Separation method of palladium and platinum metal by using sulfuric acid solutions containing oxidizing agents
The method using sulfuric acid and sodium hypochlorite or sodium chlorate effectively separates palladium and platinum metals, enhancing efficiency and reducing energy requirements in the separation process.
Patent Information
- Application Number
- KR1020240161737
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-11-14
- Publication Date
- 2026-11-06
- Estimated Expiration
- 2044-11-14
AI Technical Summary
Existing methods for separating palladium and platinum metals are inefficient and require additional separation processes, such as solvent extraction and ion exchange, which are energy-intensive and costly.
A method using a mixed solution of sulfuric acid and sodium hypochlorite or sodium chlorate to selectively dissolve and separate palladium and platinum metals, optimizing concentrations and conditions for efficient separation without organic solvents.
Achieves high separation efficiency of palladium and platinum metals, eliminating the need for additional separation processes and reducing energy consumption.
Smart Images

Figure 112024125262031-PAT00002_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a method for separating palladium (Pd) and platinum (Pt) metals by selective dissolution using a sulfuric acid solution containing an oxidizing agent. Background Technology
[0003] Platinum group metals, particularly palladium (Pd) and platinum (Pt), are essential in catalysts, chemical engineering, automotive exhaust gas treatment, and the manufacture of high-grade materials due to their high catalytic activity, electrical conductivity, and corrosion resistance. However, platinum group metal ores are concentrated in specific regions such as South Africa and Russia and generally exist at low concentrations of 2 to 10 mg / L.
[0004] Dry smelting and wet smelting methods are used to recover palladium (Pd) and platinum (Pt). Wet smelting has the advantage of reducing process energy because it is a low-temperature process and offers a high purification yield.
[0005] However, in recovering platinum group metals through a wet process, generally, after dissolving the platinum group metals through a leaching process, separation processes such as solvent extraction, ion exchange, and fractional precipitation are carried out. Prior art literature
[0007] Republic of Korea Published Patent Application No. 2023-0131356 The problem to be solved
[0008] The present invention provides a method for separating palladium (Pd) and platinum (Pt) with excellent efficiency by controlling the leaching process.
[0009] The problems that the present invention aims to solve are not limited to those mentioned above, and other unmentioned problems will be clearly understood by those skilled in the art from the description below. means of solving the problem
[0011] To solve the above problem, the present invention provides a method for separating palladium and platinum metal according to (1) to (10) below.
[0012] (1) A method for separating palladium and platinum metals by selectively dissolving and separating palladium from platinum through a process of leaching a material containing palladium and platinum using a leaching solution.
[0013] (2) A method for separating palladium and platinum metals, wherein the leaching solution in (1) is a mixed solution of sulfuric acid (H2SO4) and sodium hypochlorite (NaClO).
[0014] (3) A method for separating palladium and platinum metals, wherein the leaching solution in (1) is a mixed solution of sulfuric acid (H2SO4) and sodium chlorate (NaClO3).
[0015] (4) A method for separating palladium and platinum metals according to (2), wherein in the above mixed solution, the concentration of sulfuric acid (H2SO4) is 3 M or more and the concentration of sodium hypochlorite (NaClO) is 0.15 M or more.
[0016] (5) A method for separating palladium and platinum metals, wherein, in (4), the density of the liquid leaching is 6 g / L or less.
[0017] (6) A method for separating palladium and platinum metals according to (3), wherein in the above mixed solution, the concentration of sulfuric acid (H2SO4) is 4 to 6 M and the concentration of sodium chlorate (NaClO3) is 0.35 M or more. Effects of the invention
[0019] According to the method of the present invention, a method using a selective solvent method combining an acid such as hydrochloric acid or sulfuric acid with a strong oxidizing agent such as sodium chlorate and sodium hypochlorite can separate and recover palladium and platinum without a separate separation process using an organic solvent.
[0020] The effects of the present invention are not limited to those mentioned above, and other unmentioned effects will be clearly understood by a person skilled in the art from the description below. Brief explanation of the drawing
[0022] Figure 1 shows the effect of sulfuric acid concentration on the leaching of palladium (Pd) and platinum (Pt) when NaClO3 is used as an oxidizing agent. Figure 2 shows the effect of sulfuric acid concentration on the leaching of palladium (Pd) and platinum (Pt) when NaClO is used as an oxidizing agent. Figure 3 shows the effect of sulfuric acid concentration on the leaching of palladium (Pd) and platinum (Pt) when H2O2 is used as an oxidizing agent. Figure 4 shows the effect of NaClO concentration on the leaching rate of palladium (Pd) and platinum (Pt). Figure 5 shows the effect of NaClO3 concentration on the leaching rate of palladium (Pd) and platinum (Pt). Figure 6 shows the effect of slurry density on the leaching rate of palladium (Pd) and platinum (Pt). Figure 7 shows the effect of hydrochloric acid concentration on the leaching of platinum (Pt) using H2O2. Figure 8 shows the effect of hydrochloric acid concentration on the leaching of platinum (Pt) using NaClO. Figure 9 shows the effect of hydrochloric acid concentration on the leaching of platinum (Pt) using NaClO3. Figure 10 shows the effect of NaClO3 concentration on the leaching rate of platinum (Pt). Figure 11 shows the effect of reaction temperature on the leaching of platinum (Pt). Specific details for implementing the invention
[0023] Embodiments of the present invention are described below with reference to the attached drawings so that those skilled in the art can easily implement them. However, the present invention may be embodied in various different forms and is not limited to the embodiments described herein.
[0024] In addition, to clearly explain the present invention in the drawings, parts unrelated to the explanation have been omitted, and similar parts throughout the specification have been given similar reference numerals.
[0025] Throughout this specification, when a part is described as "comprising" a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but may include additional components.
[0026] As used herein, terms of degree such as “about,” “substantially,” etc., are used to mean at or near the stated value when inherent manufacturing and material tolerances are presented in the stated meaning, and are used to prevent unscrupulous infringers from unfairly exploiting the disclosure in which precise or absolute values are mentioned to aid in understanding the invention. Furthermore, throughout this specification, “a step of” or “a step of” does not mean “a step for”.
[0027] Throughout this specification, the term “combination thereof” included in a Markush-style expression means one or more mixtures or combinations selected from the group consisting of components described in the Markush-style expression, and means including one or more selected from the group consisting of said components. Throughout this specification, the description “A and / or B” means “A or B, or A and B”.
[0029] <Example>
[0030] In experiments to simulate the method of the present invention, palladium (Pd, particle size 60 mesh, Alfa Aesar, Ward Hill, USA, 99.8%) and platinum (Pt, particle size 200 mesh, Sigma-Aldrich Co., 99.9%) metal powders were used. In all experiments, the weight ratio of platinum (Pt) to palladium (Pd) in the mixture was kept constant. Sulfuric acid solution (H2SO4, Daejeong Chemical & Metal Co., >95%, Korea) and hydrochloric acid solution (HCl, Daejeong Chemical & Metal Co., 35%) were diluted with secondary distilled water and used at the desired concentration. Hydrogen peroxide (H2O2, Daejeong Chemical & Metal Co., 30%), sodium hypochlorite (NaClO, Daejeong Chemical & Metal Co., >8%), and sodium chlorate (NaClO 3, Daejeong Chemical Metals Co. was used as an oxidizing agent in leaching experiments.
[0031] The leaching experiment of palladium (Pd) and platinum (Pt) was performed in a 250 mL three-necked flask. During this process, the reaction temperature and stirring speed were controlled using a magnetic heating stirrer (WiseStir MSH-20D, Daehan Science). After reaching the set temperature, a certain amount of the mixture of the two metals was added to the three-necked flask. Subsequently, an oxidizing agent was slowly added to the flask to suppress the occurrence of a vigorous reaction. A lid was used on the flask to prevent the evaporation loss of the reactants. Once the reaction was complete, the solution and insoluble residue were separated using filter paper (ADVANTEC NO.2, 110 mm, Toyo Roshi Kaisha, Ltd.).
[0032] The concentration of metal ions in the leaching solution was measured by ICP-OES, and the leaching rate (%L) was calculated using the following [Equation 1].
[0033] [Equation 1]
[0034] %L = m ii / m i x 100%
[0035] (here, here m i and mii represents the initial mass of the metal and the leached dissolved metal mass in the metal mixture, respectively.
[0037] The influence of oxidizing agent types on the selective leaching of palladium (Pd)
[0038] Palladium (Pd) and platinum (Pt) are chemically very stable and have low reactivity, making them difficult to leach without pretreatment. Therefore, the effects of mixed acids and oxidizing agents were investigated to promote the leaching of palladium (Pd) and platinum (Pt). To consider the effects of oxidizing agent characteristics and sulfuric acid concentration on the dissolution efficiency of palladium (Pd) and platinum (Pt), three oxidizing agents (H2O 2, The leaching rates were compared by adding NaClO and NaClO3 to a sulfuric acid solution. At this time, the sulfuric acid concentration was adjusted to 1 to 9 M, the slurry density was fixed at 2 g / L, the process was carried out at 20°C for 60 minutes, and the oxidizing agent concentration was maintained at 0.4 M.
[0039] Figure 1 shows the effect of sulfuric acid concentration on the leaching of palladium (Pd) and platinum (Pt) when NaClO3 is used as an oxidizing agent, Figure 2 shows the effect of sulfuric acid concentration on the leaching of palladium (Pd) and platinum (Pt) when NaClO is used as an oxidizing agent, and Figure 3 shows the effect of sulfuric acid concentration on the leaching of palladium (Pd) and platinum (Pt) when H2O2 is used as an oxidizing agent. Referring to Figures 1 to 3, the leaching rate of palladium (Pd) by NaClO and NaClO3 was much higher than that of H2O2.
[0040] Specifically, the leaching rate of palladium (Pd) using NaClO3 increased significantly as the sulfuric acid concentration increased, rising from 8.4% at 1 M to a maximum of 99.6% at 5 M. However, as the sulfuric acid concentration increased to 9 M, the leaching rate decreased sharply to 22.2%. Therefore, when using NaClO3 as an oxidizing agent, a sulfuric acid concentration of 4 to 6 M is preferable, and 4.5 to 5.5 M is more preferable.
[0041] In addition, the leaching rate of palladium (Pd) using NaClO increased from 84.6% to 99.9% as the sulfuric acid concentration increased from 1 M to 5 M, and remained constant even when the sulfuric acid concentration increased to 9 M. Therefore, when using NaClO as an oxidizing agent, the concentration of sulfuric acid can be 3 M or higher, preferably 4 M or higher, more preferably 4.5 M or higher, and most preferably 5 M or higher, and it is desirable to keep it 9 M or lower when considering the amount of oxidizing agent used.
[0042] Meanwhile, the leaching of palladium (Pd) using H2O2 remained consistently low, and even at a sulfuric acid concentration of 9 M, the leaching rate of palladium (Pd) was only 2.41%, indicating that there was almost no leaching effect.
[0043] Under the three leaching conditions described above, the leaching rate of platinum (Pt) was close to 0%. In other words, when NaClO or NaClO3 is mixed with sulfuric acid (H2SO4) as an oxidizing agent, separation of palladium (Pd) from platinum (Pt) by selective dissolution is possible. Furthermore, it can be seen that NaClO is more preferable as an oxidizing agent than NaClO3.
[0045] Effect of Oxidizing Agent Concentration on the Selective Leaching of Palladium (Pd)
[0046] The effect of oxidizing agent concentration on the selective leaching of palladium (Pd) was investigated by varying the concentrations of NaClO and NaClO3 from 0.1 M to 0.5 M. Leaching was performed under conditions of 5 M sulfuric acid, a slurry density of 2 g / L, 20 ℃, and 500 rpm for 60 minutes.
[0047] Figure 4 shows the effect of NaClO concentration on the leaching rate of palladium (Pd) and platinum (Pt), and Figure 5 shows the effect of NaClO3 concentration on the leaching rate of palladium (Pd) and platinum (Pt).
[0048] Referring to Figures 4 and 5, as the concentration of NaClO increased from 0.1 M to 0.2 M, the leaching rate of palladium (Pd) increased from 45.9% to 99.9%, and the leaching rate remained constant even when the concentration was increased to 0.5 M. Therefore, when using NaClO as an oxidizing agent, the concentration of NaClO is preferably 0.15 M or higher, more preferably 0.2 M or higher, and, considering the amount of oxidizing agent used, it is preferable to have a concentration of 0.5 M or lower.
[0049] In addition, as the concentration of NaClO3 increased from 0.1 M to 0.5 M, the leaching rate of palladium (Pd) increased from 16.3% to 99.9%. When using NaClO3 as an oxidizing agent, the concentration of NaClO3 is preferably 0.35 M or higher, more preferably 0.4 M or higher, and considering the amount of oxidizing agent used, it is preferable that the concentration be 0.5 M or lower.
[0050] Meanwhile, under the above leaching conditions, the dissolution of platinum (Pt) was minimal.
[0052] Effect of slurry density on the selective leaching of palladium (Pd)
[0053] The effect of slurry density on the leaching of palladium (Pd) was investigated by varying the slurry density from 1 g / L to 20 g / L. Leaching was performed using 5 M sulfuric acid and 0.2 M NaClO at 20 ℃ for 60 minutes at 500 rpm.
[0054] Figure 6 shows the effect of slurry density on the leaching rate of palladium (Pd) and platinum (Pt). Referring to Figure 6, all palladium (Pd) metal dissolved when the pulp density increased from 1 g / L to 5 g / L, but the leaching rate decreased to 36.1% when it increased to 20 g / L. Furthermore, under these leaching conditions, the dissolution of platinum (Pt) was negligible. Therefore, a slurry density of 6 g / L or less is desirable, 5.5 g / L or less is more desirable, and 5 g / L or less is most desirable.
[0055] The decrease in the leaching rate of palladium (Pd) under conditions of high slurry density may be due to an insufficient amount of oxidizing agent required for the complete dissolution of palladium (Pd) metal. Additionally, it is attributed to a decrease in the mass transfer rate of reactants involved in the leaching reaction to the particle surfaces, as the liquid flow resistance to the particles increases proportionally to the slurry density.
[0056] From the above results, it can be seen that palladium (Pd) metal can be selectively separated from platinum (Pt) metal through selective dissolution using a mixture of sulfuric acid and sodium hypochlorite. The preferred leaching conditions are as follows.
[0057] Under these conditions, palladium (Pd) metal could be completely dissolved, and the leaching rate of platinum (Pt) metal was close to 0%.
[0059] Effect of hydrochloric acid concentration on the leaching of platinum (Pt) metal
[0060] In general, the formation of complexes during the oxidative leaching process promotes the leaching of platinum (Pt) metal because platinum (Pt) metal can form stable complexes with chloride ion ligands. This characteristic indicates that hydrochloric acid is a suitable solvent for the leaching of platinum (Pt) metal. Due to the high reduction potential of platinum (Pt)(IV), oxidizing agents such as H2O2, NaClO, and NaClO₃ were used. Leaching was carried out at 60 °C for 60 minutes with a slurry density of 1 g / L and a stirring speed of 500 rpm, while adjusting the hydrochloric acid concentration from 1 M to 9 M. During this process, the concentrations of all three oxidizing agents were fixed at 0.4 M.
[0061] Figure 7 shows the effect of hydrochloric acid concentration on the leaching of platinum (Pt) using H2O2, Figure 8 shows the effect of hydrochloric acid concentration on the leaching of platinum (Pt) using NaClO, and Figure 9 shows the effect of hydrochloric acid concentration on the leaching of platinum (Pt) using NaClO3.
[0062] Referring to FIGS. 7 to 9, the leaching rate of platinum (Pt) varied depending on the oxidizing agent used. Specifically, the leaching rate of platinum (Pt) by NaClO3 increased significantly from 1.8% to 99.9% as the hydrochloric acid concentration increased from 1 M to 5 M, and remained constant even when the hydrochloric acid concentration increased to 9 M. Therefore, when using NaClO3 as an oxidizing agent, a hydrochloric acid concentration of 4 M or higher is preferable, 4.5 M or higher is more preferable, and 5 M or higher is most preferable. Additionally, considering the amount of hydrochloric acid used, a hydrochloric acid concentration of 9 M or lower is preferable.
[0063] Similarly, the leaching rate of platinum (Pt) using NaClO increased significantly from 1.7% to 99.9% as the hydrochloric acid concentration increased from 1 M to 7 M, and then remained constant up to 9 M. Therefore, when using NaClO as an oxidizing agent, a hydrochloric acid concentration of 6 M or higher is preferable, 6.5 M or higher is more preferable, and 7 M or higher is most preferable. In addition, considering the amount of hydrochloric acid used, a hydrochloric acid concentration of 9 M or lower is preferable.
[0064] In contrast, the platinum (Pt) leaching rate when H2O2 was used as an oxidizing agent was negligible even under the same conditions. Furthermore, considering the amount of hydrochloric acid used, it can be seen that NaClO3 is more preferable as an oxidizing agent for platinum (Pt) leaching.
[0065] Under conditions of high hydrochloric acid concentration, chloride ions can form stable platinum (Pt)-Cl complexes, which significantly promotes the leaching of platinum (Pt). NaClO and NaClO3 release additional chloride ions from the hydrochloric acid solution to aid in the formation of these complexes, thereby increasing the leaching rate of platinum (Pt). On the other hand, while H2O2 can react with hydrochloric acid to produce strong oxidizing agents such as HClO and Cl₂, its efficiency is low. At high temperatures, H2O2 readily decomposes into O2 and H2O, releasing dissolved oxygen, which can act as an oxidizing agent, into the atmosphere. This reduces the availability of HClO and Cl₂, the oxidizing agents required for platinum (Pt) oxidation; consequently, H2O2 fails to provide sufficient oxidative action for the dissolution of platinum (Pt), resulting in a platinum (Pt) leaching rate that is negligible compared to NaClO and NaClO3.
[0067] Effect of Oxidizer Concentration on Platinum (Pt) Metal Leaching
[0068] The concentration of NaClO3 was varied from 0.1 M to 0.5 M, and the concentration of hydrochloric acid was fixed at 5 M. Leaching was carried out at 60 ℃ for 60 minutes with a slurry density of 1 g / L and a stirring speed of 500 rpm.
[0069] Figure 10 shows the effect of NaClO3 concentration on the leaching rate of platinum (Pt). Referring to Figure 10, it shows that as the NaClO₃ concentration increases from 0.1 M to 0.3 M, the leaching rate of platinum (Pt) increases from 50.1% to 99.9%, and remains constant even when the concentration is further increased to 0.5 M. Therefore, when using NaClO3 as an oxidizing agent for platinum (Pt) leaching, a NaClO3 concentration of 0.25 M or higher is preferable, and 0.3 M or higher is more preferable. Additionally, in terms of the amount of oxidizing agent used, a NaClO3 concentration of 0.5 M or lower is preferable.
[0071] Effect of reaction temperature on the leaching of platinum (Pt) metal
[0072] To investigate the effect of temperature on leaching, experiments were conducted in a temperature range from 20 to 80°C. Leaching was carried out for 60 minutes with a slurry density of 1 g / L and a stirring speed of 500 rpm, at hydrochloric acid and NaClO3 concentrations of 5 M and 0.3 M, respectively.
[0073] Figure 11 shows the effect of reaction temperature on the leaching of platinum (Pt). Referring to Figure 11, it shows that the leaching rate of platinum (Pt) increased from 12.4% to 99.9% as the temperature increased from 20 to 60 ℃. However, when the temperature increased to 80 ℃, the leaching rate decreased slightly.
[0074] Therefore, when leaching platinum (Pt), the reaction temperature is preferably 50 to 90 ℃, more preferably 55 to 80 ℃, and most preferably 58 to 70 ℃.
Claims
Claim 1 A method for separating palladium and platinum metals by selectively dissolving and separating palladium from platinum through a process of leaching a material containing palladium and platinum using a leaching solution, wherein the leaching solution is an aqueous solution of sulfuric acid (H2SO4) and sodium hypochlorite (NaClO) that does not contain an organic solvent, wherein the concentration of the sulfuric acid (H2SO4) is 3 to 9 M and the concentration of the sodium hypochlorite (NaClO) is 0.15 to 0.5 M, and the density of the liquid in the leaching process is 6 g / L or less. Claim 2 A method for separating palladium and platinum metals according to claim 1, wherein the concentration of sodium hypochlorite (NaClO) is 0.3 to 0.5 M. Claim 3 A method for separating palladium and platinum metals according to claim 1, wherein in the leaching process, the leaching rate of palladium is 99% or more and the leaching rate of platinum is 1% or less. Claim 4 A method for separating palladium and platinum metals by selectively dissolving and separating palladium from platinum through a process of leaching a material containing palladium and platinum using a leaching solution, wherein the leaching solution is an aqueous solution of sulfuric acid (H2SO4) and sodium chlorate (NaClO3) that does not contain an organic solvent, the concentration of the sulfuric acid (H2SO4) is 4 to 6 M, and the concentration of the sodium chlorate (NaClO3) is 0.35 to 0.5 M. Claim 5 delete Claim 6 delete
Citation Information
Patent Citations
Method for leaching and recovering platinum group metals from organic solvents
KR1020230062828A
Methods for selective leaching and extraction of precious metals in organic solvents
US20220364201A1
Recovery of platinum-group metals from ores
US4337226A