Catalyst for the production of methacrylic acid, method for the production of the same, and method for the production of methacrylic acid and methacrylic acid esters using the same

A heteropoly acid catalyst with defined P-NMR spectral characteristics and composition is developed to improve heat resistance and yield in methacrylic acid production, overcoming the limitations of existing catalysts.

KR103044535B1Active Publication Date: 2026-11-06MITSUBISHI CHEM CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
KR1020247034439
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-03-24
Filing Date
2023-03-23
Publication Date
2026-11-06
Estimated Expiration
2043-03-23

AI Technical Summary

Technical Problem

Existing catalysts for producing methacrylic acid exhibit low heat resistance and insufficient lifespan, limiting their effectiveness in industrial applications.

Method used

A catalyst comprising a heteropoly acid with specific P-NMR spectral characteristics, including areas A, B, and C, and a composition of P, Mo, W, V, Cu, and O, is developed to enhance heat resistance and yield.

Benefits of technology

The catalyst achieves high heat resistance and high yield in the production of methacrylic acid, addressing the limitations of existing catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112024112235611-PCT00001
    Figure 112024112235611-PCT00001
Patent Text Reader

Abstract

The objective is to provide a catalyst capable of producing methacrylic acid with high heat resistance and high yield, and to provide a method for producing methacrylic acid and methacrylic acid esters using said catalyst, and the objective is solved by using a catalyst having a specific 31P-NMR spectrum.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a catalyst for the production of methacrylic acid, a method for producing the same, and a method for producing methacrylic acid and methacrylic acid esters using the same. Background Technology

[0002] As a catalyst for the production of methacrylic acid (hereinafter also simply referred to as "catalyst") used when producing methacrylic acid by the oxidation of methacrolein, a heteropolyacid-based catalyst including molybdenum and phosphorus is known, for example. A heteropolyacid is a condensed oxyacid formed by the oxide of a heteroatom and 12 coordination atoms (hereinafter referred to as "poly atoms") that form the basic framework of a polyacid. Examples of heteropolyacid-based catalysts include a proton-type heteropolyacid in which the counter cation is a proton, and a heteropolysalt in which a portion of the proton is substituted with a cation other than a proton (hereinafter, the proton-type heteropolyacid is simply referred to as "heteropolyacid," and at least one selected from the proton-type heteropolyacid and the heteropolysalt is simply referred to as "heteropolyacid (salt)").

[0003] Regarding the structure of heteropolyacid (salt), Non-patent Literature 1 describes that phosphorus, silicon, arsenic, germanium, titanium, antimony, etc. can be heteroatoms, and tungsten, molybdenum, vanadium, niobium, tantalum, etc. can be polyatoms of the heteropolyacid (salt). In addition, Kegyn type, Dawson type, and Plésler type are described as basic structures of heteropolyacid (salt).

[0004] In addition, Patent Document 1 discloses a catalyst for the production of methacrylic acid comprising a Keggine-type heteropolyphosphate having a composition represented by the following formula.

[0005] P a Mo b V c X d Y e O f

[0006] (In the formula, P, Mo, V, and O represent phosphorus, molybdenum, vanadium, and oxygen, respectively; X represents at least one element selected from potassium, rubidium, cesium, and thallium; and Y represents at least one element selected from copper, arsenic, antimony, boron, silver, bismuth, iron, cobalt, lanthanum, and cerium. a, b, c, d, e, and f represent the atomic ratios of P, Mo, V, X, Y, and O, respectively; when b=12, a, c, d, and e are each independently values ​​greater than 0 and less than or equal to 3, and f is a value determined by the oxidation state and atomic ratio of each element other than oxygen.)

[0007] As a Keggin-type heteropoly acid, H3PMo 12 O 40 , H4PMo 11 VO 40 H3, PW 12 O 40 Etc. is known, and in Non-Patent Literature 1, H3PMo 12 O 40 Ina H4PMo 11 VO 40 Compared to H3, PW 12 O 40 It is disclosed that the thermal decomposition temperature of is high. Meanwhile, Non-patent Literature 2 describes H3PMo as a catalyst for the production of methacrylic acid. 12 O 40 If used, methacrylic acid is obtained well, but PW 12 O 40 It is stated that using it results in very low activity and selectivity. Prior art literature

[0008] Japanese Patent Publication No. 2003-010691

[0009] Toshio Okuhara, Noritaka Mizuno, Makoto Misono, Advances in Catalysis, volume 41.Shuhei Yasuda, Atsuki Iwakura, Jun Hirata, Mitsuru Kanno, Wataru Ninomiya, Ryoichi Otomo, Yuichi Kamiya, Catalysis Communications, 125(2019), 43-47. The problem to be solved

[0010] However, known catalysts for the production of methacrylic acid have low heat resistance and their lifespan is still insufficient. Therefore, in order to use them as industrial catalysts, there is a need to develop a catalyst that has high heat resistance and can produce methacrylic acid with a high yield.

[0011] The object of the present invention is to provide a catalyst capable of producing methacrylic acid with high heat resistance and high yield. Additionally, the object of the present invention is to provide a method for producing methacrylic acid and methacrylic acid esters using this catalyst. means of solving the problem

[0012] The inventors, having conducted a careful review in consideration of the above problem, have found a specific 31 By using a catalyst having a P-NMR spectrum, it was discovered that the above problem could be solved, and the present invention was completed.

[0013] That is, the present invention includes the following.

[0014] [1]: A catalyst used to produce methacrylic acid by the oxidation of methacrolein, and

[0015] The above catalyst contains a heteropoly acid comprising phosphorus, molybdenum, and tungsten, and

[0016] of the above catalyst 31A catalyst for producing methacrylic acid, wherein in a P-NMR spectrum, the area of ​​the signal observed in the range of -5.2 ppm or more and less than 0 ppm is A, the area of ​​the signal observed in the range of -10 ppm or more and less than -5.2 ppm is B, and the area of ​​the signal observed in the range of -20 ppm or more and less than -10 ppm is C, and C / (A+B+C) is 0.015 to 0.085.

[0017] [2]: The above 31 A catalyst for producing methacrylic acid as described in [1], in which B / (A+B+C) in the P-NMR spectrum is 0.1 to 0.485.

[0018] [3]: The above 31 A catalyst for the production of methacrylic acid as described in [1] or [2], wherein A / (A+B+C) in the P-NMR spectrum is 0.5 to 0.885.

[0019] [4]: The above 31 A catalyst for the production of methacrylic acid described in any one of [1] to [3], wherein C / (A+B+C) in the P-NMR spectrum is 0.02 to 0.08.

[0020] [5]: The above 31 A catalyst for the production of methacrylic acid as described in any one of [1] to [4], wherein B / (A+B+C) in the P-NMR spectrum is 0.2 to 0.45.

[0021] [6]: The above 31 A catalyst for the production of methacrylic acid described in any one of [1] to [5], wherein the A / (A+B+C) in the P-NMR spectrum is 0.53 to 0.75.

[0022] [7]: A catalyst for the production of methacrylic acid described in any one of [1] to [6] having a composition represented by the following formula (I).

[0023] P a Mo b W c V d Cu e A f Eg G h O i (I)

[0024] In formula (I), P, Mo, W, V, Cu, and O represent phosphorus, molybdenum, tungsten, vanadium, copper, and oxygen, respectively. A represents at least one element selected from the group consisting of antimony, bismuth, arsenic, germanium, tellurium, selenium, and silicon. E represents at least one element selected from the group consisting of iron, zinc, chromium, tantalum, cobalt, nickel, manganese, titanium, and niobium. G represents at least one element selected from the group consisting of potassium, rubidium, and cesium. a to i represent the molar ratios of each component, b+c=12, a=0.5 to 3, c=0.22 to 5, d=0.01 to 3, e=0.01 to 2, f=0 to 3, g=0 to 3, h=0.01 to 3, and i is the molar ratio of oxygen required to satisfy the valence of each component.

[0025] [8]: In the above formula (I), the catalyst for producing methacrylic acid described in [7], wherein c=0.22 to 3

[0026] [9]: A method for producing a catalyst for producing methacrylic acid as described in any one of [1] to [8], and

[0027] (i) a process of mixing phosphorus raw material, molybdenum raw material and tungsten raw material with a solvent to prepare a solution or slurry (Solution A) having a pH of 0.1 to 4, and

[0028] (ii) A process of obtaining a dried product by drying the above liquid A, and

[0029] (iii) A process of obtaining a sintered product by sintering the above-mentioned dried product.

[0030] A method for preparing a catalyst for the production of methacrylic acid comprising

[0031]

[10] : A method for producing a catalyst for producing methacrylic acid as described in [9], wherein in the above process (i), the tungsten raw material having a solubility in water at 20°C of 4.1 g / 100 mL or more is 50 mass% or more of the total tungsten raw material.

[0032]

[11] : A method for producing a catalyst for producing methacrylic acid as described in [9] or

[10] , wherein in the above process (i), the pH of the above liquid A is 0.1 to 3.

[0033]

[12] : A method for producing methacrylic acid comprising a process of oxidizing methacrolein using a catalyst for producing methacrylic acid described in any one of [1] to [8] and producing methacrylic acid.

[0034]

[13] : A method for producing methacrylic acid comprising a process of oxidizing methacrolein using a catalyst for producing methacrylic acid prepared by any one of the methods described in [9] to

[12] and producing methacrylic acid.

[0035]

[14] : A method for producing a methacrylic acid ester comprising a process of esterifying methacrylic acid produced by the method described in

[12] or

[13] . Effects of the invention

[0036] According to the present invention, a catalyst with high heat resistance and capable of producing methacrylic acid with a high yield can be provided. Specific details for implementing the invention

[0037] Embodiments of the present invention are described below, but the present invention is not limited to the following.

[0038] In addition, in this specification, a numerical range indicated using “to” means a range that includes the values ​​described before and after “to” as lower and upper limits, and “A to B” means greater than or equal to A and less than or equal to B.

[0039] [Catalyst for Methacrylic Acid Production]

[0040] The catalyst for producing methacrylic acid according to the present embodiment is a catalyst used when producing methacrylic acid by the oxidation of methacrolein, and contains a heteropoly acid comprising phosphorus, molybdenum, and tungsten. In addition, the catalyst 31 In the P-NMR spectrum, when the area of ​​the signal observed in the range of -5.2 ppm or more and less than 0 ppm is A, the area of ​​the signal observed in the range of -10 ppm or more and less than -5.2 ppm is B, and the area of ​​the signal observed in the range of -20 ppm or more and less than -10 ppm is C, C / (A+B+C) is 0.015 to 0.085.

[0041] These catalysts have high heat resistance and can also produce methacrylic acid in high yield.

[0042] <catalyst's 31 P-NMR Spectrum

[0043] catalyst's 31 In the P-NMR spectrum, A, B, and C are the areas of signals originating mainly from Kegyn-type heteropolyacid structures. Specifically, A is the area of ​​a signal originating from a structure in which the heterovalence is mainly phosphorus and the polyvalence is molybdenum (hereinafter also referred to as Structure A). B is the area of ​​a signal originating from a structure in which the heterovalence is mainly phosphorus, 1 to 5 of the polyvalence atoms are atoms such as tungsten or vanadium, and the remainder is molybdenum (hereinafter also referred to as Structure B). Additionally, C is the area of ​​a signal originating from a structure in which the heterovalence is mainly phosphorus, 6 to 12 of the polyvalence atoms are atoms such as tungsten or vanadium, and the remainder is molybdenum (hereinafter also referred to as Structure C).

[0044] The inclusion of structures A and B in the catalyst results in a good yield in the production of methacrylic acid. On the other hand, when structure A is present in excess, the sequential oxidation reaction of methacrylic acid is promoted, so the yield tends to decrease. Furthermore, structures B and C have higher thermal decomposition temperatures and excellent heat resistance compared to structure A. Structure C, in which most of the poly atoms are atoms such as W or V, exhibits particularly excellent heat resistance.

[0045] The catalyst for producing methacrylic acid according to the present embodiment 31 In the P-NMR spectrum, C / (A+B+C) is 0.015 to 0.085. At this time, structures A and B, which exhibit good yield in the production of methacrylic acid, and structure C, which has particularly excellent heat resistance, are present in a suitable ratio in the catalyst. Therefore, it is expected that a catalyst with high heat resistance and excellent methacrylic acid yield will be obtained. The lower limit of C / (A+B+C) is preferably 0.02 or higher, and more preferably 0.025 or higher. In addition, the upper limit of C / (A+B+C) is preferably 0.08 or lower, and more preferably 0.75 or lower.

[0046] B / (A+B+C) is preferably 0.1 or higher. At this time, since structure B, which has excellent yield and heat resistance in the production of methacrylic acid, is appropriately present in the catalyst, a catalyst with superior heat resistance and methacrylic acid yield is obtained. B / (A+B+C) is more preferably 0.2 or higher. In addition, the upper limit of B / (A+B+C) is preferably 0.985 or lower, more preferably 0.98 or lower, even more preferably 0.485 or lower, and particularly preferably 0.45 or lower.

[0047] The lower limit of A / (A+B+C) is preferably 0.5 or higher, more preferably 0.53 or higher, and even more preferably 0.56 or higher from the perspective of methacrylic acid yield. In addition, the upper limit of A / (A+B+C) is preferably 0.885 or lower, more preferably 0.78 or lower, and particularly preferably 0.75 or lower from the perspective of inhibiting sequential oxidation of methacrylic acid.

[0048] In addition, the preferred upper and lower limits of the above C / (A+B+C), B / (A+B+C), and A / (A+B+C) can each be selected from any combination, for example, C / (A+B+C) may be 0.015 to 0.085, B / (A+B+C) may be 0.1 to 0.985, and A / (A+B+C) may be 0 to 0.885; C / (A+B+C) may be 0.015 to 0.085, B / (A+B+C) may be 0.1 to 0.485, and A / (A+B+C) may be 0.5 to 0.885; or C / (A+B+C) may be 0.02 to 0.08, B / (A+B+C) may be 0 to 0.98, and A / (A+B+C) may be 0 to It may be 0.98, C / (A+B+C) may be 0.02 to 0.08, B / (A+B+C) may be 0.2 to 0.98, A / (A+B+C) may be 0 to 0.78, C / (A+B+C) may be 0.02 to 0.08, B / (A+B+C) may be 0.2 to 0.45, and A / (A+B+C) may be 0.53 to 0.75.

[0049] 31 As a method for obtaining a catalyst having C / (A+B+C) and A / (A+B+C) within a specified range in a P-NMR spectrum, for example, a method of preparing a catalyst by a method including processes (i) to (iii) described below, a method of adjusting the amount of tungsten raw material used in process (i) and the pH of the obtained A solution, and a method of adjusting the calcination temperature or time in process (iii).

[0050] also 31The P-NMR spectrum is obtained by packing 300 mg of powdered catalyst into a sample tube and performing measurements at room temperature using an instrument such as the AVANCE 300 (Bruker). A 7 mm MAS probe is used for the measurement, and the measurement conditions are set as follows: resonance frequency 121.4 MHz, pulse width 5.5 μsec, signal introduction time 0.066 sec, integration cycles 64, repeat waiting time 150 sec, and MAS rotation speed 5000 Hz. With the horizontal axis representing chemical shift (ppm) and the vertical axis representing the detection signal 31 In the P-NMR spectrum, for signals observed in the ranges of -5.2 ppm or higher and less than 0 ppm, -10 ppm or higher and less than -5.2 ppm, and -20 ppm or higher and less than -10 ppm, the absolute values ​​of the areas calculated by Riemann summation are designated as A, B, and C, respectively. Additionally, the horizontal axis is set to the chemical shift of an 85% aqueous phosphoric acid solution as 0 ppm.

[0051] <Composition of the catalyst>

[0052] The catalyst for producing methacrylic acid according to the present embodiment preferably has a composition represented by the following formula (I) in terms of methacrylic acid yield. Additionally, the catalyst may contain a small amount of an element not listed in the following formula (I).

[0053] P a Mo b W c V d Cu e A f E g G h O i (I)

[0054] In formula (I), P, Mo, W, V, Cu, and O represent phosphorus, molybdenum, tungsten, vanadium, copper, and oxygen, respectively. A represents at least one element selected from the group consisting of antimony, bismuth, arsenic, germanium, tellurium, selenium, and silicon. E represents at least one element selected from the group consisting of iron, zinc, chromium, tantalum, cobalt, nickel, manganese, titanium, and niobium. G represents at least one element selected from the group consisting of potassium, rubidium, and cesium. a to i represent the molar ratios of each component, b+c=12, a=0.5 to 3, c=0.22 to 5, d=0.01 to 3, e=0.01 to 2, f=0 to 3, g=0 to 3, h=0.01 to 3, and i is the molar ratio of oxygen required to satisfy the valence of each component.

[0055] In the above formula (I), the molar ratio of W (tungsten), c, satisfies c = 0.22 to 5. By doing so, a structure C with particularly excellent heat resistance is formed well. It is preferable that the lower limit of c be 0.23 or higher, and more preferable that it be 0.3 or higher. In addition, it is preferable that the upper limit of c be 3 or lower, more preferable that it be 2 or lower, even more preferable that it be 1 or lower, and particularly preferable that it be 0.8 or lower.

[0056] In addition, regarding the above formula (I), from the perspective of improving methacrylic acid yield, the lower limit of a is preferably 0.6 or higher, and more preferably 0.7 or higher. Also, the upper limit of a is preferably 2.5 or lower, and more preferably 2 or lower. The lower limit of d is preferably 0.1 or higher, and more preferably 0.15 or higher, and more preferably 0.2 or higher. Also, the upper limit of d is preferably 2.5 or lower, more preferably 2 or lower, and more preferably 1.5 or lower. The lower limit of e is preferably 0.03 or higher, and more preferably 0.05 or higher. Also, the upper limit of e is preferably 2.5 or lower, and more preferably 2 or lower. The lower limit of f is preferably 0.01 or higher, and more preferably 0.1 or higher. Also, the upper limit of f is preferably 2.5 or lower, and more preferably 2 or lower. The upper limit of g is preferably 2 or lower, more preferably 1.5 or lower, and more preferably 1 or lower. The lower limit of h is preferably 0.1 or higher, and more preferably 0.3 or higher. In addition, the upper limit of h is preferably 2.8 or lower, and more preferably 2.5 or lower.

[0057] In addition, the molar ratio of each component is defined as the value obtained by analyzing the component in which the catalyst is dissolved in ammonia water using ICP emission analysis.

[0058] [Method for manufacturing a catalyst for methacrylic acid]

[0059] The catalyst for producing methacrylic acid according to the present embodiment is, 31 If the C / (A+B+C) value in the P-NMR spectrum is 0.015 to 0.085 as described above, it can be manufactured according to a known method for manufacturing catalysts, but it is preferable to manufacture it by a method including the following processes (i) to (iii).

[0060] (i) A process of mixing phosphorus raw material, molybdenum raw material and tungsten raw material with a solvent to prepare a solution or slurry (Solution A) having a pH of 0.1 to 4.

[0061] (ii) A process of obtaining a dried product by drying the above liquid A.

[0062] (iii) A process of obtaining a sintered product by firing the above-mentioned dried product.

[0063] In addition, the method for manufacturing a catalyst for producing methacrylic acid according to the present embodiment may further include a molding process described below.

[0064] Below, each process is explained in detail.

[0065] <Process (i)>

[0066] In process (i), a phosphorus raw material, a molybdenum raw material, and a tungsten raw material are mixed with a solvent to prepare a solution or slurry (Solution A) having a pH of 0.1 to 4. Solution A may be prepared by mixing raw materials of elements other than phosphorus, molybdenum, and tungsten in formula (I), and it is preferable to mix raw materials of element G.

[0067] Solution A can be prepared by dissolving or suspending raw materials of catalyst components, including phosphorus raw materials, molybdenum raw materials, and tungsten raw materials, in a solvent.

[0068] (Raw material of catalyst component)

[0069] The raw materials of the above catalyst components are not particularly limited, and nitrates, carbonates, acetates, ammonium salts, oxides, halides, oxosic acids, oxosates, etc. of each constituent element of the catalyst can be used alone or in combination of two or more types.

[0070] Examples of phosphorus raw materials include phosphoric acid, phosphorus pentoxide, and ammonium phosphate. Examples of molybdenum raw materials include molybdenum oxide such as molybdenum trioxide, ammonium molybdate such as ammonium paramolybdate and ammonium dimolybdate, and molybdenum chloride.

[0071] Examples of tungsten raw materials include tungsten oxide, sodium tungstate, phosphotungstic acid, and ammonium metatungstate; however, it is preferable that the tungsten raw material having a solubility in water at 20°C of 4.1 g / 100 mL or more constitutes 50 mass% or more of the total tungsten raw material. By doing so, a heteropoly acid having poly-valence tungsten is efficiently formed, and a catalyst having C / (A+B+C) within the specified range can be easily obtained. Examples of tungsten raw materials having a solubility in water at 20°C of 4.1 g / 100 mL or more include phosphotungstic acid and ammonium metatungstate. As for the tungsten raw material, it is more preferable that the tungsten raw material having a solubility in water at 20°C of 4.1 g / 100 mL or more constitutes 70 mass% or more, and even more preferable that it constitutes 90 mass% or more.

[0072] In addition, when manufacturing a catalyst containing vanadium and copper, examples of vanadium raw materials include ammonium metavanadate, vanadium pentoxide, vanadium chloride, vanadyl oxalate, etc. Examples of copper raw materials include copper sulfate, copper nitrate, copper oxide, copper carbonate, copper acetate, copper chloride, etc.

[0073] The concentration of the raw material of the catalyst component in liquid A is not particularly limited, but it is preferable to keep it within the range of 5 to 90 mass%.

[0074] (menstruum)

[0075] Examples of the above solvents include water, ethyl alcohol, acetone, etc. One of these may be used, or two or more may be used in combination. Among these, it is preferable to use water from an industrial perspective.

[0076] (Preparation of Amount)

[0077] It is preferable to prepare Solution A by using a preparation container, adding the raw material of the catalyst component to a solvent, and stirring while heating. By doing so, a sufficient amount of heteropoly acid suitable for the production of methacrylic acid is produced.

[0078] The heating temperature can typically be performed in the range of 30 to 150°C, but it is preferable to perform it in the range of 60 to 150°C. By making the heating temperature 60°C or higher, the rate of formation of heteropolyacid can be sufficiently accelerated, and by making it 150°C or lower, the evaporation of the solvent can be suppressed. The lower limit of the heating temperature is more preferably 80°C or higher, and even more preferably 90°C or higher. In addition, the upper limit of the heating temperature is more preferably 130°C or lower, and even more preferably 110°C or lower. Furthermore, depending on the vapor pressure of the solvent used, the process may be concentrated or refluxed during heating, or heat treated under pressurized conditions by operating in a sealed container.

[0079] The heating rate is not particularly limited, but 0.8 to 15°C / min is preferred. By having a heating rate of 0.8°C / min or higher, the time required for process (i) can be shortened. Additionally, by having a heating rate of 15°C / min or lower, heating can be performed using conventional heating equipment.

[0080] It is preferable to perform stirring with a stirring power of 0.01 kW / m³ or more, and more preferable to perform stirring with a stirring power of 0.05 kW / m³ or more. By making the stirring power 0.01 kW / m³ or more, local fluctuations in the temperature, components, and temperature of liquid A are reduced, and a structure suitable for the production of methacrylic acid is stably formed. In addition, from the perspective of the manufacturing cost of the catalyst, it is generally preferable to perform stirring with a stirring power of 3.5 kW / m³ or less.

[0081] (Physical properties of Liquid A)

[0082] The pH of solution A is preferably 0.1 to 4, with a lower limit of 0.5 or higher and an upper limit of 3 or lower. By doing so, the reaction for the formation of heteropoly acids suitable for the production of methacrylic acid is stabilized. Methods for setting the pH of solution A to 0.1 to 4 include, for example, using molybdenum trioxide as a molybdenum raw material, or appropriately selecting raw material compounds and adjusting the content of nitrate ions or oxalate ions.

[0083] <Fairness (ii)>

[0084] In process (ii), liquid A obtained in process (i) is spray-dried to obtain a dried product.

[0085] As drying methods, known methods such as drum drying, airflow drying, evaporative drying, and spray drying can be cited. Among these, spray drying is preferred because it yields a granular dried product and the shape of the dried product is an orderly spherical shape.

[0086] The drying temperature varies depending on the drying method, but it can generally be performed at 100 to 500°C, preferably at a lower limit of 140°C or higher, and preferably at an upper limit of 400°C or lower. It is preferable to perform drying so that the moisture content of the obtained dried product is 4.5 mass% or less, and more preferable to perform drying so that it is 0.1 to 4.5 mass%. These conditions are not particularly limited and can be appropriately selected according to the shape or size of the desired dried product.

[0087] The dried product obtained in process (ii) may be subjected to the molding described below as necessary.

[0088] Molding Process

[0089] In the molding process, the dried product obtained in the above process (ii) is molded as needed. Additionally, molding may be performed after the process (iii) described later.

[0090] The molding method is not particularly limited, and known dry and wet molding methods can be applied, such as tablet compression, press molding, extrusion molding, and assembly molding. The shape of the molded product is not particularly limited, such as cylindrical, ring-shaped, or spherical shapes. Furthermore, when molding, it is preferable to mold only the dried product without adding a carrier, but if necessary, known additives such as graphite or talc may be added. In addition, when using a carrier, the carrier is not particularly limited, but silica is preferably used.

[0091] <Process (iii)>

[0092] In the firing process, the dried product obtained in the above process (ii) and the dried product after molding obtained in the above molding process are fired to obtain a fired product.

[0093] Calcination can be performed under the flow of at least one of an oxygen-containing gas, such as air, and an inert gas, and it is preferable to perform calcination under the flow of an oxygen-containing gas, such as air. Here, an inert gas refers to a gas that does not reduce catalytic activity, and examples include nitrogen, carbon dioxide, helium, and argon. Only one of these may be used, or two or more may be used in combination.

[0094] The shape of the firing vessel is not particularly limited, but a box-shaped or tubular vessel may be used. Additionally, the material may be filled and fired by dividing it into multiple vessels. Among these, it is preferable to use a tubular vessel with a cross-sectional area of ​​1 to 100 cm².

[0095] The firing temperature (maximum temperature during firing) is preferably 200 to 700°C, the lower limit is 320°C or higher, and the upper limit is 450°C or lower.

[0096] The calcined product obtained as described above can be used as a catalyst for the production of methacrylic acid. Additionally, the calcined product may be molded as described in the molding process above. In this embodiment, the calcined product and the calcined product after molding are collectively referred to as catalysts.

[0097] [Method for manufacturing methacrylic acid]

[0098] In the method for producing methacrylic acid according to the present embodiment, methacrolein is oxidized using a catalyst for producing methacrylic acid according to the present embodiment. In addition, in the method for producing methacrylic acid according to the present embodiment, methacrolein is oxidized using a catalyst for producing methacrylic acid produced by the method according to the present embodiment. According to these methods, methacrylic acid can be produced in a high yield.

[0099] The method for producing methacrylic acid according to the present embodiment can be carried out by contacting a catalyst for producing methacrylic acid according to the present embodiment with a source gas containing methacrolein. A fixed-bed reactor may be used for this reaction. The reaction can be carried out by filling the reactor with a catalyst and supplying the source gas to the reactor. The catalyst layer may be a single layer, or multiple catalysts with different activities may be filled by dividing them into multiple layers. In addition, to control activity, the catalyst may be filled by diluting it with an inert support.

[0100] The concentration of methacrolein in the raw gas is preferably 1 to 20 volume%, and the lower limit is 3 volume% or more, and the upper limit is 10 volume% or less. The raw material methacrolein may contain a small amount of impurities that do not substantially affect the reaction, such as lower saturated aldehydes.

[0101] As for the oxygen source for the raw gas, it is not particularly limited, but it is industrially advantageous to use air. Additionally, if necessary, a gas mixed with pure oxygen, such as air, may be used. The ratio of oxygen in the raw gas is not particularly limited, but it is preferable to have 0.4 to 4 moles per 1 mole of metacrolein, and more preferable that the lower limit is 0.5 moles or more and the upper limit is 3 moles or less.

[0102] For economic reasons, the source gas may be diluted with an inert gas such as nitrogen or carbon dioxide. Additionally, water vapor may be added to the source gas. By carrying out the reaction in the presence of water vapor, methacrylic acid can be obtained in a higher yield. The concentration of water vapor in the source gas is preferably 0.1 to 50 volume%, with a lower limit of 1 volume% or more and an upper limit of 40 volume% being more preferable.

[0103] The contact time between the source gas and the catalyst for producing methacrylic acid is preferably 1.5 to 15 seconds, with a lower limit of 2 seconds or more and an upper limit of 10 seconds or less being more preferable. The reaction pressure is preferably 0.1 to 1 MPa (G). Provided, (G) refers to gauge pressure. The reaction temperature is preferably 200 to 450°C, with a lower limit of 250°C or more and an upper limit of 400°C or less being more preferable.

[0104] In the production of methacrylic acid, the position of the catalyst in the reactor, the proportion of the catalyst in the reactor, etc., are not particularly limited, and commonly used forms can be applied.

[0105] [Method for manufacturing methacrylic acid ester]

[0106] In the method for producing a methacrylic acid ester according to the present embodiment, the methacrylic acid produced by the method according to the present embodiment is esterified. That is, the method for producing a methacrylic acid ester according to the present embodiment includes a process of producing methacrylic acid by the method according to the present embodiment and a process of esterifying the said methacrylic acid.

[0107] The alcohol reacted with methacrylic acid is not particularly limited and may include, for example, methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, etc. Examples of the resulting methacrylic acid esters include, for example, methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, butyl methacrylate, isobutyl methacrylate, etc. The esterification reaction may be carried out in the presence of an acidic catalyst such as a sulfonic acid-type cation exchange resin. The temperature during the esterification reaction is preferably 50 to 200°C.

[0108] The pressure during the esterification reaction, the position of the catalyst in the reactor, and the proportion of the catalyst in the reactor are not particularly limited, and commonly used forms can be applied.

[0109] Examples

[0110] Hereinafter, examples of the preparation of the catalyst and reaction examples using the same according to the present embodiment are described together with comparative examples. In the following examples and comparative examples, "part" refers to parts by mass.

[0111] (Composition ratio of catalyst)

[0112] The molar ratio of each component was determined by analyzing the components in which the catalyst was dissolved in ammonia water using ICP emission analysis.

[0113] ( 31 P-NMR measurement)

[0114] 31 P-NMR spectra were measured at room temperature using an AVANCE 300 (Bruker) after packing 300 mg of powdered catalyst into a sample tube. A 7 mm MAS probe was used for the measurement, and the measurement conditions were set as follows: resonance frequency 121.4 MHz, pulse width 5.5 μsec, signal introduction time 0.066 sec, integration cycles 64, repeat waiting time 150 sec, and MAS rotation speed 5000 Hz. With the horizontal axis representing chemical shift (ppm) and the vertical axis representing the detection signal31 In the P-NMR spectrum, for signals observed in the ranges of -5.2 ppm to less than 0 ppm, -10 ppm to less than -5.2 ppm, and -20 ppm to less than -10 ppm, the absolute values ​​of the areas calculated by Riemann sums were designated as A, B, and C, respectively. Additionally, the horizontal axis was set to 0 ppm for the chemical shift of the 85% aqueous phosphoric acid solution.

[0115] (The thermal decomposition temperature of the catalyst)

[0116] The thermal decomposition temperature, which is an indicator of the heat resistance of the catalyst, was measured as follows using a TG / DTA measuring device. 50 mg of alumina was used as a reference, and 50 mg of powdered catalyst was heated from room temperature to 550°C at a rate of 10°C / min in an air atmosphere. In the temperature region of the obtained DTA curve above 380°C, the temperature at which an exothermic reaction of 1.8 μV or more was observed upon a 15°C increase in temperature was defined as the thermal decomposition temperature. A higher thermal decomposition temperature of the catalyst indicates higher heat resistance.

[0117] (Analysis of raw gas and products)

[0118] The analysis of the source gas and product was performed using the following gas chromatography.

[0119] Shimadzu Seisakusho GC-2014 (Column: J&W DB-FFAP, 30 m × 0.32 mm, film thickness 1.0 µm)

[0120] Shimadzu Seisakusho GC-8A (Column: Molecular sieve, 2.0M × 3.0㎜ ID)

[0121] Shimazu Seisakusho GC-8A (Column: Polar Pack Q, 2.0M×3.0㎜ ID)

[0122] The yield of methacrylic acid was calculated by the following formula.

[0123] Yield of methacrylic acid (%) = (N2 / N1) × 100

[0124] Here, N1 is the number of moles of supplied methacrolein, and N2 is the number of moles of methacrylic acid produced.

[0125] (Tungsten raw material)

[0126] The tungsten raw materials used in the examples and comparative examples are as follows.

[0127] Ammonium metatungstate (manufactured by Nippon Muki Kagaku High School) Solubility in water at 20°C: 10g / 100mL

[0128] Phosphotungstic acid (manufactured by Nippon Muki Kagaku High School) Solubility in water at 20℃: 40g / 100mL or more

[0129] <Example 1>

[0130] A diluted solution was prepared by diluting 294.0 parts of molybdenum trioxide, 10.2 parts of ammonium metavanadate, 10.6 parts of ammonium metatungstate, and 30.0 parts of an 85 mass% aqueous phosphoric acid solution with 36 parts of pure water to 1200 parts of pure water at room temperature, and a solution was prepared by dissolving 6.3 parts of copper(II) nitrate trihydrate in 9.0 parts of pure water. The resulting slurry was heated to 95°C at a rate of 2°C / min and stirred for 2 hours. Subsequently, a solution prepared by dissolving 40.4 parts of cesium bicarbonate in 60 parts of pure water at room temperature was mixed and stirred at 95°C for 15 minutes. Subsequently, a solution prepared by dissolving 27.5 parts of ammonium carbonate in 78 parts of pure water was mixed and stirred at 95°C for 15 minutes to obtain Solution A. The pH of Solution A is shown in Table 1.

[0131] The obtained liquid A was heated and evaporated to dry the product, and a dried product was obtained.

[0132] The obtained dried material was pressure-molded and crushed, and classified using a sieve so that the particle size was within the range of 710 μm to 2.36 mm. The obtained granular sieve was calcined at 380°C for 5 hours under air circulation, and the resulting calcined material was used as a catalyst. The oxygen-excluding composition of the said catalyst is P 1. 5Mo 11 .8 W 0.2 V 0. 5Cu0 .15 Cs1 . It was 2. Also, regarding the catalyst in question 31 P-NMR measurements and pyrolysis temperatures were performed. The results are shown in Table 1.

[0133] 8 g of the obtained catalyst was diluted with 10 g of silicon carbide and loaded into a fixed-bed flow-through reactor. Subsequently, a source gas containing 5 volume% methacrolein, 10 volume% oxygen, 30 volume% water vapor, and 55 volume% nitrogen was flowed at a contact time of 178 hr·g / mol, and the oxidation reaction of methacrolein was carried out at a reaction temperature of 300°C. The reaction results are shown in Table 1.

[0134] <Example 2>

[0135] Solution A was obtained in the same manner as in Example 1, except that molybdenum trioxide was 292.1 parts and ammonium metatungstate was 13.6 parts. The pH of Solution A is shown in Table 1.

[0136] The obtained liquid A was heated and evaporated to dry the product, and a dried product was obtained.

[0137] The obtained dried material was used, and a catalyst was obtained in the same manner as in Example 1. The oxygen-excluding composition of the said catalyst is P 1. 5Mo 11 .7 W 0.3 V 0. 5Cu0 . 15 Cs1 . It was 2. Also, regarding the catalyst in question 31 P-NMR measurements and pyrolysis temperatures were performed. The results are shown in Table 1.

[0138] Using the obtained catalyst, the oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The reaction results are shown in Table 1.

[0139] <Example 3>

[0140] Solution A was obtained in the same manner as in Example 1, except that molybdenum trioxide was 287.1 parts and ammonium metatungstate was 22.6 parts. The pH of Solution A is shown in Table 1.

[0141] The obtained liquid A was heated and evaporated to dry the product, and a dried product was obtained.

[0142] The obtained dried material was used, and a catalyst was obtained in the same manner as in Example 1. The oxygen-excluding composition of the said catalyst is P 1. 5Mo 11 .5 W 0.5 V 0. 5Cu0 . 15 Cs1 . It was 2. Also, regarding the catalyst in question 31 P-NMR measurements and pyrolysis temperatures were performed. The results are shown in Table 1.

[0143] Using the obtained catalyst, the oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The reaction results are shown in Table 1.

[0144] <Example 4>

[0145] Solution A was obtained in the same manner as in Example 1, except that molybdenum trioxide was used in an amount of 285.0 parts, an 85 mass% aqueous phosphoric acid solution in an amount of 29.0 parts, and phosphotungstic acid in an amount of 29.7 parts instead of ammonium metatungstate in an amount of 10.6 parts. The pH of Solution A is shown in Table 1.

[0146] The obtained liquid A was heated and evaporated to dry the product, and a dried product was obtained.

[0147] The obtained dried material was used, and a catalyst was obtained in the same manner as in Example 1. The oxygen-excluding composition of the said catalyst is P 1. 5Mo 11 .4 W 0.6 V 0. 5Cu0 . 15 Cs1 .It was 2. Also, regarding the catalyst in question 31 P-NMR measurements and pyrolysis temperatures were performed. The results are shown in Table 1.

[0148] Using the obtained catalyst, the oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The reaction results are shown in Table 1.

[0149] <Example 5>

[0150] Solution A was obtained in the same manner as in Example 1, except that molybdenum trioxide was 277.2 parts and ammonium metatungstate was 40.8 parts. The pH of Solution A is shown in Table 1.

[0151] The obtained liquid A was heated and evaporated to dry the product, and a dried product was obtained.

[0152] The obtained dried material was used, and a catalyst was obtained in the same manner as in Example 1. The oxygen-excluding composition of the said catalyst is P 1. 5Mo 11 .1 W 0.9 V 0. 5Cu0 . 15 Cs1 . It was 2. Also, regarding the catalyst in question 31 P-NMR measurements and pyrolysis temperatures were performed. The results are shown in Table 1.

[0153] Using the obtained catalyst, the oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The reaction results are shown in Table 1.

[0154] <Comparative Example 1>

[0155] Solution A was obtained in the same manner as in Example 1, except that molybdenum trioxide was 270.0 parts and ammonium metatungstate was 53.2 parts. The pH of Solution A is shown in Table 1.

[0156] The obtained liquid A was heated and evaporated to dry the product, and a dried product was obtained.

[0157] The obtained dried material was used, and a catalyst was prepared in the same manner as in Example 1. The oxygen-excluding composition of the said catalyst is P 1. 5Mo 10 .8 W 1.2 V 0. 5Cu0 . 15 Cs1 . It was 2. Also, regarding the catalyst in question 31 P-NMR measurements and pyrolysis temperatures were performed. The results are shown in Table 1.

[0158] Using the obtained catalyst, the oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The reaction results are shown in Table 1.

[0159] <Comparative Example 2>

[0160] Solution A was obtained in the same manner as in Example 1, except that molybdenum trioxide was 255.0 parts and ammonium metatungstate was 79.8 parts. The pH of Solution A is shown in Table 1.

[0161] The obtained liquid A was heated and evaporated to dry the product, and a dried product was obtained.

[0162] The obtained dried material was used, and a catalyst was prepared in the same manner as in Example 1. The oxygen-excluding composition of the said catalyst is P 1. 5Mo 10 .2 W 1.8 V 0. 5Cu0 . 15 Cs1 . It was 2. Also, regarding the catalyst in question 31 P-NMR measurements and pyrolysis temperatures were performed. The results are shown in Table 1.

[0163] Using the obtained catalyst, the oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The reaction results are shown in Table 1.

[0164] <Comparative Example 3>

[0165] Solution A was obtained in the same manner as in Example 1, except that molybdenum trioxide was used in an amount of 270.0 parts, an 85 mass% aqueous phosphoric acid solution in an amount of 27.4 parts, and phosphotungstic acid in an amount of 59.4 parts instead of ammonium metatungstate in an amount of 10.6 parts. The pH of Solution A is shown in Table 1.

[0166] The obtained liquid A was heated and evaporated to dry the product, and a dried product was obtained.

[0167] The obtained dried material was used, and a catalyst was prepared in the same manner as in Example 1. The oxygen-excluding composition of the said catalyst is P 1. 47 Mo 10 .8 W 1.2 V 0. 5Cu0 . 15 Cs1 . It was 2. Also, regarding the catalyst in question 31 P-NMR measurements and pyrolysis temperatures were performed. The results are shown in Table 1.

[0168] Using the obtained catalyst, the oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The reaction results are shown in Table 1.

[0169] <Comparative Example 4>

[0170] 300.0 parts of phosphotungstic acid were pressure-molded and crushed, and then sieved to obtain a particle size within the range of 710 μm to 2.36 mm. The obtained granular sieves were calcined at 380°C for 5 hours under air circulation, and the resulting calcined product was used as a catalyst. The oxygen-excluding composition of the said catalyst was P1W 12 was. Also, regarding the catalyst in question 31 P-NMR measurements and pyrolysis temperatures were performed. The results are shown in Table 1.

[0171] Using the obtained catalyst, the oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The reaction results are shown in Table 1.

[0172] <Comparative Example 5>

[0173] 300.0 parts of phosphomolybdic acid (manufactured by Nippon Muki Kagaku High School) were calcined at 380°C for 5 hours, the resulting powder was crushed, and the particles were sieved to obtain a particle size within the range of 710 μm to 2.36 mm. The resulting granular sieve was calcined at 380°C for 5 hours under air circulation to prepare a catalyst. The oxygen-excluding composition of the catalyst was P1Mo 12 was. Also, regarding the catalyst in question 31 P-NMR measurements and pyrolysis temperatures were performed. The results are shown in Table 1.

[0174] Using the obtained catalyst, the oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The reaction results are shown in Table 1.

[0175]

[0176] As shown in Table 1, 31 Examples 1 to 5, which used a catalyst having C / (A+B+C) within the specified range in the P-NMR spectrum, had a high thermal decomposition temperature of the catalyst and were able to obtain methacrylic acid in a high yield.

[0177] In addition, a methacrylic acid ester can be obtained by esterifying the methacrylic acid obtained in this embodiment. Industrial applicability

[0178] According to the present invention, a catalyst with high heat resistance and capable of producing methacrylic acid in high yield can be provided.

Claims

Claim 1 A catalyst used in the production of methacrylic acid by the oxidation of methacrolein, wherein the catalyst contains a heteropoly acid comprising phosphorus, molybdenum, and tungsten, and the catalyst 31 A catalyst for producing methacrylic acid, wherein in a P-NMR spectrum, the area of ​​the signal observed in the range of -5.2 ppm or more and less than 0 ppm is A, the area of ​​the signal observed in the range of -10 ppm or more and less than -5.2 ppm is B, and the area of ​​the signal observed in the range of -20 ppm or more and less than -10 ppm is C, and C / (A+B+C) is 0.015 to 0.

085. Claim 2 In paragraph 1, the above 31 A catalyst for the production of methacrylic acid, wherein B / (A+B+C) in the P-NMR spectrum is 0.1 to 0.

485. Claim 3 In paragraph 1 or 2, the above 31 A catalyst for the production of methacrylic acid, wherein A / (A+B+C) in the P-NMR spectrum is 0.5 to 0.

885. Claim 4 In paragraph 1, the above 31 A catalyst for the production of methacrylic acid, wherein C / (A+B+C) in the P-NMR spectrum is 0.02 to 0.

08. Claim 5 In paragraph 4, the above 31 A catalyst for the production of methacrylic acid, wherein B / (A+B+C) is 0.2 to 0.45 in the P-NMR spectrum. Claim 6 In paragraph 4 or 5, the above 31 A catalyst for the production of methacrylic acid, wherein A / (A+B+C) is 0.53 to 0.75 in the P-NMR spectrum. Claim 7 A catalyst for the production of methacrylic acid according to claim 1, having a composition represented by the following formula (I). a Mo b W c V d Cu e A f E g G h O i (I) In formula (I), P, Mo, W, V, Cu, and O represent phosphorus, molybdenum, tungsten, vanadium, copper, and oxygen, respectively. A represents at least one element selected from the group consisting of antimony, bismuth, arsenic, germanium, tellurium, selenium, and silicon. E represents at least one element selected from the group consisting of iron, zinc, chromium, tantalum, cobalt, nickel, manganese, titanium, and niobium. G represents at least one element selected from the group consisting of potassium, rubidium, and cesium. a to i represent the molar ratios of each component, b+c=12, a=0.5 to 3, c=0.22 to 5, d=0.01 to 3, e=0.01 to 2, f=0 to 3, g=0 to 3, h=0.01 to 3, and i is the molar ratio of oxygen required to satisfy the valence of each component. Claim 8 In claim 7, a catalyst for producing methacrylic acid, wherein c=0.22 to 3 in the above formula (I). Claim 9 A method for manufacturing a catalyst for producing methacrylic acid as described in claim 1, comprising: (i) a process of mixing a phosphorus raw material, a molybdenum raw material, and a tungsten raw material with a solvent to prepare a solution or slurry (solution A) having a pH of 0.1 to 4; (ii) a process of drying the solution A to obtain a dried product; and (iii) a process of calcining the dried product to obtain a calcined product. Claim 10 A method for producing a catalyst for producing methacrylic acid according to claim 9, wherein in process (i) above, the tungsten raw material having a solubility in water at 20°C of 4.1 g / 100 mL or more is 50 mass% or more of the total tungsten raw material. Claim 11 A method for producing a catalyst for producing methacrylic acid, wherein, in claim 9 or 10, in process (i), the pH of liquid A is 0.1 to 3. Claim 12 A method for producing methacrylic acid, comprising a process of oxidizing methacrolein using a catalyst for producing methacrylic acid described in claim 1 and producing methacrylic acid. Claim 13 A method for producing methacrylic acid, comprising a process of oxidizing methacrolein using a catalyst for producing methacrylic acid produced by the method described in claim 9, and producing methacrylic acid. Claim 14 A method for producing a methacrylic acid ester, comprising a process of esterifying methacrylic acid produced by the method described in claim 12 or 13.

Citation Information

Patent Citations

  • Catalyst

    JP1980001880A

  • Catalyst for manufacturing methacrylic acid and manufacturing method therefor, and manufacturing method of methacrylic acid

    JP2016168591A

  • Dehydration granules for catalyst manufacture, catalyst, and manufacturing method compound

    JP2021041403A

  • Process for preparing heteropolyacids

    KR1019790001938B1

  • A preparation method of heteropolyacid catalyst andpreparation method of metacrylic acid using thereof

    KR1020030093654A