Temporary capping material for oxide prevention during low-temperature direct metal-to-metal bonding

Stimulus-responsive polymers prevent oxidation during metal-to-metal bonding in semiconductor manufacturing, enabling low-temperature bonding and maintaining interface quality.

KR103045693B1Active Publication Date: 2026-11-10LAM RES CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
KR1020227044793
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-10
Filing Date
2021-09-09
Publication Date
2026-11-10
Estimated Expiration
2041-09-09

AI Technical Summary

Technical Problem

Direct metal-to-metal bonding in semiconductor manufacturing is challenged by high temperatures and metal oxide formation, which can damage components and degrade bonding quality.

Method used

The use of stimulus-responsive polymers (SRPs) as capping materials to prevent oxidation during bonding, allowing for low-temperature metal-to-metal bonding by removing the SRP layer under mild conditions.

Benefits of technology

Enables high-quality metal-to-metal bonding without damaging sensitive components, while maintaining residue-free interfaces and optimizing bonding quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023039620571-PCT00035_ABST
    Figure 112023039620571-PCT00035_ABST
Patent Text Reader

Abstract

The present disclosure relates to the use of SRP (stimulus-sensitive polymer) as a capping material during direct metal-metal bonding. Processes and layers employing SRP are described herein.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present disclosure relates to the use of stimulus-responsive polymers (SRPs) as capping materials during direct metal-metal bonding. Processes and layers employing SRPs are described herein. Background Technology

[0002] During semiconductor manufacturing, direct metal-to-metal bonds can be formed using thermal compression, where two clean metal features come into contact. Typically, high-quality bonding requires significant force and high temperatures, which can damage critical components on next-generation chips and heterogeneous integrated assemblies. Furthermore, some metals, such as copper, readily react with oxygen to form metal oxides at bonding interfaces, and these interface oxides can degrade bonding quality and impair chip performance.

[0003] The description of the background technology provided in this specification is intended to provide a general context for the technology. The work of the inventors named in this specification to the extent described in this background technology section, as well as aspects of the technology that may not otherwise be recognized as prior art at the time of filing, are not explicitly or implicitly acknowledged as prior art for the technology.

[0004] Citation as a reference

[0005] A PCT application form has been filed concurrently with this specification as part of this application. Each application claiming priority or benefit as identified in the PCT application form filed concurrently with this application is incorporated herein by reference in its entirety for all purposes. This application claims the benefit of priority of U.S. Provisional Patent Application No. 63 / 076,861 filed on September 10, 2020, which is incorporated herein by reference in its entirety.

[0006] The present disclosure relates to a temporary capping material for protecting surfaces prior to bonding. In certain embodiments, the capping material comprises a stimulus-responsive polymer (SRP) that can be deposited on sensitive surfaces to prevent oxide formation. Sensitive surfaces include substrates and metal features exposed during semiconductor processing for the manufacture of integrated circuits (ICs) and 3D ICs. Prior to further processing, the capping material may be removed under mild conditions to provide a residue-free interface for optimal metal-to-metal bond formation. In some embodiments, SRP removal and metal-to-metal bonding are performed under low-temperature conditions and, optionally, within the same tool or device.

[0007] Accordingly, in a first embodiment, the present disclosure comprises a method comprising: a step of aligning a first capped feature with a second capped feature, wherein each of the first capped feature and the second capped feature independently comprises a stimulus-responsive polymer (SRP) layer disposed on the surface of a metal feature; and a step of bonding the first capped feature and the second capped feature in an atmosphere to remove the SRP and form a metal-metal bond between the metal features. In some embodiments, the SRP layer prevents oxidation of the metal feature. In other embodiments, the SRP layer has a thickness of about 10 nm to 10 µm.

[0008] In some embodiments, the bonding step comprises: an exposure step of exposing a first capped feature and a second capped feature to a removal temperature for removing SRP, thereby providing metal features exposed accordingly; and a step of contacting the exposed metal features to form a metal-metal bond. In some embodiments, the removal temperature is about 50°C to about 250°C.

[0009] In other embodiments, the exposing step comprises the use of acidic vapor, heat, extreme ultraviolet (EUV) light or ultraviolet (UV) light or vacuum ultraviolet light, plasma, metastable neutrons from noble gas plasma, or a combination thereof.

[0010] In some embodiments, the bonding includes a bonding temperature of about 25°C to about 250°C. In other embodiments, the bonding includes the use of an inert atmosphere, a vacuum atmosphere, a reducing gas, or ambient air.

[0011] In other embodiments, the method comprises (e.g., before the alignment): (i) a deposition step of depositing a first SRP layer on the surface of a first metal feature, thereby providing a first capped feature; and (ii) a deposition step of depositing a second SRP layer on the surface of a second metal feature, wherein the deposition provides a second capped feature. In some embodiments, the first SRP layer is further disposed on the surface of a gap-filling layer surrounding the first metal feature. In other embodiments, the second SRP layer is further disposed on the surface of a gap-filling layer surrounding the second metal feature. In other embodiments, the method comprises (e.g., before the deposition in (i) and / or (ii): a step of pre-treating the surfaces of the first metal feature and the second metal feature to clean the surfaces and / or remove the oxide layer. In other embodiments, the step of depositing in (i) and / or (ii) includes vapor-based or solvent-based deposition of SRP.

[0012] In a second aspect, the present disclosure comprises a method comprising the step of depositing an SRP to form an SRP layer on the surface of a first metal feature comprising an electrical contact, thereby providing a first capped feature. In some embodiments, the method further comprises (e.g., after the deposition): the step of removing the SRP layer to provide a first exposed metal feature; and the step of contacting the first exposed metal feature to a second exposed metal feature, thereby forming a metal-metal bond between the exposed metal features.

[0013] In some embodiments, the deposition step comprises vapor-based or solvent-based deposition of SRP. In other embodiments, the removal step comprises exposing the SRP layer to heat, extreme ultraviolet light, ultraviolet light or vacuum ultraviolet light, metastable neutrons from a noble gas plasma, acidic vapor, or basic vapor.

[0014] In other embodiments, the method comprises: a deposition step of providing a second capped feature by depositing an SRP to form an SRP layer on the surface of a second metal feature; and a step of removing the SRP layer from the second capped feature to provide a second exposed metal feature. In yet other embodiments, the method further comprises: a step of removing the SRP layer from the second capped feature to provide an exposed metal feature; and a bonding step of bonding the exposed first metal feature and the exposed second metal feature, thereby forming a metal-to-metal bond.

[0015] In a third aspect, the present disclosure comprises a deposition step of depositing an SRP to form an SRP layer on the surface of a first metal feature and a second metal feature, thereby providing a first capped feature and a second capped feature; a step of aligning the first capped feature with the second capped feature; a step of removing the SRP layer to provide exposed metal features; and a step of contacting the exposed metal features to form a metal-metal bond between the exposed metal features.

[0016] In any embodiment of this specification, the SRP includes a ceiling temperature of about 300°C or less. In some embodiments, the ceiling temperature is about 60°C or less, about 50°C or less, about 40°C or less, about 30°C or less.

[0017] In any embodiment of this specification, the SRP further comprises an acid catalyst, an organic acid, a photocatalyst, or a thermal acid catalyst (e.g., any described herein).

[0018] In any embodiment of this specification, the SRP further comprises a metal-binding moiety (e.g., any one described herein). Non-limiting metal-binding moietyes include optionally substituted heterocyclil (e.g., azole), optionally substituted heterocyclyloxy, optionally substituted heterocyclilloyl, thiol, optionally substituted amino, optionally substituted aminoalkyl, carboxyl, optionally substituted carboxyalkyl, hydroxyl, and / or optionally substituted hydroxyalkyl, and other ones described herein.

[0019] In any embodiment of this specification, SRP is the formula (as described in this specification) I ) to chemical formula ( XIII ), chemical formula ( Ia ), chemical formula ( Ib It includes one of the structures, or a salt thereof.

[0020] In any embodiment of the present specification, the SRP layer prevents oxidation of the first metal feature.

[0021] In any embodiment of the present specification, the SRP layer has a thickness of about 10 nm to 10 μm.

[0022] In any embodiment of the present specification, metal features include electrical contacts, raised metal pillars, bonding pads, bumps, microbumps, metal contacts surrounded by a dielectric, or interconnects.

[0023] In any embodiment of this specification, the metal feature (e.g., the first metal feature and / or the second metal feature) comprises copper (Cu), tin (Sn), silver (Ag), gold (Au), aluminum (Al), or alloys thereof. Additional embodiments are described herein.

[0024] Definitions

[0025] "Alkenyl" refers to an optionally substituted C having one or more double bonds. 2-24 It refers to an alkyl group. An alkenyl group is cyclic (e.g., C 3-24 It may be cycloalkenyl or acyclic. The alkenyl group may also be substituted or not substituted. For example, the alkenyl group may be substituted with one or more substituents as described herein for the alkyl group.

[0026] "Alkoxy" means -OR, where R is an alkyl group optionally substituted as described herein. Exemplary alkoxy groups include methoxy, ethoxy, butoxy, trihaloalkoxy, e.g. trifluoromethoxy, etc. The alkoxy group may or may not be substituted. For example, the alkoxy group may be substituted with one or more substituents as described herein with respect to the alkyl group. Exemplary unsubstituted alkoxy groups are C 1-3 , C 1-6 , C 1-12 , C 1-16 , C 1-18 , C 1-20 , or C 1-24 It includes alkoxy groups.

[0027] "alkyl" and the prefix "alk" refer to branched or unbranched saturated hydrocarbon groups of 1 to 24 carbon atoms, e.g., methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, s-butyl, t-butyl, n-pentyl, isopentyl, s-pentyl, neopentyl, hexyl, heptyl, octyl, nonyl, decyl, dodecyl, tetradecyl, hexadecyl, eicosyl, tetracosyl, etc. Alkyl groups are cyclic (e.g., C 3-24 It may be cycloalkyl or acyclic. The alkyl group may be branched or unbranched. The alkyl group may also be substituted or unsubstituted. For example, in the case of alkyl groups of 1, 2, 3, or 2 or more carbons, the alkyl group may be substituted with four substituents independently selected from the group consisting of the following: (1) C 1-6 Alkoxy (e.g., -O-Ak, where Ak is an optionally substituted C) 1-6 (2) C 1-6 Alkylsulfinyl (e.g., -S(O)-Ak, where Ak is an optionally substituted C 1-6 (3) C 1-6Alkylsulfonyl (e.g., -SO2-Ak, where Ak is optionally C 1-6 (4) Amino (e.g., -NR) N1 R N2 , here R N1 and R N2 Each is independently H or an optionally substituted alkyl, or R N1 and R N2 (5) aryl; (6) aryl alkoxy (e.g., -OL-Ar, where L is the divalent form of a selectively substituted alkyl and Ar is a selectively substituted aryl); (7) aryloyl (e.g., -C(O)-Ar, where Ar is a selectively substituted aryl); (8) azido (e.g., -N3); (9) cyano (e.g., -CN); (10) carboxyaldehyde (e.g., -C(O)H); (11) C 3-8 Cycloalkyl (e.g., monovalent saturated or unsaturated non-aromatic cyclic C) 3-8 (12) a hydrocarbon group); (12) a halo (e.g., F, Cl, Br, or I); (13) a heterocyclile (e.g., a 5-membered ring, 6-membered ring, or 7-membered ring containing 1, 2, 3, or 4 non-carbon heteroatoms such as nitrogen, oxygen, phosphorus, sulfur, or a halo, unless otherwise specified); (14) a heterocyclyloxy (e.g., -O-Het, where Het is a heterocyclile as described herein); (15) a heterocyclilloyl (e.g., -C(O)-Het, where Het is a heterocyclile as described herein); (16) a hydroxyl (e.g., -OH); (17) an N-protected amino; (18) a nitro (e.g., -NO2); (19) an oxo (e.g., =O); (20) a C 3-8Spirocyclil (e.g., alkylene or heteroalkylene diradical, with both ends bonded to the same carbon atom of the parent group); (21) C 1-6 Thioalkoxy (e.g., -S-Ak, where Ak is an optionally substituted C 1-6 (22) alkyl); (22) thiol (e.g., -SH); (23)-CO2R A , here R A is (a) hydrogen, (b) C 1-6 Alkyl, (c) C 4-18 Aryl, and (d) (C 4-18 Aril) C 1-6 Selected from a group consisting of alkyl (e.g., -L-Ar, where L is the divalent form of an optionally substituted alkyl group and Ar is an optionally substituted aryl); (24)-C(O)NR B R C , here R B and R C Each independently (a) hydrogen, (b) C 1-6 Alkyl, (c) C 4-18 Aryl, and (d) (C 4-18 Aril) C 1-6 Selected from a group consisting of alkyl (e.g., -L-Ar, where L is the divalent form of the optionally substituted alkyl group and Ar is the optionally substituted aryl); (25)-SO2R D , here R D is (a) C 1-6 Alkyl, (b) C 4-18 Aryl, and (c) (C 4-18 Aril) C 1-6 Selected from a group consisting of alkyl (e.g., -L-Ar, where L is the divalent form of the optionally substituted alkyl group and Ar is the optionally substituted aryl); (26)-SO2NR E R F , R E and R F Each, independently, (a) hydrogen, (b) C 1-6 Alkyl, (c) C4-18 Aryl, and (d) (C 4-18 Aril) C 1-6 Selected from a group consisting of alkyl (e.g., -L-Ar, where L is the divalent form of the optionally substituted alkyl group and Ar is the optionally substituted aryl); and (27)-NR G R H , here R G and R H Each independently consists of (a) hydrogen, (b) N-protector, (c) C 1-6 Alkyl, (d) C 2-6 Alkenyl (e.g., optionally substituted alkyl having one or more double bonds), (e) C 2-6 Alkynyl (e.g., optionally substituted alkyl having one or more triple bonds), (f) C 4-18 Aryl, (g) (C 4-18 Aril) C 1-6 Alkyl (e.g., L-Ar, where L is the divalent form of the optionally substituted alkyl group and Ar is the optionally substituted aryl), (h) C 3-8 Cycloalkyl, and (i) (C 3-8 cycloalkyl) C 1-6 The alkyl group is selected from the group consisting of alkyls (e.g., -L-Cy, where L is the divalent form of an optionally substituted alkyl group as described herein, and Cy is an optionally substituted cycloalkyl), and in one embodiment, the two groups are not bound to the nitrogen atom via a carbonyl or sulfonyl group. The alkyl group may be a primary, secondary, or tertiary alkyl group substituted with one or more substituents (e.g., one or more halo or alkoxy). In some embodiments, the unsubstituted alkyl group is C 1-3 , C 1-6 , C 1-12 , C 1-16 , C 1-18 , C 1-20 , or C1-24 It is an alkyl group.

[0028] "Alkylene" refers to the polyvalent (e.g., divalent) form of an alkyl group as described herein. Exemplary alkylene groups include methylene, ethylene, propylene, butylene, etc. In some embodiments, the alkylene group is C 1-3 , C 1-6 , C 1-12 , C 1-16 , C 1-18 , C 1-20 , C 1-24 , C 2-3 , C 2-6 , C 2-12 , C 2-16 , C 2-18 , C 2-20 , or C 2-24 It is an alkylene group. The alkylene group may or may not be branched. The alkylene group may also be substituted or may not be substituted. For example, the alkylene group may be substituted with one or more substituents as described herein for alkyl.

[0029] "Alkynyl" is an optionally substituted C having one or more triple bonds. 2-24 It means an alkyl group. The alkynyl group may be cyclic or acyclic and is exemplified by ethinyl, 1-propynyl, etc. The alkynyl group may also be substituted or not substituted. For example, the alkynyl group may be substituted with one or more substituents as described herein for the alkyl group.

[0030] "Amino (amino)" is -NR N1 R N2 It means, and as defined in this specification, R N1 and R N2 Each is independently H, optionally substituted alkyl, or optionally substituted aryl, or R N1 and R N2Each is taken together with an attached nitrogen atom to form a heterocyclyl group.

[0031] "Aminoalkyl" means an alkyl group as defined in this specification, substituted by an amino group as defined in this specification.

[0032] "Aralkyl" or "arylalkyl" means an aryl group as defined herein, attached to a parent molecular group via an alkylene group as defined herein. In some embodiments, the aralkyl group is -Ak-Ar, where Ak is an optionally substituted alkylene as defined herein, and Ar is an optionally substituted aryl as defined herein. The aralkyl group may be substituted or unsubstituted. For example, the aralkyl group may be substituted with one or more substituents as described herein for aryl and / or alkyl. Exemplary unsubstituted aralkyl groups have 7 to 16 carbons (C 7-16 aryl group having 4 to 18 carbons and alkylene group having 1 to 6 carbons (i.e., (C 4-18 Aril)C 1-6 These are things that have alkyl.

[0033] "Aryl" is not limited to, but includes, for example, fused benzo-C (as defined herein, for example), such as indanyl, tetrahydronaphthyl, fluorenyl, etc. 4-8It means a group comprising any carbon-based aromatic group including phenyl, benzyl, anthracenyl, anthryl, benzocyclobutenyl, benzocyclooctenyl, biphenylyl, chrysenyl, dihydroindenyl, fluoranthenyl, indacenyl, indenyl, naphthyl, phenanthryl, phenoxybenzyl, fisenyl, pyrenyl, terphenyl, etc., which includes cycloalkyl radicals. The term aryl also includes "heteroaryl," defined as a group comprising an aromatic group having at least one heteroatom incorporated within the ring of the aromatic group. Examples of heteroatoms include, but are not limited to, nitrogen, oxygen, sulfur, and phosphorus. Similarly, the term non-heteroaryl, which is also included in the term aryl, defines a group comprising an aromatic group that does not contain a heteroatom. The aryl group may or may not be substituted. The aryl group may be substituted with 1, 2, 3, 4, or 5 substituents such as any of those described herein for the alkyl group. In specific embodiments, the unsubstituted aryl group is C 4-18 , C 4-14 , C 4-12 , C 4-10 , C 6-18 , C 6-14 , C 6-12 , or C 6-10 It is Arilgi.

[0034] "Arylene" refers to the polyvalent (e.g., divalent) form of an aryl group as described herein. Exemplary arylene groups include phenylene, naphthylene, biphenylene, triphenylene, diphenyl ether, acenaphtenylene, anthrylene, or phenanthrylene. In some embodiments, the arylene group is C 4-18 , C 4-14 , C 4-12 , C 4-10 , C 6-18 , C 6-14 , C 6-12 , or C 6-10It is an arylene group. The arylene group may or may not be branched. The arylene group may also be substituted or may not be substituted. For example, the arylene group may be substituted with one or more substituents as described herein for aryl.

[0035] "(aryl)(alkyl)ene" means a divalent form comprising an arylene group as described herein, attached to an alkylene or heteroalkylene group as described herein. In some embodiments, the (aryl)(alkyl)ene group is -L-Ar- or -L-Ar-L- or -Ar-L-, where Ar is an arylene group and L is, respectively, an optionally substituted alkylene group or an optionally substituted heteroalkylene group.

[0036] "Azido" means -N3 group.

[0037] "Azidoalkyl" means an azido group attached to a parent molecular group through an alkyl group, as defined in this specification.

[0038] "Carboxyaldehyde" means the -C(O)H group.

[0039] "Carboxyalkyl" means an alkyl group as defined in this specification, substituted by a carboxyl group as defined in this specification.

[0040] "Carboxyl" refers to the -CO2H group.

[0041] "Cyano" means -CN group.

[0042] "Cycloalkenyl" means a non-aromatic carbon-based ring composed of 3 to 10 carbon atoms and containing at least one double bond, i.e., C=C. Examples of cycloalkenyl groups include, but are not limited to, cyclopropenyl, cyclobutenyl, cyclopentenyl, cyclopentadienyl, cyclohexenyl, cyclohexadienyl, etc.

[0043] "Cycloalkyl" means a monovalent saturated or unsaturated non-aromatic cyclic hydrocarbon group having 3 to 8 carbons, unless otherwise specified, and is exemplified by cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, bicyclo[2.2.1.]heptyl, etc. The cycloalkyl group may also be substituted or not substituted. For example, the cycloalkyl group may be substituted with one or more groups including those described herein with respect to the alkyl group.

[0044] "Cycloalkylene" refers to the polyvalent (e.g., divalent) form of a cycloalkyl group as described herein. Exemplary cycloalkylene groups include cyclopropylene, cyclobutylene, cyclopentylene, cyclohexylene, cyclohexenylene, cyclohexadienylene, etc. In some embodiments, the cycloalkylene group is C 3-6 , C 3-12 , C 3-16 , C 3-18 , C 3-20 , or C 3-24 It is a cycloalkylene group. The cycloalkylene group may or may not be branched. The cycloalkylene group may also be substituted or may not be substituted. For example, the cycloalkylene group may be substituted with one or more substituents as described herein with respect to the alkyl group.

[0045] "Fluorosic acid" is A 1 It means CO2H, where A1 is an optionally substituted alkyl or an optionally substituted aryl substituted with one or more fluoro(F) groups.

[0046] "Ester" as used herein refers to -OC(O)A 1 or -C(O)OA 1 It means, and here A 1 As described in this specification, it may be an alkyl, alkenyl, alkynyl, aryl, heteroaryl, cycloalkyl, cycloalkenyl, heterocycloalkyl, or heterocycloalkenyl group.

[0047] "Ether" as used in this specification is A 1 OA 2 It means, and here A 2 As described in this specification, it may independently be an alkyl, alkenyl, alkynyl, aryl, heteroaryl, cycloalkyl, cycloalkenyl, heterocycloalkyl, or heterocycloalkenyl group.

[0048] "Halo" means F, Cl, Br, or I.

[0049] "Haloalkyl" means an alkyl group as defined herein, substituted with one or more halos.

[0050] "Heteroalkyl" means an alkyl group as defined herein containing 1, 2, 3, or 4 non-carbon heteroatoms (e.g., independently selected from the group consisting of nitrogen, oxygen, phosphorus, sulfur, selenium, or halos).

[0051] "Heteroalkylene" means an alkylene group as defined herein containing one, two, three, or four or more non-carbon heteroatoms (e.g., independently selected from groups composed of nitrogen, oxygen, phosphorus, sulfur, selenium, or halogens). In some embodiments, the heteroalkylene group is -Ak-X-, -X-Ak-, -(Ak-X) h1 -Ak-, or -X-(Ak-X) h1 - and, where Ak is an optionally substituted alkylene as defined herein, and X is a non-carbon heteroatom (e.g., -O-, -S-, or -NR N1 -, R N1 H (optionally alkyl, or optionally substituted aryl) or comprises a non-carbon heteroatom, and h1 is an integer from 1 to 5. The heteroalkylene group may or may not be substituted. For example, the heteroalkylene group may be substituted with one or more substituents as described herein for the alkyl group. The heteroalkylene group may be linear or cyclic, such as a divalent heterocyclyl group formed by removing hydrogen from a heterocyclyl group as described herein. Exemplary cyclic heteroalkylene groups include piperylidene, quinolinediyl, etc.

[0052] The term “heterocycloalkenyl” is a cycloalkenyl group of the type defined herein, in which at least one of the carbon atoms of the ring is substituted with O, S, N, or NH. The cycloalkenyl group and the heterocycloalkenyl group may or may not be substituted. The cycloalkenyl group and the heterocycloalkenyl group may be substituted with one or more groups, including but not limited to alkyl, alkoxy, alkenyl, alkynyl, aryl, heteroaryl, carboxyaldehyde, amino, carboxyl, sulfonic acid, sulfinic acid, fluoroacid, phosphonic acid, ester, ether, halo, hydroxyl, ketone, nitro, cyano, azido, silyl, sulfonyl, sulfinyl, or thiol, as described herein.

[0053] The term “heterocycloalkyl” is a cycloalkyl group of the type defined herein, wherein at least one of the carbon atoms and the attached hydrogen atoms is replaced with O, S, N, or NH. The heterocycloalkyl group and the heterocycloalkenyl group may or may not be substituted. The cycloalkyl group and the heterocycloalkyl group may be substituted with one or more groups comprising, but not limited to, alkyl, alkoxy, alkenyl, alkynyl, aryl, heteroaryl, carboxyaldehyde, amino, carboxyl, sulfonic acid, sulfinic acid, fluoroic acid, phosphonic acid, ester, ether, halo, hydroxyl, ketone, nitro, cyano, azido, silyl, sulfonyl, sulfinyl, or thiol as described herein.

[0054] "Heterocyclyl" means a ternary, quaternary, pentary, hexanal, or heptacyclic ring (e.g., pentary, hexanal, or heptacyclic ring) comprising 1, 2, 3, or 4 non-carbon heteroatoms (e.g., independently selected from the group consisting of nitrogen, oxygen, phosphorus, sulfur, selenium, or halos). A ternary ring has 0 to 1 double bond, a quaternary ring and a pentary ring have 0 to 2 double bonds, and a hexanal ring and a heptacyclic ring have 0 to 3 double bonds. The term “heterocyclile” also includes a bicyclic group, a tricyclic group, and a tetracyclic group fused to one, two, or three rings independently selected from the group consisting of any of the heterocyclile rings, an aryl ring, a cyclohexane ring, a cyclohexene ring, a cyclopentane ring, a cyclopentene ring, and another monocyclic heterocyclic ring, such as indolyl, quinolyl, isoquinolyl, tetrahydroquinolyl, benzofuryl, benzothienyl, etc. Heterocyclics include acrridinyl, adenyl, alloxazinil, azaadamantanil, azabenzimidazolyl, azabicyclononil, azacycloheptyl, azacyclooctyl, azacyclononil, azahipoxanthinyl, azaindazolyl, azaindolyl, azecinil, azephanil, azefinil, azetidinil, azetyl, aziridinil, azirinil, azocanil, azocinil, azonanil, benzimidazolyl, benzisothiazolyl, benzisoxazolyl, benzodiazefinil, benzodiazodiazosinyl, benzodihydrofuryl, benzodioxephinil, benzodioxynil, benzodioxanil, benzodioxosinil, benzodioxolyl, benzodithiepinil, benzoditinyl, benzodioxosinil, Benzofuranil, Benzofenazinil, Benzopyranonil, Benzopyranil, Benzopyrenil, Benzopyronil, Benzoquinolinil, Benzoquinolidinil, Benzothiazopinil, Benzothiazolyl, Benzothiazepinil, Benzothiazocinil,Benzothiazolyl, benzothienyl, benzothiophenyl, benzothiazinonil, benzothiazinil, benzothiopyranil, benzothiopyronil, benzotriazefinil, benzotriazinonil, benzotriazinil, benzotriazolyl, benzoxatiinil, benzotrioxefinil, benzoxadiazefinil, benzoxatiazefinil, benzoxatiaefinil, benzoxathiocinil, benzoxazefinil, benzoxazinil, benzoxazozosinil, benzoxazolinonil, benzoxazolinil, benzoxazolyl, benzylsulfamil, benzylsulfimil, bipyrazinil, bipyridinil, carbazolyl (e.g., 4H-carbazolyl), carvolinil (e.g., β-carbvolinil), chromanonil, chromanyl, chromenil, cinolinil, coumarinil, Citdinyl, Cytocinyl, Decahydroisoquinolinil, Decahydroquinolinil, Diazabicyclooctyl, Diazetyl, Diaziridinethionil, Diaziridinonil, Diaziridinyl, Diaziridinyl, Diaziridinyl, Dibenzisoquinolinil, Dibenzoacridinyl, Dibenzocarbazolyl, Dibenzofuranil, Dibenzofenazinil, Dibenzopyranonil, Dibenzopyronil (Xanthonyl), Dibenzoquinoxalinil, Dibenzothiazepinil, Dibenzothiepinil, Dibenzothiophenyl, Dibenzozephinil, Dihydroazepinil, Dihydroazetyl, Dihydrofuranil, Dihydrofuryl, Dihydroisoquinolinil, Dihydropyranil, Dihydropyridinyl, Dihydroypyridyl, Dihydroquinolinyl, dihydrothienyl, dihydroindolyl, dioxanil, dioxazinyl, dioxindolyl, dioxyranil, dioxenyl, dioxinyl, dioxobenzofuranil, dioxolyl, dioxotetrahydrofuranil, dioxothiomorpholinil, dithianil, dithiazolil, dithienyl, dithiinyl, furanil, furazanil, furoyl, furil, guaniyl, homopiperazinil, homopiperidinyl, hypoxanthinyl, hydantoinyl, imidazolidinyl, imidazolininil, imidazolyl, indazollyl (e.g., 1H-indazolyl), indolenyl, indolinyl, indolizinil, indolyl (e.g., 1H-indolyl or 3H-indolyl), isatinyl, Isathil, isobenzofuranil, isocromanil, isochromenil,Isoindazoyl, isoindolinyl, isoindolyl, isopyrazolonil, isopyrazolyl, isoxazolidinyl, isoxazolyl, isoquinolinyl, isothiazolidinyl, isothiazolyl, morpholinyl, naftindazollil, naftindolyl, naftiridinyl, naftopyranil, naftthiazolyl, naftothioxolyl, nafttriazolyl, naftoxindolyl, naftiridinyl, octahydroisoquinolinyl, oxabicycloheptyl, oxauracil, oxadiazollyl, oxazinil, oxaziridinyl, oxazolidinyl, oxazolidonil, oxazolinyl, oxazolonil, oxazolyl, oxepanyl, oxetanonyl, oxetanil, Oxetyl, oxtenayl, oxindolyl, oxiranil, oxobenzisothiazolyl, oxochromenyl, oxoisoquinolinil, oxoquinolinil, oxothiolanil, phenanthridinil, phenanthrolinil, phenazinil, phenothiazinil, phenothienyl (benzothiofuranyl), phenoxatiinil, phenoxazinil, phthalazinil, phthalazonil, phthalidyl, phthalimidinil, piperazinil, piperidinil, piperidonil (e.g., 4-piperidonil), pteridinyl, furinyl, pyranil, pyrazinil, pyrazolidinil, pyrazolinil, pyrazolopyrimidinil, pyrazolil, pyridazinil, pyridinyl, Pyridopyrazinil, pyridopyrimidinil, pyridyl, pyrimidinil, pyrimidyl, pyronil, pyrrolidinil, pyrrolidonil (e.g., 2-pyrrolidonil), pyrrolinil, pyrrolizidinil, pyrrolil (e.g., 2H-pyrrolil), pyrillium, quinazolinil, quinolinil, quinolidinil (e.g., 4H-quinolidinil), quinoxalinil, quinuclidinil, selenazolinil, selenazolyl, selenophenyl, succinimidyl, sulforanil, tetrahydrofuranil, tetrahydrofuril, tetrahydroisoquinolinil, tetrahydroisoquinolil, tetrahydropyridinil, tetrahydropyridyl (piperidyl), tetrahydropyranil, tetrahydropyronil, tetrahydroquinolidinil, Tetrahydroquinolyl, tetrahydrothienyl, tetrahydrothiophenyl,Tetrazinyl, Tetrazolyl, Thiadiazinyl (e.g., 6H-1,2,5-Thiadiazinyl or 2H,6H-1,5,2-Dithiazinyl), Thiadiazolyl, Tiantrenyl, Tianil, Tianaptenil, Thiazefinil, Thiazinyl, Thiazolidinionil, Thiazolidinyl, Thiazolyl, Tienyl, Tiefanyl, Tiepinyl, Tietanyl, Tiethyl, Tiranil, Thiocanil, Thiochromenonil, Thiochromemanil, Thiochromemenil, Thiodiazinyl, Thiodiazolyl, Thioindoxyl, Thiomorpholinyl, Thiophenyl, Thiopyranil, Thiopyrronil, Thiotriazolyl, Thiourazolyl, Thioxanil, Thioxoryl, Thymidinyl, Thyminyl, Triazinyl, Triazolyl, Trithianil, Includes urajinyl, urazolyl, urethidinyl, urethinyl, urisil, uridinyl, xanthenyl, xanthinyl, xantionyl, etc., as well as modified forms thereof (e.g., comprising one or more oxos and / or aminos) and salts thereof. The heterocyclyl group may or may not be substituted. For example, the heterocyclyl group may be substituted with one or more substituents as described herein for the aryl group.

[0055] "Heterocyclildiyl" means a heterocyclil group in a divalent form, as described herein. In one example, a heterocyclildiyl is formed by removing a hydrogen from a heterocyclil group. Exemplary heterocyclildiyl groups include piperidylidene, quinolinediyl, etc. A heterocyclildiyl group may also be substituted or not substituted. For example, a heterocyclildiyl group may be substituted with one or more substituents, as described herein for heterocyclil.

[0056] "Heterocyclyloxy" means a heterocyclyl group attached to a parent molecular group via an oxygen atom, as defined in this specification.

[0057] "Heterocyclil" means a heterocyclil group attached to a parent molecular group via a carbonyl group, as defined in this specification.

[0058] "Hydroxyl" means -OH.

[0059] "Hydroxyalkyl" means an alkyl group as defined in this specification that is substituted by one to three hydroxyl groups, with the caveat that one or fewer hydroxyl groups may be attached to a single carbon atom of the alkyl group, and is exemplified by hydroxymethyl, dihydroxypropyl, etc.

[0060] "Ketone" is A 1 C(O)A 2 It means, and here A 1 and A 2 As described in this specification, it may independently be an alkyl, haloalkyl, alkenyl, alkynyl, aryl, heteroaryl, cycloalkyl, cycloalkenyl, heterocycloalkyl, or heterocycloalkenyl group.

[0061] "Nitro" means -NO2 group.

[0062] "Oxy" means -O-

[0063] "Phosphonic acid" means -P(O)(OH)2.

[0064] "Silic" is -SiA 1 A 2 A 3 It means, and here A 1 , A 2 , and A 3 Each may independently be an alkyl, haloalkyl, alkenyl, alkynyl, aryl, heteroaryl, cycloalkyl, cycloalkenyl, heterocycloalkyl, or heterocycloalkenyl group as described in this specification.

[0065] "Sulfinic acid" means -S(O)OH.

[0066] "Sulfinyl" means -S(O)A1, where A1 may be hydrogen, alkyl, haloalkyl, alkenyl, alkynyl, aryl, heteroaryl, cycloalkyl, cycloalkenyl, heterocycloalkyl, or heterocycloalkenyl group as described in this specification.

[0067] "Sulfonic acid" means -S(O)2OH.

[0068] "Sulfonyl" is -S(O)2A 1 It means, and here A 1 As described in this specification, it may be hydrogen, alkyl, halogenated alkyl, alkenyl, alkynyl, aryl, heteroaryl, cycloalkyl, cycloalkenyl, heterocycloalkyl, or heterocycloalkenyl group.

[0069] "Tio" means -S-.

[0070] "Thiol" means -SH group.

[0071] As used herein, the term “about” means + / - 10% of any mentioned value. As used herein, this term modifies any mentioned value, a range of values, or the endpoints of one or more ranges.

[0072] As used herein, the terms "top," "bottom," "upper," "lower," "above," and "below" are used to provide relative relationships between structures. The use of these terms does not indicate or require that a particular structure be located at a specific position on the device.

[0073] Reference to specific embodiments of the present disclosure is made in detail in this specification. Examples of specific embodiments are illustrated in the accompanying drawings. While the present disclosure will be described together with these specific embodiments, it will be understood that this is not intended to limit the present disclosure to these specific embodiments. On the contrary, it is intended to cover alternatives, modifications, and equivalents as may be included within the spirit and scope of the present disclosure. In the following description, numerous specific details are presented to provide a complete understanding of the present disclosure. The present disclosure may be practiced without some or all of these specific details. In other examples, known process operations have not been described in detail so as not to unnecessarily obscure the present disclosure.

[0074] Other features and advantages of the present invention will become apparent from the following description and claims. Brief explanation of the drawing

[0075] FIGS. 1a and 1b illustrate flowcharts having specific operations in examples of semiconductor manufacturing processes using SRP (stimulus response polymer). (A) a method (100) of employing SRP layers (118, 128) to form a bonded assembly (130); and (B) a bonding operation comprising removing the SRP and contacting the exposed features to form a bonded assembly (130). FIGS. 2a and 2b illustrate flowcharts having different specific operations. (A) a method of employing thin layers (218, 228) of SRP and (B) another method of employing thick layers (248, 258) of SRP are provided. FIG. 3 illustrates a flowchart having other specific operations. A method of employing a metal feature (314) surrounded by a gap-filling material (315) is provided. FIGS. 4a through 4d illustrate process flow diagrams for non-limiting methods using SRP during the process of forming metal-metal bonds. Figure 5 illustrates a process flowchart for another non-limiting method of using SRP during the process of forming metal-metal bonds. Figure 6 illustrates a process flowchart for another non-limiting method of using SRP during the process of forming metal-metal bonds. FIG. 7 is a functional block diagram of an example of an electroplating cell according to the present disclosure. FIG. 8 is a functional block diagram of an example of an electrodeposition device according to the present disclosure. FIG. 9 is a functional block diagram of an example of another electrodeposition device according to the present disclosure. FIG. 10 is a functional block diagram of an example of an electroplating apparatus according to the present disclosure. FIG. 11 is a functional block diagram of an example of a substrate processing system including a plurality of substrate processing tools and a storage buffer according to the present disclosure. FIG. 12 illustrates a schematic cross-sectional view of an example of a dry deposition apparatus for depositing SRP according to the present disclosure. FIG. 13 shows a detailed side view and a top view of a portion of the top plate, substrate, and edge ring. FIG. 14 is a plan view of an example of a wet deposition apparatus for depositing SRP according to the present disclosure. FIG. 15 is a cross-sectional view along line III-III of FIG. 14. Fig. 16 is an enlarged view of Detail IV of Fig. 15. FIG. 17 is a plan view of a heating assembly of an example of a wet deposition apparatus. FIG. 18 illustrates another example of a wet deposition apparatus for depositing SRP according to the present disclosure. FIG. 19 illustrates an embodiment of FIG. 18 of the loading position and unloading position. Specific details for implementing the invention

[0076] Stimuli-responsive polymers (SRPs) may be used in semiconductor manufacturing processes as temporary or sacrificial layers that can be removed later. Low ceiling temperature SRPs can be naturally removed when exposed to stimuli such as slightly elevated temperatures or acidic vapors, and prevent aggressive wet or dry removal chemicals that could damage the substrate surface. Other processes for removing SRPs are described herein. In specific embodiments, these SRPs can result in residue-free removal, thereby providing a clean surface amenable for forming metal-to-metal bonds.

[0077] Capping processes are described herein in which an SRP is deposited on a metal feature (e.g., a plated metal feature) to serve as a protective layer. This temporary layer prevents oxide from forming on the feature when the wafer is queued and transferred to a thermal press bonding tool. Once it enters the chamber of the thermal press bonding tool, the temperature is ramped to a removal temperature (e.g., below 250°C) to volatilize or bake off the capping material. Subsequently, the metal features are aligned and brought into contact for high-quality bonding. Thus, what is described herein are also bonding processes in which the SRP is removed to form a metal-to-metal bond.

[0078] When in use, sacrificial films can provide Q-time extension. In one example, the SRP film may be a thin or thick sacrificial polymer layer configured to protect sensitive metal features during substrate transfer and feature alignment or for extended periods prior to thermal compression bonding. Sacrificial surface protection layers can eventually be removed by using appropriate stimuli (e.g., acidic, thermal, and / or electromagnetic) to induce spontaneous depolymerization and vaporization of the protection layer above ceiling temperatures, thereby minimizing the impact on sensitive surfaces. These surfaces may include surfaces susceptible to atmospheric Q-time effects or prone to unwanted oxidation, corrosion, and / or halogenation. Examples of such surfaces include, but are not limited to, copper (Cu), tin (Sn), tin-silver (SnAg), silver (Ag), gold (Au), aluminum (Al), silicon (Si), silicon / germanium (Si / Ge), tungsten (W), cobalt (Co), ruthenium (Ru), molybdenum (Mo), and titanium nitride (TiN).

[0079] Referring to FIG. 1a, an example of a method (100) for protecting a metal feature is illustrated. First, a substrate (116) comprising a metal feature (114) is provided. The feature may be a pillar (e.g., a raised metal pillar), a bonding pad, a bump, a microbump, a metal contact surrounded by a dielectric, or an electrical contact such as an interconnect. In the next operation (101), an SRP is deposited on the surface of the metal feature (114) to form an SRP layer (118). The SRP may be deposited in a vapor phase (e.g., with a carrier gas) or in a liquid phase (e.g., with a solvent or as a formulation). When using solvent-based deposition, the SRP may be selectively dried or solidified by removing the liquid portion, thereby forming a layer or film.

[0080] SRP is the thermodynamically unstable low ceiling temperature (T c It may be a polymer (e.g., a homopolymer or copolymer). T c T is the temperature at which the polymer and its monomers exist in equilibrium. c In the following, it is a polymer, and T c In the above, it is a monomer. Low T c Polymers have excellent storage life T c It can be kinetically trapped at much higher temperatures. For example, poly(phthalaldehyde) (PPHA) at -40 °C T c It has [unclear] but is stable for 2.5 years at room temperature. Stability is achieved by kinetically inhibiting the depolymerization mechanism. Additional SRPs, as well as formulations thereof, are described herein.

[0081] SRP can be deposited in any useful way. Low T cThe volatile polymer capping layer may be formulated with only a spin coating solvent, dry-deposited from the vapor phase, or formulated with a spin coating solvent and a weak acid to lower the degradation temperature. Devices such as tape coaters (doctor blades) may be used to coat thick films (e.g., greater than 1 μm) with some modification of the formulation.

[0082] For wet deposition, the choice of solvent used in the spin coating formulation can affect the amount of residual solvent remaining in the polymer layer or film. Residual solvent can plasticize the polymer, thereby lowering the glass transition temperature. By plasticizing the polymers, the relief of stresses from the spin coating process and the filling of features can be achieved at temperatures below the polymer's degradation temperature. These features may include high-density features (e.g., having a pitch of less than about 20 μm between features), high aspect ratio features (e.g., high aspect ratios (ARs) such as at least 8, 10, 20, 30, 40, or 80), and / or thick features (e.g., having a thickness of about 30 μm to 50 μm).

[0083] Furthermore, SRP can be formulated using acid catalysts such as weak organic acids (e.g., pKa ≥ 1). These weak organic acids can accelerate the degradation of SRP without impairing membrane stability. By accelerating polymer degradation, the onset degradation temperature can be lowered, and the degradation rate can be increased.

[0084] SRP can be deposited as a uniform or non-uniform layer on the feature. In addition, the thickness of the SRP layer can be about 10 nm to 10 µm. Depending on the dimensions of the feature, the SRP layer can provide conformal or non-conformal step coverage or planar coverage. If vias or openings are present, the SRP layer can be used to fill these openings.

[0085] Referring again to FIG. 1a, after SRP deposition, a capped feature (110) is formed. The capped feature may include an SRP layer (118) disposed on any exposed surface of a metal feature (114). In some examples, the metal feature may be surrounded by another material (e.g., a dielectric material or a gap-filling material), and the SRP layer is disposed on the exposed top surface of the feature. In other examples, the metal feature may be a pillar having an exposed top surface and a side surface, and the SRP layer is disposed on these surfaces or a part thereof. The capped feature may be employed immediately, as well as stored or queued before further processing.

[0086] Further processing may include a step (102) of aligning the first capped feature (110) with the second capped feature (120), which may ultimately include an SRP layer (128) disposed on the surface of the second metal feature (124) on the substrate (126). The second capped feature may be formed by using any of the SRP deposition processes of this specification. Alignment may include aligning the top surfaces of the first metal feature and the second metal feature vertically and / or horizontally. In FIG. 1a, the top surface of the first feature (114) is distal with respect to the substrate (116), and the top surface of the second feature (124) is distal with respect to the substrate (126).

[0087] In operation (103), features (114, 124) may undergo metal-to-metal bonding to form a metal structure (134) within a bonded assembly (130). In some non-limiting embodiments, the bonded assembly does not contain solder. In other embodiments, the bonded assembly includes direct metal-to-metal bonding. In yet another embodiment, the metal structure provides a reduction in interconnect wire length, which can improve performance and reduce power consumption. These bonded assemblies may exist in any useful stack, device, substrate, vertically integrated architecture, multilayer integrated architecture, or high-pitch density circuit. For example, direct metal-to-metal bonding may enable a tighter pitch (e.g., packed more densely in the xy direction, with axes parallel to the plane of the substrate) and / or shorter connection height or length (e.g., in the z direction, where the axes are orthogonal to the plane of the substrate).

[0088] Bonding may include a removal step of removing SRP layers (118, 128) thereby providing exposed features; and a step of contacting the exposed features to form a metal-to-metal bond. Conditions for removing the SRP may include exposure to a removal temperature at which the degraded SRP is volatile, and conditions for bonding may include exposure to a bonding temperature at which metal-to-metal bonds are formed. When the removal temperature and the bonding temperature are similar, one continuous operation may be performed at the temperature condition for removing the SRP and from the metal-to-metal bond. Alternatively, removal and contact may be performed as discrete operations. Non-limiting removal temperatures include about 50 °C to about 250 °C, e.g., about 50 °C to 150 °C; non-limiting bonding temperatures include about 25 °C to about 250 °C, e.g., about 100 °C to 250 °C.

[0089] As can be further seen in FIG. 1b, the operation (103a) comprises the step of removing SRP from a first capped feature (110) and a second capped feature (120), thereby providing a first exposed metal feature (114) and a second exposed metal feature (124). The capped features may be exposed to a stimulus to degrade all or only part of the SRP. Volatile monomers or fragments from the degraded polymer may be removed (e.g., by purging the chamber). The stimulus may be any stimulus that cuts the bonds of the SRP to degrade the SRP.

[0090] Controlled SRP degradation may involve depolymerization that can be promoted by the presence of acid. This catalytic action may be promoted by formulating SRP using an acid (e.g., a weak organic acid, a photoacid generator, or a thermal acid generator). In other embodiments, SRP removal may be performed in the presence of an acidic vapor (e.g., formic acid, acetic acid, citric acid, etc. as described herein) to promote a breakdown reaction. The use of acid can not only promote degradation at lower temperatures (e.g., below 100°C) but also incidentally remove metal oxides formed on metal features. Other removal methods include the use of thermal, extreme ultraviolet (EUV), ultraviolet (UV), or vacuum UV, which may be combined with acidic vapor as described herein. In other embodiments, SRP removal may involve the use of heat along with another stimulus, such as UV exposure or acid vapor exposure.

[0091] Referring again to FIG. 1b, the operation (103b) comprises contacting exposed features to provide a metal structure (134) bonded within the assembly (130). In specific embodiments, the bonding process is low T to enable high-integrity metal-to-metal direct bonding at low temperatures (e.g., less than 250 °C) and to prevent oxide formation. c Volatile SRPs are used. In some embodiments, the temporary capping layer is cleanly evaporated from the surface at low temperatures (e.g., about 50°C to 250°C) to treat oxide formation while enabling metal-to-metal bonding at low temperatures (e.g., 250°C or lower). Such contacts may include thermal compression bonding in which heat and pressure are applied to metal features to allow atomic interdiffusion and grain growth at the metal-to-metal interface.

[0092] SRP removal and thermal compression can be performed in any traditional thermal compression tool or chamber using an inert atmosphere (e.g., oxygen-free), vacuum, reducing gas, or ambient air (e.g., containing oxygen). Depending on the conditions, the cue time can be controlled and minimized to prevent oxide formation. For example, if the ambient air contains oxygen, bonding can lead directly to the volatilization of the capping layer. Otherwise, oxide may eventually form on the feature surfaces.

[0093] The processes of this specification include any useful combination of operations for forming features, depositing SRP layers, and bonding exposed features. As can be seen in FIG. 2a, a non-limiting process may include applying a temporary capping layer to a device having plated metal features. Initially, the stack may include a substrate (216), a seed layer or barrier layer (211) disposed on the surface of the substrate, and a patterned photoresist (212) having an opening (213) defined within and disposed on the surface of the seed / barrier layer. In operation (201), a plated metal pillar (213a) is formed within the opening (213). Next, in operation (202), the photoresist is stripped to provide a released metal pillar (213b). Operation (203) includes etching away the seed / barrier layer to provide a freestanding or isolated metal feature (214). Optionally, operation (204) may be performed to clean the surface of the metal feature using a wet cleaning process or a plasma treatment process. This cleaning step may be performed immediately before depositing the SRP layer, thus ensuring a clean, oxide-free surface before capping.

[0094] In operation (205), an SRP layer (218) is deposited on exposed surfaces that may include the top surface and / or sidewalls of the metal feature (214) and, optionally, the surface of the substrate (216). Thus, a first capped feature (210) is formed. In a similar manner, a second capped feature (220) may be formed. Although the first capped feature and the second capped feature are shown to have similar geometry in FIG. 2a, each feature may be the same or different. In one non-limiting example, the first capped feature may be a pillar and the second capped feature may be a contact pad. In other embodiments, both the first capped feature and the second capped feature may be pillars having similar or different dimensions.

[0095] In operation (206), the first capped feature (210) is aligned with the second capped feature (220), which includes a substrate (226), a second metal feature (224), and an SRP layer (228). Subsequently, in operation (207), the first feature and the second feature are bonded together to form a metal structure (234) within a bonded assembly (230). As described herein, this bonding may include a series of separate operations to remove the SRP layers (218, 228) and to contact the exposed features (214, 224) to form a metal-to-metal bond. Furthermore, the capping material does not need to be completely removed or evaporated as long as a sufficient amount is removed from the bonding surfaces of the features to allow for low-temperature bonding. In some examples, the capping material may be retained within the stack or assembly after bonding the features.

[0096] The capping material does not need to be applied uniformly to the surface of the feature and / or substrate. As can be seen in FIG. 2b, the first capped feature (240) may include a non-uniform SRP layer (248) having variable thicknesses in proximity to the metal feature (214). This non-uniformity may result from the dimensions, aspect ratio, pitch density, surface chemistry, or material composition at the deposition surface. Capped features having uniform or non-uniform SRP layers are covered by the present disclosure.

[0097] Referring again to FIG. 2b, in operation (206), the first capped feature (240) can be aligned with the second capped feature (250) having a non-uniform SRP layer (258), a metal feature (254), and a substrate (256). As can be seen in operation (207), the bonding provides a metal structure (264) within the bonded assembly (260).

[0098] Metal-to-metal bonds can be formed between features provided in any useful device. In some examples, the device includes freestanding or isolated metal features, such as pillars. However, in other examples, these features may be embedded within layers, and only the bonding surface is accessible on the surface of the device.

[0099] As illustrated in FIG. 3, a non-limiting process may include applying a temporary capping layer to a device having a gap-filling material surrounding a plated metal feature. Initially, the stack may include a substrate (316), a seed layer or barrier layer (311), and a patterned photoresist (312) having a defined opening (313) inside. In operation (301), a plated metal pillar (313a) is formed within the opening (313). Next, in operation (302), the photoresist is stripped to provide an emitted metal pillar (313b). Operation (303) includes etching the seed / barrier layer to provide a freestanding or isolated metal feature (314).

[0100] Operation (304) involves depositing gap-filling material around the metal feature (314), which may cause incidental deposition on the metal surface. Accordingly, operation (305) etch-back cleans the stack, which etches away a portion of the gap-filling layer and cleans the metal surface before capping. This etch-back clean may involve the use of reducing chemicals, for example, ammonia or a combination of nitrogen (N2) and hydrogen (H2) gases. Next, in operation 306, an SRP layer (318) is deposited on the exposed surfaces, which may include the surface of the metal feature (314) and the surface of the gap-filling layer (315). Thus, a first capped feature (310) is formed. In a similar manner, a second capped feature (320) having a second SRP layer (328), a second metal feature (324), a gap-filling layer (325), and a second substrate (326) can be formed.

[0101] In operation (307), the first capped feature (310) is aligned with the second capped feature (320). Alignment may include arranging the top surfaces of each capped feature so that vertical compression provides contact between the surfaces and creates a metal-to-metal bond. Subsequently, in operation (308), the first feature and the second feature are bonded together to form a metal structure (334) within the bonded assembly (330). As described herein, this bonding may include a series of separate operations to remove the SRP layers (318, 328) and bring the exposed features (314, 324) into contact to form a metal-to-metal bond. In some examples, the removal of the SRP involves only exposing the surface of the metal feature so that only a portion of the SRP layer is removed.

[0102] The present disclosure generally covers the use of SRP having metal features such as electrical contacts. One non-limiting method includes the step of forming an SRP layer on a first metal feature, and the step of forming the SRP layer may include providing a first capped feature. As can be seen in FIG. 4a, one example of the method (400) includes the action (401) of providing a substrate having one or more metal features (e.g., electrical contact(s)) and the action (405) of depositing the SRP on the surface of the metal feature(s) to form the SRP and thereby provide a capped feature. This method may optionally include the action (403) of pretreating the surface of the metal feature before depositing the SRP, and such pretreatment may include a wet cleaning process or a plasma process (e.g., a non-thermal plasma process). The methods of this specification may include one or more pre-bonding operations (e.g., before SRP deposition), such as cleaning metal features, isolating metal features by depositing dielectric or gap-filling materials, and recessing one or more non-metallic layers.

[0103] Another non-limiting method may include aligning capped features having an SRP layer. As can be seen in FIG. 4b, one example of the method (420) includes an action (407) of aligning a first capped feature and a second capped feature, wherein each capped feature comprises an SRP layer disposed on the surface of a metal feature; and an action (409) of bonding the first capped feature and the second capped feature in an atmosphere that removes the SRP and forms a metal-metal bond between the metal features. Such an atmosphere may have any removal temperature or bonding temperature described herein. Furthermore, the exposed features may be contacted at a contact pressure that facilitates metal-metal bond formation, such as a pressure of about 0.2 MPa to about 1 MPa or about 0.7 MPa (about 100 psi). The methods of this specification may include one or more post-bonding operations, such as annealing of a metal structure within a bonded assembly, wafer thinning, or other backside processing.

[0104] Other methods may include SRP deposition, alignment of capped features, and bonding. As can be seen in FIG. 4c, an example of the method (440) includes: an action (401) of providing a substrate comprising one or more metal features; an optional action (403) of pre-treating the surface of the metal feature(s) to provide a clean surface and / or an oxide-free surface; an action (405) of providing a first capped feature by depositing SRP on the surface of the metal feature(s); an action (407) of aligning the first capped feature with a second capped feature having an SRP layer disposed on the surface of the metal feature; and an action (409) of removing the SRP and bonding the first capped feature with the second capped feature in an atmosphere to form a metal-metal bond between the metal features.

[0105] Bonding may include individual steps if desired. As illustrated in FIG. 4d, the method (460) includes an action (409a) of removing SRP by exposing to a removal temperature to volatilize the SRP and / or exposing to an acidic vapor to facilitate SRP removal, and an action (409b) of contacting the exposed features to provide a metal-to-metal bond. Such contact may be performed at any bonding temperature and / or contact pressure described herein.

[0106] The processes of this specification may include additional operations for forming a stack prior to SRP deposition. As can be seen in FIG. 5, an example of method (500) includes: an operation (501) of forming one or more openings in a resist layer that may be optionally disposed on a seed layer or a barrier layer; an operation (503) of plating or depositing metal in the opening(s) to provide one or more metal features; an operation (503) of stripping the resist layer to release the metal feature(s); an operation (504) of etching the seed / barrier layer to provide freestanding or electrically isolated metal feature(s); an operation (505) of depositing a first capped feature by depositing SRP on the surface of the metal feature(s); and an operation (507) of aligning the first capped feature with a second capped feature having an SRP layer disposed on the surface of the metal feature. It may include an operation (509) of bonding the first capped feature and the second capped feature in an atmosphere that removes SRP and forms a metal-metal bond between the metal features.

[0107] The stack may include additional materials used with metal features, and the methods of this specification may include operations for depositing such materials. As can be seen in FIG. 6, an example of method (600) includes the operation (601) of providing a substrate comprising one or more metal features; the operation (603) of depositing a gap-filling material around the metal feature(s) to electrically insulate the features (604); the operation (604) of etching back-cleaning the surface of the gap-filling material and the surface of the metal feature(s); the operation (605) of depositing SRP on the cleaned surface of the metal feature(s) to provide a first capped feature; and the operation (607) of aligning the first capped feature with a second capped feature having an SRP layer disposed on the surface of the metal feature. It may include an operation (609) of bonding the first capped feature and the second capped feature in an atmosphere that removes SRP and forms a metal-metal bond between the metal features.

[0108] Metal features and substrates

[0109] The SRPs and methods of this specification may be used with metal features and associated structures. These metal features may exhibit oxide formation during exposure to air, and such interfacial oxide layers must be prevented when forming metal-metal bonds. Accordingly, in one embodiment, the SRPs of this specification may be employed to reduce the oxidation of these metal features.

[0110] SRP may be placed on any useful feature, substrate, or surface. The surface may be a planar surface or may include one or more electrical contacts, pillars, bonding pads, bumps, microbumps, interconnects, vias, holes, gaps, and trenches. However, other surfaces may include surfaces on devices such as electronic components, printed circuit boards, packages, etc. Examples of substrate surfaces include silicon, silicon germanium, and germanium structures, metal surfaces including but not limited to copper, cobalt, titanium, titanium nitride, tungsten, ruthenium, or molybdenum, and / or other structures and materials. In particular, metal features may include conductive metals, transition metals, as well as alloys or doped forms thereof.

[0111] Deposition of SRPs

[0112] In many embodiments, SRPs are low ceiling temperatures (T c ) They are polymers. T c is the equilibrium temperature between the polymer and the monomers of the polymer. As used herein, the term "low T" c T below the removal temperature c Refers to values. In some embodiments, T c is below room temperature, so that the polymers are thermodynamically unstable at room temperature. Instead, low T c Polymers are kinetically trapped to allow for prolonged storage at room temperature. In some examples, the stable storage period is approximately several months or years. Low T cPolymers will rapidly depolymerize into their monomer constituents when terminal groups or main chain bonds are broken. Thus, polymers depolymerize in response to stimuli such as acidic catalysts, basic catalysts, extreme ultraviolet (EUV) light, ultraviolet (UV) light, heat, thermal catalysts, and / or photocatalysts. The monomer products are volatile and can remain on the surface and chamber or be easily removed.

[0113] In some embodiments, T c Although it is below room temperature, in the context of semiconductor processing, low T c It may also refer to ceiling temperatures higher than room temperature. For example, removal temperatures of up to 400°C may be used, which means that the ceiling temperature is 400°C or lower.

[0114] In some embodiments, the SRP may comprise one or more metal-bonding moietyes. The metal-bonding moiety may facilitate the binding or adhesion of the SRP layer to a metal feature. In addition, these moietyes may be present within a specific number or percentage of monomers in the polymer. In other embodiments, the SRP may be a copolymer in which one of the monomers comprises at least one metal-bonding moiety.

[0115] Non-limiting metal-bonding moietyes may include one or more of the following: as defined herein, optionally substituted heterocyclil, optionally substituted heterocyclyloxy, optionally substituted heterocyclilloyl, thiol (-SH), optionally substituted amino (e.g., -NH2 or -NR N1 R N2 ), optionally substituted aminoalkyl (e.g., -Ak-NH2 or -Ak-NR N1 R N2), carboxyl (-CO2H), optionally substituted carboxyalkyl (e.g., -Ak-CO2H), hydroxyl (-OH), and / or optionally substituted hydroxyalkyl (e.g., -Ak-OH), where Ak is optionally substituted alkylene, and R N1 and R N2 Each is independently H, optionally substituted alkyl, or optionally substituted aryl, or R N1 and R N2 Each is taken together with an attached nitrogen atom to form a heterocyclyl group. In specific embodiments, the optionally substituted heterocyclile comprises an optionally substituted azole group, such as optionally substituted imidazolyl, isoxazolil, isothiazolyl, oxadiazolil (e.g., 1,2,3-oxadiazolil, 1,2,4-oxadiazolil, 1,2,5-oxadiazolil, or 1,3,4-oxadiazolil), oxazolil, pyrazolil, tetrazolyl, thiadiazolyl (e.g., 1,2,3-thiadiazolyl, 1,2,4-thiadiazolyl, 1,2,5-thiadiazolyl, or 1,3,4-thiadiazolyl), thiazolyl, triazolil (e.g., 1,2,3-triazolil or 1,2,4-triazolil), or any heterocyclile described herein.

[0116] In other embodiments, the metal-bonding moiety is a multidentate (e.g., two-dentate, four-dentate, or eight-dentate) ligand. Non-limiting multidentate ligands are R 1 -L 1 -R 2 Includes, where L 1 is an optionally substituted alkylene, an optionally substituted heteroalkylene, an optionally substituted arylene, or an optionally substituted heterocyclyldiyl; R 1 and R 2 Each independently comprises a thiol, an optionally substituted amino, carboxyl, or hydroxyl. In some embodiments, R1 and R 2 Each independently, -L 2 -R 3 Igo; L 2 is a covalent bond, optionally substituted alkylene, or optionally substituted heteroalkylene; R 3 is independently a thiol, optionally substituted amino, carboxyl, or hydroxyl.

[0117] Another non-restrictive multidentate ligand is R 1 -L 1 -R 2 Includes, where L 1 is an optionally substituted alkylene; R 1 and R 2 Each independently comprises a selectively substituted heterocycline (e.g., a selectively substituted azole). In other embodiments, the metal-bonding moiety is a Schiff base ligand. Other metal-bonding moietys include imidazolyl, pyrazolyl, triazolyl, thiol, nitrile, 3,4-dihydroxyphenylalanine (DOPA), histidine, ethylenediamine, 1,4,7,10-tetraazcyclododecane-1,4,7,10-tetraacetic acid (DOTA), as well as derivatives thereof.

[0118] Examples of SRPs are provided below. However, the methods described herein may be used with any SRPs. In some embodiments, the SRPs are homopolymers or copolymers comprising poly(aldehydes). In certain embodiments, they may be self-immolative polymers as described in U.S. Patent Publication No. 2018 / 0155483, published June 7, 2018, and incorporated herein by reference in its entirety.

[0119] SRPs may be any suitable polymer of linear or cyclic form (e.g., homopolymer or copolymer). Non-limiting SRPs include poly(phthalaldehyde), poly(aldehyde), poly(benzyl carbamate), poly(benzyl ether), poly(alpha-methyl styrene), poly(carbonate), poly(norbornene), poly(olefin sulfone), poly(glyoxylate), poly(glyoxyamide), poly(ester), or poly(methyl methacrylate), as well as derivatives thereof. These derivatives may include the replacement of the oxy (-O-) group with an optionally substituted heteroalkylene as defined herein, as well as substitution with one or more substituents as described herein for the alkyl group.

[0120] Other SRPs have chemical formulas ( I )-( XV ), chemical formula ( Ia ), chemical formula ( Ib ), or chemical formula ( IcIt may include those having one of the structures. These SRPs may be linear polymers or cyclic polymers. If linear, the polymer may include all useful end groups that terminate the molecule. These end groups may be dependent on reactive end groups present on the monomers employed to synthesize the polymer. In specific embodiments, the end groups may include fragments formed from the use of an acylation reagent or an alkylation reagent, from the use of an anionic initiator (e.g., fragments such as alkyl anions, e.g., n-BuLi, s-BuLi, etc.), (e.g., fragments such as acyl or optionally substituted alkanoyl, e.g., formyl, acetyl, benzoyl, methyl, ethyl, etc.), from the use of a conjugated alkylene monomer (e.g., quinone methide monomer), or from the use of an alcohol terminator (e.g., fragments such as optionally substituted alkoxy). The terminal groups may include any useful linking or reactive groups (e.g., those including optionally substituted trialkylsiloxy, optionally substituted alkenyl, optionally substituted aryl, etc.).

[0121] SRP may include poly(phthalaldehyde) or a derivative thereof, which may be a linear or cyclic polymer. In one embodiment, SRP has the formula ( I The structure of ) or a salt thereof, or containing it,

[0122]

[0123] Each R1 is independently H, optionally substituted alkyl, optionally substituted alkoxy, optionally substituted alkenyl, optionally substituted aryl, or halo;

[0124] R 2' and R 2"Each is independently H, an optionally substituted alkyl, an optionally substituted heteroalkyl, or an optionally substituted aryl;

[0125] Z1 and Z2 are each independently -O-, -S-, or optionally substituted heteroalkylenes;

[0126] r1 is an integer from 1 to 4; and

[0127] n is approximately 2 to approximately 100,000.

[0128] (e.g., chemical formula ( I In specific embodiments of ), R 2' and R 2'' Each is independently H or an optionally substituted alkyl. In some embodiments, Z1 and Z2 are each -O-. In other embodiments, R1, R 2' , or R 2'' At least one of them includes a metal-bonded moiety (e.g., any moiety described herein).

[0129] SRP may include a poly(aldehyde) or a derivative thereof, which may be a linear or cyclic polymer. In one embodiment, SRP has the formula ( II The structure of ) or a salt thereof, or containing it,

[0130]

[0131] R2 and R3 are each independently H, optionally substituted alkyl, optionally substituted heteroalkyl, or optionally substituted aryl;

[0132] Z1 is -O-, -S-, or optionally substituted heteroalkylene; and

[0133] n is approximately 2 to approximately 100,000.

[0134] In some embodiments, at least one of R2 or R3 comprises a metal-bonding moiety (e.g., as described herein).

[0135] SRP may include poly(benzyl carbamate) or a derivative thereof, which may be a linear or cyclic polymer. In one embodiment, SRP has the formula ( III The structure of ) or a salt thereof, or containing it,

[0136]

[0137] Each R1 is independently H, optionally substituted alkyl, optionally substituted alkoxy, optionally substituted alkenyl, optionally substituted aryl, or halo;

[0138] R2 and R3 are each independently H, optionally substituted alkyl, optionally substituted heteroalkyl, or optionally substituted aryl;

[0139] R4 is H or optionally substituted alkyl;

[0140] Z1 is -O-, -S-, or optionally substituted heteroalkylene;

[0141] r1 is an integer from 1 to 4; and

[0142] n is approximately 2 to approximately 100,000.

[0143] (e.g., chemical formula ( IIIIn specific embodiments of ), R1 is optionally a substituted alkoxy. In other embodiments, n is about 2 to about 100 (e.g., about 2 to 10, 2 to 15, 2 to 20, 2 to 25, 2 to 30, 2 to 40, 2 to 50, 2 to 75, 4 to 10, 4 to 15, 4 to 20, 4 to 25, 4 to 30, 4 to 40, 4 to 50, 4 to 75, and 4 to 100). In other embodiments, at least one of R1, R2, R3, or R4 comprises a metal-bonding moiety (e.g., any moiety described herein).

[0144] SRP may comprise poly(benzyl ether) or a derivative thereof, which may be a linear or cyclic polymer. In one embodiment, SRP is of the formula ( IV The structure of ) or a salt thereof, or containing it,

[0145]

[0146] Each R1 is independently H, optionally substituted alkyl, optionally substituted alkoxy, optionally substituted alkenyl, optionally substituted aryl, or halo;

[0147] R2 and R3 are each independently H, optionally substituted alkyl, optionally substituted heteroalkyl, or optionally substituted aryl;

[0148] R4 is H or optionally substituted alkyl;

[0149] Z1 is -O-, -S-, or optionally substituted heteroalkylene;

[0150] r1 is an integer from 1 to 4; and

[0151] n is approximately 2 to approximately 100,000.

[0152] (e.g., chemical formula ( IIIIn specific embodiments of ), R1 is optionally a substituted alkoxy. In other embodiments, n is about 2 to about 100 (e.g., about 2 to 10, 2 to 15, 2 to 20, 2 to 25, 2 to 30, 2 to 40, 2 to 50, 2 to 75, 4 to 10, 4 to 15, 4 to 20, 4 to 25, 4 to 30, 4 to 40, 4 to 50, 4 to 75, and 4 to 100). In other embodiments, at least one of R1, R2, R3, or R4 comprises a metal-bonding moiety (e.g., any moiety described herein).

[0153] SRP may comprise poly(benzyl ether) or a derivative thereof, which may be a linear or cyclic polymer. In one embodiment, SRP is of the formula ( IV The structure of ) or a salt thereof, or containing it,

[0154]

[0155] Each R1 is independently H, optionally substituted alkyl, optionally substituted alkoxy, optionally substituted alkenyl, optionally substituted aryl, or halo;

[0156] R2 and R3 are each independently H, optionally substituted alkyl, optionally substituted heteroalkyl, or optionally substituted aryl;

[0157] R 4' and R 4'' Each is independently H or optionally substituted alkyl;

[0158] L1 is an optionally substituted alkylene, an optionally substituted heteroalkylene, an optionally substituted arylene, or an optionally substituted cycloalkylene;

[0159] Z1 and Z2 are each independently -O-, -S-, or optionally substituted heteroalkylenes;

[0160] r1 is an integer from 1 to 4; and

[0161] n is approximately 2 to approximately 100,000.

[0162] (e.g., chemical formula ( V In specific embodiments of ), R1 is an optionally substituted alkyl. In other embodiments, Ar is an optionally substituted phenyl. In other embodiments, n is about 2 to about 5000. (e.g., chemical formula ( V In other embodiments of ), R 4' and R 4'' Each is independently, optionally substituted alkyl. In some embodiments, L1 is optionally substituted alkylene. In other embodiments, Z1 and Z2 are -O-. In other embodiments, R1, R2, R3, R 4' , or R 4'' At least one of them includes a metal-bonded moiety (e.g., any moiety described herein).

[0163] SRP may include a poly(dicarbamate) or a derivative thereof, which may be a linear or cyclic polymer. In one embodiment, SRP has the chemical formula ( VI The structure of ) or a salt thereof, or containing it,

[0164]

[0165] R 4' and R 4'' Each is independently H or optionally substituted alkyl;

[0166] L1 and L2 are each independently optionally substituted alkylene, optionally substituted heteroalkylene, optionally substituted arylene, or optionally substituted cycloalkylene; L2 may optionally be a covalent bond;

[0167] Z1 and Z2 are each independently -O-, -S-, or optionally substituted heteroalkylenes; and

[0168] n is approximately 2 to approximately 100,000.

[0169] (e.g., chemical formula ( VI In specific embodiments of ), R 4' and R 4'' Each is independently, optionally, a substituted alkyl. In some embodiments, L1 and L2 are independently, optionally, a substituted alkylene. In other embodiments, Z1 and Z2 are independently -O- or -S-. In yet other embodiments, Z1 and Z2 are -O-. In other embodiments, L1, L2, R 4' , or R 4'' At least one of them includes a metal-bonded moiety (e.g., any moiety described herein).

[0170] SRP may comprise poly(alpha-methyl styrene) or a derivative thereof, which may be a linear or cyclic polymer. In one embodiment, SRP is of the formula ( VII The structure of ) or a salt thereof, or containing it,

[0171]

[0172] R 2' , R 2" , and R3 are each independently H, optionally substituted alkyl, optionally substituted heteroalkyl, or optionally substituted aryl;

[0173] Ar is an optionally substituted aryl, an optionally substituted alkyl, or an optionally substituted aralkyl; and

[0174] n is approximately 2 to approximately 100,000.

[0175] In other embodiments, Ar, R 2' , R 2'', or at least one of R3 comprises a metal-bonded moiety (e.g., any moiety described herein).

[0176] SRP may include poly(carbonate) or a derivative thereof, which may be a linear or cyclic polymer. In one embodiment, SRP has the chemical formula ( VIII The structure of ) or a salt thereof, or containing it,

[0177]

[0178] L1 is an optionally substituted alkylene, an optionally substituted heteroalkylene, an optionally substituted arylene, or an optionally substituted cycloalkylene; and

[0179] n is approximately 2 to approximately 100,000.

[0180] (e.g., chemical formula ( VIII In specific embodiments of ), L1 is optionally substituted alkylene, optionally substituted heteroalkylene, or optionally substituted cycloalkylene; in some embodiments, the optionally substituted heteroalkylene is -X-Ak-X-, where X is oxy and Ak is optionally substituted alkylene. In other embodiments, L1 comprises a metal-bonded moiety (e.g., any moiety described herein). Non-limiting SRPs may include poly(ethylene carbonate), poly(propylene carbonate) (PPC), poly(butylene carbonate) (PBC), poly(cyclohexene carbonate) (PCHC), poly(norbornene carbonate) (PNC), and poly(cyclohexene propylene carbonate) (PCPC).

[0181] SRP may include poly(norbornene) or a derivative thereof, which may be a linear or cyclic polymer. In one embodiment, SRP is of the formula ( IX The structure of ) or a salt thereof, or containing it,

[0182]

[0183] R3 is H, optionally substituted alkyl, optionally substituted heteroalkyl, or optionally substituted aryl; and

[0184] n is approximately 2 to approximately 100,000.

[0185] In other embodiments, R3 includes a metal-bonded moiety (e.g., any moiety described herein).

[0186] SRP may include a poly(olefin sulfone) or a derivative thereof, which may be a linear or cyclic polymer. In one embodiment, SRP has the chemical formula ( X The structure of ) or a salt thereof, or containing it,

[0187]

[0188] R3 is H, optionally substituted alkyl, optionally substituted heteroalkyl, or optionally substituted aryl; and

[0189] n is approximately 2 to approximately 100,000.

[0190] (e.g., chemical formula ( X In specific embodiments of ), R3 is, for example, -OC(O)-R O1 , -NR N1 -C(O)-R O1 , -OC(O)NR N1 R N2 , -(Ak-O) h1 R O1 or -Ak-NR N1 R N2 It is an optionally substituted heteroalkyl such as, where Ak is an optionally substituted alkylene, h1 is 1 to 5, and R O1 , R N1 and R N2Each is independently H or an optionally substituted alkyl (e.g., hydroxyalkyl, carboxyalkyl, aminoalkyl, or azidoalkyl). In other embodiments, R3 comprises a metal-bonding moiety (e.g., any moiety described herein).

[0191] SRP may comprise a poly(glyoxylate) or a derivative thereof, which may be a linear or cyclic homopolymer. In one embodiment, SRP is of the formula ( XI The structure of ) or a salt thereof, or containing it,

[0192]

[0193] R3 is H, optionally substituted alkyl, optionally substituted heteroalkyl, or optionally substituted aryl; and

[0194] n is approximately 2 to approximately 100,000.

[0195] (e.g., chemical formula ( XI In specific embodiments of ), R3 is, for example, -(Ak-O) h1 R O1 or -Ak-NR N1 R N2 It is an optionally substituted alkyl or optionally substituted heteroalkyl such as, wherein Ak is an optionally substituted alkylene, h1 is 1 to 5, and R O1 , R N1 and R N2 Each is independently H or an optionally substituted alkyl. In other embodiments, R3 comprises a metal-bonding moiety (e.g., any moiety described herein).

[0196] SRP may comprise poly(methyl methacrylate) or a derivative thereof, which may be a linear or cyclic polymer. In one embodiment, SRP is of the formula ( XII The structure of ) or a salt thereof, or containing it,

[0197]

[0198] R2 and R3 are each independently H, optionally substituted alkyl, optionally substituted heteroalkyl, or optionally substituted aryl; and

[0199] n is approximately 2 to approximately 100,000.

[0200] (e.g., chemical formula ( XII In specific embodiments of ), R2 is an optionally substituted alkyl. (e.g., formula ( XII In other embodiments of ), R3 is, for example, -(Ak-O) h1 R O1 or -Ak-NR N1 R N2 It is an optionally substituted alkyl or optionally substituted heteroalkyl such as, wherein Ak is an optionally substituted alkylene, h1 is 1 to 5, and R O1 , R N1 and R N2 Each is independently H or an optionally substituted alkyl. In other embodiments, at least one of R2 or R3 comprises a metal-bonding moiety (e.g., any moiety described herein).

[0201] SRP may comprise poly(glyoxylamide) or a derivative thereof, which may be a linear or cyclic polymer. In one embodiment, SRP is of the formula ( XIII The structure of ) or a salt thereof, or containing it,

[0202]

[0203] R 4' and R 4" Each is independently H, an optionally substituted alkyl, an optionally substituted aminoalkyl, an optionally substituted heteroalkyl, or R 4' , and R 4"Each is taken together with an attached nitrogen atom to form a heterocyclyl group as defined herein; and

[0204] n is approximately 2 to approximately 100,000.

[0205] (e.g., chemical formula ( XIII In specific embodiments of ), R 4' and / or R 4'' Each is, for example, -(Ak-O) h1 R O1 or -Ak-NR N1 R N2 It is an optionally substituted alkyl, an optionally substituted heteroalkyl, or an optionally substituted aminoalkyl such as, wherein Ak is an optionally substituted alkylene, h1 is 1 to 5, and R O1 , R N1 and R N2 Each is independently H or an optionally substituted alkyl. In other embodiments, R 4' is H or alkyl, and R 4" is an optionally substituted alkyl, an optionally substituted heteroalkyl, or an optionally substituted aminoalkyl (e.g., as described above). In another embodiment, R 4' and R 4" Each is taken together with an attached nitrogen atom to form a heterocyclyl group as defined in this specification. Non-limiting heterocyclyl groups include pyrrolidinyl, piperidinyl, morpholinyl, oxazolyl, isoxazolyl, pyrrolyl, pyrazolyl, etc.

[0206] Chemical formula ( I ) and chemical formula ( IIAs can be seen from ), the SRP may be a poly(aldehyde) comprising a general poly(aldehyde) having a backbone composed of alternating carbon and oxygen, including poly(phthalaldehyde) or poly(oxymethylene). These SRPs may be linear or cyclic polymers. The SRP is any R1, R described herein. 2' , R 2'' Poly(phthalaldehyde) or derivatives thereof for , r1, and n, e.g., formula ( Ia It may be a polymer containing the structure of ) or a salt thereof.

[0207]

[0208] In some examples, n is an integer from 4 to 100,000. In other embodiments, R1, R 2' , or R 2'' At least one of them includes a metal-bonded moiety (e.g., any moiety described herein).

[0209] In other embodiments, poly(phthalaldehyde) is cyclic. In some cases, the polymer is any R1, R5, R6, R described herein. 2' , R 2'' , R 3' , R 3'' , R 4' , R 4'' For , Z1, Z2, Z3, Z4, Z5, Z6, r1, r5, r6, and n1, chemical formula ( Ib ) or chemical formula ( Ic ) :

[0210] , It has the structure of, or a salt thereof. In some examples, n1 is an integer from 1 to 100. In other embodiments, R1, R5, R6, R 2' , R 2'' , R 3' , R 3'', R 4' , or R 4'' At least one of the includes a metal-bonded moiety (e.g., any moiety described herein).

[0211] In any embodiment of the present specification (e.g., chemical formula ( I ) to chemical formula ( VI ) and chemical formula ( Ib ), Z1 to Z6, L1, and L2, respectively, are, if present, independently -CR2R3O-, -OCR2R3-, -OCR2R3O-, -(CR2R3S) h1 CR2R3-, -S(CR2R3S) h1 -, -CR2R3S-, -SCR2R3-, -SCR2R3S-, -(CR2R3S) h1 CR2R3-, and -S(CR2R3S) h1 - is an optionally substituted heteroalkylene selected from, where R2 and R3 are each independently H, an optionally substituted alkyl, or an optionally substituted aryl, and h1 is an integer from 1 to 5.

[0212] In other embodiments, Z1 to Z6, L1, and L2 are each, if present, independently -O- or optionally substituted heteroalkylenes.

[0213] In any embodiment of the present specification (e.g., chemical formula ( I ) to chemical formula ( V ), chemical formula ( VII ), and chemical formula ( XII ) in), R2, R 2' , and R 2" Each, if present, is independently H or an optionally substituted alkyl (e.g., C 1-6 It is an alkyl.

[0214] In any embodiment of the present specification (e.g., chemical formula ( II ), chemical formula ( III ), chemical formula ( V), chemical formula ( VII ), chemical formula ( IX ), chemical formula ( X ), chemical formula ( XI ), and chemical formula ( XII ), R3 is an optionally substituted aryl.

[0215] (e.g., chemical formula ( II ), chemical formula ( III ), chemical formula ( V ), chemical formula ( VII ), chemical formula ( IX ), chemical formula ( X ), chemical formula ( XI ), and chemical formula ( XII In any embodiment of this specification, R3 is, for example, -OC(O)-R O1 , -NR N1 -C(O)-R O1 , -OC(O)NR N1 R N2 , -(Ak-O) h1 R O1 or -Ak-NR N1 R N2 It is an optionally substituted heteroalkyl such as, where Ak is an optionally substituted alkylene, h1 is 1 to 5, and R O1 , R N1 and R N2 Each is independently H or an optionally substituted alkyl (e.g., hydroxyalkyl, carboxyalkyl, aminoalkyl, or azidoalkyl).

[0216] In any embodiment of this specification, the polymer is a homopolymer or a copolymer. Such polymers may have any useful number n monomers, for example, n is about 2 to about 100,000 (e.g., about 2 to 50, 2 to 100, 2 to 200, 2 to 300, 2 to 400, 2 to 500, 2 to 1,000, 2 to 2,000, 2 to 5,000, 2 to 10,000, 2 to 20,000, 2 to 50,000, 2 to 100,000, 3 to 50, 3 to 100, 3 to 200, 3 to 300, 3 to 400, 3 to 500, 3 to 1,000, 3 to 2,000 Pieces, 3 to 5,000 pieces, 3 to 10,000 pieces, 3 to 20,000 pieces, 3 to 50,000 pieces, 3 to 100,000 pieces, 4 to 50 pieces, 4 to 100 pieces, 4 to 200 pieces, 4 to 300 pieces, 4 to 400 pieces, 4 to 500 pieces, 4 to 1,000 pieces, 4 to 2,000 pieces, 4 to 5,000 pieces, 4 to 10,000 pieces, 4 to 20,000 pieces, 4 to 50,000 pieces, 4 to 100,000 pieces, 5 to 50 pieces, 5 to 100 pieces, 5 to 200 pieces, 5 to 300 pieces, 5 to 400 pieces, 5 to 500 pieces, 5 to 1,000 pieces, 5 to 2,000 pieces, 5 to 5,000 pieces, 5 to 10,000 pieces, 5 to 20,000 pieces, 5 to 50,000 pieces, 5 to 100,000 pieces, 10 to 50 pieces, 10 to 100 pieces, 10 to 200 pieces, 10 to 300 pieces, 10 to 400 pieces, 10 to 500 pieces, 10 to 1,000 pieces, 10 to 2,000 pieces, 10 to 5,000 pieces, 10 to 10,000 pieces, 10 to 20,000 pieces, 10 to 50,000 pieces, 10 to 100,000 pieces,50 to 100 pieces, 50 to 200 pieces, 50 to 300 pieces, 50 to 400 pieces, 50 to 500 pieces, 50 to 1,000 pieces, 50 to 2,000 pieces, 50 to 5,000 pieces, 50 to 10,000 pieces, 50 to 20,000 pieces, 50 to 50,000 pieces, 50 to 100,000 pieces, 100 to 200 pieces, 100 to 300 pieces, 100 to 400 pieces, 100 to 500 pieces, 100 to 1,000 pieces, 100 to 2,000 pieces, 100 to 5,000 pieces, 10 to 10,000 pieces, 100 to 20,000, 100 to 50,000, and 100 to 100,000). In other embodiments, the polymer is cyclic, where n is about 3 to about 100. In other embodiments, the cyclic polymer comprises any useful number of n1+2 monomers, such as n1 of about 1 to about 100.

[0217] In specific embodiments, SRPs may also be any suitable linear or cyclic copolymer comprising a pure phthalaldehyde homopolymer, a homopolymer of poly(phthalaldehyde) derivatives such as poly(4,5-dichlorophthalaldehyde), or a homopolymer of poly(aldehyde) derivatives. SRPs are formulas ( I ) to chemical formula ( XIII ), chemical formula ( Ia ), chemical formula ( Ib ), chemical formula ( Ic One of the structures of ) or salts thereof, as well as any copolymer described herein (e.g., formula ( XIV ) or chemical formula ( XV It may include a copolymer containing one of ).

[0218] Examples of SRPs are provided below. In some embodiments, the SRPs are copolymers comprising poly(aldehydes). In specific embodiments, they may be self-immolative polymers as described in U.S. Patent Publication No. 2018 / 0155483, published June 7, 2018, and incorporated herein by reference in its entirety. Examples of copolymers in the reference literature are provided by the formula ( XIV Includes copolymers of ):

[0219] , here :

[0220] R is substituted or unsubstituted C 1-20 Alkyl, C 1-20 Alkoxy, C 2-20 Alkenyl, C 2-20 Alkinyl, C 6-10 Heteroaryl, C 3-10 Cycloalkyl, C 3-10 Cycloalkenyl, C 3-10 Heterocycloalkyl, or C 3-10 It is a heterocycloalkenyl; and when substituted, R is C 1-20 Alkyl, C 1-20 Alkoxy, C 2-20 Alkenyl, C 2-20 Alkinyl, C 6-10 Aril, C 6-10 It is substituted with heteroaryl, carboxyaldehyde, amino, sulfonic acid, sulfinic acid, fluoric acid, phosphonic acid, ether, halo, hydroxyl, ketone, nitro, cyano, azido, silyl, sulfonyl, sulfinyl, or thiol. In other embodiments, at least one R comprises a metal-bonding moiety (e.g., any moiety described herein).

[0221] In specific embodiments, the SRPs are cyclic copolymers of a phthalaldehyde monomer and a secondary aldehyde, such as ethanol, propanal, or butanal. Examples of such copolymers are provided in U.S. Patent Publication No. 2018 / 0155483 ( XV Provided as:

[0222] , where n is an integer from 1 to 100,000 and R is (e.g., chemical formula ( XIV ) may be any of those described in this specification. In other embodiments, at least one R comprises a metal-bonded moiety (e.g., any moiety described in this specification).

[0223] Specific examples of U.S. Patent Publication No. 2018 / 0155483 include phthalaldehyde and acetaldehyde, propanal, butanal, pentanal, hexanal, heptaneal, octaneal, nonanal, decaneal, undecanal, propenal, butenal, pentenal, hexenal, heptaneal, octenal, nonenal, deceneal, undecenal, and one or more copolymers of any combination thereof.

[0224] SRPs may also be any suitable linear or cyclic copolymer comprising a pure phthalaldehyde homopolymer. This may also be a homopolymer of poly(phthalaldehyde) derivatives such as poly(4,5-dichlorophthalaldehyde).

[0225] In any embodiment of this specification, SRP is the formula ( I ) to chemical formula ( XV ), chemical formula ( Ia Any one of the structures of ) or a salt thereof, or chemical formula ( I ) to chemical formula ( XV ), chemical formula ( IaIt comprises a monomer having any one of the structures of ) or a salt thereof, wherein n is 1, and is subsequently connected to another monomer through a linker. Non-limiting linkers include optionally substituted alkylenes, optionally substituted heteroalkylenes, optionally substituted (aryl)(alkyl)enes, optionally substituted arylenes, optionally substituted cycloalkylenes, oxy, or thio. In other embodiments, the linker is -Ak-, -Ak-X-, -X-Ak-, -(Ak-X) h1 -Ak-, -X-(Ak-X) h1 -, -Ak-Ar-, -Ak-Ar-Ak-, -Ar-Ak-, -(Ak-X) h1 -Ar-, -(Ak-X) h1 -Ar-(Ak-X) h1 -, -Ar-(Ak-X) h1 -, -X-(Ak-X) h1 -Ar-, -X-(Ak-X) h1 -Ar-X-(Ak-X) h1 -, and-Ar-X-(Ak-X) h1 -can be, where Ak is an optionally substituted alkylene, Ar is an optionally substituted arylene, and X is a non-carbon heteroatom (e.g., -O-, -S-, or -NR N1 -, here R N1 H is optionally alkyl, or optionally a substituted aryl), and h1 is an integer from 1 to 5.

[0226] In any embodiment of the present specification, SRP may be an amorphous polymer that retains solvent solubility.

[0227] SRP can be synthesized using any corresponding monomer. For example, the monomer has the chemical formula (where n is 1) I ) to chemical formula ( XV ), ( IaIt may be any one of the structures or a salt thereof. The monomer may have any useful terminal groups disposed on both ends of such a structure. In other embodiments, the monomer may be volatile and may have a melting point of 20°C or lower.

[0228] In certain embodiments, the SRP is formed without unwanted side products. In this way, residue-free vaporization of the polymer can be achieved because there is no need to remove the side products. For removal, the cleavage of one (or a few) chemical bonds within the SRP propagates the complete and rapid depolymerization of the polymer. Since all bonds are identical (without unintended impurities), little to no residue is expected.

[0229] SRP, or a formulation thereof, can be deposited in any useful manner. For example, SRP can be spin-coated or vapor-deposited.

[0230] Preparations including solvents and additives

[0231] The SRP may be provided as a formulation having a solvent or a combination of solvents. In one embodiment, the formulation comprises one or more SRPs (e.g., about 5 wt.% to 20 wt.%) in an amount of about 0.1 wt.% to about 50 wt.%, and the remainder is a solvent. Exemplary solvents include diglyme, tetrahydrofuran, N-methylpyrrolidone, dimethylformamide, propylene carbonate, cyclopentanone, anisole, dichlorobenzene, and propylene glycol methyl ether acetate.

[0232] The formulation may comprise one or more additional additives selected from organic acids having a pKa of 1 or more, photocatalysts (e.g., photo-generating agents or photo-base generating agents), thermal catalysts (e.g., thermal acid generating agents or thermal base generating agents), plasticizers and / or dyes. The amount of the additive may comprise a single additive in an amount of about 0.001 wt.% to about 25 wt.%, as well as a combination of additives in an amount of about 0.001 wt.% to about 25 wt.%.

[0233] In some embodiments, the SRP and additive(s) (e.g., any additive described herein) may be formulated and stored as separate solutions, but may also be mixed together at the deposition point on the wafer, or at any point relatively immediately prior. In some embodiments, the SRP and additive(s) may be provided as powders to be mixed in a solvent prior to spin coating. The SRP and additive may be provided (alone or together) in a relative wt.% of at least 5:1 SRP:additive, or at least 10:1, or 20:1.

[0234] That T c Polymers can be formulated with weak acids that not only produce stable films under ambient conditions but also exhibit accelerated degradation characteristics compared to neat, unformulated polymers in solvents. Specific examples of acids having this behavior include weak organic acids (e.g., having a pKa of 1 or greater). Other acids include tartaric acid, oxalic acid, and acetic acid.

[0235] Examples are linear alkyl carboxylic acids, C X H 2XIncludes O2 (where X is an integer), and corresponding dicarboxylic acid modifications. Specific examples include methanoic acid (X=1) and acetic acid (X=2). Specific examples of dicarboxylic acids include ethanedioic acid and propanedioic acid. Organic weak acids may also be any modifications thereof having additional alcohol substitutions and / or unsaturated bonds. For example, oxoethanoic acid, 2-hydroxyethanoic acid, prop-2-enoic acid, 2-propynoic acid, 2-hydroxypropanedioic acid, oxopropanedioic acid, 2,2-dihydroxypropanedioic acid, 2-oxopropanoic acid, 2-hydroxypropanoic acid, 3-hydroxypropanoic acid, 2,3-dihydroxypropanoic acid, etc. may be used.

[0236] However, other organic acids can exhibit similar abilities. Low T c The polymer may be pre-formulated with a suitable acid prior to tool installation and subsequently spin-coated onto substrates for sacrificial bracing or surface protection applications. Alternatively, low low T cThe polymer may be mixed with an acid at the point of use immediately before spin-coating. This approach may be used to extend the shelf life of the polymer formulation, but because it is stable in film form (solid state), it may not be stable in solution once it comes into contact with an acid. In some embodiments, the formulation is provided as about 5 to 20 wt.% SRP and less than 1 wt.% organic weak acid, with the remainder being a solvent.

[0237] The formulation, and thus the resulting membrane, may contain a photoacid generator (PAG) in which exposure of the SRP to electromagnetic radiation generates acid. In this way, exposure to energetic light (e.g., UV light, IR light, or X-rays) generates acid to promote in situ degradation of the membrane. Non-limiting photoacid generators include onium salts, e.g., iodium salts having perfluorinated anions, and sulfonium salts (e.g., diaryl iodium salts and triaryl sulfonium salts), bissulfonyldiazomethane compounds, N-sulfonyloxydicarboximide compounds, and O-arylsulfonyloxime compounds. The photoresist may optionally include a photosensitive agent (e.g., having modified polyaromatic hydrocarbons or fused aromatic rings).

[0238] Other acid generators, such as thermal acid generators that release acidic moieties upon exposure to heat, may be used. In this way, the depolymerization of SRP may involve both thermal and acidic processes. Non-limiting thermal acid generators include ammonium salts, sulfonyl esters, and acid amplifiers.

[0239] Plasticizers may be employed to promote the plasticity or flexibility of the membrane. Non-limiting plasticizers may include adipates, alkylene glycol dibenzosates, dialkyl phthalates, trialkyl trimellitates, tertiary amines, quaternary ammonium compounds, azelates, citrates, ether esters, polyethers, glutarates, glycols, isobutyrates, maleates, phosphates, phosphonium compounds, organic phosphates, sebacates, sulfonamides, sulfonium compounds, as well as ionic liquids, surfactants, and acid amplifiers, or combinations thereof.

[0240] Removal of SRPs

[0241] Several methods have been developed to achieve residue-free removal of SRPs without modifying sensitive substrates. One method of depolymerizing materials involves exposing the polymer to elevated temperatures under vacuum conditions. While this method can cause rapid volatilization of the polymer, angstrom-level residues consisting of char and residual monomers often remain on the surface.

[0242] SRPs can be removed by using less aggressive triggers, such as light or mild temperatures. These sacrificial polymers can allow for the protection of sensitive surfaces and the subsequent removal of barrier films without exposing the surfaces to aggressive plasmas or wet chemical solutions. For certain challenging applications, there may be limitations on the temperatures to which substrates can be exposed, or very strict contamination or throughput requirements. SRPs and their films can be designed to handle these applications.

[0243] Non-limiting removal conditions also include exposure to acidic or basic vapors. These vapors may be provided by a reactive substance such as an acid (e.g., having a pKa of less than 7, and in some embodiments, less than 4, or less than 2) or a base (e.g., having a pKa of less than 7, and in some embodiments, less than 4 or less than 2). Non-limiting reactive substances include sulfurous acid, formic acid, nitric acid, carbonate, or ammonium hydroxide.

[0244] Other non-limiting catalysts may be hydrogen bromide (HBr), hydrogen chloride (HCl), hydrogen fluoride (HF), hydrogen iodide (HI), nitric acid (HNO3), formic acid (CH2O2), acetic acid (CH3COOH), formonitrile (HCN), sulfurous acid (H2SO3), carbonic acid (H2CO3), nitrous acid (HNO2), or ammonia (NH3), and methyl or ethylamine gas or vapor. In some examples, when HBr vapor is used, the substrate is maintained at a pressure in the range of 1 mTorr to 5000 mTorr (e.g., 5 mTorr to 5000 mTorr) and a temperature in the range of 0 °C to 200 °C (e.g., 0 °C to 100 °C). In some examples, the substrate is maintained at a pressure in the range of 750 mTorr to 1500 mTorr and a temperature in the range of 35 °C to 70 °C. In some examples, the temperature of the substrate is maintained at a pressure of 1000 mTorr and a temperature of 60 °C. The amount of acidic vapor or vapor of other compounds is controlled to limit diffusion. The exposure time may depend on the strength of the acid or base, as well as the film thickness and the exposure temperature (e.g., about 20 °C to about 125 °C or about 100 °C to about 125 °C). Non-limiting exposure times are less than about 60 seconds or approximately a few It can include minutes.

[0245] In other embodiments, removal may involve exposure to two reactants that react to form an acid or base capable of triggering the degradation of the SRP. The exposure occurs sequentially to provide more precise top-down control. In some embodiments, the methods involve diffusing the compound, or the reactant reacting to form the compound, only into the top portion of the SRP. The top portion is then degraded and removed, leaving the remaining SRP intact. The exposure cycle and removal cycle may be repeated. Optionally, a purge operation may follow the exposure operation to remove the compound or reactant from the chamber.

[0246] Non-limiting reactants (for, for example, to form an acid or base) may include water vapor and one of ammonia (NH3) or a gaseous oxide that reacts with water vapor to form an acidic or basic species. For example, NH3 and water may react to form ammonium hydroxide (NH4OH). Examples of gaseous oxides include nitrogen dioxide (NO2, which can react with water to form nitric acid (HNO3)), sulfur dioxide (SO2, which can react with water to form sulfurous acid (H2SO3)), and carbon dioxide (CO2, which can react with water to form carbonic acid (H2CO3)). Other oxides may also react with water or other reactants to form acids or bases.

[0247] Alternative polymer removal processes can provide lower contamination levels. In one such process, the polymer is exposed to long-lived metastable species from a noble gas plasma under vacuum at elevated temperatures. In another process, the polymer is exposed to infrared (IR), ultraviolet (UV), or extreme ultraviolet (EUV) radiation at elevated temperatures while under vacuum. Other processes involve high-temperature exposure (e.g., about 50 °C to about 250 °C) under vacuum conditions (e.g., less than 760 Torr) for limited exposure times. Another process may involve simultaneous high-temperature exposure and radiation exposure by UV or IR under vacuum. Yet another process may involve simultaneous high-temperature exposure and noble gas metastable exposure under vacuum. In specific embodiments, these removal processes also exhibit low contamination without increasing surface modification of sensitive substrates.

[0248] Inside the chamber, the substrate may be exposed to heat for SRP removal. Heat may be provided as a constant temperature hold. Alternatively, heat may be provided as a ramped temperature where rising or falling temperature ramps can be used between these temperature holds. This thermal energy is T c By providing heat at temperatures above this level, sufficient energy can be provided to depolymerize SRP. These conditions are T below 250 ℃. c For an SRP having , exposure to temperatures up to 250 ℃ may be included, where SRP is T cIt is kinetically trapped below. In other embodiments, thermal exposure may include a temperature of about 50 °C to about 250 °C (e.g., about 50 °C to 150 °C, 50 °C to 250 °C, 150 °C to 200 °C to 250 °C, or 200 °C to 250 °C, etc.). In other embodiments, thermal exposure includes exposure to a temperature raised by a rapid ramp rate and for a shorter time (e.g., up to 800 °C). When additives (e.g., a photoacid generator (PAG) or any additive of this specification) are used, the temperature for removal may be about 50 °C to about 125 °C in addition to exposure to other stimuli that can advantageously activate the additive (e.g., UV exposure to activate the PAG).

[0249] For the basic thermal removal of surface protection films (e.g., by placing a substrate on a hot plate), the exposure time may be about 20 seconds to about 400 seconds (e.g., about 30 to 300 seconds). Thicker films may require longer exposure to heat for SRP removal compared to thinner films. The required film thickness will be application-dependent. For example, some removal thermal processes (e.g., using a rapid thermal processor; RTP) may involve higher temperatures (e.g., exceeding about 400°C) for very short periods (e.g., 1 to 2 seconds for RTP exposure, as well as millisecond exposure times for flash ramp-type processes). For applications sensitive to thermal budget, RTP-type conditions may be employed, while other processes may employ a hot plate under vacuum.

[0250] Alternatively, SRP can be removed by exposure to radiation (e.g., UV radiation or IR radiation) with or without vacuum. In some examples, process conditions include exposure to about 200°C under vacuum at a UV dose rate of about 2.5 W / cm². In other examples, process conditions (e.g., for SRP employed with a photogenerator) include exposure to about 110°C under vacuum at a UV dose rate of about 0.05 mW / cm². Under any of these process conditions, exposure may include about 100 seconds to about 400 seconds (e.g., about 300 seconds).

[0251] For the radiation removal of surface protective films (e.g., pure SRP), the exposure time may be approximately 20 seconds to approximately 400 seconds (e.g., approximately 30 to 300 seconds). Thicker films may require longer exposure to radiation (e.g., UV) for SRP removal compared to thinner films. The required film thickness will be application-dependent. For films containing acid-generating additives (e.g., PAG), exposure times may range from 2 minutes to 10 minutes. The exposure time may depend on many conditions, including the loading of additives, wafer temperature, UV dose rate, and film thickness. These requirements will ultimately be application-dependent (e.g., dependent on feature dimensions, aspect ratio, pattern density, etc.).

[0252] The radiation dose can be, for example, about 0.1 mW / cm² to about 15 W / cm² for UV. For decay-sensitive applications where rate control of degradation is targeted, lower dose rates, for example, about 0.01 to about 0.07 mW / cm² may be employed. For the removal of a pure SRP film from blanket surfaces, higher dose rates, for example, about 2.5 W / cm² may be employed. Generally, the higher the dose rate, the cleaner the removal. Of course, radiation exposure can also be application-dependent, and excessive radiation can be prevented to mitigate substrate damage.

[0253] During radiation exposure, the substrate may be maintained at an elevated temperature (e.g., from about 50°C to about 250°C, including about 200°C). If the formulation contains acid-generating additives (e.g., PAG), lower temperatures (e.g., a temperature range of about 50°C to about 125°C or about 100°C to about 110°C) may be combined with UV exposure to provide a controlled degradation rate.

[0254] Metastable atoms may be employed. Metastable atoms may be generated from a noble gas plasma to provide an excited state, and the noble gas is one or more of helium (He), neon (Ne), argon (Ar), krypton (Kr), and xenon (Xe) to remove residues from the substrate. In some embodiments, the metastable species are chemically non-reactive and do not significantly affect the surface placed underneath. Metastable species from the noble gas plasma may be effective in removing residues remaining after exposure to other stimuli, such as heat. In the methods described herein, removing SRPs involves exposure to high-energy metastable species generated from the noble gas plasma at elevated temperatures. The metastable species possess sufficient energy and lifetimes to cleave bonds on the polymer or other residues. At temperatures higher than the ceiling temperature, there is a strong thermodynamic driving force that reverts to volatile monomers once bond cleaving occurs. Metastable species are chemically non-reactive and do not significantly affect the underlying surface. Metastable species are effective in removing residues remaining after exposure to other stimuli, such as heat. These residues may be some polymerized or cross-linked SRPs and / or carbonized shards that remain detectable by ellipsometry. While most SRPs can be removed by the stimuli described above, these residues may be difficult to completely remove by these methods. Without being bound by a specific theory, metastable species may also remove residues by restarting chain cleavage that might be prematurely interrupted due to byproduct formation, by breaking down char that might be formed during the depolymerization process, and by assisting in monomer desorption.

[0255] In some embodiments, most of the SRP is removed before the substrate is exposed to metastable atoms. In some embodiments, the substrate is exposed to metastable atoms before most of the SRP is removed. In some embodiments, the plasma pressure is about 10 mTorr to 10 Torr. In some embodiments, the plasma pressure is about 100 mTorr to 1 Torr. In some embodiments, the SRP is provided as a protective coating on the substrate. In some embodiments, the plasma is generated from an inductively coupled plasma (ICP) source. In some of these embodiments, the ICP source is separated from the substrate by a showerhead or other filter. In some embodiments, the plasma is generated from a capacitively coupled plasma (CCP) source. Any other type of plasma source may be used. In some embodiments, the step of exposing the substrate to stimulation and the step of exposing the substrate to metastable atoms are performed in the same chamber.

[0256] The processing and plasma source chamber pressure may also be used to control plasma-based removal. Pressure is important for controlling the density of metastable atoms. If the pressure is too low, the density of metastable atoms may not be high enough to efficiently clean the surface. If the pressure is too high, metastable species may be lost due to collisions. Exemplary pressures may be in the range of 10 mTorr to 10 Torr, 100 mTorr to 1 Torr, 100 mTorr to 700 mTorr, 200 mTorr to 1 Torr, or 200 mTorr to 2 Torr.

[0257] Substrate temperature and plasma power may also be used to control removal. The temperature is sufficiently high to be higher than the ceiling temperature of the polymer. Higher temperatures assist removal to the maximum temperature limited by the thermal budget of the device or other materials on the substrate. Exemplary temperatures may be in the range of 150 °C to 1000 °C or 150 °C to 250 °C. Plasma power is sufficiently high to generate metastable atoms. Exemplary power may be in the range of 500 W to 5000 W or 800 W to 5000 W, for example, 2500 W for a 300 mm wafer, and may scale linearly with the substrate area. Exemplary exposure times may be in the range of 10 seconds to 300 seconds or 10 seconds to 180 seconds.

[0258] Removal may occur in a single step or multiple steps. A non-limiting method may include providing an SRP film to a substrate. Subsequently, a stimulus that degrades the SRP is pulsed within a chamber. Such stimulus may include exposure to a compound (e.g., acid, base, acid or base-forming compound, plasma, metastable compound, etc.) or reaction conditions (e.g., UV radiation, IR radiation, heat, etc.). In some embodiments, removal involves exposure to heat and / or radiation, thereby eliminating the need for harsh wet chemicals and / or plasma to modify sensitive surfaces that need to be protected.

[0259] When the compound is used, the partial pressure of the vapor and / or the pulse time can be controlled to control the total exposure and diffusion depth to the vapor. Subsequently, the chamber can be purged. Purging may involve exhausting the chamber and / or flowing an inert gas to sweep out through the chamber. This gas may be, for example, continuous or self-pulsed into the chamber. The volatile monomer or SRP fragment may be pumped out or purged from the chamber, and this may be repeated until the SRP is removed. As indicated above, in some embodiments, the SRP is sequentially exposed to the reaction materials in each cycle. This can provide additional control over the process and may be implemented in various ways.

[0260] Depending on various embodiments, the reaction may or may not be catalyzed. In some embodiments, a catalyst (e.g., a thermally activated catalyst) may be provided to the SRP, delivered together with the reaction material, or introduced as a separate pulse. However, in many embodiments, the reaction is not catalyzed so that the SRP is provided without a catalyst. This can facilitate SRP removal. In some embodiments, the reaction is byproduct-free.

[0261] Methods of using SRPs and additional examples of SRPs are described in U.S. Patents No. 9,466,511, 9,666,427, 10,008,396, and 10,068,781, each of which is incorporated herein by reference in its entirety.

[0262] device

[0263] The metal features described herein may be formed using electroplating or electrodeposition processes and devices. Such electroplating or electrodeposition devices may be used in conjunction with one or more additional substrate processing tools used to process substrates, including the deposition of SRPs, removal of SRPs, alignment of metal features, bonding of metal features, and other upstream and downstream processing. In other embodiments, the electroplating or electrodeposition devices may be configured to deposit SRPs within a process chamber to cap the metal features after deposition.

[0264] FIG. 7 provides an example of an electroplating cell in which electroplating may occur. Often, an electroplating apparatus comprises one or more electroplating cells in which substrates (e.g., wafers) are processed. For clarity, only one electroplating cell is shown in FIG. 7. To optimize bottom-up electroplating, additives (e.g., accelerators, inhibitors, and levelers) are added to the electrolyte; however, an electrolyte containing additives may react with the anode in undesirable ways. Therefore, the anode and cathode regions of the plating cell are sometimes separated by a membrane, and plating solutions of different compositions may be used in each region. The plating solution in the cathode region is called the catholyte, and in the anode region, the anolyte. A number of engineering designs may be used to introduce the anolyte and catholyte into the plating apparatus.

[0265] Referring to FIG. 7, a diagrammatic cross-sectional view of an electroplating apparatus (701) according to one embodiment is shown. A plating bath (703) contains an electroplating solution (having a composition as provided herein), shown as a level (705). The cathode portion of this vessel is configured to accommodate substrates within the cathode solution. A wafer (707) is immersed in the plating solution and held by a "clamshell" substrate holder (709), which is mounted on a rotatable spindle (711) that allows rotation of the clamshell substrate holder (709) together with the wafer (707), for example. General technology of a clamshell-type plating apparatus having embodiments suitable for use with the present invention is described in detail in U.S. Patent No. 6,156,167 granted to Patton et al. and U.S. Patent No. 6,800,187 granted to Reid et al., which are incorporated herein by reference.

[0266] An anode (713) is placed beneath the wafer within a plating bath (703) and separated from the wafer region by a membrane (715), preferably an ion-selective membrane. For example, a Nafion™ cationic exchange membrane (CEM) may be used. The region beneath the anode membrane is often referred to as the "anode chamber." The ion-selective anode membrane (715) allows ion communication between the anode region and the cathode region of the plating cell, while preventing particles generated from the anode from entering the vicinity of the wafer and contaminating the wafer. The anode membrane is also useful for improving plating uniformity by redistributing current flow during the plating process. Detailed descriptions of suitable anode membranes are provided in U.S. Patents No. 6,126,798 and No. 6,569,299 granted to Reid et al., all of which are incorporated herein by reference in their entirety. Ion exchange membranes, such as cation exchange membranes, are particularly suitable for these applications. These membranes are typically composed of ionomer materials, such as perfluorinated copolymers containing sulfonate groups (e.g., Nafion™), sulfonated polyimides, and other materials known to those skilled in the art as suitable for cation exchange. Selected examples of suitable Nafion™ membranes include N324 and N424 membranes available from Dupont de Nemours Co.

[0267] During plating, ions from the plating solution are deposited onto the substrate. Metal ions must diffuse through the diffusion boundary layer and into TSV (through silicon via) holes, openings, or other features. A conventional method to assist in diffusion is through the convective flow of the electroplating solution provided by the pump (717). Additionally, wafer rotation, as well as vibration stirring or sonic stirring elements, may be used. For example, a vibration transducer (708) may be attached to the clamshell substrate holder (709).

[0268] The plating solution is continuously supplied to the plating bath (703) by a pump (717). Typically, the plating solution flows radially outward across the wafer (707) through an anode membrane (715) and a diffuser plate (719) toward the center of the wafer (707). The plating solution may also be supplied from the side of the plating bath (703) into the anode region of the bath. The plating solution then overflows the plating bath (703) into an overflow reservoir (721). The plating solution is then filtered (not shown) and returned to the pump (717) to complete the recirculation of the plating solution. In certain configurations of the plating cell, a distinct electrolyte is circulated through the portion of the plating cell containing the anode, while mixing with the main plating solution is prevented using low-permeability membranes or ion-selective membranes.

[0269] A reference electrode (731) is located outside the plating bath (703) within a separate chamber (733), and the chamber is replenished by an overflow from the main plating bath (703). Alternatively, in some embodiments, the reference electrode is positioned as close as possible to the substrate surface, and the reference electrode chamber is connected to the side of the wafer substrate or directly beneath the wafer substrate via a capillary or by another method. In some preferred embodiments, the device further includes contact sensing leads that are connected to the periphery of the wafer and configured to sense the potential of the metal seed layer at the periphery of the wafer but do not transmit any current to the wafer.

[0270] A reference electrode (731) is typically employed when electroplating is targeted at a controlled potential. The reference electrode (731) may be one of various commonly used types, such as mercury / mercury sulfate, silver chloride, saturated calomel, or copper metal. Contact sensing leads that make direct contact with the wafer (707) may be used in addition to the reference electrode in some embodiments for more accurate potential measurements (not shown).

[0271] A DC power supply (735) may be used to control the current flow to the wafer (707). The power supply (735) has a negative output lead (739) electrically connected to the wafer (707) through one or more slip rings, brushes, and contacts (not shown). The positive output lead (741) of the power supply (735) is electrically connected to an anode (713) located within the plating bath (703). The power supply (735), reference electrode (731), and contact sensing lead (not shown) may be connected to a system controller (747) that, among other functions, allows modulation of the current and potential provided to the elements of the electroplating cell. For example, the controller may allow electroplating in a potential-controlled regime and a current-controlled regime. The controller may include program instructions that specify the current and voltage levels to be applied to the various elements of the plating cell, as well as the times at which these levels should be changed. When a forward current is applied, the power supply (735) biases the wafer (707) to have a negative potential with respect to the anode (713). This causes current to flow from the anode (713) to the wafer (707) and electrochemical reduction (e.g., Cu 2 + + 2 e - = Cu 0 This occurs on the wafer surface (cathode), and causes the deposition of an electrically conductive layer (e.g., copper) on the surfaces of the wafer. The inert anode (714) may be installed under the wafer (707) in a plating bath (703) or separated from the wafer area by a membrane (715).

[0272] The device may also include a heater (745) for maintaining the temperature of the plating solution at a specific level. The plating solution may also be used to transfer heat to other elements of the plating bath. For example, when a wafer (707) is loaded into the plating bath, the heater (745) and pump (717) may be turned on to circulate the plating solution through the electroplating device (701) until the temperature throughout the device becomes substantially uniform. In one embodiment, the heater is connected to a system controller (747). The system controller (747) may be connected to a thermocouple to receive feedback on the temperature of the plating solution within the electroplating device and to determine the need for additional heating.

[0273] The controller will typically include one or more memory devices and one or more processors. The processor may include a CPU or computer, analog input / output connections and / or digital input / output connections, stepper motor controller boards, etc. In specific embodiments, the controller controls all activities of the electroplating device. A non-transient, machine-readable medium containing instructions for controlling process operations according to the embodiments may be coupled to the system controller.

[0274] Typically, there will be a user interface associated with a controller (747). The user interface may include a display screen, graphic software displays of device and / or process conditions, and user input devices such as pointing devices, keyboards, touch screens, microphones, etc. Computer program code for controlling electroplating processes may be written in any conventional computer-readable programming language, e.g., assembly language, C, C++, Pascal, Fortran, or other languages. Compiled object code or script is executed by a processor to perform tasks identified in the program. An example of a plating device that may be used according to the embodiments of this specification is the Lam Research Sabre tool. Electroplating may be performed on components forming a larger electroplating device.

[0275] FIG. 8 illustrates a schematic plan view of an exemplary electrodeposition apparatus. The electrodeposition apparatus (800) may include three distinct electroplating modules (802, 804, and 806). The electrodeposition apparatus (800) may also include three distinct modules (812, 814, and 816) configured for various process operations. For example, in some embodiments, one or more of the modules (812, 814, and 816) may be Spin Rinse Drying (SRD) modules. In other embodiments, one or more of the modules (812, 814, and 816) may be post-electrofill modules (PEMs), each configured to perform functions such as edge bevel removal, back etching, and acid cleaning of substrates after the substrate is processed by one of the electroplating modules (802, 804, and 806). In yet another embodiment, one or more of the modules (812, 814, and 816) may be configured to deposit SRP on the surface of the substrate after it is processed by one of the electroplating modules (802, 804, and 806).

[0276] The electrodeposition device (800) includes a central electrodeposition chamber (824). The central electrodeposition chamber (824) is a chamber that holds the chemical solution used as the electroplating solution in the electroplating modules (802, 804, 806). The electrodeposition device (800) also includes a dosing system (826) that may store and deliver additives for the electroplating solution. A chemical dilution module (822) may store and mix chemicals to be used as an etchant. A filtration and pumping unit (828) may filter the electroplating solution for the central electrodeposition chamber (824) and pump it to the electroplating modules (802, 804, 806).

[0277] A system controller (830) provides the electronic control and interface control necessary to operate the electroplating device (800). The system controller (830), which may include one or more physical or logical controllers, controls some or all attributes of the electroplating device (800). The system controller (830) typically includes one or more memory devices and one or more processors. The processor may include a CPU (Central Processing Unit) or computer, analog input / output connections and / or digital input / output connections, stepper motor controller boards, and other similar components. Instructions for implementing the appropriate control operations described herein may be executed on the processor. These instructions may be stored on memory devices associated with the system controller (830), or they may be provided via a network. In specific embodiments, the system controller (830) executes system control software.

[0278] System control software within the electrodeposition device (800) may include instructions for controlling timing, mixture of electrolyte components, inlet pressure, plating cell pressure, plating cell temperature, substrate temperature, current and potential applied to the substrate and any other electrodes, substrate position, substrate rotation, and other parameters of a specific process performed by the electrodeposition device (800). System control logic may be configured in any suitable manner. For example, various process tool component subroutines or control objects may be written to control the operation of process tool components necessary to perform various process tool processes. System control software may be coded in any suitable computer-readable programming language. The logic may also be implemented in hardware on a programmable logic device (e.g., FPGA), ASIC, or other suitable means (vehicle).

[0279] In some embodiments, the system control logic includes IOC (Input / Output Control) sequencing instructions for controlling the various parameters described above. For example, each phase of the electroplating process may include one or more instructions for execution by the system controller (830). Instructions for setting process conditions for the immersion process phase may be included in the corresponding immersion recipe phase. In some embodiments, the electroplating recipe phases may be arranged sequentially so that all instructions for the electroplating process phase are executed simultaneously with the process phase.

[0280] In some embodiments, the control logic may be divided into various components, such as programs or sections of programs. Examples of logic components for this purpose include a substrate positioning component, an electrolyte composition control component, a pressure control component, a heater control component, and a potential / current power supply control component.

[0281] In some embodiments, there may be a user interface associated with a system controller (830). The user interface may include user input devices such as a display screen, graphic software displays of device and / or process conditions and pointing devices, keyboards, touch screens, microphones, etc.

[0282] In some embodiments, parameters adjusted by the system controller (830) may relate to process conditions. Non-limiting examples include bath conditions (temperature, composition, and flow rate), substrate position at various stages (rotation rate, linear (vertical) speed, angle from horizontal), etc. These parameters may be provided to the user in the form of a recipe that can be entered using a user interface.

[0283] Signals for monitoring the process may be provided from various process tool sensors by the analog input and / or digital input connections of the system controller (830). Signals for controlling the process may be output on the analog output and digital output connections of the process tool. Non-limiting examples of process tool sensors that may be monitored include mass flow controllers, pressure sensors (such as manometers), thermocouples, optical position sensors, etc. Appropriately programmed feedback and control algorithms may be used with data from these sensors to maintain process conditions.

[0284] The hand-off tool (840) may select a substrate from a substrate cassette, such as a cassette (842) or a cassette (844). The cassettes (842 or 844) may be FOUPs (Front Opening Unified Pods). A FOUP is an enclosure designed to hold a substrate securely and firmly in a controlled atmosphere, allowing the substrate to be removed for processing or measurement by tools equipped with appropriate load ports and robotic handling systems. The hand-off tool (840) may hold the substrate using vacuum attachment or some other attachment mechanism.

[0285] The hand-off tool (840) may interface with a wafer handling station (832), cassettes (842 or 844), a transfer station (850), or an aligner (848). From the transfer station (850), the hand-off tool (846) may obtain access to the substrate. The transfer station (850) may be a slot or position where the hand-off tools (840 and 846) may pass through the substrates without passing through the aligner (848). However, in some embodiments, to ensure that the substrate is properly aligned with the hand-off tool (846) for precise transfer to the electroplating module, the hand-off tool (846) may align the substrate with the aligner (848). The hand-off tool (846) may also transfer the substrate to one of the electroplating modules (802, 804, or 806) or to one of three separate modules (812, 814, or 816) configured for various process operations.

[0286] An example of process operation according to the methods described above may proceed as follows: (1) electrodepositing copper or another material onto a substrate of an electroplating module (804); (2) rinsing and drying the substrate in an SRD of a module (812); and (3) performing edge bevel removal in a module (814). Another method comprises: (1) electrodepositing copper or another material onto a substrate of an electroplating module (804); (2) rinsing and drying the substrate in an SRD of a module (812); and (3) depositing SRP onto a substrate in a module (814). Another method comprises: (1) electrodepositing copper or another material onto a substrate of an electroplating module (804); (2) rinsing and drying the substrate in an SRD of a module (812); (3) performing acid cleaning of the substrate in a module (814); and (4) depositing SRP onto a substrate in a module (816).

[0287] A device configured to allow efficient cycling of substrates through sequential plating, rinsing, drying, and PEM process operations may be useful for embodiments intended for use in a fabrication atmosphere. To achieve this, the module (812) may be configured as a spin rinse dryer and an edge bevel removal chamber. Using this module (812), the substrate will only need to be transferred between the electroplating module (804) and the module (812) for copper plating and EBR operations. In some embodiments, the methods described herein will be implemented in a system comprising an electroplating device and a stepper.

[0288] An alternative embodiment of the electrodeposition apparatus (900) is schematically illustrated in FIG. 9. In this embodiment, the electrodeposition apparatus (900) has a set of electroplating cells (907), each comprising an electroplating bath in a pair or a plurality of "duets" configurations. Electroplating 그 자체 (per se) In addition, the electrodeposition apparatus (900) may perform, for example, various other electroplating-related processes and sub-steps, such as spin-rinsing, spin-drying, metal and silicon wet etching, electroless deposition, pre-wet treatment and pre-chemical treatment, reduction, annealing, electro-etching and / or electro-polishing, photoresist stripping and surface pre-activation. The electrodeposition apparatus (900) is schematically illustrated in FIG. 9 as viewed from above, and only a single level or "floor" is shown in the drawing, but such an apparatus, for example, Lam Sabre TM It is readily understood by those skilled in the art that 3D tools may have two or more levels "stacked" on top of each other, and each may potentially have the same or different types of processing stations.

[0289] Referring again to FIG. 9, a substrate (906) to be electroplated is typically fed into an electrodeposition device (900) via a front-end loading FOUP (901), and in this example, is transferred from the FOUP to the main substrate processing area of ​​the electrodeposition device (900) via a front-end robot (902) capable of retracting and moving the substrate (906), driven by a spindle (903), from one station of accessible stations to another station in multiple dimensions—two front-end accessible stations (904) and two front-end accessible stations (908) are shown in this example. The front-end accessible stations (904 and 908) may include, for example, pretreatment stations and SRD (spin rinse drying) stations. Lateral movement from side to side of the front-end robot (902) is achieved by utilizing the robot track (902a). Each of the substrates (906) may be held by a cup / cone assembly (not shown) driven by a spindle (903) connected to a motor (not shown), and the motor may be attached to a mounting bracket (909). Also shown in this example are four "duets" of electroplating cells (907), for a total of eight electroplating cells (907). A system controller (not shown) may be coupled to the electroplating device (900) to control some or all of the properties of the electroplating device (900). The system controller may be programmed or otherwise configured to execute instructions according to the processes described prior to this specification.

[0290] FIG. 10 illustrates a simplified cross-sectional view of an electroplating apparatus. The apparatus includes an electroplating cell (1001) together with a substrate (1002) positioned within a substrate holder (1003). The substrate holder (1003) is often referred to as a cup, and the substrate holder (1003) may also support the substrate (1002) at its periphery. An anode (1004) is positioned near the bottom of the electroplating cell (1001). The anode (1004) is separated from the substrate (1002) by a membrane (1005), which is supported by a membrane frame (1006). The membrane frame (1006) is sometimes referred to as an anode chamber membrane frame because it defines the top of the anode chamber housing the anode. Additionally, the anode (1004) is separated from the substrate (1002) by an ion-resistant element (1007). The ion-resistant element (1007) includes openings that allow the electrolyte to move through the ion-resistant element (1007) to collide with the substrate (1002). A front insert (1008) is positioned on the ion-resistant element (1007) in close proximity to the periphery of the substrate (1002). The front side insert (1008) may be ring-shaped as illustrated and may be non-uniform in azimuth. The front insert (1008) is sometimes also referred to as a cross-flow confinement ring.

[0291] The anode chamber (1012) is located below the membrane (1005), and the anode (1004) is positioned therein. The ion-resistant element manifold (1011) is located above the membrane (1005) and below the ion-resistant element (1007). An inlet (1016), which may be connected to an irrigation flute (1040), delivers cathodic liquid to the ion-resistant element manifold (1011) and may also function to irrigate the membrane (1005) during electroplating. In this example, the inlet (1016) and the irrigation flute (1040) are fed by an electrolyte passing through the cathodic liquid inlet (1018). A cross-flow manifold (1010) is located above the ion-resistant element (1007) and below the substrate (1002). The height of the cross-flow manifold is considered to be the distance between the substrate (1002) and the plane of the ion-resistant element (1007) (excluding, if present, ribs (1015) on the upper surface of the ion-resistant element (1007). In some cases, the cross-flow manifold may have a height of about 1 mm to 4 mm, or about 0.5 mm to 15 mm. The cross-flow manifold (1010) is defined on its sides by a front insert (1008) that functions to contain the cross-flow electrolyte within the cross-flow manifold (1010). A side inlet (1013) to the cross-flow manifold (1010) is provided azimuthal opposite to a side outlet (1014) to the cross-flow manifold (1010). The side inlet (1013) and side outlet (1014) may be formed at least partially by the front insert (1008).

[0292] As illustrated by the arrows in FIG. 10, the electrolyte moves from the cathode liquid inlet (1018), through the side inlet (1013), into the cross-flow manifold (1010), and from the side outlet (1014). In addition, the electrolyte may move through one or more inlets to the ion-resistant element manifold (1011) (e.g., irrigation flutes (1040) and / or other inlets), into the ion-resistant element manifold (1011), through the openings of the ion-resistant element (1007), into the cross-flow manifold (1010), and from the side outlet (1014). After passing through the side outlet (1014), the electrolyte spills over the weir wall (1009). The electrolyte may be recovered and recycled.

[0293] In certain embodiments, the ionically resistive element (1007) is positioned near a nearly constant and uniform current source in the vicinity of the substrate (cathode) and may therefore be referred to as a high-resistance virtual anode (HRVA) or a channeled ionically resistive element (CIRP) in some contexts. Generally, the ionically resistive element (1007) is positioned very close to the wafer. In contrast, an anode positioned equally close to the substrate would be significantly less suitable for supplying a nearly constant current to the wafer, but would only support a constant potential plane on the anode metal surface, thereby allowing the current to be maximum, and the net resistance from the anode plane to the terminals (e.g., to peripheral contact points on the wafer) would be smaller. Thus, the ionically resistive element (1007) is referred to as a high-resistance virtual anode (HRVA), but this does not imply that the two are electrochemically interchangeable. Under specific operating conditions, the ionic resistive element (1007) will be more closely approximated and perhaps better described as a virtual uniform current source through which a nearly constant current is sourced across the upper plane of the ionic resistive element (1007).

[0294] In many but not all embodiments, the ion-resistive element (1007) comprises micro-sized (typically less than 0.04") through-holes that are spatially and ionically isolated from one another and do not form interconnected channels within the body of the ion-resistive element. These through-holes are often referred to as non-connected through-holes. They do not typically need to be perpendicular to the plated surface of the wafer, but often extend in one dimension (in some embodiments, the non-connected holes are generally angled to the wafer parallel to the front of the ion-resistive element). Often, the through-holes are parallel to each other. Often, the holes are arranged in a square array. In other cases, the layout is in an offset spiral pattern. These through-holes are distinguished from 3-D porous networks where channels extend in three dimensions and form interconnected pore structures, because the through-holes reconfigure both ion current flow and (in certain cases) fluid flow parallel to the inner surface and straighten the paths of both current and fluid flow toward the wafer surface. However, in certain embodiments, the interconnected Such a porous plate having a network of pores may also be used as an ion-resistant element. When the distance from the top surface of the plate to the wafer is small (e.g., about 1 / 10 of the wafer radius, e.g., a gap of less than about 5 mm), the divergence of both current flow and fluid flow is locally confined, imposed, and aligned into the ion-resistant element channels.

[0295] An example of an ionic resistive element (1007) is a disk made of a rigid, non-porous dielectric material that is ionically and electrically resistive. The material is also chemically stable in the plating solution used. In certain cases, the ionic resistive element (1007) is made of a ceramic material (e.g., aluminum oxide, tin oxide, titanium oxide, or a mixture of metal oxides) or a plastic material (e.g., polyethylene, polypropylene, polyvinylidene difluoride (PVDF), polytetrafluoroethylene, polysulfone, polyvinyl chloride (PVC), polycarbonate, etc.) having about 6,000 to 12,000 non-connecting through-holes. In many embodiments, the ion-resistant element (1007) occupies substantially the same space as the wafer (coextensive with) (e.g., the ion-resistant element (1007) has a diameter of about 300 mm when used with a 300 mm wafer) and is located very close to the wafer, for example, directly below the wafer in a wafer-down-faced electroplating device. Preferably, the plating surface of the wafer is placed within about 10 mm, more preferably within about 5 mm, of the nearest ion-resistant element surface. To this end, the top surface of the ion-resistant element (1007) may be flat or substantially flat. Often, both the top surface and the bottom surface of the ion-resistant element (1007) are flat or substantially flat. However, in many embodiments, the top surface of the ion-resistant element (1007) includes a series of linear ribs as further described below.

[0296] As described above, the overall ionicity and flow resistance of the plate (1007) depend on the thickness of the plate, the overall porosity (the fraction of the area available for flow through the plate), and the size / diameter of the holes. Plates with lower porosity will have higher collision flow velocities and ionic resistances. When comparing plates of the same porosity, plates with smaller diameter 1-D holes (and therefore a greater number of 1-D holes) will have a finer, more uniform current distribution on the wafer because there are more individual current sources acting as point sources that can spread across the same gap and also have a higher total pressure drop (higher viscous flow resistance).

[0297] In some cases, about 1 to 10 percent of the ion resistive element (1007) is an open area through which ion current can pass (and through which electrolyte can pass, provided there are no other elements blocking the openings). In certain embodiments, about 2 to 5 percent of the ion resistive element (1007) is an open area. In a specific example, the open area of ​​the ion resistive element (1007) is about 3.2 percent, and the effective total open cross-sectional area is about 23 cm². In some embodiments, the non-communication holes formed in the ion resistive element (1007) have a diameter of about 0.01 to 0.08 inches. In some cases, the holes have a diameter of about 0.02 to 0.03 inches, or about 0.03 to 0.06 inches. In various embodiments, the holes have a diameter that is up to about 0.2 times the gap distance between the ion-resistant element (1007) and the wafer. The holes generally have a circular cross-section, but are not necessarily so. Additionally, to facilitate configuration, all holes in the ion-resistant element (1007) may have the same diameter. However, this is not necessarily true, and both the individual size and local density of the holes may vary across the surface of the ion-resistant element as specific requirements dictate.

[0298] The ion-resistant element (1007) illustrated in FIG. 10 includes a series of linear ribs (1015) extending in and out of the page. The ribs (1015) are sometimes referred to as protrusions. The ribs (1015) are positioned on the top surface of the ion-resistant element (1007), and in many cases, the ribs are oriented such that their length (e.g., the longest dimension) is perpendicular to the direction of the inter-flowing electrolyte. In a specific embodiment, the ribs (1015) may be oriented such that their length is parallel to the direction of the inter-flowing electrolyte. The ribs (1015) influence fluid flow and current distribution within the cross-flow manifold (1010). For example, the cross-flow of the electrolyte is largely confined to the area above the top surface of the ribs (1015), and this area generates a high rate of electrolyte cross-flow. In the regions between adjacent ribs (1015), the current transmitted upward through the ion-resistant element (1007) is redistributed and becomes more uniform before being transmitted to the substrate surface.

[0299] In FIG. 10, the direction of the cross-flowing electrolyte is from left to right (e.g., from the side inlet (1013) to the side outlet (1014), and the ribs (1015) are oriented so that their lengths extend in / out of the page. In certain embodiments, the ribs (1015) may have a width of about 0.5 mm to 1.5 mm, or about 0.25 mm to 10 mm (measured from left to right in FIG. 10). The ribs (1015) may have a height of about 1.5 mm to 3.0 mm, or about 0.25 mm to 7.0 mm (measured from top to bottom in FIG. 10). The ribs (1015) may have a height-to-width aspect ratio (height / width) of about 1 / 5 to 1 / 2, or about 1 / 7 to 1 / 7. The ribs (1015) may have a pitch of about 10 mm to 30 mm, or about 5 mm to 150 mm. The ribs (1015) may have variable lengths (measured within / outside the page in FIG. 10) extending across the surface of the ion-resistant element (1007). The distance between the upper surface of the ribs (1015) and the surface of the substrate (1002) may be about 1 mm to 4 mm, or about 0.5 mm to 15 mm. The ribs (1015) may be provided on an area that occupies approximately the same space as the substrate, as shown in FIG. 10. The channels / openings of the ion-resistant element (1007) may be positioned between adjacent ribs (1015) or may extend through the ribs (1015) (i.e., the ribs (1015) may or may not be channeled). In some other embodiments, the ion-resistant element (1007) may have a flat top surface (e.g., not including the ribs (1015)).The electroplating apparatus illustrated in FIG. 10, comprising an ion-resistant element having ribs on the upper part, is further discussed in U.S. Patent No. 9,523,155, titled “ENHANCEMENT OF ELECTROLYTE HYDRODYNAMICS FOR EFFICIENT MASS TRANSFER,” which is incorporated herein by reference in its entirety.

[0300] The device may include various additional elements as needed for a specific application. In some cases, edge flow elements may be provided at the periphery of the substrate within a cross-flow manifold. Edge flow elements may be formed and positioned near the edges of the substrate to facilitate higher-order electrolyte flow (e.g., cross-flow). In certain embodiments, edge flow elements may be ring-shaped or arc-shaped, and may be uniform or non-uniform in azimuth. Edge flow elements are further discussed in U.S. Patent Application No. 14 / 924,124, titled “EDGE FLOW ELEMENT FOR ELECTROPLATING APPARATUS,” filed October 27, 2015, granted by U.S. Patent No. 10,094,034, the entirety of which is incorporated herein by reference.

[0301] In some cases, the device may include a sealing member for temporarily sealing a cross-flow manifold. The sealing member may be ring-shaped or arc-shaped and may be positioned close to the edges of the cross-flow manifold. A ring-shaped sealing member may seal the entire cross-flow manifold, while an arc-shaped sealing member may seal a portion of the cross-flow manifold (leaving the side outlets open in some cases). During electroplating, the sealing member may be repeatedly engaged and disengaged to seal and unseal the cross-flow manifold. The sealing member may be engaged and disengaged by moving a substrate holder, an ion-resistant element, a front insert, or other part of the device engaging with the sealing member. Sealing members and methods for controlling cross-flow are further discussed in the following U.S. patent applications, each of which is incorporated herein by reference in its entirety: U.S. Patent Application No. 15 / 225,716, filed August 1, 2016, granted as U.S. Patent No. 10,364,505, titled “DYNAMIC MODULATION OF CROSS FLOW MANIFOLD DURING ELECTROPLATING”; and U.S. Patent Application No. 15 / 161,081, filed May 20, 2016, granted as U.S. Patent No. 10,233,556, titled “DYNAMIC MODULATION OF CROSS FLOW MANIFOLD DURING ELECTROPLATING”.

[0302] In various embodiments, one or more electrolyte jets may be provided to deliver additional electrolyte over an ion-resistant element. The electrolyte jets may deliver the electrolyte near the periphery of the substrate, or at a location closer to the center of the substrate, or both. The electrolyte jets may be oriented at any position and may deliver an inter-flowing electrolyte, an impacting electrolyte, or a combination thereof. Electrolyte jets are further described in U.S. Patent Application No. 15 / 455,011, filed March 9, 2017, titled “ELECTROPLATING APPARATUS AND METHODS UTILIZING INDEPENDENT CONTROL OF IMPINGING ELECTROLYTE” and published as U.S. Patent Application Publication No. 2018 / 0258546, the entirety of which is incorporated herein by reference.

[0303] The described SRP removal processes may be implemented in a chamber that may be part of a substrate processing system. The substrate processing system may further include one or more additional substrate processing tools used to process substrates, including the deposition of SRPs and upstream and downstream processing. Referring now to FIG. 11, the substrate processing system (1100) includes one or more substrate processing tools (1102) (substrate processing tools (1102a and 1102b) are shown for illustrative purposes) and a substrate buffer (1130) or other substrate storage unit. Each of the substrate processing tools (1102a and 1102b) includes a plurality of processing chambers (1104a, 1104b, 1104c, etc.) (collectively, processing chambers (1104)). Only, for example, each of the processing chambers (1104) may be configured to perform substrate processing. In some examples, substrates may be loaded into one of the processing chambers (1104), processed, and then moved to one or more other chambers of the processing chambers (1104) and / or removed from the substrate processing tool (1100) (e.g., if all perform the same processing).

[0304] The substrates to be processed are loaded into the substrate processing tools (1102a and 1102b) through the ports of the loading station of the ATV (atmospheric-to-vacuum) transfer module (1108). In some examples, the ATV transfer module (1108) includes an EFEM (equipment front end module). The substrates are then transferred to one or more of the processing chambers (1104). For example, a transfer robot (1112) is configured to transfer the substrates from the loading stations (1116) to the load locks (1120). A vacuum transfer robot (1124) of the vacuum transfer module (1128) is configured to transfer the substrates from the load locks (1120) to the various processing chambers (1104).

[0305] After processing one or more of the substrate processing tools (1102a and 1102b), the substrates may be transferred out of the vacuum atmosphere. For example, the substrates may be moved to a storage location (such as a substrate buffer (1130)). In other examples, the substrates may be moved directly from a substrate processing tool to another substrate processing tool for further processing, or from a storage buffer (1130) to another substrate processing tool for further processing.

[0306] Exposure of metal feature(s) or substrate to ambient conditions may cause defects or otherwise have a negative impact on downstream processing. A sacrificial capping layer containing SRP may be applied to the metal feature(s) or substrate before exposure to ambient conditions. In some examples, the sacrificial capping layer is applied to a substrate processing tool before transferring the substrate to a substrate buffer for storage or, for example, to another substrate processing tool for thermal compression bonding. In other examples, the sacrificial capping layer is applied to another processing chamber (not associated with the substrate processing tool).

[0307] Before performing another process on the substrate (e.g., before bonding metal features), the sacrificial capping layer is removed as described herein. For example, the substrate may be transferred to the substrate processing tool (1102b) after a storage period in the storage buffer (1130) or after processing in the substrate processing tool (1102a). The sacrificial capping layer may be removed in one of the processing chambers in the substrate processing tool (1102b) or in another processing chamber (not associated with the substrate processing tool (1102b)). In some embodiments, the sacrificial capping layer is removed from the load lock (1120).

[0308] In some examples, the sacrificial capping layer is applied by a processing chamber within the same substrate processing tool (performing electroplating or substrate processing) prior to exposure to atmospheric conditions. Since the substrate processing tool operates under vacuum, the substrate's exposure to atmospheric conditions is prevented. In some examples, the sacrificial layer is deposited after a wet cleaning process or a plasma treatment process. In this case, oxides and residues may be removed by the wet cleaning process or the plasma treatment process, and the sacrificial capping layer is deposited sequentially before or immediately after drying the wafer. In some examples, this process is not performed under vacuum and is carried out without any exposure of the dry and pristine surface to the atmosphere. In other examples, the substrate is transferred from the substrate processing tool to another processing chamber located outside the substrate processing tool to apply the sacrificial capping layer. Using this approach limits or reduces the duration of the substrate's exposure to atmospheric conditions. Exposure is limited to a short transfer period from the substrate processing tool to the processing chamber where the sacrificial capping layer is applied. Storage of the substrate may be performed for longer periods without additional exposure to ambient conditions.

[0309] Subsequently, the sacrificial capping layer may be removed before further processing. In some examples, the sacrificial capping layer is removed from another substrate processing tool under vacuum conditions before substrate processing in the processing chambers of the same substrate processing tool. In other examples, the substrate is transferred to a processing chamber to remove the sacrificial capping layer and then transferred to the substrate processing tool for further processing. This approach also limits exposure to atmospheric conditions between the processing chamber and the substrate processing tool or other atmosphere. In one example, the sacrificial capping layer is formed immediately after etching, deposition, or other processes by exposing the substrate to small molecule vapors that condense on the surface to form a film. This can be performed immediately inside the tool where the etching or deposition occurred (e.g., substrate processing tool (1102a)) and may also occur in the same processing chamber where the etching or deposition occurred. The substrate is then taken to the next tool (e.g., substrate processing tool (1102b)) for processing. Once the substrate is no longer exposed to atmospheric conditions (e.g., by bringing the substrate under vacuum or atmospheric purging with an inert gas), vacuum and compounds, and in some cases, other stimuli as described above, are applied to induce a film to degrade the substrate and are removed from the substrate. This may occur inside a processing chamber (e.g., the process chamber (1104a) of the substrate processing chamber (1102b)) as described above.

[0310] The metal-to-metal bonding processes described herein may be implemented in a bonding chamber that may be part of a substrate processing system. Alternatively, a metal-to-metal bonding tool may be positioned in proximity to a processing chamber for SRP removal, where transfer passages, transfer chambers, and / or handling robots coordinate the movement of the wafer from the SRP removal chamber to the bonding tool. The bonding tool or chamber may be configured to provide the bonding temperature or bonding pressure described herein. Non-limiting bonding tools and chambers may be thermal compression bonding tools or other bonding platforms, such as EV Group (EV Group Europe & Asia / Pacific GmbH, Sankt Florian am Inn, Austria). ® 500 Series Bonding Module, S This includes the XBS200 platform or SB6 / 8 Gen2 platform from SS MicroTec SE (Garching, Germany), the Esec series for die bonding and the Datacon series for die attachment (e.g., Datacon 8800 TC) from BE Semiconductor Industries NV (Duiven, Netherlands), and the Fineplacer series for bonding from Finetech GmbH & Co. KG (Berlin, Germany).

[0311] In various embodiments, a system controller is employed to control process conditions during processing, including during SRP removal and / or metal bonding formation. The controller will typically include one or more memory devices and one or more processors. The processor may include a CPU or computer, analog input / output connections and / or digital input / output connections, stepper motor controller boards, etc.

[0312] The controller may also control all activities of the removal device. The system controller executes system control software that includes sets of instructions for controlling timing, mixture of gases, chamber pressure, chamber temperature, wafer temperature, wafer chuck or pedestal position, plasma power, and other parameters of a specific process. In some embodiments, other computer programs stored on memory devices associated with the controller may be employed.

[0313] Typically, there will be a user interface associated with the controller. The user interface may include display screens, graphic software displays of device and / or process conditions, and user input devices such as pointing devices, keyboards, touch screens, microphones, etc.

[0314] System control logic may be configured in any suitable manner. Generally, the logic may be configured or designed in hardware and / or software. Instructions for controlling the driving circuit may be hard-coded or provided as software. Instructions may also be provided by "programming." Such programming is understood to include any form of logic, including hard-coded logic on digital signal processors, application-specific integrated circuits, and other devices having specific algorithms implemented as hardware. Programming is also understood to include software or firmware instructions that may be executed on a general-purpose processor. System control software may be coded in any suitable computer-readable programming language.

[0315] Computer program code for controlling reactant pulses, purge gas flows, and other processes in a process sequence may be written in any conventional computer-readable programming language: for example, assembly language, C, C++, Pascal, Fortran, or other languages. Compiled object code or scripts are executed by a processor to perform tasks identified in the program. Also, as indicated, the program code may be hardcoded.

[0316] Controller parameters relate to process conditions, such as process gas composition and flow rates, temperature, pressure, substrate temperature, and plasma power. These parameters may be entered using a user interface or provided to the user in the form of a recipe.

[0317] Signals for monitoring the process may be provided by the analog input connections and / or digital input connections of the system controller. Signals for controlling the process are output on the analog output connections and digital output connections of the system.

[0318] System software can be designed or configured in many ways.

[0319] For example, various chamber component subroutines or control objects may be written to control the operation of chamber components necessary to perform deposition processes according to the disclosed embodiments. Examples of programs or sections of programs for this purpose include substrate positioning code, process gas control code, pressure control code, and heater control code.

[0320] FIG. 12 illustrates an example of a deposition chamber (for vapor-based deposition, such as for SRP, for example). As can be seen, an apparatus (1200) having a processing chamber (1202) including a lead (1208) is illustrated. The processing chamber (1202), on which a substrate (1222) may be placed on a wafer support (1224), may include a wafer transfer passage (1204) through one of the walls of the processing chamber (1202) sized to allow the substrate (1222) to pass through and enter the interior of the processing chamber (1202). The wafer transfer passage (1204) may have a gate valve (1206) or a similar door mechanism that may be operated to seal or unseal the wafer transfer passage, thereby isolating the atmosphere inside the processing chamber (1202) from the atmosphere on the other side of the gate valve (1206). For example, substrates (1222) may be provided to the processing chamber (1202) via a wafer handling robot located within an adjacent transfer chamber. This transfer chamber may, for example, have a plurality of processing chambers (1202) arranged around the periphery, and each of these processing chambers (1202) is connected to the transfer chamber through a corresponding gate valve (1206).

[0321] The wafer support (1224) may include an electrostatic chuck (ESC) (1226) that may be used to provide a wafer support surface to support a substrate (1222), for example. The ESC (1226) may include a base plate (1234) that is bonded to a top plate (1228) that is placed on top of a base plate (1234), for example. The top plate (1228) may be made of a ceramic material, for example, and may have several other components embedded therein. In the illustrated example, the top plate (1228) has two separate electrical systems embedded therein. One of these systems is an electrostatic clamping electrode system that may have one or more clamping electrodes (1232) that may be used to generate an electric charge within the substrate (1222) so that the substrate (1222) is pulled out against the wafer support surface of the top plate (1228). In the embodiment of FIG. 12, there are two clamping electrodes (1232) providing a bipolar electrostatic clamping system, but some embodiments may use only a single clamping electrode (1232) to provide a unipolar electrostatic clamping system.

[0322] Another system is a thermal control system that may be used to control the temperature of the substrate (1222) during processing conditions. In FIG. 12, the thermal control system is a multi-zone thermal control system featuring four annular resistance heater traces (1230a, 1230b, 1230c, and 1230d) that are concentric with each other and positioned under clamping electrodes (1232). The central resistance heater traces (1230a) may, in some embodiments, generally fill a circular area, and each of the resistance heater traces (1230a / 1230b / 1230c / 1230d) may generally follow a serpentine path or otherwise a meander path within the corresponding annular area. Each of the resistance heater traces (1230a, 1230b, 1230c, and 1230d) may be individually controlled to provide various radial heating profiles within the top plate (1228); in some cases, this 4-zone heating system may be controlled to maintain the substrate (1222) with, for example, a temperature uniformity of ± 0.5 °C. The device (1200) of FIG. 12 features a 4-zone heating system within the ESC (1226), but other embodiments may use single-zone or multi-zone heating systems having more or fewer than four zones.

[0323] For example, in some implementations of the temperature control mechanisms discussed above, heat pumps may be used instead of resistance heating traces. For example, in some implementations, resistance heater traces may be replaced or augmented by Peltier junctions or other similar devices that may be controlled to "pump" heat from one side to another. These mechanisms may be used, for example, to draw heat from the top plate (1228) (and thus the substrate (1222)) and direct the heat into the base plate (1234) and heat exchange passages (1236), thereby allowing the substrate (1222) to be cooled more quickly and effectively if desired.

[0324] The ESC (1226) may also include a base plate (1234) which may be used to provide structural support to the underside of the top plate (1228), for example, and may also function as a heat dissipation system. For example, the base plate (1234) may include one or more heat exchange passages (1236) arranged in a generally distributed manner throughout the base plate (1234), for example, the heat exchange passages (1236) may follow a meandering, circular switchback, or spiral pattern around the center of the base plate (1234). A heat exchange medium, for example, water or an inert fluorinated liquid, may be circulated through the heat exchange passages (1236) during use. The flow rate and temperature of the heat exchange medium may be externally controlled to produce a specific heating or cooling behavior in the base plate (1234).

[0325] The ESC (1226) may be supported, for example, by a wafer support housing (1242) that is connected to and supported by the wafer support column (1244). The wafer support column (1244) may have routing passages (1248) other than other pass-throughs for routing cabling, fluid flow conduits, and other equipment to, for example, the underside of the base plate (1234) and / or the top plate (1228). For example, although not shown in FIG. 12, cabling for providing power to resistance heater traces (1230a / 1230b / 1230c / 1230d) may be routed through the routing passages (1248), just as cabling for providing power to clamping electrodes (1232) may be routed. Other cables, for example, cables for temperature sensors, may also be routed through routing channels (1248) to locations inside the wafer support (1224). In embodiments using a temperature-controllable base plate (1234), conduits for transferring a heat exchange medium to and from the base plate (1234) may also be routed through routing channels (1248). To avoid excessive clutter, these cables and conduits are not shown in FIG. 12, but it should be understood that they will nevertheless be present.

[0326] The device (1200) of FIG. 12 also includes a wafer support z-actuator (1246) that may provide a movable support to the wafer support column (1244). The wafer support z-actuator (1246) may be actuated to cause the wafer support column (1244) and the wafer support (1224) supported by it to move vertically up or down, for example, by several inches, within the reaction space (1220) of the processing chamber (1202). In doing so, the gap distance X between the substrate (1222) and the underside of the showerhead (1210) may be tuned according to various process conditions.

[0327] The wafer support (1224) may also include one or more edge rings that, in some embodiments, may be used to control and / or fine-tune various process conditions. In FIG. 12, for example, an upper edge ring (1238) is provided that rests on the top of the lower edge rings (1240a and 1240b), which is ultimately supported by the wafer support housing (1242) and the third lower edge ring (1240c). The upper edge ring (1238) may generally undergo the same processing atmosphere as the substrate (1222), while the lower edge rings (1240a / 1240b / 1240c) may generally be shielded from the processing atmosphere. Due to the increased exposure of the upper edge ring (1238), the upper edge ring (1238) may have a limited lifespan and may require more frequent replacement or cleaning compared to the lower edge rings (1240a / 1240b / 1240c).

[0328] The device (1200) may also include a system for removing process gases from the processing chamber (1202) during and after the processing is finished. For example, the processing chamber (1202) may include an annular plenum (1256) surrounding a wafer support column (1244). The annular plenum (1256) may eventually be fluidly connected to a vacuum foreline (1252) which may be connected to a vacuum pump, such as being located under a subfloor below the device (1200), for example. A regulator valve (1254) may be provided between the vacuum foreline (1252) and the processing chamber (1202) and may be operated to control the flow into the vacuum foreline (1252). In some embodiments, a baffle (1250), e.g., an annular plate or other structure, which may function to create a flow into an annular plenum (1256) that is more evenly distributed around the circumference of the wafer support column (1244), may be provided to reduce the chance of flow non-uniformity occurring in the reaction materials flowing across the substrate (1222).

[0329] As illustrated, the showerhead (1210) is a dual-plenum showerhead (1210) and includes a first plenum (1212) to which process gas is supplied through a first inlet (1216) and a second plenum (1214) to which process gas is supplied through a second inlet (1218). In some embodiments, the showerhead (1210) may have one plenum or more than two plenums. In some embodiments, a single plenum is used to deliver precursor(s) into the reaction space (1220) of the processing chamber (1202). Each plenum may have a corresponding set of gas distribution ports that fluidly connect the reaction space (1220) and each plenum through a facing plate of the showerhead (1210) (the facing plate is a part of the showerhead (1210) interposed between the bottom plenum and the reaction space (1220)).

[0330] The first inlet (1216) and the second inlet (1218) of the showerhead (1210) may be configured to provide one or more SRPs, as discussed in this specification, and processing gases may be provided through a gas supply system.

[0331] The first valve manifold (1268a) may be configured to provide one or more SRPs to the first inlet (1216), while the second valve manifold (1268b) may be configured to provide other SRPs or other reactive materials to the second inlet (1218). In this example, the first valve manifold (1268a) includes, for example, a plurality of valves (A1 to A5). Valve A2 may be a three-way valve having, for example, one port fluidically connected to the first vaporizer (1272a), another port fluidly connected to the bypass line (1270a), and a third port fluidly connected to a port on another three-way valve A3. Similarly, valve A4 may be another 3-way valve having one port fluidically connected to the second vaporizer (1272b), another port fluidly connected to the bypass line (1270a), and a third port fluidly connected to a port on another 3-way valve A5. One of the other ports on valve A5 may be fluidly connected to the first inlet (1216), while the remaining port on valve A5 may be fluidly connected to one of the remaining ports on valve A3. The remaining port on valve A3 may eventually be fluidly connected to valve A1, which may be fluidly interposed between valve A3 and a purge gas source (1274), e.g. nitrogen, argon, or other suitably inert gas (for SRPs). In some embodiments, only the first valve manifold is employed.

[0332] For the purposes of the present disclosure, the term “fluidically connected” is used for volumes, plenums, holes, etc., which may be connected to one another to form a fluid connection, similar to how the term “electrically connected” is used for components connected together to form an electrical connection. The term “fluidically interposed” may, if used, be used to refer to a component, volume, plenum, or hole that is fluidly connected to at least two other components, volumes, plenums, or holes, so that a fluid flowing from one of these other components, volumes, plenums, or holes to another of these components, volumes, plenums, or holes will first flow through the “fluidly interposed” component before reaching the other of these components, volumes, plenums, or holes. For example, if a pump is fluidly interposed between the reservoir and the outlet, the fluid flowing from the reservoir to the outlet will first flow through the pump before reaching the outlet.

[0333] The first valve manifold (1268a) may be controllable to allow vapors from one or both of the vaporizers (1272a and 1272b), for example, to flow into the processing chamber (1202) or through the first bypass line (1270a) and into the vacuum foreline (1252). The first valve manifold (1268a) may also be controllable to allow purge gas to flow from the purge gas source (1274) into the first inlet (1216).

[0334] For example, to flow steam from the first vaporizer (1272a) into the reaction space (1220), valve A2 may be operated to allow steam from the first vaporizer (1272a) to first flow into the first bypass line (1270a). This flow may be maintained for a sufficient period of time to allow the steam flow to reach steady-state flow conditions. After a sufficient period of time has elapsed (or, if used, after a flow meter indicates that the flow rate is stable), valves (A2, A3, and A5) may be operated to direct the steam flow from the first vaporizer (1272a) toward the first inlet. Similar operations using valves (A4 and A5) may be performed to deliver steam from the second vaporizer (1272b) to the first inlet (1216). In some examples, it may be desirable to purge one of the vapors from the first plenum (1212) by operating valves (A1, A3, and A5) so that purge gas from the purge gas source (1274) flows into the first inlet (1216). In some additional embodiments, it may be desirable to simultaneously flow vapor from one of the vaporizers (1272a or 1272b) in tandem with flowing gas from the purge gas into the first inlet (1216). These embodiments may be used to dilute the concentration of the reactant(s) contained in these vapor(s).

[0335] It will be understood that the second valve manifold (1268b) may be controlled in a similar manner, for example, by controlling the valves (B1 to B5) to provide vapors from the vaporizers (1272c and 1272d) to the second inlet (1218) or the second bypass line (1270b). It will also be recognized that different manifold arrangements may also be utilized, including a single unitary manifold comprising valves for controlling the flow of SRPs, or other reactive materials, to the first inlet (1216) and the second inlet (1218).

[0336] As previously mentioned, some devices (1200) may feature fewer steam sources, for example, only two vaporizers (1272), and in this case, the valve manifold(s) (1268) may be modified to have fewer valves, for example, only valves (A1 to A3).

[0337] As discussed above, devices such as device (1200) that may be used to provide dry deposition of SRP films may be configured to maintain specific temperature profiles within a processing chamber (1202). In particular, these devices (1200) may be configured to maintain the substrate (1222) at a temperature lower than most of the equipment of device (1202) that comes into direct contact with the SRP(s), for example, at least 25°C to 50°C lower. Additionally, the temperature of the equipment of device (1200) that comes into direct contact with the SRP(s) may be maintained at a sufficiently high elevated level that prevents the condensation of vaporized reactive materials on the surfaces of such equipment. At the same time, the temperature of the substrate (1222) may be controlled to a level that promotes the condensation, or at least deposition, of reactive materials on the substrate (1222).

[0338] To provide such temperature control, various heating systems may be included in the device (1200). For example, the processing chamber (1202) may have receptacles for receiving cartridge heaters (1258), and for example, for a processing chamber (1202) that generally has a cylindrical internal volume but has a square or rectangular external shape, vertical holes for receiving cartridge heaters (1258) may be bore into the four corners of the chamber (1202) housing. In some embodiments, the showerhead (1210) may be covered with heater blankets (1260) that may be used to apply heat across the exposed upper surface of the showerhead (1210) to maintain an elevated showerhead temperature. It may also be advantageous to heat the various gas lines used to conduct vaporized reactive materials from the vaporizers (1272) to the showerhead (1210). For example, a resistive heater tape may be wound around these gas lines to heat them to an elevated temperature. As illustrated in FIG. 12, all gas lines potentially having SRP(s) flowing through them are shown as being heated, including bypass lines (1270). The only exceptions are the gas lines from the valve manifolds (1268) to the first inlet (1216) and the second inlet (1218), which may be very short and may be heated indirectly by the showerhead (1210). Of course, even these gas lines may be actively heated if desired. In some embodiments, heaters may also be provided near the gate valve (1206) to provide heat to the gate valve.

[0339] Various operating systems of the device (1200) may be controlled by a controller (1284), and the controller (1284) may include one or more processors (1286) and one or more memory devices (1288) which are operably connected to each other and communically connected to various systems and subsystems of the device (1200) to provide control functions for these systems. For example, the controller (1284) may be configured to control valves (A1 to A5 and B1 to B5), various heaters (1258, 1260), vaporizers (1272), regulator valve (1254), gate valve (1206), wafer support z-actuator, etc.

[0340] Another feature that the device (1200) may include is illustrated in FIG. 13, and enlarged side and top views of a portion of the substrate (1222), top plate (1228), and upper edge ring (1238) of FIG. 12 are shown. As can be seen, in some embodiments, the substrate (1222) may be raised from most of the top plate (1228) by a plurality of small mesas (1276) which may be shallow bosses protruding a small distance from the nominal upper surface of the top plate (1228) to provide a back gap (1278) between the bottom surface of the substrate (1222) and most of the top plate (1228). A circumferential wall feature (1277) may be provided at the periphery of the top plate (1228). The cylindrical wall feature (1277) may extend around the entire periphery of the top plate (1228) and may be nominally the same height as the mesa (1276). During processing operations, an inert gas, such as helium, may flow into the back gap (1278) through one or more gas ports (1282). This gas may then flow radially outward before encountering the cylindrical wall feature (1277), which may then restrict this radially outward flow and cause a higher pressure region of the gas to be trapped between the substrate (1222) and the top plate (1228). Inert gas leaking through the cylindrical wall (1277) may eventually flow through the radial gap (1280) between the outer edge of the substrate (1222) and a portion of the upper edge ring (1238). This gas may function to protect the bottom of the substrate from being undesirably affected by processing operations to be performed by acting to prevent gases released by the showerhead (1210) from reaching the bottom surface of the substrate (1222).At the same time, the gas released into the back gap (1278) region may also act to increase the thermal coupling between the substrate (1222) and the top plate (1228), thereby causing the top plate (1228) to heat or cool the substrate (1222) more effectively. Due to the higher pressure provided by the cylindrical wall, the gas within the back gap (1278) region may also have a higher density than the gas in the rest of the chamber, and thus may provide more effective thermal coupling between the substrate (1222) and the top plate (1228).

[0341] The controller (1284) may be configured to cause the device (1200) to perform various operations consistent with the provided initiation, for example, through the execution of computer-executable instructions.

[0342] Once the SRP layer is deposited on the substrate (1222), the substrate (1222) may be transferred to one or more subsequent processing chambers or tools for additional operations (e.g., any operations described herein). Additional deposition apparatuses are described in International Patent Application No. PCT / US2020 / 038968, filed June 22, 2020, titled “APPARATUS FOR PHOTORESIST DRY DEPOSITION,” which is incorporated herein by reference in its entirety.

[0343] Solvent-based deposition or liquid-based deposition may employ a device having a liquid dispensing system and a heater. FIG. 14 illustrates an example of a device in which a rotating chuck (10) is designed to hold and rotate a wafer (W) of a predetermined diameter, e.g., 300 mm or 450 mm. In this embodiment, the wafer (W) is held by a series of six circular gripping pins (16). The pins (16) pass through openings within a transparent plate (25) made of quartz or sapphire. The plate (25) is secured to the chuck (10) by screws (26) and rotates together with the chuck (10). When the wafer (W) is positioned on the chuck, it is held on the plate (25) such that the lower surface of the wafer is parallel to the plate (25) and spaced apart by a small gap.

[0344] A radiant heating assembly (50) is mounted under a transparent plate (25), which will be described in more detail below.

[0345] Adjacent to the chuck (10), a boom swing arm (30) is mounted to pivot around a drive motor (34). Process and / or rinse liquid is supplied to the arm (30) and discharged downward through a discharge nozzle (32). The boom swing arm (30) is movable between the standby position shown by the solid line in FIG. 14 and the center position shown by the dashed line. Thus, the discharge nozzle (32) can scan over the entire radius of the wafer (W) and, when the wafer (W) is rotated by the chuck (10), accordingly dispenses liquid onto the entire upward facing surface.

[0346] Now, referring to FIG. 15, it can be seen that the rotating chuck (10) is composed of a lower chuck body (12) and an upper chuck body (14) that are fixed to each other and journaled for rotation around a fixed center post (20). The pins (16) and the transparent plate (25) also rotate with the chuck (10) in this embodiment, such as a ring gear (18) that meshes continuously with each of the gripping pins (16) through the gear teeth provided on the bases of the chuck (10). The ring gear (18) can also rotate to a limited degree with respect to the chuck (10), thereby rotating the pins (16) around their respective axes and moving the uppermost eccentric gripping portions between an open position and a closed position in a manner known in itself.

[0347] A fixed post (20), such as a stator (44), is mounted on the machine frame (40) of the device, while a rotor (42) is fixed to a lower chuck body (12) which constitutes a magnetic motor that rotates the chuck (10). Further details of the entire chuck structure are described, for example, in the jointly owned U.S. Patent No. 9,245,777.

[0348] In this embodiment, the radiant heating assembly (50) is mounted on a fixed post (20) and thus does not rotate, but is enveloped by a rotating structure of a chuck comprising elements (25, 14, 16). In this embodiment, the radiant heating assembly (50) includes a plurality of blue light-emitting diodes (LEDs) (51) mounted facing a transparent plate (25), and a controller (52) (e.g., an onboard controller (not shown) mounted on the underside of the heating assembly (50)). The controller (52) controls the turn-on and turn-off of the blue LEDs (51), as well as the power, and also communicates wirelessly with the motor (34) of the boom swing arm (30).

[0349] As illustrated in FIG. 16, the radiant heating assembly (50) is composed of an aluminum substrate consisting of an upper piece and a lower piece (54 and 55) that are brazed together, and the aluminum substrate acts as a heat sink to prevent excessive heating of the structure under the blue LED elements (51). A printed circuit board (PCB) (53) is mounted on top of the upper piece (54), traces for the LED elements are formed on the upper piece (54), and the LED elements (51) are mounted.

[0350] Onboard chips (56) are mounted on a printed circuit board (60) fixed to the underside of the lower piece (55). Wires (58) interconnecting the output pins of the onboard chips (56) and the input terminals of the traces formed on the PCB (53) are accommodated in pockets (57) passing through the aluminum substrate (53, 54).

[0351] As illustrated in FIG. 17, the PCB (53) of this embodiment is formed into four quadrants joined together by connectors (59). The LED elements (51) are formed into 16 groups, that is, the arrangement of onboard chips (56) and the connections from these chips to the PCB (53) together with the onboard controller (52) allow the LEDs to be powered individually into 16 small groups.

[0352] As can be seen in FIG. 17, the LEDs (51) are arranged in 20 concentric circles, and the number of LEDs in each circle is a multiple of 16. Thus, each concentric circle can be individually controlled as a separate heating zone by the arrangement described above.

[0353] The blue LED lamps (51) have a maximum intensity at a wavelength of about 450 nm. Other radiation sources may be used, but it is preferable to use sources that emit radiation having a maximum intensity in a wavelength range of 390 nm to 550 nm and more preferably in a wavelength range of 400 nm to 500 nm.

[0354] While radiation of wavelength characteristics is largely transmitted by the plate (25), the same radiation is largely absorbed by the semiconductor material of the wafer (W), especially when the wafer (W) is silicon.

[0355] This arrangement allows for very rapid localized heating of the wafer (W) in a manner that causes the rinsing liquid to evaporate before a damaging meniscus has a chance to form. For example, each LED (51) may have a power consumption of 10 W and provide 3 W of photovoltaic power, and photovoltaic power can be generated almost instantaneously. Additionally, less photovoltaic power can be generated for the selected LEDs (51) when desired, for example, by pulsing the power supply to the selected LEDs (51) at 500 Hz in a self-known manner.

[0356] FIGS. 18 and 19 illustrate an alternative embodiment in which a magnetic ring rotor (70) is positioned within a closed chamber (80) and rotated by a stator (72) positioned outside the chamber (80). A wafer (W) is held by gripping elements (71) protruding downward from the ring rotor (70).

[0357] The chamber (80) can be opened for loading and removing the wafer (W) as shown in FIG. 19. The heating assembly (50') is integrated into the lower part of the housing (80) and is similar to that described in relation to the previous embodiment, except that in this embodiment, the transparent plate (25') is fixed and does not rotate with the magnetic rotor (70).

[0358] Furthermore, in this embodiment, instead of a radially movable liquid dispenser (30), a series of fixed liquid dispensing nozzles (74) fed by a manifold (73) are provided. Rinse liquid can be supplied in series to these nozzles (74), starting from the center and continuing to the periphery, to approximate the dispensing action of the boom swing arm (30) of the preceding embodiments. Thus, in this case, the controller (52) will control the power supply to a selected group of LEDs (51) based on the liquid being dispensed by the nozzles (74). Additional devices and components are described in U.S. Patent No. 10,720,343, titled “METHOD AND APPARATUS FOR PROCESSING WAFER-SHAPED ARTICLES,” which is incorporated herein by reference in its entirety.

[0359] In some embodiments, the controller is part of a system that may be any part of the examples described above. Such systems may include semiconductor processing equipment, including processing tools or tools, chambers or chambers, a platform for processing or platforms and / or specific processing components (wafer pedestals, gas flow systems, etc.). These systems may be integrated with electronic devices to control their operation before, during, and after the processing of a semiconductor wafer or substrate. An electronic device may be referred to as a “controller” capable of controlling the system or various components or sub-parts of the systems. Depending on the processing requirements and / or type of the system, the controller may be programmed to control any of the processes disclosed herein, including the delivery of processing gases, temperature settings (e.g., heating and / or cooling), pressure settings, vacuum settings, power settings, flow rate settings, fluid delivery settings, position and operation settings, tools and other transfer tools and / or wafer transfer into and out of load locks connected to or interfacing with a specific system.

[0360] Generally speaking, a controller may be defined as an electronic device having various integrated circuits, logic, memory, and / or software that receives instructions, issues instructions, controls operations, enables cleaning operations, enables endpoint measurements, etc. Integrated circuits may include chips in the form of firmware that store program instructions, digital signal processors (DSPs), chips defined as ASICs (Application Specific Integrated Circuits), and / or one or more microprocessors or microcontrollers that execute program instructions (e.g., software). Program instructions may be instructions that communicate with the controller or the system in the form of various individual settings (or program files) that define operation parameters for performing a specific process on or for a semiconductor wafer. In some embodiments, the operation parameters may be part of a recipe defined by process engineers to achieve one or more processing steps during the manufacture of one or more layers, materials, metals, oxides, silicon, silicon dioxide, surfaces, circuits and / or wafer dies.

[0361] In some implementation examples, the controller may be integrated with the system, coupled to the system, otherwise networked to the system, or coupled to or part of a computer that is a combination of these. For example, the controller may be all or part of a fab host computer system capable of enabling remote access to wafer processing, or it may be located within the "cloud." The computer may enable remote access to the system to monitor the current progress of manufacturing operations, examine the history of past manufacturing operations, examine trends or performance measurements from multiple manufacturing operations, change parameters of the current processing, set processing steps following the current processing, or start a new process. In some examples, a remote computer (e.g., a server) may provide process recipes to the system over a network, which may include a local network or the Internet. The remote computer may include a user interface that enables the input or programming of parameters and / or settings to be subsequently transmitted from the remote computer to the system. In some examples, the controller receives instructions in the form of data that specify parameters for each of the processing steps to be performed during one or more operations. The parameters may be specific to the type of tool configured to be controlled or interfaced by the controller and the type of process to be performed. Accordingly, as described above, the controller may be distributed by including one or more individual controllers that are networked and operate together toward a common purpose, such as the processes and controls described herein, for example. An example of a distributed controller for such purposes would be one or more integrated circuits on a chamber that communicate with one or more integrated circuits located remotely (e.g., at the platform level or as part of a remote computer) to be combined to control a process on the chamber.

[0362] Exemplary systems may include, without limitation, a plasma etching chamber or module, a deposition chamber or module, a spin-rinse chamber or module, a metal plating chamber or module, a cleaning chamber or module, a bevel edge etching chamber or module, a physical vapor deposition (PVD) chamber or module, a chemical vapor deposition (CVD) chamber or module, an atomic layer deposition (ALD) chamber or module, an atomic layer etch (ALE) chamber or module, an ion implantation chamber or module, a track chamber or module, and any other semiconductor processing systems that may be used or associated in the manufacture and / or fabrication of semiconductor wafers.

[0363] As described above, depending on the process steps or steps to be performed by the tool, the controller may communicate with one or more of other tool circuits or modules, other tool components, cluster tools, other tool interfaces, adjacent tools, neighboring tools, tools located throughout the factory, a main computer, another controller, or tools used in material transfer for moving containers of wafers from / to / from tool locations and / or load ports within the semiconductor manufacturing plant.

[0364] The controller may include various programs. A substrate positioning program may include program code for controlling chamber components used to load the substrate onto a pedestal or chuck and to control the spacing between the substrate and other parts of the chamber, such as the gas inlet and / or target. A process gas control program may include code for controlling gas composition, flow rates, and pulse times, and for selectively flowing gas into the chamber. A pressure control program may include code for controlling the pressure in the chamber, for example, by adjusting a throttle valve of the chamber's exhaust system. A heater control program may include code for controlling the current to a heating unit used to heat the substrate. Alternatively, a heater control program may control the delivery of a heat transfer gas, such as helium, to the wafer chuck. A plasma power program may control the plasma power.

[0365] Examples of chamber sensors that may be monitored during removal include mass flow controllers, pressure sensors such as manometers, and thermocouples located on the pedestal or chuck. Appropriately programmed feedback and control algorithms may be used with data from these sensors to maintain targeted process conditions.

[0366] The foregoing describes examples of implementations of the disclosed embodiments of single or multi-chamber semiconductor processing tools. The apparatus and processes described herein may be used in conjunction with lithographic patterning tools or processes for the manufacture or fabrication of, for example, semiconductor devices, displays, LEDs, photoelectric panels, etc. Typically, but not necessarily, these tools / processes will be used or performed together in a common manufacturing facility. Lithographic patterning of a film typically comprises the following steps, each of which is provided using a plurality of possible tools: (1) applying a photoresist onto a workpiece, i.e., a substrate, using a spin-on tool or a spray-on tool; (2) curing the photoresist using a hot plate, a furnace, or a UV curing tool; (3) exposing the photoresist to visible light, UV, or X-ray light using a tool such as a wafer stepper; (4) a step of developing the resist to pattern the resist by selectively removing the resist using a tool such as a wet bench; (5) a step of transferring the resist pattern into the underlying film or workpiece by using a dry or plasma-assisted etching tool; and (6) some or all of the step of removing the resist using a tool such as an RF or microwave plasma resist stripper, and each step is enabled with a number of possible tools.

[0367] conclusion

[0368] Although the foregoing embodiments have been described in some detail for the sake of clarity of understanding, it will be apparent that specific variations and modifications may be made within the scope of the appended claims. The embodiments disclosed herein may be made without some or all of these specific details. In other examples, known process operations have not been described in detail so as not to unnecessarily obscure the disclosed embodiments. Furthermore, it will be understood that while the disclosed embodiments will be described together with specific embodiments, specific embodiments are not intended to limit the disclosed embodiments. It should be noted that there are many alternative ways to implement the processes, systems, and devices of the embodiments. Accordingly, the embodiments are to be considered exemplary and non-limiting, and the embodiments are not to be limited to the details given herein.

Claims

Claim 1 A method comprising: a step of aligning a first capped feature with a second capped feature, wherein each of the first capped feature and the second capped feature independently comprises a stimulus-responsive polymer (SRP) layer disposed on the surface of a metal feature; and a step of bonding the first capped feature and the second capped feature in an atmosphere that removes the SRP and forms a metal-metal bond between the metal features. Claim 2 A method according to claim 1, wherein the SRP layer prevents oxidation of the metal feature. Claim 3 A method according to claim 1, wherein the bonding step comprises: the step of exposing the first capped feature and the second capped feature to a removal temperature for removing the SRP, thereby providing the exposed metal features; and the step of contacting the exposed metal features to form the metal-metal bond. Claim 4 In claim 3, the exposing step comprises the use of acidic vapor, heat, extreme ultraviolet (EUV) light or ultraviolet (UV) light or vacuum ultraviolet light, plasma, metastable neutrons from noble gas plasma, or a combination thereof. Claim 5 A method according to claim 1, wherein the bonding step comprises the use of an inert atmosphere, a vacuum atmosphere, a reducing gas, or ambient air. Claim 6 A method according to claim 1, wherein the metal feature comprises copper (Cu), tin (Sn), silver (Ag), gold (Au), aluminum (Al), or alloys thereof. Claim 7 A method according to claim 1, further comprising, prior to the alignment step, (i) a step of depositing a first SRP layer on the surface of a first metal feature, wherein the deposition provides a first capped feature; and (ii) a step of depositing a second SRP layer on the surface of a second metal feature, wherein the deposition provides a second capped feature. Claim 8 In claim 7, the method wherein the first SRP layer is further disposed on the surface of the gap-filling layer surrounding the first metal feature. Claim 9 In claim 8, the method wherein the second SRP layer is further disposed on the surface of the gap-filling layer surrounding the second metal feature. Claim 10 A method according to claim 7, further comprising the step of pretreating the surfaces of the first metal feature and the second metal feature to perform at least one of the steps of cleaning the surface and removing the oxide layer before the deposition step in at least one of the steps (i) and (ii). Claim 11 In claim 7, the deposition step in step (i) and / or step (ii) comprises vapor-based or solvent-based deposition of the SRP. Claim 12 A method comprising the step of depositing SRP to form an SRP layer on the surface of a first metal feature including an electrical contact, wherein the deposition provides a first capped feature. Claim 13 A method according to claim 12, further comprising: a step of removing the SRP layer to provide a first exposed metal feature after the deposition step; and a step of contacting the first exposed metal feature to a second exposed metal feature to form a metal-metal bond between the exposed metal features. Claim 14 In claim 12, the deposition step comprises vapor-based or solvent-based deposition of the SRP. Claim 15 A method according to claim 12, wherein the removing step comprises exposing the SRP layer to heat, extreme ultraviolet light or ultraviolet light or vacuum ultraviolet light, metastable neutrons from a noble gas plasma, acidic vapor, or basic vapor. Claim 16 In claim 12, the method wherein the SRP layer prevents oxidation of the first metal feature. Claim 17 In claim 12, the method wherein the SRP layer has a thickness of 10 nm to 10 μm. Claim 18 A method according to claim 13, further comprising the step of depositing an SRP to form an SRP layer on the surface of the second metal feature, wherein the deposition provides a second capped feature; and the step of removing the SRP layer from the second capped feature to provide a second exposed metal feature. Claim 19 A method according to claim 18, further comprising: a step of removing the SRP layer from the second capped feature to provide an exposed metal feature; and a step of bonding the exposed first metal feature and the exposed second metal feature, wherein the bonding forms a metal-metal bond. Claim 20 In claim 12, the method wherein the electrical contact comprises a raised metal pillar, a bonding pad, a bump, a microbump, a metal contact surrounded by a dielectric, or an interconnect. Claim 21 A method comprising: a step of depositing an SRP to form an SRP layer on the surface of a first metal feature and a second metal feature, wherein the deposition provides a first capped feature and a second capped feature; a step of aligning the first capped feature with the second capped feature; a step of removing the SRP layer to provide exposed metal features; and a step of contacting the exposed metal features to form a metal-metal bond between the exposed metal features. Claim 22 In claim 21, the method further comprises an acid catalyst, an organic acid, a photoacid generator, or a thermal acid generator. Claim 23 A method according to any one of claims 1 to 21, wherein the SRP further comprises a metal-bonded moiety. Claim 24 In any one of claims 1 to 21, the SRP is a chemical formula ( I ) to chemical formula ( XIII ): , , , , , , , , , , , , It comprises one of the structures, or a salt thereof, wherein each R1 is independently H, optionally substituted alkyl, optionally substituted alkoxy, optionally substituted alkenyl, optionally substituted aryl, or halo; and R2, R 2' , R 2" , and R3 are each independently H, optionally substituted alkyl, optionally substituted heteroalkyl, or optionally substituted aryl; R4, R 4' , and R 4" Each is independently H, an optionally substituted alkyl, an optionally substituted aminoalkyl, an optionally substituted heteroalkyl, or R 4' , and R 4" Each is taken together with an attached nitrogen atom to form a heterocyclyl group as defined herein; Ar is an optionally substituted aryl, an optionally substituted alkyl, or an optionally substituted aralkyl; L1 and L2 are each independently covalently bonded and are an optionally substituted alkylene, an optionally substituted heteroalkylene, an optionally substituted arylene, or an optionally substituted cycloalkylene; Z1 and Z2 are each independently -O-, -S-, -CR2R3O-, -OCR2R3O-, -OCR2R3-, -CR2R3S-, -SCR2R3S-, or -SCR2R3-; r1 is an integer from 1 to 4; and n is from 3 to 100,000; the SRP comprises a linear polymer or a cyclic polymer; and R1, R2, R 2' , R 2'' , R3, R4, R 4' , R 4'' A method in which at least one of Ar, L1, L2, Z1, or Z2 may optionally further comprise a metal-bonding moiety. Claim 25 In any one of claims 1 to 21, the SRP is a chemical formula ( Ia The structure of ), or comprising a salt thereof, wherein each R1 is independently H, optionally substituted alkyl, optionally substituted alkoxy, optionally substituted alkenyl, optionally substituted aryl, or halo; and R2 and R 2" Each is independently H, optionally substituted alkyl, or optionally substituted aryl; r1 is an integer from 1 to 4; and n is from 4 to 100,000; and the SRP comprises a linear polymer or a cyclic polymer, a method. Claim 26 In any one of claims 1 to 21, the SRP is a chemical formula ( Ib The structure of ), or comprising a salt thereof, wherein R1, R5, and R6 are each independently H, optionally substituted alkyl, optionally substituted alkoxy, optionally substituted alkenyl, optionally substituted aryl, or halo; R 2' , R 2" , R 3' , R 3" , R 4' , and R 4" Each is independently H, optionally substituted alkyl, or optionally substituted aryl; Z1, Z2, Z3, Z4, Z5, and Z6 are each independently -O-, -S-, -CR2R3O-, -OCR2R3O-, -OCR2R3-, -CR2R3S-, -SCR2R3S-, or -SCR2R3-, and R2 and R3 are each independently H, optionally substituted alkyl, or optionally substituted aryl; r1, r5, and r6 are each independently integers from 1 to 4; and n1 is 1 to 100, method.

Citation Information

Patent Citations

  • Method of manufacturing semiconductor-element mounting substrate, and the semiconductor-element mounting substrate

    JP2007251009A

  • Electric connection structure and electric connection member

    JP2016157660A

  • Chip connector

    KR1020110132485A

  • Signal-responsive plastics

    US20140242623A1

  • Self-immolative polymers, articles thereof, and methods of making and using same

    US20180155483A1