Photosensitive resin film and uses thereof

The photosensitive resin film with controlled light absorption and composite structure addresses glare and adhesion issues in CMOS image sensor packaging, ensuring high pattern accuracy and low light transmittance for miniaturized automotive systems.

KR103046027B1Active Publication Date: 2026-11-10CHANG CHUN PLASTICS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
KR1020250073818
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2024-12-18
Filing Date
2025-06-05
Publication Date
2026-11-10
Estimated Expiration
2045-06-05

AI Technical Summary

Technical Problem

Existing photosensitive resin films used in CMOS image sensor packaging suffer from glare issues due to light reflection and require high aspect ratios and high adhesion, which are not adequately addressed by current materials, especially in miniaturized automotive applications.

Method used

A photosensitive resin film with specific light absorption characteristics, characterized by absorbance ratios A355/T, Aw1/T, and A450/T within defined ranges, and a composite film structure with protective layers, ensuring low light transmittance, anti-glare properties, and high pattern accuracy.

Benefits of technology

The film provides effective glare reduction and high pattern accuracy while maintaining high adhesion, suitable for miniaturized CMOS image sensor packaging, particularly in automotive applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112025063263720-PAT00001
    Figure 112025063263720-PAT00001
  • Figure 112025063263720-PAT00003
    Figure 112025063263720-PAT00003
  • Figure 112026096167281-PAT00004
    Figure 112026096167281-PAT00004
Patent Text Reader

Abstract

A photosensitive resin film having a thickness T in μm units is provided. When the photosensitive resin film is characterized by ultraviolet-visible spectroscopy, the resulting spectrum has an absorbance A355 at 355 nm and 0.003 ≤ A355 / T ≤ 0.03. The spectrum has at least one point within a first wavelength range where the first derivative is 0 and the second derivative is less than 0, and each of the points independently has an Aw1 / T value, where w1 represents the corresponding wavelength of the point and Aw1 represents the corresponding absorbance, and 0.003 ≤ Aw1 / T. The first wavelength range is greater than 450 nm to 780 nm, and the thickness T is in the range of 20 μm to 200 μm.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] Claim of priority

[0002] This application claims the benefit of Chinese patent application No. 202411867068.X filed on December 18, 2024 and Taiwan patent application No. 113149450 filed on December 18, 2024, the full contents of which are incorporated herein by reference.

[0003] Technology field

[0004] The present application provides a photosensitive resin film, in particular a photosensitive resin film having specific light absorption characteristics. The photosensitive resin film of the present application is used to form a package structure comprising a semiconductor device. Background Technology

[0005] Photosensitive resin films are films that undergo chemical changes after exposure to light. Photosensitive resin films can be classified into positive and negative photosensitive resin films based on the changes that occur after exposure and development. In the case of positive photosensitive resin films, the areas exposed to light dissolve during the development process, leaving only the unexposed areas. In the case of negative photosensitive resin films, the areas unexposed to light dissolve during the development process, leaving only the areas exposed to light. Due to their ease of patterning, photosensitive resin films are widely used in semiconductor component packaging, including CMOS (Complementary Metal-Oxide-Semiconductor) image sensor packaging.

[0006] CMOS image sensors are semiconductor devices used to capture digital images. Due to their advantages such as high resolution, high speed, and low light performance, they are widely used in various fields requiring image capture, including smartphones, digital cameras, webcams, automotive surround systems, and advanced driver assistance systems (ADAS).

[0007] Generally, the package structure of a CMOS image sensor involves placing a patterned structure, formed after curing a photosensitive resin layer on a glass plate, onto the sensor chip, and arranging the formed patterned structure to surround the photosensitive area of ​​the sensor chip. However, light passing through the glass plate can be partially reflected by the patterned structure, which can affect the photosensitive area and cause glare issues. This can pose a serious safety risk in automotive applications, including automotive surround systems and advanced driver assistance systems. Furthermore, in line with the trend toward miniaturization of CMOS image sensors, the package structure must also be miniaturized accordingly. Therefore, there is an urgent need for packaging materials capable of achieving high aspect ratios, high adhesion, and high pattern accuracy.

[0008] Given the aforementioned technical problems, the present application aims to provide a photosensitive resin film capable of meeting the requirements for low light transmittance, anti-glare, and high pattern accuracy. In particular, the photosensitive resin film can have high adhesion.

[0009] Specifically, the object of the present application is to provide a photosensitive resin film having a thickness T in μm units,

[0010] When the above photosensitive resin film is characterized by ultraviolet-visible spectroscopy, the resulting spectrum shows absorbance A at 355 nm. 355 With, 0.003 ≤ A 355 / T ≤ 0.03 and;

[0011] The spectrum has at least one point within a first wavelength range where the first derivative is 0 and the second derivative is less than 0, and each of the points is independently A w1 It has the value / T, where w1 represents the corresponding wavelength of the above point, and A w1 represents the corresponding absorbance, and 0.003 ≤ A w1 / T, preferably 0.003 ≤ A w1 / T ≤ 0.08, more preferably 0.003 ≤ A w1 / T ≤ 0.03 and; and

[0012] The first wavelength range is greater than 450 nm to 780 nm, more specifically greater than 480 nm to 730 nm, and the thickness T is in the range of 20 μm to 200 μm.

[0013] In one embodiment of the present application, the ultraviolet-visible spectroscopy is measured using an ultraviolet-visible spectrophotometer under the following conditions: the photosensitive resin film is positioned perpendicular to the direction of incident light; the diffraction grating is configured as a light splitter; a test temperature of 25°C is applied; a test pressure of 1 atm is applied; an absorbance analysis mode is used; a scan wavelength range of 190 nm to 1100 nm is used; air is used as a blank sample; a scan speed of 2200 nm / min is used; the transition wavelength at which the light source switches from a deuterium lamp to a tungsten lamp is 340.8 nm; a sampling interval of 0.2 nm is used; and a slit width of 2.0 nm is used.

[0014] In one embodiment of the present application, the spectrum is absorbance A at 450 nm. 450 With, 0 ≤ A 450 / T ≤ 0.003.

[0015] In one embodiment of the present application, the absorbance of the spectrum at each wavelength within the second wavelength range is independently A w2It is denoted as , where w2 represents the corresponding wavelength of absorbance, and 0 ≤ A w2 / T ≤ 0.003, and the second wavelength range is 440 nm to 470 nm.

[0016] In one embodiment of the present application, the photosensitive resin film is a negative dry film.

[0017] In one embodiment of the present application, the photosensitive resin film comprises an epoxy film.

[0018] Another object of the present application is to provide a composite film comprising the photosensitive resin film and a protective film on at least one surface of the photosensitive resin film.

[0019] Another object of the present application is a package structure,

[0020] Substrate;

[0021] A semiconductor device electrically connected to the above substrate; and

[0022] It includes a package for encapsulating the above semiconductor device, and

[0023] Here, the package structure is provided such that the material of the package comprises a cured product of the photosensitive resin film.

[0024] In one embodiment of the present application, the semiconductor device is an image sensor chip, the image sensor chip has a photosensitive region, and the material of the package comprises a first portion formed from a cured product of the photosensitive resin film and a second portion formed from a transparent material, the first portion surrounds the image sensor chip laterally, and the second portion is disposed over the photosensitive region. Specific details for implementing the invention

[0025] Some embodiments of the present application are described in detail below. However, the present application may be implemented in various embodiments and should not be limited to the embodiments described in the specification.

[0026] Unless otherwise stated, expressions such as "one (a)", "the", etc. cited in the specification and claims must include both singular and plural forms.

[0027] Unless otherwise noted, expressions such as “first,” “second,” etc., mentioned in the specification and claims are used merely to distinguish elements or components shown in the drawings without any special meaning. These expressions are not used to indicate any priority.

[0028] The advantage of the present application over the prior art lies in providing a photosensitive resin film having anti-glare, low light transmittance, and high pattern accuracy (good cross-sectional profile of the pattern formed after exposure) by controlling the absorption conditions of the photosensitive resin film, particularly for light of a specific wavelength. In particular, the photosensitive resin film can have high adhesion. Details regarding the photosensitive resin film of the present application and its applications are provided below.

[0029] 1. Photosensitive resin film

[0030] The photosensitive resin film of the present application refers to a film comprising a photosensitive resin composition and may be a positive photosensitive resin film or a negative photosensitive resin film. In one embodiment of the present application, the photosensitive resin film is a negative photosensitive resin film. That is, after the photosensitive resin film is exposed to light, the portion not exposed to light dissolves during the development process, and only the portion exposed to light remains.

[0031] Before using a photosensitive resin film, it is common practice to provide a protective film on the surface of the photosensitive resin film to provide protection and support functions, thereby forming a composite film structure, facilitating the storage of the photosensitive resin film, and protecting the photosensitive resin film from contamination or damage. Unless otherwise stated, the "thickness" and "absorbance" mentioned in the specification and claims describe the photosensitive resin film itself and do not include other parts, such as the protective film used in conjunction with the photosensitive resin film.

[0032] In one embodiment of the present application, the photosensitive resin film is a dry film, that is, a photosensitive resin film with a low solvent content. The low solvent content means that the amount of solvent based on the total weight of the photosensitive resin film is 10% by weight or less, specifically 5% by weight or less, and more specifically 0.1% to 4% by weight. Compared to ink or liquid wet films, the dry film has a low solvent content, so it is less likely to flow or deform, and can be attached to a substrate without additional processes such as coating or drying. Therefore, the dry film is easy to control and has good operability.

[0033] The thickness of the photosensitive resin film of the present application may be adjusted as needed. In one embodiment of the present application, the photosensitive resin film has a thick thickness. Specifically, the photosensitive resin film may have a thickness of 20 μm to 200 μm. For example, the thickness of the photosensitive resin film may be 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, or 200 μm, or may be within a range between any two values ​​described herein.

[0034] The photosensitive resin film of the present application may be formed by a single photosensitive resin layer or by laminating two or more photosensitive resin layers. For example, the photosensitive resin film of the present application may be formed by laminating two, three, or four photosensitive resin layers, but the present application is not limited thereto.

[0035] 1.1. Light Absorption Characteristics of Photosensitive Resin Films

[0036] [A 355 / T]

[0037] The photosensitive resin film of the present application has specific light absorption characteristics. Specifically, when the photosensitive resin film is characterized by ultraviolet-visible spectroscopy, the resulting spectrum shows an absorbance A at 355 nm. 355 With, A 355 The relationship between and thickness T (unit: μm) is 0.003 ≤ A 355 It satisfies / T ≤ 0.03. For example, A 355 The values ​​of / T are 0.0035, 0.004, 0.0045, 0.005, 0.0055, 0.006, 0.0065, 0.007, 0.0075, 0.008, 0.0085, 0.009, 0.0095, 0.01, 0.0105, 0.011, 0.0115, 0.012, 0.0125, 0.013, 0.0135, 0.014, 0.0145, 0.015, 0.0155, 0.016, 0.0165, 0.017, 0.0175, 0.018, 0.0185, 0.019, 0.0195, 0.02, 0.0205, 0.021, 0.0215, 0.022, 0.0225, 0.023, 0.0235, 0.024, 0.0245, 0.025, 0.0255, 0.026, 0.0265, 0.027, 0.0275, 0.028, 0.0285, 0.029, 0.0295, or 0.03, or may be within the range between any two values ​​described herein. A 355 If the value of / T is smaller than the above range, the photosensitive resin film does not have sufficient reactivity after exposure, resulting in insufficient photocuring. A355 If the value of / T is greater than the above range, the photosensitive resin film cannot form a high-precision pattern after exposure and development, and the cross-sectional profile is poor.

[0038] [A w1 / T]

[0039] In addition, when the photosensitive resin film is characterized by UV-visible spectroscopy, 0.003 ≤ A 355 In addition to satisfying the condition / T ≤ 0.03, the resulting spectrum has at least one point within the first wavelength range where the first derivative is 0 and the second derivative is less than 0; that is, the resulting spectrum within the first wavelength range has at least one absorption peak. Each of the above points is independently A w1 It has the value / T, where w1 represents the corresponding wavelength of the above point, and A w1 represents the corresponding absorbance. The first wavelength range is greater than 450 nm to 780 nm, more specifically greater than 480 nm to 730 nm. In this application, A w1 and thickness T (unit: μm) is 0.003 ≤ A w1 Satisfying / T, preferably 0.003 ≤ A w1 Satisfies / T ≤ 0.08, and more preferably 0.003 ≤ A w1 It satisfies / T ≤ 0.03. For example, A w1 The value of / T may be 0.003, 0.004, 0.005, 0.006, 0.007, 0.008, 0.009, 0.01, 0.011, 0.012, 0.013, 0.014, 0.015, 0.016, 0.017, 0.018, 0.019, 0.02, 0.021, 0.022, 0.023, 0.024, 0.025, 0.026, 0.027, 0.028, 0.029, or 0.03, or may be within the range of the two values ​​described herein. A w1If the value of / T is within the above range, the effects of low glare and low light transmittance are provided. In addition, within the above preferred range, the effects of low glare and low light transmittance can be obtained while simultaneously reducing the influence on the adhesion and pattern accuracy of the photosensitive resin film.

[0040] [A 450 / T]

[0041] In a preferred embodiment of the present application, when the photosensitive resin film is characterized by ultraviolet-visible spectroscopy, 0.003 ≤ A 355 / T ≤ 0.03 and 0.003 ≤ A w1 In addition to satisfying the condition / T, there is no light absorption at 450 nm, substantially no light absorption, or only a small amount of light absorption. Specifically, when the photosensitive resin film is characterized by UV-visible spectroscopy, the resulting spectrum shows an absorbance A at 450 nm. 450 With, A 450 The relationship between and thickness T (unit: μm) is 0 ≤ A 450 / T ≤ 0.003, preferably 0 ≤ A 450 It satisfies / T ≤ 0.0025. For example, A 450 The value of / T may be within the range of 0, 0.0005, 0.001, 0.0015, 0.002, or 0.0025, or any two values ​​described herein. In the above preferred range, the photosensitive resin film may have better pattern accuracy and adhesion.

[0042] [A w2 / T]

[0043] In a preferred embodiment of the present application, when the photosensitive resin film is characterized by ultraviolet-visible spectroscopy, 0.003 ≤ A 355 In addition to satisfying the condition / T ≤ 0.03, the spectrum has 0.003 ≤ A in the first wavelength range of greater than 480 nm to 730 nm. w1Having the above technical features of / T, there is no light absorption, no light absorption, substantially no light absorption, or only a small amount of light absorption within the second wavelength range. The second wavelength range is 440 nm to 470 nm. Specifically, when the photosensitive resin film is characterized by ultraviolet-visible spectroscopy, the absorbance of the spectrum at each wavelength within the second wavelength range is independently A w2 Represented as, and 0 ≤ A w2 The condition / T ≤ 0.003 is satisfied, where w2 represents the corresponding wavelength of absorbance. For example, A w2 / T can independently be 0, 0.0005, 0.001, 0.0015, 0.002, 0.0025, or 0.003, and may be within the range between any two values ​​described herein. In the above preferred range, the photosensitive resin film may have better pattern accuracy and adhesion.

[0044] In the present application, the ultraviolet-visible spectroscopy is measured using an ultraviolet-visible spectrophotometer under the following conditions: the photosensitive resin film is positioned perpendicular to the incident direction of the light source; the diffraction grating is configured as a beam splitter; a test temperature of 25°C is applied; a test pressure of 1 atm is applied; an absorbance analysis mode is used; a scanning wavelength range of 190 nm to 1100 nm is used; air is used as a blank sample; a scanning speed of 2200 nm / min is used; the transition wavelength at which the light source switches from a deuterium lamp to a tungsten lamp is 340.8 nm; a sampling interval of 0.2 nm is used; and a slit width of 2.0 nm is used. Under the above test conditions, the photosensitive resin film sample used for analysis is prepared by cutting the photosensitive resin film to a size of 5 cm × 3 cm at any location along the transverse direction (TD) and mechanical direction (MD); Alternatively, a composite film comprising a photosensitive resin film and protective films on both sides of the photosensitive resin film is cut to a size of 5 cm × 3 cm at any location along the transverse and machine directions, and then the protective films on both sides of the cut photosensitive resin film are removed to obtain the composite film. To accurately measure the absorbance of the photosensitive resin film, the photosensitive resin film must be positioned perpendicular to the direction of incident light. The wavelength of the tungsten lamp used as the incident light source is 340.8 nm. In addition, the “sampling interval” means collecting data points every 0.2 nm in the scanning wavelength range of 190 nm to 1100 nm and recording the values.

[0045] The light absorption characteristics of the photosensitive resin film of the present application can be controlled by adjusting the constituent components of the photosensitive resin film or the process conditions of the photosensitive resin film. For example, the constituent components of the photosensitive resin film can be controlled according to the type and amount of additives used. Additives include, but are not limited to, photopolymerization initiators, light absorbers, dyes, etc. The process conditions of the photosensitive resin film may be, for example, drying conditions. A person skilled in the art will be able to manufacture a photosensitive resin film having the above light absorption characteristics by referring to the specification of the present application, and in particular by referring to the specific descriptions shown in the embodiments.

[0046] 1.2. Other characteristics of photosensitive resin films

[0047] A 355 / T and A w1 Assuming that / T satisfies the above range, other properties of the photosensitive resin film of the present application can be adjusted according to the required application.

[0048] For example, a photosensitive resin film can be adjusted to have an appropriate film tensile strength. Film tensile strength refers to the adhesion between the photosensitive resin film and the protective film covering it, and is expressed as the force required to tear a protective film of a specific size vertically from the photosensitive resin film. The protective film may be a PET protective film or a PE protective film. Generally, the lower the film tensile strength of the photosensitive resin film, the harder and more elastic the photosensitive resin film is; conversely, the higher the film tensile strength of the photosensitive resin film, the softer and stickier the photosensitive resin film is. Film tensile strength is measured by the following method: a protective film is attached to the surface of a photosensitive resin film to form a composite film, the composite film is cut to a size of 10 cm × 10 cm, the protective film is cut to a width of 50 mm in the transverse direction (TD), the composite film is fixed to the stage of a tensile testing machine, the protective film cut to a width of 50 mm is peeled off, tape is applied to the inside of the protective film (i.e., the side facing the photosensitive resin film), and the composite film is fixed to the tensile axis of the tensile testing machine so that the tensile direction is perpendicular to the stage, the stage is moved transversely toward the inside of the peeled protective film at a speed of 70 mm / min, the protective film is peeled off by 2 cm in the transverse direction (TD), and the tensile strength is measured. The unit of film tensile strength is g / 50 mm.

[0049] In one embodiment of the present application, the film tensile strength of the photosensitive resin film is 2 g / 50 mm or more, more specifically 2 g / 50 mm to 1000 g / 50 mm, and the adhesive strength is superior. For example, the film tensile strength of the photosensitive resin film may be 2 g / 50 mm, 5 g / 50 mm, 10 g / 50 mm, 50 g / 50 mm, 100 g / 50 mm, 200 g / 50 mm, 300 g / 50 mm, 400 g / 50 mm, 500 g / 50 mm, 600 g / 50 mm, 700 g / 50 mm, 800 g / 50 mm, 900 g / 50 mm, or 1000 g / 50 mm, or within a range between any two values ​​described herein.

[0050] 1.3. Composition of Photosensitive Resin Film

[0051] A 355 / T and A w1 Assuming that / T satisfies the above range, the composition of the photosensitive resin film can be adjusted according to the required application. In one embodiment of the present application, the photosensitive resin film is an epoxy resin-based photosensitive resin film containing an epoxy resin and optionally containing an ethylene-based unsaturated compound, a photopolymerization initiator, and other additives.

[0052] 1.3.1. Epoxy Resin

[0053] Examples of epoxy resins include, but are not limited to, bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, bisphenol A novolak epoxy resin, novolak epoxy resin, alkyl novolak epoxy resin, phenol novolak epoxy resin, cresol novolak epoxy resin, alicyclic epoxy resin, biphenyl epoxy resin, aralkyl epoxy resin, naphthalene cyclic epoxy resin, naphthol epoxy resin, biphenyl aralkyl epoxy resin, fluorene epoxy resin, xanthen epoxy resin, dicyclopentadiene epoxy resin, triglycidyl polyisocyanate, and oxyheterocyclic epoxy resin. The above epoxy resins may each be used alone or in combination. In one embodiment of the present application, bisphenol A epoxy resin, bisphenol A novolak epoxy resin, phenol novolak epoxy resin, cresol novolak epoxy resin, aliphatic epoxy resin, or oxetane epoxy resin is used.

[0054] In the photosensitive resin film of the present application, based on the total weight of the photosensitive resin film, the amount of epoxy resin may be 50% to 99% by weight, specifically 55% to 98% by weight, and more specifically 60% to 95% by weight. For example, based on the total weight of the photosensitive resin film, the amount of epoxy resin is 50 wt%, 51 wt%, 52 wt%, 53 wt%, 54 wt%, 55 wt%, 56 wt%, 57 wt%, 58 wt%, 59 wt%, 60 wt%, 61 wt%, 62 wt%, 63 wt%, 64 wt%, 65 wt%, 66 wt%, 67 wt%, 68 wt%, 69 wt%, 70 wt%, 71 wt%, 72 wt%, 73 wt%, 74 wt%, 75 wt%, 76 wt%, 77 wt%, 78 wt%, 79 wt%, 80 wt%, 81 wt%, 82 wt%, 83 wt%, 84 wt%, 85 wt%, 86 wt%, It may be 87 wt%, 88 wt%, 89 wt%, 90 wt%, 91 wt%, 92 wt%, 93 wt%, 94 wt%, 95 wt%, 96 wt%, 97 wt%, 98 wt%, or 99 wt%, or within a range between any two values ​​described herein.

[0055] 1.3.2. Ethylene-based unsaturated compounds

[0056] Ethylene-based unsaturated compounds refer to compounds having at least one reactive ethylene functional group, for example, difunctional compounds having two reactive ethylene functional groups. Examples of ethylenically unsaturated compounds include ethoxylated trimethylolpropane triacrylate, ethoxylated bisphenol-A diacrylate, ethoxylated bisphenol-A dimethacrylate, tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, polypropylene glycol diacrylate, tris((meth)acrylate)hexamethylene isocyanurate, ethoxylated urethane di(meth)acrylate, propoxylated urethane di(meth)acrylate, ethoxylated / propoxylated urethane di(meth)acrylate, ethoxylated tris(methacrylate)hexamethylene isocyanurate, acrylated tris(methacrylate)hexamethylene isocyanurate, and ethoxylated / propoxylated It includes, but is not limited to, tris(methacrylate) hexamethylene isocyanurate. In one embodiment of the present application, ethoxylated trimethylolpropane triacrylate is used.

[0057] In the photosensitive resin film of the present application, the amount of an ethylene-based unsaturated compound may be 0% to 70% by weight based on the total weight of the photosensitive resin film. For example, based on the total weight of the photosensitive resin film, the amount of an ethylene-based unsaturated compound may be 5% by weight, 10% by weight, 15% by weight, 20% by weight, 25% by weight, 30% by weight, 35% by weight, 40% by weight, 45% by weight, 50% by weight, 55% by weight, 60% by weight, 65% by weight, or 70% by weight, or within a range between any two values ​​described herein.

[0058] 1.3.3. Photopolymerization Initiator

[0059] Examples of photopolymerization initiators include, but are not limited to, imidazole compounds, ketone compounds, quinone compounds, benzoin or benzoin ether compounds, polyhalogenated compounds, triazine compounds, organic peroxide compounds, and onium salt compounds. The photopolymerization initiators may be used alone or in combination. In one embodiment of the present application, an onium salt compound is used. Examples of the above onium salt compounds include, but are not limited to, diaryl iodonium salts and triaryl sulfonium salts obtained from combinations of diphenyl iodonium, 4,4'-dichlorodiphenyl iodonium, 4,4'-dimethoxydiphenyl iodonium, 4,4'-di-tert-butyldiphenyl iodonium, 4-methyl-4'-isopropyldiphenyl iodonium or 3,3'-dinitrodiphenyl iodonium with chlorides, bromides, tetrafluoroborates, hexafluorophosphates, hexafluoroarsenates, hexafluoroantimonates and tetrakis(pentafluorophenyl)borates or trifluoromethanesulfonic acid.

[0060] In a photosensitive resin film, the amount of photopolymerization initiator based on the total weight of the photosensitive resin film may be 0.5% by weight to 10% by weight, more specifically 1% by weight to 5% by weight. For example, the amount of photopolymerization initiator based on the total weight of the photosensitive resin film may be 0.5% by weight, 1% by weight, 1.5% by weight, 2% by weight, 2.5% by weight, 3% by weight, 3.5% by weight, 4% by weight, 4.5% by weight, 5% by weight, 5.5% by weight, 6% by weight, 6.5% by weight, 7% by weight, 7.5% by weight, 8% by weight, 8.5% by weight, 9% by weight, 9.5% by weight, or 10% by weight, or within a range between any two values ​​described herein.

[0061] 1.3.4. Additives

[0062] A 355 / T and A w1Assuming that / T satisfies the above range, the photosensitive resin film of the present application may further include additives to improve the properties of the photosensitive resin film. Examples of additives include, but are not limited to, light absorbers, dyes, pigments, radical inhibitors, surfactants, reinforcing agents, and plasticizers. The aforementioned additives may each be used alone or in combination. In one embodiment of the present application, the photosensitive resin film may further include a silane coupling agent, a light absorber, and a dye.

[0063] In the photosensitive resin film, the amount of additive based on the total weight of the photosensitive resin film is preferably less than 20 wt%. For example, the amount of additive based on the total weight of the photosensitive resin film may be 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, or 19 wt%, or within a range between any two values ​​described herein.

[0064] 1.4. Preparation of Photosensitive Resin Film

[0065] The method for manufacturing the photosensitive resin film of the present application is not particularly limited. A person skilled in the art can manufacture the photosensitive resin film by referring to the specification of the present application. For example, a resin composition can be prepared by uniformly mixing each component of the photosensitive resin film using a stirrer and dissolving or dispersing it in a solvent. Subsequently, the resin composition is coated onto a substrate and then dried to obtain a photosensitive resin film.

[0066] The coating method of the resin composition is not particularly limited and may be any conventional coating method commonly used in the field of this application. Examples of conventional coating methods include, but are not limited to, gravure coating, reverse roll coating, die coating, air scraper coating, scraper coating, rod coating, scraper rod coating, curtain coating, knife coating, transfer roll coating, extrusion press coating, dip coating, kiss coating, spray coating, calender coating, and extrusion coating.

[0067] A detailed method for manufacturing the photosensitive resin film of the present application is described in the following embodiments.

[0068] 2. Composite film

[0069] Generally, a protective film providing protection and support functions may be applied to both sides of a photosensitive resin film before use. This facilitates the storage of the photosensitive resin film and protects it from contamination or damage. Accordingly, the present application also provides a composite film comprising said photosensitive resin film and a protective film formed on at least one surface of said photosensitive resin film. In a preferred embodiment of the present application, a protective film is provided on both sides of the photosensitive resin film, and the material of the protective film on two different surfaces of the photosensitive resin film may be the same or different.

[0070] The type of protective film is not particularly limited and may be made of ordinary materials known in the art. For example, the protective film that may be used in this application may be selected from the group consisting of polyethylene terephthalate films (PET films), polyolefin films, and composites thereof. Examples of polyolefin films include, but are not limited to, polyethylene films (PE films) and polypropylene films (PP films), for example, oriented polypropylene films. The composite may be a composite of polyethylene terephthalate films and polyolefin films, or a composite of different polyolefin films. In a preferred embodiment of this application, the composite film comprises a PET film formed on two surfaces of a photosensitive resin film; or the composite film comprises a PET film on one surface of the photosensitive resin film and a PE film on the other surface of the photosensitive resin film.

[0071] The method for manufacturing the composite film of the present application is not particularly limited, and any conventional method commonly used in the field of the present application may be used. For example, the composite film may be manufactured by stacking protective films on both sides of a photosensitive resin film to provide an overlapping object, and then compressing the overlapping object to obtain the composite film. Alternatively, the composite film may be manufactured by the following method: a resin composition for forming a photosensitive resin film is coated onto a first protective film and then dried to form a photosensitive resin film on the first protective film; a second protective film is attached to the surface of the photosensitive resin film that does not come into contact with the first protective film; and then, the composite film is obtained. Alternatively, the composite film may be manufactured by extruding a resin composition for forming a photosensitive resin film with a certain distance between the two protective films and then drying to form a photosensitive resin film between the two protective films.

[0072] 3. Package Structure

[0073] A cured product of the photosensitive resin film of the present application can be used as a material for a package for manufacturing a package structure of a semiconductor device. Accordingly, the present application further provides a package structure comprising a substrate, a semiconductor device electrically connected to the substrate, and a package for encapsulating the semiconductor device, wherein the material of the package comprises a cured product of the photosensitive resin film.

[0074] The type or function of the semiconductor device is not particularly limited. In one embodiment of the present application, the semiconductor device may be an image sensor chip, and the image sensor chip may have a photosensitive region. When the semiconductor device is an image sensor chip, the material of the package may include, for example, a first portion formed from a cured product of the photosensitive resin film and a second portion formed from a transparent material, wherein the first portion surrounds the image sensor chip laterally, the second portion is placed over the photosensitive region, and the first portion may be directly connected to the second portion or connected to the second portion through a medium to form a package. Additionally, the first portion may be directly connected to a substrate or connected to a substrate through a medium. Alternatively, the first portion may be directly connected to a non-photosensitive region of the image sensor chip or connected to a non-photosensitive region of the image sensor chip through a medium.

[0075] 4. Examples

[0076] 4.1. Test Method

[0077] [Thickness of photosensitive resin film]

[0078] A manufactured composite film containing a photosensitive resin film is cut to a size of 5 cm × 3 cm, and the protective film on both sides of the photosensitive resin film is removed. The resulting photosensitive resin film is placed on the base (MS-11C base) of a film thickness gauge (model name: Nikon Digimicro MFC-101+MS-11C, purchased from Nikon), and measurements are performed under a pressure of 140 gf using the MFC-101 meter. The thickness of the photosensitive resin film is measured at 10 different points, and the average is calculated.

[0079] [Absorbance of photosensitive resin film]

[0080] The prepared composite film containing the photosensitive resin film is cut to a size of 5 cm × 3 cm, and the protective film on both sides of the photosensitive resin film is removed. The absorbance of the resulting photosensitive resin film is measured using an ultraviolet-visible spectrophotometer (Model: Shimadzu UV-1601, purchased from Shimadzu) in the following manner. The photosensitive resin film is positioned perpendicular to the direction of incidence of light and analyzed to obtain an absorbance spectrum under the following conditions: the diffraction grating is configured as a light splitter; a test temperature of 25°C is applied; a test pressure of 1 atm is applied; an absorbance analysis mode is used; a scanning wavelength range of 190 nm to 1100 nm is used; air is used as the blank sample; a scanning speed of 2200 nm / min is applied; the transition wavelength at which the light source switches from a deuterium lamp to a tungsten lamp is 340.8 nm; a sampling interval of 0.2 nm is used; and a slit width of 2.0 nm is used; Shimadzu UV Probe V1.11 software is used.

[0081] [Film Tensile Strength]

[0082] A manufactured composite film containing a photosensitive resin film is cut to a size of 10 cm × 10 cm, and a PET protective film is cut to a width of 50 mm in the transverse direction (TD). The composite film is secured to the stage of a tensile testing machine (Model: FM-50N, purchased from YOTEC) using double-sided tape. The 50 mm wide cut PET protective film is peeled off, tape is applied to the inside of the PET protective film (i.e., the side facing the photosensitive resin film), and the film is fixed to the tensile axis of the tensile testing machine so that the tensile direction is perpendicular to the stage. The stage is moved transversely toward the inside of the peeled protective film at a speed of 70 mm / min, and the force required to tear off 2 cm of the PET protective film is measured as the film tensile force. The unit of film tensile force is g / 50 mm.

[0083] [Cross-sectional profile of photoresist pattern]

[0084] 2mm thick low-alkali glass is preheated to 80°C for 10 minutes in a batch oven, and the surface temperature is maintained at 50°C prior to lamination. The prepared photosensitive resin film is placed on the low-alkali glass and pressed using a lamination machine (Model: CSL-M25E, purchased from C SUN), with the temperature and pressure of the lamination machine set to 80°C and 3 kg / cm², respectively. 2 The lamination speed is 2.0 m / min. After lamination is completed, the excess film is removed, and the resulting photosensitive resin film is left for 15 minutes to cool to room temperature.

[0085] Next, the photosensitive resin film is exposed using an exposure machine (Model: Contact Aligner, purchased from Deya Optronic). The wavelength of the exposure light source is 365 nm (i-line). The exposure energy is 300 mJ / cm². 2Continue exposure until it is reached. The aspect ratio of the photoresist pattern to be formed is 2.0, and the linear spatial width of the graphic dimensions:photoresist width is 1:1. After the exposure is complete, bake the exposed photosensitive resin film at 70°C for 5 minutes.

[0086] Then, the exposed photosensitive resin film is developed under the following conditions to obtain a developed photosensitive resin film: propylene glycol methyl ether acetate (PGMEA) is used as the developer, the liquid temperature is set to 24°C to 26°C, and the immersion time for development is 5 minutes.

[0087] Using a glass cutter, the developed photosensitive resin film is cut along with the low-alkali glass at the outer edge of the linear space, and the cross-sectional profile of the photoresist pattern is observed using a scanning electron microscope, with the specimen tilted at 75° and a magnification of 200x. The top width is obtained by the following method: a photoresist cross-section is randomly selected, and starting from the top edge of the photoresist (away from the low-alkali glass), the width of the photoresist is measured at thicknesses of 1 / 25, 2 / 25, 3 / 25, 4 / 25, and 5 / 25 of the total thickness of the photoresist, and the average of the width values ​​measured at these five positions is obtained to obtain the top width value. Likewise, the bottom width is obtained in the following manner: a photoresist cross-section is randomly selected, and starting from the bottom edge of the photoresist (the side touching the low-alkali glass), the width of the photoresist is measured at thicknesses of 1 / 25, 2 / 25, 3 / 25, 4 / 25, and 5 / 25 of the total photoresist thickness, and the bottom width value is obtained by averaging the width values ​​measured at these five locations. If the value of “|(top width - bottom width)| / thickness” is less than 0.04, it is recorded as “rectangular,” which means that the cross-sectional profile of the photoresist pattern is good; if the value of “|(top width - bottom width)| / thickness” is 0.04 or greater, it is recorded as “trapezoidal,” which means that the cross-sectional profile of the photoresist pattern is poor. In the formula, “|(top width - bottom width)|” means taking the absolute value.

[0088] [Footing length of photoresist pattern]

[0089] A photosensitive resin film developed in the same manner as described in the [Cross-sectional profile of the photoresist pattern] above is prepared. Then, the developed photosensitive resin film is cut along with low-alkali glass at the outer edge of the linear space using a glass cutter, and the cross-sectional profile of the photoresist pattern is observed using a scanning electron microscope, wherein the test specimen is 75o A magnification of 5000x is used with the image tilted. The footing length is obtained by randomly selecting a cross-section of the photoresist and selecting a side where the bottom protrudes further toward the linear space. Specifically, the footing length is obtained by the following calculation: starting from the lower edge of the photoresist, a reference point is taken at the position of the photoresist sidewall, the thickness of which is 1 / 5 of the total thickness of the photoresist, a reference line perpendicular to the low-alkali glass surface is extended downward from the reference point, and the length from the intersection of the reference line and the low-alkali glass surface to the intersection of the photoresist sidewall and the low-alkali glass surface is measured and taken as the footing length.

[0090] [Light transmittance]

[0091] The manufactured composite film containing the photosensitive resin film is cut to a size of 5 cm × 3 cm, and the protective films on both sides of the photosensitive resin film are removed. The light transmittance of the photosensitive resin film is measured using an ultraviolet-visible spectrophotometer (Model: Shimadzu UV-1601, purchased from Shimadzu) in the following manner. The photosensitive resin film is placed on the analysis stage using a fixture, positioned perpendicular to the direction of the incident light source, and under the following conditions at a wavelength of 550 nm (T 550nm The light transmittance in ) is measured: a transmittance analysis mode is used; a scanning wavelength range of 190 nm to 1100 nm is used; air is used as the blank sample; a scanning speed of 2200 nm / min is used; the switching wavelength at which the light source switches from a deuterium lamp to a tungsten lamp is 340.8 nm; and a sampling interval of 0.2 nm is used.

[0092] [Silicone Adhesion Test]

[0093] 2mm thick low-alkali glass is preheated in a batch oven to 80°C for 10 minutes, and the surface temperature is maintained at 50°C prior to lamination. The prepared photosensitive resin film is placed on the low-alkali glass, and the temperature is 80°C and the pressure is 3 kg / cm²2 , press using a lamination machine with a lamination speed of 2.0 m / min (Model: CSL-M25E, purchased from C SUN). After lamination is completed, remove the excess film and let the resulting photosensitive resin film sit for 15 minutes to cool to room temperature.

[0094] Next, the photosensitive resin film is exposed using an exposure machine (Model: Contact Aligner, purchased from Deya Optronic). The wavelength of the exposure light source is 365 nm (i-line). The exposure energy is 300 mJ / cm². 2 Continue exposure until it reaches. After the exposure is complete, bake the exposed photosensitive resin film at 70°C for 5 minutes.

[0095] Then, the exposed photosensitive resin film is developed under the following conditions to obtain a developed photosensitive resin film without a pattern: propylene glycol methyl ether acetate (PGMEA) is used as the developer, the liquid temperature is set to 24°C to 26°C, and the immersion time for development is 5 minutes.

[0096] A 3 mm² bare Si substrate is placed on one side of a photosensitive resin film that does not come into contact with low-alkali glass, and bonding is performed by applying a pressure of 3 kgf / cm² at 130°C for 5 minutes. Subsequently, a tensile testing machine is used to measure the force required to tear off the bare Si substrate. In the test, the direction of force application is parallel to the interface between the bare Si substrate and the photosensitive resin film. The force acts directly on the bare Si substrate, and the point of application of the specific force is located at the mid-height of the sidewall of the bare Si substrate, with the sidewall perpendicular to the photosensitive resin film. The unit of adhesion force is kgf / 3 mm² 2 am.

[0097] 4.2. Preparation of Photosensitive Resin Film

[0098] Information on the raw materials used in the following examples and comparative examples is shown in Table 1 below.

[0099] [Table 1]

[0100]

[0101] [Example 1]

[0102] The following components were mixed and stirred for 5 hours to be uniformly mixed to obtain the resin composition of Example 1: 90 parts by weight of BNE200 epoxy resin, 10 parts by weight of BE507 epoxy resin, 25 parts by weight of acetone, 2 parts by weight of triphenylsulfonium hexafluoroantimonate, 5 parts by weight of KBE-403 silane coupling agent, 0.2 parts by weight of solvent blue, and 12 parts by weight of tetrahydrofuran.

[0103] The resin composition of Example 1 was coated onto a PET film acting as a protective film using a Kodaira wire-wound rod, and the coated resin composition was dried in an oven. Subsequently, a PE film acting as a protective film was laminated onto the surface of the dried resin composition to obtain a photosensitive resin film (i.e., a composite film) wrapped with the protective film of Example 1. The conditions for coating and drying were as follows: the coating thickness was 160 μm, a drying temperature of 100°C was applied, a drying time of 20 minutes was used, and the thickness after drying was 120 μm.

[0104] [Example 2]

[0105] The following components were mixed and stirred for 5 hours to be uniformly mixed to obtain the resin composition of Example 2: 20 parts by weight of BNE200 epoxy resin, 60 parts by weight of BE507 epoxy resin, 20 parts by weight of CNE200ELA epoxy resin, 30 parts by weight of acetone, 1.8 parts by weight of triphenylsulfonium tetrakis(pentafluorophenyl)borate, 3 parts by weight of silane coupling agent KBE-400, 1.2 parts by weight of oil blue, and 12 parts by weight of tetrahydrofuran.

[0106] The resin composition of Example 2 was coated onto a PET film acting as a protective film using a Kodaira wire-wound rod, and the coated resin composition was dried in an oven. Subsequently, a PE film acting as a protective film was laminated onto the surface of the dried resin composition to obtain a photosensitive resin film (i.e., a composite film) wrapped with the protective film of Example 2. The conditions for coating and drying were as follows: the coating thickness was 25 μm, a drying temperature of 100°C was applied, a drying time of 15 minutes was used, and the thickness after drying was 20 μm.

[0107] [Example 3]

[0108] The following components were mixed and stirred for 5 hours to be uniformly mixed, thereby obtaining the resin composition of Example 3: 30 parts by weight of BNE200 epoxy resin, 20 parts by weight of BE507 epoxy resin, 50 parts by weight of PNE177 epoxy resin, 35 parts by weight of acetone, 4 parts by weight of triphenylsulfonium tetrakis(pentafluorophenyl)borate, 5 parts by weight of KBE-403 silane coupling agent, 0.5 parts by weight of solvent blue, and 12 parts by weight of tetrahydrofuran.

[0109] The resin composition of Example 3 was coated onto a PET film acting as a protective film using a Kodaira wire-wound rod, and the coated resin composition was dried in an oven. Subsequently, a PE film acting as a protective film was laminated onto the surface of the dried resin composition to obtain a photosensitive resin film wrapped with the protective film of Example 3 (i.e., a composite film). The coating and drying conditions were as follows: the coating thickness was 85 μm, the drying temperature was 90°C, the drying time was 19 minutes, and the thickness after drying was 60 μm.

[0110] [Example 4]

[0111] The following components were mixed and stirred for 5 hours to be uniformly mixed, thereby obtaining the resin composition of Example 4: 75 parts by weight of BNE200 epoxy resin, 10 parts by weight of BE507 epoxy resin, 5 parts by weight of BNE220 epoxy resin, 10 parts by weight of 3EO TMPTA (ethylenically unsaturated compound), 25 parts by weight of acetone, 4 parts by weight of triarylsulfonium tetrakis(pentafluorophenyl)borate, 5 parts by weight of KBE-403 silane coupling agent, 0.5 parts by weight of oil blue, and 15 parts by weight of tetrahydrofuran.

[0112] The resin composition of Example 4 was coated onto a PET film acting as a protective film using a Kodaira wire-wound rod, and the coated resin composition was dried in an oven. Subsequently, a PE film acting as a protective film was laminated onto the surface of the dried resin composition to obtain a photosensitive resin film (i.e., a composite film) wrapped with the protective film of Example 4. The conditions for coating and drying were as follows: the coating thickness was 275 μm, a drying temperature of 95°C was applied, a drying time of 30 minutes was used, and the thickness after drying was 200 μm.

[0113] [Example 5]

[0114] The following components were mixed and stirred for 5 hours to be uniformly mixed, thereby obtaining the resin composition of Example 5: 20 parts by weight of BNE200 epoxy resin, 20 parts by weight of BE507 epoxy resin, 20 parts by weight of PNE177 epoxy resin, 20 parts by weight of BNE220 epoxy resin, 10 parts by weight of Celloxide 2021P epoxy resin, 10 parts by weight of TCM201 epoxy resin, 25 parts by weight of acetone, 2 parts by weight of triphenylsulfonium hexafluoroantimonate, 5 parts by weight of KBE-403 silane coupling agent, 0.2 parts by weight of solvent blue, and 12 parts by weight of tetrahydrofuran.

[0115] The resin composition of Example 5 was coated onto a PET film acting as a protective film using a Kodaira wire-wound rod, and the coated resin composition was dried in an oven. Subsequently, a PE film acting as a protective film was laminated onto the surface of the dried resin composition to obtain a photosensitive resin film (i.e., a composite film) wrapped with the protective film of Example 5. The conditions for coating and drying were as follows: the coating thickness was 130 μm, a drying temperature of 100°C was applied, a drying time of 20 minutes was used, and the thickness after drying was 100 μm.

[0116] [Example 6]

[0117] The following components were mixed and stirred for 5 hours to be uniformly mixed, thereby obtaining the resin composition of Example 6: 50 parts by weight of BNE200 epoxy resin, 40 parts by weight of BE507 epoxy resin, 10 parts by weight of BNE220 epoxy resin, 25 parts by weight of acetone, 1.5 parts by weight of triphenylsulfonium hexafluoroantimonate, 0.5 parts by weight of triarylsulfonium tetrakis(pentafluorophenyl)borate, 4 parts by weight of KBE-403 silane coupling agent, 0.3 parts by weight of solvent blue, 0.05 parts by weight of solvent yellow, and 12 parts by weight of tetrahydrofuran.

[0118] The resin composition of Example 6 was coated onto a PET film acting as a protective film using a Kodaira wire-wound rod, and the coated resin composition was dried in an oven. Subsequently, a PE film acting as a protective film was laminated onto the surface of the dried resin composition to obtain a photosensitive resin film wrapped with the protective film of Example 6 (i.e., a composite film). The conditions for coating and drying were as follows: the coating thickness was 130 μm, a drying temperature of 90°C was applied, a drying time of 25 minutes was used, and the thickness after drying was 100 μm.

[0119] delete

[0120] delete

[0121] delete

[0122] [Comparative Example 1]

[0123] The following components were mixed and stirred for 5 hours to be uniformly mixed, thereby obtaining the resin composition of Comparative Example 1. 100 parts by weight of cellulose 2021P epoxy resin, 25 parts by weight of acetone, 0.3 parts by weight of triphenylsulfonium hexafluoroantimonate, 2 parts by weight of SI-45, 5 parts by weight of KBE-403 silane coupling agent, 0.3 parts by weight of solvent blue, and 12 parts by weight of tetrahydrofuran.

[0124] The resin composition of Comparative Example 1 was coated onto a PET film acting as a protective film using a Kodaira wire-wound rod, and the coated resin composition was dried in an oven. Subsequently, a PE film acting as a protective film was laminated onto the surface of the dried resin composition to obtain a photosensitive resin film (i.e., a composite film) wrapped with the protective film of Comparative Example 1. The conditions for coating and drying were as follows: the coating thickness was 130 μm, a drying temperature of 100°C was applied, a drying time of 20 minutes was used, and the thickness after drying was 100 μm.

[0125] [Comparative Example 2]

[0126] The following components were mixed and stirred for 5 hours to be uniformly mixed, thereby obtaining the resin composition of Comparative Example 2. 90 parts by weight of BNE220 epoxy resin, 10 parts by weight of TCM201 epoxy resin, 25 parts by weight of acetone, 1 part by weight of triphenylsulfonium tetrakis(pentafluorophenyl)borate, 4 parts by weight of triarylsulfonium tetrakis(pentafluorophenyl)borate, 5 parts by weight of KBE-403 silane coupling agent, and 12 parts by weight of tetrahydrofuran.

[0127] The resin composition of Comparative Example 2 was coated onto a PET film acting as a protective film using a Kodaira wire-wound rod, and the coated resin composition was dried in an oven. Subsequently, a PE film acting as a protective film was laminated onto the surface of the dried resin composition to obtain a photosensitive resin film (i.e., a composite film) wrapped with the protective film of Comparative Example 2. The conditions for coating and drying were as follows: the coating thickness was 85 μm, a drying temperature of 90°C was applied, a drying time of 19 minutes was used, and the thickness after drying was 60 μm.

[0128] [Comparative Example 3]

[0129] The following components were mixed and stirred for 5 hours to be uniformly mixed, thereby obtaining the resin composition of Comparative Example 3. 20 parts by weight of BNE200 epoxy resin, 60 parts by weight of BE507 epoxy resin, 20 parts by weight of CNE200ELA epoxy resin, 30 parts by weight of acetone, 4 parts by weight of triphenylsulfonium tetrakis(pentafluorophenyl)borate, 5 parts by weight of KBE-403 silane coupling agent, 0.06 parts by weight of solvent black, and 15 parts by weight of tetrahydrofuran.

[0130] The resin composition of Comparative Example 3 was coated onto a PET film acting as a protective film using a Kodaira wire-wound rod, and the coated resin composition was dried in an oven. Subsequently, a PE film acting as a protective film was laminated onto the surface of the dried resin composition to obtain a photosensitive resin film (i.e., a composite film) wrapped with the protective film of Comparative Example 3. The conditions for coating and drying were as follows: the coating thickness was 160 μm, a drying temperature of 100°C was applied, a drying time of 15 minutes was used, and the thickness after drying was 120 μm.

[0131] [Comparative Example 4]

[0132] The following components were mixed and stirred for 5 hours to be uniformly mixed, thereby obtaining the resin composition of Comparative Example 4. 30 parts by weight of BNE200 epoxy resin, 20 parts by weight of BE507 epoxy resin, 50 parts by weight of PNE177 epoxy resin, 25 parts by weight of acetone, 2 parts by weight of triphenylsulfonium hexafluoroantimonate, 0.3 parts by weight of diphenyliodonium tetrakis(pentafluorophenyl)borate, 5 parts by weight of KBE-403 silane coupling agent, 0.05 parts by weight of solvent blue, and 12 parts by weight of tetrahydrofuran.

[0133] The resin composition of Comparative Example 4 was coated onto a PET film acting as a protective film using a Kodaira wire-wound rod, and the coated resin composition was dried in an oven. Subsequently, a PE film acting as a protective film was laminated onto the surface of the dried resin composition to obtain a photosensitive resin film (i.e., a composite film) wrapped with the protective film of Comparative Example 4. The conditions for coating and drying were as follows: the coating thickness was 160 μm, a drying temperature of 100°C was applied, a drying time of 20 minutes was used, and the thickness after drying was 120 μm.

[0134] [Comparative Example 5]

[0135] The following components were mixed and stirred for 5 hours to be uniformly mixed, thereby obtaining the resin composition of Comparative Example 5. 20 parts by weight of BNE200 epoxy resin, 60 parts by weight of BE507 epoxy resin, 20 parts by weight of CNE200ELA epoxy resin, 25 parts by weight of acetone, 2 parts by weight of triphenylsulfonium hexafluoroantimonate, 5 parts by weight of KBE-403 silane coupling agent, 0.2 parts by weight of reactive yellow, 0.01 parts by weight of solvent black, and 15 parts by weight of tetrahydrofuran.

[0136] The resin composition of Comparative Example 5 was coated onto a PET film acting as a protective film using a Kodaira wire-wound rod, and the coated resin composition was dried in an oven. Subsequently, a PE film acting as a protective film was laminated onto the surface of the dried resin composition to obtain a photosensitive resin film (i.e., a composite film) wrapped with the protective film of Comparative Example 5. The conditions for coating and drying were as follows: the coating thickness was 140 μm, a drying temperature of 100°C was applied, a drying time of 20 minutes was used, and the thickness after drying was 95 μm.

[0137] 4.3. Testing of Photosensitive Resin Films

[0138] The characteristics of the photosensitive resin films of Examples 1 to 6 (E1 to E6) and Comparative Examples 1 to 5 (CE1 to CE5) were tested according to the above test method. The results are summarized in Tables 2-1 and 2-2.

[0139] [Table 2-1]

[0140]

[0141] [Table 2-2]

[0142]

[0143] As shown in Tables 2-1 and 2-2, the photoresist patterns formed after exposure and development of the photosensitive resin films of Examples 1 to 6 of the present application have an excellent cross-sectional profile (rectangular cross-section, short footing length) and low light transmittance (wavelength of 550 nanometers). Examples 1 to 6 show that if the film tensile strength of the photosensitive resin film is greater than 2, the silicone adhesion strength of the photosensitive resin film can be further improved.

[0144] On the other hand, the photoresist pattern formed after exposing and developing the photosensitive resin films of Comparative Examples 1 to 5 cannot simultaneously have a good cross-sectional profile and low light transmittance. Comparative Examples 1 and 3 are A 355It shows that if / T is lower or higher than the specified range of this application, the cross-sectional profile of the photoresist pattern will be defective. Comparative Examples 2 and 4 do not have at least one point in the spectrum where the first derivative is 0 and the second derivative is less than 0 within the first wavelength range, or A within the first wavelength range w1 It shows that if / T is smaller than the range specified in this application, the cross-sectional profile of the photoresist pattern is poor and the light transmittance is high, causing glare problems when applied to the packaging of an image sensor chip. Comparative Example 5 shows that the spectrum does not have at least one point within the first wavelength range where the first derivative is 0 and the second derivative is less than 0, and the absorbance within the second wavelength range is A w2 It shows that if / T ≤ 0.003 is not satisfied, the cross-sectional profile of the photoresist pattern is poor and the light transmittance is high, which causes glare problems when applied to the packaging of an image sensor chip.

[0145] The above examples are used to explain the principles and efficacy of the present application and to demonstrate the inventive features of the present application, and are not intended to limit the scope of the present application. Those skilled in the art may make various modifications and substitutions based on the disclosure and proposal of the described invention. Accordingly, the scope of protection of the present application is as defined in the appended claims.

Claims

Claim 1 As a photosensitive resin film having a thickness T in the μm range, when said photosensitive resin film is characterized by ultraviolet-visible spectroscopy, the resulting spectrum has an absorbance A at 355 nm. 355 With, 0.003 ≤ A 355 / T ≤ 0.03 and; the spectrum has at least one point within the first wavelength range where the first derivative is 0 and the second derivative is less than 0, and each of the points is independently A w1 It has the value / T, where w1 represents the corresponding wavelength of the above point, and A w1 represents the corresponding absorbance, and 0.003 ≤ A w1 / T; and the first wavelength range is greater than 450 nm to 780 nm, the thickness T is in the range of 20 μm to 200 μm, the photosensitive resin film is a negative dry film, and comprises a photopolymerization initiator selected from the group consisting of imidazole compounds, ketone compounds, quinone compounds, benzoin or benzoin ether compounds, polyhalogenated compounds, triazine compounds, organic peroxide compounds, and onium salt compounds. Claim 2 In paragraph 1, 0.003 ≤ A w1 A photosensitive resin film in which / T ≤ 0.

08. Claim 3 In claim 1, the photosensitive resin film, wherein the ultraviolet-visible spectroscopy is measured using an ultraviolet-visible spectrophotometer under the following conditions: the photosensitive resin film is positioned perpendicular to the direction of incident light; the diffraction grating is composed of a light splitter; the test temperature is 25°C; the test pressure is 1 atm; the analysis mode is absorbance; the scan wavelength range is 190 nm to 1100 nm; the blank sample is air; the scan rate is 2200 nm / min; the transition wavelength at which the light source switches from a deuterium lamp to a tungsten lamp is 340.8 nm; the sampling interval is 0.2 nm; and the slit width is 2.0 nm. Claim 4 In claim 1, the spectrum has an absorbance A at 450 nm. 450 With, 0 < A 450 A photosensitive resin film in which / T ≤ 0.

003. Claim 5 A photosensitive resin film according to claim 1, wherein the first wavelength range is greater than 480 nm and up to 730 nm. Claim 6 In paragraph 5, the absorbance of the spectrum at each wavelength within the second wavelength range is independently A w2 It is denoted as , where w2 represents the wavelength of the corresponding absorbance, and 0 ≤ A w2 A photosensitive resin film having / T ≤ 0.003 and the second wavelength range being 440 nm to 470 nm. Claim 7 A photosensitive resin film comprising an epoxy resin in any one of claims 1 to 6. Claim 8 A composite film comprising: a photosensitive resin film described in any one of claims 1 to 6; and a protective film on at least one surface of the photosensitive resin film. Claim 9 A package structure comprising: a substrate; a semiconductor device electrically connected to the substrate; and a package for encapsulating the semiconductor device, wherein the material of the package comprises a cured product of a photosensitive resin film described in any one of claims 1 to 6. Claim 10 A package structure according to claim 9, wherein the semiconductor device is an image sensor chip, and the image sensor chip has a photosensitive region; and the material of the package comprises a first portion formed from a cured photosensitive resin film and a second portion formed from a transparent material, wherein the first portion surrounds the image sensor chip laterally and the second portion is disposed over the photosensitive region. Claim 11 delete

Citation Information

Patent Citations

  • Photosensitive dry film

    CN114706274A

  • Photosensitive resin laminate

    KR1020230033718A

  • Photoresist film and application thereof

    KR1020240031884A

  • Photosensitive resin multilayer body

    WO2022085366A1