Apparatus for manufacturing sintered ore and method for manufacturing sintered ore

The apparatus and method enhance sintered ore manufacturing by using multi-sensor feedback to accurately control sintering trolley speed and raw material supply, improving the sintering completion point accuracy and quality.

KR103046845B1Active Publication Date: 2026-11-10POHANG IRON & STEEL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
KR1020210167156
Authority / Receiving Office
KR · KR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-11-29
Publication Date
2026-11-10
Estimated Expiration
2041-11-29

AI Technical Summary

Technical Problem

Conventional sintered ore manufacturing devices inaccurately determine the sintering completion point, leading to reduced usability and increased production of defective products due to temperature measurement failures in high-temperature environments.

Method used

A sintered ore manufacturing apparatus and method that utilize multiple sensors to measure gas temperature, carbon monoxide concentration, and oxygen concentration to calculate an averaged sintering completion point, controlling the movement speed of sintering trolleys and raw material supply to achieve a preset target completion point.

Benefits of technology

Significantly improves the accuracy of sintering completion point determination, minimizing quality deviations and maximizing the production of high-quality sintered ore.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 112021137928906-PAT00001_ABST
    Figure 112021137928906-PAT00001_ABST
Patent Text Reader

Abstract

A sintered ore manufacturing device comprises a plurality of sintering trolleys, an ignition furnace, a plurality of wind boxes, a temperature measuring device for measuring the temperature of a gas passing through the plurality of wind boxes, a carbon monoxide concentration measuring device for measuring the carbon monoxide concentration of the gas passing through the plurality of wind boxes, and a control unit connected to the plurality of sintering trolleys, the temperature measuring device, and the carbon monoxide concentration measuring device, and controlling the movement speed of the plurality of sintering trolleys based on a calculated sintering completion point calculated by averaging a first sintering completion point where the temperature of the gas measured by the temperature measuring device is maximum and a second sintering completion point where the carbon monoxide concentration of the gas measured by the carbon monoxide concentration measuring device is minimum.
Need to check novelty before this filing date? Find Prior Art

Description

Technology Field

[0001] This description relates to an apparatus for manufacturing sintered ore and a method for manufacturing sintered ore. Background Technology

[0002] Generally, a sintered ore manufacturing device is a device that sinters pulverized iron ore into sintered ore of a size suitable for use in a blast furnace. The sintered ore manufacturing device loads the sintering raw material, which is a mixture and granulated of the main raw material (pulverized iron ore), auxiliary raw materials (limestone and quicklime), and solid fuels (pulverized coke and atomized briquettes), into a sintering trolley; ignites the surface of the sintered raw material loaded into the sintering trolley in an ignition furnace; and produces sintered ore by suctioning the interior of the sintering trolley through a wind box.

[0003] Conventional sintering ore manufacturing devices identify the location where the temperature of the gas sucked in through the wind box is highest as the current burn-through point (BTP) and control the movement speed of the sintering trolley to move the current burn-through point to a preset target burn-through point.

[0004] However, conventional sintered ore manufacturing devices determine the sintering completion point solely by utilizing the temperature of the gas sucked in through the wind box. Consequently, errors in calculating the completion point easily occur when the thermometer fails in high-temperature environments, leading to reduced usability. Furthermore, since the sintering speed is controlled by calculating the completion point even when the overall sintering temperature is low, there is a problem that a large number of defective products can be manufactured. The problem to be solved

[0005] One embodiment aims to provide a sintering ore manufacturing apparatus and a sintering ore manufacturing method that significantly improve the target hit rate for the sintering completion point, minimize deviations in sintering ore quality, and maximize the production of high-quality sintering ore. means of solving the problem

[0006] One aspect provides a sintering ore manufacturing apparatus comprising: a plurality of sintering trolleys that move along a movement path and have raw materials loaded inside; an ignition furnace that ignites the raw materials at the top of the plurality of sintering trolleys; a plurality of wind boxes arranged along the movement path at the bottom of the plurality of sintering trolleys and sucking in gas inside the plurality of sintering trolleys; a temperature measuring device that measures the temperature of the gas passing through the plurality of wind boxes; a carbon monoxide concentration measuring device that measures the carbon monoxide concentration of the gas passing through the plurality of wind boxes; and a control unit connected to the plurality of sintering trolleys, the temperature measuring device, and the carbon monoxide concentration measuring device, and controlling the movement speed of the plurality of sintering trolleys based on a calculated sintering completion point calculated by averaging a first sintering completion point where the temperature of the gas measured by the temperature measuring device is maximum and a second sintering completion point where the carbon monoxide concentration of the gas measured by the carbon monoxide concentration measuring device is minimum.

[0007] The above control unit can control the movement speed of the plurality of sintering trolleys so that the calculation sintering completion point moves to a preset target sintering completion point.

[0008] The apparatus further includes an oxygen concentration meter for measuring the oxygen concentration of the gas passing through the plurality of wind boxes, and the control unit is connected to the oxygen concentration meter, and the calculated sintering completion point calculated by the control unit may be the average of the first sintering completion point, the second sintering completion point, and the third sintering completion point in which the oxygen concentration of the gas measured by the oxygen concentration meter is 15% or higher.

[0009] The system further includes a raw material supply unit that supplies the raw material to the plurality of sintering trolleys, and the control unit is connected to the raw material supply unit and can control the supply amount of the raw material based on the calculated sintering completion point.

[0010] The supply amount of the above raw material may be proportional to the movement speed of the plurality of sintering carts controlled based on the calculated sintering completion point.

[0011] The apparatus further includes a main duct connected to the lower part of the plurality of wind boxes to discharge the gas as exhaust gas, and an exhaust gas temperature measuring device that measures the temperature of the exhaust gas passing through the main duct, wherein the control unit is connected to the exhaust gas temperature measuring device and can correct the movement speed of the plurality of sintering trolleys based on the difference between the temperature of the exhaust gas measured by the exhaust gas temperature measuring device and a preset average exhaust gas temperature.

[0012] The system further includes a flue gas pressure gauge for measuring the pressure of the flue gas passing through the main duct, and the control unit is connected to the flue gas pressure gauge and can correct the movement speed of the plurality of sintering trolleys based on the difference between the flue gas pressure measured by the flue gas pressure gauge and a preset average flue gas pressure.

[0013] Additionally, one aspect provides a method for manufacturing sintered ore comprising the steps of: measuring the temperature of a gas passing through a plurality of wind boxes arranged along a movement path and sucking gas inside the plurality of sintering trolleys, wherein the wind boxes are positioned below a plurality of sintering trolleys loaded with raw materials moving along a movement path; measuring the carbon monoxide concentration of the gas passing through the plurality of wind boxes; calculating a calculated sintering completion point which is the average of a first sintering completion point where the gas temperature is maximum and a second sintering completion point where the carbon monoxide concentration is minimum; and controlling the movement speed of the plurality of sintering trolleys based on the calculated sintering completion point.

[0014] The step of controlling the movement speed of the plurality of sintering trolleys can be performed by controlling the movement speed of the plurality of sintering trolleys so that the calculated sintering completion point moves to a preset target sintering completion point.

[0015] The method further includes the step of measuring the oxygen concentration of the gas passing through the plurality of wind boxes, and the step of calculating the calculated sintering completion point can be performed by calculating the average of the first sintering completion point, the second sintering completion point, and the third sintering completion point in which the oxygen concentration of the gas is 15% or more.

[0016] The method may further include a step of controlling the supply amount of the raw material loaded into the plurality of sintering carts based on the above-mentioned calculation sintering completion point.

[0017] The supply amount of the above raw material may be proportional to the movement speed of the plurality of sintering carts controlled based on the calculated sintering completion point.

[0018] The method further includes the step of measuring the temperature of the exhaust gas passing through a main duct connected to the lower part of the plurality of wind boxes and discharging the gas as exhaust gas, and the step of controlling the movement speed of the plurality of sintering trolleys can be performed by correcting the movement speed of the plurality of sintering trolleys based on the difference between the temperature of the exhaust gas and a preset average temperature of the exhaust gas.

[0019] The method further includes a step of measuring the pressure of the exhaust gas, and the step of controlling the movement speed of the plurality of sintering trolleys can be performed by correcting the movement speed of the plurality of sintering trolleys based on the difference between the pressure of the exhaust gas and a preset average pressure of the exhaust gas. Effects of the invention

[0020] According to one embodiment, a sintering ore manufacturing apparatus and a sintering ore manufacturing method are provided, which significantly improve the target hit rate for the sintering completion point, minimize deviations in sintering ore quality, and maximize the production of high-quality sintering ore. Brief explanation of the drawing

[0021] FIG. 1 is a drawing showing a sintered ore manufacturing apparatus according to one embodiment. FIG. 2 is a graph showing one example and another example of a first sintering completion point, a second sintering completion point, and a third sintering completion point of a sintered ore manufacturing device according to one embodiment. FIG. 3 is a flowchart illustrating a method for manufacturing sintered ore according to another embodiment. FIG. 4 is a flowchart showing an example of a method for manufacturing sintered ore according to another embodiment. FIG. 5 is a table showing values ​​according to an example of a method for manufacturing sintered ore according to another embodiment. Specific details for implementing the invention

[0022] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings so that those skilled in the art can easily implement the present invention. The present invention may be embodied in various different forms and is not limited to the embodiments described herein.

[0023] To clearly explain the present invention, parts unrelated to the explanation have been omitted, and the same reference numerals are used for identical or similar components throughout the specification.

[0024] Furthermore, throughout the specification, when a part is described as "including" a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but may include additional components.

[0025] Hereinafter, a sintered ore manufacturing apparatus according to one embodiment will be described with reference to FIGS. 1 and FIGS. 2.

[0026] FIG. 1 is a drawing showing a sintered ore manufacturing apparatus according to one embodiment.

[0027] Referring to FIG. 1, a sintered ore manufacturing device according to one embodiment includes a raw material supply unit (100), a plurality of sintering trolleys (200), an ignition furnace (300), a plurality of wind boxes (400), a temperature measuring device (500), a carbon monoxide concentration measuring device (600), an oxygen concentration measuring device (700), a main duct (800), an exhaust gas temperature measuring device (900), an exhaust gas pressure measuring device (950), and a control unit (1000).

[0028] The raw material supply unit (100) supplies sintering raw materials, which are a mixture and assembly of the main raw material, iron ore, auxiliary raw materials, limestone and quicklime, and solid fuels, pulverized coke and sprayed briquettes, to a plurality of sintering trolleys (200). The raw material supply unit (100) is connected to a control unit (1000), and the amount of raw materials supplied by the raw material supply unit (100) is controlled by the control unit (1000).

[0029] A plurality of sintering trolleys (200) move along a movement path. Raw materials supplied from a raw material supply unit (100) are loaded into the interiors of the plurality of sintering trolleys (200). The plurality of sintering trolleys (200) can form an effective image distance of 100m along the movement path where sintering ore is formed, but are not limited thereto. The plurality of sintering trolleys (200) are connected to a control unit (1000), and the movement speed of the plurality of sintering trolleys (200) can be controlled by the control unit (1000). For example, the movement speed of the plurality of sintering trolleys (200) can be controlled by a control unit (1000) that controls the rotational speed of a sprocket, which is a means for driving the plurality of sintering trolleys (200), but is not limited thereto.

[0030] The ignition furnace (300) ignites the surface of the raw material loaded inside the plurality of sintering trolleys (200) from the upper part of the plurality of sintering trolleys (200). The raw material ignited by the ignition furnace (300) is sintered into sintered ore as the plurality of sintering trolleys (200) move along the movement path.

[0031] Multiple wind boxes (400) are arranged along a movement path below multiple sintering trolleys (200). The multiple wind boxes (400) draw in gas from inside the multiple sintering trolleys (200). Gas generated by the sintering reaction of raw materials inside the multiple sintering trolleys (200) is moved to the main duct (800) through the multiple wind boxes (400). The multiple wind boxes (400) are arranged as wind boxes 1 through 25 at intervals of 4m in an effective imaging distance of 100m, and the interiors of the wind boxes (400) from number 16 onwards may be evenly divided, but are not limited thereto.

[0032] A temperature measuring device (500) measures the temperature of the gas passing through a plurality of wind boxes (400). The temperature measuring device (500) includes a plurality of temperature sensors located inside the plurality of wind boxes (400). The temperature measuring device (500) measures the temperature of the gas passing through the plurality of wind boxes (400) using the plurality of temperature sensors. The temperature measuring device (500) is connected to a control unit (1000), and the temperature of the gas measured by the temperature measuring device (500) is transmitted to the control unit (1000).

[0033] A carbon monoxide concentration meter (600) measures the carbon monoxide concentration of gas passing through multiple wind boxes (400). The carbon monoxide concentration meter (600) includes multiple carbon monoxide concentration sensors located inside multiple wind boxes (400). The carbon monoxide concentration meter (600) measures the carbon monoxide concentration of gas passing through multiple wind boxes (400) using multiple carbon monoxide concentration sensors. The carbon monoxide concentration meter (600) is connected to a control unit (1000), and the carbon monoxide concentration of the gas measured by the carbon monoxide concentration meter (600) is transmitted to the control unit (1000).

[0034] The oxygen concentration meter (700) measures the oxygen concentration of the gas passing through the plurality of wind boxes (400). The oxygen concentration meter (700) includes a plurality of oxygen concentration sensors located inside the plurality of wind boxes (400). The oxygen concentration meter (700) measures the oxygen concentration of the gas passing through the plurality of wind boxes (400) using the plurality of oxygen concentration sensors. The oxygen concentration meter (700) is connected to the control unit (1000), and the oxygen concentration of the gas measured by the oxygen concentration meter (700) is transmitted to the control unit (1000).

[0035] The main duct (800) is connected to the lower part of a plurality of wind boxes (400). The main duct (800) discharges gas through the plurality of wind boxes (400) as exhaust gas. The exhaust gas through the main duct (800) may be transferred to a chimney via a dust collector, a large blower, and a cleaning facility, but is not limited thereto.

[0036] The exhaust gas temperature measuring device (900) measures the temperature of the exhaust gas passing through the main duct (800). The exhaust gas temperature measuring device (900) measures the temperature of the exhaust gas passing through the main duct (800) using a temperature sensor located inside the main duct (800). The exhaust gas temperature measuring device (900) is connected to a control unit (1000), and the temperature of the exhaust gas measured by the exhaust gas temperature measuring device (900) is transmitted to the control unit (1000).

[0037] The exhaust gas pressure gauge (950) measures the pressure of the exhaust gas passing through the main duct (800). The exhaust gas pressure gauge (950) measures the pressure of the exhaust gas passing through the main duct (800) using a pressure sensor located inside the main duct (800). The exhaust gas pressure gauge (950) is connected to the control unit (1000), and the pressure of the exhaust gas measured by the exhaust gas pressure gauge (950) is transmitted to the control unit (1000).

[0038] The control unit (1000) is connected to a raw material supply unit (100), a plurality of sintering trolleys (200), a temperature measuring device (500), a carbon monoxide concentration measuring device (600), an oxygen concentration measuring device (700), an exhaust gas temperature measuring device (900), and an exhaust gas pressure measuring device (950), and calculates a calculated sintering completion point and controls the movement speed of the plurality of sintering trolleys (200) so that the calculated sintering completion point moves to a preset target sintering completion point.

[0039] FIG. 2 is a graph showing one example and another example of the first sintering completion point, the second sintering completion point, and the third sintering completion point of a sintered ore manufacturing apparatus according to one embodiment. FIG. 2 (A) shows an example where the first sintering completion point, the second sintering completion point, and the third sintering completion point coincide, and FIG. 2 (B) shows another example where the first sintering completion point, the second sintering completion point, and the third sintering completion point do not coincide. In FIG. 2, the X-axis represents the effective image distance, the Y-axis on the left represents the gas concentration, and the Y-axis on the right represents the gas temperature.

[0040] Referring to FIG. 2 and FIG. 1, the control unit (1000) controls the movement speed of a plurality of sintering carts (200) based on a calculated sintering completion point calculated by averaging the first sintering completion point (BTP1) where the gas temperature measured by the temperature meter (500) is maximum and the second sintering completion point (BTP2) where the carbon monoxide concentration of the gas measured by the carbon monoxide concentration meter (600) is minimum. The control unit (1000) controls the movement speed of a plurality of sintering carts (200) based on a calculated sintering completion point calculated by averaging the first sintering completion point (BTP1) where the gas temperature measured by the temperature meter (500) is maximum, the second sintering completion point (BTP2) where the carbon monoxide concentration of the gas measured by the carbon monoxide concentration meter (600) is minimum, and the third sintering completion point (BTP3) where the oxygen concentration of the gas measured by the oxygen concentration meter (700) is 15% or more. The control unit (1000) controls the movement speed of a plurality of sintering trolleys (200) so that the calculated sintering completion point, which is the average of the first sintering completion point (BTP1), the second sintering completion point (BTP2), and the third sintering completion point (BTP3), moves to a preset target sintering completion point.

[0041] For example, the control unit (1000) may increase the movement speed of a plurality of sintering carts (200) when the calculated sintering completion point within the effective image distance is smaller than the target sintering completion point, but is not limited thereto.

[0042] As another example, the control unit (1000) may reduce the movement speed of a plurality of sintering carts (200) when the calculated sintering completion point within the effective image distance is greater than the target sintering completion point, but is not limited thereto.

[0043] Additionally, the control unit (1000) controls the raw material supply unit (100) based on the calculated sintering completion point to control the supply amount of raw material loaded into a plurality of sintering carts (200). Here, the supply amount of raw material controlled by the control unit (1000) is proportional to the movement speed of the plurality of sintering carts (200) controlled based on the calculated sintering completion point.

[0044] For example, if the calculated sintering completion point within the effective image distance is smaller than the target sintering completion point, the control unit (1000) may increase the movement speed of the plurality of sintering carts (200) and increase the amount of raw material supplied by the raw material supply unit (100), but is not limited thereto. Meanwhile, if the sintering completion point is set as a distance from the end point rather than from the start point within the effective image distance, the control unit (1000) may decrease the movement speed of the plurality of sintering carts (200) and decrease the amount of raw material supplied by the raw material supply unit (100), but is not limited thereto.

[0045] As another example, if the calculated sintering completion point within the effective image distance is greater than the target sintering completion point, the control unit (1000) may reduce the movement speed of the plurality of sintering carts (200) and simultaneously reduce the amount of raw material supplied by the raw material supply unit (100), but is not limited thereto. Meanwhile, if the sintering completion point is set as a distance from the end point rather than from the start point within the effective image distance, if the calculated sintering completion point within the effective image distance is greater than the target sintering completion point, the control unit (1000) may increase the movement speed of the plurality of sintering carts (200) and simultaneously increase the amount of raw material supplied by the raw material supply unit (100), but is not limited thereto.

[0046] Additionally, the control unit (1000) corrects the movement speed of a plurality of sintering trolleys (200) based on the difference between the temperature of the exhaust gas measured by the exhaust gas temperature measuring device (900) and the preset average temperature of the exhaust gas, and corrects the movement speed of a plurality of sintering trolleys (200) based on the difference between the pressure of the exhaust gas measured by the exhaust gas pressure measuring device (950) and the preset average pressure of the exhaust gas.

[0047] The control unit (1000) inputs a preset target sintering completion point, average flue gas temperature, and average flue gas pressure for selecting a production priority or quality priority operating condition mode according to the operating situation and for speed control of the sintering trolleys (200), and then continuously measures the temperature of the gas, the carbon monoxide concentration of the gas, and the oxygen concentration of the gas transmitted from a temperature measuring device (500), a carbon monoxide concentration measuring device (600), and an oxygen concentration measuring device (700) that measure the gas passing through a plurality of wind boxes (400) installed at an effective image distance at 4-second intervals, converts the data into digital signals in an A / D converter, and then transmits them to a process computer.

[0048] The process computer calculates the sintering completion point by combining the gas temperature, carbon monoxide concentration, and oxygen concentration measured in real-time at the effective imaging distance.

[0049] When the sintering reaction of the raw materials loaded into the multiple sintering trolleys (200) is completed at the effective image distance, cooling begins, so the point with the highest temperature at the effective image distance before cooling is designated as the first sintering completion point (BTP1). At this time, the reliability of selecting the highest temperature location is improved by dividing the interior of the wind box (400) evenly.

[0050] In addition, when the sintering reaction of the raw materials loaded into the multiple sintering trolleys (200) is completed at the effective image distance, the concentration of carbon monoxide generated during the incomplete combustion of carbon contained in the raw materials becomes minimum, so the point where the carbon monoxide concentration is minimum is designated as the second sintering completion point (BTP2).

[0051] In addition, when the sintering reaction of the raw materials loaded into the multiple sintering trolleys (200) at the effective image distance is completed, the oxygen concentration of the gas rises above the reference value, so a point where the oxygen concentration is 15% or higher is designated as the third sintering completion point (BTP3).

[0052] The first sintering completion point (BTP1), the second sintering completion point (BTP2), and the third sintering completion point (BTP3), which are three points of the temperature, carbon monoxide concentration, and oxygen concentration of the gas generated during suction in multiple wind boxes (400), can all coincide or be reached at the effective image distance, and when the first sintering completion point (BTP1), the second sintering completion point (BTP2), and the third sintering completion point (BTP3) do not coincide, the first sintering completion point (BTP1) and the second sintering completion point (BTP2) may be prioritized, but are not limited thereto.

[0053] The control unit (1000) calculates a deviation by comparing the calculated sintering completion point, which is the average of the first sintering completion point (BTP1), the second sintering completion point (BTP2), and the third sintering completion point (BTP3), with the preset target sintering completion point according to the operation mode setting. For example, if the calculated sintering completion point is smaller than the target sintering completion point, the control unit (1000) can increase the speed of the sintering machine, which is the movement speed of the multiple sintering carts (200), and in order to maintain stable control of the raw material supply amount, the sintering machine speed and raw material supply amount control calculation can be controlled by first-in, first-out of 10 data points at 1-minute intervals.

[0054] Additionally, the control unit (1000) can determine the final sintering speed by correcting the final calculated sintering speed control value according to the difference between the temperature and pressure of the exhaust gas discharged through a plurality of wind boxes (400) and connected as one through a main duct (800) and the preset average temperature and average pressure of the exhaust gas.

[0055] In this way, a sintered ore manufacturing apparatus according to one embodiment controls the movement speed of a plurality of sintering carts (200) so that a calculated sintered ore point, calculated by averaging a first sintered ore point (BTP1) using the temperature of the gas passing through a plurality of wind boxes (400), a second sintered ore point (BTP2) using the carbon monoxide concentration of the gas, and a third sintered ore point (BTP3) using the oxygen concentration of the gas, moves to a preset target sintered ore point, thereby greatly improving the target hit rate for the sintered ore point, minimizing deviations in sintered ore quality, and maximizing the production of high-quality sintered ore.

[0056] In other words, a sintering ore manufacturing device is provided that significantly improves the target hit rate for the sintering completion point, minimizes deviations in sintering ore quality, and maximizes the production of high-quality sintering ore.

[0057] Hereinafter, a method for manufacturing sintered ore according to another embodiment will be described with reference to FIGS. 3 to 5. The method for manufacturing sintered ore according to another embodiment may be performed using a sintered ore manufacturing apparatus according to the above-described embodiment, but is not limited thereto.

[0058] FIG. 3 is a flowchart illustrating a method for manufacturing sintered ore according to another embodiment.

[0059] First, referring to FIG. 3, the temperature of the gas passing through a plurality of wind boxes is measured (S100).

[0060] Specifically, the temperature of the gas passing through multiple wind boxes arranged along the path and sucking in the gas inside the multiple sintering trolleys is measured at the bottom of the multiple sintering trolleys loaded with raw materials moving along the path.

[0061] Next, the carbon monoxide concentration of the gas passing through multiple wind boxes is measured (S200).

[0062] Specifically, the carbon monoxide concentration of the gas passing through multiple wind boxes is measured.

[0063] Next, the oxygen concentration of the gas passing through multiple wind boxes is measured (S300).

[0064] Specifically, the oxygen concentration of the gas passing through multiple wind boxes is measured.

[0065] Next, the calculation completion point for sintering is calculated (S400).

[0066] Specifically, the sintering completion point is calculated by averaging the first sintering completion point where the gas temperature is maximum, the second sintering completion point where the carbon monoxide concentration is minimum, and the third sintering completion point where the oxygen concentration of the gas is 15% or higher.

[0067] Next, the temperature of the exhaust gas passing through the main duct is measured (S500).

[0068] Specifically, the temperature of the exhaust gas passing through the main duct, which is connected to the lower part of multiple wind boxes and discharges gas as exhaust gas, is measured.

[0069] Next, the pressure of the exhaust gas passing through the main duct is measured (S600).

[0070] Specifically, the pressure of the exhaust gas passing through the main duct, which is connected to the lower part of multiple wind boxes and discharges the gas as exhaust gas, is measured.

[0071] Next, the movement speed of multiple sintering trolleys is controlled based on the calculated sintering completion point (S700).

[0072] Specifically, the movement speeds of multiple sintering trolleys are controlled based on the calculated sintering completion point so that the calculated sintering completion point moves to a preset target sintering completion point. At this time, the movement speeds of the multiple sintering trolleys are corrected based on the difference between the exhaust gas temperature and the preset average exhaust gas temperature, and the movement speeds of the multiple sintering trolleys are corrected based on the difference between the exhaust gas pressure and the preset average exhaust gas pressure.

[0073] Next, the supply amount of raw materials loaded into a plurality of sintering carts is controlled based on the calculated sintering completion point (S800).

[0074] Specifically, the supply amount of raw materials loaded into a plurality of sintering trolleys is controlled based on the calculated sintering completion point. At this time, the supply amount of raw materials is proportional to the movement speed of the plurality of sintering trolleys controlled based on the calculated sintering completion point.

[0075] FIG. 4 is a flowchart showing an example of a method for manufacturing sintered ore according to another embodiment.

[0076] Referring to FIG. 4, in Step 1 of an example of a method for manufacturing sintered ore according to another embodiment, control is initiated by an instrumentation controller while the sintering machine is in normal operation to control the speed of the sintering machine of the process computer, and the average temperature value of the exhaust gas and the average pressure value of the exhaust gas are measured.

[0077] In addition, the temperature, carbon monoxide concentration, and oxygen concentration values ​​of the gas passing through each wind box are measured and transmitted to the real-time process computer. When the program starts for the first time, since it is a transition from manual use, the current sintering machine speed is stored in 10 total buffers, and the expected sintering machine speed becomes the current sintering machine speed.

[0078] In Step 2, there are production mode and quality mode as speed control setting modes for the sintering machine. For example, when production mode is selected, the average temperature of the flue gas is set to be 5% to 10% lower and the average pressure of the flue gas is set to be 5% to 10% higher than when quality mode is selected, and these variables are pre-entered into the process computer.

[0079] Step 3 is a step for inputting target values ​​for sintering machine speed control, in which the sintering completion point, the average flue gas temperature, and the average flue gas pressure are input. Then, temperature, carbon monoxide, and oxygen concentration data from each wind box are continuously measured at 4-second intervals, converted from analog signals to digital signals, and collected as data for the control system, which is the control unit. Using the three collected data, the location of the sintering machine's highest temperature point is calculated.

[0080] The method for calculating the location of the highest temperature point of the sintering furnace involves analyzing the gas sucked in among wind boxes 1 through 25 and using the analysis values ​​measured by 120 (40 × 3) gas sensors starting from wind box 16.

[0081] For example, in the case of carbon monoxide concentration values, the location indicating the minimum concentration is used; in the case of oxygen concentration values, the location exceeding 15% is used; and in the case of temperature values, the location indicating the maximum temperature value is used. For example, in (A) of Fig. 2, the point where three points coincide becomes the maximum temperature point.

[0082] However, if the three points do not coincide, the current sintering completion point for control can be used by using the average of two points at the location of the lowest value indicated for carbon monoxide concentration and the location of the highest temperature value indicated in (B) of Fig. 2.

[0083] In addition, the average value of the control sintering completion point is shown in mathematical formulas 1 and 2 below.

[0084] [Mathematical Formula 1]

[0085] Average value of sintering completion point = {(carbon monoxide concentration point + oxygen concentration point + maximum temperature point) ÷ 3}

[0086] [Mathematical Formula 2]

[0087] Average value of sintering completion point = {(carbon monoxide concentration point + peak temperature point) ÷ 2}

[0088] In Step 4, the expected sintering machine speed is calculated using the following mathematical formula 3 based on the calculated sintering completion point, which is the average value of the calculated sintering completion point, and an example is shown in Fig. 5.

[0089] FIG. 5 is a table showing values ​​according to an example of a method for manufacturing sintered ore according to another embodiment. In FIG. 5, BTP represents the sintering completion point, and BTT represents the sintering completion time. In FIG. 5, the sintering completion point represents the distance from the endpoint within the effective image distance.

[0090] [Mathematical Formula 3]

[0091] Estimated sintering machine speed after 10 minutes = {(Effective burn distance - Target sintering completion point) ÷ (Effective burn distance - Average sintering completion point) × Sintering machine speed}

[0092] It is stored in 10 buffers, moving one step at a time over time.

[0093] When the expected sintering speed passes after 10 minutes, it moves from buffer 10 to buffer 0, and that value is finally determined as the sintering speed value.

[0094] In Step 5, raw material supply amount control is simultaneously performed to stably supply raw materials at the expected sintering machine speed value after 10 minutes, and the formula for raw material supply amount control is shown in Equation 4 below.

[0095] [Mathematical Formula 4]

[0096] Total raw material supply (t / hr) = (Sintering machine filling time × Trolley width × Estimated sintering machine speed × Specific gravity × 60) ÷ 1000

[0097] In Step 6, the deviation of the current value from the flue gas average temperature setpoint and the flue gas average pressure setpoint was calculated and shown in Equation 5.

[0098] [Mathematical Formula 5]

[0099] Flue gas temperature deviation calculation = Flue gas temperature setpoint - Current flue gas temperature

[0100] Calculation of flue gas pressure deviation = Flue gas pressure set value - Current flue gas pressure value

[0101] In Step 7, since rapid process fluctuations occur when the sintering machine speed is affected whenever deviations in flue gas temperature and pressure occur, fluctuations are prevented within a set predetermined range, and in order to achieve stable control corresponding to the target sintering completion point, a predetermined range limit and a sintering machine speed correction value are calculated as shown in Equations 6 and 7 below and used for final sintering machine speed control.

[0102] [Mathematical Formula 6]

[0103] Calculate deceleration rate when flue gas temperature deviation > 5

[0104] Flue gas temperature deviation = Flue gas temperature deviation - 5.0

[0105] Estimated Sintering Speed ​​= Estimated Sintering Speed ​​+ {Estimated Sintering Speed ​​× Sintering Completion Point Correction Value(0.050) × [(Flue Gas Temperature Deviation - 5) ÷ Correction Ratio)]}

[0106] If 5.0 > flue gas temperature deviation > -5.0, the deceleration rate is 0.

[0107] [Mathematical Formula 7]

[0108] Calculate deceleration rate when exhaust gas pressure deviation > 5

[0109] Flue gas pressure deviation = Flue gas pressure deviation - 5.0

[0110] Estimated Sintering Speed ​​= Estimated Sintering Speed ​​+ {Estimated Sintering Speed ​​× Sintering Completion Point Correction Value(0.020) × [(Exhaust Gas Pressure Deviation - 5) ÷ Correction Ratio)]}

[0111] If 5.0 > flue gas pressure deviation > -5.0, the deceleration rate is 0.

[0112] In this way, a method for manufacturing sintered ore according to another embodiment controls the movement speeds of a plurality of sintering carts so that a calculated sintering completion point—calculated by averaging a first sintering completion point using the temperature of the gas passing through a plurality of wind boxes, a second sintering completion point using the carbon monoxide concentration of the gas, and a third sintering completion point using the oxygen concentration of the gas—moves to a preset target sintering completion point, thereby significantly improving the target hit rate for the sintering completion point, minimizing deviations in sintered ore quality, and maximizing the production of high-quality sintered ore.

[0113] In other words, a method for manufacturing sintered ore is provided that significantly improves the target hit rate for the sintering completion point, minimizes the variation in sintered ore quality, and maximizes the production of high-quality sintered ore.

[0114] Although embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements by those skilled in the art using the basic concept of the present invention as defined in the following claims also fall within the scope of the present invention. Explanation of the symbols

[0115] Sintering trolley (200), ignition furnace (300), wind box (400), temperature gauge (500), carbon monoxide concentration gauge (600), control unit (1000)

Claims

Claim 1 A plurality of sintering trolleys that move along a movement path and have raw materials loaded inside; an ignition furnace that ignites the raw materials at the top of the plurality of sintering trolleys; a plurality of wind boxes arranged along the movement path at the bottom of the plurality of sintering trolleys and sucking in gas inside the plurality of sintering trolleys; a temperature measuring device that measures the temperature of the gas passing through the plurality of wind boxes; a carbon monoxide concentration measuring device that measures the carbon monoxide concentration of the gas passing through the plurality of wind boxes; and a control unit connected to the plurality of sintering trolleys, the temperature measuring device, and the carbon monoxide concentration measuring device, and controlling the movement speed of the plurality of sintering trolleys based on a calculated sintering completion point calculated by averaging a first sintering completion point where the temperature of the gas measured by the temperature measuring device is maximum and a second sintering completion point where the carbon monoxide concentration of the gas measured by the carbon monoxide concentration measuring device is minimum. A sintered ore manufacturing apparatus comprising a raw material supply unit that supplies the raw material to the plurality of sintering trolleys, wherein the control unit is connected to the raw material supply unit and controls the supply amount of the raw material based on the calculated sintering completion point. Claim 2 In claim 1, the control unit controls the movement speed of the plurality of sintering carts so that the calculated sintering completion point moves to a preset target sintering completion point. Claim 3 A sintered ore manufacturing apparatus according to claim 1, further comprising an oxygen concentration meter for measuring the oxygen concentration of the gas passing through the plurality of wind boxes, wherein the control unit is connected to the oxygen concentration meter, and the calculated sintering completion point calculated by the control unit is the average of the first sintering completion point, the second sintering completion point, and the third sintering completion point in which the oxygen concentration of the gas measured by the oxygen concentration meter is 15% or more. Claim 4 delete Claim 5 A sintering ore manufacturing apparatus according to claim 1, wherein the supply amount of the raw material is proportional to the moving speed of the plurality of sintering carts controlled based on the calculated sintering completion point. Claim 6 A sintering ore manufacturing apparatus according to claim 1, further comprising: a main duct connected to the lower part of the plurality of wind boxes to discharge the gas as exhaust gas; and an exhaust gas temperature measuring device that measures the temperature of the exhaust gas passing through the main duct, wherein the control unit is connected to the exhaust gas temperature measuring device and corrects the movement speed of the plurality of sintering trolleys based on the difference between the temperature of the exhaust gas measured by the exhaust gas temperature measuring device and a preset average temperature of the exhaust gas. Claim 7 A sintering ore manufacturing apparatus according to claim 6, further comprising a flue gas pressure measuring device for measuring the pressure of the flue gas passing through the main duct, wherein the control unit is connected to the flue gas pressure measuring device and corrects the movement speed of the plurality of sintering trolleys based on the difference between the pressure of the flue gas measured by the flue gas pressure measuring device and a preset average flue gas pressure. Claim 8 A method for manufacturing sintered ore, comprising: a step of measuring the temperature of a gas passing through a plurality of wind boxes arranged along a movement path and sucking gas inside the plurality of sintering trolleys, wherein the gas is loaded with raw materials and moves along a movement path; a step of measuring the carbon monoxide concentration of the gas passing through the plurality of wind boxes; a step of calculating a calculated sintering completion point which is the average of a first sintering completion point where the gas temperature is maximum and a second sintering completion point where the carbon monoxide concentration is minimum; a step of controlling the movement speed of the plurality of sintering trolleys based on the calculated sintering completion point; and a step of controlling the supply amount of the raw materials loaded into the plurality of sintering trolleys based on the calculated sintering completion point. Claim 9 In claim 8, the step of controlling the movement speed of the plurality of sintering carts is performed by controlling the movement speed of the plurality of sintering carts so that the calculated sintering completion point moves to a preset target sintering completion point. A method for manufacturing sintered ore. Claim 10 A method for manufacturing sintered ore according to claim 8, further comprising the step of measuring the oxygen concentration of the gas passing through the plurality of wind boxes, wherein the step of calculating the calculated sintering completion point is performed by calculating the average of the first sintering completion point, the second sintering completion point, and the third sintering completion point in which the oxygen concentration of the gas is 15% or more. Claim 11 delete Claim 12 A method for producing sintered ore according to claim 8, wherein the supply amount of the above raw material is proportional to the moving speed of the plurality of sintering carts controlled based on the calculated sintering completion point. Claim 13 A method for manufacturing sintered ore according to claim 8, further comprising the step of measuring the temperature of the exhaust gas passing through a main duct connected to the lower part of the plurality of wind boxes and discharging the gas as exhaust gas, and the step of controlling the movement speed of the plurality of sintering trolleys by correcting the movement speed of the plurality of sintering trolleys based on the difference between the temperature of the exhaust gas and a preset average temperature of the exhaust gas. Claim 14 A method for manufacturing sintered ore according to claim 13, further comprising the step of measuring the pressure of the exhaust gas, and the step of controlling the movement speed of the plurality of sintering trolleys by correcting the movement speed of the plurality of sintering trolleys based on the difference between the pressure of the exhaust gas and a preset average pressure of the exhaust gas.

Citation Information

Patent Citations

  • Operation of sintering machine

    JP1994287647A

  • Method for estimating progressing condition of sintering reaction

    JP2000256759A