Coating compositions containing bio-derived components and automotive interior materials comprising the same
A bio-derived paint composition with specific resin and curing agent formulations addresses the challenge of increasing biocarbon content in automotive interiors, ensuring durable and resistant film properties.
Patent Information
- Application Number
- KR1020250058069
- Authority / Receiving Office
- KR · KR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-02
- Publication Date
- 2026-11-10
AI Technical Summary
Existing paint compositions for automotive interiors face challenges in increasing biocarbon content while maintaining durability properties such as adhesion, sunscreen resistance, heat resistance, and light resistance due to the inferior physical properties of bio-resins compared to petroleum-derived resins.
A paint composition incorporating bio-derived acrylic resin and modified acrylic resin, along with a bio-derived isocyanate curing agent, is formulated to achieve a biocarbon content of 15% to 45% by weight, with specific ranges for acid value, hydroxyl value, glass transition temperature, and molecular weight to ensure excellent film properties.
The composition effectively increases biocarbon content while securing durability properties, achieving good adhesion, sunscreen resistance, heat resistance, and light resistance, meeting the requirements for automotive interior materials.
Smart Images

Figure PAT00001_ABST
Abstract
Description
Technology Field
[0001] The disclosed embodiments relate to a paint composition containing bio-derived components and an automotive interior material containing the same. Background Technology
[0002] With the recent rise in environmental concern, significant efforts are being made across various sectors to reduce carbon dioxide, which is identified as the primary culprit behind global warming. Consequently, bio-based raw materials are gaining attention as alternatives to conventional petroleum and coal resources.
[0003] Bio-based raw materials do not increase the amount of carbon dioxide in the atmosphere because the sum of carbon dioxide emissions and absorption in their life cycle on Earth is zero. Furthermore, they can be considered an essential choice not only for environmental issues but also to replace dwindling petroleum resources.
[0004] With the active development of eco-friendly vehicles, the need for automotive interior materials with a high content of bio-based raw materials is increasing. However, because bio-resins inherently possess inferior physical properties compared to petroleum-derived resins, it becomes difficult to secure the properties required for automotive interior materials—such as appearance, scratch resistance, sunscreen resistance, moisture resistance, and light resistance—as the bio-resin content increases.
[0005] It is necessary to develop a new paint composition that can secure durable properties, such as chemical resistance, required for automobiles, and increase the bio-carbon content within the paint. The problem to be solved
[0006] The disclosed embodiment aims to provide a paint composition capable of increasing the biocarbon content in the paint while securing the durability properties required for automobiles.
[0007] The disclosed embodiments aim to provide a paint composition having excellent film properties such as adhesion, sunscreen resistance, heat resistance, moisture resistance, and light resistance.
[0008] The purpose of the disclosed embodiments is not limited to the purposes mentioned above. The purpose of the disclosed embodiments will become more apparent from the following description and will be realized by the means and combinations thereof described in the claims. means of solving the problem
[0009] The paint composition according to the disclosed embodiment may include a bio-derived acrylic resin; and a bio-derived modified acrylic resin.
[0010] The above bio-derived acrylic resin may have a bio-carbon content of 30% to 35% by weight.
[0011] The acid value of the above bio-derived acrylic resin may be 2 mgKOH / g to 5 mgKOH / g.
[0012] The hydroxyl value of the above bio-derived acrylic resin may be 60 mgKOH / g to 80 mgKOH / g.
[0013] The glass transition temperature (Tg) of the above bio-derived acrylic resin may be 80°C to 100°C.
[0014] The weight-average molecular weight (Mw) of the above bio-derived acrylic resin may be 9,000 g / mol to 13,000 g / mol.
[0015] The solid content of the above bio-derived acrylic resin may be 40% to 50% by weight.
[0016] The above bio-derived acrylic resin may include a polymer of a bio-derived monomer comprising at least one of butyl acrylate, butyl methacrylate, ethyl acrylate, ethyl methacrylate, isobornyl acrylate, isobornyl methacrylate, isobutyl acrylate, isobutyl methacrylate, lauric acrylate, or lauric methacrylate.
[0017] The above bio-derived modified acrylic resin may have a bio-carbon content of 30% to 40% by weight.
[0018] The acid value of the above bio-derived modified acrylic resin may be 2 mgKOH / g or less.
[0019] The hydroxyl value of the above bio-derived modified acrylic resin may be 125 mgKOH / g to 145 mgKOH / g.
[0020] The glass transition temperature (Tg) of the above bio-derived modified acrylic resin may be 40°C to 50°C.
[0021] The weight-average molecular weight (Mw) of the above bio-derived modified acrylic resin may be 3,000 g / mol to 6,000 g / mol.
[0022] The solid content of the above bio-derived modified acrylic resin may be 60% to 80% by weight.
[0023] The above bio-derived modified acrylic resin may comprise a bio-derived monomer comprising at least one of butyl acrylate, butyl methacrylate, ethyl acrylate, ethyl methacrylate, isobornyl acrylate, isobornyl methacrylate, isobutyl acrylate, isobutyl methacrylate, lauric acrylate, or lauric methacrylate; and a polymer of a diol compound modified with maleic anhydride.
[0024] The paint composition further comprises a curing agent, and the curing agent may include a bio-derived isocyanate curing agent.
[0025] The paint composition comprises a main component and a curing agent, wherein the main component comprises 10% to 20% by weight of a base resin, 25% to 35% by weight of a bio-derived acrylic resin, 10% to 25% by weight of a bio-derived modified acrylic resin, 1% to 3% by weight of a pigment, 15% to 25% by weight of a solvent, and 5% to 20% by weight of an additive, and the paint composition may comprise 20% to 30% by weight of the curing agent based on 100% by weight of the main component.
[0026] The paint composition comprises a main component and a curing agent, wherein the main component comprises 30% to 45% by weight of a bio-derived acrylic resin, 15% to 25% by weight of a bio-derived modified acrylic resin, 25% to 40% by weight of a solvent, and 2% to 15% by weight of an additive, and the paint composition may comprise 20% to 30% by weight of the curing agent based on 100% by weight of the main component.
[0027] The paint composition may have a biocarbon content of 15% to 45% by weight.
[0028] An automotive interior material according to a disclosed embodiment comprises a substrate; and a multilayer coating layer positioned on the substrate; wherein the coating layer comprises a primer layer on the substrate; an intermediate layer on the primer layer; and a top layer on the intermediate layer, and at least one of the primer layer and the intermediate layer may comprise the paint composition. Effects of the invention
[0029] According to the disclosed embodiment, a paint composition can be obtained that can increase the content of biocarbon in the paint while securing the durability properties required for automobiles.
[0030] According to the disclosed embodiments, a paint composition with excellent film properties such as adhesion, sunscreen resistance, heat resistance, moisture resistance, and light resistance can be obtained.
[0031] The effects of the disclosed embodiments are not limited to those mentioned above. It should be understood that the effects of the disclosed embodiments include all effects that can be inferred from the following description. Brief explanation of the drawing
[0032] FIG. 1 illustrates an automotive interior material according to a disclosed embodiment. Specific details for implementing the invention
[0033] The purposes, other purposes, features, and advantages of the above-disclosed embodiments will be readily understood through the following preferred embodiments associated with the accompanying drawings. The disclosed embodiments may be embodied in other forms. Rather, the embodiments presented herein are provided to ensure that the disclosed content is thorough and complete, and to ensure that the spirit of the invention is sufficiently conveyed to a person skilled in the art.
[0034] In describing each drawing, similar reference numerals have been used for similar components. In the attached drawings, the dimensions of the structures are depicted enlarged from their actual size for clarity of the disclosed embodiments.
[0035] In this specification, terms such as "comprising" or "having" are intended to specify the existence of the features, numbers, steps, actions, components, parts, or combinations thereof described in the specification, and should be understood as not precluding the existence or addition of one or more other features, numbers, steps, actions, components, parts, or combinations thereof. Furthermore, when a part such as a layer, film, region, or plate is described as being "on" another part, this includes not only the case where it is "immediately above" the other part, but also the case where there is another part in between. Conversely, when a part such as a layer, film, region, or plate is described as being "below" another part, this includes not only the case where it is "immediately below" the other part, but also the case where there is another part in between.
[0036] Unless otherwise specified, all numbers, values, and / or expressions used herein to represent amounts of ingredients, reaction conditions, polymer compositions, and formulations should be understood to be modified by the term “approximately” in all cases, as these numbers are essentially approximations reflecting the various uncertainties of measurement that occur in obtaining these values among other things. Furthermore, where numerical ranges are disclosed herein, such ranges are continuous and, unless otherwise indicated, include all values from the minimum value of such range to the maximum value including said maximum value. Moreover, where such ranges refer to integers, they include all integers from the minimum value to said maximum value including said maximum value, unless otherwise indicated.
[0038] FIG. 1 is a cross-sectional view illustrating an automotive interior material according to a disclosed embodiment. The automotive interior material may include a substrate (10) and a multilayer coating layer (20) coated on the substrate (10).
[0039] The above material (10) may include acrylonitrile butadiene styrene, a copolymer of polycarbonate and acrylonitrile butadiene styrene, etc. The above material (10) may be injection molded.
[0040] The coating layer (20) may include a base layer (21) on the substrate (10), an intermediate layer (22) on the base layer (21), and a top layer (23) on the intermediate layer (22).
[0041] The above underlayer (21) can reinforce the surface of the substrate (10) and increase the adhesion between the substrate (10) and the coating layer (20). The above underlayer (21) can be provided by a hydraulic transfer method.
[0042] The above intermediate layer (22) is a layer that determines color, appearance, etc., and can provide resistance to environmental factors such as weather resistance and UV resistance to the coating layer (20). The above intermediate layer (22) may be a film.
[0043] The top layer (23) can form a visible appearance and protect the inner components from the external environment. The top layer (23) may be glossy or matte. The top layer (23) may be provided by a hydraulic transfer method.
[0044] A paint composition according to the disclosed embodiment may be applied to at least one of the above-mentioned undercoat layer (21) and topcoat layer (23).
[0045] The above paint composition may include a bio-derived acrylic resin, a bio-derived modified acrylic resin, a solvent, a curing agent, etc.
[0046] The above bio-derived acrylic resin may have a bio-carbon content of 30% to 35% by weight.
[0047] The above biocarbon content may have been measured using radiocarbon analysis techniques according to ASTM D6866 (% Biobased Carbon Content). Accurate biomass content can be measured through experiments in accordance with the ASTM D6866 standard. Radiocarbon (C), an isotope of carbon 14 ) exists only in biomass materials and not in petrochemical resins. The biocarbon content of a specimen can be calculated through the radiocarbon content of the specimen.
[0048] The above biocarbon content may be in accordance with EN 16640. The EN 16640 standard can also determine the ratio of bio-based and fossil-based carbon in a sample based on radiocarbon dating.
[0049] The above ASTM D6866 is the total organic carbon content (X B TOCCalculate ), and the above EN 16640 is the total carbon content (X B TC It may be calculating ). For example, when the composition of 10g of Product A is as shown in Table 1 below, the total organic carbon content (X according to ASTM D6866). B TOC ) is 25.9% (=1.5 / (1.5+4.3)), and the total carbon content according to EN 16640 (X B TC ) can be 24.8% (=1.5 / (1.5+4.3+0.24)). However, the following example is intended to show the difference between ASTM D6866 and EN 16640, and mostly the total organic carbon content (X according to ASTM D6866) B TOC ) and total carbon content according to EN 16640 (X B TC ) are the same as each other.
[0050] division Weight [g] Carbon weight [g] PLA (Poly lactic acid) 3 1.5 PP (Polypropylene) 5 4.3 CaCO3 2 0.24
[0051] Preferably, the biocarbon content of the bio-derived acrylic resin is the total organic carbon content (X) measured by ASTM D6866. B TOC It can be.
[0052] The acid value of the above bio-derived acrylic resin may be 2 mgKOH / g to 5 mgKOH / g. The hydroxyl value of the above bio-derived acrylic resin may be 60 mgKOH / g to 80 mgKOH / g. If the acid value and / or hydroxyl value is below the above numerical range, the adhesion between the substrate (10) and the coating layer (20) decreases, and the curing reaction occurs incompletely, which may result in a decrease in the curing speed or strength. If the acid value and / or hydroxyl value exceed the above numerical range, the curing reaction occurs excessively, which may reduce the stability of the paint composition and increase the viscosity of the paint composition, which may make coating difficult. The acid value and hydroxyl value can be calculated based on the number of milligrams of potassium hydroxide required when titrating the sample with a potassium hydroxide solution.
[0053] The glass transition temperature (Tg) of the above bio-derived acrylic resin may be 80°C to 100°C. If the glass transition temperature is less than 80°C, the paint composition may become excessively flexible, which may result in reduced adhesion or mechanical properties and lower resistance to the external environment. If the glass transition temperature exceeds 100°C, flexibility may decrease, which may lead to reduced durability.
[0054] The weight-average molecular weight (Mw) of the above bio-derived acrylic resin may be 9,000 g / mol to 13,000 g / mol. When the weight-average molecular weight falls within the above numerical range, the paint composition forms a film well, and mechanical properties can be improved.
[0055] The above bio-derived acrylic resin may be in a form mixed with an organic solvent. The solid content of the above bio-derived acrylic resin may be 40% to 50% by weight. When the solid content is within the above range, the sprayability of the paint composition may be excellent. If the solid content is less than 40% by weight, the mechanical properties may deteriorate as the coating film is not properly formed due to the decrease in the resin content within the paint composition.
[0056] The above bio-derived acrylic resin may include a polymer of a bio-derived monomer comprising at least one of butyl acrylate, butyl methacrylate, ethyl acrylate, ethyl methacrylate, isobornyl acrylate, isobornyl methacrylate, isobutyl acrylate, isobutyl methacrylate, lauric acrylate, or lauric methacrylate.
[0057] The above bio-derived modified acrylic resin may have a bio-carbon content of 30% to 40% by weight.
[0058] The above biocarbon content may be measured using radiocarbon analysis techniques according to ASTM D6866 (% Biobased Carbon Content). The above biocarbon content may also be according to EN 16640. Preferably, the biocarbon content of the bio-derived modified acrylic resin is the total organic carbon content (X) measured by ASTM D6866. B TOC It can be.
[0059] The acid value of the above bio-derived modified acrylic resin may be 2 mgKOH / g or less. The lower limit of the above acid value is not specifically limited and may be greater than 0 mgKOH / g, greater than or equal to 0.1 mgKOH / g, or greater than or equal to 0.5 mgKOH / g. The hydroxyl value of the above bio-derived modified acrylic resin may be 125 mgKOH / g to 145 mgKOH / g. If the above acid value and / or hydroxyl value is below the above numerical range, the adhesion between the substrate (10) and the coating layer (20) decreases, and the curing reaction occurs incompletely, which may result in a decrease in curing speed or strength. If the above acid value and / or hydroxyl value exceeds the above numerical range, the curing reaction occurs excessively, which may reduce the stability of the paint composition and increase the viscosity of the paint composition, which may make coating difficult. The above acid value and hydroxyl value can be calculated based on the number of milligrams of potassium hydroxide required when titrating the sample with a potassium hydroxide solution.
[0060] The glass transition temperature (Tg) of the above bio-derived modified acrylic resin may be 40°C to 50°C. If the glass transition temperature is less than 40°C, the paint composition may become excessively flexible, which may result in reduced adhesion or mechanical properties and lower resistance to the external environment. If the glass transition temperature exceeds 50°C, flexibility may decrease, which may lead to reduced durability.
[0061] The weight-average molecular weight (Mw) of the above bio-derived modified acrylic resin may be 3,000 g / mol to 6,000 g / mol. When the weight-average molecular weight falls within the above numerical range, the paint composition can form a film well, thereby improving mechanical properties.
[0062] The above bio-derived modified acrylic resin may be in a form mixed with an organic solvent. The solid content of the above bio-derived modified acrylic resin may be 60% to 80% by weight. When the solid content is within the above range, the sprayability of the paint composition may be excellent.
[0063] The above bio-derived modified acrylic resin may comprise a bio-derived monomer comprising at least one of butyl acrylate, butyl methacrylate, ethyl acrylate, ethyl methacrylate, isobornyl acrylate, isobornyl methacrylate, isobutyl acrylate, isobutyl methacrylate, raulic acrylate, or raulic methacrylate; and a polymer of a diol compound modified with maleic anhydride. The diol compound is not particularly limited and may include, for example, 1,3-propanediol.
[0064] The above solvent may include acetate-based solvents, ketone-based solvents, etc. The above solvent is a solvent with good compatibility with the resin and additives, and can lower the viscosity of the paint composition to facilitate the painting process. The smoothness and appearance of the paint film can be ensured by controlling the volatilization rate of the above solvent.
[0065] The above curing agent may be used by mixing a general curing agent and a bio-curing agent. The general curing agent may include an HDI trimer-type isocyanate. The general curing agent has excellent yellowing resistance and curing properties. The bio-curing agent is a bio-derived isocyanate curing agent and may include 1,5-pentamethylene diisocyanate. Since the bio-curing agent has excellent yellowing resistance and curing properties but relatively poor chemical resistance, it may be preferable to use it mixed with a general curing agent. The disclosed embodiment is characterized by further increasing the bio-carbon content of the paint composition by using a bio-derived isocyanate curing agent as well.
[0066] The paint composition may further include additives. The types of additives are not particularly limited and may include pigments, aluminum paste, reaction catalysts, matting agents, anti-settling agents, surface additives, wetting dispersants, UV stabilizers, etc.
[0067] The above pigment can impart color to the coating film. The above pigment may include carbon black, black iron oxide, black spinel, black titanium pigment, etc. The above aluminum paste can impart a metallic color to the coating film. The above reaction catalyst can promote a urethane reaction. The above matting agent can impart gloss to the coating film. The above anti-settling agent can prevent the matting agent, pigment, etc. from settling. The above surface additive is a silicone-based additive that can improve leveling and workability during painting and prevent defects in the coating film such as pinholes. The above wetting dispersant can disperse the pigment to make the color of the coating film vivid and prevent the pigment from aggregating during storage. The above UV stabilizer can prevent defects such as loss of gloss, yellowing, and cracking.
[0068] When the paint composition forms the undercoat layer (21), the paint composition may include a main component and a curing agent. The main component may include 10% to 20% by weight of a base resin, 25% to 35% by weight of a bio-derived acrylic resin, 10% to 25% by weight of a bio-derived modified acrylic resin, 1% to 3% by weight of a pigment, 15% to 25% by weight of a solvent, and 5% to 20% by weight of an additive. The content of the curing agent may be 20% to 30% by weight based on 100% by weight of the main component.
[0069] If the content of the above base resin is less than 10% by weight, scratch resistance and chemical resistance may decrease. If the content of the above base resin exceeds 20% by weight, paint leveling performance may decrease.
[0070] If the content of the above bio-derived acrylic resin is less than 25% by weight, heat cycle resistance and acid resistance may decrease, and if it exceeds 35% by weight, adhesion and moisture resistance may decrease.
[0071] If the content of the above bio-derived modified acrylic resin is less than 10% by weight, chemical resistance such as sunscreen resistance may be reduced, and if it exceeds 25% by weight, gloss and compatibility may be reduced.
[0072] If the content of the above pigment is less than 1 weight%, it is difficult to conceal the color of the substrate (10), and if it exceeds 3 weight%, the interlayer adhesion may be reduced.
[0073] The above additives may include 5% to 10% by weight of aluminum paste, 0.01% to 0.03% by weight of a reaction catalyst, 0.8% to 2% by weight of an anti-settling agent, 0.1% to 0.5% by weight of a surface additive, 0.5% to 3% by weight of a wetting dispersant, 0.5% to 1.5% by weight of a UV stabilizer, etc. The content of the above additives may be based on the total weight of the above main component.
[0074] When the paint composition forms the top layer (23), the paint composition may include a main component and a curing agent. The main component may include 30% to 45% by weight of bio-derived acrylic resin, 15% to 25% by weight of bio-derived modified acrylic resin, 25% to 40% by weight of solvent, and 2% to 15% by weight of additive. The content of the curing agent may be 20% to 30% by weight based on 100% by weight of the main component.
[0075] If the content of the above bio-derived acrylic resin is less than 30% by weight, heat cycle resistance and acid resistance may decrease, and if it exceeds 45% by weight, adhesion and moisture resistance may decrease.
[0076] If the content of the above bio-derived modified acrylic resin is less than 15% by weight, chemical resistance such as sunscreen resistance may be reduced, and if it exceeds 25% by weight, gloss and compatibility may be reduced.
[0077] The above additives may include 0.01% to 0.03% by weight of a reaction catalyst, 1% to 6% by weight of a matting agent, 0.8% to 2% by weight of an anti-settling agent, 0.1% to 0.5% by weight of a surface additive, and 0.5% to 1.5% by weight of a UV stabilizer. The content of the above additives may be based on the total weight of the above subject.
[0078] The paint composition may have a biocarbon content of 15% to 45% by weight. The biocarbon content may be measured using a radiocarbon analysis technique according to ASTM D6866 (% Biobased Carbon Content). The biocarbon content may also be according to EN 16640. Preferably, the biocarbon content of the paint composition is the total organic carbon content (X) measured by ASTM D6866. B TOC ) It may be. The above paint composition is an eco-friendly paint and is characterized by having a very high biomass content compared to conventional general paint compositions.
[0080] The present invention will be explained in more detail below through specific embodiments. The following embodiments are merely examples to aid in understanding the present invention and do not limit the scope of the present invention.
[0082] Preparation Example 1 - Preparation of Bio-derived Acrylic Resin
[0083] A thermometer, condenser, stirrer, and heater were attached to a 4-neck flask. 42.0 wt% of butyl acetate was placed in the 4-neck flask and heated to approximately 110°C. Then, 13.0 wt% of methyl methacrylate, 20.0 wt% of bio-isobornyl acrylate, 5.0 wt% of normal butyl methacrylate, 7.5 wt% of 2-hydroxyethyl methacrylate, 0.5 wt% of methacrylic acid, and 0.5 wt% of t-butylperoxy 2-ethylhexanoite were added dropwise at a uniform rate for approximately 3 hours. After maintaining the mixture for 1 hour, a mixture of 0.3 wt% of t-butylperoxy 2-ethylhexanoite and 10.0 wt% of butyl acetate was added dropwise for 1 hour. After maintaining the resulting product for 2 hours, the reaction was terminated to obtain a bio-derived acrylic resin with a bio-carbon content of about 32% by weight. The weight-average molecular weight of the bio-derived acrylic resin is about 9,000 g / mol to 13,000 g / mol, the hydroxyl group value is about 60 mgKOH / g to 80 mgKOH / g, and the acid value is 2 mgKOH / g to 5 mgKOH / g.
[0085] Preparation Example 2 - Preparation of Bio-derived Modified Acrylic Resin
[0086] A thermometer, condenser, stirrer, and heater were attached to a 4-neck flask. 22.0 wt% maleic anhydride and 20.0 wt% bio-1,3-propanediol were placed in the 4-neck flask and heated to 60°C. After heating, 60.0 wt% of CARDURA E10P was added at an acid value of 300 mgKOH / g or less, and the temperature was raised to 130°C. While maintaining the temperature, if the acid value was 2 mgKOH / g or less, the mixture was cooled and packaged to obtain a bio-derived modified monomer with a bio-carbon content of approximately 20 wt%.
[0087] A thermometer, condenser, stirrer, and heater were attached to a 4-neck flask. 34.0 wt% of butyl acetate was placed in the 4-neck flask and heated to approximately 126°C. Then, 17.0 wt% of 2-hydroxyethyl methacrylate, 30.0 wt% of bio-isobornyl acrylate, 3.0 wt% of butyl acrylate, 20 wt% of the above-mentioned bio-derived modified monomer, and 3.0 wt% of t-butylperoxy 2-ethylhexanoite were added dropwise at a uniform rate for approximately 4 hours. After maintaining the mixture for 1 hour, a mixture of 0.3 wt% of t-butylperoxy 2-ethylhexanoite and 1 wt% of butyl acetate was added. The resulting mixture was maintained for 3 hours, after which the reaction was terminated to obtain a bio-derived modified acrylic resin with a bio-carbon content of approximately 35 wt%. The weight-average molecular weight of the above bio-derived modified acrylic resin is about 3,000 g / mol to 6,000 g / mol, the hydroxyl group value is about 125 mgKOH / g to 145 mgKOH / g, and the acid value is about 2 mgKOH / g or less.
[0089] Examples 1 to 3 and Comparative Examples 1 to 4 - Formation of Undercoat
[0090] A paint composition was mixed as shown in Tables 2 and 3 below and a primer layer was formed by hydraulic transfer onto a substrate.
[0091] division Example 1 Example 2 Example 3 Subject [Weight %] Base resin 18 10 5 Bio-derived acrylic resin 30 38 40 Bio-derived modified acrylic resin 20 20 23 pigment 2 2 2 reaction catalyst 0.01 0.01 0.01 Anti-settling agent 1 1 1 Surface additive 0.3 0.3 0.3 Wetting dispersant 2 2 2 solvent 26.69 26.69 26.69 Curing agent [parts by weight] General hardener 20 10 10 Bio-derived curing agent - 10 10
[0092] division Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Subject [Weight %] Base resin 38 23 18 18 Bio-derived acrylic resin 30 45 10 10 Bio-derived modified acrylic resin - - 40 40 pigment 2 2 2 2 reaction catalyst 0.01 0.01 0.01 0.01 Anti-settling agent 1 1 1 1 Surface additive 0.3 0.3 0.3 0.3 Wetting dispersant 2 2 2 2 solvent 26.69 26.69 26.69 26.69 Curing agent [parts by weight] General hardener 20 - 20 10 Bio-derived curing agent - 20 - 10
[0093] Each component of Tables 2 and 3 is as follows.
[0094] Base resin: Acrylic resin
[0095] Pigment: Orion Carbon Black FW200
[0096] Reaction Catalyst: Songwon Industrial Co., Ltd. TL-100
[0097] Anti-settling agent: Heungsanhwasung Co., Ltd. Modapol-7000
[0098] Surface Additive: BYK BYK-306,331
[0099] Wetting Dispersant: BYK BYK-2013
[0100] General curing agent: BASF Desmodur N-3300
[0102] The bio-carbon content, sunscreen resistance, moisture resistance, and light resistance of the undercoat layer according to Examples 1 to 3 and Comparative Examples 1 to 4 were measured and evaluated as follows. The results are shown in Table 4.
[0103] - Biocarbon content: Measured according to the ASTM D6866 test method. ASTM D6866 covers C, which is not found in petroleum-derived compounds. 14 The biocarbon content is measured by detecting it.
[0104] - Sunscreen resistance: Two sheets of white cotton cloth (equivalent to Toyosynthetic CH2070-3) of the same size were placed overlappingly on an acrylic plate (50 mm x 50 mm, width x length), and 0.25 g of sunscreen (Nivea SPF47) was applied to the entire surface. The area with the applied sunscreen was placed on the coating film, and the acrylic plate was pressed to ensure close adhesion. After leaving it in a constant temperature bath at 80 ± 2°C for 1 hour, it was removed, the white cotton cloth and acrylic plate were removed, and it was left at room temperature for 10 minutes. After washing with a neutral detergent and drying, the appearance and adhesion of the coating film were evaluated.
[0105] - Moisture resistance: After removing moisture from a coated specimen left at a temperature of 50°C for 240 hours, the appearance and adhesion were checked.
[0106] - Lightfastness: In accordance with the standards of SAE J 2412, the appearance and adhesion were checked after irradiating with a xenon arc at 1050 KJ / m2 (340 nm) or 126 MJ / m2 (300~400 nm). For the appearance evaluation of lightfastness, a spectrophotometer was used to measure the color difference values (L*a*b*) before and after evaluation, and the difference, △E*, was calculated.
[0107] - Adhesion: The adhesion of the final film was evaluated based on the number of peeled sections out of 100 1 mm x 1 mm (width x height) markings according to the ASTM D3359 tape adhesion test method. The test was repeated three times, and the acceptance condition was an adhesion level of M-2.5 or higher as specified in ISO 2409.
[0108] division Comparative example Examples 1 2 3 4 1 2 3 Biocarbon content 10 25 20 22 20 25 35 appearance Good Good Haze Haze Good Good Good Sunscreen M-1.0 M-3.0 M-1.0 M-3.0 M-1.0 M-1.0 M-1.0 Heat cycle resistance M-1.0 M-1.0 M-1.0 M-1.0 M-1.0 M-1.0 M-1.0 moisture resistance M-1.0△E<1.5 M-3.0△E<1.5 M-3.0△E<1.5 M-3.0△E<1.5 M-1.0△E<1.5 M-1.0△E<1.5 M-1.0△E<1.5 light resistance M-1.5△E<1.5 M-1.0△E<1.5 M-3.0△E<1.5 M-5.0△E<1.5 M-1.0△E<1.5 M-1.0△E<1.5 M-1.0△E<1.5
[0109] Comparative Example 1 has good evaluated physical properties, but the bio-carbon content is at the level of 10 wt%, so the bio-carbon content is not significantly higher compared to existing paint compositions. Comparative Example 2 satisfied the bio-carbon content but failed to satisfy the physical properties of automotive interior materials due to insufficient chemical resistance. Comparative Examples 3 and 4 increased the bio-carbon content and added an excessive amount of bio-derived modified acrylic resin to improve chemical resistance, but failed to satisfy the appearance and physical properties due to poor compatibility with the bio-derived acrylic resin.
[0110] Comparative Example 4 is a case in which the proportion of a bio-derived curing agent was increased when the bio-derived modified acrylic resin was in excess to maximize the bio-carbon content. Comparative Example 4 did not satisfy sunscreen resistance (chemical resistance).
[0111] Examples 1 to 3 selected the optimal ratio of base resin, bio-derived acrylic resin, and bio-derived modified acrylic resin to achieve a bio-carbon content of 20% to 35% by weight while satisfying the appearance and physical property quality of automotive interior materials.
[0113] Examples 4 to 6 and Comparative Examples 5 to 8 - Formation of top layer
[0114] A paint composition was mixed as shown in Tables 5 and 6 below, and a top layer was formed by hydraulic transfer onto an intermediate layer.
[0115] division Example 4 Example 5 Example 6 Subject [Weight %] Bio-derived acrylic resin 40 40 35 Bio-derived modified acrylic resin 20 20 25 Anti-settling agent 1 1 1 Surface additive 0.4 0.4 0.4 Wetting dispersant 0.2 0.2 0.2 UV stabilizer 1 1 1 reaction catalyst 0.01 0.01 0.01 Matting agent 5.5 5.5 5.5 solvent 31.89 31.89 31.89 Curing agent [parts by weight] General hardener 25 12.5 8 Bio-derived curing agent - 12.5 17
[0116] division Comparative Example 5 Comparative Example 6 Comparative Example 7 Comparative Example 8 Subject [Weight %] Bio-derived acrylic resin 60 - 50 40 Bio-derived modified acrylic resin - 50 10 20 Anti-settling agent 1 1 1 1 Surface additive 0.4 0.4 0.4 0.4 Wetting dispersant 0.2 0.2 0.2 0.2 UV stabilizer 1 1 1 1 reaction catalyst 0.01 0.01 0.01 0.01 Matting agent 5.5 5.5 5.5 5.5 solvent 31.89 41.89 31.89 31.89 Curing agent [parts by weight] General hardener 25 25 - - Bio-derived curing agent - - 25 25
[0117] Each component of Tables 5 and 6 is as follows.
[0118] Anti-settling agent: Heungsanhwasung Co., Ltd. Modapol-7000
[0119] Surface Additive: BYK BYK-306,331
[0120] Wetting Dispersant: BYK BYK-2013
[0121] UV Stabilizer: BASF TINUVIN #1130, #292
[0122] Reaction Catalyst: Songwon Industrial Co., Ltd. TL-100
[0123] Matting agent: TOSOH SILICA NIPSIL E-220A
[0124] General curing agent: BASF Desmodur N-3300
[0126] The bio-carbon content, sunscreen resistance, moisture resistance, and light resistance of the topcoat layer according to Examples 4 to 6 and Comparative Examples 5 to 8 were measured and evaluated as described above. The results are shown in Table 7.
[0127] division Comparative example Examples 5 6 7 8 4 5 6 Biocarbon content 20 25 35 35 20 30 40 appearance Leveling failure light stain Good Good Good Good Good Sunscreen M-3.0 M-1.0 M-3.0 M-3.0 M-1.0 M-1.0 M-1.0 Heat cycle resistance M-1.0 M-1.0 M-1.0 M-1.0 M-1.0 M-1.0 M-1.0 moisture resistance M-3.0△E<1.5 M-1.0△E<1.5 M-3.0△E<1.5 M-1.0△E<1.5 M-1.0△E<1.5 M-1.0△E<1.5 M-1.0△E<1.5 light resistance M-1.5△E<1.5 M-5.0△E<1.5 M-1.5△E<1.5 M-1.5△E<1.5 M-1.5△E<1.5 M-1.5△E<1.5 M-1.5△E<1.5
[0128] Comparative Example 5 used bio-derived acrylic resin alone, and the rapid drying resulted in reduced surface leveling quality, and the lack of chemical resistance of the coating film failed to satisfy the physical properties of automotive interior materials.
[0129] Comparative Example 6 used bio-derived modified acrylic resin alone, and due to slow drying, the appearance (gloss stain) quality deteriorated, and the film properties were insufficient in the light resistance category.
[0130] Comparative Examples 7 and 8 attempted to obtain a bio-carbon content by mixing a bio-derived acrylic resin and a bio-derived modified acrylic resin and using a bio-derived curing agent, but failed to satisfy the physical properties of automotive interior materials due to insufficient chemical resistance. When a bio-derived curing agent was used alone, the physical properties, particularly chemical resistance, were insufficient.
[0131] Examples 4 to 6 optimized the ratio of bio-derived acrylic resin and bio-derived modified acrylic resin to achieve a bio-carbon content of 20% to 40% by weight while satisfying the appearance and physical property quality of automotive interior materials.
[0133] Example 7
[0134] A paint composition was prepared as shown in Table 8 below by removing the matting agent from the composition of Example 6, and a glossy topcoat was formed by hydraulic transfer onto the intermediate layer.
[0135] division Example 7 Subject [Weight %] Bio-derived acrylic resin 35 Bio-derived modified acrylic resin 25 Anti-settling agent 1 Surface additive 0.4 Wetting dispersant 0.2 UV stabilizer 1 reaction catalyst 0.01 solvent 37.39 Curing agent [parts by weight] General hardener 8 Bio-derived curing agent 17
[0136] The biocarbon content of the top layer according to Example 7 is about 47% by weight.
[0138] Experimental Example
[0139] A coating layer was formed on a substrate by adjusting the color of the undercoat, the gloss of the topcoat, and the biocarbon content of the undercoat and topcoat as shown in Table 9 below. The appearance and physical properties of the coating layer were evaluated.
[0140] division Underlayer color Topcoat gloss Biocarbon content appearance Physical properties Sublayer [weight%] Top layer [weight%] 1 black Semi-gloss 20 30 Good Good 2 black Semi-gloss 20 40 Good Good 3 black Semi-gloss 35 40 Good Good 4 black glossy 20 20 Good Good 5 black glossy 23 20 Good NG 6 black glossy 20 25 Good NG 7 Silver Semi-gloss 25 30 Good Good 8 Silver Semi-gloss 25 40 Good Good 9 Silver glossy 15 30 Good Good 10 Silver glossy 25 45 Good Good
[0141] Specimens 5 and 6 showed somewhat poor lightfastness and adhesion.
[0143] Although embodiments of the present invention have been described above, those skilled in the art will understand that the present invention may be implemented in other specific forms without changing its technical concept or essential features. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. Explanation of the symbols
[0144] 10: Entry 20: Coating layer 21: Lower layer 22: Centrists 23: Upper class
Claims
Claim 1 A paint composition comprising a bio-derived acrylic resin; and a bio-derived modified acrylic resin. Claim 2 In claim 1, the bio-derived acrylic resin is a paint composition having a bio-carbon content of 30% to 35% by weight. Claim 3 A paint composition according to claim 1, wherein the acid value of the bio-derived acrylic resin is 2 mgKOH / g to 5 mgKOH / g. Claim 4 A paint composition according to claim 1, wherein the hydroxyl value of the bio-derived acrylic resin is 60 mgKOH / g to 80 mgKOH / g. Claim 5 A paint composition according to claim 1, wherein the glass transition temperature (Tg) of the bio-derived acrylic resin is 80°C to 100°C. Claim 6 A paint composition according to claim 1, wherein the weight-average molecular weight (Mw) of the bio-derived acrylic resin is 9,000 g / mol to 13,000 g / mol. Claim 7 A paint composition according to claim 1, wherein the solid content of the bio-derived acrylic resin is 40% to 50% by weight. Claim 8 A paint composition according to claim 1, wherein the bio-derived acrylic resin comprises a polymer of a bio-derived monomer comprising at least one of butyl acrylate, butyl methacrylate, ethyl acrylate, ethyl methacrylate, isobornyl acrylate, isobornyl methacrylate, isobutyl acrylate, isobutyl methacrylate, lauric acrylate, or lauric methacrylate. Claim 9 In claim 1, the bio-derived modified acrylic resin is a paint composition having a bio-carbon content of 30% to 40% by weight. Claim 10 A paint composition according to claim 1, wherein the acid value of the bio-derived modified acrylic resin is 2 mgKOH / g or less. Claim 11 A paint composition according to claim 1, wherein the hydroxyl value of the bio-derived modified acrylic resin is 125 mgKOH / g to 145 mgKOH / g. Claim 12 A paint composition according to claim 1, wherein the glass transition temperature (Tg) of the bio-derived modified acrylic resin is 40°C to 50°C. Claim 13 A paint composition according to claim 1, wherein the weight-average molecular weight (Mw) of the bio-derived modified acrylic resin is 3,000 g / mol to 6,000 g / mol. Claim 14 A paint composition according to claim 1, wherein the solid content of the bio-derived modified acrylic resin is 60% to 80% by weight. Claim 15 A paint composition according to claim 1, wherein the bio-derived modified acrylic resin comprises a bio-derived monomer comprising at least one of butyl acrylate, butyl methacrylate, ethyl acrylate, ethyl methacrylate, isobornyl acrylate, isobornyl methacrylate, isobutyl acrylate, isobutyl methacrylate, lauric acrylate, or lauric methacrylate; and a polymer of a diol compound modified with maleic anhydride. Claim 16 In claim 1, the paint composition further comprises a curing agent, and the curing agent comprises a bio-derived isocyanate curing agent. Claim 17 The paint composition according to claim 1 comprises a main component and a curing agent, wherein the main component comprises 10% to 20% by weight of a base resin, 25% to 35% by weight of a bio-derived acrylic resin, 10% to 25% by weight of a bio-derived modified acrylic resin, 1% to 3% by weight of a pigment, 15% to 25% by weight of a solvent, and 5% to 20% by weight of an additive, and the paint composition comprises 20% to 30% by weight of the curing agent based on 100% by weight of the main component. Claim 18 The paint composition according to claim 1 comprises a main component and a curing agent, wherein the main component comprises 30% to 45% by weight of a bio-derived acrylic resin, 15% to 25% by weight of a bio-derived modified acrylic resin, 25% to 40% by weight of a solvent, and 2% to 15% by weight of an additive, and the paint composition comprises 20% to 30% by weight of the curing agent based on 100% by weight of the main component. Claim 19 In claim 1, the paint composition is a paint composition having a biocarbon content of 15% to 45% by weight. Claim 20 An automotive interior material comprising: a substrate; and a multilayer coating layer positioned on the substrate; wherein the coating layer comprises a primer layer on the substrate; an intermediate layer on the primer layer; and a top layer on the intermediate layer, and at least one of the primer layer and the intermediate layer comprises a paint composition according to any one of claims 1 to 19.