferably 15% or less, particularly preferably 10% or less, and most preferably 5% or less. The lower limit of the ultraviolet transmittance of the gas generating layer at a wavelength of 360 nm is, for example, 0% (preferably 0.05%, more preferably 0.1%).
[0059] The haze value of the above gas generating layer is preferably 55% or less, more preferably 0.1% to 50%, and even more preferably 0.5% to 40%.
[0060] B-1. UV absorber
[0061] As the above-mentioned ultraviolet absorber, any suitable ultraviolet absorber may be used as long as the effects of the present invention are obtained. Examples of ultraviolet absorbers include benzotriazole-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, triazine-based ultraviolet absorbers, salicylate-based ultraviolet absorbers, cyanoacrylate-based ultraviolet absorbers, etc. Among these, preferably, it is a triazine-based ultraviolet absorber or a benzotriazole-based ultraviolet absorber, and particularly preferably, a triazine-based ultraviolet absorber. In particular, when an acrylic adhesive is used as adhesive A, a triazine-based ultraviolet absorber may be preferably used due to its high compatibility with the base polymer of the acrylic adhesive. It is more preferable that the triazine-based ultraviolet absorber be composed of a compound having a hydroxyl group, and it is particularly preferable that it be an ultraviolet absorber composed of a hydroxyphenyltriazine-based compound (hydroxyphenyltriazine-based ultraviolet absorber).
[0062] As hydroxyphenyltriazine-based UV absorbers, for example, the reaction product of 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl)-5-hydroxyphenyl and [(C10-C16 (mainly C12-C13)alkyloxy)methyl]oxirane (trade name "TINUVIN 400", manufactured by BASF), 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl]-5-[3-(dodecyloxy)-2-hydroxypropoxy]phenol, the reaction product of 2-(2,4-dihydroxyphenyl)-4,6-bis-(2,4-dimethylphenyl)-1,3,5-triazine and (2-ethylhexyl)-glycidic acid ester (trade name "TINUVIN 405", manufactured by BASF), 2,4-Bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-dibutoxyphenyl)-1,3,5-Triazine (Trade name "TINUVIN 460", manufactured by BASF), 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[(hexyl)oxy]-phenol (Trade name "TINUVIN 1577", manufactured by BASF), 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]-phenol (Trade name "Adecastab LA-46", manufactured by ADEKA Corp.), 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-Bis(4-phenylphenyl)-1,3,5-Triazine (Trade name Examples include "TINUVIN 479" (manufactured by BASF), and the BASF product name "TINUVIN 477".
[0063] Benzotriazole-based UV absorbers (benzotriazole compounds) include, for example, 2-(2-hydroxy-5-tert-butylphenyl)-2H-benzotriazole (trade name "TINUVIN PS", manufactured by BASF), ester compounds of benzenepropanoic acid and 3-(2H-benzotriazole-2-yl)-5-(1,1-dimethylethyl)-4-hydroxy(C7-9 side-chain and straight-chain alkyl) (trade name "TINUVIN 384-2", manufactured by BASF), octyl 3-[3-tert-butyl-4-hydroxy-5-(5-chloro-2H-benzotriazole-2-yl)phenyl]propionate and A mixture of 2-ethylhexyl-3-[3-tert-butyl-4-hydroxy-5-(5-chloro-2H-benzotriazole-2-yl)phenyl]propionate (trade name "TINUVIN 109", BASF), 2-(2H-benzotriazole-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (trade name "TINUVIN 900", BASF), 2-(2H-benzotriazole-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol (trade name "TINUVIN 928", BASF), and methyl 3-(3-(2H-benzotriazole-2-yl)-5-tert-butyl-4-hydroxyphenyl)propionate / polyethylene glycol 300 Product (trade name "TINUVIN 1130", manufactured by BASF), 2-(2H-benzotriazole-2-yl)-p-cresol (trade name "TINUVIN P", manufactured by BASF), 2-(2H-benzotriazole-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (trade name "TINUVIN 234", manufactured by BASF), 2-[5-chloro-2H-benzotriazole-2-yl]-4-methyl-6-(tert-butyl)phenol (trade name "TINUVIN 326", manufactured by BASF), 2-(2H-benzotriazole-2-yl)-4,6-di-tert-pentylphenol (trade name "TINUVIN 328", manufactured by BASF), 2-(2H-benzotriazole-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol (trade name "TINUVIN 329", manufactured by BASF), 2,2'-methylenebis[6-(2H-benzotriazole-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol](trade name "TINUVIN 360",BASF), reaction product of methyl 3-(3-(2H-benzotriazole-2-yl)-5-tert-butyl-4-hydroxyphenyl)propionate with polyethylene glycol 300 (trade name "TINUVIN 213", BASF), 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol (trade name "TINUVIN 571", BASF), 2-[2-hydroxy-3-(3,4,5,6-tetrahydrophthalimide-methyl)-5-methylphenyl]benzotriazole (trade name "Sumisorb 250", Sumitomo Chemical Corporation), 2-(3-tert-butyl-2-hydroxy-5-methylphenyl)-5-chloro-2H-benzotriazole (trade name "SEESORB") 703」, cipro gasseisasase), 2-(2H-benzotriazole-2-yl)-4-methyl-6-(3,4,5,6-tetrahydrophthalimidylmethyl)phenol (trade name "SEESORB 706", cipro gasseisasase), 2-(4-benzoyloxy-2-hydroxyphenyl)-5-chloro-2H-benzotriazole (trade name for cipro gasseisasase "SEESORB 7012BA"), 2-tert-butyl-6-(5-chloro-2H-benzotriazole-2-yl)-4-methylphenol (trade name "KEMISORB 73", chemipro gasseisasase), 2,2'-methylenebis[6-(2H-benzotriazole-2-yl)-4-tert-octylphenol] (trade name "Adecastab LA-31", Examples include ADEKA Co., Ltd.), 2-(2H-benzotriazole-2-yl)-p-cellulose (product name "Adecastab LA-32", ADEKA Co., Ltd.), 2-(5-chloro-2H-benzotriazole-2-yl)-6-tert-butyl-4-methylphenol (product name "Adecastab LA-36", ADEKA Co., Ltd.), etc.
[0064] The molecular weight of the compound constituting the above ultraviolet absorber is preferably 200 to 1500, more preferably 250 to 1200, and even more preferably 300 to 1000. Within this range, an adhesive sheet capable of forming a better deformation portion can be obtained by laser light irradiation.
[0065] The maximum absorption wavelength of the above ultraviolet absorber is preferably 300 nm to 450 nm, more preferably 320 nm to 400 nm, and even more preferably 330 nm to 380 nm.
[0066] The content ratio of the above-mentioned ultraviolet absorber is preferably 1 to 100 parts by weight, more preferably 1 to 50 parts by weight, and even more preferably 5 to 30 parts by weight, with respect to 100 parts by weight of the gas generating layer. Within this range, an adhesive sheet capable of forming a better deformation portion by laser light irradiation can be obtained.
[0067] B-2. Adhesive A
[0068] As adhesive A included in the gas generating layer, pressure-sensitive adhesive A is preferably used. Examples of adhesive A include acrylic adhesives, rubber adhesives, vinylalkyl ether adhesives, silicone adhesives, polyester adhesives, polyamide adhesives, urethane adhesives, styrene-diene block copolymer adhesives, etc. Among these, preferably, it is an acrylic adhesive or a rubber adhesive, and more preferably, an acrylic adhesive. In addition, the adhesive may be used alone or in combination of two or more types.
[0069] Examples of the above acrylic adhesives include acrylic adhesives having an acrylic polymer (homopolymer or copolymer) as a base polymer that uses one or more types of (meth)acrylate alkyl esters as monomer components. Specific examples of (meth)acrylate alkyl esters include (meth)acrylate methyl, (meth)acrylate ethyl, (meth)acrylate propyl, (meth)acrylate isopropyl, (meth)acrylate butyl, (meth)acrylate isobutyl, (meth)acrylate s-butyl, (meth)acrylate t-butyl, (meth)acrylate pentyl, (meth)acrylate hexyl, (meth)acrylate heptyl, (meth)acrylate octyl, (meth)acrylate 2-ethylhexyl, (meth)acrylate iso-octyl, (meth)acrylate nonyl, (meth)acrylate isononyl, (meth)acrylate decyl, (meth)acrylate isodecyl, (meth)acrylate undecyl, (meth)acrylate dodecyl, (meth)acrylate tridecyl. Examples of (meth)acrylate C1-20 alkyl esters include (meth)acrylate tetradecyl, (meth)acrylate pentadecyl, (meth)acrylate hexadecyl, (meth)acrylate heptadecyl, (meth)acrylate octadecyl, (meth)acrylate nonadecyl, (meth)acrylate eicosyl, etc. Among these, (meth)acrylate alkyl esters having a straight or branched alkyl group having 4 to 18 carbon atoms may be preferably used.
[0070] The above acrylic polymer may, for the purpose of modifying properties such as cohesiveness, heat resistance, and crosslinkability, include, if necessary, units corresponding to other monomer components copolymerizable with the above (meth)acrylate alkyl ester. As such monomer components, examples include carboxyl group-containing monomers such as acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid; acid anhydride monomers such as maleic anhydride and itaconic anhydride; Hydroxyl group-containing monomers such as (meth)acrylate hydroxyethyl, (meth)acrylate hydroxypropyl, (meth)acrylate hydroxybutyl, (meth)acrylate hydroxyhexyl, (meth)acrylate hydroxyoctyl, (meth)acrylate hydroxydecyl, (meth)acrylate hydroxylauryl, (4-hydroxymethylcyclohexyl)methyl methacrylate; sulfonic acid group-containing monomers such as styrenesulfonic acid, allylsulfonic acid, 2-(meth)acrylamide-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, sulfopropyl(meth)acrylate, (meth)acryloyloxynaphthalenesulfonic acid; (N-substituted)amide monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N-butyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methylolpropane(meth)acrylamide; (meth)acrylate aminoalkyl monomers such as (meth)acrylate aminoethyl, (meth)acrylate N,N-dimethylaminoethyl, (meth)acrylate t-butylaminoethyl; (meth)acrylate alkoxyalkyl monomers such as (meth)acrylate methoxyethyl, (meth)acrylate ethoxyethyl; maleimide monomers such as N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, N-phenylmaleimide; Taconimide-based monomers such as N-methyl itaconimide, N-ethyl itaconimide, N-butyl itaconimide, N-octyl itaconimide, N-2-ethylhexyl itaconimide, N-cyclohexyl itaconimide, N-lauryl itaconimide;Succinimide-based monomers such as N-(meth)acryloyloxymethylene succinimide, N-(meth)acryloyl-6-oxyhexamethylene succinimide, N-(meth)acryloyl-8-oxyoctamethylene succinimide; vinyl-based monomers such as vinyl acetate, vinyl propionate, N-vinylpyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, vinylmorpholine, N-vinylcarboxylic acid amides, styrene, α-methylstyrene, N-vinylcaprolactam; cyanoacrylate monomers such as acrylonitrile and methacrylonitrile; epoxy group-containing acrylic monomers such as (meth)acrylate glycidyl; Glycol-based acrylate monomers such as (meth)acrylate polyethylene glycol, (meth)acrylate polypropylene glycol, (meth)acrylate methoxyethylene glycol, (meth)acrylate methoxypolypropylene glycol, etc.; acrylic acid ester-based monomers having heterocyclic rings, halogen atoms, silicon atoms, etc., such as (meth)acrylate tetrahydrofurfuryl, fluorine (meth)acrylate, silicon (meth)acrylate, etc.; Examples include polyfunctional monomers such as hexanediol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, epoxy acrylate, polyester acrylate, and urethane acrylate; olefin monomers such as isoprene, butadiene, and isobutylene; and vinyl ether monomers such as vinyl ether. These monomer components may be used individually or in combination of two or more types.
[0071] Examples of the above rubber-based adhesives include, for instance, natural rubber; synthetic rubbers such as polyisoprene rubber, styrene-butadiene (SB) rubber, styrene-isoprene (SI) rubber, styrene-isoprene-styrene block copolymer (SIS) rubber, styrene-butadiene-styrene block copolymer (SBS) rubber, styrene-ethylene-butylene-styrene block copolymer (SEBS) rubber, styrene-ethylene-propylene-styrene block copolymer (SEPS) rubber, styrene-ethylene-propylene block copolymer (SEP) rubber, recycled rubber, butyl rubber, polyisobutylene, and modified products thereof; and rubber-based adhesives having the same as a base polymer.
[0072] The gas generated from the above gas generating layer is preferably a hydrocarbon (preferably an aliphatic hydrocarbon) gas. A gas generating layer capable of generating a hydrocarbon gas is composed, for example, of a hydrocarbon compound as the main component. It is preferable that the gas generating layer does not contain a compound containing a halogen element. If the generated gas is a hydrocarbon gas, corrosion of the electronic component to be processed can be prevented. This effect is made more pronounced by forming a gas generating layer that does not contain a compound containing a halogen element. The amount of ion generated from the gas generating layer is preferably 10 m / z to 800 m / z, more preferably 11 m / z to 700 m / z, even more preferably 12 m / z to 500 m / z, and particularly preferably 13 m / z to 400 m / z.
[0073] The above adhesive A may include any suitable additives as needed. Examples of such additives include crosslinking agents, tackifiers (e.g., rosin-based tackifiers, terpene-based tackifiers, hydrocarbon-based tackifiers, etc.), plasticizers (e.g., trimellitic acid ester-based plasticizers, pyromellitic acid ester-based plasticizers), pigments, dyes, anti-aging agents, conductive agents, antistatic agents, light stabilizers, release control agents, softeners, surfactants, flame retardants, antioxidants, etc.
[0074] Examples of the above-mentioned crosslinking agents include, in addition to isocyanate-based crosslinking agents, epoxy-based crosslinking agents, melamine-based crosslinking agents, and peroxide-based crosslinking agents, urea-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, carbodiimide-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, amine-based crosslinking agents, etc. Among these, preferably, it is an isocyanate-based crosslinking agent or an epoxy-based crosslinking agent.
[0075] Specific examples of the above isocyanate-based crosslinking agents include lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate; alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate, and isophorone diisocyanate; and aromatic isocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, and xylylene diisocyanate. Examples include isocyanate adducts such as trimethylolpropane / tolylene diisocyanate trimer adduct (manufactured by Nippon Polyurethane Kogyo Co., Ltd., trade name "Coronate L"), trimethylolpropane / hexamethylene diisocyanate trimer adduct (manufactured by Nippon Polyurethane Kogyo Co., Ltd., trade name "Coronate HL"), and isocyanurate of hexamethylene diisocyanate (manufactured by Nippon Polyurethane Kogyo Co., Ltd., trade name "Coronate HX"). The content of the isocyanate-based crosslinking agent can be set to any appropriate amount depending on the desired adhesive strength, and is typically 0.1 to 20 parts by weight, and more preferably 0.5 to 10 parts by weight, per 100 parts by weight of base polymer.
[0076] As the above-mentioned epoxy-based crosslinking agent, for example, N,N,N',N'-tetraglycidyl-m-xylenediamine, diglycidylaniline, 1,3-bis(N,N-glycidylaminomethyl)cyclohexane (manufactured by Mitsubishi Gas Corporation, trade name "Tetrad C"), 1,6-hexanediol diglycidyl ether (manufactured by Kyoesa Corporation, trade name "Epolite 1600"), neopentyl glycol diglycidyl ether (manufactured by Kyoesa Corporation, trade name "Epolite 1500NP"), ethylene glycol diglycidyl ether (manufactured by Kyoesa Corporation, trade name "Epolite 40E"), propylene glycol diglycidyl ether (manufactured by Kyoesa Corporation, trade name "Epolite 70P"), polyethylene glycol diglycidyl ether (manufactured by Nippon Yoshida, trade name "Epiol E-400"), Polypropylene glycol diglycidyl ether (manufactured by Nippon Yushi Co., Ltd., trade name "Epiol P-200"), sorbitol polyglycidyl ether (manufactured by Nagase Chemtex, trade name "Denacol EX-611"), glycerol polyglycidyl ether (manufactured by Nagase Chemtex, trade name "Denacol EX-314"), pentaerythritol polyglycidyl ether, polyglycerol polyglycidyl ether (manufactured by Nagase Chemtex, trade name "Denacol EX-512"), sorbitan polyglycidyl ether, trimethylolpropane polyglycidyl ether, adipic acid diglycidyl ester, o-phthalic acid diglycidyl ester, triglycidyl-tris(2-hydroxyethyl)isocyanurate, resorcinol diglycidyl ether, bisphenol-S-diglycidyl ether, epoxy resin having two or more epoxy groups within the molecule Examples include the above. The content of the epoxy crosslinking agent can be set to any appropriate amount depending on the desired adhesive strength, and is typically 0.01 to 10 parts by weight and more preferably 0.03 to 5 parts by weight per 100 parts by weight of the base polymer.
[0077] C. Adhesive layer
[0078] The above adhesive layer comprises any suitable adhesive B. As adhesive B, it may be a pressure-sensitive adhesive B1 or a curable adhesive B2.
[0079] The thickness of the adhesive layer is preferably 0.1 μm to 50 μm, more preferably 0.5 μm to 40 μm, even more preferably 1 μm to 30 μm, and particularly preferably 2 μm to 20 μm. Within this range, an adhesive layer having desirable adhesive strength and functioning well as a gas barrier layer can be formed.
[0080] The water vapor permeability of the adhesive layer is preferably 20,000 g / (m²·day) or less, more preferably 10,000 g / (m²·day) or less, even more preferably 7,000 g / (m²·day) or less, even more preferably 5,000 g / (m²·day) or less, even more preferably 4,800 g / (m²·day) or less, and particularly preferably 4,500 g / (m²·day) or less. Within this range, the adhesive layer functions well as a gas barrier layer, and a deformation portion with excellent shape is formed. By using such an adhesive sheet, small substrates (e.g., electronic components) can be peeled off with high precision. It is preferable for the water vapor permeability of the adhesive layer to be as low as possible, but the lower limit is, for example, 100 g / (m²·day).
[0081] The piercing strength of the adhesive layer is preferably 10 mN to 3000 mN, more preferably 30 mN to 2500 mN, even more preferably 50 mN to 2000 mN, and particularly preferably 100 mN to 2000 mN. Within this range, the adhesive layer functions well as a gas barrier layer, and shape changes due to gas generation occur preferably, and as a result, a deformation portion with an excellent shape is formed. By using such an adhesive sheet, small substrates (e.g., electronic components) can be peeled off with high precision.
[0082] The ultraviolet transmittance of the adhesive layer at a wavelength of 360 nm is preferably 50% to 100%, and more preferably 60% to 95%.
[0083] C-1. Pressure-sensitive adhesive B1
[0084] Examples of the pressure-sensitive adhesive B1 include, for instance, acrylic adhesives, rubber adhesives, vinylalkyl ether adhesives, silicone adhesives, polyester adhesives, polyamide adhesives, urethane adhesives, styrene-diene block copolymer adhesives, etc. Among these, preferably, it is an acrylic adhesive or a rubber adhesive, and more preferably, an acrylic adhesive. As the adhesive B1 included in the adhesive layer containing the pressure-sensitive adhesive, the adhesive described in Clause B-2 may be used.
[0085] C-2. Curable adhesive B2
[0086] Examples of curable adhesive B2 include thermosetting adhesives and active energy beam curing adhesives. Preferably, an active energy beam curing adhesive is used. The adhesive layer formed by the active energy beam curing adhesive is an adhesive layer formed by irradiating active energy beams, that is, an adhesive layer having a predetermined adhesive strength after irradiation with active energy beams.
[0087] As resin materials constituting the above active energy beam curable adhesive, examples include resin materials described in the UV curing system (Kiyomi Kato, published by the Comprehensive Technology Center (1989)), photocuring technology (compiled by the Technical Information Association (2000)), Japanese Patent Publication No. 2003-292916, and Japanese Patent No. 4151850. More specifically, examples include a resin material (B2-1) comprising a polymer that serves as a matrix and an active energy beam reactive compound (monomer or oligomer), and a resin material (B2-2) comprising an active energy beam reactive polymer.
[0088] Examples of polymers that serve as the above matrix include rubber-based polymers such as natural rubber, polyisobutylene rubber, styrene-butadiene rubber, styrene-isoprene-styrene block copolymer rubber, recycled rubber, butyl rubber, polyisobutylene rubber, and nitrile rubber (NBR); silicone-based polymers; acrylic-based polymers, etc. These polymers may be used alone or in combination of two or more types.
[0089] Examples of the above-mentioned active energy beam reactive compounds include photoreactive monomers or oligomers having multiple functional groups having carbon-carbon multiple bonds, such as acryloyl groups, methacryloyl groups, vinyl groups, allyl groups, and acetylene groups. Among these, compounds having ethylenically unsaturated functional groups are preferably used, and (meth)acrylic compounds having ethylenically unsaturated functional groups are more preferably used. Since compounds having ethylenically unsaturated functional groups readily generate radicals when exposed to ultraviolet rays, using said compounds allows for the formation of an adhesive layer that can be cured in a short time. Additionally, using (meth)acrylic compounds having ethylenically unsaturated functional groups allows for the formation of an adhesive layer having appropriate hardness after curing. Specific examples of photoreactive monomers or oligomers include compounds containing (meth)acryloyl groups, such as trimethylolpropane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol monohydroxypenta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, polyethylene glycol di(meth)acrylate, and urethane (meth)acrylate-based compounds; 2 to 5mers of said (meth)acryloyl group-containing compounds; etc. These compounds may be used alone or in combination of two or more types.
[0090] In addition, as the above active energy beam reactive compound, monomers such as epoxidized butadiene, glycidyl methacrylate, acrylamide, vinylsiloxane, etc.; or oligomers composed of said monomers may be used. A resin material (B2-1) containing these compounds can be cured by high energy beams such as ultraviolet rays or electron beams.
[0091] In addition, as the above-mentioned active energy beam reactive compound, a mixture of organic salts such as onium salts and a compound having multiple heterocyclic rings in its molecule may be used. In the mixture, upon irradiation with an active energy beam (e.g., ultraviolet rays, electron beams), the organic salts cleave to generate ions, which act as initiating species to cause a ring-opening reaction of the heterocyclic rings, thereby forming a three-dimensional network structure. Examples of the above-mentioned organic salts include iodonium salts, phosphonium salts, antimonium salts, sulfonium salts, borate salts, etc. Examples of the heterocyclic rings in the compound having multiple heterocyclic rings in its molecule include oxirane, oxetane, oxolane, tyran, aziridine, etc.
[0092] In the resin material (B2-1) comprising the above-mentioned polymer that serves as the base material and an active energy beam reactive compound, the content ratio of the active energy beam reactive compound is preferably 0.1 to 500 parts by weight, more preferably 1 to 300 parts by weight, and even more preferably 10 to 200 parts by weight, with respect to 100 parts by weight of the polymer that serves as the base material.
[0093] Examples of the above active energy beam reactive polymers include polymers having active energy beam reactive functional groups having carbon-carbon multiple bonds, such as acryloyl groups, methacryloyl groups, vinyl groups, allyl groups, and acetylene groups. Preferably, a compound (polymer) having an ethylenically unsaturated functional group is used, and more preferably, a (meth)acrylic polymer having an acryloyl group or a methacryloyl group is used. Specific examples of polymers having active energy beam reactive functional groups include polymers composed of polyfunctional (meth)acrylates. The polymer composed of the polyfunctional (meth)acrylate preferably has an alkyl ester having 4 or more carbon atoms in its side chain, more preferably has an alkyl ester having 6 or more carbon atoms, even more preferably has an alkyl ester having 8 or more carbon atoms, particularly preferably has an alkyl ester having 8 to 20 carbon atoms, and most preferably has an alkyl ester having 8 to 18 carbon atoms.
[0094] The resin material (B2-2) containing the above active energy beam reactive polymer may further contain the above active energy beam reactive compound (monomer or oligomer).
[0095] The above active energy beam curable adhesive can be cured by irradiation with active energy beams. In the adhesive sheet of the present invention, the substrate can be adhered before the adhesive is cured, and then the adhesive can be cured by irradiating with active energy beams. Examples of active energy beams include gamma rays, ultraviolet rays, visible light, infrared rays (heat rays), radio waves, alpha rays, beta rays, electron beams, plasma, ionizing rays, particle beams, etc. Conditions such as the wavelength and irradiation dose of the active energy beam can be set to any appropriate condition depending on the type of resin material used. For example, the adhesive can be cured by irradiating with ultraviolet rays having an irradiation dose of 10 to 1000 mJ / cm².
[0096] D. Intermediate layer
[0097] Examples of the form of the above intermediate layer include a resin layer, an adhesive layer, etc.
[0098] In one embodiment, the intermediate layer comprises a thermoplastic resin. Such an intermediate layer may be a resin film comprising a thermoplastic resin, a layer comprising an adhesive C composed of a thermoplastic resin, etc. In another embodiment, the intermediate layer comprises a curable resin (e.g., a UV-curing resin, a thermosetting resin). Such an intermediate layer may be a resin film comprising a curable resin, a layer comprising a curable adhesive D, etc.
[0099] The thickness of the intermediate layer is preferably 0.1 μm to 50 μm, more preferably 1 μm to 40 μm, and even more preferably 1.5 μm to 30 μm. Within this range, an intermediate layer that functions well as a gas barrier layer can be formed.
[0100] The water vapor permeability of the intermediate layer is preferably 5000 g / (m²·day) or less, more preferably 4800 g / (m²·day) or less, even more preferably 4500 g / (m²·day) or less, and even more preferably 4200 g / (m²·day) or less. Within this range, the intermediate layer functions well as a gas barrier layer, and a deformation portion with an excellent shape is formed. By using such an adhesive sheet, small substrates (e.g., electronic components) can be peeled off with high precision. It is preferable for the water vapor permeability of the intermediate layer to be as low as possible, but the lower limit is, for example, 0.1 g / (m²·day).
[0101] The piercing strength of the intermediate layer is preferably 300 mN to 5000 mN, more preferably 500 mN to 4500 mN, and even more preferably 1000 mN to 4000 mN. Within this range, the intermediate layer functions well as a gas barrier layer, and shape changes due to gas generation occur preferably, and as a result, a deformation portion with an excellent shape is formed. By using such an adhesive sheet, small substrates (e.g., electronic components) can be peeled off with high precision.
[0102] The ultraviolet transmittance of the above intermediate layer at a wavelength of 360 nm is preferably 50% to 100%, and more preferably 60% to 95%.
[0103] D-1. Intermediate layer as a resin layer
[0104] The intermediate layer as a resin layer is formed, for example, as a resin film. Examples of resins forming said resin film include polyethylene terephthalate-based resins, polyolefin-based resins, styrene-based elastomer resins (e.g., SEBS, etc.), UV-curing resins, thermosetting resins, urethane-based resins, epoxy-based resins, etc. In one embodiment, said resin film is composed of a thermoplastic resin.
[0105] The thickness of the resin film is preferably 0.1 μm to 50 μm, more preferably 0.5 μm to 30 μm, and even more preferably 1 μm to 20 μm.
[0106] D-2. Intermediate layer as an adhesive layer
[0107] Examples of intermediate layers having adhesive properties include intermediate layers containing pressure-sensitive adhesives and intermediate layers containing curable adhesives. Preferably, an intermediate layer containing curable adhesive D is disposed. In particular, as an adhesive layer, an adhesive layer containing pressure-sensitive adhesive A and an intermediate layer containing curable adhesive D are combined to obtain an adhesive sheet capable of forming a better deformable portion upon laser light irradiation. As the curable adhesive D, the adhesive described in Clause C-2 may be used.
[0108] The thickness of the intermediate layer as an adhesive layer is preferably 5 μm to 50 μm, and more preferably 5 μm to 30 μm.
[0109] E. Method for manufacturing adhesive sheets
[0110] The adhesive sheet of the present invention can be manufactured by any suitable method. For example, the adhesive sheet of the present invention may be manufactured by a method in which a gas generating layer is formed by directly coating a composition for forming a gas generating layer, comprising adhesive A and a UV absorber, onto a predetermined substrate to form a gas generating layer, and then coating a composition for forming an adhesive layer, comprising adhesive B, onto the gas generating layer to form an adhesive layer. In one embodiment, when the adhesive sheet has an intermediate layer, the intermediate layer is formed by coating a composition for forming an intermediate layer onto the gas generating layer before forming the adhesive layer, and then the adhesive layer is formed by coating a composition for forming an adhesive layer onto the intermediate layer. Alternatively, the adhesive sheet may be formed by bonding the layers after forming each layer separately.
[0111] Any suitable coating method may be employed as the coating method of the above composition. For example, each layer may be formed by drying after coating. Examples of coating methods include using a multicoater, die coater, gravure coater, applicator, etc. Examples of drying methods include natural drying, heat drying, etc. When heat drying, the heating temperature may be set to any suitable temperature depending on the characteristics of the material to be dried. In addition, active energy irradiation (e.g., ultraviolet irradiation) may be performed depending on the shape of each layer.
[0112] F. Processing Methods for Electronic Components
[0113] The electronic component processing method of the present invention comprises adhering an electronic component to the adhesive sheet, irradiating the adhesive sheet with a laser light, and peeling off the electronic component from the adhesive sheet. Examples of electronic components include semiconductor chips, LED chips, MLCCs, etc.
[0114] The peeling of the above electronic components can be performed selectively by position. Specifically, the peeling of electronic components can be performed by bonding and fixing a plurality of electronic components to an adhesive sheet, peeling off a part of the electronic components, and keeping the other electronic components fixed.
[0115] In one embodiment, the electronic component processing method of the present invention comprises attaching an electronic component to an adhesive sheet and, before peeling the electronic component from the adhesive sheet, performing a predetermined treatment on the electronic component. The treatment is not particularly limited and may include, for example, grinding, dicing, die bonding, wire bonding, etching, deposition, molding, circuit formation, inspection, quality inspection, cleaning, transfer, arrangement, repair, protection of the device surface, etc.
[0116] The size of the above electronic component (area of the bonding surface) is, for example, 1㎛ 2 to 250,000㎛ 2 is. In one embodiment, the size of the electronic component (area of the bonding surface) is 1 μm. 2 to 6400㎛ 2 The electronic component can be provided for processing. In another embodiment, the size of the electronic component (area of the bonding surface) is 1 μm 2 to 2500㎛ 2 The electronic components of can be provided for processing.
[0117] In one embodiment, as described above, a plurality of electronic components may be placed on an adhesive sheet. The spacing between the electronic components is, for example, 1 μm to 500 μm. The present invention is advantageous in that the spacing can be narrowed to temporarily fix the workpiece.
[0118] For example, UV laser light may be used as the laser light. The irradiation output of the laser light is, for example, 1 μJ to 1000 μJ. The wavelength of the UV laser light is, for example, 240 nm to 380 nm.
[0119] In one embodiment, the method for processing the electronic component includes placing the electronic component on another sheet (e.g., adhesive sheet, substrate, etc.) after peeling off the electronic component.
[0120] Examples
[0121] The present invention will be specifically described below by way of examples, but the present invention is not limited by these examples. The evaluation method in the examples is as follows. In addition, for the following evaluation, an adhesive sheet with the separator peeled off was used. Also, in the examples, unless specifically stated otherwise, "parts" and "%" are based on weight.
[0122] (1) Transmittance
[0123] In the case of an adhesive sheet having an intermediate layer, the adhesive sheet was set in a spectrophotometer (product name "UV-VIS Ultraviolet-Visible Spectrophotometer SolidSpec3700", manufactured by Shimadzu Seisakusho Co., Ltd.), incident light was directed perpendicularly to the gas barrier layer side of the sample, and the light transmittance in the wavelength range of 300 nm to 800 nm was measured. The transmittance at a wavelength of 360 nm was extracted from the obtained transmission spectrum. In the case of an adhesive sheet consisting only of an adhesive layer, the sheet was set in a spectrophotometer with one release liner left on and measured; then, the transmission spectrum of the release liner alone was measured and subtracted to obtain the transmission spectrum of the adhesive layer alone. The transmittance at a wavelength of 360 nm was extracted from the obtained transmission spectrum.
[0124] (2) Maximum gas generation peak temperature
[0125] Approximately 0.5 mg of adhesive sheet sample was set in a furnace-type pyrolysis unit, and a mass chromatogram was obtained by mass spectrometry of the volatilized components after heating. The temperature was raised from 40°C to 500°C at a heating rate of 10°C / min using a furnace-type pyrolysis unit (manufactured by Frontier Research Co., Ltd., product name "PY2020iD"), and the maximum gas generation peak temperature was calculated from the mass chromatogram with a mass range of m / z = 10 to 800 using a GC / MS analysis device (manufactured by JEOL, product name "JMS-T100GCV").
[0126] (3) Gasification initiation temperature
[0127] By the same method as in (2) above, the adhesive sheet was heated, and the gas generation temperature rise calculated from EGA analysis was set as the gasification initiation temperature. The gas generation temperature rise is defined as the temperature at which half of the maximum gas generation peak of the EGA / MS chromatogram obtained from EGA analysis is reached.
[0128] (4) Types of generated gas
[0129] An adhesive sheet sample was set in an automatic sample combustion device (manufactured by Mitsubishi Chemical Analytica, product name “AQF-2100H”) and heated at 400°C for 30 minutes to collect the generated gas. The species of the generated gas was identified by analyzing the collected liquid by ion chromatography.
[0130] (5) 5% weight loss temperature
[0131] Using a differential thermal analysis device (manufactured by TA Instruments, product name “Discovery TGA”), the temperature at which the weight of the adhesive sheet decreased by 5% was measured at a temperature of 10℃ / min, under an N2 atmosphere, and at a flow rate of 25ml / min.
[0132] (6) 10% weight loss temperature
[0133] Using a differential thermal analysis device (manufactured by TA Instruments, product name “Discovery TGA”), the temperature at which the weight of the adhesive sheet decreased by 10% was measured at a temperature of 10℃ / min, under an N2 atmosphere, and at a flow rate of 25ml / min.
[0134] For each of the adhesive sheet and the gas generating layer (UV absorber), the 10% weight loss temperature was measured.
[0135] (7) Water vapor permeability
[0136] A measurement sample was prepared by attaching the sample to cover the opening of an Al jig having a 10 mm × 10 mm opening, and the measurement sample was placed between the first and second chambers of a water vapor permeability measuring device (manufactured by MOCON, product name “PERMATRAN-W3 / 34G”) and evaluated by the MOCON measurement method. The temperature and humidity conditions were set to 30℃ / 90%RH, the gas (water vapor) flow rate was set to 10.0 ± 0.5 cc / min, and the measurement time was set to 20 hours.
[0137] Water vapor permeability was measured for each of the adhesive sheet, adhesive layer, and intermediate layer.
[0138] (8) Changes in surface shape
[0139] A measurement sample was obtained by bonding a glass plate (Matsunami Glass Co., Ltd., large slide glass S9112 (standard large white polishing No. 2)) to the gas generation layer side (opposite side to the adhesive layer) of the adhesive sheet. From the glass plate side of the measurement sample, a UV laser light with a wavelength of 355 nm and a beam diameter of approximately 20 μmφ was pulsed at 0.80 mW output and a frequency of 40 kHz, and gas was generated from the gas generation layer. The surface of the adhesive layer corresponding to any single spot of the pulsed scan was observed with a confocal laser microscope 1 minute after laser light irradiation, and the vertical displacement Y and horizontal displacement X (diameter; half full width) were measured.
[0140] When displacement Y is 8㎛ or greater, peelability is significantly excellent (◎ in the table); when displacement Y is 0.6㎛ or greater and less than 8㎛, peelability is good (○ in the table); when displacement Y is less than 0.6㎛, peelability is insufficient (× in the table).
[0141] (9) Adhesion (gas generating layer side)
[0142] A measurement sample was obtained by bonding PET#25 to the adhesive layer side of the adhesive sheet. The adhesion strength of the measurement sample to SUS430 on the gas generating layer side was measured by a method in accordance with JIS Z 0237:2000 (bonding conditions: 1 reciprocating of a 2 kg roller, tensile speed: 300 mm / min, peel angle 180°).
[0143] (10) Adhesion (adhesive layer)
[0144] A measurement sample was obtained by bonding PET#25 to the gas generating layer side of the adhesive sheet. The adhesion strength of the adhesive layer side of the measurement sample to SUS430 was measured by a method in accordance with JIS Z 0237:2000 (bonding conditions: 1 reciprocating of a 2 kg roller, tensile speed: 300 mm / min, peel angle 180°).
[0145] (11) In-plane uniformity of deformation
[0146] UV laser light was irradiated onto the gas generating layer as in (8) above.
[0147] A randomly selected deformed area of 2 mm × 2 mm was observed under a microscope, and if 90% or more of the convex parts were of the same size, it was classified as good (○ in the table); if 80% or more but less than 90% of the convex parts were of the same size, it was classified as good (△ in the table); and if less than 80% of the convex parts were of the same size, it was classified as poor (× in the table). "Same size" means that the difference in displacement X is within ±20%.
[0148] (12) Position selectivity of deformation
[0149] UV laser light was irradiated onto the gas generating layer as in (8) above.
[0150] Cases where only the laser irradiation part was deformed were considered Pass (○), and cases where multiple deformations occurred around the laser irradiation part were considered Failure (×).
[0151] (13) Elasticity
[0152] Using a nanoindenter (Triboindenter TI-950 manufactured by Hysitron Inc.), the elastic modulus of the cross-section of the gas generating layer was measured by a single indentation method at a predetermined temperature (25℃) under measurement conditions of an indentation speed of about 500 nm / sec, a drawing speed of about 500 nm / sec, and an indentation depth of about 1500 nm.
[0153] [Preparation Example 1] Preparation of adhesive a
[0154] In toluene, 30 parts by weight of 2-ethylhexyl acrylate, 70 parts by weight of ethyl acrylate, 4 parts by weight of 2-hydroxyethyl acrylate, 5 parts by weight of methyl methacrylate, and 0.2 parts by weight of benzoyl peroxide as a polymerization initiator were added, and then heated to 70°C to obtain a toluene solution of an acrylic copolymer (polymer A).
[0155] Adhesive a was prepared by mixing a toluene solution of polymer A (polymer A: 100 parts by weight), 3 parts by weight of an isocyanate-based crosslinking agent (manufactured by Nippon Polyurethane Co., Ltd., trade name "Coronate L"), and 5 parts by weight of a surfactant (manufactured by Kao Co., Ltd., trade name "Exepal IPP"). The composition of adhesive a is shown in Table 1.
[0156] [Preparation Example 2] Preparation of adhesive b
[0157] 95 parts by weight of 2-ethylhexyl acrylate, 5 parts by weight of acrylic acid, and 0.15 parts by weight of benzoyl peroxide as a polymerization initiator were added to ethyl acetate, and then heated to 70°C to obtain an ethyl acetate solution of an acrylic copolymer (polymer A2).
[0158] Adhesive b was prepared by mixing an ethyl acetate solution of polymer A2 (polymer A2: 100 parts by weight), 1 part by weight of an epoxy-based crosslinking agent (manufactured by Mitsubishi Gas Chemical Co., Ltd., trade name "TETRAD-C"), and 3 parts by weight of an isocyanate-based crosslinking agent (manufactured by Nippon Polyurethane Co., Ltd., trade name "Coronate L"). The composition of adhesive b is shown in Table 1.
[0159] [Preparation Example 3] Preparation of Adhesive I
[0160] Adhesive I was prepared in the same manner as in Preparation Example 1, except that the amount of crosslinking agent was 1 part by weight and no surfactant was included. The composition of Adhesive I is shown in Table 1.
[0161] [Preparation Example 3'] Preparation of adhesive c
[0162] Adhesive I was prepared in the same manner as in Preparation Example 2, except that the amount of isocyanate-based crosslinking agent was 1 part by weight and the amount of epoxy-based crosslinking agent was 0.4 parts by weight. The composition of Adhesive I is shown in Table 1.
[0163]
[0164] [Preparation Example 4] Preparation of composition a for forming an intermediate layer
[0165] 30 parts by weight of 2-ethylhexyl acrylate, 70 parts by weight of methyl acrylate, 10 parts by weight of acrylic acid, and 0.2 parts by weight of benzoyl peroxide as a polymerization initiator were added to ethyl acetate, and then heated to 70°C to obtain an ethyl acetate solution of an acrylic copolymer (polymer B).
[0166] Composition a for forming an intermediate layer was prepared by mixing an ethyl acetate solution of polymer B (polymer B: 100 parts by weight), 1 part by weight of an epoxy crosslinking agent (manufactured by Mitsubishi Gas Chemical Co., Ltd., trade name "Tetrad C"), 50 parts by weight of a UV oligomer (manufactured by Mitsubishi Chemical Co., Ltd., trade name "Shiko UV-1700B"), and 3 parts by weight of a photopolymerization initiator (manufactured by BASF, trade name "Omnirad 127"). The composition of composition a for forming an intermediate layer is shown in Table 2.
[0167] [Preparation Example 5] Preparation of composition b for forming an intermediate layer
[0168] 100 parts by weight of a maleic acid-modified styrene-ethylene-butylene-styrene block copolymer (SEBS: styrene portion / ethylene-butylene portion (weight ratio) = 30 / 70, acid value: 10 (mg-CH3ONa / g), manufactured by Asahi Kasei Chemicals, trade name "Toughtec M1913"), 3 parts by weight of an epoxy-based crosslinking agent (manufactured by Mitsubishi Gas Chemicals, trade name "TETRAD-C"), 3 parts by weight of a fatty acid ester-based surfactant (manufactured by Kao, trade name "Exepal IPP", molecular weight: 298.5, number of carbon atoms in alkyl group: 16), and toluene as a solvent were mixed to obtain composition b for forming an intermediate layer. The composition of composition b for forming an intermediate layer is shown in Table 2.
[0169]
[0170] [Preparation Example 6] Preparation of composition a for forming a gas generating layer
[0171] Polymer A was obtained in the same manner as in Preparation Example 1.
[0172] Composition a for forming a gas generating layer was prepared by mixing a toluene solution of polymer A (polymer A: 100 parts by weight), 1.5 parts by weight of an isocyanate-based crosslinking agent (manufactured by Nippon Polyurethane Co., Ltd., trade name "Coronate L"), and 20 parts by weight of an ultraviolet absorber (manufactured by BASF, trade name "Tinuvin 477"). The composition of composition a for forming a gas generating layer is shown in Table 3.
[0173] [Preparation Example 7] Preparation of composition b for forming a gas generating layer
[0174] Composition b for forming a gas generating layer was prepared in the same manner as in Preparation Example 5, except that the amount of UV absorber was 10 parts by weight. The composition of composition b for forming a gas generating layer is shown in Table 3.
[0175] [Preparation Example 8] Preparation of composition c for forming a gas generating layer
[0176] Composition c for forming a gas generating layer was prepared in the same manner as in Preparation Example 5, except that 10 parts by weight of 2,4-bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-dibutoxyphenyl)-1,3,5-triazine (product name "TINUVIN 460", manufactured by BASF) was used as a UV absorber. The composition of composition c for forming a gas generating layer is shown in Table 3.
[0177] [Preparation Example 9] Preparation of composition d for forming a gas generating layer
[0178] Composition d for forming a gas generating layer was prepared in the same manner as in Preparation Example 5, except that 20 parts by weight of the reaction product of 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine-2-yl)-5-hydroxyphenyl and [(C10-C16 (mainly C12-C13)alkyloxy)methyl]oxirane (product name “TINUVIN 400”, manufactured by BASF) was used as a UV absorber. The composition of composition d for forming a gas generating layer is shown in Table 3.
[0179] [Preparation Example 10] Preparation of composition e for forming a gas generating layer
[0180] Composition e for forming a gas generating layer was prepared in the same manner as in Preparation Example 5, except that 20 parts by weight of 2-[5-chloro-2H-benzotriazole-2-yl]-4-methyl-6-(tert-butyl)phenol (product name "TINUVIN 326", manufactured by BASF) was used as a UV absorber. The composition of composition e for forming a gas generating layer is shown in Table 3.
[0181] [Preparation Example 11] Preparation of composition f for forming a gas generating layer
[0182] Polymer B was obtained in the same manner as in Preparation Example 3.
[0183] Composition f for forming a gas generating layer was prepared by mixing an ethyl acetate solution of polymer B (polymer B: 100 parts by weight), 1 part by weight of an isocyanate-based crosslinking agent (manufactured by Nippon Polyurethane Co., Ltd., trade name "Coronate L"), and 20 parts by weight of an ultraviolet absorber (manufactured by BASF, trade name "Tinuvin 477"). The composition of composition f for forming a gas generating layer is shown in Table 3.
[0184] [Preparation Example 12] Preparation of composition g for forming a gas generating layer
[0185] 95 parts by weight of 2-ethylhexyl acrylate, 5 parts by weight of acrylic acid, and 0.15 parts by weight of benzoyl peroxide as a polymerization initiator were added to ethyl acetate, and then heated to 70°C to obtain an ethyl acetate solution of an acrylic copolymer (polymer C).
[0186] Composition g for forming a gas generating layer was prepared by mixing an ethyl acetate solution of polymer C (polymer C: 100 parts by weight), 1 part by weight of an isocyanate-based crosslinking agent (manufactured by Nippon Polyurethane Co., Ltd., trade name "Coronate L"), and 20 parts by weight of an ultraviolet absorber (manufactured by BASF, trade name "Tinuvin 477"). The composition of composition g for forming a gas generating layer is shown in Table 3.
[0187] [Preparation Example 13] Preparation of composition h for forming a gas generating layer
[0188] 95 parts by weight of 2-ethylhexyl acrylate, 5 parts by weight of acrylic acid, and 0.15 parts by weight of benzoyl peroxide as a polymerization initiator were added to ethyl acetate, and then heated to 70°C to obtain an ethyl acetate solution of an acrylic copolymer (polymer C).
[0189] Composition h for forming a gas generating layer was prepared by mixing an ethyl acetate solution of polymer C (polymer C: 100 parts by weight), 0.1 parts by weight of an epoxy-based crosslinking agent (manufactured by Mitsubishi Gas Chemical Co., Ltd., trade name “TETRAD-C”), and 20 parts by weight of an ultraviolet absorber (manufactured by BASF, trade name “Tinuvin477”). The composition of composition h for forming a gas generating layer is shown in Table 3.
[0190] [Preparation Example 14] Preparation of composition i for forming a gas generating layer
[0191] 100 parts by weight of a maleic acid-modified styrene-ethylene-butylene-styrene block copolymer (SEBS: styrene portion / ethylene-butylene portion (weight ratio) = 30 / 70, acid value: 10 (mg-CH3ONa / g), manufactured by Asahi Kasei Chemicals, trade name "Tough Tec M1913"), 3 parts by weight of an epoxy-based crosslinking agent (manufactured by Mitsubishi Gas Chemicals, trade name "TETRAD-C"), 20 parts by weight of an ultraviolet absorber (manufactured by BASF, trade name "Tinuvin477"), and toluene as a solvent were mixed to prepare composition i for forming a gas generating layer. The composition of composition i for forming a gas generating layer is shown in Table 3.
[0192] [Preparation Example 15] Preparation of Composition I for Forming a Gas Generation Layer
[0193] Composition I for forming a gas generating layer was prepared in the same manner as in Preparation Example 5, except that no ultraviolet absorber was incorporated. The composition of Composition I for forming a gas generating layer is shown in Table 3.
[0194] [Preparation Example 16] Preparation of Composition I Containing Thermally Expandable Microspheres
[0195] Composition I containing thermally expandable microspheres was prepared in the same manner as in Preparation Example 5, except that no ultraviolet absorber was added, the amount of crosslinking agent was 1.4 parts by weight, 30 parts by weight of thermally expandable microspheres (manufactured by Matsumoto Yushi Seiyaku Co., Ltd., product name "Matsumoto Micro Sphere F-50D"), and 10 parts by weight of a terpene phenol-based tackifying resin (manufactured by Sumitomo Bakelite Co., Ltd., product name "Sumilite Resin PR51732") were added.
[0196] [Preparation Example 17] Preparation of Composition II Containing Thermally Expandable Microspheres
[0197] Composition II containing thermally expandable microspheres was prepared in the same manner as in Preparation Example 13, except that 20 parts by weight of a terpenephenol-based tackifying resin (manufactured by Yasuhara Chemical, product name "YS Polystar T160") was used instead of 10 parts by weight of a terpenephenol-based tackifying resin (manufactured by Sumitomo Bakelite, product name "Sumilite Resin PR51732").
[0198] [Preparation Example 14'] Preparation of composition j for forming a gas generating layer
[0199] 95 parts by weight of 2-ethylhexyl acrylate, 5 parts by weight of acrylic acid, and 0.15 parts by weight of benzoyl peroxide as a polymerization initiator were added to ethyl acetate, and then heated to 70°C to obtain an ethyl acetate solution of an acrylic copolymer (polymer C).
[0200] Composition j for forming a gas generating layer was prepared by mixing an ethyl acetate solution of polymer C (polymer C: 100 parts by weight), 1 part by weight of an isocyanate-based crosslinking agent (manufactured by Nippon Polyurethane Co., Ltd., trade name "Coronate L"), 0.1 part by weight of an epoxy-based crosslinking agent (manufactured by Mitsubishi Gas Chemical Co., Ltd., trade name "TETRAD-C"), and 10 parts by weight of an ultraviolet absorber (manufactured by BASF, trade name "TINUVIN 400"). The composition of composition j for forming a gas generating layer is shown in Table 3.
[0201] [Preparation Example 14] Preparation of composition k for forming a gas generating layer
[0202] Composition k for forming a gas generating layer was prepared in the same manner as in Preparation Example 14, except that the amount of UV absorber was 5 parts by weight. The composition of composition k for forming a gas generating layer is shown in Table 3.
[0203]
[0204] [Example 1]
[0205] Adhesive a obtained in Preparation Example 1 was applied to a polyethylene terephthalate film (thickness: 75 μm) having a silicone release agent-treated surface such that the thickness after solvent volatilization (drying) was 15 μm, and then dried to form an adhesive layer precursor layer a on the polyethylene terephthalate film.
[0206] Composition a for forming a gas generating layer obtained in Preparation Example 5 was applied to a polyethylene terephthalate film (manufactured by Toray, product name "Cerafil", thickness: 38 μm) having a silicone release agent-treated surface such that the thickness after solvent volatilization (drying) was 7 μm, and then dried to form a gas generating layer precursor layer a on the polyethylene terephthalate film.
[0207] The above adhesive layer precursor layer a and the above gas generating layer precursor layer a were laminated and bonded between rolls to obtain an adhesive sheet (adhesive layer / gas generating layer) fitted onto a polyethylene terephthalate film having a silicone release agent-treated surface.
[0208] The obtained adhesive sheets were provided to the evaluations (1) to (12) above. The results are shown in Table 4.
[0209] [Example 2]
[0210] Adhesive a obtained in Preparation Example 1 was applied to a polyethylene terephthalate film (thickness: 75 μm) having a silicone release agent-treated surface such that the thickness after solvent volatilization (drying) was 15 μm, and then dried to form an adhesive layer precursor layer a on the polyethylene terephthalate film.
[0211] Composition a for forming an intermediate layer obtained in Preparation Example 3 was applied to a polyethylene terephthalate film (manufactured by Toray, trade name "Cerafil", thickness: 38 μm) having a silicone release agent-treated surface such that the thickness after solvent volatilization (drying) was 15 μm, and then dried to form an intermediate layer precursor layer a on the polyethylene terephthalate film.
[0212] Next, the above adhesive layer precursor layer a and the above intermediate layer precursor layer a are laminated and bonded between rolls, UV irradiated at 500 mJ / ㎠ on the intermediate layer precursor layer side, and a laminated precursor layer a is obtained by being fitted onto a polyethylene terephthalate film having a silicone release agent treated surface.
[0213] Composition a for forming a gas generating layer obtained in Preparation Example 5 was applied to a polyethylene terephthalate film (manufactured by Toray, product name "Cerafil", thickness: 38 μm) having a silicone release agent-treated surface such that the thickness after solvent volatilization (drying) was 7 μm, and then dried to form a gas generating layer precursor layer a on the polyethylene terephthalate film.
[0214] After peeling off a polyethylene terephthalate film having a silicone release agent treated surface on the side of the intermediate layer precursor layer a of the laminate, the intermediate layer precursor layer a of the laminate and the gas generating layer precursor layer a are laminated and bonded between rolls to obtain an adhesive sheet (adhesive layer / intermediate layer / gas generating layer) fitted onto a polyethylene terephthalate film having a silicone release agent treated surface.
[0215] The obtained adhesive sheets were provided to the evaluations (1) to (12) above. The results are shown in Table 4.
[0216] [Example 3]
[0217] Adhesive a obtained in Preparation Example 1 was applied to a polyethylene terephthalate film (thickness: 75 μm) having a silicone release agent-treated surface such that the thickness after solvent volatilization (drying) was 15 μm, and then dried to form an adhesive layer precursor layer a on the polyethylene terephthalate film.
[0218] The intermediate layer forming composition b obtained in Preparation Example 4 was applied to a polyethylene terephthalate film (manufactured by Toray, product name "Cerafil", thickness: 38 μm) having a silicone release agent-treated surface such that the thickness after solvent volatilization (drying) was 15 μm, and then dried to form an intermediate layer precursor layer a on the polyethylene terephthalate film.
[0219] Next, the adhesive layer precursor a and the intermediate layer precursor b were laminated and bonded between rolls, and a laminated precursor b was obtained that was fitted onto a polyethylene terephthalate film having a silicone release agent treated surface.
[0220] Composition a for forming a gas generating layer obtained in Preparation Example 5 was applied to a polyethylene terephthalate film (manufactured by Toray, product name "Cerafil", thickness: 38 μm) having a silicone release agent-treated surface such that the thickness after solvent volatilization (drying) was 7 μm, and then dried to form a gas generating layer precursor layer a on the polyethylene terephthalate film.
[0221] After peeling off a polyethylene terephthalate film having a silicone release agent treated surface on the side of the intermediate layer of the laminated precursor layer b, the intermediate layer of the laminated precursor layer b and the gas generating layer precursor layer a were laminated and bonded between rolls to obtain an adhesive sheet (adhesive layer / intermediate layer / gas generating layer) fitted onto a polyethylene terephthalate film having a silicone release agent treated surface.
[0222] The obtained adhesive sheets were provided to the evaluations (1) to (12) above. The results are shown in Table 4.
[0223] [Example 4]
[0224] Adhesive a obtained in Preparation Example 1 was applied to a polyethylene terephthalate film (thickness: 75 μm) having a silicone release agent-treated surface such that the thickness after solvent volatilization (drying) was 15 μm, and then dried to form an adhesive layer precursor layer a on the polyethylene terephthalate film.
[0225] Composition a for forming a gas generating layer obtained in Preparation Example 5 was applied to a polyethylene terephthalate film (manufactured by Toray, product name "Cerafil", thickness: 38 μm) having a silicone release agent-treated surface such that the thickness after solvent volatilization (drying) was 7 μm, and then dried to form a gas generating layer precursor layer a on the polyethylene terephthalate film.
[0226] The above adhesive layer precursor layer a was laminated and bonded to one side of a polyethylene terephthalate film (manufactured by Toray, product name "Lumirr #2F51N", thickness: 2㎛) in a roll-to-roll manner.
[0227] Next, the gas generating layer precursor layer a was laminated and bonded between rolls on the opposite side from the adhesive layer precursor layer a of the polyethylene terephthalate film.
[0228] In this way, an adhesive sheet (adhesive layer / intermediate layer / gas generating layer) sandwiched in a polyethylene terephthalate film having a silicone release agent-treated surface was obtained.
[0229] The obtained adhesive sheets were provided to the evaluations (1) to (12) above. The results are shown in Table 4.
[0230] [Example 5]
[0231] An adhesive sheet was obtained in the same manner as in Example 4, except that composition b for forming a gas generating layer was used instead of composition a for forming a gas generating layer. The obtained adhesive sheet was provided to the evaluations (1) to (12) above. The results are shown in Table 4.
[0232] [Example 6]
[0233] An adhesive sheet was obtained in the same manner as in Example 4, except that composition c for forming a gas generating layer was used instead of composition a for forming a gas generating layer. The obtained adhesive sheet was provided to the evaluations (1) to (12) above. The results are shown in Table 4.
[0234] [Example 7]
[0235] An adhesive sheet was obtained in the same manner as in Example 4, except that composition d for forming a gas generating layer was used instead of composition a for forming a gas generating layer. The obtained adhesive sheet was provided to the evaluations (1) to (12) above. The results are shown in Table 4.
[0236] [Example 8]
[0237] An adhesive sheet was obtained in the same manner as in Example 4, except that composition e for forming a gas generating layer was used instead of composition a for forming a gas generating layer. The obtained adhesive sheet was provided to the evaluations (1) to (12) above. The results are shown in Table 5.
[0238] [Example 9]
[0239] An adhesive sheet was obtained in the same manner as in Example 4, except that the thickness of the adhesive layer was 1 μm and the thickness of the gas generating layer was 10 μm. The obtained adhesive sheet was provided to the evaluations (1) to (12) above. The results are shown in Table 5.
[0240] [Example 10]
[0241] An adhesive sheet was obtained in the same manner as in Example 4, except that the thickness of the adhesive layer was 1 μm and the thickness of the gas generating layer was 15 μm. The obtained adhesive sheet was provided to the evaluations (1) to (12) above. The results are shown in Table 5.
[0242] [Example 11]
[0243] An adhesive sheet was obtained in the same manner as in Example 4, except that the thickness of the adhesive layer was 5 μm and the thickness of the gas generating layer was 5 μm. The obtained adhesive sheet was provided to the evaluations (1) to (12) above. The results are shown in Table 5.
[0244] [Example 12]
[0245] An adhesive sheet was obtained in the same manner as in Example 4, except that the thickness of the adhesive layer was 10 μm and the thickness of the gas generating layer was 5 μm. The obtained adhesive sheet was provided to the evaluations (1) to (12) above. The results are shown in Table 5.
[0246] [Example 13]
[0247] An adhesive sheet was obtained in the same manner as in Example 4, except that composition f for forming a gas generating layer was used instead of composition a for forming a gas generating layer. The obtained adhesive sheet was provided to the evaluations (1) to (12) above. The results are shown in Table 5.
[0248] [Example 14]
[0249] An adhesive sheet was obtained in the same manner as in Example 4, except that composition g for forming a gas generating layer was used instead of composition a for forming a gas generating layer. The obtained adhesive sheet was provided to the evaluations (1) to (12) above. The results are shown in Table 5.
[0250] [Example 15]
[0251] A gas generating layer was formed on one side of a polyethylene terephthalate film (manufactured by Toray, product name "Lumirr S10", thickness: 50㎛) by coating a gas generating layer forming composition h such that the thickness after solvent volatilization (drying) is 20㎛.
[0252] Next, adhesive b was coated onto a polyethylene terephthalate film (manufactured by Toray, product name "Cerafil", thickness: 38 μm) having a silicone release agent-treated surface, such that the thickness after solvent volatilization (drying) was 10 μm, thereby forming an adhesive layer.
[0253] Next, a gas generating layer and an adhesive layer were laminated to obtain an adhesive sheet (adhesive layer / gas generating layer / substrate) protected by a polyethylene terephthalate film having a silicone release agent treated surface.
[0254] The obtained adhesive sheet was provided for the above evaluation. The results are shown in Table 6.
[0255] [Example 16]
[0256] An adhesive sheet was obtained in the same manner as in Example 14, except that composition i for forming a gas generating layer was used instead of composition h for forming a gas generating layer. The obtained adhesive sheet was provided for the above evaluation. The results are shown in Table 6.
[0257] [Example 17]
[0258] A gas generating layer was formed on one side of a polyethylene terephthalate film (manufactured by Toray, product name "Lumirr S10", thickness: 50㎛) by coating it with a composition j for forming a gas generating layer so that the thickness after solvent volatilization (drying) is 20㎛.
[0259] Next, adhesive a was coated onto a polyethylene terephthalate film (manufactured by Toray, product name "Cerafil", thickness: 38 μm) having a silicone release agent-treated surface, such that the thickness after solvent volatilization (drying) was 5 μm, thereby forming an adhesive layer.
[0260] Next, a gas generating layer and an adhesive layer were laminated to obtain an adhesive sheet (adhesive layer / gas generating layer / substrate) protected by a polyethylene terephthalate film having a silicone release agent treated surface.
[0261] The obtained adhesive sheet was provided for the above evaluation. The results are shown in Table 6.
[0262] [Example 18]
[0263] An adhesive sheet was obtained in the same manner as in Example 17, except that composition k for forming a gas generating layer was used instead of composition j for forming a gas generating layer. The obtained adhesive sheet was provided for the above evaluation. The results are shown in Table 6.
[0264]
[0265]
[0266]
[0267] [Comparative Example 1]
[0268] An adhesive sheet was obtained in the same manner as in Example 4, except that composition I for forming a gas generating layer was used instead of composition a for forming a gas generating layer. The obtained adhesive sheet was provided to the evaluations (1) to (12) above. The results are shown in Table 7.
[0269] [Comparative Example 2]
[0270] An adhesive sheet was obtained in the same manner as in Example 4, except that adhesive I was used instead of adhesive a, the thickness of the adhesive layer was 10 μm, a PET film with a thickness of 188 μm was used as an intermediate layer, and a gas generating layer with a thickness of 48 μm was formed using thermally expandable microsphere-containing composition I instead of composition a for forming the gas generating layer. The obtained adhesive sheet was provided to the evaluations (1) to (12) above. The results are shown in Table 7.
[0271] [Comparative Example 3]
[0272] An adhesive sheet was obtained in the same manner as in Example 4, except that adhesive I was used instead of adhesive a, the thickness of the adhesive layer was 10 μm, a PET film with a thickness of 100 μm was used as an intermediate layer, and a composition containing thermally expandable microspheres II was used instead of composition a for forming a gas generating layer to form a gas generating layer with a thickness of 48 μm. The obtained adhesive sheet was provided to the evaluations (1) to (12) above. The results are shown in Table 7.
[0273] Explanation of the symbols
[0274] 10: Gas generating layer 20: Adhesive layer 30: Intermediate layer 100, 200: Adhesive sheet
Claims
Claim 1 An adhesive sheet comprising a gas generating layer and at least one adhesive layer disposed on one side of the gas generating layer, wherein the adhesive layer comprises a pressure-sensitive adhesive, and the adhesive layer is a layer whose surface is deformed by laser light irradiation to the adhesive sheet, wherein the amount of deformation of the surface of the adhesive layer by laser light irradiation to the adhesive sheet is 0.6 μm or more in vertical displacement of the adhesive layer, and the piercing strength of the adhesive layer is 10 mN to 3000 mN. Claim 2 An adhesive sheet according to claim 1, wherein the gas generating layer is a layer capable of absorbing ultraviolet rays. Claim 3 In paragraph 2, the adhesive sheet wherein the gas generating layer comprises a UV absorber. Claim 4 An adhesive sheet according to claim 1, wherein the thickness of the gas generating layer is 0.1㎛ to 50㎛. Claim 5 An adhesive sheet according to claim 1, wherein the gas generating layer is a layer that generates hydrocarbon gas. Claim 6 An adhesive sheet according to claim 1, wherein the gasification initiation temperature of the gas generating layer is 150°C to 500°C. Claim 7 In claim 1, the elastic modulus Er(gas) [unit: MPa] and thickness h(gas) [unit: μm] of the gas generating layer by the nanoindentation method satisfy the following formula (1), an adhesive sheet.Log(Er(gas)×10 6 )≥8.01×h(gas) -0.116 … (1) Claim 8 An adhesive sheet according to claim 1, wherein the thickness of the adhesive layer is 0.1㎛ to 50㎛. Claim 9 An adhesive sheet according to claim 1, having an ultraviolet transmittance of 30% or less at a wavelength of 360 nm. Claim 10 An adhesive sheet according to claim 1, wherein the 10% weight reduction temperature is 200℃ to 500℃. Claim 11 An adhesive sheet according to claim 1, having a water vapor permeability of 5000 g / (㎡·day) or less. Claim 12 A method for processing an electronic component, comprising bonding an electronic component onto an adhesive sheet described in claim 1, and irradiating a laser light onto the adhesive sheet to peel off the electronic component from the adhesive sheet. Claim 13 A method for processing electronic components according to claim 12, wherein the peeling of the electronic component is performed selectively by position. Claim 14 A method for processing an electronic component according to claim 12, comprising, after adhering the electronic component to the adhesive sheet, performing a predetermined treatment on the electronic component before peeling the electronic component from the adhesive sheet. Claim 15 A method for processing electronic components according to claim 14, wherein the above processing is grinding, dicing, die bonding, wire bonding, etching, deposition, molding, circuit formation, inspection, quality inspection, cleaning, transfer, arrangement, repair, or protection of the device surface. Claim 16 A method for processing an electronic component according to claim 12, comprising peeling the electronic component from the adhesive sheet and then placing the electronic component on another sheet.