Catalyst for the production of methacrylic acid, method for the production of the same, and method for the production of methacrylic acid and methacrylic acid esters using the same
A heteropoly acid catalyst with specific X-ray diffraction characteristics and thermal stability is used to enhance the heat resistance and yield of methacrylic acid production, overcoming the limitations of existing catalysts.
Patent Information
- Application Number
- KR1020247034440
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-03-24
- Filing Date
- 2023-03-23
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2043-03-23
AI Technical Summary
Existing catalysts for producing methacrylic acid have low heat resistance and insufficient lifespan, leading to low yield and efficiency in industrial applications.
A catalyst comprising a heteropoly acid with specific X-ray diffraction peak intensities and thermal stability characteristics, containing phosphorus, molybdenum, and tungsten, is developed to enhance heat resistance and yield.
The catalyst achieves high heat resistance and produces methacrylic acid with improved yield and selectivity, addressing the limitations of existing catalysts.
Smart Images

Figure 112024112235767-PCT00001
Abstract
Description
Technology Field
[0001] The present invention relates to a catalyst for the production of methacrylic acid, a method for producing the same, and a method for producing methacrylic acid and methacrylic acid esters using the same. Background Technology
[0002] As a catalyst for the production of methacrylic acid (hereinafter also referred to simply as "catalyst") used when producing methacrylic acid by the oxidation of methacrolein, a heteropolyacid-based catalyst including molybdenum and phosphorus is known, for example. A heteropolyacid is a condensed oxyacid formed by the oxide of a heteroatom and 12 coordination atoms (hereinafter referred to as "poly atoms") that form the basic framework of a polyacid. Examples of heteropolyacid-based catalysts include a proton-type heteropolyacid in which the counter cation is a proton, and a heteropolysalt in which a portion of the proton is substituted with a cation other than a proton (hereinafter, the proton-type heteropolyacid is simply referred to as "heteropolyacid," and at least one selected from the proton-type heteropolyacid and the heteropolysalt is simply referred to as "heteropolyacid (salt)").
[0003] Regarding the structure of heteropolyacid (salt), Non-patent Literature 1 describes that phosphorus, silicon, arsenic, germanium, titanium, antimony, etc. can be heteroatoms, and tungsten, molybdenum, vanadium, niobium, tantalum, etc. can be polyatoms of the heteropolyacid (salt). In addition, Kegyn type, Dawson type, and Plésler type are described as basic structures of heteropolyacid (salt).
[0004] In addition, Patent Document 1 discloses a catalyst for the production of methacrylic acid comprising a Keggine-type heteropolyphosphate having a composition represented by the following formula.
[0005] P a Mo b V c X d Y e O f
[0006] (In the formula, P, Mo, V, and O represent phosphorus, molybdenum, vanadium, and oxygen, respectively; X represents at least one element selected from potassium, rubidium, cesium, and thallium; and Y represents at least one element selected from copper, arsenic, antimony, boron, silver, bismuth, iron, cobalt, lanthanum, and cerium. a, b, c, d, e, and f represent the atomic ratios of P, Mo, V, X, Y, and O, respectively; when b=12, a, c, d, and e are each independently values greater than 0 and less than or equal to 3, and f is a value determined by the oxidation state and atomic ratio of each element other than oxygen.)
[0007] As a Keggin-type heteropoly acid, H3PMo 12 O 40 , H4PMo 11 VO 40 H3, PW 12 O 40 Etc. is known, and in Non-Patent Literature 1, H3PMo 12 O 40 Ina H4PMo 11 VO 40 Compared to H3, PW 12 O 40 It is disclosed that the thermal decomposition temperature of is high. Meanwhile, Non-patent Literature 2 describes H3PMo as a catalyst for the production of methacrylic acid. 12 O 40 If used, methacrylic acid is obtained well, but PW 12 O 40 It is stated that using it results in very low activity and selectivity. Prior art literature
[0008] Japanese Patent Publication No. 2003-010691
[0009] Toshio Okuhara, Noritaka Mizuno, Makoto Misono, Advances in Catalysis, volume 41.Shuhei Yasuda, Atsuki Iwakura, Jun Hirata, Mitsuru Kanno, Wataru Ninomiya, Ryoichi Otomo, Yuichi Kamiya, Catalysis Communications, 125(2019), 43-47. The problem to be solved
[0010] However, known catalysts for the production of methacrylic acid have low heat resistance and their lifespan is still insufficient. Therefore, in order to use them as industrial catalysts, there is a need to develop a catalyst that has high heat resistance and can produce methacrylic acid with a high yield.
[0011] The object of the present invention is to provide a catalyst that has high heat resistance and can produce methacrylic acid with a high yield. Additionally, the object of the present invention is to provide a method for producing methacrylic acid and methacrylic acid esters using this catalyst. means of solving the problem
[0012] The inventors, having conducted a thorough examination in consideration of the above problem, discovered that the problem can be solved by using a catalyst having a specific peak in powder X-ray measurement, and thus completed the present invention.
[0013] That is, the present invention includes the following.
[0014] [1]: A catalyst used to produce methacrylic acid by the oxidation of methacrolein, and
[0015] Containing a heteropoly acid containing phosphorus, molybdenum, and tungsten,
[0016] (a1) In powder X-ray diffraction measurement at 25℃, when the intensity of the diffraction peak (peak A) with 2θ=26.1±0.2° is denoted as IA and the intensity of the diffraction peak (peak B) with 2θ=23.0±0.2° is denoted as IB, IB / IA is 0.015 or less, and
[0017] (b) A catalyst for the production of methacrylic acid, wherein the lowest temperature T1 at which a diffraction peak (peak E) with 2θ=27.1±0.2° appears is 440°C or higher when powder X-ray diffraction measurements are performed at 10°C intervals starting from 400°C while increasing the temperature at 10°C / min.
[0018] [2]: A catalyst for producing methacrylic acid as described in [1], wherein the IB / IA is 0.01 or less.
[0019] [3]: (a2) A catalyst for producing methacrylic acid as described in [1] or [2], wherein, when the intensity of the diffraction peak (peak C) at 2θ=34.1±0.2° is taken as IC in powder X-ray diffraction measurements at 25°C, the IC / IA is 0.0055 or less.
[0020] [4]: A catalyst for producing methacrylic acid as described in [3], wherein the IC / IA is 0.0005 to 0.0055.
[0021] [5]: A catalyst for producing methacrylic acid as described in [3] or [4], wherein the IC / IA is 0.001 to 0.0053.
[0022] [6]: (a3) A catalyst for producing methacrylic acid as described in any one of [1] to [5], wherein, in powder X-ray diffraction measurements at 25°, the ID / IA is 0.003 or less when the intensity of the diffraction peak (peak D) at 2θ=48.3±0.2° is taken as ID.
[0023] [7]: A catalyst for producing methacrylic acid as described in any one of [1] to [6], wherein T1 is 440 to 500°C.
[0024] [8]: A catalyst for the production of methacrylic acid described in any one of [1] to [7] having a composition represented by the following formula (I).
[0025] P a Mo b W c V d Cu e A f E g G h O i (I)
[0026] In formula (I), P, Mo, W, V, Cu, and O represent phosphorus, molybdenum, tungsten, vanadium, copper, and oxygen, respectively. A represents at least one element selected from the group consisting of antimony, bismuth, arsenic, germanium, tellurium, selenium, and silicon. E represents at least one element selected from the group consisting of iron, zinc, chromium, tantalum, cobalt, nickel, manganese, titanium, and niobium. G represents at least one element selected from the group consisting of potassium, rubidium, and cesium. a to i represent the molar ratios of each component, b+c=12, a=0.5 to 3, c=0.22 to 5, d=0.01 to 3, e=0.01 to 2, f=0 to 3, g=0 to 3, h=0.01 to 3, and i is the molar ratio of oxygen required to satisfy the valence of each component.
[0027] [9]: A catalyst for producing methacrylic acid as described in [8], wherein c=0.22 to 3 in the above formula (I).
[0028]
[10] : A method for producing a catalyst for producing methacrylic acid as described in any one of [1] to [9], and
[0029] (i) a process of mixing phosphorus raw material, molybdenum raw material and tungsten raw material with a solvent to prepare a solution or slurry (Solution A) having a pH of 0.1 to 4, and
[0030] (ii) A process of obtaining a dried product by drying the above liquid A, and
[0031] (iii) A process of obtaining a sintered product by sintering the above-mentioned dried product.
[0032] A method for preparing a catalyst for the production of methacrylic acid comprising
[0033]
[11] : A method for producing a catalyst for producing methacrylic acid as described in
[10] , wherein in the above process (i), the tungsten raw material having a solubility in water at 20°C of 4.1 g / 100 mL or more is 50 mass% or more of the total tungsten raw material.
[0034]
[12] : A method for producing a catalyst for producing methacrylic acid as described in
[10] or
[11] , wherein in the above process (i), the pH of the above liquid A is 0.1 to 3.
[0035]
[13] : A method for producing methacrylic acid comprising a process of oxidizing methacrolein using a catalyst for producing methacrylic acid described in any one of [1] to [9] and producing methacrylic acid.
[0036]
[14] : A method for producing methacrylic acid comprising the process of oxidizing methacrolein and producing methacrylic acid using a catalyst for producing methacrylic acid produced by any one of
[10] to
[12] .
[0037]
[15] : A method for producing a methacrylic acid ester comprising a process of esterifying methacrylic acid produced by the method described in
[13] or
[14] . Effects of the invention
[0038] According to the present invention, a catalyst with high heat resistance and capable of producing methacrylic acid with a high yield can be provided. Specific details for implementing the invention
[0039] Embodiments of the present invention are described below, but the present invention is not limited to the following.
[0040] In addition, in this specification, a numerical range indicated using “to” means a range that includes the values described before and after “to” as lower and upper limits, and “A to B” means greater than or equal to A and less than or equal to B.
[0041] [Catalyst for Methacrylic Acid Production]
[0042] The catalyst for producing methacrylic acid according to the present embodiment is a catalyst used when producing methacrylic acid by the oxidation of methacrolein, contains a heteropoly acid comprising phosphorus, molybdenum and tungsten, and satisfies the following conditions (a1) and (b).
[0043] (a1) In powder X-ray diffraction measurement at 25°, when the intensity of the diffraction peak (peak A) with 2θ=26.1±0.2° is denoted as IA and the intensity of the diffraction peak (peak B) with 2θ=23.0±0.2° is denoted as IB, IB / IA is 0.015 or less.
[0044] (b) When powder X-ray diffraction measurements are taken at 10°C intervals starting from 400°C while increasing the temperature by 10°C / min, the lowest temperature T1 at which a diffraction peak (peak E) with 2θ=27.1±0.2° appears is 440°C or higher.
[0045] These catalysts have high heat resistance and can also produce methacrylic acid in high yield.
[0046] In addition, the catalyst for producing methacrylic acid according to the present embodiment is also preferably satisfied with the following conditions (a2) or (a3), and more preferably satisfied with (a2) and (a3).
[0047] (a2) When measuring powder X-ray diffraction at 25°, the intensity of the diffraction peak (peak C) at 2θ=34.1±0.2° is set as IC, and the IC / IA is 0.0055 or less.
[0048] (a3) When measuring powder X-ray diffraction at 25°, ID is the intensity of the diffraction peak (peak D) at 2θ=48.3±0.2°, ID / IA is 0.003 or less.
[0049] X-ray diffraction measurement of catalyst powder
[0050] (Conditions (a1) to (a3))
[0051] When a catalyst containing a heteropolyacid containing phosphorus, molybdenum, and tungsten is subjected to powder X-ray diffraction at 25°, the diffraction peak observed at 2θ = 26.1±0.2° (Peak A) and the diffraction peak observed at 2θ = 23.0±0.2° (Peak B) are peaks that originate mainly from the heteropolyacid structure. Specifically, Peak A originates from a structure in which the heterovalence is mainly phosphorus and at least 10 of the polyatoms are molybdenum (hereinafter also referred to as Structure A). Additionally, Peak B originates from a structure in which the heterovalence is mainly phosphorus, 6 to 11 of the polyatoms are elements other than molybdenum such as tungsten or vanadium, and the remainder is molybdenum (hereinafter also referred to as Structure B). Structure B causes a decrease in activity in the oxidation reaction of methacrolein.
[0052] In addition, the diffraction peak observed at 2θ=34.1±0.2° (peak C) and the diffraction peak observed at 2θ=48.3±0.2° (peak D) are peaks originating from oxide structures composed mainly of elements that do not form heteropolyacid structures. Specifically, peak C originates mainly from a molybdenum-containing oxide structure. Also, peak D originates mainly from a tungsten-containing oxide structure. These oxides promote sequential oxidation in the oxidation reaction of methacrolein and cause a decrease in the selectivity of methacrylic acid.
[0053] In the powder X-ray diffraction measurement of the catalyst for producing methacrylic acid according to the present embodiment at 25°C, when the intensity of peak A is denoted as IA and the intensity of peak B as IB, IB / IA is 0.015 or less. At this time, it is thought that the content of structure B, which is unsuitable for the production of methacrylic acid, is sufficiently low and a good methacrylic acid yield can be obtained. The upper limit of IB / IA is preferably 0.01 or less, and more preferably 0.005 or less.
[0054] In addition, when the intensity of peak C is denoted as IC, it is preferable that IC / IA be 0.0055 or less. At this time, it is believed that the content of molybdenum-containing oxides unsuitable for methacrylic acid production is sufficiently low, and a good methacrylic acid yield can be obtained. The upper limit of IC / IA is more preferably 0.0053 or less, and even more preferably 0.0052 or less. Furthermore, from the perspective of improving the activity of the methacrolein oxidation reaction, the lower limit of IC / IA is preferably 0.0005 or more, and even more preferably 0.001 or more.
[0055] As a method for obtaining a catalyst having IB / IA and IC / IA within the specified range, for example, a method of preparing the catalyst by a method including processes (i) to (iii) described below, and adjusting the amount of tungsten raw material used in process (i) and the pH of the obtained liquid A.
[0056] In addition, when the intensity of peak D is set to ID, ID / IA is preferably 0.003 or less, more preferably 0.002 or less, and even more preferably 0.001 or less.
[0057] As a method for obtaining a catalyst having an ID / IA within the specified range, for example, a method of preparing a catalyst by a method including processes (i) to (iii) described below, and in process (i), using 50 mass% or more of a tungsten raw material having a solubility in water at 20°C of 4.1 g / 100 mL or more of the total tungsten raw material.
[0058] (condition(b))
[0059] When powder X-ray diffraction measurements are performed while increasing the temperature of a catalyst containing a heteropoly acid comprising phosphorus, molybdenum, and tungsten, the peak observed at 2θ = 27.1 ± 0.2° (peak E) originates from molybdenum oxide generated by the decomposition of the heteropoly acid. For the catalyst for methacrylate production according to the present embodiment, when powder X-ray diffraction measurements are performed at 10°C intervals starting from 400°C while increasing the temperature at 10°C / min, the lowest temperature T1 at which peak D appears is 440°C or higher. A catalyst with T1 of 440°C or higher implies that the heteropoly acid in the catalyst forms a thermodynamically metastable crystal structure. At this time, the heteropoly acid is considered to have high heat resistance and also possess active sites suitable for the oxidation reaction of methacrolein. The lower limit of T1 is preferably 450°C or higher, more preferably 460°C or higher, and even more preferably 470°C or higher. In addition, the upper limit of T1 is preferably 500℃ or lower, more preferably 490℃ or lower, and even more preferably 480℃ or lower.
[0060] As a method for obtaining a catalyst that exhibits a specified range of T1, for example, a method of manufacturing the catalyst by a method including processes (i) to (iii) described below, and adjusting the amount of tungsten raw material or G element raw material used in process (i).
[0061] For X-ray measurement of the catalyst powder, for example, the X-ray diffraction device X'PertProMPD manufactured by PANalytical and the high-temperature strip heater chamfer manufactured by Anton Paar may be used. For the measurement, CuKα rays (λ=0.154 nm) are used, with an output of 45 kV, 40 mA, and a measurement range of 5 to 60°. The goniometer radius is set to 240 mm, and an automatic continuously variable slit or a fixed slit is used for the diverging slit. Additionally, when using an automatic continuously variable slit, the slit size is set to 0 to 8.0 mm, and when using a fixed slit, the slit size is set to 1.75 mm and the slit opening angle is set to 1.00°. From the obtained X-ray diffraction pattern, the Kα2 rays are separated to perform peak search, and IA, IB, IC, and ID are determined. The conditions for peak search are: minimum significance: 1 degree, minimum peak chip: 0.2 degrees, maximum peak chip: 1 degree, peak base width: 2 degrees, and method: minimum value of the second derivative. Peak search can be performed, for example, using Panalytical's High Score Plus. In addition, the lowest temperature at which peak E appears is the lowest temperature at which a peak is detected at 2θ = 27.1 ± 0.2° by performing peak search on the X-ray diffraction pattern obtained by measuring powder X-ray diffraction at 10° intervals starting from 400°C while heating the catalyst at 10°C / min.
[0062] <Composition of the catalyst>
[0063] The catalyst for producing methacrylic acid according to the present embodiment preferably has a composition represented by the following formula (I) in terms of methacrylic acid yield. Additionally, the catalyst may contain a small amount of an element not listed in the following formula (I).
[0064] P a Mo b W c V d Cu e A f E g G h O i (I)
[0065] In formula (I), P, Mo, W, V, Cu, and O represent phosphorus, molybdenum, tungsten, vanadium, copper, and oxygen, respectively. A represents at least one element selected from the group consisting of antimony, bismuth, arsenic, germanium, tellurium, selenium, and silicon. E represents at least one element selected from the group consisting of iron, zinc, chromium, tantalum, cobalt, nickel, manganese, titanium, and niobium. G represents at least one element selected from the group consisting of potassium, rubidium, and cesium. a to i represent the molar ratios of each component, b+c=12, a=0.5 to 3, c=0.22 to 5, d=0.01 to 3, e=0.01 to 2, f=0 to 3, g=0 to 3, h=0.01 to 3, and i is the molar ratio of oxygen required to satisfy the valence of each component.
[0066] In the above formula (I), the molar ratio of W (tungsten), c, satisfies c = 0.22 to 5. By doing so, a catalyst satisfying conditions (a1) and (b) can be easily obtained. It is preferable that the lower limit of c be 0.23 or higher, and more preferable that it be 0.3 or higher. In addition, it is preferable that the upper limit of c be 3 or lower, more preferable that it be 2 or lower, even more preferable that it be 1 or lower, and particularly preferable that it be 0.8 or lower.
[0067] In addition, regarding the above formula (I), from the perspective of improving methacrylic acid yield, the lower limit of a is preferably 0.6 or higher, and more preferably 0.7 or higher. Also, the upper limit of a is preferably 2.5 or lower, and more preferably 2 or lower. The lower limit of d is preferably 0.1 or higher, and more preferably 0.15 or higher, and more preferably 0.2 or higher. Also, the upper limit of d is preferably 2.5 or lower, more preferably 2 or lower, and more preferably 1.5 or lower. The lower limit of e is preferably 0.03 or higher, and more preferably 0.05 or higher. Also, the upper limit of e is preferably 2.5 or lower, and more preferably 2 or lower. The lower limit of f is preferably 0.01 or higher, and more preferably 0.1 or higher. Also, the upper limit of f is preferably 2.5 or lower, and more preferably 2 or lower. The upper limit of g is preferably 2 or lower, more preferably 1.5 or lower, and more preferably 1 or lower. The lower limit of h is preferably 0.1 or higher, and more preferably 0.3 or higher. In addition, the upper limit of h is preferably 2.8 or lower, and more preferably 2.5 or lower.
[0068] In addition, the molar ratio of each component is defined as the value obtained by analyzing the component in which the catalyst is dissolved in ammonia water using ICP emission analysis.
[0069] [Method for manufacturing a catalyst for methacrylic acid]
[0070] The catalyst for producing methacrylic acid according to the present embodiment comprises phosphorus, molybdenum, and tungsten, and can be produced in accordance with a known method for producing catalysts if conditions (a1) and (b) are satisfied, but it is preferable to produce it by a method including the following processes (i) to (iii).
[0071] (i) A process of mixing phosphorus raw material, molybdenum raw material and tungsten raw material with a solvent to prepare a solution or slurry (Solution A) having a pH of 0.1 to 4.
[0072] (ii) A process of obtaining a dried product by drying the above liquid A.
[0073] (iii) A process of obtaining a sintered product by firing the above-mentioned dried product.
[0074] In addition, the method for manufacturing a catalyst for producing methacrylic acid according to the present embodiment may further include a molding process described below.
[0075] Below, each process is explained in detail.
[0076] <Process (i)>
[0077] In process (i), a phosphorus raw material, a molybdenum raw material, and a tungsten raw material are mixed with a solvent to prepare a solution or slurry (Solution A) having a pH of 0.1 to 4. Solution A may be prepared by mixing raw materials of elements other than phosphorus, molybdenum, and tungsten in formula (I), and it is preferable to mix raw materials of element G.
[0078] Solution A can be prepared by dissolving or suspending raw materials of catalyst components, including phosphorus raw materials, molybdenum raw materials, and tungsten raw materials, in a solvent.
[0079] (Raw material of catalyst component)
[0080] The raw materials of the above catalyst components are not particularly limited, and nitrates, carbonates, acetates, ammonium salts, oxides, halides, oxosic acids, oxosates, etc. of each constituent element of the catalyst can be used alone or in combination of two or more types.
[0081] Examples of phosphorus raw materials include phosphoric acid, phosphorus pentoxide, and ammonium phosphate. Examples of molybdenum raw materials include molybdenum oxide such as molybdenum trioxide, ammonium molybdate such as ammonium paramolybdate and ammonium dimolybdate, and molybdenum chloride.
[0082] Examples of tungsten raw materials include tungsten oxide, sodium tungstate, phosphotungstic acid, and ammonium metatungstate, but it is preferable that the tungsten raw material having a solubility in water at 20°C of 4.1 g / 100 mL or more constitutes 50 mass% or more of the total tungsten raw material. By doing so, a catalyst satisfying conditions (a1) and (b) can be easily obtained. Examples of tungsten raw materials having a solubility in water at 20°C of 4.1 g / 100 mL or more include phosphotungstic acid and ammonium metatungstate. As for the tungsten raw material, it is more preferable that the tungsten raw material having a solubility in water at 20°C of 4.1 g / 100 mL or more constitutes 70 mass% or more, and even more preferable that it constitutes 90 mass% or more.
[0083] In addition, when manufacturing a catalyst containing vanadium and copper, examples of vanadium raw materials include ammonium metavanadate, vanadium pentoxide, vanadium chloride, vanadyl oxalate, etc. Examples of copper raw materials include copper sulfate, copper nitrate, copper oxide, copper carbonate, copper acetate, copper chloride, etc.
[0084] The concentration of the raw material of the catalyst component in liquid A is not particularly limited, but it is preferable to keep it within the range of 5 to 90 mass%.
[0085] (menstruum)
[0086] Examples of the above solvents include water, ethyl alcohol, acetone, etc. One of these may be used, or two or more may be used in combination. Among these, it is preferable to use water from an industrial perspective.
[0087] (Preparation of Amount)
[0088] It is preferable to prepare Solution A by using a preparation container, adding the raw material of the catalyst component to a solvent, and stirring while heating. By doing so, a sufficient amount of heteropoly acid suitable for the production of methacrylic acid is produced.
[0089] The heating temperature can typically be performed in the range of 30 to 150°C, but it is preferable to perform it in the range of 60 to 150°C. By making the heating temperature 60°C or higher, the rate of formation of heteropolyacid can be sufficiently accelerated, and by making it 150°C or lower, the evaporation of the solvent can be suppressed. The lower limit of the heating temperature is more preferably 80°C or higher, and even more preferably 90°C or higher. In addition, the upper limit of the heating temperature is more preferably 130°C or lower, and even more preferably 110°C or lower. Furthermore, depending on the vapor pressure of the solvent used, the process may be concentrated or refluxed during heating, or heat treated under pressurized conditions by operating in a sealed container.
[0090] The heating rate is not particularly limited, but 0.8 to 15°C / min is preferred. By having a heating rate of 0.8°C / min or higher, the time required for process (i) can be shortened. Additionally, by having a heating rate of 15°C / min or lower, heating can be performed using conventional heating equipment.
[0091] It is preferable to perform stirring with a stirring power of 0.01 kW / m³ or more, and more preferable to perform stirring with a stirring power of 0.05 kW / m³ or more. By making the stirring power 0.01 kW / m³ or more, local fluctuations in the temperature, composition, and temperature of liquid A are reduced, and a structure suitable for the production of α,β-unsaturated carboxylic acid is stably formed. In addition, from the perspective of the manufacturing cost of the catalyst, it is generally preferable to perform stirring with a stirring power of 3.5 kW / m³ or less.
[0092] (Physical properties of Liquid A)
[0093] The pH of solution A is preferably 0.1 to 4, with a lower limit of 0.5 or higher and an upper limit of 3 or lower. By doing so, the reaction for the formation of heteropoly acids suitable for the production of α,β-unsaturated carboxylic acids is stabilized. Methods for setting the pH of solution A to 0.1 to 4 include, for example, using molybdenum trioxide as a molybdenum raw material, or appropriately selecting raw material compounds and adjusting the content of nitrate ions or oxalate ions.
[0094] <Fairness (ii)>
[0095] In process (ii), liquid A obtained in process (i) is spray-dried to obtain a dried product.
[0096] As drying methods, known methods such as drum drying, airflow drying, evaporative drying, and spray drying can be cited. Among these, spray drying is preferred because it yields a granular dried product and the shape of the dried product is an orderly spherical shape.
[0097] The drying temperature varies depending on the drying method, but it can generally be performed at 100 to 500°C, preferably at a lower limit of 140°C or higher, and preferably at an upper limit of 400°C or lower. It is preferable to perform drying so that the moisture content of the obtained dried product is 4.5 mass% or less, and more preferable to perform drying so that it is 0.1 to 4.5 mass%. These conditions are not particularly limited and can be appropriately selected according to the shape or size of the desired dried product.
[0098] The dried product obtained in process (ii) may be subjected to the molding described below as necessary.
[0099] Molding Process
[0100] In the molding process, the dried product obtained in the above process (ii) is molded as needed. Additionally, molding may be performed after the process (iii) described later.
[0101] The molding method is not particularly limited, and known dry and wet molding methods can be applied, such as tablet compression, press molding, extrusion molding, and assembly molding. The shape of the molded product is not particularly limited, such as cylindrical, ring-shaped, or spherical shapes. Furthermore, when molding, it is preferable to mold only the dried product without adding a carrier, but if necessary, known additives such as graphite or talc may be added. In addition, when using a carrier, the carrier is not particularly limited, but silica is preferably used.
[0102] <Process (iii)>
[0103] In the firing process, the dried product obtained in the above process (iii) and the dried product after molding obtained in the above molding process are fired to obtain a fired product.
[0104] Calcination can be performed under the flow of at least one of an oxygen-containing gas, such as air, and an inert gas, and it is preferable to perform calcination under the flow of an oxygen-containing gas, such as air. Here, an inert gas refers to a gas that does not reduce catalytic activity, and examples include nitrogen, carbon dioxide, helium, and argon. Only one of these may be used, or two or more may be used in combination.
[0105] The shape of the firing vessel is not particularly limited, but a box-shaped or tubular vessel may be used. Additionally, the material may be filled and fired by dividing it into multiple vessels. Among these, it is preferable to use a tubular vessel with a cross-sectional area of 1 to 100 cm².
[0106] The firing temperature (maximum temperature during firing) is preferably 200 to 700°C, the lower limit is 320°C or higher, and the upper limit is 450°C or lower.
[0107] The calcined product obtained as described above can be used as a catalyst for the production of methacrylic acid. Additionally, the calcined product may be molded as described in the molding process above. In this embodiment, the calcined product and the calcined product after molding are collectively referred to as catalysts.
[0108] [Method for manufacturing methacrylic acid]
[0109] In the method for producing methacrylic acid according to the present embodiment, methacrolein is oxidized using a catalyst for producing methacrylic acid according to the present embodiment. In addition, in the method for producing methacrylic acid according to the present embodiment, methacrolein is oxidized using a catalyst for producing methacrylic acid produced by the method according to the present embodiment. According to these methods, methacrylic acid can be produced in a high yield.
[0110] The method for producing methacrylic acid according to the present embodiment can be carried out by contacting a catalyst for producing methacrylic acid according to the present embodiment with a source gas containing methacrolein. A fixed-bed reactor may be used for this reaction. The reaction can be carried out by filling the reactor with a catalyst and supplying the source gas to the reactor. The catalyst layer may be a single layer, or multiple catalysts with different activities may be filled by dividing them into multiple layers. In addition, to control activity, the catalyst may be filled by diluting it with an inert support.
[0111] The concentration of methacrolein in the raw gas is preferably 1 to 20 volume%, and the lower limit is 3 volume% or more, and the upper limit is 10 volume% or less. The raw material methacrolein may contain a small amount of impurities that do not substantially affect the reaction, such as lower saturated aldehydes.
[0112] As for the oxygen source for the raw gas, it is not particularly limited, but it is industrially advantageous to use air. Additionally, if necessary, a gas mixed with pure oxygen, such as air, may be used. The ratio of oxygen in the raw gas is not particularly limited, but it is preferable to have 0.4 to 4 moles per 1 mole of metacrolein, and more preferable that the lower limit is 0.5 moles or more and the upper limit is 3 moles or less.
[0113] For economic reasons, the source gas may be diluted with an inert gas such as nitrogen or carbon dioxide. Additionally, water vapor may be added to the source gas. By carrying out the reaction in the presence of water vapor, methacrylic acid can be obtained in a higher yield. The concentration of water vapor in the source gas is preferably 0.1 to 50 volume%, with a lower limit of 1 volume% or more and an upper limit of 40 volume% being more preferable.
[0114] The contact time between the source gas and the catalyst for producing methacrylic acid is preferably 1.5 to 15 seconds, with a lower limit of 2 seconds or more and an upper limit of 10 seconds or less being more preferable. The reaction pressure is preferably 0.1 to 1 MPa (G). Provided, (G) refers to gauge pressure. The reaction temperature is preferably 200 to 450°C, with a lower limit of 250°C or more and an upper limit of 400°C or less being more preferable.
[0115] In the production of methacrylic acid, the position of the catalyst in the reactor, the proportion of the catalyst in the reactor, etc., are not particularly limited, and commonly used forms can be applied.
[0116] [Method for manufacturing methacrylic acid ester]
[0117] In the method for producing a methacrylic acid ester according to the present embodiment, the methacrylic acid produced by the method according to the present embodiment is esterified. That is, the method for producing a methacrylic acid ester according to the present embodiment includes a process of producing methacrylic acid by the method according to the present embodiment and a process of esterifying the said methacrylic acid.
[0118] The alcohol reacted with methacrylic acid is not particularly limited and may include, for example, methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, etc. Examples of the resulting methacrylic acid esters include, for example, methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, butyl methacrylate, isobutyl methacrylate, etc. The esterification reaction may be carried out in the presence of an acidic catalyst such as a sulfonic acid-type cation exchange resin. The temperature during the esterification reaction is preferably 50 to 200°C.
[0119] The pressure during the esterification reaction, the position of the catalyst in the reactor, and the proportion of the catalyst in the reactor are not particularly limited, and commonly used forms can be applied.
[0120] Examples
[0121] Hereinafter, examples of the preparation of the catalyst and reaction examples using the same according to the present embodiment are described together with comparative examples. In the following examples and comparative examples, "part" refers to parts by mass.
[0122] (Composition ratio of catalyst)
[0123] The molar ratio of each component was determined by analyzing the components in which the catalyst was dissolved in ammonia water using ICP emission analysis.
[0124] (X-ray diffraction measurement of catalyst powder)
[0125] For the X-ray diffraction measurement of the catalyst powder, a PANalytical X-ray diffraction device X'PertProMPD and an Anton Paar high-temperature strip heater chamfer were used. For the measurement, CuKα rays (λ=0.154 nm) were used, with an output of 45 kV, 40 mA, and a measurement range of 5 to 60°. The goniometer radius was set to 240 mm, and either an automatic continuously variable slit or a fixed slit was used for the diverging slit. Additionally, when using an automatic continuously variable slit, the slit size was set to 0 to 8.0 mm, and when using a fixed slit, the slit size was set to 1.75 mm and the slit opening angle to 1.00°. For the obtained X-ray diffraction pattern, the Kα2 rays were separated and peak search was performed using a Panalytical High Score Plus, and IA, IB, IC, and ID were determined. The conditions for peak search were set as follows: minimum significance: 1 degree, minimum peak chip: 0.2 degrees, maximum peak chip: 1 degree, peak base width: 2 degrees, and method: minimum value of the second derivative. Additionally, while increasing the temperature of the catalyst at 10°C / min, X-ray diffraction measurements were performed on the powder at 10°C intervals starting from 400°C, and peak search was performed on the X-ray diffraction pattern obtained using the above method, and the lowest temperature at which a peak was detected at 2θ=27.1±0.2° was set as T1.
[0126] (The thermal decomposition temperature of the catalyst)
[0127] The thermal decomposition temperature, which is an indicator of the heat resistance of the catalyst, was measured as follows using a TG / DTA measuring device. 50 mg of alumina was used as a reference, and 50 mg of powdered catalyst was heated from room temperature to 550°C at a rate of 10°C / min in an air atmosphere. In the temperature region of the obtained DTA curve above 380°C, the temperature at which an exothermic reaction of 1.8 μV or more was observed upon a 15°C increase in temperature was defined as the thermal decomposition temperature. A higher thermal decomposition temperature of the catalyst indicates higher heat resistance.
[0128] (Analysis of raw gas and products)
[0129] The analysis of the source gas and product was performed using the following gas chromatography.
[0130] Shimadzu Seisakusho GC-2014 (Column: J&W DB-FFAP, 30 m × 0.32 mm, film thickness 1.0 µm)
[0131] Shimadzu Seisakusho GC-8A (Column: Molecular sieve, 2.0M × 3.0㎜ ID)
[0132] Shimazu Seisakusho GC-8A (Column: Polar Pack Q, 2.0M×3.0㎜ ID)
[0133] The yield of the generated methacrylic acid was calculated by the following formula.
[0134] Yield of methacrylic acid (%) = (N2 / N1) × 100
[0135] Here, N1 is the number of moles of supplied methacrolein, and N2 is the number of moles of methacrylic acid produced.
[0136] (Tungsten raw material)
[0137] The tungsten raw materials used in the examples and comparative examples are as follows.
[0138] Ammonium metatungstate (manufactured by Nippon Muki Kagaku High School) Solubility in water at 20°C: 10g / 100mL
[0139] Phosphotungstic acid (manufactured by Nippon Muki Kagaku High School) Solubility in water at 20℃: 40g / 100mL or more
[0140] <Example 1>
[0141] A diluted solution was prepared by diluting 294.0 parts of molybdenum trioxide, 10.2 parts of ammonium metavanadate, 10.6 parts of ammonium metatungstate, and 30.0 parts of an 85 mass% aqueous phosphoric acid solution with 36 parts of pure water to 1200 parts of pure water at room temperature, and a solution was prepared by dissolving 6.3 parts of copper(II) nitrate trihydrate in 9.0 parts of pure water. The resulting slurry was heated to 95°C at a rate of 2°C / min and stirred for 2 hours. Subsequently, a solution prepared by dissolving 40.4 parts of cesium bicarbonate in 60 parts of pure water at room temperature was mixed and stirred at 95°C for 15 minutes. Subsequently, a solution prepared by dissolving 27.5 parts of ammonium carbonate in 78 parts of pure water was mixed and stirred at 95°C for 15 minutes to obtain Solution A. The pH of Solution A is shown in Table 1.
[0142] The obtained liquid A was heated to evaporate, dry, and solidify, thereby obtaining a dried product.
[0143] The obtained dried material was pressure-molded and crushed, and classified using a sieve so that the particle size was within the range of 710 μm to 2.36 mm. The obtained granular sieve was calcined at 380°C for 5 hours under air circulation, and the resulting calcined material was used as a catalyst. The oxygen-excluding composition of the said catalyst is P 1. 5Mo 11 .8 W 0.2 V 0. 5Cu0 . 15 Cs1 . It was 2. In addition, powder X-ray diffraction measurements and thermal decomposition temperature measurements were performed on the corresponding catalyst. The results are shown in Table 1.
[0144] 8 g of the obtained catalyst was diluted with 10 g of silicon carbide and loaded into a fixed-bed flow-through reactor. Subsequently, a source gas containing 5 volume% methacrolein, 10 volume% oxygen, 30 volume% water vapor, and 55 volume% nitrogen was flowed at a contact time of 178 hr·g / mol, and the oxidation reaction of methacrolein was carried out at a reaction temperature of 300°C. The reaction results are shown in Table 1.
[0145] <Example 2>
[0146] Solution A was obtained in the same manner as in Example 1, except that molybdenum trioxide was 292.1 parts and ammonium metatungstate was 13.6 parts. The pH of Solution A is shown in Table 1.
[0147] The obtained liquid A was heated to evaporate, dry, and solidify, thereby obtaining a dried product.
[0148] The obtained dried material was used, and a catalyst was obtained in the same manner as in Example 1. The oxygen-excluding composition of the said catalyst is P 1. 5Mo 11 .7 W 0.3 V 0. 5Cu0 . 15 Cs1 . It was 2. In addition, powder X-ray diffraction measurements and thermal decomposition temperature measurements were performed on the corresponding catalyst. The results are shown in Table 1.
[0149] Using the obtained catalyst, the oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The reaction results are shown in Table 1.
[0150] <Example 3>
[0151] Solution A was obtained in the same manner as in Example 1, except that molybdenum trioxide was 287.1 parts and ammonium metatungstate was 22.6 parts. The pH of Solution A is shown in Table 1.
[0152] The obtained liquid A was heated to evaporate, dry, and solidify, thereby obtaining a dried product.
[0153] The obtained dried material was used, and a catalyst was obtained in the same manner as in Example 1. The oxygen-excluding composition of the said catalyst is P 1.5 Mo 11.5 W 0.5 V 0.5 Cu 0.15 Cs 1.2 It was. In addition, powder X-ray diffraction measurements and thermal decomposition temperature measurements were performed on the corresponding catalyst. The results are shown in Table 1.
[0154] Using the obtained catalyst, the oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The reaction results are shown in Table 1.
[0155] <Example 4>
[0156] Solution A was obtained in the same manner as in Example 1, except that molybdenum trioxide was used in an amount of 285.0 parts, an 85 mass% aqueous phosphoric acid solution in an amount of 29.0 parts, and phosphotungstic acid in an amount of 29.7 parts instead of ammonium metatungstate in an amount of 10.6 parts. The pH of Solution A is shown in Table 1.
[0157] The obtained liquid A was heated to evaporate, dry, and solidify, thereby obtaining a dried product.
[0158] The obtained dried material was used, and a catalyst was obtained in the same manner as in Example 1. The oxygen-excluding composition of the said catalyst is P 1. 5Mo 11 .4 W 0.6 V 0. 5Cu0 . 15 Cs1 . It was 2. In addition, powder X-ray diffraction measurements and thermal decomposition temperature measurements were performed on the corresponding catalyst. The results are shown in Table 1.
[0159] Using the obtained catalyst, the oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The reaction results are shown in Table 1.
[0160] <Example 5>
[0161] Solution A was obtained in the same manner as in Example 1, except that molybdenum trioxide was 277.2 parts and ammonium metatungstate was 40.8 parts. The pH of Solution A is shown in Table 1.
[0162] The obtained liquid A was heated to evaporate, dry, and solidify, thereby obtaining a dried product.
[0163] The obtained dried material was used, and a catalyst was obtained in the same manner as in Example 1. The oxygen-excluding composition of the said catalyst is P 1. 5Mo 11 .1 W 0.9 V 0. 5Cu0 . 15 Cs1 . It was 2. In addition, powder X-ray diffraction measurements and thermal decomposition temperature measurements were performed on the corresponding catalyst. The results are shown in Table 1.
[0164] Using the obtained catalyst, the oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The reaction results are shown in Table 1.
[0165] <Comparative Example 1>
[0166] Solution A was obtained in the same manner as in Example 1, except that molybdenum trioxide was 270.0 parts and ammonium metatungstate was 53.2 parts. The pH of Solution A is shown in Table 1.
[0167] The obtained liquid A was heated to evaporate, dry, and solidify, thereby obtaining a dried product.
[0168] The obtained dried material was used, and a catalyst was prepared in the same manner as in Example 1. The oxygen-excluding composition of the said catalyst is P 1. 5Mo 10 .8 W 1.2 V 0. 5Cu0 . 15 Cs1 . It was 2. In addition, powder X-ray diffraction measurements and thermal decomposition temperature measurements were performed on the corresponding catalyst. The results are shown in Table 1.
[0169] Using the obtained catalyst, the oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The reaction results are shown in Table 1.
[0170] <Comparative Example 2>
[0171] Solution A was obtained in the same manner as in Example 1, except that molybdenum trioxide was used in an amount of 270.0 parts, an 85 mass% aqueous phosphoric acid solution in an amount of 27.4 parts, and phosphotungstic acid in an amount of 59.4 parts instead of ammonium metatungstate in an amount of 10.6 parts. The pH of Solution A is shown in Table 1.
[0172] The obtained liquid A was heated to evaporate, dry, and solidify, thereby obtaining a dried product.
[0173] The obtained dried material was used, and a catalyst was prepared in the same manner as in Example 1. The oxygen-excluding composition of the said catalyst is P 1. 5Mo 10 .8 W 1.2 V 0. 5Cu0 . 15 Cs1 . It was 2. In addition, powder X-ray diffraction measurements and thermal decomposition temperature measurements were performed on the corresponding catalyst. The results are shown in Table 1.
[0174] Using the obtained catalyst, the oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The reaction results are shown in Table 1.
[0175] <Comparative Example 3>
[0176] 300.0 parts of phosphotungstic acid were pressure-molded and crushed, and then sieved to obtain a particle size within the range of 710 μm to 2.36 mm. The obtained granular sieves were calcined at 380°C for 5 hours under air circulation, and the resulting calcined product was used as a catalyst. The oxygen-excluding composition of the said catalyst was P1W 12 It was. In addition, powder X-ray diffraction measurements and thermal decomposition temperature measurements were performed on the corresponding catalyst. The results are shown in Table 1.
[0177] Using the obtained catalyst, the oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The reaction results are shown in Table 1.
[0178] <Comparative Example 4>
[0179] 300.0 parts of phosphomolybdic acid (manufactured by Nippon Muki Kagaku High School) were calcined at 380°C for 5 hours, the resulting powder was crushed, and the powder was sieved to obtain a particle size within the range of 710 μm to 2.36 mm. The resulting granular sieve was calcined at 380°C for 5 hours under air circulation to prepare a catalyst. The oxygen-excluding composition of the catalyst was P1Mo 12 It was. In addition, powder X-ray diffraction measurements and thermal decomposition temperature measurements were performed on the corresponding catalyst. The results are shown in Table 1.
[0180] Using the obtained catalyst, the oxidation reaction of methacrolein was carried out in the same manner as in Example 1. The reaction results are shown in Table 1.
[0181]
[0182] As shown in Table 1, Examples 1 to 5 using catalysts satisfying conditions (a1) and (b) had high heat resistance and could obtain methacrylic acid in high yield because the heteropolyacid in the catalyst formed a thermodynamically metastable crystal structure.
[0183] In addition, a methacrylic acid ester can be obtained by esterifying the methacrylic acid obtained in this embodiment. Industrial applicability
[0184] According to the present invention, a catalyst with high heat resistance and capable of producing methacrylic acid in high yield can be provided.
Claims
Claim 1 A catalyst used to produce methacrylic acid by the oxidation of methacrolein, comprising a heteropoly acid containing phosphorus, molybdenum, and tungsten, wherein (a1) in powder X-ray diffraction measurements at 25°C, when the intensity of the diffraction peak (peak A) with 2θ=26.1±0.2° is denoted as IA and the intensity of the diffraction peak (peak B) with 2θ=23.0±0.2° is denoted as IB, the IB / IA ratio is 0.015 or less, and (b) when powder X-ray diffraction measurements are performed at 10°C intervals starting from 400°C while increasing the temperature at 10°C / min, the lowest temperature T1 at which the diffraction peak (peak E) with 2θ=27.1±0.2° appears is 440°C or higher. Claim 2 A catalyst for producing methacrylic acid according to claim 1, wherein the IB / IA ratio is 0.01 or less. Claim 3 A catalyst for producing methacrylic acid according to claim 1, wherein (a2) in powder X-ray diffraction measurement at 25°, when the intensity of the diffraction peak (peak C) at 2θ=34.1±0.2° is set as IC, the IC / IA is 0.0055 or less. Claim 4 In paragraph 2, (a2) a catalyst for producing methacrylic acid, wherein when the intensity of the diffraction peak (peak C) at 2θ=34.1±0.2° is taken as IC, the IC / IA is 0.0055 or less. Claim 5 In paragraph 3, a catalyst for producing methacrylic acid, wherein the IC / IA is 0.0005 to 0.0055. Claim 6 In paragraph 3, a catalyst for producing methacrylic acid, wherein the IC / IA is 0.001 to 0.0053. Claim 7 A catalyst for producing methacrylic acid according to any one of claims 1 to 6, wherein (a3) in powder X-ray diffraction measurement at 25°, when the intensity of the diffraction peak (peak D) at 2θ=48.3±0.2° is denoted as ID, the ID / IA is 0.003 or less. Claim 8 A catalyst for producing methacrylic acid, wherein, in any one of claims 1 to 6, T1 is 440 to 500°C. Claim 9 A catalyst for producing methacrylic acid, having a composition represented by the following formula (I) in any one of claims 1 to 6. a Mo b W c V d Cu e A f E g G h O i (I) In formula (I), P, Mo, W, V, Cu, and O represent phosphorus, molybdenum, tungsten, vanadium, copper, and oxygen, respectively. A represents at least one element selected from the group consisting of antimony, bismuth, arsenic, germanium, tellurium, selenium, and silicon. E represents at least one element selected from the group consisting of iron, zinc, chromium, tantalum, cobalt, nickel, manganese, titanium, and niobium. G represents at least one element selected from the group consisting of potassium, rubidium, and cesium. a to i represent the molar ratios of each component, b+c=12, a=0.5 to 3, c=0.22 to 5, d=0.01 to 3, e=0.01 to 2, f=0 to 3, g=0 to 3, h=0.01 to 3, and i is the molar ratio of oxygen required to satisfy the valence of each component. Claim 10 In claim 9, a catalyst for producing methacrylic acid, wherein c=0.22 to 3 in the above formula (I). Claim 11 A method for manufacturing a catalyst for producing methacrylic acid as described in any one of claims 1 to 6, comprising: (i) a process of mixing a phosphorus raw material, a molybdenum raw material, and a tungsten raw material with a solvent to prepare a solution or slurry (solution A) having a pH of 0.1 to 4; (ii) a process of drying the solution A to obtain a dried product; and (iii) a process of calcining the dried product to obtain a calcined product. Claim 12 A method for producing a catalyst for producing methacrylic acid according to claim 11, wherein in process (i) above, the tungsten raw material having a solubility in water at 20°C of 4.1 g / 100 mL or more is 50 mass% or more of the total tungsten raw material. Claim 13 A method for producing a catalyst for producing methacrylic acid, wherein, in the above process (i), the pH of the above liquid A is 0.1 to 3. Claim 14 A method for producing methacrylic acid, comprising a process of oxidizing methacrolein using a catalyst for producing methacrylic acid described in any one of claims 1 to 6, and producing methacrylic acid. Claim 15 A method for producing methacrylic acid, comprising a process of oxidizing methacrolein and producing methacrylic acid using a catalyst for producing methacrylic acid produced by the method described in claim 11. Claim 16 A method for producing a methacrylic acid ester, comprising a process of esterifying methacrylic acid produced by the method described in paragraph 14.
Citation Information
Patent Citations
Catalyst
JP1980001880A
Catalyst for manufacturing methacrylic acid and manufacturing method therefor, and manufacturing method of methacrylic acid
JP2016168591A
Dehydration granules for catalyst manufacture, catalyst, and manufacturing method compound
JP2021041403A
Process for preparing heteropolyacids
KR1019790001938B1
Catalyst for producing methacrylic acid and method for producing the same, and method for producing methacrylic acid and methacrylic acid ester
KR1020190042095A