High-efficiency and high-stability perovskite photovoltaic device and its manufacturing method

A perovskite photovoltaic device with a three-dimensional perovskite and electron density-differentiated quasi-two-dimensional intermediate layers addresses efficiency and stability issues, achieving high performance and longevity.

KR103044584B1Active Publication Date: 2026-11-06UNIST (ULSAN NAT INST OF SCI & TECH) +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
KR1020250005374
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2025-01-14
Publication Date
2026-11-06
Estimated Expiration
2045-01-14

AI Technical Summary

Technical Problem

Existing perovskite solar cells face challenges in achieving high photovoltaic conversion efficiency, thermal stability, and air stability due to low exciton bonding strength in three-dimensional perovskites and inadequate optimization of intermediate layers in two-dimensional perovskite structures.

Method used

A perovskite photovoltaic device with a three-dimensional perovskite thin film and an intermediate layer comprising two or more types of quasi-two-dimensional perovskites, formed by mixing compounds with differing electron densities, is developed to enhance charge transfer and stability.

Benefits of technology

The device exhibits high photovoltaic conversion efficiency, thermal stability, and air stability, maintaining 90% efficiency after heat treatment and 9,000 hours of storage, with reduced defects and improved charge transfer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112025005099374-PAT00013_ABST
    Figure 112025005099374-PAT00013_ABST
Patent Text Reader

Abstract

The present disclosure relates to a perovskite photovoltaic device having high efficiency, high stability, and high durability, and a method for manufacturing the same. The present disclosure may provide a perovskite photovoltaic device comprising: a perovskite thin film having a three-dimensional perovskite crystal structure; and an intermediate layer located on the perovskite thin film, wherein the intermediate layer comprises a first intermediate layer compound having a first cation and a first anion; and a second intermediate layer compound having a second cation and a second anion, wherein the electron density of the first cation is greater than the electron density of the second cation.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present disclosure relates to a high-efficiency, high-stability perovskite photovoltaic device and a method for manufacturing the same. Background Technology

[0002] Recently, organic-inorganic hybrid perovskite materials have been attracting attention as key materials for next-generation optoelectronic devices due to their advantages, such as high light absorption, high external quantum efficiency (EQE), fast charge transfer rate, and solution processability. Over the past decade, extensive research has been conducted on perovskite materials, primarily focusing on solar cells, and they are on the verge of commercialization, with peak photoelectric conversion efficiencies reaching 25%. However, active research is being conducted to address numerous challenges remaining for the commercialization of perovskite solar cells, such as improving stability against light, heat, and moisture, enhancing charge transfer efficiency, reducing toxic substances, and developing low-cost, large-area perovskite thin film manufacturing methods.

[0003] In three-dimensional perovskites, the bonding strength of excitons within the structure is low due to the high dielectric constant, making it difficult to expect high luminous efficiency (PLQY). Therefore, the research focus of perovskite solar cells is concentrated on designing interfacial interlayers that eliminate defects at the perovskite thin film-charge carrier interface and perform efficient charge separation and transport. Energy level aligning at the interface of the perovskite thin film-interlayer is reported to play a major role in controlling the flow of excited carriers in the perovskite thin film.

[0004] Recently, intermediate layers containing layered two-dimensional perovskite crystals containing long alkylammonium cations have been studied. However, two-dimensional perovskite structures formed from single organic ammonium cations studied until recently have not significantly contributed to improving air stability, thermal stability, and photoelectric conversion efficiency of perovskite solar cells, and research on the intermediate layers is sluggish because the optimal thickness, surface morphology, and energy level alignment of the intermediate layers of the two-dimensional perovskite structures are intertwined with complex factors. The problem to be solved

[0005] The present disclosure can provide a perovskite photovoltaic device having high photovoltaic conversion efficiency, high thermal stability, and high stability in air.

[0006] The present disclosure can provide a method for manufacturing a perovskite photovoltaic device capable of achieving high photovoltaic conversion efficiency, high thermal stability, and high stability in air at low cost. means of solving the problem

[0007] The present disclosure may provide a perovskite photovoltaic device comprising: a perovskite thin film including a three-dimensional perovskite; and an intermediate layer located on the perovskite thin film; wherein the intermediate layer comprises two or more types of quasi-two-dimensional perovskites, and the quasi-two-dimensional perovskites are prepared by mixing a first intermediate layer compound including a first cation and a first anion; and a second intermediate layer compound including a second cation and a second anion; in an intermediate layer solvent, and wherein the electron density of the first cation is greater than the electron density of the second cation.

[0008] In one embodiment of the present disclosure, the three-dimensional perovskite may be a compound represented by the following chemical formula 1.

[0009] (Chemical Formula 1)

[0010] ABX3

[0011] (In the above Chemical Formula 1, A is a monovalent alkylammonium cation, a monovalent amidinium cation, Li + , Na + , K + , Rb + , Cs + , Fr + , Cu(I) + , Ag(I) + and Au(I) + It comprises one or more monovalent cations selected from the group consisting of, where B is a divalent metal cation, and X is I - , Br - , Cl - ...and includes one or more halogen anions selected from the group consisting of combinations thereof.)

[0012] In one embodiment of the present disclosure, the first cation may satisfy the following chemical formula 2.

[0013] [Chemical Formula 2]

[0014]

[0015] (In the above Chemical Formula 2, R1 comprises one or more selected from the group consisting of a straight-chain or branched-chain alkoxy group having 1 to 10 carbon atoms, an aryloxy group having 6 to 60 carbon atoms, and derivatives thereof.)

[0016] In one embodiment of the present disclosure, the second cation may satisfy the following chemical formula 3.

[0017] [Chemical Formula 3]

[0018]

[0019] (In the above chemical formula 3, R2 is selected from one or more of the group comprising straight-chain or branched-chain alkyl having 1 to 10 carbon atoms, straight-chain or branched-chain alkenyl having 1 to 10 carbon atoms, straight-chain or branched-chain alkanyl having 1 to 10 carbon atoms, monocyclic or polycyclic cycloalkane having 3 to 30 carbon atoms, monocyclic or polycyclic aryl having 6 to 30 carbon atoms, and derivatives thereof.)

[0020] In one embodiment of the present disclosure, the first cation may be methoxyphenylammonium.

[0021] In one embodiment of the present disclosure, the second cation may be cyclohexylammonium.

[0022] In one embodiment of the present disclosure, the first anion and the second anion are each independently fluorine (F - ), chlorine (Cl - ), Bromine (Br - ) and iodine(I - It may be selected from a group consisting of ).

[0023] In one embodiment of the present disclosure, the mixing ratio of the first intermediate layer compound and the second intermediate layer compound may be 0.1:1 to 1:0.1.

[0024] In one embodiment of the present disclosure, the quasi-two-dimensional perovskite formation energy of the first intermediate compound and the second intermediate compound dissolved in the intermediate solvent may be -100 eV or less.

[0025] In one embodiment of the present disclosure, the intermediate layer solvent may be an alcohol-based solvent.

[0026] In one embodiment of the present disclosure, the intermediate layer solvent may be isopropanol (IPA).

[0027] In one embodiment of the present disclosure, the quasi-two-dimensional perovskite of the intermediate layer may be a quasi-two-dimensional perovskite with n=2.

[0028] In one embodiment of the present disclosure, the thickness of the intermediate layer may be 0.1 to 10 nm.

[0029] In one embodiment of the present disclosure, the perovskite photovoltaic device may have a power conversion efficiency (PCE) of 90% or more compared to the initial efficiency even after heat treatment at a temperature of 80°C for 3 hours.

[0030] In one embodiment of the present disclosure, the perovskite photovoltaic device may maintain a power conversion efficiency (PCE) of 90% or more compared to the initial value after being stored at room temperature for 9,000 hours.

[0031] In one embodiment of the present disclosure, a method for manufacturing a perovskite photovoltaic device is provided, comprising: (S1) a step of manufacturing a perovskite thin film having a three-dimensional perovskite crystal structure; and (S2) a step of depositing an intermediate layer by applying an intermediate layer solution onto the perovskite thin film; wherein the intermediate layer solution comprises a first intermediate layer compound having a first cation and a first anion; a second intermediate layer compound having a second cation and a second anion; and an intermediate layer solvent; wherein the electron density of the first cation is greater than the electron density of the second cation.

[0032] In one embodiment of the present disclosure, the intermediate layer solvent may be an alcohol.

[0033] In one embodiment of the present disclosure, the intermediate layer solvent may be isopropanol (IPA).

[0034] In one embodiment of the present disclosure, the formation energy of the quasi-two-dimensional perovskite of the intermediate layer solution may be -150 eV or less.

[0035] In one embodiment of the present disclosure, the mixing ratio of the first intermediate layer compound and the second intermediate layer compound included in the intermediate layer solution may be 0.1:1 to 1:0.1.

[0036] In one embodiment of the present disclosure, the perovskite thin film may be a compound represented by the following chemical formula 1.

[0037] (Chemical Formula 1)

[0038] ABX3

[0039] (In the above Chemical Formula 1, A is a monovalent alkylammonium cation, a monovalent amidinium cation, Li + , Na + , K + , Rb + , Cs + , Fr + , Cu(I) + , Ag(I) + and Au(I) + It comprises one or more monovalent cations selected from the group consisting of, where B is a divalent metal cation, and X is I - , Br - , Cl - ...and includes one or more halogen anions selected from the group consisting of combinations thereof.)

[0040] In one embodiment of the present disclosure, the first cation may satisfy the following chemical formula 2.

[0041] [Chemical Formula 2]

[0042]

[0043] (In the above Chemical Formula 2, R1 comprises one or more selected from the group consisting of a straight-chain or branched-chain alkoxy group having 1 to 10 carbon atoms, an aryloxy group having 6 to 60 carbon atoms, and derivatives thereof.)

[0044] In one embodiment of the present disclosure, the second cation may satisfy the following chemical formula 3.

[0045] [Chemical Formula 3]

[0046]

[0047] (In the above chemical formula 3, R2 is selected from one or more of the group comprising straight-chain or branched-chain alkyl having 1 to 10 carbon atoms, straight-chain or branched-chain alkenyl having 1 to 10 carbon atoms, straight-chain or branched-chain alkanyl having 1 to 10 carbon atoms, monocyclic or polycyclic cycloalkane having 3 to 30 carbon atoms, monocyclic or polycyclic aryl having 6 to 30 carbon atoms, and derivatives thereof.)

[0048] In one embodiment of the present disclosure, the first cation may be methoxyphenylammonium.

[0049] In one embodiment of the present disclosure, the second cation may be cyclohexylammonium.

[0050] In one embodiment of the present disclosure, the first anion and the second anion are each independently fluorine (F - ), chlorine (Cl - ), Bromine (Br - ) and iodine(I - It may be selected from a group consisting of ).

[0051] In one embodiment of the present disclosure, the step of forming an intermediate layer may be performed by a method selected from the group consisting of screen printing, spin coating, bar coating, gravure coating, blade coating, and roll coating.

[0052] In one embodiment of the present disclosure, after step (S2), the step of heat-treating the intermediate layer at a temperature in the range of 80 to 150°C for 3 to 60 minutes may be further included.

[0053] In one embodiment of the present disclosure, a perovskite photovoltaic device manufactured according to the above-described manufacturing method may be provided.

[0054] In another embodiment of the present disclosure, a perovskite solar cell is provided, comprising: a substrate; a first electrode formed on the substrate; the aforementioned perovskite photovoltaic element and a second electrode formed on the photovoltaic element.

[0055] In one embodiment of the present disclosure, the perovskite photovoltaic device may further include an electron transport layer or a hole transport layer on the upper or lower part. Effects of the invention

[0056] The perovskite photovoltaic device according to the present disclosure can exhibit high photovoltaic conversion efficiency.

[0057] The perovskite photovoltaic device according to the present disclosure can exhibit the effect of high thermal stability.

[0058] The perovskite photovoltaic device according to the present disclosure can provide the effect of exhibiting high stability in air.

[0059] The method for manufacturing a perovskite photovoltaic device according to the present disclosure can manufacture a perovskite photovoltaic device capable of achieving high photovoltaic conversion efficiency, high thermal stability, and high stability in air at low cost. Brief explanation of the drawing

[0060] Figure 1 shows the FT-IR and NMR analyses of the intermediate layer solution and the intermediate layer of the example and comparative example. FIG. 2 illustrates the interface between the three-dimensional (3D) perovskite and the intermediate layer and the crystal structure of the intermediate layer of the example and comparative example. Figure 3 shows the change in XRD peaks over time at a high temperature of 85°C for Comparative Example 1 and Example 2. Figure 4 shows SEM image analysis of the surface conditions before and after heat treatment of Comparative Example 1 and Example 2. Figure 5 shows a table comparing PCE, J, V, and FF of Example 2 and Comparative Example 1. Figure 6 shows the PCE (%), J of the examples and comparative examples. SC (mA cm -2 ), FF(%), V OC This illustrates a comparison of the performance of (V). Figure 7 illustrates the electrical characteristics of a perovskite solar cell (PSC) using the JV curve (Current density vs. Voltage) of Example 2. Figure 8 is a comparative analysis of the long-term photo-stability of Comparative Example 1 and Example 2. Specific details for implementing the invention

[0061] The advantages and features of the present disclosure and the methods for achieving them will become clear by referring to the embodiments described in detail below. However, the present disclosure is not limited to the embodiments disclosed below but may be implemented in various different forms. These embodiments are provided merely to ensure that the disclosure of the present disclosure is complete and to fully inform those skilled in the art of the scope of the invention, and the present disclosure is defined only by the scope of the claims.

[0062] Unless otherwise defined, all terms used in this specification (including technical and scientific terms) may be used in a meaning that is commonly understood by those skilled in the art to which this disclosure pertains.

[0063] Unless otherwise specifically indicated, the singular form of a term used in this specification may be interpreted to include the plural form.

[0064] The numerical ranges used herein include lower and upper limits and all values ​​within the range, increments logically derived from the form and width of the defined range, all of which are limited values, and all possible combinations of upper and lower limits of the numerical range defined in different forms. Unless otherwise specifically defined in the specification of this disclosure, values ​​outside the numerical range that may occur due to experimental error or rounding of values ​​are also included in the defined numerical range.

[0065] As used in this specification, "comprising" is an open description equivalent to expressions such as "comprising," "containing," "having," and "characteristics," and does not exclude elements, materials, or processes not additionally listed.

[0066] Hereinafter, the high-efficiency, high-stability perovskite photovoltaic device of the present disclosure and the method for manufacturing the same will be described in detail. However, this is merely illustrative and the present disclosure is not limited to the specific embodiments described illustratively.

[0067] The present disclosure may provide a perovskite photovoltaic device comprising: a perovskite thin film including a three-dimensional perovskite; and an intermediate layer located on the perovskite thin film; wherein the intermediate layer comprises two or more types of quasi-two-dimensional perovskites, and the quasi-two-dimensional perovskites are prepared by mixing a first intermediate layer compound including a first cation and a first anion; and a second intermediate layer compound including a second cation and a second anion; and wherein the electron density of the first cation is greater than the electron density of the second cation.

[0068] The perovskite optoelectronic device of the present disclosure includes an intermediate layer comprising two or more compounds of a quasi-two-dimensional perovskite structure on a three-dimensional perovskite thin film, thereby effectively suppressing the hole-hole recombination rate and extending the carrier lifetime, and improving conductivity by increasing the charge transfer rate and transfer efficiency.

[0069] In addition, the difference in electron density between the first and second cations strengthens the bonding strength of the intermediate layer compound due to cation-to-cation interactions, and can form a stable quasi-two-dimensional perovskite.

[0070] Three-dimensional perovskites have a problem in which, in addition to degradation caused by the surrounding environment, internal ions move to and escape from the charge transfer layer adjacent to the thin film, causing the thin film to decompose. Accordingly, the present disclosure forms an intermediate layer on a three-dimensional perovskite thin film to passivate surface defects of the three-dimensional perovskite with the intermediate layer, thereby suppressing non-radiative recombination occurring at the interface and degradation of the thin film caused by the movement of external ions or the external environment. This can improve the overall stability of the optoelectronic device and its resistance to changes in the external environment (heat, humidity, etc.). Therefore, the optoelectronic device of the present disclosure can provide excellent effects with improved photoelectric conversion efficiency, thermal stability, and stability in air.

[0071] In one embodiment of the present disclosure, the perovskite thin film may include a compound represented by the following chemical formula 1.

[0072] (Chemical Formula 1)

[0073] ABX3

[0074] (In the above Chemical Formula 1, A is a monovalent alkylammonium cation, a monovalent amidinium cation, Li + , Na + , K + , Rb + , Cs + , Fr + , Cu(I) + , Ag(I) + and Au(I) + It comprises one or more monovalent cations selected from the group consisting of, where B is a divalent metal cation, and X is I - , Br - , Cl - ...and includes one or more halogen anions selected from the group consisting of combinations thereof.)

[0075] More specifically, if A in Chemical Formula 1 is an organic cation, such as a monovalent alkylammonium cation or a monovalent amidinium cation, the perovskite compound may be an organic-inorganic hybrid perovskite compound composed of organic A and inorganic M and X. Alternatively, if A in Chemical Formula 1 is an inorganic cation, the perovskite compound may be an inorganic metal halide perovskite compound composed entirely of inorganic A, M, and X.

[0076] In this case, if the perovskite compound is an organic-inorganic hybrid perovskite compound, it can improve durability and stability by possessing the advantages of both organic and inorganic materials, and if it is an inorganic metal halide perovskite compound, it can have higher durability and stability characteristics because it does not use organic materials.

[0077] By including the above three-dimensional perovskite structure of Chemical Formula 1, a photoelectric effect can be exhibited when irradiated with light of a specific wavelength band according to the band gap of the perovskite crystal, and through this, a photoelectric device can be realized.

[0078] In one embodiment of the present disclosure, the first cation may satisfy the following chemical formula 2.

[0079] [Chemical Formula 2]

[0080]

[0081] (In the above Chemical Formula 2, R1 comprises one or more selected from the group consisting of a straight-chain or branched-chain alkoxy group having 1 to 10 carbon atoms, an aryloxy group having 6 to 60 carbon atoms, and derivatives thereof.)

[0082] R1 of the above chemical formula 2 can be designed in various ways to have an electron density rich in the first cation. Specifically, R1 of the above chemical formula 2 may be a straight-chain or branched-chain alkoxy group having 1 to 10 carbon atoms, and more specifically, R1 may be a straight-chain or branched-chain alkoxy group having 1 to 10 carbon atoms.

[0083] More specifically, R1 may be a methoxy group. When R1 is a methoxy group, it can be uniformly dispersed in an organic solvent while having high solubility in the solvent. Accordingly, the intermediate layer can be formed through a solution process, which is a simpler process. In addition, the methoxy group (-OCH3) can enable the first cation to have a high electron density through the electron contribution of the methoxy group.

[0084] However, R1 of Chemical Formula 2 is not limited to a methoxy group, and a person skilled in the art may appropriately select and use it to achieve various effects such as solubility of the first intermediate compound in a solvent, control of electron density of the first cation, control of energy levels, and recovery of trap levels.

[0085] In one embodiment of the present disclosure, the second cation may satisfy the following chemical formula 3.

[0086] [Chemical Formula 3]

[0087]

[0088] (In the above chemical formula 3, R2 is selected from one or more of the group comprising straight-chain or branched-chain alkyl having 1 to 10 carbon atoms, straight-chain or branched-chain alkenyl having 1 to 10 carbon atoms, straight-chain or branched-chain alkanyl having 1 to 10 carbon atoms, monocyclic or polycyclic cycloalkane having 3 to 30 carbon atoms, monocyclic or polycyclic aryl having 6 to 30 carbon atoms, and derivatives thereof.)

[0089] R2 of Chemical Formula 3 above can be designed in various ways so that the second cation has an electron density lower than that of the first cation. Because the second cation has an electron density lower than that of the first cation and has a small molecular size, the band state and crystal structure of the intermediate layer are controlled, thereby providing high stability and high charge transfer capability, which can enable the perovskite photovoltaic device to have a high power conversion efficiency (PCE).

[0090] Specifically, R2 of the above chemical formula 3 may be a monocyclic or polycyclic cycloalkane having 3 to 30 carbon atoms, or a monocyclic or polycyclic aryl having 6 to 30 carbon atoms. More specifically, it may be a monocyclic or polycyclic cycloalkane having 3 to 30 carbon atoms.

[0091] More specifically, it may be cyclohexyl. When R2 is cyclohexyl, it may be solubility in a solvent high enough to allow the intermediate layer to be stacked, while the second cation may have a lower electron density than the first cation. However, R2 of Formula 2 is not limited to cyclohexyl, and R2 may be selected from various molecular structures to achieve the above-described effect.

[0092] In one embodiment of the present disclosure, the first cation may have a greater electron density than the second cation.

[0093] More specifically, the first intermediate layer compound containing the first cation may have a Fermi energy level greater than the Conduction Band Minimum (CBM), and the second intermediate layer compound containing the second cation may have a Fermi energy level smaller than the Conduction Band Minimum (CBM). Accordingly, the first intermediate layer compound may have a greater electron density and energy density.

[0094] Due to the strong interaction between the two substances resulting from the difference in electron density in the solvent, the first cation has a high electron density and exhibits rapid reactivity with the surface of the FAPbI3 perovskite layer, for example, when the 3D perovskite is FAPbI3, while the second cation can react intensively with unbonded PbI2 located at the grain boundary, which has low reactivity. Therefore, when an intermediate layer containing a 2D perovskite is stacked on a 3D perovskite, a low-roughness, flat, and defect-free intermediate layer can be formed.

[0095] That is, when a two-dimensional perovskite intermediate layer is formed, the unbonded cations present in the three-dimensional perovskite can participate in the reaction due to the bonding of two materials including the first cation and the second cation, thereby forming a quasi-two-dimensional perovskite. The intermediate layer containing the quasi-two-dimensional perovskite formed in this way can improve thermal stability, high efficiency, and long-term storage based on rapid hole transport due to appropriate energy level control and non-radiative recombination mitigation due to defect control.

[0096] The greater the difference in electron density between the first cation and the second cation, the more negative the formation energy of the two-dimensional perovskite becomes, allowing for the formation of a structurally stable two-dimensional perovskite and the efficient formation of a quasi-two-dimensional perovskite, and the faster the crystallization rate, the more stable the quasi-two-dimensional perovskite can be formed even in the short time it takes for the solvent to vaporize.

[0097] In one embodiment of the present disclosure, the first anion and the second anion are each independently fluorine (F - ), chlorine (Cl - ), Bromine (Br - ) and iodine(I - It may be selected from a group consisting of ).

[0098] More specifically, the second anion is a bromide ion (Br - As ), the divalent cation contained in the perovskite thin film, for example, lead cation (Pb 2+ It may be an anion having a strong bonding affinity with ). The bromide ion can effectively relieve traps contained in the perovskite thin film. However, the first anion and the second anion of the present invention are not limited to the effects described above, and may be selected differently for purposes such as improving trap density and perovskite crystal structure.

[0099] In one embodiment of the present disclosure, the mixing ratio of the first intermediate layer compound and the second intermediate layer compound may be 0.1:1 to 1:0.1.

[0100] Specifically, the ratio of the first intermediate layer compound and the second intermediate layer compound included in the intermediate layer may be such that, based on 100 moles of the first intermediate layer compound, the second intermediate layer compound is included in an amount of 10 moles or more, 20 moles or more, 30 moles or more, 40 moles or more, or 45 moles or more, and as an upper limit, it may be 90 moles or less, 80 moles or less, 70 moles or less, 60 moles or less, or 55 moles or less. More specifically, the ratio of the first intermediate layer compound and the second intermediate layer compound included in the intermediate layer may be 10 to 90 moles, 20 to 80 moles, 30 to 70 moles, 40 to 60 moles, or 45 to 55 moles based on 100 moles of the first intermediate layer compound. Even more specifically, it may be 30 to 70 moles.

[0101] When the first intermediate layer compound and the second intermediate layer compound are included within the above range, the intermediate layer can be coated and stacked to satisfy a two-dimensional perovskite crystal structure, and a more thermodynamically stabilized two-dimensional perovskite can be formed.

[0102] In one embodiment of the present disclosure, the first intermediate compound may be methoxyphenylammonium iodide (M-PEAI), and the second intermediate compound may be cyclohexylammonium bromide ((CHA)Br).

[0103] When quasi-two-dimensional perovskites were prepared by mixing methoxyphenylammonium iodide (M-PEAI) and cyclohexylammonium bromide ((CHA)Br), the quasi-two-dimensional perovskite crystal structures, namely M-PEA2Pb2I7 (n=2) and CHA2Pb2I7 7-x Br x (n=2) can be formed.

[0104] Here, the quasi-2D perovskite interlayer for n=2 is the 2D perovskite for n=1 (M-PEA2PbI4(n=1) and CHA2PbI4 4-x Br x Compared to (n=1), it can have higher thermal stability, higher atmospheric stability, and higher charge transfer capacity.

[0105] In one embodiment of the present disclosure, the intermediate layer solvent may be an organic polar solvent. Specifically, it may be one or more selected from gamma-butyrolactone, formamide, N,N-dimethylformamide, diformamide, acetonitrile, tetrahydrofuran, dimethyl sulfoxide, diethylene glycol, 1-methyl-2-pyrrolidone, N,N-dimethylacetamide, acetone, α-terpineol, β-terpineol, dihydroterpineol, 2-methoxyethanol, acetylacetone, methanol, ethanol, propanol, butanol, pentanol, hexanol, ketone, methyl isobutyl ketone, etc., but is not necessarily limited thereto, and is a polar organic solvent in which the first intermediate compound and the second intermediate compound are dissolved and uniformly dispersed and can be easily volatilized and removed upon drying, and at the same time, the two-dimensional perovskite formation energy is low to 0 eV or less, and the first intermediate compound and Any solvent capable of forming a two-dimensional perovskite by the interaction of the second intermediate layer compounds can be used without limitation.

[0106] More specifically, the intermediate layer solvent may be an alcohol-based organic solvent, and even more specifically, the intermediate layer solvent may be isopropanol (IPA), but is not necessarily limited thereto.

[0107] In one embodiment of the present disclosure, the quasi-two-dimensional perovskite formation energy of the first intermediate compound and the second intermediate compound dissolved in the intermediate solvent may be -100 eV or less. More specifically, it may be -100 eV or less, -120 eV or less, -150 eV or less, or -200 eV or less.

[0108] As described above, an intermediate layer containing a quasi-two-dimensional perovskite can be prepared only under extremely limited conditions by appropriately adjusting the chemical species, composition ratio, solvent selection, and application method of the first intermediate layer compound and the second intermediate layer compound.

[0109] In one embodiment of the present disclosure, when the solvent of the intermediate layer is isopropanol (IPA), the formation energy of the quasi-two-dimensional perovskite formed from the first intermediate layer compound and the second intermediate layer compound dissolved in isopropanol (IPA) may be -150 eV or less.

[0110] Specifically, when the solvent of the intermediate layer is isopropanol (IPA), the formation energy may be -100 eV or less, -120 eV or less, -150 eV or less, or -200 eV or less, and as a lower limit, it may be -400 eV or more, -350 eV or more, -300 eV or more, or -250 eV or more. More specifically, it may be -400 to -100 eV, -350 to -120 eV, or -300 to -150 eV, and even more specifically, -250 to -200 eV.

[0111] Since the formation energy is within the above range, an intermediate layer containing stable quasi-2D perovskites can be manufactured. Furthermore, stable quasi-2D perovskites can be formed by minimizing structural defects or instability of the quasi-2D perovskites and accelerating the crystallization rate. By minimizing impurities or defects during the crystallization process, charge recombination is reduced and electron / hole mobility is improved, thereby providing optoelectronic devices with excellent electrical performance.

[0112] In one embodiment of the present disclosure, the thickness of the intermediate layer may be 0.1 to 10 nm.

[0113] The thickness of the intermediate layer may be 0.1 nm or more, 0.5 nm or more, 1 nm or more, or 2 nm or more, and as an upper limit, may be 20 nm or less, 10 nm or less, 5 nm or less, or 3 nm or less. Specifically, the thickness of the intermediate layer may be 0.1 to 20 nm, 0.1 to 20 nm, 0.1 to 10 nm, 1 to 5 nm, or 2 to 3 nm.

[0114] The above intermediate layer has a thickness within the range described above, maintaining interaction with the charge transfer layer or the three-dimensional perovskite, and can facilitate the transfer of electrons or holes extracted from the perovskite thin film. The electrons or holes may pass through the intermediate layer due to a tunneling effect, or pass through voids that occur when the intermediate layer is not applied to a certain portion of the three-dimensional perovskite thin film.

[0115] In one embodiment of the present disclosure, the perovskite optoelectronic device can provide a 3D / 2D perovskite stacked structure with excellent thermal stability. More specifically, at a temperature of 70°C or higher, 75°C or higher, and more specifically at 85°C, no decomposition or defects appear in the 2D perovskite intermediate layer formed therein, thereby providing a perovskite optoelectronic device with a uniform crystal structure. This improves the stability of the device, thereby improving the performance and lifespan of the optoelectronic device.

[0116] In one embodiment of the present disclosure, the perovskite optoelectronic device of the present disclosure may maintain a power conversion efficiency (PCE) of 90% or more, 91% or more, 92% or more, 93% or more, or 94% or more compared to the initial efficiency even after heat treatment at a temperature of 80°C for 3 hours. More specifically, it may maintain 95% or more, thereby maintaining the structural and electrical characteristics of the device even in a high-temperature environment. That is, the two-dimensional (2D) perovskite intermediate layer of the present disclosure can significantly improve the stability and reliability of the device and contribute to an extended device lifespan.

[0117] In one embodiment of the present disclosure, the perovskite optoelectronic device of the present disclosure may exhibit low hysteresis in the current-voltage curve. This is due to the low defect density of the 3D / 2D perovskite stacked structure.

[0118] Defects in thin films can act as trap sites and consequently induce capacitance associated with the accumulation of interfacial charges and / or photogenerated charge carrier trapping, which leads to large JV hysteresis. Accordingly, the present disclosure provides a 2D perovskite interlayer with improved stability and improved defects in thin films, which can improve the JV hysteresis coefficient (HF).

[0119] The perovskite optoelectronic device of the present disclosure may have a power conversion efficiency (PCE) of 25% or more and maintain a power conversion efficiency (PCE) of 90% or more compared to the initial value after storage at room temperature for 9,000 hours. More specifically, it may maintain a power conversion efficiency (PCE) of 90% or more, 91% or more, 92% or more, 93% or more, 94% or more, 95% or more, 96% or more, 97% or more, or 98% or more. Even more specifically, it may maintain 99% or more.

[0120] The perovskite optoelectronic device of the present disclosure can maintain a power conversion efficiency of 85% or more relative to the initial power conversion efficiency (PCE) after 440 hours under conditions of 30°C and 15-30% relative humidity without a UV blocking filter. Specifically, it can maintain a power conversion efficiency (PCE) of 85% or more, 86% or more, 87% or more, 88% or more, or 89% or more relative to the initial level, and more specifically, it can maintain a performance of 90% or more power conversion efficiency (PCE).

[0121] That is, the present disclosure can provide a photovoltaic device with excellent thermal stability, photostability, and storage stability.

[0122] The following describes a method for manufacturing a perovskite photovoltaic device. In describing the method for manufacturing the perovskite photovoltaic device, the first cation, the first anion, the first intermediate layer compound, and the second intermediate layer compound, etc., are identical or similar to those described above in the perovskite photovoltaic device; therefore, the method for manufacturing the perovskite photovoltaic device according to the present invention includes all the details described above in the perovskite photovoltaic device.

[0123] The present disclosure provides a method for manufacturing a perovskite photovoltaic device, comprising: (S1) a step of manufacturing a perovskite thin film having a three-dimensional perovskite crystal structure; and (S2) a step of forming an intermediate layer by applying an intermediate layer solution onto the perovskite thin film; wherein the intermediate layer solution comprises a first intermediate layer compound having a first cation and a first anion; a second intermediate layer compound having a second cation and a second anion; and an intermediate layer solvent; wherein the electron density of the first cation is greater than the electron density of the second cation.

[0124] In one embodiment of the present disclosure, the step (S1) may include a step of applying and heat-treating a perovskite precursor solution to crystallize the anions and cations contained in the perovskite precursor solution to produce a three-dimensional perovskite crystal.

[0125] The heat treatment step may be 30°C or higher, 40°C or higher, 50°C or higher, 60°C or higher, 70°C or higher, or 80°C or higher, and the upper limit may be 160°C or lower, 150°C or lower, 140°C or lower, 130°C or lower, 120°C or lower, or 110°C or lower. Specifically, it may be 30 to 160°C, 40 to 150°C, 50 to 140°C, 60 to 130°C, or 70 to 120°C, and more specifically, it may be 80 to 110°C.

[0126] Since the above heat treatment step is performed within the above temperature range, it is possible to grow dense and uniform three-dimensional perovskite crystals without decomposing chemical species contained in other components.

[0127] In addition, the heat treatment time of the above three-dimensional perovskite may be 30 seconds or more, 1 minute or more, 10 minutes or more, or 30 minutes or more, and the upper limit may be 24 hours or less, 12 hours or less, 10 hours or less, 6 hours or less, or 3 hours or less. Specifically, it may be 30 seconds to 24 hours, 1 minute to 12 hours, 10 minutes to 10 hours, 30 minutes to 6 hours, and more specifically, 30 minutes to 3 hours.

[0128] Within the time range described above, thermal degradation of the perovskite thin film may be minimal, and perovskite crystals can be grown densely and uniformly.

[0129] According to one embodiment of the present disclosure, the ratio of the first intermediate layer compound and the second intermediate layer compound included in the intermediate layer solution may be 0.1:1 to 1:0.1. The intermediate layer may be prepared by applying the intermediate layer solution. Accordingly, as described above, the molar ratio of the first intermediate layer compound and the second intermediate layer compound included in the intermediate layer may be selected to be the same as the molar ratio of the first intermediate layer compound and the second intermediate layer compound included in the intermediate layer described above.

[0130] In one embodiment of the present disclosure, the step of coating the intermediate layer solution may be performed by a method selected from the group consisting of screen printing, spin coating, bar coating, gravure coating, blade coating, and roll coating.

[0131] In one embodiment of the present disclosure, the step of heat-treating the intermediate layer formed after step (S2) may be further included.

[0132] The above heat treatment temperature may be 30°C or higher, 40°C or higher, 50°C or higher, 60°C or higher, 70°C or higher, or 75°C or higher, and the upper limit may be 160°C or lower, 150°C or lower, 140°C or lower, 130°C or lower, 120°C or lower, or 110°C or lower. Specifically, it may be 30 to 160°C, 40 to 150°C, 50 to 140°C, 60 to 130°C, or 70 to 120°C, and more specifically, it may be 80 to 120°C.

[0133] The heat treatment time may be 30 seconds or more, 1 minute or more, 2 minutes or more, or 3 minutes or more, and the upper limit may be 24 hours or less, 10 hours or less, 5 hours or less, 1 hour or less, or 30 minutes or less. Specifically, it may be 30 seconds to 10 hours, 1 minute to 5 hours, 3 minutes to 1 hour, and more specifically, 3 minutes to 30 minutes.

[0134] As such, the method for manufacturing a perovskite photovoltaic device according to the present disclosure can form an intermediate layer in which two or more types of n=2 quasi-two-dimensional perovskites are uniformly distributed over a large area, thereby providing a perovskite photovoltaic device that exhibits high tube conversion efficiency, high thermal stability, and high stability in air at low cost.

[0135] A perovskite solar cell comprising the perovskite photovoltaic element of the present disclosure will be described below.

[0136] According to another embodiment of the present disclosure, a perovskite solar cell may be provided comprising: a substrate; a first electrode formed on the substrate; a perovskite photovoltaic device according to claim 30 formed on the first electrode; and a second electrode stacked on the photovoltaic device.

[0137] In one embodiment of the present disclosure, the first electrode can be used without limitation as long as it is a conductive electrode that is ohmic-junctioned with the perovskite thin film.

[0138] Specifically, the first electrode may be a transparent conductive electrode, and the transparent conductive electrode may be one or more selected from the group consisting of fluorine-doped tin oxide (FTO), indium-doped tin oxide (ITO), zinc oxide, carbon nanotubes, graphene, and combinations thereof, but is not necessarily limited thereto.

[0139] In one embodiment of the present disclosure, the second electrode may be a conductive electrode ohmic-bonded to the perovskite thin film, and if the work function is different from that of the first electrode so that electrons and holes generated by the photoelectric effect in the perovskite thin film are transferred to the first electrode and the second electrode, respectively, and a photocurrent can be generated, a person skilled in the art may appropriately select and use the electrode material without limitation.

[0140] Specifically, the second electrode may be one or more selected from the group consisting of gold (Au), silver (Ag), platinum (Pt), palladium (Pd), copper (Cu), aluminum (Al), carbon, cobalt sulfide, copper sulfide, nickel oxide, and combinations thereof, but is not necessarily limited thereto.

[0141] In one embodiment of the present disclosure, an electron transport layer or a hole transport layer may be further included on the upper or lower portion of each component of the aforementioned perovskite photovoltaic device. By further including an electron transport layer or a hole transport layer, the electrical performance of the solar cell can be improved.

[0142] Specifically, the electron transport layer may be an electron-conducting organic or inorganic material. More specifically, it may be an electron-conducting organic thin film such as 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP) or a metal oxide thin film such as titanium oxide, zinc oxide, indium oxide, tin oxide, tungsten oxide, niobium oxide, molybdenum oxide, magnesium oxide, zirconium oxide, strontium oxide, lanthanum oxide, vanadium oxide, aluminum oxide, yttrium oxide, gallium oxide, or a composite thereof, but is not necessarily limited thereto, and it is sufficient if it is a material layer commonly used for electron conduction in conventional perovskite optoelectronic devices.

[0143] Specifically, the hole transport layer may be a hole-conducting organic or inorganic material. More specifically, it may be a hole-conducting organic thin film such as poly(3,4-ethylenedioxythiophene) polystyrene sulfonate (PEDOT:PSS) or copper phthalocyanine (CuPc), or a metal oxide thin film such as tungsten oxide, molybdenum oxide, vanadium oxide, nickel oxide, or a composite thereof, but is not necessarily limited thereto, and any material layer commonly used for hole conduction in conventional perovskite optoelectronic devices can be appropriately selected and used by a person skilled in the art.

[0144] To facilitate understanding of the present disclosure, it will be described in detail below through examples and the like. However, the embodiments according to the present disclosure are not limited to the embodiments described herein and may be modified in various other forms, and the scope of the present disclosure should not be interpreted as being limited to the following embodiments. The embodiments of the present disclosure are provided to more completely explain the present disclosure to those with average knowledge in the art, and are provided merely to sufficiently convey the concept of the present disclosure to those skilled in the art.

[0146] <Example 1>

[0147] An FTO glass substrate (Asahi VU glass, 12-13 Ω·cm-2) was ultrasonically treated sequentially in acetone, detergent, and ethanol for 20 minutes each. The FTO glass substrate was immersed in a solution prepared by mixing SnCl2·2H2O (108 mg), urea (500 mg), thioglycolic acid (10 μl), and hydrochloric acid (500 μl) in 40 ml of deionized water. SnO2 was deposited on the glass substrate by immersing the FTO and the solution in a Hellendahl staining dish in a water bath at 70°C for 6 hours.

[0148] The FTO substrate (FTO / SnO2) on which SnO2 was deposited was cleaned by ultrasonically treating it with ethanol for 1 minute. The FTO / SnO2 substrate was annealed at 150°C for 1 hour, then spin-coated with a KCl solution (40 mM) in non-ionized water and annealed at 150°C for 15 minutes.

[0149] A perovskite precursor solution was prepared by dissolving 1.4 M FAPbI3 powder in ACCl (0.75 mol%), PACl (4 mol%), and MACI (35 mol%) in a mixed solvent of DMF:DMSO = 8:1. The perovskite solution was spin-coated onto the FTO / SnO2 substrate at 1,000 rpm for 10 seconds and at 5,000 rpm for 15 seconds. While the substrate was rotating, 1 ml of ethyl ether was dropped onto the substrate. The perovskite layer was heat-treated at 120°C for 1 hour.

[0150] A 100 mol% MC solution (M / C) was prepared by dissolving 16 mM MeO-PEAI and 16 mM CHABr in 2-propanol (IPA). The MC solution was spin-coated onto a perovskite-coated substrate at 5,000 rpm for 30 seconds and annealed at 100°C for 5 minutes.

[0151] A Spiro-OMeTAD solution prepared by mixing 90 mg / ml of Spiro-OMeTAD in chlorobenzene with 37 μl of t-BP, 23 μl of Li-TFSI salt (516 mg / ml in ACN), and 9 μl of Co-TFSI salt (375 mg / ml in ACN) was spin-coated onto an intermediate layer of the MC solution at 3,500 rpm for 30 seconds.

[0152] Finally, a perovskite photovoltaic device was fabricated by depositing a gold counter electrode with a thickness of 70 nm using thermal evaporation.

[0154] <Example 2>

[0155] In Example 1, a perovskite photovoltaic device was prepared in the same manner as in Example 1, except that the 8 mM CHABr was dissolved to prepare a 50 mol% MC solution (M / 0.5C).

[0157] <Comparative Example 1>

[0158] In Example 1, a perovskite photovoltaic device was prepared in the same manner as in Example 1, except that a 0 mol % MC(M) solution was prepared without dissolving the CHABr.

[0160] <Comparative Example 2>

[0161] In Example 1, a perovskite photovoltaic device was prepared using the same method as in Example 1, except that MeO-PEAI was not dissolved.

[0163] Physical property evaluation methods

[0164] 1) Thermal stability measurement (XRD, SEM, JV curve)

[0165] The efficiency device test JV curve measurements were performed using a Keithley 2420 source meter and conducted under illumination with an AM 1.5G filter and an irradiation intensity of 100 mW / cm² via a solar simulator (Newport, Oriel Sol3A class AAA). The tests were performed with a starting voltage of -0.2 V and a ending voltage of 1.5 V. The number of measurement points was 170, the voltage stabilization time was 10 ms, and the NPLC (Number of Power Line Cycles) was 0.01 (Fast mode). The following formula was used to calculate the Power Conversion Efficiency (PCE, %).

[0166] (4)

[0167] J sc (Short-Circuit Current Density, mA / cm 2 ) is the short-circuit current density, V oc (Open-circuit voltage, V) is the open-circuit voltage, FF (fill factor, %), P in is the intensity of incident sunlight (light) (mainly 1 sun, 1000W / m²) 2 )am.

[0169] 2) Measurement of device efficiency (JV curve)

[0170] The efficiency device test JV curve measurements were performed using a Keithley 2420 source meter and conducted under illumination with an AM 1.5G filter and an irradiation intensity of 100 mW / cm² via a solar simulator (Newport, Oriel Sol3A class AAA). The tests were performed with a starting voltage of -0.2 V and a ending voltage of 1.5 V. The number of measurement points was 170, the voltage stabilization time was 10 ms, and the NPLC (Number of Power Line Cycles) was 0.01 (Fast mode). The following formula was used to calculate the Power Conversion Efficiency (PCE, %).

[0171] (4)

[0172] J sc (Short-Circuit Current Density, mA / cm 2 ) is the short-circuit current density, V oc (Open-circuit voltage, V) is the open-circuit voltage, FF (fill factor, %), P in is the intensity of incident sunlight (light) (mainly 1 sun, 1000W / m²) 2 )am.

[0174] 3) Measurement of photostability and storage stability (MPPT, JV curve)

[0175] 3-1) Thermal Stability Device Test

[0176] Samples coated with FTO / tin oxide / perovskite / intermediate layer were placed on a hot plate at a temperature of 85°C for 3 hours. Subsequently, devices were fabricated by depositing Spiro-OMeTAD (HTL) and Au, and the performance of the devices was measured over time.

[0178] 3-2) Device Stability Test

[0179] 1. Stability tests for continuous maximum output power tracking device operation under sunlight (AM 1.5G, Xe lamp, 450 W) were performed on the packaged devices in a nitrogen (N2) atmosphere, and V MPP After fixing the voltage, the current output was tracked.

[0181] Evaluation Example 1: Evaluation of 3D / 2D interfacial defects through FT-IR, NMR, and SEM analysis.

[0182] Figure 1 shows the FT-IR and NMR analyses of the intermediate layer solution and the intermediate layer of the example and comparative example.

[0183] Referring to Figure 1b, when the intermediate layer solution of Example 1 is physically mixed and dried, the O-H group peak decreases, which confirms that hydrogen bonds are weakened or new bonds are formed through strong chemical interactions between MeO-PEAI and CHABr.

[0184] Referring to FIGS. 1c and 1d, Examples 1 and 2 have NH3 due to the mixing of the two compounds. + It can be seen that the peaks of the phenyl group and the phenyl group are shifted, which means that an intermediate layer of a new structure of the two-dimensional perovskite has been formed due to electronic interactions of the material.

[0185] FIG. 2 illustrates the interface between the three-dimensional (3D) perovskite and the intermediate layer and the crystal structure of the intermediate layer of the example and comparative example.

[0186] Referring to the surface SEM of Fig. 2, it can be seen that in Examples 1 and 2, there are almost no grain boundaries on the surface and a uniform crystal structure is exhibited overall.

[0187] Furthermore, by referring to the cross-SEM, the interface between the 3D perovskite and the intermediate layer can be confirmed. Examples 1 and 2 exhibit a smooth structure with minimized defects between the interfaces of the perovskite and the intermediate layer, and Example 2, in particular, exhibits the most stable interface characteristics. This implies that due to the electron density difference and the interaction between the two materials, the first cation has a high electron density and exhibits rapid reactivity with the surface of the perovskite layer, while the second cation reacts intensively with unbonded perovskite cations to form a low-roughness and uniform quasi-2D perovskite, thereby minimizing defects on the 3D / 2D interface.

[0188] Accordingly, Examples 1 and 2 of the present disclosure confirmed that by satisfying the conditions of the first intermediate layer compound and the second intermediate layer compound, the interaction between the first cation and the second cation is optimized, thereby forming a stable 3D / 2D stacked structure.

[0190] Evaluation Example 2: Evaluation of thermal stability of a photovoltaic device through XRD analysis.

[0191] 1) XRD peak and SEM surface analysis

[0192] To compare the thermal stability of the two-dimensional structure at a high temperature of 85℃ and 40%RH (Room humidity), the time-dependent change of the XRD (X-Ray diffraction) peaks was observed.

[0193] Figure 3 shows the change in XRD peaks over time at a high temperature of 85°C for Comparative Example 1 and Example 2.

[0194] Referring to Fig. 3, it can be seen that in Comparative Example 1, the n=1 diffraction peak of M-PEA2PbI4 (5°) with 2D (n=1) has mostly disappeared after heat treatment for 1 hour. This result is M-PEA +This means that cations easily move into the interior of the 3D perovskite under thermal stress, causing the intermediate layer of the 2D perovskite with n=1 to decompose. In other words, Comparative Example 1 implies that device instability may result from a weak 2D / 3D perovskite structure.

[0195] Figure 4 shows SEM image analysis of the surface conditions before and after heat treatment of Comparative Example 1 and Example 2.

[0196] Referring to Fig. 4, it can be seen that in Comparative Example 1, defects on the surface of the intermediate layer are visible even before heat treatment, and after heat treatment, the surface decomposes due to heat, resulting in low structural stability.

[0197] In contrast, looking at Example 2, it can be seen that the peak intensity of (MC)2FAPb2I7 (3.8°) with Quasi-2D (n=2) remained almost unchanged even after heat treatment at 85°C for 5 hours. In addition, referring to Figure 4, it was confirmed that Example 2 formed a uniform and stable crystal structure on the surface even before heat treatment, and that the crystal structure remained unchanged and stable even after heat treatment.

[0198] That is, it was confirmed that when the intermediate layer of the present disclosure is heated at a high temperature of 85°C and for more than 5 hours, the thermal decomposition of the intermediate layer 2D perovskite is minimal, and a stable stacked structure of 3D / 2D perovskite is exhibited, thereby improving the stability of the optoelectronic device and improving the performance and lifespan of the device.

[0200] 2) JV curve analysis

[0201] This time, the JV curve for the thermal stability of the device was analyzed.

[0202] The following table compares the performance changes of the optoelectronic devices of Example 2 and Comparative Example 1 according to the heat treatment time.

[0203] Interlayer Themal time J sc (mA / cm 2 ) V oc (V) FF (%) PCE Reverse Comparative Example 1 0h 24.47 1.15 83.17 23.37 1h 24.69 1.12 81.18 22.40 3h 24.85 1.09 71.77 19.40 Example 2 0h 25.02 1.18 83.82 24.89 1h 25.01 1.17 82.66 24.15 3h 24.86 1.16 81.81 23.55

[0204] Figure 5 shows a table comparing PCE, J, V, and FF of Example 2 and Comparative Example 1. Referring to Figure 5 and Table 1, the unstable M-PEA + Due to the displacement of the unit, the power conversion efficiency (PCE) of Comparative Example 1 gradually decreased to 82.8% of the initial efficiency (23.37%). However, it can be confirmed that Example 2 stably maintained 96% of the initial efficiency (24.89%).

[0205] Referring to Fig. 5d, it can be seen that the filling rate (FF) of the comparative example has decreased to 86.5% of the initial efficiency (83.17%). On the other hand, it was confirmed that Example 2 can be stably maintained at 98.4% of the initial efficiency (83.82%) with almost no change.

[0206] In other words, it has been confirmed that the photovoltaic device of the present disclosure improves thermal stability, thereby maintaining the structural and electrical characteristics of the device even in high-temperature environments, which can significantly improve the stability and reliability of the device and contribute to an extended device lifespan.

[0208] Evaluation Example 3: Performance evaluation of perovskite solar cells (PSC)

[0209] The performance of perovskite solar cells (PSCs) according to each intermediate layer was compared.

[0210] Figure 6 shows the PCE (%), J of the examples and comparative examples. SC (mA cm -2 ), FF(%), V OC This illustrates a comparison of the performance of (V).

[0211] Referring to Figure 6, most Jsc and Voc were similar, but Example 2 recorded the highest average value along with the highest FF, exhibiting superior thermal stability and electrical performance compared to other conditions.

[0212] Table 2 below shows the solar cell performance of Example 2.

[0213] J SC (mA cm -2 ) V OC (V) FF(%) PCE(%) Reverse 25.76 1.19 85.71 26.28 Forward 25.66 1.19 85.55 26.12

[0214] Figure 7 illustrates the electrical characteristics of a perovskite solar cell (PSC) using the JV curve (Current density vs. Voltage) of Example 2. Example 2 shows J in reverse scan mode sc , V oc The and FF values ​​are 25.76 mAcm, respectively. -2 , with 1.19 V and 85.71%, the PCE is 26.28%, and at forward bias J sc is 25.66 mAcm -2 , V oc It was measured as 1.19 V, FF as 85.55%, and PCE as 26.12%.

[0215] Example 2 was confirmed to exhibit low hysteresis with almost no difference in performance between the forward and reverse directions. This indicates that the stability and reliability of the device are excellent.

[0217] Evaluation Example 4: Evaluation of long-term optical stability of a photovoltaic device.

[0218] To measure the long-term optical stability of the device, Maximum Power Point Tracking (MPPT) was performed at 30°C with 15-30% relative humidity without a UV blocking filter.

[0219] Figure 8 is a comparative analysis of the long-term photo-stability of Comparative Example 1 and Example 2.

[0220] Referring to Fig. 8, Comparative Example 1 showed that the PCE performance decreased by about 20% or less over time, and it was confirmed that this was a decrease of about 22% or more compared to the initial PCE (25.7%). It can be predicted that this decrease in performance is a phenomenon caused by the degradation of the device and the thermal instability of the intermediate layer.

[0221] On the other hand, Example 2 maintained approximately 90% of the initial efficiency (25.91%) after 440 hours, and storage stability maintained approximately 100% of the initial efficiency (25.14%) for 9,000 hours. That is, the present disclosure can provide a photoelectric device with excellent light stability and storage stability.

[0222] Although embodiments of the present invention have been described above with reference to the attached drawings, those skilled in the art will understand that the present invention may be implemented in other specific forms without changing its technical concept or essential features. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive.

Claims

Claim 1 A perovskite photovoltaic device comprising: a perovskite thin film including a three-dimensional perovskite; and an intermediate layer located on the perovskite thin film; wherein the intermediate layer comprises two or more types of quasi-two-dimensional perovskites, and the quasi-two-dimensional perovskite is prepared by mixing a first intermediate layer compound including a first cation and a first anion; and a second intermediate layer compound including a second cation and a second anion; in an intermediate layer solvent, wherein the electron density of the first cation is greater than the electron density of the second cation, and the first cation satisfies the following chemical formula 2. [Chemical Formula 2] (In the above Chemical Formula 2, R1 comprises one or more selected from the group consisting of a straight-chain or branched-chain alkoxy group having 1 to 10 carbon atoms, an aryloxy group having 6 to 60 carbon atoms, and derivatives thereof.) Claim 2 A perovskite photovoltaic device according to claim 1, wherein the three-dimensional perovskite is a compound represented by the following chemical formula 1. (Chemical Formula 1) ABX3 (wherein A is a monovalent alkylammonium cation, a monovalent amidinium cation, Li + , Na + , K + , Rb + , Cs + , Fr + , Cu(I) + , Ag(I) + and Au(I) + It comprises one or more monovalent cations selected from the group consisting of, where B is a divalent metal cation, and X is I - , Br - , Cl - ...and includes one or more halogen anions selected from the group consisting of combinations thereof.) Claim 3 delete Claim 4 The perovskite photovoltaic device according to claim 1, wherein the second cation satisfies the following chemical formula 3. [Chemical Formula 3] (In the above Chemical Formula 3, R2 is selected from one or more of the group comprising straight-chain or branched-chain alkyl having 1 to 10 carbon atoms, straight-chain or branched-chain alkenyl having 1 to 10 carbon atoms, straight-chain or branched-chain alkanyl having 1 to 10 carbon atoms, monocyclic or polycyclic cycloalkane having 3 to 30 carbon atoms, monocyclic or polycyclic aryl having 6 to 30 carbon atoms, and derivatives thereof.) Claim 5 A perovskite photovoltaic device according to claim 1, wherein the first cation is methoxyphenylammonium. Claim 6 A perovskite photovoltaic device according to claim 1, wherein the second cation is cyclohexylammonium. Claim 7 In claim 1, the first anion and the second anion are each independently fluorine (F - ), chlorine (Cl - ), Bromine (Br - ) and iodine(I - A perovskite photovoltaic device selected from the group consisting of ). Claim 8 A perovskite photovoltaic device according to claim 1, wherein the mixing ratio of the first intermediate layer compound and the second intermediate layer compound is 0.1:1 to 1:0.

1. Claim 9 A perovskite photovoltaic device according to claim 1, wherein the quasi-two-dimensional perovskite formation energy of the first intermediate layer compound and the second intermediate layer compound dissolved in the intermediate layer solvent is -100 eV or less. Claim 10 A perovskite photovoltaic device according to claim 1, wherein the intermediate layer solvent is an alcohol-based solvent. Claim 11 A perovskite photovoltaic device according to claim 10, wherein the intermediate layer solvent is isopropanol (IPA). Claim 12 A perovskite photovoltaic device according to claim 1, wherein the intermediate layer is a quasi-2D perovskite of n=2. Claim 13 A perovskite photovoltaic device according to claim 1, wherein the thickness of the intermediate layer is 0.1 to 10 nm. Claim 14 The perovskite photovoltaic device according to claim 1, wherein the perovskite photovoltaic device has a power conversion efficiency (PCE) of 90% or more compared to the initial efficiency even after heat treatment at a temperature of 80°C for 3 hours. Claim 15 A perovskite photovoltaic device according to claim 1, wherein the perovskite photovoltaic device maintains a power conversion efficiency (PCE) of 90% or more compared to the initial value after storage at room temperature for 9,000 hours. Claim 16 (S1) a step of manufacturing a perovskite thin film comprising a three-dimensional perovskite crystal structure; and (S2) a step of depositing an intermediate layer by applying an intermediate layer solution onto the perovskite thin film; wherein the intermediate layer solution comprises a first intermediate layer compound comprising a first cation and a first anion; a second intermediate layer compound comprising a second cation and a second anion; and an intermediate layer solvent; wherein the electron density of the first cation is greater than the electron density of the second cation, and the first cation satisfies the following Chemical Formula 2, a method for manufacturing a perovskite photovoltaic device. [Chemical Formula 2] (In the above Chemical Formula 2, R1 comprises one or more selected from the group consisting of a straight-chain or branched-chain alkoxy group having 1 to 10 carbon atoms, an aryloxy group having 6 to 60 carbon atoms, and derivatives thereof.) Claim 17 A method for manufacturing a perovskite photovoltaic device according to claim 16, wherein the intermediate layer solvent is an alcohol. Claim 18 A method for manufacturing a perovskite photovoltaic device according to claim 16, wherein the intermediate layer solvent is isopropanol (IPA). Claim 19 A method for manufacturing a perovskite photovoltaic device according to claim 16, wherein the quasi-two-dimensional perovskite formation energy of the intermediate layer solution is -150 eV or less. Claim 20 A method for manufacturing a perovskite photovoltaic device according to claim 16, wherein the mixing ratio of the first intermediate layer compound and the second intermediate layer compound included in the intermediate layer solution is 0.1:1 to 1:0.

1. Claim 21 A method for manufacturing a perovskite photovoltaic device according to claim 16, wherein the perovskite thin film is a compound represented by the following chemical formula 1. (Chemical Formula 1) ABX3 (wherein A is a monovalent alkylammonium cation, a monovalent amidinium cation, Li + , Na + , K + , Rb + , Cs + , Fr + , Cu(I) + , Ag(I) + and Au(I) + It comprises one or more monovalent cations selected from the group consisting of, where B is a divalent metal cation, and X is I - , Br - , Cl - ...and includes one or more halogen anions selected from the group consisting of combinations thereof.) Claim 22 delete Claim 23 In claim 16, a method for manufacturing a perovskite photovoltaic device, wherein the second cation satisfies the following chemical formula 3. [Chemical Formula 3] (In the above Chemical Formula 3, R2 is selected from one or more of the group comprising straight-chain or branched-chain alkyl having 1 to 10 carbon atoms, straight-chain or branched-chain alkenyl having 1 to 10 carbon atoms, straight-chain or branched-chain alkanyl having 1 to 10 carbon atoms, monocyclic or polycyclic cycloalkane having 3 to 30 carbon atoms, monocyclic or polycyclic aryl having 6 to 30 carbon atoms, and derivatives thereof.) Claim 24 A method for manufacturing a perovskite photovoltaic device, wherein, in paragraph 16, the first cation is methoxyphenylammonium. Claim 25 A method for manufacturing a perovskite photovoltaic device, wherein, in claim 16, the second cation is cyclohexylammonium. Claim 26 In paragraph 16, the first anion and the second anion are each independently fluorine (F - ), chlorine (Cl - ), Bromine (Br - ) and iodine(I - A method for manufacturing a perovskite photovoltaic device, selected from the group consisting of ). Claim 27 A method for manufacturing a perovskite optoelectronic device according to claim 16, wherein the step of forming an intermediate layer is performed by a method selected from the group consisting of screen printing, spin coating, bar coating, gravure coating, blade coating, and roll coating. Claim 28 A method for manufacturing a perovskite photovoltaic device according to claim 16, further comprising the step of heat-treating the intermediate layer at a temperature in the range of 80 to 150°C for 3 to 60 minutes after the above step (S2). Claim 29 A perovskite photovoltaic device manufactured according to any one of paragraphs 16 through 21 and paragraphs 23 through 28. Claim 30 A perovskite solar cell comprising: a substrate; a first electrode formed on the substrate; a perovskite photovoltaic device according to claim 29 and a second electrode formed on the photovoltaic device. Claim 31 A perovskite solar cell according to claim 30, further comprising an electron transport layer or a hole transport layer on the upper or lower part of the perovskite photovoltaic device.

Citation Information

Patent Citations

  • Organic-inorganic perovskite, film, luminescent film, delayed fluorescent emission film, light-emitting device and method for manufacturing light-emitting device

    KR1020200083505A

  • Method for forming a crystalline or polycrystalline layer of organic-inorganic metal halide perovskite

    KR1020210063371A

  • Manufacturing method of perovskite solar cell

    KR1020230157146A

  • Sequential deposition of perovskites

    KR1020240160196A