Anode Material Coated with Metal Oxide and Secondary Battery using the Same

Coating silicon anode materials with lithium metal phosphate and carbon in secondary batteries addresses the issue of particle breakage and leaching by suppressing volume expansion, enhancing battery performance.

KR103045890B1Active Publication Date: 2026-11-06CHEONGJU UNIV IND & ACADEMY COOPERATION FOUND
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020230075249
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-06-13
Publication Date
2026-11-06
Estimated Expiration
2043-06-13

AI Technical Summary

Technical Problem

Silicon anode materials in secondary batteries experience rapid capacity decline due to particle breakage and leaching into the electrolyte caused by significant volume expansion during electrochemical reactions, limiting their electrochemical performance.

Method used

Coating silicon anode materials with a lithium metal phosphate having an olivine structure and a carbon layer to suppress volume expansion and enhance electrical conductivity.

Benefits of technology

The coating stabilizes the silicon anode, preventing particle breakage and leaching, thereby improving the lifespan, capacity, and stability of the secondary battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112023064585838-PAT00002_ABST
    Figure 112023064585838-PAT00002_ABST
Patent Text Reader

Abstract

This invention is a technology for improving the electrochemical properties of a cathode material that has high capacity but exhibits low electrochemical characteristics due to significant volume expansion during electrochemical reactions. This invention improves the electrochemical properties of a secondary battery by coating the active material of the cathode with an oxide to suppress volume expansion. The present invention was completed with research support from the Industry-Academic Cooperation Foundation of Cheongju University. The names of the research projects are "Support Project for Industry-Academic Convergence R&D in the 4th Year of the Chungbuk Eumseong Industry-Academic Convergence District Development Project" and "Basic Research Laboratory Project." The names of the research tasks are "Development of High-Performance Binders for Graphite-Silicon Composite Anode Materials" and "Development of Source Technology for Human-Wearable Stretchable Energy Self-Sufficient Devices." The project numbers are P0011933 and 2021R1A4A2001687.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] The present invention relates to a negative electrode material for a secondary battery. The present invention relates to a silicon (Si) negative electrode among the negative electrodes of a secondary battery. More specifically, the present invention relates to a technology for preventing the breakage of particles of the silicon negative electrode active material and the leaching of the silicon negative electrode active material into the electrolyte by causing the silicon negative electrode of the secondary battery to repeatedly expand and contract during an electrochemical reaction. The present invention relates to a technology for preventing the breakage of particles of the silicon negative electrode active material and the leaching of the silicon negative electrode active material into the electrolyte by coating the silicon negative electrode material with a metal oxide to prevent the silicon negative electrode material from expanding and contracting during an electrochemical reaction. Background Technology

[0002] The use of secondary batteries is increasing. As electronic devices using secondary batteries become increasingly smaller, lighter, and larger in capacity, interest in high-capacity, high-density secondary batteries is growing.

[0003] Commercially available rechargeable batteries generally consist of a carbon-based anode capable of lithium ion intercalation, a transition metal oxide-based cathode containing lithium, a liquid electrolyte composed of an organic solvent and a lithium salt, and a separator that prevents contact between the cathode and anode. During discharge, lithium ions de-intercalate from the anode and move to the cathode through the liquid electrolyte and separator, while electrons generated during the ionization of lithium ions also move from the anode to the cathode via an external circuit. The electrons moving from the anode to the cathode through the external circuit perform work on the external circuit. Conversely, during charging, lithium atoms in the cathode ionize into lithium ions and electrons; the lithium ions move to the anode through the liquid electrolyte and separator and are intercalated within the cathode, while electrons also move from the cathode to the anode via the external circuit. Rechargeable batteries generate and consume electrical energy by repeating these charging and discharging cycles. The capacity of the rechargeable battery is determined by the amount of lithium ions moving from the anode to the cathode or from the cathode to the anode.

[0004] The reaction in which lithium is added to the electrode active material during the charging and discharging of a secondary battery is called lithiation, and the reaction in which lithium is removed from the electrode active material is called delithiation.

[0005] Currently, graphite is primarily used as the anode material for secondary batteries. The theoretical capacity of graphite is 350 mAh / g. However, to increase energy density, there is growing interest in anode materials with high theoretical capacities, such as tin or silicon. The theoretical capacity of tin is 993 mAh / g, which is approximately three times that of graphite. The theoretical capacity of silicon is 4,200 mAh / g, which is more than 11 times that of graphite. Silicon also has advantages such as a low reaction potential for cathode materials, low toxicity, and low cost. However, during the electrochemical reaction of a secondary battery, as the cycle of lithium ions inserting into and extracting from silicon repeats, the silicon anode repeatedly expands and contracts. The volume expansion rate is over 300%. Consequently, silicon particles break and leach into the electrolyte, leading to a rapid decline in capacity after the initial few cycles. This process is illustrated in Figure 1. Therefore, silicon anode materials have low electrochemical performance. The problem to be solved

[0006] The problem that this invention aims to solve is to prevent the particles of the cathode material from breaking or leaching into the electrolyte by repeatedly expanding and contracting during the electrochemical reaction, even though silicon has a higher capacity than graphite. means of solving the problem

[0007] To solve the above problem, the present invention prevents particle breakage caused by volume expansion of the cathode material by coating a metal oxide onto a high-capacity cathode material. High-capacity cathode materials include alloy materials, transition metal oxides, transition metal chalgogenides, transition metal oxalates, transition metal carbides, transition metal nitrides, aluminum niobate, etc. Examples of alloy materials include Si and SiO2. Examples of transition metal oxides include Fe3O4. Examples of transition metal chalgogenides include FeS2. Examples of transition metal oxalates include ZnC2O4. Examples of transition metal carbides include Ti3C2Tx (where T is Zr, Nb, Mo, Ti, V, Cr, W, Mn, Ni, Co, Fe, or Cu, and x is 0). <x<1이다) 등이다. 전이 금속 질화물의 예는 CrN 등이다. 알루미늄 나이오베이트의 예는 TiNb2O7등이다.

[0008] More specifically, while continuing research to solve the above problem, the inventor of the present invention discovered a solution by coating a high-capacity cathode material that expands in volume during an electrochemical reaction with an olivine-structured lithium metal phosphate (LiMPO4, where M is Fe, Mn, Co, Ni, Al, or an alloy thereof). While continuing research to solve the above problem, the inventor of the present invention discovered a solution by coating a high-capacity cathode material that expands in volume during an electrochemical reaction with an olivine-structured lithium metal phosphate (LiMPO4, where M is Fe, Mn, Co, Ni, Al, or an alloy thereof) and applying a carbon coating thereon. When the cathode material is coated with lithium metal phosphate or coated with lithium metal phosphate and carbon in this way, the volume expansion of the cathode material is suppressed during the charging and discharging process of the secondary battery, so that the particles of the cathode material do not break. Effects of the invention

[0009] The present invention can improve the lifespan, capacity, and stability of a secondary battery by preventing particle breakage through coating a high-capacity cathode material to replace graphite, such as an alloy material, transition metal oxide, transition metal chalgogen compound, transition metal oxalate, transition metal carbide, transition metal nitride, aluminum niobate, etc., with lithium metal phosphate or by coating it with lithium metal phosphate and carbon. The present invention can suppress the volume expansion of silicon and improve the electrochemical properties of a secondary battery by coating the surface of a silicon cathode with a stable olivine-structured lithium iron phosphate oxide or a stable olivine-structured lithium iron phosphate oxide and carbon. Brief explanation of the drawing

[0010] Figure 1 illustrates the phenomenon in which the silicon anode expands as lithium ions are added to it during charging, and then contracts as lithium ions are removed from the silicon anode during discharging. When this charging and discharging cycle is repeated, the silicon anode particles break. Figure 2 illustrates how, by coating silicon particles with lithium metal phosphate, the silicon anode expands when lithium ions are added to the silicon anode during charging, and then contracts when lithium ions are removed from the silicon anode during discharging, so that the silicon anode particles do not break. Figure 3 illustrates a method of coating silicon particles with lithium metal phosphate and coating the lithium metal phosphate with carbon. Figure 4 shows the charge-discharge curves of a silicon cathode coated with LiFePO4 and a pure silicon cathode. Figure 5 is a graph of the lifespan of a secondary battery using a silicon anode coated with LiFePO4 and a pure silicon anode. Figure 6 is an SEM image of pure silicon cathode particles and silicon cathode particles coated with LiFePO4. Figure 7 shows the charge-discharge graph of a secondary battery using a pure MoS2 cathode and the charge-discharge graph of a secondary battery using a LiFePO4-coated MoS2 cathode. Figure 8 is an SEM image of MoS2 cathode particles coated with LiFePO4. Figure 9 shows the charge-discharge graph of a secondary battery using a pure Sn cathode and the charge-discharge graph of a secondary battery using a Sn cathode coated with LiFePO4. Figure 10 is a graph of the cycle life of a secondary battery using a Sn cathode coated with LiFePO4. Specific details for implementing the invention

[0011] One embodiment of the present invention is a cathode material in which a lithium metal phosphate with an olivine structure (LiMPO4, where M is Fe, Mn, Co, Ni, Al, or an alloy thereof) is coated on a cathode active material that undergoes volume expansion during an electrochemical reaction.

[0012] One embodiment of the present invention is a cathode material in which a lithium metal phosphate with an olivine structure (LiMPO4, where M is Fe, Mn, Co, Ni, Al, or an alloy thereof) and carbon are sequentially coated on a cathode active material that undergoes volume expansion during an electrochemical reaction.

[0013] One embodiment of the present invention is a cathode material in which the cathode active material is Si, SiOx (0.7≤x≤1.9), Sn, SnO2, MoS2, WS2, SnS2, FeS2, MnO2, Fe3O4, TiNb2O7, MnC2O4, or a mixture thereof.

[0014] One embodiment of the present invention is that the lithium metal phosphate having the olivine structure is LiFePO4, LiMnPO4, LiCoPO4, LiFe x Mn 1-x PO4(0 <x<1), LiFe x Mn y Co 1-x-y PO4(0 <x<1이고, 0<y<1이다) 또는 이들의 혼합물인 음극 소재이다.

[0015] One embodiment of the present invention is a cathode material in which the weight ratio of the lithium metal phosphate of the olivine structure is 2% to 20% by weight based on the total cathode material.

[0016] One embodiment of the present invention is a cathode material in which the weight ratio of the lithium metal phosphate of the olivine structure is 5% to 12% by weight based on the total cathode material.

[0017] One embodiment of the present invention is a cathode material in which the weight ratio of the lithium metal phosphate of the olivine structure is 3% to 20% by weight based on the total cathode material, and the weight ratio of the carbon is 1% to 10% by weight based on the total cathode material.

[0018] One embodiment of the present invention is a cathode material in which the weight ratio of the lithium metal phosphate of the olivine structure is 3% to 20% by weight based on the total cathode material, and the weight ratio of the carbon is 2% to 6% by weight based on the total cathode material.

[0019] One embodiment of the present invention is a secondary battery comprising a negative electrode material in which a negative electrode active material undergoing volume expansion during an electrochemical reaction is coated with a lithium metal phosphate having an olivine structure (LiMPO4, where M is Fe, Mn, Co, Ni, Al, or an alloy thereof).

[0020] One embodiment of the present invention is a secondary battery comprising a cathode material in which a lithium metal phosphate with an olivine structure (LiMPO4, where M is Fe, Mn, Co, Ni, Al or an alloy thereof) and carbon are sequentially coated on a cathode active material that undergoes volume expansion during an electrochemical reaction.

[0021] One embodiment of the present invention is a secondary battery comprising a negative electrode material in which the negative electrode active material is Si, SiOx (0.7≤x≤1.9), Sn, SnO2, MoS2, WS2, SnS2, FeS2, MnO2, Fe3O4, TiNb2O7, MnC2O4, or a mixture thereof.

[0022] One embodiment of the present invention is that the lithium metal phosphate having the olivine structure is LiFePO4, LiMnPO4, LiCoPO4, LiFe x Mn 1-x PO4(0 <x<1), LiFe x Mn y Co 1-x-y PO4(0 <x<1이고, 0<y<1이다) 또는 이들의 혼합물인 음극 소재를 포함하는 이차전지이다.

[0023] One embodiment of the present invention is a secondary battery comprising a negative electrode material in which the weight ratio of the lithium metal phosphate of the olivine structure is 2% to 20% by weight based on the total negative electrode material.

[0024] One embodiment of the present invention is a secondary battery comprising a negative electrode material in which the weight ratio of the lithium metal phosphate of the olivine structure is 5% to 12% by weight based on the total negative electrode material.

[0025] One embodiment of the present invention is a secondary battery comprising a negative electrode material in which the weight ratio of the lithium metal phosphate having an olivine structure is 3% to 20% by weight based on the total negative electrode material, and the weight ratio of the carbon is 1% to 10% by weight based on the total negative electrode material.

[0026] One embodiment of the present invention is a secondary battery comprising a negative electrode material in which the weight ratio of the lithium metal phosphate having an olivine structure is 3% to 20% by weight based on the total negative electrode material, and the weight ratio of the carbon is 2% to 6% by weight based on the total negative electrode material.

[0027] As a cathode material, Si, SiOx (0.7≤x≤1.9), Sn, SnO2, MoS2, WS2, SnS2, FeS2, MnO2, Fe3O4, TiNb2O7, MnC2O4, or a mixture thereof may be used.

[0028] To improve the stability of the cathode material, it is preferable to use LiMPO4 with an olivine structure (where M is Fe, Mn, Co, Ni, Al, or an alloy thereof) as the lithium metal phosphate coating the cathode material, considering the volume expansion or dissolution characteristics of the cathode material. More specifically, LiFePO4, LiMnPO4, LiCoPO4, and LiFe x Mn 1-x PO4(0 <x<1) 등을 사용할 수 있다.

[0029] The weight ratio of the olivine-structured lithium metal phosphate coating the cathode material may be 2% to 20% by weight. The weight ratio of the olivine-structured lithium metal phosphate coating the cathode material may preferably be 5% to 12% by weight.

[0030] A structure in which the cathode material is coated with lithium metal phosphate having an olivine structure and carbon sequentially coats the lithium metal phosphate having an olivine structure may be preferred. The weight ratio of carbon may be 1 weight% to 10 weight%. The weight ratio of carbon may be 2 weight% to 6 weight%.

[0031] Figure 3 illustrates an example of a method for preparing a negative electrode active material having a structure in which silicon is coated with LiFePO4 and carbon is coated over the LiFePO4. Silicon powder is mixed with distilled water, Li2CO3 (a raw material for LiFePO4), FeC2O4·2H2O, NH4H2PO4, and citric acid, and then mixed at 80°C for 12 hours to evaporate the solvent. The gel-like mixture obtained in this way is subjected to a first heat treatment at 300°C for 3 hours and a second heat treatment at 700°C for 10 hours to obtain silicon particles sequentially coated with LiFePO4 and carbon. At this time, silicon particles coated only with LiFePO4 without a carbon coating layer can be obtained by omitting citric acid. The heat treatment may be performed only once at 500°C to 800°C for 1 to 15 hours.

[0032] In a silicon anode material coated solely with LiFePO4, volume expansion is suppressed during the charge-discharge process, so silicon particles do not break and do not leach into the electrolyte. Thus, the characteristics of the secondary battery can be improved. The thickness of the LiFePO4 coating layer is preferably 15 nm to 1 nm, more preferably 8 nm to 1 nm, and most preferably 5 nm to 2 nm.

[0033] The carbon coating layer can improve electronic conductivity. The thickness of the carbon coating layer is preferably 5 nm to 0.1 nm, more preferably 3 nm to 0.2 nm, and most preferably 2 nm to 0.5 nm. Micropores may be formed between the LiFePO4 coating layer and the carbon coating layer. Micropores may be formed between silicon particles coated with LiFePO4 and a carbon layer coated on top thereof. The micropores may be continuous or discontinuous.

[0034] The carbon coating layer can be prepared by mixing or ball-milling at least one carbon-based material selected from Ketjen black, Denka black, acetylene black, Super-p, fullerene, single-wall carbon nanotubes (SWNT), multi-wall carbon nanotubes (MWNT), carbon nanofiber, graphene, graphene oxide, reduced graphene oxide, doped graphene, carbon nanoribbon, natural graphite, and artificial graphite with silicon particles coated with LiFePO4. Alternatively, citric acid, sugar, etc., can be mixed with silicon powder, Li2CO3, FeC2O, which are raw materials for LiFePO4. 4ㆍ It can also be made by mixing with 2H2O, NH4H2PO4, and distilled water, followed by heat treatment.

[0035] Heat treatment may be completed in a single step or divided into two steps. If heat treatment is performed in a single step, it may be carried out at a temperature in the range of 500 to 800°C for 1 to 15 hours using the sol-gel method or the solid-state method. It is preferable to perform the treatment at a temperature in the range of 500 to 800°C, and more preferable to perform it at a temperature in the range of 550 to 700°C. It is preferable to perform the heat treatment in the range of 1 to 15 hours, and more preferable to perform it in the range of 2 to 10 hours. If heat treatment is divided into two steps, the first heat treatment may be performed in argon or nitrogen at a temperature of 200°C to 500°C. It is preferable to perform it at a temperature of 250°C to 400°C. It is more preferable to perform it at a temperature of 280°C to 350°C. After the first heat treatment, a second heat treatment may be performed at a temperature of 500°C to 900°C. It is preferable to perform the process at a temperature of 550°C to 800°C. It is more preferable to perform the process at a temperature of 600°C to 750°C. After the first heat treatment, the temperature can be increased to the second heat treatment temperature at a rate of 5°C per minute.

[0036] The carbon coating layer can uniformly cover the surface of the LiFePO4 layer or non-uniformly cover at least a portion of the LiFePO4 surface. LiFePO4 not only suppresses the volume expansion of the anode material but also plays a role in transporting lithium ions to the anode material. However, LiFePO4 has low electrical conductivity. Therefore, it may be beneficial to coat LiFePO4 with carbon, which has good electrical conductivity, to improve electrical conductivity. The LiFePO4 layer can also be coated with materials other than carbon, provided that electrical conductivity can be improved without hindering the transport of lithium ions.

[0037] A carbon coating layer containing micropores can increase the surface electrical conductivity of silicon particles to improve the high-rate characteristics of a secondary battery, form a buffer layer that suppresses volume expansion occurring during the charging and discharging of silicon, and form a stable solid electrolyte interface layer (SEI layer) on the surface of the negative electrode active material for a secondary battery.

[0038] Silicon particles coated with a highly conductive carbon layer containing micropores and a lithium metal phosphate layer can have a high electrical conductivity of 10 S / cm or more.

[0039] Examples

[0040] Example 1

[0041] Example 1 involved 100 g of pure silicon particles with 2.3 g of Li2CO3 and FeC2O, which are raw materials for LiFePO4. 4ㆍ 11.3 g of 2H2O, 7.2 g of NH4H2PO4, and 1.25 g of citric acid (6 wt% relative to the total amount of raw materials of LiFePO4) were added to 0.5 liters of distilled water and mixed for 6 hours. The distilled water was dried at 80°C for 3 hours, and then the distilled water was completely evaporated at 85°C for 2 hours. A gel-like mixed particle was obtained. A first heat treatment was performed at 300°C for 3 hours under an argon atmosphere. The product from the first heat treatment was subjected to a second heat treatment at 700°C for 10 hours. After the first heat treatment, the temperature was raised to the temperature for the second heat treatment at a rate of 5°C per minute. In this way, the final product, Si particles coated with 10 wt% LiFePO4 and 2 wt% carbon, was obtained. The citric acid was converted into carbon and coated onto the LiFePO4.

[0042] A secondary battery of Example 1 was prepared by making a negative electrode with a silicon negative electrode material sequentially coated with LiFePO4 and carbon made in Example 1, making a lithium metal counter electrode, using LiPF6EC / DMC as an electrolyte, and using PE as a separator. A secondary battery of Comparative Example 1 was prepared under the same conditions except that the negative electrode material was made of pure silicon. The performance of the two secondary batteries was compared at a current density of 0.1 C in the voltage range of 0 V to 2.5 V.

[0043] As shown in Fig. 4, the discharge capacity of the pure silicon anode initially exhibited a high capacity of 4,000 mAh / g, but decreased sharply to 2,200 mAh / g in the second cycle. This is a typical phenomenon of silicon anodes caused by high volume expansion and contraction. However, the silicon anode coated with LiFePO4 and carbon initially showed a capacity of 3,900 mAh / g, and the capacity did not decrease significantly as the cycles progressed. As shown in Fig. 5, the secondary battery using the silicon anode coated with LiFePO4 and carbon suppressed volume expansion, stably maintaining a discharge capacity exceeding 1,000 mAh / g even up to 30 cycles. In contrast, the secondary battery using the pure silicon anode experienced a rapid decrease in capacity, showing a low discharge capacity of 2,000 mAh / g starting from cycle number 2, and then dropping to 200 mAh / g starting from cycle number 8.

[0044] From this, it was confirmed that a secondary battery using a silicon anode material coated with carbon and a lithium metal phosphate with an olivine structure having a stable crystal structure improves the performance of the secondary battery by preventing the phenomenon of particles of the anode material breaking due to volume expansion and contraction of the anode material during the electrochemical reaction and the phenomenon of silicon leaching into the electrolyte.

[0045] Silicon anode materials coated with LiFePO4 and carbon and pure silicon anode materials were observed using SEM. The results of the observation are shown in Figure 6. The pure silicon anode material had a uniform spherical shape. On the other hand, the silicon anode coated with LiFePO4 and carbon had an irregular particle shape.

[0046] Example 2

[0047] Example 2 involves 125 g of MoS2 particles, 2.3 g of Li2CO3 and FeC2O, which are raw materials for LiFePO4. 4ㆍ 11.3 g of 2H2O, 7.2 g of NH4H2PO4, and 1.25 g of sugar (6 wt% relative to the total amount of raw materials of LiFePO4) were mixed by ball milling in a dry state for 3 hours and heat-treated at 600°C for 15 hours in a nitrogen atmosphere.

[0048] In this way, MoS2 coated with 8 wt% LiFePO4 and 2.5 wt% carbon was finally obtained. Sugar was transformed into carbon and uniformly coated on the LiFePO4.

[0049] Since sulfur (S) leaches into the electrolyte during charging and discharging, secondary batteries using MoS2 as the anode have a problem in that their capacity drops rapidly with each cycle. To solve this problem, 8 wt% LiFePO4 and 2.5 wt% carbon were coated onto MoS2 particles. The secondary battery of Example 2 was fabricated using MoS2 coated with 8 wt% LiFePO4 and 2.5 wt% carbon as the anode material, lithium metal as the counter electrode, LiPF6EC / DMC as the electrolyte, and PE as the separator. The secondary battery of Comparative Example 2 was fabricated using the same method as Example 2, except that pure MoS2 was used as the anode material. Charge-discharge tests were performed on the secondary batteries of Example 2 and Comparative Example 2 at a current density of 0.1 C in a voltage range of 0.3 V to 2.7 V.

[0050] The charge-discharge graphs of Example 2 and Comparative Example 2 are shown in Fig. 7. The theoretical capacity of MoS2 is 1,675 mAh / g. A secondary battery using pure MoS2 anode material showed a capacity of 680 mAh / g in the first cycle, 400 mAh / g in the second cycle, and 220 mAh / g in the fifth cycle. However, a secondary battery using LiFePO4 and carbon-coated MoS2 anode material showed a capacity of 680 mAh / g in the first cycle, 480 mAh / g in the second cycle, and 400 mAh / g in the third cycle. The secondary battery of Example 2 showed a higher capacity retention rate compared to the secondary battery of Comparative Example 2.

[0051] From this, it was confirmed that a secondary battery using a carbon-coated MoS2 cathode material and a lithium metal phosphate with an olivine structure having a stable crystal structure improves the performance of the secondary battery by preventing the phenomenon of particles of the cathode material breaking due to volume expansion and contraction of the cathode material during the electrochemical reaction and the phenomenon of MoS2 leaching into the electrolyte.

[0052] SEM images of MoS2 particles coated with LiFePO4 and carbon were taken. Figure 8 is an SEM image of MoS2 particles coated with LiFePO4 and carbon. It was confirmed that the surface of MoS2 has a rough shape as it is coated with LiFePO4 and carbon.

[0053] Example 3

[0054] Example 3 uses 83 g of Sn particles with 2.3 g of Li2CO3 and FeC2O, which are raw materials for LiFePO4. 4ㆍ11.3 g of 2H2O, 7.2 g of NH4H2PO4, and 1.25 g of sugar (6 wt% relative to the total amount of raw materials of LiFePO4) were ball-milled and mixed in a dry state for 3 hours, and then heat-treated at 600°C for 15 hours in a nitrogen atmosphere. In this way, LiFePO4 and carbon-coated Sn were finally obtained. The amount of LiFePO4 was 12 wt% based on the total weight of LiFePO4 and carbon-coated Sn. The sugar was converted into carbon and was uniformly coated on LiFePO4 in an amount of 2.5 wt% based on the total weight of LiFePO4 and carbon-coated Sn.

[0055] A secondary battery of Example 3 was prepared using 12 wt% LiFePO4 and 2.5 wt% carbon-coated Sn as the negative electrode material, lithium metal as the counter electrode, LiFP6EC / DMC as the electrolyte, and PE as the separator. A secondary battery of Comparative Example 3 was prepared in the same manner as Example 3, except that pure Sn was used as the negative electrode material. Charge-discharge tests were performed on the secondary batteries of Example 3 and Comparative Example 3 at a current density of 0.1 C in a voltage range of 0 V to 1.8 V.

[0056] The charge-discharge graphs of Example 3 and Comparative Example 3 are shown in FIG. 9. As shown in FIG. 9(a), the secondary battery of Comparative Example 3, which used pure Sn as the negative electrode material, showed a discharge capacity of about 105 mAh / g in the first cycle, increased to 370 mAh / g in the second cycle, and then decreased to 250 mAh / g in the fifth cycle. The secondary battery of Comparative Example 3 had a large irreversible capacity due to the large difference between the charge capacity and the discharge capacity. As such, the secondary battery using pure Sn as the negative electrode material has a problem in that the negative electrode material particles break and the capacity of the secondary battery decreases rapidly because the volume of the negative electrode expands significantly and then contracts during the charging and discharging process, similar to the secondary battery using a silicon negative electrode.

[0057] On the other hand, as shown in Fig. 9(a), the secondary battery of Example 3 using a Sn anode material coated with LiFePO4 and carbon exhibited a discharge capacity of 570 mAh / g in the first cycle, 500 mAh / g in the second cycle, and 490 mAh / g in the fifth cycle. From this, it was confirmed that the secondary battery of Example 3 using a Sn anode material coated with LiFePO4 and carbon possesses a stable capacity retention rate. Fig. 10 is a lifetime graph showing the discharge capacity up to 30 cycles for the secondary battery of Example 3 using a Sn anode material coated with LiFePO4 and carbon. It exhibited a high capacity retention rate of 88% from the first cycle up to 30 cycles. From this, it was confirmed that a secondary battery using an olivine-structured lithium metal phosphate with a stable crystal structure and a carbon-coated Sn anode material improves the performance of the secondary battery by preventing the phenomenon of particles of the anode material breaking due to volume expansion and contraction of the anode material during the electrochemical reaction and the phenomenon of Sn leaching into the electrolyte.

Claims

Claim 1 A cathode material coated with lithium metal phosphate of an olivine structure (LiMPO4, where M is Fe, Mn, Co, Ni, Al or an alloy thereof) on a cathode active material that undergoes volume expansion during an electrochemical reaction. Claim 2 A cathode material in which a cathode active material undergoes volume expansion during an electrochemical reaction is sequentially coated with olivine-structured lithium metal phosphate (LiMPO4, where M is Fe, Mn, Co, Ni, Al or an alloy thereof) and carbon. Claim 3 In claim 1 or 2, the cathode active material is a cathode material which is Si, SiOx (0.7≤x≤1.9), Sn, SnO2, MoS2, WS2, SnS2, FeS2, MnO2, Fe3O4, TiNb2O7, MnC2O4, or a mixture thereof. Claim 4 In claim 1 or 2, the lithium metal phosphate with an olivine structure is LiFePO4, LiMnPO4, LiCoPO4, LiFe x Mn 1-x PO4(0 <x<1), LiFe x Mn y Co 1-x-y PO4(0 <x<1이고, 0<y<1이다) 또는 이들의 혼합물인 음극 소재. Claim 5 A cathode material according to claim 1, wherein the weight ratio of the lithium metal phosphate of the olivine structure is 2% to 20% by weight based on the total cathode material. Claim 6 A cathode material according to claim 5, wherein the weight ratio of the lithium metal phosphate of the olivine structure is 5% to 12% by weight based on the total cathode material. Claim 7 A cathode material according to claim 2, wherein the weight ratio of the lithium metal phosphate of the olivine structure is 3% to 20% by weight based on the total cathode material, and the weight ratio of the carbon is 1% to 10% by weight based on the total cathode material. Claim 8 In claim 7, the cathode material having a weight ratio of carbon of 2% to 6% based on the total cathode material. Claim 9 A secondary battery comprising a cathode material in which a negative electrode active material undergoes volume expansion during an electrochemical reaction is coated with lithium metal phosphate of an olivine structure (LiMPO4, where M is Fe, Mn, Co, Ni, Al or an alloy thereof). Claim 10 A secondary battery comprising a cathode material in which a cathode active material undergoes volume expansion during an electrochemical reaction is sequentially coated with olivine-structured lithium metal phosphate (LiMPO4, where M is Fe, Mn, Co, Ni, Al or an alloy thereof) and carbon. Claim 11 A secondary battery according to claim 9 or 10, wherein the negative electrode active material comprises a negative electrode material which is Si, SiOx (0.7≤x≤1.9), Sn, SnO2, MoS2, WS2, SnS2, FeS2, MnO2, Fe3O4, TiNb2O7, MnC2O4, or a mixture thereof. Claim 12 In claim 9 or 10, the lithium metal phosphate with an olivine structure is LiFePO4, LiMnPO4, LiCoPO4, LiFe x Mn 1-x PO4(0 <x<1), LiFe x Mn y Co 1-x-y PO4(0 <x<1이고, 0<y<1이다) 또는 이들의 혼합물인 음극 소재를 포함하는 이차전지. Claim 13 A secondary battery comprising a negative electrode material in which the weight ratio of the lithium metal phosphate of the olivine structure is 2% to 20% by weight based on the total negative electrode material in claim 9. Claim 14 A secondary battery comprising a negative electrode material in which the weight ratio of the lithium metal phosphate of the olivine structure is 5% to 12% by weight based on the total negative electrode material in claim 13. Claim 15 A secondary battery comprising a cathode material according to claim 10, wherein the weight ratio of the lithium metal phosphate of the olivine structure is 3% to 20% by weight based on the total cathode material, and the weight ratio of the carbon is 1% to 10% by weight based on the total cathode material. Claim 16 A secondary battery comprising a cathode material in which the weight ratio of the carbon in item 15 is 2% to 6% by weight based on the total cathode material.

Citation Information

Patent Citations

  • High-conductivity silicon-oxygen negative electrode material and application thereof

    CN111048756A

  • Negative active material for rechargeable lithium battery, and rechargeable lithium battery including same

    KR1020210107419A