Refining method for recycling waste oil recovered from fabric tenter process
A multi-stage vacuum distillation and chemical treatment process purifies waste oil from fabric tenter processes, producing a refined product suitable for leather processing and coating applications, addressing the inadequacies of existing recycling methods.
Patent Information
- Application Number
- KR1020230185871
- Authority / Receiving Office
- KR · KR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-12-19
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2043-12-19
AI Technical Summary
Existing methods for recycling waste oil from fabric tenter processes fail to prepare the recovered oil into a state with sufficient physical properties for reuse, particularly in leather processing and coating applications.
A multi-stage vacuum distillation process followed by chemical treatments with activated clay and anhydrous magnesium or sodium sulfate is employed to purify waste oil, removing solvents, moisture, and impurities, resulting in a refined product suitable for use as a fatliquor or coating agent.
The refined waste oil achieves high solid content and purity, enabling its recycling as a leather softener and coating agent, improving leather quality and surface properties without color transfer or hazardous substance contamination.
Smart Images

Figure 112023142534895-PAT00001_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to a purification treatment method for recycling waste oil recovered from a fabric tenter process. Background Technology
[0002] The tenter process is a process that improves the quality of fibers by drying or ironing (heat treating) dyed fabrics, and chemicals such as water repellents, antistatic agents, and fabric softeners are used. These chemicals vaporize during the high-temperature (180~230℃) treatment process and are observed in complex forms such as white smoke, oil mist, and fine dust, causing odors.
[0003] Fabric softeners used as post-processing agents in the tenter process include anionic softeners such as emulsion emulsions of higher aliphatic sulfonates and higher alcohol sulfate esters, cationic softeners such as emulsion emulsions of higher alcohol quaternary ammonium salts and aminosilicones, and nonionic softeners such as emulsion emulsions of polyethylene glycol fatty acid esters, polyethylene glycol higher alcohol esters, exicylconones, and dimethylpolysiloxanes.
[0004] In addition, the components used as post-processing agents in the tenter process include water-repellent agents such as wax-based, urethane-based, acrylic-based, fluorine-based resins, silicone-based resins, and zirconium resins; antistatic agents such as cationic surfactants and anionic ester compounds (Polyoxyethylene mono fatty acid ester Polyoxyethylene alkyl ether Water); organic antibacterial agents composed of chemical structures such as phenol, triazine, isothiazolone, and imidazole; and inorganic antibacterial agents prepared with metal ions such as silver, zinc, and copper.
[0005] Accordingly, cyclone scrubbers, condensation-heating heat exchange facilities, electrostatic precipitators, and activated carbon filters are being used to treat complex air pollutants at the downstream end of tenter facilities, including particulate matter such as dust, fine dust, and oil mist, as well as gaseous substances such as VOCs and odors, with excellent efficiency and to recover and reuse heat from high-temperature exhaust gases.
[0006] There is a continuous demand for the provision of various technologies to recycle various types of waste recovered at the downstream end of such tenter processes.
[0007] In this regard, prior art for providing a method to manufacture a recyclable leather sheet using waste and scrap such as leather or textiles includes Korean Registered Patent Publication No. 10-1846665, titled "Method for manufacturing a recyclable leather sheet using waste and scrap such as leather or textiles and a recyclable leather sheet manufactured by said method" (hereinafter referred to as "prior art").
[0008] However, in the case of existing technologies for recycling waste oil recovered from fabric tenter processes, including conventional technology, there was a problem in that the waste oil separated and recovered from exhaust gas substances through an electrostatic precipitator at the end of the tenter process of dyed fabric was not prepared through sufficiently diverse treatment processes to a state with sufficient physical properties for recycling. The problem to be solved
[0009] The present invention was created to solve the above problems, and the objective of the present invention is to provide a method for purifying waste oil separated and recovered from exhaust gas substances through an electrostatic precipitator at the end of the tenter process into a state suitable for recycling by mixing it with a top coating agent in a coating process that includes a tanning process and a process of adding oil (fat) to give the leather softness and elasticity properties along with the tanning process during the processing of raw hides in the light color leather preparation process, or by mixing it with a top coating agent in a coating process that includes applying a resin liquid to the leather and drying it to form a resin film during the leather preparation process. means of solving the problem
[0010] To achieve the above objective, the purification treatment method for recycling waste oil recovered in a fabric tenter process according to the present invention comprises: Step A, wherein the waste oil separated and recovered from exhaust gas substances through an electrostatic precipitator at the downstream end of the tenter process of a dyed fabric is purified for recycling; and wherein the waste oil is subjected to primary vacuum distillation treatment at a temperature of 50°C to 70°C and a pressure of 700mmHg or higher to remove the solvent, and the distillate obtained from the primary vacuum distillation is subjected to secondary vacuum distillation treatment at a temperature of 70°C to 150°C and a pressure of 700mmHg or higher to recover the purified waste oil for the first time, and subsequently subjected to tertiary vacuum distillation treatment at a temperature of 150°C to 250°C and a pressure of 700mmHg or higher to additionally recover the purified waste oil for the second time; Step B, in which activated clay is reacted with the waste oil purified material recovered in the first and second stages through Step A, and then filtered to recover the filtrate; Step C, in which moisture is removed by depressurizing the waste oil reaction material filtered and recovered through Step B for 50 to 70 minutes under conditions of a temperature of 50°C to 70°C and a pressure of 700 mmHg or higher; and Step D, in which sodium sulfate anhydrous or magnesium sulfate anhydrous is reacted with the waste oil reaction material from which moisture has been removed through Step C, and then filtered to recover the filtrate.
[0011] Here, the waste oil purified product recovered in the first and second stages through the above A step is purified and recovered at a yield of 70 to 80 parts by weight based on 100 parts by weight of the waste oil recovered from the above tenter process of the dyed fabric, and has a solid content of 85 to 95% by weight.
[0012] In addition, Step B is a step of adding 4 to 6 parts by weight of activated clay to 100 parts by weight of the waste oil purified material recovered in the first and second stages through Step A, reacting it for 1 to 2 hours in a temperature environment of 90°C to 110°C, and then filtration to recover the filtrate.
[0013] In addition, the above step D is a step of preparing a final waste oil product by adding 4 to 6 parts by weight of sodium sulfate anhydrous or magnesium sulfate anhydrous, based on 100 parts by weight of the waste oil product recovered in the first and second stages through the above step A, to the waste oil reactant from which moisture has been removed through the above step C, reacting the mixture, and then recovering the filtrate through filtration treatment.
[0014] In addition, the final waste oil purified product prepared through the above step D is purified and recovered at a yield of 75 to 80 parts by weight based on 100 parts by weight of the waste oil recovered from the above tenter process of the dyed fabric, and has a solid content of 95 to 99% by weight. Effects of the invention
[0015] According to the present invention, waste oil separated and recovered from exhaust gas substances through an electrostatic precipitator at the end of the tenter process can be recycled as a fatliquor in the process of adding oil (fat) to give softness and elasticity to the leather in addition to the tanning process during the processing of raw hides in the light color leather preparation process, or can be prepared as a refined product suitable for recycling by mixing it into a top coating agent in a coating process that includes a coating process in which a resin liquid is applied to the leather and dried to form a resin film during the leather preparation process. Brief explanation of the drawing
[0016] FIG. 1 is a flowchart illustrating a purification treatment method for recycling waste oil recovered from the fabric tenter process of the present invention. Figure 2 is the result of performing Fourier transform infrared spectroscopy analysis on waste oil recovered from the fabric tenter process used in the purification treatment method of the present invention. Figure 3 is the result of performing an analysis using a thermogravimetric analyzer on waste oil recovered from the fabric tenter process used in the purification treatment method of the present invention. Figure 4 is the result of analyzing waste oil recovered from the fabric tenter process used in the purification treatment method of the present invention using a gas chromatography mass spectrometer. Specific details for implementing the invention
[0017] Preferred embodiments of the present invention will be described in more detail with reference to the attached drawings, provided that technical details that are already well known are omitted or compressed for the sake of brevity.
[0018] 1. Description of the purification treatment method for the recycling of waste oil recovered from the fabric tenter process
[0019] The purification treatment method for recycling waste oil recovered in the fabric tenter process of the present invention relates to a method for purifying waste oil separated and recovered from exhaust gas substances through an electrostatic precipitator at the downstream end of the tenter process of dyed fabric for recycling. Specifically, the process is described in detail below with reference to the flowchart of FIG. 1.
[0020] (1) Waste oil distillation treatment step<S110, A단계>
[0021] In this stage, the waste oil separated and recovered from the exhaust gas material through an electrostatic precipitator at the downstream end of the tenter process is subjected to multiple distillation treatments to obtain purified waste oil.
[0022] Here, waste oil refers to waste oil recovered from the electrostatic precipitator among the cyclone scrubber, condensation-heating heat exchanger, electrostatic precipitator, and activated carbon filter, which are operated in conjunction with the tenter process to improve the quality of the fiber by performing drying or heat-based ironing treatment on the dyed fabric.
[0023] Such waste oil has a composition mixed with various substances due to the tenter process, which involves drying by mixing chemicals such as fabric softeners, antistatic agents, water repellents, and gloss agents, rather than simple drying, while taking into account the degree of shrinkage and expansion that occurs when dyed fibers are washed.
[0024] Specifically, the results of analyzing the waste oil separated and recovered from the exhaust gas material through an electrostatic precipitator at the downstream end of the tenter process using Fourier-transform infrared spectroscopy (FT-IR) with Nicolet 10 are as shown in Figure 2 and Table 1 below.
[0025] Match Compound Name 89.50 Thermoplastic elastomer 89.16 Poly(acrylic acid, ammonium salt) 89.06 Poly(ethylene:propylene) 88.32 Sorbitan monostearate: Span 60
[0026] As shown in Figure 2 and Table 1, peaks of CH3 and CH2 stretching absorptions, which are Aliphatic Groups, were identified; in particular, the CH3 peak was at 2975–2950 cm⁻¹. -1 , 1470-1440 cm -1 CH2 is approximately 2870-2840cm -1 It could be observed in.
[0027] In addition, the ester absorption peak of the Aliphatic Ester Group is at 1750 cm⁻¹. -1 CO peak and 1300-1180 cm in the vicinity -1 The C=O peak could be qualitatively confirmed.
[0028] In addition, the results of analyzing waste oil separated and recovered from exhaust gas substances through an electrostatic precipitator at the downstream end of the tenter process using a thermogravimetric analysis (TGA) and a gas chromatography mass spectrometer (GC-MS) are as shown in Figures 3 and 4 and Table 2 below.
[0029] Retention Time(min) Putative compounds in the GC-MS Library RMF(%) Area(%) 6.463 Cyclotrisiloxane, hexamethyl- 87.9 0.09 10.606 Cyclotetrasiloxane, octamethyl- 86.0 0.09 18.353 E-11,13-Tetradecadien-1-ol 94.9 0.40 20.573 Benzene, 1,1'-[methylenebis(oxymethylene)]bis- 95.1 11.6 28.562 Oxalic acid, 2-ethylhexyl octadecyl ester 91.1 37.7 30.237 Octadecanoic acid, octyl ester 90.4 47.8 32.403 1-Decanol, 2-hexyl- 93.2 0.72 33.343 Hexadecanoic acid, dodecyl ester 94.8 1.57 - RMF (reverse match factor): The probability of matching a sample's spectrum based on the spectrum in the database.
[0030] Specifically, thermal analysis is a test analysis in which a sample is placed in a container, weighed, and then the weight is increased to confirm the weight loss. It was conducted using a TGA Q 500 (TA) at a heating rate of 10°C per minute under an inert gas nitrogen atmosphere, and the temperature range was set from room temperature to 800°C.
[0031] As shown in Fig. 3, the thermal analysis results of waste oil show that weight loss occurs starting from 100°C, which is presumed to be due to low molecular weight organic matter, moisture, or solvents. The weight loss rate increases significantly up to 261.78°C in the derivative weight obtained by differentiating the thermal analysis (TGA) curve, and this is determined to be due to the vaporization of organic matter. At temperatures thereafter, weight loss is expected to be due to thermal decomposition, combustion of organic matter, or combustion of elemental carbon such as carbon black.
[0032] In addition, as shown in Figure 4, gas chromatography-mass spectrometry (GC-MS) analysis results showed that 2-ethylhexyl octadecyl ester and octyl ester were detected in large proportions, and this result was identical to the result of confirming the ester peak in infrared spectroscopic analysis.
[0033] Specifically, stearic acid is a saturated fatty acid composed of 18 carbons, and its IUPAC name is octadecanoic acid. Since stearic acid esters are mainly used as fabric softeners, it is presumed that the main component of waste oil is stearic acid esters.
[0034] Furthermore, the waste oil separated and recovered from the exhaust gas through an electrostatic precipitator at the downstream end of the tenter process has a dark brown, mucilaginous appearance; more specifically, it has a pH of 3 to 4, a viscosity of 34 cPs, and a solid content of 90 to 92, and contains less than 5 mg / kg of cadmium (Cd), less than 10 mg / kg of lead (Pb), and hexavalent chromium (Cr 6+ It has a heavy metal content of less than 2 mg / kg and less than 1 mg / kg of mercury (Hg).
[0035] The process of distilling the recovered waste oil with such characteristics is divided into three stages and proceeds sequentially. To carry out the distillation process, a heating reactor, a distillation tube that provides a cooling function through water circulation, a vacuum pump, and a vacuum flask for storing the recovered material are used.
[0036] First, the waste oil is subjected to primary vacuum distillation at a temperature of 50°C to 70°C and a pressure of 700 mmHg or higher to remove the solvent.
[0037] Through this primary vacuum distillation treatment, water, low molecular weight organic matter, and volatile components are removed, amounting to 65 to 75 parts by weight of water, low molecular weight organic matter, and volatile components removed based on 500 parts by weight of recovered waste oil.
[0038] Next, the distillate obtained from the first vacuum distillation is subjected to a second vacuum distillation treatment at a temperature of 70°C to 150°C and a pressure of 700 mmHg or higher to recover the purified waste oil, and as a result, a portion of the recovered purified waste oil, including fatty acid esters, amounts to 150 to 175 parts by weight based on 500 parts by weight of the recovered waste oil.
[0039] In addition, a portion of the purified waste oil among the distilled products from the first vacuum distillation is subjected to a third vacuum distillation treatment at a temperature of 150°C to 250°C and a pressure of 700 mmHg or higher to additionally recover purified waste oil, and as a result, the remainder of the purified waste oil containing stearic acid, acetic acid, octyl, etc. recovered amounts to 160 to 235 parts by weight based on 500 parts by weight of the recovered waste oil.
[0040] Here, it is important that the temperature conditions during the third vacuum distillation process do not exceed 250°C to prevent polymerization of waste oil, and the first to third vacuum distillation processes are carried out using a reactor that can be stirred with a magnetic bar.
[0041] Accordingly, the waste oil purified product recovered in the first and second stages through this step (S110) is purified and recovered at a yield of 70 to 80 parts by weight based on 100 parts by weight of waste oil recovered from the tenter process of the dyed fabric, and has a solid content of 85 to 95% by weight.
[0042] As a result, the waste oil purified product recovered in the first and second stages through this step (S110) has an opaque and dark brown appearance, is purified and recovered at a yield of 70 to 80 parts by weight based on 100 parts by weight of waste oil recovered from the tenter process of the dyed fabric, and has a solid content of 85 to 95% by weight.
[0043] (2) Activated clay reaction step<S120, B단계>
[0044] In this step, the process of recovering the filtrate is carried out by reacting activated clay with the purified waste oil recovered in the first and second stages through the previous waste oil distillation treatment step (S110) and then filtering it.
[0045] Specifically, 4 to 6 parts by weight (most preferably 5 parts by weight) of activated clay are added to 100 parts by weight of the purified waste oil recovered in the first and second stages through the preceding waste oil distillation treatment step (S110), reacted for 1 to 2 hours at a temperature environment of 90°C to 110°C (most preferably 100°C), and then filtered to recover the filtrate containing the reacted activated clay, thereby removing primary impurities and improving color.
[0046] Here, the activated clay forms a surface with fine pores by leaching soluble substances within its structure through activation treatment, and the surface area is 150 m² 2 / g to 300m 2 / g, the average diameter of the pores is 30Å to 50Å.
[0047] The filtration process for this purpose uses filter paper, and the pore size can be 3 μm to 5 μm. Examples of products include Advantec’s NO.3 (Pore size: 5 μm), NO.5B (Pore size: 4 μm), NO.6 (Pore size: 3 μm), NO.7 (Pore size: 4 μm).
[0048] As a result, the waste oil reaction product filtered and recovered through this step (S120) has a transparent bright red appearance and has a solid content of 85 to 90 weight% due to the moisture contained in the activated clay.
[0049] (3) Depressurization step for moisture removal<S130, C단계>
[0050] In this step, the waste oil reaction product filtered and recovered through the previously performed activated clay reaction step (S120) is subjected to reduced pressure treatment for 50 to 70 minutes at a temperature of 50 to 70°C and a pressure of 700 mmHg or more to remove moisture.
[0051] As a result of performing vacuum treatment for 60 minutes at a temperature of 50°C to 70°C and a pressure of 70 cmHg to remove residual moisture before the reaction of anhydrous magnesium sulfate, it has a transparent crimson appearance and a solid content of 95 to 99 weight%.
[0052] (4) Anhydrous magnesium sulfate reaction step<S140, D단계>
[0053] In this step, a process is carried out to recover the filtrate by reacting anhydrous magnesium sulfate with the waste oil reactant from which moisture has been removed through the previous vacuum treatment step (S130) for moisture removal, and then filtering it.
[0054] Depending on the implementation, this step (S140) may be modified into a process of reacting sodium sulfate anhydrous with waste oil reactants from which moisture has been removed through the preceding moisture removal vacuum treatment step (S130), and then filtering to recover the filtrate, so that sodium sulfate anhydrous may be used instead of magnesium sulfate anhydrous.
[0055] Specifically, this step (S140) involves adding 4 to 6 parts by weight (most preferably 5 parts by weight) of magnesium sulfate anhydrous, based on 100 parts by weight of the waste oil purified product recovered in the first and second stages through the waste oil distillation treatment step (S110) prior to the waste oil reaction product from which moisture has been removed through the previous moisture removal vacuum treatment step (S130), reacting the mixture, and then filtering it to recover a filtrate containing sodium sulfate anhydrous or magnesium sulfate anhydrous to prepare the final waste oil purified product.
[0056] The filtration process for this purpose uses filter paper, and the pore size can be 3 μm to 5 μm. Examples of products include Advantec’s NO.3 (Pore size: 5 μm), NO.5B (Pore size: 4 μm), NO.6 (Pore size: 3 μm), NO.7 (Pore size: 4 μm).
[0057] Through this, the final purified waste oil product has a transparent crimson appearance, with the removal of residual moisture and improvement of color being more effectively achieved, and is purified and recovered at a yield of 75 to 80 parts by weight based on 100 parts by weight of waste oil recovered from the tenter process of the dyed fabric, and has a solid content of 95 to 99% by weight.
[0058] In addition, the final waste oil product contains cadmium (Cd), lead (Pb), and hexavalent chromium (Cr 6+ Heavy metals such as mercury (Hg) and others were not detected at all.
[0059] These final refined waste oils can be recycled as fats in the light color leather preparation process. This process involves adding oil (fat) to the raw hides to impart softness and elasticity to the leather, alongside the tanning and tanning processes.
[0060] In addition, the final refined waste oil can be recycled by being mixed into a top coating agent in a painting process that includes a coating process in which a resin solution is applied to the leather and dried to form a resin film during the leather preparation process.
[0061] 2. Description of the application test of the final purified product that has undergone the purification treatment method for the recycling of waste oil recovered from the fabric tenter process
[0062] (1) Test to confirm the possibility of recycling the final waste oil as a branch.
[0063] The final purified waste oil produced through the purification treatment method for recycling waste oil recovered in the fabric tenter process of the present invention was confirmed to have the potential to be used as a light color agent that imparts flexibility to leather without causing color change and has excellent lightfastness.
[0064] First, to hydrophilize the final waste oil purified product produced through a purification treatment method for recycling waste oil recovered from a single tenter process, Lauryl alcohol ethylene oxide (LAE), a primary ethoxylated alcohol-based nonionic surfactant that is not sensitive to pH and water hardness and has a relatively low CMC compared to ionic surfactants, was used.
[0065] Here, LAE-3, LAE-5, LAE-7, and LAE-9, which have a carbon length of 12 and ethylene oxide (EO) addition moles of 3, 5, 7, and 9 moles, were selected and formulated with compositions as shown in Table 3 (unit: g) below to prepare Experimental Examples 1 to 16, and the separation safety of each experimental example was confirmed based on 3 months.
[0066] Experimental Example Final waste oil purification LAE-3 LAE-5 LAE-7 LAE-9 Methanol Water stability 1 35 1 - - - 3 60 separation 2 35 3 - - - 3 60 separation 3 35 5 - - - 3 60 stability 4 35 7 - - - 3 60 stability 5 35 - 1 - - 3 60 separation 6 35 - 3 - - 3 60 separation 7 35 - 5 - - 3 60 separation 8 35 - 7 - - 3 60 separation 9 35 - - 1 - 3 60 separation 10 35 - - 3 - 3 60 separation 11 35 - - 5 - 3 60 separation 12 35 - - 7 - 3 60 separation 13 35 - - - 1 3 60 separation 14 35 - - - 3 3 60 separation 15 35 - - - 5 3 60 separation 16 35 - - - 7 3 60 separation
[0067] As shown in Table 3, as the lower the molar amount of LAE, the smaller the HLB value (indicating hydrophobicity), and as the higher the molar amount, the larger the HLB value (indicating hydrophilicity), it was found that stability was ensured without layer separation in Experimental Examples 3 and 4, in which 14 to 20 parts by weight of the hydrophobic LAE-3 were used per 100 parts by weight of the final purified waste oil.
[0068] Accordingly, the leather preparation characteristics using the final waste oil purified product blended by applying LAE-3 according to Experimental Examples 3 and 4 showed a light brown color, a solid content of 37 wt% (based on KS M 6638), and a solubility of 98.3% (based on KS K ISO 105-Z09).
[0069] Accordingly, the neutralizing process in the leather preparation process is carried out at a temperature of 35°C for 30 minutes using a composition of 200 parts by weight of water, 2 parts by weight of Tanigan BS2, 1.5 parts by weight of sodium foroxide, and 1.5 parts by weight of sodium nitrate, followed by draining and rinsing. Subsequently, the fatliquoring process is carried out at a temperature of 60°C for 60 minutes using a composition of 100 parts by weight of water, 5 parts by weight of fatliquoring agent, and 1.5 parts by weight of formic acid (1:10), followed by draining and rinsing.
[0070] The eggplant agent used here is composed by varying the ratio of the commercial eggplant agent (Freefat WRF (White Eggplant Agent), Pretech) and Experimental Example 3 for each example.
[0071] Finally, the physical properties of the leather fabric prepared by sequentially carrying out the processes of Horse up, Vacuum dryer (55℃, 240sec.), and Vibration staking (3 steps) were inspected, and the results are as shown in Table 4 below.
[0072] Example 1 Example 2 Example 3 Example 4 Gajije Gajije Gajije Gajije Commercial Experimental Example 3 Commercial Experimental Example 3 Commercial Experimental Example 3 Commercial Experimental Example 3 10 - 7 3 5 5 - 10 Flexibility (mm) 3.5 3.4 3.2 2.5 touch Oilish & Waxy Oilish & Waxy Oilish & Dry Dry Color transfer - Slight ear inflammation otitis otitis Stability with commercially available ingredients - stability stability -
[0073] As shown in Table 4, when the commercial eggplant agent and Experimental Example 3 were mixed in a 7:3 ratio, equivalent physical properties and tactile sensations were confirmed compared to when the commercial eggplant agent was used alone. Regarding the leather preparation, slight color transfer of the leather occurred, but no color transfer phenomenon was observed when dyes (red, green, brown, etc.) were added.
[0074] (2) Test to confirm the possibility of recycling the final waste oil as a coating agent
[0075] Next, regarding the final waste oil purified product produced through the purification treatment method for recycling waste oil recovered in the fabric tenter process of the present invention, it was confirmed whether it is recyclable when mixed with a top coating agent on base-coated leather in relation to a coating process that includes applying a resin liquid to leather and drying it to form a resin film in order to protect the leather from moisture or dust and obtain surface effects such as gloss.
[0076] First, the top coating agent was composed of 50 parts by weight of Pigment (White), 80 parts by weight of Compact Binder, 130 parts by weight of Acryl Binder, 100 parts by weight of Water Dispersible PU Binder, 80 parts by weight of Wax, and 560 parts by weight of Water. The final waste oil purified product was mixed with the Wax component for each example, and physical property tests were conducted for each example.
[0077] Specifically, the coating process for each example proceeds sequentially with Formulation (Binder, Pigment, Wax), Blending (Homogenizer: 5,200 rpm, 30 min), Roll coating, Dry (80℃, 2 min), and Finishing leather, and the physical property test results of the resulting product are as shown in Table 5 below.
[0078] Example 5 Example 6 Example 7 Example 8 Wax Wax Wax Wax Wax Final waste oil purification Wax Final waste oil purification Wax Final waste oil purification Wax Final waste oil purification 80 - 60 20 40 40 0 100 Wear resistance (mg.loss) 78.5 80.8 76.4 79.8 Flexion test 20,000↑ 20,000↑ 20,000↑ 20,000↓ UV test 3-4 3-4 3-4 3 Rupture strength 39.8 38.2 36.8 38.9 appearance Good Good Good Good
[0079] As shown in Table 5, when the final waste oil refined product was mixed with commercial wax in a ratio of 40 parts by weight or more to 80 to 100 parts by weight of the total wax composition, equivalent physical properties and appearance were confirmed compared to when the existing wax was used alone, and no color transfer of the coated leather was confirmed.
[0080] In addition, it was confirmed that the KC safety standard test analysis results did not detect arylamine and four other items, which are hazardous substances, in the coated leather manufactured in this manner.
[0081] The embodiments disclosed in this invention are intended to illustrate, not limit, the technical concept of the invention, and the scope of the technical concept of the invention is not limited by these embodiments. The scope of protection shall be interpreted by the claims below, and all technical concepts within an equivalent scope shall be interpreted as being included within the scope of rights of this invention.
Claims
Claim 1 A method for purifying waste oil separated and recovered from exhaust gas substances via an electrostatic precipitator at the downstream end of a tenter process of a dyed fabric for recycling, comprising: Step A, in which the waste oil is subjected to primary vacuum distillation at a temperature of 50°C to 70°C and a pressure of 700mmHg or higher to remove a solvent, and the distillate obtained from the primary vacuum distillation is subjected to secondary vacuum distillation at a temperature of 70°C to 150°C and a pressure of 700mmHg or higher to recover the purified waste oil for the first time, and subsequently subjected to tertiary vacuum distillation at a temperature of 150°C to 250°C and a pressure of 700mmHg or higher to recover the purified waste oil for the second time; Step B, in which activated clay is reacted with the purified waste oil recovered in the first and second stages through Step A above, and then filtered to recover the filtrate; Step C, in which moisture is removed by depressurizing the waste oil reaction product filtered and recovered through Step B above for 50 to 70 minutes under conditions of a temperature of 50°C to 70°C and a pressure of 700 mmHg or higher; A purification treatment method for recycling waste oil recovered from a fabric tenter process, comprising: a step D in which sodium sulfate anhydrous or magnesium sulfate anhydrous is reacted with the waste oil reactant from which moisture has been removed through step C, and then filtered to recover the filtrate; wherein step B is a step in which 4 to 6 parts by weight of activated clay are added to 100 parts by weight of the purified waste oil recovered in the first and second stages through step A, reacted for 1 to 2 hours in a temperature environment of 90°C to 110°C, and then filtered to recover the filtrate. Claim 2 A purification treatment method for recycling waste oil recovered from a fabric tenter process, characterized in that, in claim 1, the purified waste oil recovered in the first and second stages through step A is purified and recovered at a yield of 70 to 80 parts by weight based on 100 parts by weight of the waste oil recovered from the tenter process of the dyed fabric, and has a solid content of 85 to 95% by weight. Claim 3 delete Claim 4 A purification treatment method for recycling waste oil recovered in a fabric tenter process according to claim 1, wherein step D is a step of adding 4 to 6 parts by weight of sodium sulfate anhydrous or magnesium sulfate anhydrous, based on 100 parts by weight of the waste oil purified product recovered in the first and second stages through step A, to the waste oil reactant from which moisture has been removed through step C, reacting the mixture, and then filtration to recover the filtrate to prepare a final waste oil purified product. Claim 5 A purification treatment method for recycling waste oil recovered from a fabric tenter process, characterized in that, in claim 4, the final purified waste oil prepared through step D is purified and recovered at a yield of 75 to 80 parts by weight based on 100 parts by weight of the waste oil recovered from the tenter process of the dyed fabric, and has a solid content of 95 to 99% by weight.
Citation Information
Patent Citations
Preparation method of lithium-based recycled grease using waste oil
KR100715742B1
Exhaust gas elutriation and oil recovery system of dyeing tenter process
KR101581668B1
Recycling method for mineral oil-based waste oil
KR1019860007356A
Catalyst composition and method for the reproduction of waste oil
KR1019900003888B1
System for Refining Waste Oil
KR2020100009287U