Phase shift mask and method for manufacturing a phase shift mask
The phase shift mask with a gas-permeable protective film addresses haze defects by preventing oxidizing gas permeation, enhancing exposure performance by reducing surface reflectance and flare.
Patent Information
- Application Number
- KR1020247023579
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-01-31
- Filing Date
- 2023-01-30
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2043-01-30
AI Technical Summary
Existing phase shift masks suffer from haze defects when exposed to wavelengths of 200 nm or less, leading to reduced exposure performance due to increased surface reflectance and flare.
A phase shift mask design incorporating a transparent substrate, a phase shift film with adjustable phase and transmittance, and a gas-permeable protective film with a refractive index of 1.2 to 2.6 and decay coefficient of 0.0 to 0.4, where the protective film thickness is less than the phase shift film thickness and prevents oxidizing gas permeation.
The solution effectively suppresses haze and reduces surface reflectance, maintaining exposure performance by preventing gas permeation and reducing flare.
Smart Images

Figure 112024076262991-PCT00003_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a phase shift mask used in the manufacture of semiconductor devices, etc., and a method for manufacturing a phase shift mask. Background Technology
[0002] In recent years, in semiconductor processing, particularly due to the high integration of large-scale integrated circuits, the miniaturization of circuit patterns has become necessary, and there is a growing demand for technology to miniaturize wiring patterns and contact hole patterns that constitute the circuit. Consequently, the exposure light source used in the manufacture of semiconductor devices and the like is becoming shorter in wavelength, moving from the KrF excimer laser (wavelength 248 nm) to the ArF excimer laser (wavelength 193 nm).
[0003] In addition, as a mask that improves wafer transfer characteristics, there is, for example, a phase shift mask. In a phase shift mask, it is possible to adjust both the phase difference and the transmittance such that the phase difference between the ArF excimer laser light passing through the transparent substrate and the ArF excimer laser light passing through both the transparent substrate and the phase shift film (hereinafter simply referred to as "phase difference") is 180 degrees, and the ratio of the amount of light of the ArF excimer laser light passing through both the transparent substrate and the phase shift film to the amount of light of the ArF excimer laser light passing through the transparent substrate (hereinafter simply referred to as "transmittance") is 6%.
[0004] For example, when manufacturing a phase shift mask with a phase difference of 180 degrees, a method is known in which the thickness of the phase shift film is set so that the phase difference is around 177 degrees, and then the phase shift film is dry-etched with a fluorine-based gas while simultaneously processing a transparent substrate to a thickness of about 3 nm to finally adjust the phase difference to around 180 degrees.
[0005] In the case of a phase shift mask to which exposure light with a wavelength of 200 nm or less is applied, exposure may cause foreign substances called "haze" to gradually form, grow, and become visible on the mask, making the mask unusable. In particular, when the phase shift film is a film composed of silicon, transition metals, and light elements such as oxygen or nitrogen, foreign substances may occur on the surface of the phase shift film.
[0006] As for techniques for suppressing haze, there are, for example, those described in Patent Documents 1 and 2.
[0007] However, in the technology described in Patent Documents 1 and 2, there are cases where the effect of suppressing haze as described above is insufficient. Prior art literature
[0008] Japanese Patent Publication No. 2018-173621, Japanese Patent No. 4579728 The problem to be solved
[0009] The present invention is made under the circumstances described above and aims to provide a phase shift mask having low haze defects, that is, capable of sufficiently suppressing the occurrence of haze, and a method for manufacturing the phase shift mask. means of solving the problem
[0010] The present invention is made to solve the above problem, and a phase shift mask according to one embodiment of the present invention is a phase shift mask having a circuit pattern applied to an exposure light with a wavelength of 200 nm or less, and comprises a transparent substrate, a phase shift film formed on the transparent substrate having a circuit pattern, and a gas permeable protective film formed on the upper surface and side surface of the phase shift film, wherein the phase shift film is capable of adjusting a predetermined amount of phase and transmittance with respect to the transmitted exposure light, and the gas permeable protective film has a refractive index for the exposure light within the range of 1.2 or more and 2.6 or less, and also has a decay coefficient within the range of 0.0 or more and 0.4 or less, and when the film thickness of the phase shift film is denoted as d1 and the film thickness of the gas permeable protective film is denoted as d2, d2 is thinner than d1 and d2 is 15 nm or less.
[0011] In addition, a method for manufacturing a phase shift mask according to one embodiment of the present invention is the method for manufacturing a phase shift mask described above, comprising: a step of forming a phase shift film on a transparent substrate; a step of forming a light-shielding film on the phase shift film; a step of forming a resist pattern on the light-shielding film formed on the phase shift film by oxygen-containing chlorine-based etching after forming the resist pattern; a step of forming a pattern on the light-shielding film by fluorine-based etching after forming the pattern on the light-shielding film; a step of removing the resist pattern after forming the pattern on the phase shift film; a step of removing the light-shielding film by oxygen-containing chlorine-based etching from the phase shift film on which the pattern is formed after removing the resist pattern; a step of performing a defect inspection after removing the resist pattern and before removing the light-shielding film, or after removing the light-shielding film; and, if a defect is detected in the defect inspection, modifying the light-shielding film or the phase shift film at the defective area. The method is characterized by including a process and, after the modification, a process of forming the gas permeable protective film on the upper surface and side of the phase shift film having a pattern formed thereon. Effects of the invention
[0012] By using a phase shift mask according to one embodiment of the present invention, the occurrence of haze on the mask can be sufficiently suppressed. In addition, by using a phase shift mask according to one embodiment of the present invention, it is possible to suppress the increase in reflectance on the surface of the phase shift mask, thereby reducing the degradation of exposure performance caused by so-called flare. Brief explanation of the drawing
[0013] FIG. 1 is a schematic cross-sectional view showing the configuration of a phase shift mask blank according to an embodiment of the present invention. FIG. 2 is a schematic cross-sectional view showing the configuration of a phase shift mask according to an embodiment of the present invention. FIG. 3 is a schematic cross-sectional diagram showing the manufacturing process of a phase shift mask using a phase shift mask blank according to an embodiment of the present invention. FIG. 4 is a schematic cross-sectional view showing the configuration of a phase shift mask according to a modified embodiment of the present invention. FIG. 5 is a schematic plan view (a) and a schematic cross-sectional view (b) showing the structure of a phase shift mask prior to a modification process according to an embodiment of the present invention. FIG. 6 is a schematic cross-sectional view illustrating a modification process of a phase shift mask according to an embodiment of the present invention. FIG. 7 is a schematic plan view (a) and a schematic cross-sectional view (b) showing the structure of a phase shift mask after a modification process according to an embodiment of the present invention. Specific details for implementing the invention
[0014] The inventors of the present invention believed that if the three elements of the constituent material of the phase shift film constituting the phase shift mask blank or phase shift mask, an oxidizing gas such as water or oxygen, and exposure energy are not all aligned, the occurrence of haze in the mask blank or mask can be reduced, and thus the phase shift mask blank or phase shift mask was configured as follows. That is, the phase shift mask and the method of manufacturing the same according to the present embodiment are based on the technical concept of reducing the occurrence of haze by preventing the oxidizing gas from coming into contact with the constituent material of the phase shift film by providing a gas-transmitting protective film (so-called gas barrier layer) on the upper surface and side surface of a phase shift film having a circuit pattern (so-called phase shift film pattern).
[0015] A model for implementing the present invention will be described below with reference to the drawings. Additionally, the schematic cross-sectional view does not accurately reflect the actual dimensional ratios or number of patterns, and the amount of indentation in the transparent substrate or the amount of damage to the film is omitted.
[0016] Suitable embodiments of the phase shift mask blank of the present invention include the forms shown below.
[0017] (Overall configuration of the phase shift mask blank)
[0018] FIG. 1 is a schematic cross-sectional view showing the configuration of a phase shift mask blank according to an embodiment of the present invention. The phase shift mask blank (10) shown in FIG. 1 is a phase shift mask blank used to produce a phase shift mask to which exposure light with a wavelength of 200 nm or less is applied, and comprises a substrate (hereinafter simply referred to as "substrate") (11) that is transparent to the exposure wavelength, and a phase shift film (12) formed on the substrate (11). In addition, the phase shift film (12) has the function of enabling adjustment of a predetermined amount of phase and transmittance, respectively, with respect to the transmitted exposure light.
[0019] Hereinafter, each layer constituting the phase shift mask blank (10) according to an embodiment of the present invention will be described in detail.
[0020] (Circuit board)
[0021] There are no special restrictions on the substrate (11), and as the substrate (11), for example, quartz glass, CaF2, or aluminosilicate glass are generally used.
[0022] (Phase shift membrane)
[0023] The phase shift film (12) is formed on the substrate (11) with or without another film in between.
[0024] The phase shift film (12) is a film that is resistant to, for example, oxygen-containing chlorine-based etching (Cl / O system) and can also be etched by fluorine-based etching (F system).
[0025] The transmittance value of the phase shift film (12) is, for example, within a range of 3% to 80% with respect to the transmittance of the substrate (11), and it is possible to appropriately select the optimal transmittance according to the desired wafer pattern. In addition, the phase difference value of the phase shift film (12) is, for example, within a range of 160 degrees to 220 degrees, and it is more preferable if it is within a range of 175 degrees to 190 degrees. That is, the phase shift film (12) may have a transmittance to the exposure light within a range of 3% to 80% and a phase difference within a range of 160 degrees to 220 degrees. If the transmittance of the phase shift film (12) to the exposure light is less than 3%, good exposure performance may not be obtained. In addition, if the phase difference is within a range of 160 degrees to 220 degrees, the required exposure performance can be easily maintained.
[0026] That is, the phase shift film (12) is a layer that allows a predetermined amount of phase and transmittance to be adjusted, respectively, with respect to the transmitted exposure light. Here, "adjusting the phase" means, for example, reversing the phase. Also, "transmittance" means transmittance with respect to the exposure light.
[0027] The phase shift film (12) is, for example, a single layer film containing silicon and also containing at least one selected from transition metals, nitrogen, oxygen and carbon, or a multilayer film or gradient film of these, and the transmittance and phase difference with respect to the exposure wavelength are adjusted by appropriately selecting the composition and film thickness.
[0028] In terms of the elemental ratio of the entire phase shift film (12), it is preferable that the phase shift film (12) contains silicon in the range of 20 atomic% or more and 60 atomic% or less, and the transition metal in the range of 0 atomic% or more and 20 atomic% or less, and the nitrogen in the range of 30 atomic% or more and 80 atomic% or less, and the oxygen in the range of 0 atomic% or more and 30 atomic% or less, and the carbon in the range of 0 atomic% or more and 10 atomic% or less. The more desirable range of the content of each element in the phase shift film (12) is, in terms of the elemental ratio of the entire phase shift film (12), silicon is in the range of 30 atomic% or more and 50 atomic% or less, transition metal is in the range of 0 atomic% or more and 10 atomic% or less, nitrogen is in the range of 40 atomic% or more and 70 atomic% or less, oxygen is in the range of 0 atomic% or more and 20 atomic% or less, and carbon is in the range of 0 atomic% or more and 5 atomic% or less. If the content of each element in the phase shift film (12) is within the above numerical range, the phase difference can be easily controlled along with the transmittance of the phase shift film (12).
[0029] Additionally, the phase shift film (12) may contain at least one of the oxides, carbides, and nitrides of the metal silicide. In that case, the metal constituting the metal silicide may be the transition metal described above.
[0030] The transition metal contained in the phase shift film (12) is preferably at least one selected from molybdenum, titanium, vanadium, cobalt, nickel, zirconium, niobium, tantalum, and tungsten, and is more preferably molybdenum. If the transition metal contained in the phase shift film (12) is at least one selected from molybdenum, titanium, vanadium, cobalt, nickel, zirconium, niobium, tantalum, and tungsten, processing of the phase shift film (12) becomes easier, and if it is molybdenum, processing such as etching of the phase shift film (12) becomes higher.
[0031] (Overall configuration of the phase shift mask)
[0032] Hereinafter, the configuration of the phase shift mask (100) according to an embodiment of the present invention will be described.
[0033] FIG. 2(a) is a schematic cross-sectional view showing the configuration of a phase shift mask according to an embodiment of the present invention. FIG. 2(b) is a schematic cross-sectional view showing an enlarged portion of the configuration of a phase shift mask according to an embodiment of the present invention. The phase shift mask (100) shown in FIG. 2 is a phase shift mask (i.e., a patterned phase shift mask) having a circuit pattern applied to an exposure light with a wavelength of 200 nm or less, and comprises a substrate (11) that is transparent to the exposure wavelength, a phase shift film (12) formed on the substrate (11) and having a circuit pattern, and a gas-transmitting protective film (hereinafter also simply referred to as a "protective film") (13) formed to cover at least the upper surface (12t) and side surface (12s) of the phase shift film (12). Additionally, the phase shift film (12) has a function that allows a predetermined amount of phase and transmittance to be adjusted, respectively, with respect to the transmitted exposure light. Additionally, the protective film (13) has the function of preventing gas permeation into the phase shift film (12). Also, when the film thickness of the phase shift film (12) is denoted as d1 and the film thickness of the protective film (13) is denoted as d2, d1 is thicker than d2, and d2 is 15 nm or less.
[0034] The phase shift mask (100) has a phase shift film pattern (12a) (phase shift film (12) having a circuit pattern) formed by removing a portion of the phase shift film (12) constituting the phase shift mask blank (10) to expose the surface of the substrate (11).
[0035] In addition, the composition of the substrate (11) constituting the phase shift mask (100) and the phase shift film (12) having a circuit pattern according to the embodiment of the present invention is the same as the composition of the substrate (11) and the phase shift film (12) constituting the phase shift mask blank (10) according to the embodiment of the present invention described above. Therefore, a detailed description regarding the composition of the substrate (11) and the phase shift film (12) having a circuit pattern is omitted.
[0036] Hereinafter, regarding the phase shift mask (100), the protective film (13), which is a part different from the phase shift mask blank (10), will be described in detail.
[0037] (Protective shield)
[0038] The protective film (13) is formed on the phase shift film (12) with or without another film in between, and is a layer, i.e., a gas barrier layer, for preventing and suppressing gas permeation (especially permeation of oxidizing gases such as water or oxygen) into the phase shift film (12). In this embodiment, since the intrusion of gas into the phase shift film (12), which is considered to be one of the factors causing haze, can be prevented and suppressed, the occurrence of haze on the surface of the phase shift mask can be prevented and suppressed even when the mask is used for a long time (for example, when the amount of douse on the mask exceeds 100 kJ / ㎠).
[0039] In addition, the gas (atmosphere gas) whose penetration is blocked or inhibited by the protective film (13) is an oxidizing gas, specifically an oxygen-containing molecule, and more specifically a water molecule.
[0040] The protective film (13) has a refractive index n for exposure light within the range of 1.2 or more and 2.6 or less, and a decay coefficient k within the range of 0.0 or more and 0.4 or less. If the protective film (13) satisfies the above conditions, it has both the function of a gas barrier layer and the function (effect) of suppressing the increase in surface reflectance. Furthermore, if the protective film (13) satisfies the above conditions, it is possible to suppress the increase in reflectance on the surface of the phase shift mask, thereby reducing the degradation of exposure performance caused by flare. Here, "flare" refers to a phenomenon in which exposure light is diffusely reflected from the inner wall surface of an exposure device, etc.
[0041] The protective film (13) is preferably a single layer containing at least one selected from hafnium metal and hafnium compounds, or a mixed film of these compounds, or a multilayer film, but the composition is not particularly limited as long as it is a layer having a barrier function. In addition, the hafnium compound is preferably a compound containing hafnium and also containing at least one selected from nitrogen, oxygen, carbon, and fluorine. In addition, the hafnium metal mentioned above refers to a single metal.
[0042] The protective film (13) containing a hafnium compound is a single layer film or a multilayer film or gradient film containing hafnium and one or more elements selected from oxygen, nitrogen, carbon and fluorine.
[0043] The protective film (13) containing a hafnium compound preferably contains hafnium in the range of 10 atomic% to 70 atomic% in the total elemental ratio of the protective film (13), preferably contains oxygen in the range of 10 atomic% to 90 atomic%, preferably contains nitrogen in the range of 10 atomic% to 70 atomic%, preferably contains carbon in the range of 10 atomic% to 70 atomic%, and preferably contains fluorine in the range of 10 atomic% to 90 atomic%. A more preferred range of content for each element in a protective film (13) containing a hafnium compound is, in terms of the elemental ratio of the entire protective film (13), hafnium is in the range of 10 atomic% or more and 60 atomic% or less, oxygen is in the range of 60 atomic% or more and 80 atomic% or less, nitrogen is in the range of 40 atomic% or more and 60 atomic% or less, carbon is in the range of 40 atomic% or more and 60 atomic% or less, and fluorine is in the range of 70 atomic% or more and 90 atomic% or less. If the content of each element in the protective film (13) containing a hafnium compound is within the above numerical range, the barrier property of gas permeability to the phase shift film (12) of the protective film (13) is increased.
[0044] Additionally, the protective film (13) may be a single layer containing one or more elements selected from silicon, oxygen, nitrogen, and carbon, or a multilayer film of these, or a gradient film.
[0045] A protective film (13) containing a silicon-containing compound (silicon-containing compound) preferably contains silicon in the range of 10 atomic% to 70 atomic% in the total elemental ratio of the protective film (13), preferably contains oxygen in the range of 10 atomic% to 90 atomic%, preferably contains nitrogen in the range of 10 atomic% to 80 atomic%, and preferably contains carbon in the range of 10 atomic% to 70 atomic%. A more preferred range of content for each element in the protective film (13) containing the silicon-containing compound is, in the total elemental ratio of the protective film (13), silicon is in the range of 20 atomic% to 60 atomic%, oxygen is in the range of 60 atomic% to 80 atomic%, nitrogen is in the range of 50 atomic% to 70 atomic%, and carbon is in the range of 40 atomic% to 60 atomic%. If the content of each element in the protective film (13) containing a silicon-containing compound is within the above numerical range, the barrier to gas permeability to the phase shift film (12) of the protective film (13) is increased.
[0046] Additionally, the protective film (13) may be a single layer containing one or more elements selected from aluminum, oxygen, nitrogen, and carbon, or a multilayer film of these, or a gradient film.
[0047] A protective film (13) containing an aluminum-containing compound (aluminum-containing compound) preferably contains aluminum in the range of 10 atomic% to 80 atomic% in the total elemental ratio of the protective film (13), preferably contains oxygen in the range of 10 atomic% to 80 atomic%, preferably contains nitrogen in the range of 10 atomic% to 70 atomic%, and preferably contains carbon in the range of 10 atomic% to 60 atomic%. A more preferred range of content for each element in the protective film (13) containing an aluminum-containing compound is, in the total elemental ratio of the protective film (13), aluminum in the range of 30 atomic% to 70 atomic%, oxygen in the range of 50 atomic% to 70 atomic%, nitrogen in the range of 40 atomic% to 60 atomic%, and carbon in the range of 30 atomic% to 50 atomic%. If the content of each element in the protective film (13) containing an aluminum-containing compound is within the above numerical range, the barrier effect of gas permeation to the phase shift film (12) of the protective film (13) is increased.
[0048] As described above, if the protective film (13) is a film in which the composition of the protective film (13) is adjusted so that the refractive index n for exposure light is in the range of 1.2 or more and 2.6 or less, and the decay coefficient k is in the range of 0.0 or more and 0.4 or less, the effect of suppressing the increase in surface reflectance is enhanced. Specifically, if the protective film (13) is a single-layer film containing one or more materials (elements) selected from hafnium metal, hafnium compounds, silicon, and aluminum, or a mixed film of these compounds, or a multi-layer film, the effect of suppressing the increase in surface reflectance is further enhanced.
[0049] When the thickness of the phase shift film (12) is denoted as d1 and the thickness of the protective film (13) is denoted as d2, the thickness d1 of the phase shift film (12) is thicker than the thickness d2 of the protective film (13), and the thickness d2 of the protective film (13) is 15 nm or less. Additionally, it is preferable that the thickness d2 of the protective film (13) be 1 nm or more. If the thickness d2 of the protective film (13) is within the above numerical range, the barrier properties for gas permeability to the phase shift film (12) can be maintained while maintaining optical properties. If the thickness d2 of the protective film (13) is made thicker than 15 nm, there is a possibility that the optical properties may be affected.
[0050] In addition, the film thickness d1 of the phase shift film (12) may be thicker than 15 nm. When the film thickness d1 of the phase shift film (12) is thicker than 15 nm, it becomes easier to adjust the phase and transmittance.
[0051] In addition, the total thickness of the phase shift film (12) and the protective film (13) is preferably 50 nm or more, and more preferably 70 nm or more. If the total thickness of the phase shift film (12) and the protective film (13) is within the above numerical range, it becomes easier to set the function of the phase shift mask (100) to a desired value.
[0052] In addition, in this embodiment, the film thickness d2 of the protective film (13) means “the film thickness d2t of the protective film (13) formed on the upper surface (12t) of the phase shift film (12)”.
[0053] In addition, in this embodiment, the film thickness d2t of the protective film (13) formed on the upper surface (12t) of the phase shift film (12) and the film thickness d2s of the protective film (13) formed on the side surface (12s) of the phase shift film (12) may have the same thickness or different thickness. For example, the ratio (d2t / d2s) of the film thickness d2t of the protective film (13) and the film thickness d2s of the protective film (13) is preferably within the range of 0.2 to 2.0, more preferably within the range of 0.5 to 1.5, and most preferably 1. If the ratio of the film thickness d2t of the protective film (13) and the film thickness d2s of the protective film (13) is within the above numerical range, the protective film (13) functions more sufficiently as a gas barrier layer.
[0054] The protective film (13) can be formed by a known method. The atomic layer deposition (ALD) method is preferably used as the easiest method to obtain a film with excellent homogeneity and uniformity of film thickness, but in this embodiment, it is not necessary to limit it to the atomic layer deposition (ALD) method.
[0055] The ratio of the surface reflectance of the protective film (13) to the surface reflectance of the phase shift film (12) (surface reflectance of the protective film (13) / surface reflectance of the phase shift film (12)) is preferably within the range of 0.40 or more and 1.20 or less, more preferably within the range of 0.40 or more and 0.95 or less, even more preferably within the range of 0.40 or more and 0.80 or less, and even more preferably within the range of 0.40 or more and 0.70 or less. If the surface reflectance of the protective film (13) is within the above numerical range, it becomes possible to reduce the degradation of exposure performance caused by flare.
[0056] Additionally, the surface reflectance of the phase shift film (12) may be determined by measuring the relative reflectance on the surface of the phase shift film (12) using, for example, a spectrophotometer. Here, "relative reflectance" is a numerical value in units of "%" indicating how much light energy emitted from the spectrophotometer is reflected and returned from the test surface (the surface of the phase shift film (12)). That is, the brighter and glossier the test surface (the surface of the phase shift film (12)), the closer the value is to 100%.
[0057] In this embodiment, the same surface reflectance measurement was repeated 10 times for the same sample, and the average value was referred to as the "surface reflectance of the phase shift film (12)."
[0058] (Method for manufacturing a phase shift mask)
[0059] A method for manufacturing a phase shift mask (100) using a phase shift mask blank (10) according to the present embodiment comprises: a step of forming a phase shift film (12) on a substrate (11); a step of forming a light-shielding film (15) on the phase shift film (12); a step of forming a resist pattern (16) on the light-shielding film (15) formed on the phase shift film (12); a step of forming a pattern on the light-shielding film (15) using an oxygen-containing chlorine-based etching (Cl / O-based) after forming the resist pattern (16); a step of forming a pattern on the phase shift film (12) using a fluorine-based etching (F-based) after forming the pattern on the light-shielding film (15); a step of removing the resist pattern (16) after forming the pattern on the phase shift film (12); and, after removing the resist pattern (16), from the phase shift film (12) on which the pattern is formed, an oxygen-containing chlorine-based The method comprises a process of removing a light-shielding film (15) by etching (Cl / O-based), a process of performing a defect inspection after removing the resist pattern (16) and before removing the light-shielding film (15), or after removing the light-shielding film (15), a process of modifying the light-shielding film (15) or phase shift film (12) at the defective area when a defect is detected in the defect inspection, and a process of forming a protective film (13) on the upper surface (12t) and side surface (12s) of the phase shift film (12) on which a pattern is formed after modifying the light-shielding film (15) or phase shift film (12) at the defective area. Additionally, in the method for manufacturing a phase shift mask (100) using the phase shift mask blank (10) according to the present embodiment, if a defect is detected in the defect inspection described above, the light-shielding film (15) or phase shift film (12) at the defective area may be modified.
[0060] Here, a light-blocking film (15) according to an embodiment of the present invention is described.
[0061] (Sunshade)
[0062] The light-blocking film (15) is a layer formed on the phase shift mask blank (10) (phase shift film (12)) according to the embodiment of the present invention described above.
[0063] The light-blocking film (15) is, for example, a single layer containing chromium or a chromium compound, or a multilayer film of these, or a gradient film. More specifically, the light-blocking film (15) containing a chromium compound is a single layer containing chromium and one or more elements selected from nitrogen and oxygen, or a multilayer film of these, or a gradient film.
[0064] A light-shielding film (15) containing a chromium compound preferably contains chromium in the range of 30 atomic% to 100 atomic% in the total elemental ratio of the light-shielding film (15), preferably contains oxygen in the range of 0 atomic% to 50 atomic%, preferably contains nitrogen in the range of 0 atomic% to 50 atomic%, and preferably contains carbon in the range of 0 atomic% to 10 atomic%. A more preferred range of content for each element in the light-shielding film (15) containing a chromium compound is, in the total elemental ratio of the light-shielding film (15), that chromium is in the range of 50 atomic% to 100 atomic%, oxygen is in the range of 0 atomic% to 40 atomic%, nitrogen is in the range of 0 atomic% to 40 atomic%, and carbon is in the range of 0 atomic% to 5 atomic%. If the content of each element in the light-blocking film (15) containing a chromium compound is within the above numerical range, the light-blocking ability of the light-blocking film (15) is increased.
[0065] The thickness of the light-blocking film (15) is preferably in the range of, for example, 15 nm or more and 80 nm or less, particularly in the range of 20 nm or more and 75 nm or less.
[0066] The light-blocking film (15) can be formed by a known method. As the easiest method to obtain a film with excellent homogeneity, the sputtering method is preferably cited, but in this embodiment, it is not necessary to limit it to the sputtering method.
[0067] The target and sputter gas are selected based on the film composition. For example, as a method for depositing a film containing chromium, reactive sputtering can be performed using a chromium-containing target in an inert gas such as argon, a reactive gas such as oxygen, or a mixture of inert and reactive gases. The flow rate of the sputter gas can be adjusted according to the film characteristics and may be kept constant during deposition; if the amount of oxygen or nitrogen is to be varied in the thickness direction of the film, it may be varied according to the desired composition. Additionally, the applied power to the target, the distance between the target and the substrate, and the pressure inside the deposition chamber may be adjusted.
[0068] Hereinafter, each process of the method for manufacturing a phase shift mask (100) according to an embodiment of the present invention will be described in detail.
[0069] FIG. 3 is a schematic cross-sectional diagram showing the manufacturing process of a phase shift mask (100) using the phase shift mask blank (10) shown in FIG. 1. FIG. 3(a) shows a process of forming a light-blocking film (15) on a phase shift film (12). FIG. 3(b) shows a process of applying a resist film on the light-blocking film (15), performing drawing, and then performing a developing process to form a resist pattern (16). FIG. 3(c) shows a process of patterning the light-blocking film (15) by oxygen-containing chlorine-based dry etching (Cl / O system) along the resist pattern (16). FIG. 3(d) shows a process of patterning the phase shift film (12) by fluorine-based etching (F system) along the pattern of the light-blocking film (15) to form a phase shift film pattern (12a). FIG. 3(e) shows a cleaning process after peeling off the resist pattern (16). FIG. 3(f) shows a process of removing a light-blocking film (15) from the patterned phase shift film (12) (phase shift film pattern (12a)) using an oxygen-containing chlorine-based etching (Cl / O-based). FIG. 3(g) shows a process of forming a protective film (13) on the upper surface (12t) and side surface (12s) of the patterned phase shift film (12) (phase shift film pattern (12a)) after removing the light-blocking film (15). In this way, a phase shift mask (100) according to the present embodiment is manufactured.
[0070] In addition, the manufacturing process includes a defect inspection process after removing the resist pattern (16) and before removing the light-shielding film (15), or after removing the light-shielding film (15). If a defect is detected during this defect inspection, the phase shift mask (100) according to the present embodiment is manufactured by modifying the light-shielding film (15) or the phase shift film (12) at the defective area.
[0071] The phase shift mask (100) according to the present embodiment manufactured in this way is a phase shift mask to which exposure light with a wavelength of 200 nm or less is applied, and comprises a substrate (11), a phase shift film (12) formed on the substrate (11) with or without another film in between, and a protective film (13) formed on the upper surface (12t) and side surface (12s) of the phase shift film (12) (phase shift film pattern (12a)). In addition, the phase shift film (12) having a circuit pattern has the function of enabling adjustment of a predetermined amount of phase and transmittance with respect to the transmitted exposure light. In addition, the protective film (13) has the function of preventing gas transmission to the phase shift film (12).
[0072] Additionally, the phase shift mask (100) has a phase shift film pattern (12a) formed by removing a portion of the phase shift film (12) so that a portion of the substrate (11) is exposed. And, when the film thickness of the phase shift film (12) is denoted as d1 and the film thickness of the protective film (13) is denoted as d2, the film thickness d1 of the phase shift film (12) is thicker than the film thickness d2 of the protective film (13), and the film thickness d2 of the protective film (13) is 15 nm or less.
[0073] In the process of FIG. 3(b), positive-type resist or negative-type resist may be used as the material for the resist film, but it is preferable to use a chemically amplified resist for electron beam lithography that enables the formation of high-precision patterns. The film thickness of the resist film is, for example, within a range of 50 nm or more and 250 nm or less. In particular, when fabricating a phase shift mask that requires the formation of a fine pattern, it is necessary to thin the resist film so that the aspect ratio of the resist pattern (16) does not increase in order to prevent pattern collapse, and a film thickness of 200 nm or less is preferred. Meanwhile, the lower limit of the film thickness of the resist film is determined by comprehensively considering conditions such as the etching resistance of the resist material used, and 60 nm or more is preferred. When a chemically amplified type for electron beam lithography is used as the resist film, the energy density of the electron beam during lithography is within the range of 35 μC / cm² to 100 μC / cm², and after lithography, heat treatment and development treatment are performed to obtain a resist pattern (16).
[0074] In addition, in the process of Fig. 3 (e), the removal of the resist pattern (16) may be wet peeling with a peeling solution or dry peeling by dry etching.
[0075] In addition, in the process of (c) of FIG. 3, the conditions for oxygen-containing chlorine-based dry etching (Cl / O system) for patterning the light-blocking film (15) containing chromium alone or a chromium compound may be known to be used for removing chromium compound films, and in addition to chlorine gas and oxygen gas, an inert gas such as nitrogen gas or helium gas may be mixed as needed. Since the lower phase shift film (12) is resistant to oxygen-containing chlorine-based dry etching (Cl / O system), it remains without being removed or patterned in this process.
[0076] In addition, in the process of FIG. 3(d), the conditions for the fluorine-based dry etching (F-based) used to pattern the phase shift film (12) may be known ones that have been used for dry etching silicon-based compound films, tantalum compound films, or molybdenum compound films, and as for the fluorine-based gas, CF4, C2F6, or SF6 are common, and if necessary, active gases such as oxygen or inert gases such as nitrogen or helium may be mixed. In the case of FIG. 3(d), the upper layer light-shielding film (15) or resist pattern (16) is resistant to the fluorine-based dry etching (F-based), so it remains without being removed or patterned in this process. In FIG. 3(d), it is common to simultaneously cut the substrate (11) to a depth of about 1 nm to 3 nm to prevent defects in the phase shift film (12) and to perform fine adjustment of the phase difference.
[0077] In addition, in the process of (f) of FIG. 3, the conditions for the oxygen-containing chlorine-based dry etching (Cl / O system) used to remove the light-blocking film (15) may be known to be used for removing chromium compound films, and in addition to chlorine gas and oxygen gas, inert gases such as nitrogen gas or helium gas may be mixed as needed. Since both the lower phase shift film (12) and the substrate (11) are resistant to the oxygen-containing chlorine-based dry etching (Cl / O system), they remain without being removed or patterned in this process.
[0078] (Other embodiments)
[0079] In this embodiment, the case in which a protective film (13) is formed on the upper surface (12t) and side surface (12s) of the phase shift film (12) (phase shift film pattern (12a)) has been described, but the present invention is not limited thereto. For example, as shown in FIG. 4, the protective film (13) may be formed on the upper surface (12t) and side surface (12s) of the phase shift film (12), and may also be formed on the exposed substrate (11). In the above form, the reference for both the phase difference and the transmittance is the exposed portion of the substrate, and since the portion where the pattern is formed causes a phase change / transmittance change respectively, it becomes unnecessary (easy) to adjust the phase difference transmittance.
[0080] Additionally, the composition of the protective film (13) formed on the substrate (11) may be the same as the composition of the protective film (13) formed on the upper surface (12t) and side surface (12s) of the phase shift film (12).
[0081] Additionally, there may be no interface between the protective film (13) formed on the substrate (11) and the protective film (13) formed on the upper surface (12t) and side surface (12s) of the phase shift film (12), and the film may be continuous.
[0082] In addition, although the present embodiment describes the case where the protective film (13) is a single layer, the present invention is not limited to this. For example, the protective film (13) may be a multilayer (laminated film). In that case, the density of the film located on the surface side of the protective film (13) may be higher than the density of the film located on the phase shift film (12) side of the protective film (13).
[0083] In this embodiment, although the case in which a protective film (13) is formed on the upper surface (12t) and side surface (12s) of the phase shift film (12) (phase shift film pattern (12a)) has been described, the present invention is not limited thereto. For example, in the process of forming the protective film (13), the protective film (13) may be formed on the upper surface (12t) and side surface (12s) of the phase shift film (12), and may also be formed on the exposed substrate (11). In the above form, the reference for both the phase difference and the transmittance is the exposed portion of the substrate, and since the portion where the pattern is formed causes a phase change / transmittance change respectively, adjustment of the phase difference transmittance becomes unnecessary (easy).
[0084] Additionally, the composition of the protective film (13) formed on the substrate (11) may be formed to be the same as the composition of the protective film (13) formed on the upper surface (12t) and side surface (12s) of the phase shift film (12).
[0085] Additionally, a continuous film (protective film (13)) without an interface between the protective film (13) formed on the substrate (11) and the protective film (13) formed on the upper surface (12t) and side surface (12s) of the phase shift film (12) may be formed.
[0086] In addition, although the present embodiment describes the case where a single layer of protective film (13) is formed, the present invention is not limited thereto. For example, a multilayer (laminated) protective film (13) may be formed. In that case, the film density located on the surface side of the protective film (13) may be formed such that it is higher than the film density located on the phase shift film (12) side of the protective film (13).
[0087] [Example]
[0088] The embodiments of the present invention will be described more specifically below by way of examples, but the present invention is not limited to the following examples.
[0089] (Example 1)
[0090] A phase shift film containing silicon, molybdenum, oxygen, and nitrogen was deposited to a thickness of 70 nm using a DC sputtering device with two targets on a quartz substrate. Molybdenum and silicon were used as targets, and argon, oxygen, and nitrogen were used as sputtering gases. The composition of this phase shift film was analyzed by ESCA and found to be Si:Mo:O:N=40:8:7:45 (atomic % ratio).
[0091] The phase shift film formed in this way had a transmittance of 6% for the exposure light and a phase difference of 180 degrees. In addition, in this embodiment, "transmittance of the exposure light" refers to the transmittance of the exposure light in the non-aperture portion relative to the aperture portion of the phase shift film. In addition, "phase difference" refers to the phase difference in the non-aperture portion relative to the aperture portion of the phase shift film.
[0092] Next, a light-shielding film containing chromium, oxygen, and nitrogen was deposited to a thickness of 50 nm on this phase-shift film using a DC sputtering device. Chromium was used as the target, and argon, oxygen, and nitrogen were used as the sputtering gases. The composition of this light-shielding film was analyzed by ESCA and found to be Cr:O:N = 55:35:10 (atomic % ratio).
[0093] Next, a negative type chemically amplified electron beam resist was spin-coated onto the light-shielding film with a film thickness of 200 nm, an electron beam was drawn with a pattern at a dose of 35 μC / cm², heat-treated at 110°C for 10 minutes, and developed by puddle development for 90 seconds to form a resist pattern.
[0094] Next, the light-blocking film was patterned using a dry etching device. Chlorine, oxygen, and helium were used as the etching gases, and the gas pressure was set to 5 mTorr, the ICP power to 400 W, and the bias power to 40 W. Over-etching was performed at 100%.
[0095] Next, a phase-shift film was patterned using a dry etching device. CF4 and oxygen were used as the etching gas, and the gas pressure was set to 5 mTorr, the ICP power to 400 W, and the bias power to 40 W. Dry etching was stopped when the quartz substrate was etched to an average depth of 3 nm.
[0096] Next, the resist pattern was stripped and cleaned by washing with sulfuric acid water.
[0097] Next, the light-blocking film was removed using a dry etching device. Chlorine, oxygen, and helium were used as the etching gas, and the gas pressure was set to 10 mTorr, the ICP power to 500 W, and the bias power to 10 W. Over-etching was performed at 200%. At this time, no damage occurred to the underlying phase shift film and the quartz substrate.
[0098] Next, modifications were made to this phase shift mask. The method is described below.
[0099] (How to fix)
[0100] A method for modifying the phase shift mask (100) is briefly explained using FIGS. 5 to 7. Additionally, although the case described here involves performing a defect inspection and modification after removing the light-blocking film (15), the defect inspection and modification may be performed after removing the resist pattern (16) and before removing the light-blocking film (15).
[0101] FIG. 5 shows an enlarged view of a portion of the phase shift film (12) (phase shift film pattern (12a)) in the phase shift mask (100). More specifically, FIG. 5(a) is a schematic plan view showing the structure of the phase shift mask (100) according to the present embodiment before the modification process, and FIG. 5(b) is a schematic cross-sectional view showing the structure of the phase shift mask (100) according to the present embodiment before the modification process.
[0102] In FIG. 5(a), “L” indicates an area where the phase shift film (12) is formed, and “S” indicates an area where the substrate (11) is exposed. Also, in FIG. 5, “12b” indicates a modification location.
[0103] As shown in FIG. 6, modifications were made to the phase shift film (12) (phase shift film pattern (12a)) after removing the light-blocking film (15).
[0104] In this way, a phase shift mask (100) with the phase shift film (12) modified was obtained.
[0105] Finally, as shown in Fig. 7, a protective film was formed on the top and side surfaces of this phase shift film (phase shift film after modification) and further on the exposed quartz substrate. The protective film was formed by reacting the precursor tetrakisdimethylaminohafnium (Hf(N(CH3)2)4) with a fluorine-based precursor for 63 cycles using the thermal ALD method to form 5 nm of hafnium fluoride (HfF4).
[0106] In this way, a phase shift mask for Example 1 was obtained.
[0107] Next, regarding this phase shift mask, the amount of doze generated by accelerated exposure was measured to be 128 kJ / cm².
[0108] The above “dose amount in which haze is generated by accelerated exposure” means that the larger the value, the less likely haze is to occur. If the dose amount is 70 kJ / ㎠ or higher (evaluated as “△” in the table below), there is no problem at all in using the phase shift mask, and if the dose amount is 100 kJ / ㎠ or higher (evaluated as “○” in the table below), it can be said to be a phase shift mask in which haze is less likely to occur. Furthermore, if the dose amount is 110 kJ / ㎠ or higher (evaluated as “◎” in the table below), it can be said to be a phase shift mask in which haze is extremely less likely to occur. Also, if the dose amount is less than 70 kJ / ㎠ (evaluated as “×” in the table below), it is of the same degree as the phase shift mask according to the prior art.
[0109] From the above measurement results, it was confirmed that the occurrence of haze can be reduced because the phase shift mask of Example 1 has a dose amount of 128 kJ / cm².
[0110] Subsequently, the surface reflectance of this phase shift mask was measured and found to be 17.1%. In addition, the ratio of the surface reflectance of the phase shift mask of Example 1 to the surface reflectance of the phase shift mask of Comparative Example 1 described later (surface reflectance of the phase shift mask of Example 1 / surface reflectance of the phase shift mask of Comparative Example 1: relative ratio) was calculated and the value was 0.78.
[0111] The above “relative ratio” means that the smaller the value, the less likely it is for flare to occur. If the relative ratio is 0.95 or less (evaluated as “△” in the table below), there is no problem at all in using the phase shift mask, and if it is 0.80 or less (evaluated as “○” in the table below), it can be said to be a phase shift mask where flare is unlikely to occur. In addition, if the relative ratio is 0.70 or less (evaluated as “◎” in the table below), it can be said to be a phase shift mask where flare is extremely unlikely to occur. If the relative ratio is greater than 1.0, it can be said to be a phase shift mask where flare occurrence is not reduced (evaluated as “×” in the table below).
[0112] (Example 2)
[0113] A phase shift film containing silicon, molybdenum, oxygen, and nitrogen was deposited to a thickness of 70 nm using a DC sputtering device with two targets on a quartz substrate. Molybdenum and silicon were used as targets, and argon, oxygen, and nitrogen were used as sputtering gases. The composition of this phase shift film was analyzed by ESCA and found to be Si:Mo:O:N=40:8:7:45 (atomic % ratio).
[0114] The phase shift film formed in this way had a transmittance of 6% of the exposure light and a phase difference of 180 degrees.
[0115] Next, a light-shielding film containing chromium, oxygen, and nitrogen was deposited to a thickness of 50 nm on this phase-shift film using a DC sputtering device. Chromium was used as the target, and argon, oxygen, and nitrogen were used as the sputtering gases. The composition of this light-shielding film was analyzed by ESCA and found to be Cr:O:N = 55:35:10 (atomic % ratio).
[0116] Next, a negative type chemically amplified electron beam resist was spin-coated onto the light-shielding film with a film thickness of 200 nm, an electron beam was drawn with a pattern at a dose of 35 μC / cm², heat-treated at 110°C for 10 minutes, and developed by puddle development for 90 seconds to form a resist pattern.
[0117] Next, the light-blocking film was patterned using a dry etching device. Chlorine, oxygen, and helium were used as the etching gases, and the gas pressure was set to 5 mTorr, the ICP power to 400 W, and the bias power to 40 W. Over-etching was performed at 100%.
[0118] Next, a phase-shift film was patterned using a dry etching device. CF4 and oxygen were used as the etching gas, and the gas pressure was set to 5 mTorr, the ICP power to 400 W, and the bias power to 40 W. Dry etching was stopped when the quartz substrate was etched to an average depth of 3 nm.
[0119] Next, the resist pattern was stripped and cleaned by washing with sulfuric acid water.
[0120] Next, the light-blocking film was removed using a dry etching device. Chlorine, oxygen, and helium were used as the etching gas, and the gas pressure was set to 10 mTorr, the ICP power to 500 W, and the bias power to 10 W. Over-etching was performed at 200%. At this time, no damage occurred to the underlying phase shift film and the quartz substrate.
[0121] Next, this phase shift mask was modified in the same manner as in Example 1.
[0122] Finally, a protective film was formed on the top and sides of this phase shift film, and further on the exposed quartz substrate. The protective film was formed by reacting the precursor tetrakisdimethylaminohafnium (Hf(N(CH3)2)4) with O2 plasma for 130 cycles using a plasma ALD method to form 13 nm of hafnium oxide (HfO2).
[0123] In this way, a phase shift mask for Example 2 was obtained.
[0124] Next, regarding this phase shift mask, the amount of haze generated by accelerated exposure was measured and was 163 kJ / cm² or more.
[0125] From the above results, it was confirmed that the phase shift mask of Example 2 can reduce the occurrence of haze because the dose amount is 163 kJ / ㎠ or more.
[0126] Subsequently, the surface reflectance of this phase shift mask was measured and found to be 17.5%. In addition, the ratio of the surface reflectance of the phase shift mask of Example 2 to the surface reflectance of the phase shift mask of Comparative Example 1 described later (surface reflectance of the phase shift mask of Example 2 / surface reflectance of the phase shift mask of Comparative Example 1: relative ratio) was calculated and the value was 0.80.
[0127] From the above results, it was confirmed that the phase shift mask of Example 2 can reduce the occurrence of flare because the relative ratio is 0.80.
[0128] (Example 3)
[0129] A phase shift film containing silicon, molybdenum, oxygen, and nitrogen was deposited to a thickness of 70 nm using a DC sputtering device with two targets on a quartz substrate. Molybdenum and silicon were used as targets, and argon, oxygen, and nitrogen were used as sputtering gases. The composition of this phase shift film was analyzed by ESCA and found to be Si:Mo:O:N=40:8:7:45 (atomic % ratio).
[0130] The phase shift film formed in this way had a transmittance of 6% of the exposure light and a phase difference of 180 degrees.
[0131] Next, a light-shielding film containing chromium, oxygen, and nitrogen was deposited to a thickness of 50 nm on this phase-shift film using a DC sputtering device. Chromium was used as the target, and argon, oxygen, and nitrogen were used as the sputtering gases. The composition of this light-shielding film was analyzed by ESCA and found to be Cr:O:N = 55:35:10 (atomic % ratio).
[0132] Next, a negative type chemically amplified electron beam resist was spin-coated onto the light-shielding film with a film thickness of 200 nm, an electron beam was drawn with a pattern at a dose of 35 μC / cm², heat-treated at 110°C for 10 minutes, and developed by puddle development for 90 seconds to form a resist pattern.
[0133] Next, the light-blocking film was patterned using a dry etching device. Chlorine, oxygen, and helium were used as the etching gases, and the gas pressure was set to 5 mTorr, the ICP power to 400 W, and the bias power to 40 W. Over-etching was performed at 100%.
[0134] Next, a phase-shift film was patterned using a dry etching device. CF4 and oxygen were used as the etching gas, and the gas pressure was set to 5 mTorr, the ICP power to 400 W, and the bias power to 40 W. Dry etching was stopped when the quartz substrate was etched to an average depth of 3 nm.
[0135] Next, the resist pattern was stripped and cleaned by washing with sulfuric acid water.
[0136] Next, the light-blocking film was removed using a dry etching device. Chlorine, oxygen, and helium were used as the etching gas, and the gas pressure was set to 10 mTorr, the ICP power to 500 W, and the bias power to 10 W. Over-etching was performed at 200%. At this time, no damage occurred to the underlying phase shift film and the quartz substrate.
[0137] Next, this phase shift mask was modified in the same manner as in Example 1.
[0138] Finally, a protective film was formed on the top and sides of this phase shift film, and further on the exposed quartz substrate. The protective film was formed by reacting the precursor bisdiethylaminosilane (Si[N(C2H5)2)]2H2) with O2 plasma for 32 cycles using a plasma ALD method to form 5 nm of silicon oxide (SiO2).
[0139] In this way, a phase shift mask for Example 3 was obtained.
[0140] Next, regarding this phase shift mask, the amount of douse generated by accelerated exposure was measured to be 112 kJ / cm².
[0141] From the above results, it was confirmed that the phase shift mask of Example 3 can reduce the occurrence of haze because the dose amount is 112 kJ / cm².
[0142] Subsequently, the surface reflectance of this phase shift mask was measured and found to be 20.0%. In addition, the ratio of the surface reflectance of the phase shift mask of Example 3 to the surface reflectance of the phase shift mask of Comparative Example 1 described later (surface reflectance of the phase shift mask of Example 3 / surface reflectance of the phase shift mask of Comparative Example 1: relative ratio) was calculated and the value was 0.91.
[0143] From the above results, it was confirmed that the phase shift mask of Example 3 can reduce the occurrence of flare because the relative ratio is 0.91.
[0144] (Example 4)
[0145] A phase shift film containing silicon, molybdenum, oxygen, and nitrogen was deposited to a thickness of 70 nm using a DC sputtering device with two targets on a quartz substrate. Molybdenum and silicon were used as targets, and argon, oxygen, and nitrogen were used as sputtering gases. The composition of this phase shift film was analyzed by ESCA and found to be Si:Mo:O:N=40:8:7:45 (atomic % ratio).
[0146] The phase shift film formed in this way had a transmittance of 6% of the exposure light and a phase difference of 180 degrees.
[0147] Next, a light-shielding film containing chromium, oxygen, and nitrogen was deposited to a thickness of 50 nm on this phase-shift film using a DC sputtering device. Chromium was used as the target, and argon, oxygen, and nitrogen were used as the sputtering gases. The composition of this light-shielding film was analyzed by ESCA and found to be Cr:O:N = 55:35:10 (atomic % ratio).
[0148] Next, a negative type chemically amplified electron beam resist was spin-coated onto the light-shielding film with a film thickness of 200 nm, an electron beam was drawn with a pattern at a dose of 35 μC / cm², heat-treated at 110°C for 10 minutes, and developed by puddle development for 90 seconds to form a resist pattern.
[0149] Next, the light-blocking film was patterned using a dry etching device. Chlorine, oxygen, and helium were used as the etching gases, and the gas pressure was set to 5 mTorr, the ICP power to 400 W, and the bias power to 40 W. Over-etching was performed at 100%.
[0150] Next, a phase-shift film was patterned using a dry etching device. CF4 and oxygen were used as the etching gas, and the gas pressure was set to 5 mTorr, the ICP power to 400 W, and the bias power to 40 W. Dry etching was stopped when the quartz substrate was etched to an average depth of 3 nm.
[0151] Next, the resist pattern was stripped and cleaned by washing with sulfuric acid water.
[0152] Next, the light-blocking film was removed using a dry etching device. Chlorine, oxygen, and helium were used as the etching gas, and the gas pressure was set to 10 mTorr, the ICP power to 500 W, and the bias power to 10 W. Over-etching was performed at 200%. At this time, no damage occurred to the underlying phase shift film and the quartz substrate.
[0153] Next, this phase shift mask was modified in the same manner as in Example 1.
[0154] Finally, a protective film was formed on the top and sides of this phase-shift film, and further on the exposed quartz substrate. The protective film was formed by reacting the precursor trimethylaluminum (TMA) (Al(CH3)3) with O2 plasma for 36 cycles using a plasma ALD method to form 5 nm of aluminum oxide (Al2O3).
[0155] In this way, a phase shift mask for Example 4 was obtained.
[0156] Next, regarding this phase shift mask, the amount of doze generated by accelerated exposure was measured to be 116 kJ / cm².
[0157] From the above results, it was confirmed that the phase shift mask of Example 4 can reduce the occurrence of haze because the dose amount is 116 kJ / cm².
[0158] Subsequently, the surface reflectance of this phase shift mask was measured and found to be 14.4%. In addition, the ratio of the surface reflectance of the phase shift mask of Example 4 to the surface reflectance of the phase shift mask of Comparative Example 1 described later (surface reflectance of the phase shift mask of Example 4 / surface reflectance of the phase shift mask of Comparative Example 1: relative ratio) was calculated and the value was 0.65.
[0159] From the above results, it was confirmed that the phase shift mask of Example 4 can reduce the occurrence of flare because the relative ratio is 0.65.
[0160] (Comparative Example 1)
[0161] A phase shift film containing silicon, molybdenum, oxygen, and nitrogen was deposited to a thickness of 70 nm using a DC sputtering device with two targets on a quartz substrate. Molybdenum and silicon were used as targets, and argon, oxygen, and nitrogen were used as sputtering gases. The composition of this phase shift film was analyzed by ESCA and found to be Si:Mo:O:N=40:8:7:45 (atomic % ratio).
[0162] The phase shift film formed in this way had a transmittance of 6% of the exposure light and a phase difference of 180 degrees.
[0163] Next, a light-shielding film containing chromium, oxygen, and nitrogen was deposited to a thickness of 50 nm on this phase-shift film using a DC sputtering device. Chromium was used as the target, and argon, oxygen, and nitrogen were used as the sputtering gases. The composition of this light-shielding film was analyzed by ESCA and found to be Cr:O:N = 55:35:10 (atomic % ratio).
[0164] Next, a negative type chemically amplified electron beam resist was spin-coated onto the light-shielding film with a film thickness of 200 nm, an electron beam was drawn with a pattern at a dose of 35 μC / cm², heat-treated at 110°C for 10 minutes, and developed by puddle development for 90 seconds to form a resist pattern.
[0165] Next, the light-blocking film was patterned using a dry etching device. Chlorine, oxygen, and helium were used as the etching gases, and the gas pressure was set to 5 mTorr, the ICP power to 400 W, and the bias power to 40 W. Over-etching was performed at 100%.
[0166] Next, a phase-shift film was patterned using a dry etching device. CF4 and oxygen were used as the etching gas, and the gas pressure was set to 5 mTorr, the ICP power to 400 W, and the bias power to 40 W. Dry etching was stopped when the quartz substrate was etched to an average depth of 3 nm.
[0167] Next, the resist pattern was stripped and cleaned by washing with sulfuric acid water.
[0168] Next, the light-blocking film was removed using a dry etching device. Chlorine, oxygen, and helium were used as the etching gas, and the gas pressure was set to 10 mTorr, the ICP power to 500 W, and the bias power to 10 W. Over-etching was performed at 200%. At this time, no damage occurred to the underlying phase shift film and the quartz substrate.
[0169] Next, this phase shift mask was modified in the same manner as in Example 1.
[0170] In this way, a phase shift mask for Comparative Example 1 was obtained. That is, the phase shift mask for Comparative Example 1 is a phase shift mask that does not have the protective film formed in Examples 1 to 4.
[0171] Next, regarding this phase shift mask, the amount of doze generated by accelerated exposure was measured to be 58 kJ / cm².
[0172] From the above results, it was confirmed that in the phase shift mask of Comparative Example 1, the occurrence of haze cannot be sufficiently reduced because the dose amount is 58 kJ / cm².
[0173] As described above, it can be seen that forming protective films on the upper and side surfaces of the phase shift film is effective in reducing the amount of haze generated in the phase shift mask.
[0174] Next, the surface reflectance of this phase shift mask was measured to be 22.0%.
[0175] (Comparative Example 2)
[0176] A phase shift film containing silicon, molybdenum, oxygen, and nitrogen was deposited to a thickness of 70 nm using a DC sputtering device with two targets on a quartz substrate. Molybdenum and silicon were used as targets, and argon, oxygen, and nitrogen were used as sputtering gases. The composition of this phase shift film was analyzed by ESCA and found to be Si:Mo:O:N=40:8:7:45 (atomic % ratio).
[0177] The phase shift film formed in this way had a transmittance of 6% of the exposure light and a phase difference of 180 degrees.
[0178] Next, a light-shielding film containing chromium, oxygen, and nitrogen was deposited to a thickness of 50 nm on this phase-shift film using a DC sputtering device. Chromium was used as the target, and argon, oxygen, and nitrogen were used as the sputtering gases. The composition of this light-shielding film was analyzed by ESCA and found to be Cr:O:N = 55:35:10 (atomic % ratio).
[0179] Next, a negative type chemically amplified electron beam resist was spin-coated onto the light-shielding film with a film thickness of 200 nm, an electron beam was drawn with a pattern at a dose of 35 μC / cm², heat-treated at 110°C for 10 minutes, and developed by puddle development for 90 seconds to form a resist pattern.
[0180] Next, the light-blocking film was patterned using a dry etching device. Chlorine, oxygen, and helium were used as the etching gases, and the gas pressure was set to 5 mTorr, the ICP power to 400 W, and the bias power to 40 W. Over-etching was performed at 100%.
[0181] Next, a phase-shift film was patterned using a dry etching device. CF4 and oxygen were used as the etching gas, and the gas pressure was set to 5 mTorr, the ICP power to 400 W, and the bias power to 40 W. Dry etching was stopped when the quartz substrate was etched to an average depth of 3 nm.
[0182] Next, the resist pattern was stripped and cleaned by washing with sulfuric acid water.
[0183] Next, the light-blocking film was removed using a dry etching device. Chlorine, oxygen, and helium were used as the etching gas, and the gas pressure was set to 10 mTorr, the ICP power to 500 W, and the bias power to 10 W. Over-etching was performed at 200%. At this time, no damage occurred to the underlying phase shift film and the quartz substrate.
[0184] Next, this phase shift mask was modified in the same manner as in Example 1.
[0185] Finally, a protective film was formed on the top and sides of this phase shift film, and further on the exposed quartz substrate. The protective film was formed by reacting the precursor pentaethoxytantal (Ta(OC2H5)5) with O2 plasma for 91 cycles using a plasma ALD method to form 10 nm of tantalum oxide (Ta2O5).
[0186] In this way, a phase shift mask for Comparative Example 2 was obtained.
[0187] Next, regarding this phase shift mask, the amount of haze generated by accelerated exposure was measured to be 159 kJ / cm².
[0188] From the above results, it was confirmed that the phase shift mask of Comparative Example 2 can reduce the occurrence of haze because the dose amount is 159 kJ / ㎠.
[0189] Next, the surface reflectance of this phase shift mask was measured and found to be 32.5%. In addition, the ratio of the surface reflectance of the phase shift mask of Comparative Example 2 to the surface reflectance of the phase shift mask of Comparative Example 1 (surface reflectance of the phase shift mask of Comparative Example 2 / surface reflectance of the phase shift mask of Comparative Example 1: relative ratio) was calculated and the value was 1.48.
[0190] From the above results, it was confirmed that the phase shift mask of Comparative Example 2 cannot improve the occurrence of flare because the relative ratio is 1.48.
[0191]
[0192] Although the phase shift mask blank of the present invention and the phase shift mask produced using the same have been described above by way of the above embodiments, the above embodiments are merely examples for carrying out the present invention, and the present invention is not limited thereto. Furthermore, modifications to these embodiments are within the scope of the present invention, and it is obvious from the description above that various other embodiments are possible within the scope of the present invention. Industrial applicability
[0193] In the present invention, since the composition, film thickness, and layer structure of the phase shift mask blank and the manufacturing process and conditions of the phase shift mask using the same are selected within an appropriate range, it is possible to provide a phase shift mask with a fine pattern formed with high precision, corresponding to the manufacture of logic devices of 28 nm or less or memory devices of 30 nm or less. Explanation of the symbols
[0194] 10: Phase Shift Mask Blank 11: Substrate transparent to exposure wavelength (substrate) 12: Phase shift mark 12a: Phase shift membrane pattern 13: Shield (Gas Permeable Shield) 15: Shade 16: Resist Pattern 100: Phase shift mask d1: Thickness of the phase shift film d2: Thickness of the protective layer (gas-permeable protective layer)
Claims
Claim 1 A phase shift mask having a circuit pattern is applied to an exposure light with a wavelength of 200 nm or less, and comprises a transparent substrate, a phase shift film formed on the transparent substrate having a circuit pattern, and a gas-transmitting protective film formed on the upper surface and side surface of the phase shift film, wherein the phase shift film is capable of adjusting a predetermined amount of phase and transmittance with respect to the transmitted exposure light, and wherein the gas-transmitting protective film has a refractive index with respect to the exposure light within the range of 1.2 or more and 2.6 or less, and also has a decay coefficient within the range of 0.0 or more and 0.4 or less, wherein when the film thickness of the phase shift film is denoted as d1 and the film thickness of the gas-transmitting protective film is denoted as d2, d2 is thinner than d1 and d2 is 15 nm or less, the total film thickness of the phase shift film and the gas-transmitting protective film is 50 nm or more, and the phase shift film contains silicon and also transition A phase shift mask characterized by containing at least one selected from metal, nitrogen, oxygen, and carbon, wherein the transition metal is at least one selected from molybdenum, titanium, vanadium, cobalt, nickel, zirconium, niobium, tantalum, and tungsten. Claim 2 A phase shift mask according to claim 1, wherein the gas permeable protective film contains at least one selected from hafnium metal and hafnium compounds, and the hafnium compound contains hafnium and also contains at least one selected from nitrogen, oxygen, carbon, and fluorine. Claim 3 A phase shift mask according to claim 1, wherein the gas permeable protective film contains silicon and also contains at least one selected from nitrogen, oxygen, and carbon. Claim 4 A phase shift mask according to claim 1, wherein the gas permeable protective film contains aluminum and also contains at least one selected from nitrogen, oxygen, and carbon. Claim 5 A phase shift mask according to any one of claims 1 to 4, wherein the phase shift film is resistant to oxygen-containing chlorine-based etching and is also etchable by fluorine-based etching. Claim 6 delete Claim 7 A phase shift mask according to claim 1 or 2, characterized in that the ratio of the surface reflectance of the gas-permeable protective film to the surface reflectance of the phase shift film is within the range of 0.4 or more and 1.2 or less. Claim 8 A phase shift mask according to claim 1 or 2, characterized in that the gas permeable protective film is also formed on the transparent substrate. Claim 9 A method for manufacturing a phase shift mask as described in claim 1 or 2, comprising: a process of forming a phase shift film on a transparent substrate; a process of forming a light-shielding film on the phase shift film; a process of forming a resist pattern on the light-shielding film formed on the phase shift film; a process of forming a pattern on the light-shielding film by oxygen-containing chlorine-based etching after forming the resist pattern; a process of forming a pattern on the phase shift film by fluorine-based etching after forming the pattern on the light-shielding film; a process of removing the resist pattern after forming the pattern on the phase shift film; a process of removing the light-shielding film by oxygen-containing chlorine-based etching from the phase shift film on which the pattern is formed after removing the resist pattern; a process of performing a defect inspection after removing the resist pattern and before removing the light-shielding film, or after removing the light-shielding film; a process of modifying the light-shielding film or the phase shift film at the defective area when a defect is detected in the defect inspection; and after performing the modification, the pattern formed thereon A method for manufacturing a phase shift mask characterized by including a process of forming the gas permeable protective film on the upper surface and side surface of the phase shift film. Claim 10 A method for manufacturing a phase shift mask according to claim 9, wherein in the process of forming the gas permeable protective film, the gas permeable protective film is also formed on the transparent substrate.
Citation Information
Patent Citations
Photomask blank and photomask, and production method therefor
JP2017227847A
Exposure mask and the manufacturing method
KR1019920018825A
An electron device manufacturing method, a patternforming method and a photomask used for those mothods
KR1020010098405A
Method for manufacturing photomask
KR1020110126687A
Photomask and its manufacture
JP1998003162A