Substrate for magnetic disks, and magnetic disk
Patent Information
- Application Number
- LAP684
- Authority / Receiving Office
- LA · LA
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2017-06-30
- Filing Date
- 2018-07-02
- Publication Date
- 2022-10-07
AI Technical Summary
The challenge is to reduce the number of contacts between a magnetic disk and external components due to vibrations caused by external shocks in hard disk drive devices, especially as the thickness of magnetic disk substrates decreases, leading to increased fragility and potential damage.
A magnetic disk substrate with a metal film having a loss coefficient value of 0.01 or more is applied to the surface, with specific thickness and surface roughness characteristics to attenuate vibrations effectively, reducing the likelihood of contact with external members.
The solution effectively reduces the number of contacts between the magnetic disk and external components, enhancing the durability and reliability of hard disk drive devices by minimizing vibrations and preventing scratches and defects.
Smart Images

Figure 00000000_0000_ABST 
Figure 00000000_0001_ABST
Abstract
Description
Magnetic disk substrate and magnetic disk
[0001] The present invention relates to a magnetic disk substrate and a magnetic disk.
[0002] Glass substrates and aluminum alloy substrates have traditionally been used as substrates for magnetic disks. Magnetic disks are formed on the main surfaces of these substrates by forming magnetic films. It is desirable for magnetic disks to have few surface defects, no hindrance to the reading and writing of information, and the ability to read and write large amounts of information.
[0003] For example, when an aluminum alloy substrate is used as a non-magnetic substrate for a magnetic disk, the surface of the aluminum alloy substrate is plated with NiP. In this case, in order to suppress surface defects after plating, an Al alloy substrate for a magnetic recording medium is known in which a metal film is formed on the substrate surface by physical vapor deposition (Patent Document 1).
[0004] Japanese Patent Application Laid-Open No. 2006-302358
[0005] The Al alloy substrate for magnetic recording media is said to be able to reduce surface defects after NiP plating is formed on the substrate, thereby providing a magnetic disk that can read and write large amounts of information without any problems.
[0006] In recent years, the hard disk drive industry has seen a decline in the rate at which recording density has improved, as the miniaturization of magnetic particles in magnetic disks has reached its limit. Meanwhile, demand for increased storage capacity in hard disk drives (hereinafter also referred to as HDDs) is becoming increasingly intense due to big data analysis and other factors. Therefore, increasing the number of magnetic disks installed in a single hard disk drive is being considered.
[0007] To increase storage capacity by increasing the number of magnetic disks installed in a hard disk drive, it is necessary to reduce the thickness of the magnetic disk substrate, which accounts for the majority of the thickness of the magnetic disk, within the limited space within the magnetic disk drive. However, it has been found that reducing the thickness of the magnetic disk substrate reduces the substrate's rigidity, making it more susceptible to large vibrations and making it difficult to contain those vibrations. For example, cloud data centers use a huge number of hard disk drives, which require frequent replacement due to failure. It has been found that the impact of installing a new hard disk drive in a rack can cause failure or shorten the time until failure. Further detailed investigation revealed that when a hard disk drive is subjected to external impact, damage can occur even when the magnetic disk is not rotating because power is not yet supplied to the hard disk drive.
[0008] Unlike steady-state flutter vibrations caused by a rotating magnetic disk and the surrounding airflow during steady rotation, vibrations caused by external impacts decay over time. However, if the amplitude of these vibrations is large, the magnetic head may come into contact with the ramp member, which protrudes above the main surface of the magnetic disk to allow it to retreat from the magnetic disk, scraping the ramp member and generating particles, and in some cases, causing scratches and defects on the magnetic disk surface. In particular, if large vibrations do not decay and the number of contacts with external members increases, repeated contact occurs at the same position on the magnetic disk when the magnetic disk is not rotating, making particles, scratches, and defects on the magnetic disk surface even more likely to occur. Currently, for example, the thickness of a magnetic disk substrate for a nominal 3.5-inch size is 0.8 mm or more, making it difficult for vibrations caused by external impacts to generate problematic amplitudes. Furthermore, because hard disk drives typically have six or fewer magnetic disks mounted, the distance (gap) between the magnetic disk and the ramp is relatively large. As a result, contact between the magnetic disk and the ramp is rare. However, in the future, as the storage capacity of hard disk drive devices increases, and the thickness of magnetic disk substrates is reduced, problems that did not previously occur, such as vibrations due to external impacts and the resulting contact with other components such as ramp members, as well as particles and scratches and dents on the magnetic disk caused by the contact, will no longer be negligible.
[0009] Therefore, an object of the present invention is to provide a magnetic disk substrate and a magnetic disk that can effectively reduce the number of times a magnetic disk comes into contact with external members due to vibrations of the magnetic disk, which are different from flutter vibrations, caused by external impacts, even if the thickness of the substrate is thin.
[0010] One aspect of the present invention is a magnetic disk substrate. The substrate comprises: a substrate body having two main surfaces; and a film of a metal material provided on the main surfaces, the film having a loss factor of 0.01 or more. The thickness T of the magnetic disk substrate including the film is 0.700 mm or less, and the thickness D [mm] of the film provided on the main surfaces and the thickness T [mm] of the substrate including the film satisfy the following formula (1): D ≧ 0.0082 / T − 0.0015 (1)
[0011] It is preferable that the thickness D [mm] of the film and the thickness T [mm] of the substrate including the film satisfy the following formula (2): D ≧ 0.0094 / T (2)
[0012] It is preferable that the magnetic disk substrate has a disk shape, and the disk shape has an outer diameter of 90 mm or more.
[0013] Another aspect of the present invention is a magnetic disk substrate. The substrate includes: a substrate body having two main surfaces; and a film provided on the main surfaces. The magnetic disk substrate is disk-shaped with an outer diameter of 90 mm or more, the thickness T of the magnetic disk substrate including the film is 0.700 mm or less, and the film is provided so that when an impact of 120 G for 2 msec is applied in the normal direction to the main surfaces while the inner periphery of the substrate is fixed, the number of times that a displacement of 0.2 mm or more occurs due to vibration in the thickness direction of the outer peripheral edge of the substrate (the normal direction to the main surfaces of the substrate) is four or less.
[0014] Here, with regard to the substrate body (magnetic disk substrate having no film), when the impact is applied to the magnetic disk substrate, the displacement amount due to vibration in the thickness direction of the outer peripheral end of the substrate may be 0.2 mm or more more than four times.
[0015] It is preferable that the film is provided so as to cover the entire surface of the substrate, the film thickness at the end face of the substrate is thicker than the film thickness at the main surface, and the film is provided so that the film thickness at the end face is 110% or more of the film thickness at the main surface.
[0016] The thickness T of the substrate is preferably 0.640 mm or less, and more preferably 0.520 mm or less.
[0017] The Vickers hardness Hv of the film is 100 [kgf / mm 2 ] or more.
[0018] The material of the film preferably includes a Ni-P alloy.
[0019] The film is preferably formed on the main surface and the outer peripheral end face of the substrate body, and the maximum height Rz of the surface roughness of the outer peripheral end face of the substrate body that forms the interface with the film is 0.5 μm or more.
[0020] The film is preferably formed on the main surface and the outer peripheral end face of the substrate body, and the maximum height Rz of the surface roughness of the film at the outer peripheral end face of the non-magnetic substrate for a magnetic disk is smaller than the maximum height Rz of the surface roughness of the substrate body at the outer peripheral end face of the substrate body.
[0021] Another aspect of the present invention is a magnetic disk having at least a magnetic film on the surface of the magnetic disk substrate.
[0022] The above-described magnetic disk substrate and magnetic disk can effectively reduce the number of times the magnetic disk comes into contact with external members due to vibrations of the magnetic disk, which are different from flutter vibrations, caused by external impacts, even if the thickness of the substrate is thin.
[0023] Fig. 1 is a diagram showing an example of the external shape of a magnetic disk substrate of this embodiment; Fig. 2 is a diagram explaining an example of an edge and a film of a magnetic disk substrate of this embodiment; Fig. 3 is a diagram explaining an example of vibration of a magnetic disk substrate of this embodiment; Fig. 4 is a diagram explaining the range of thickness T [mm] and thickness D [mm] of a magnetic disk substrate of this embodiment.
[0024] The magnetic disk substrate of the present invention will be described in detail below. While the following description will be made using a magnetic disk glass substrate, the substrate body of the magnetic disk substrate may be a nonmagnetic metal substrate in addition to a glass substrate. That is, the substrate body is a nonmagnetic substrate made of glass or metal. Materials for the glass substrate include aluminosilicate glass, soda-lime glass, borosilicate glass, and the like. Amorphous aluminosilicate glass is particularly suitable because it can be chemically strengthened as needed and can produce a magnetic disk glass substrate with excellent main surface flatness and substrate strength. Materials for the metal substrate include, for example, aluminum alloys, titanium alloys, and single-crystal silicon. Aluminum alloys may contain magnesium as a component. Metal substrates such as aluminum alloys generally have a lower Young's modulus than glass substrates, and are therefore prone to vibration due to external impacts. Therefore, metal substrates are preferred because the application of the present invention can provide particularly significant improvements.
[0025] FIG. 1 is a diagram showing the external shape of a magnetic disk substrate according to this embodiment. As shown in FIG. 1, the magnetic disk substrate 1 (hereinafter simply referred to as substrate 1) according to this embodiment is a thin, disk-shaped substrate having an inner hole 2 formed therein. While the size of the substrate 1 is not critical, the substrate 1 can be suitably applied to magnetic disk substrates having a nominal diameter of, for example, 2.5 inches or 3.5 inches. For a magnetic disk substrate having a nominal diameter of 3.5 inches, the outer diameter (diameter) of the disk shape is preferably 90 mm or more. Specifically, the nominal value of the outer diameter of the disk shape can be 95 mm or 97 mm. Even with such a large disk shape, the formation of a film (described later) on the main surface can reduce the generation of particles, scratches, and dents caused by vibration of the magnetic disk. Furthermore, the upper limit of the outer diameter (diameter) of the disk shape is, for example, 100 mm. Since the width of a typical 3.5-inch HDD (the size that can be installed in the 3.5-inch bay of a typical PC case) is 101.6 mm, there is a risk that the wall thickness will not be sufficient if it exceeds 100 mm. Note that the vibration of the magnetic disk caused by an external impact, which is different from flutter vibration, becomes larger and more difficult to attenuate as the outer diameter of the substrate 1 increases. Therefore, the larger the outer diameter of the substrate 1, the more effectively the effects of this embodiment, which will be described later, can be achieved, and this is therefore preferable. In other words, the magnetic disk substrate of this embodiment is particularly suitable for magnetic disk substrates with a nominal size of 3.5 inches or more.
[0026] 2 is a diagram illustrating an example of an edge portion and a film of a substrate 1. As shown in FIG. 2, the substrate 1 has a substrate body 3 and a film 4. The substrate body 3 has a pair of main surfaces 3a, side wall surfaces 3b arranged along a direction perpendicular to the pair of main surfaces 3a, and a pair of chamfered surfaces 3c arranged between the pair of main surfaces 3a and the side wall surfaces 3b. The side wall surfaces 3b and the chamfered surfaces 3c are formed at the outer peripheral edge and the inner peripheral edge of the substrate 1.
[0027] When glass is used for the substrate body 3, the glass composition of the substrate body 3 is, for example, SiO 2 , 55-78%, Li 2 O, 0.1-1%, Na 2The glass substrate 3 may contain 2 to 15% of SiO, and 10 to 25% of MgO, CaO, SrO, and BaO in total, and the molar ratio of the CaO content to the total content of MgO, CaO, SrO, and BaO (CaO / (MgO+CaO+SrO+BaO)) may be 0.20 or less. This glass is called Glass 1. The glass substrate 3 may contain, for example, SiO, expressed in mol %, 2 45 to 68%, Al 2 O 3 5 to 20%, SiO 2 and Al 2 O 3 The total content (SiO 2 +Al 2 O 3 ) 60-80%, B 2 O 3 The total content of BaO and SrO (BaO+SrO) is 0-2%, the total content of alkaline earth metal oxides (MgO+CaO+SrO+BaO) is 12-30%, and the total content of alkali metal oxides (Li 2 O + Na 2 O+K 2 Alternatively, the glass may be an amorphous oxide glass containing 3.5 to 15% of ZnO, at least one oxide selected from the group consisting of Sn oxide and Ce oxide, with the total content of Sn oxide and Ce oxide being 0.05 to 2.00%. This glass is referred to as Glass 2.
[0028] As shown in FIG. 2 , a film 4 is provided on the entire surface of the substrate body 3, i.e., the main surface 3 a, the side wall surface 3 b, and the chamfered surface 3 c. The film 4 enhances the vibration-damping properties of the substrate 1. The film 4 is made of a material with a loss factor of 0.01 or greater. The film is made of a metallic material. The metallic material of the film 4 has a higher loss factor than the material of the substrate body 3. The loss factor value is the value at room temperature, e.g., 25°C. Hereinafter, the loss factor refers to the value at room temperature. Herein, the loss factor of the film 4 can be determined by a vibration test using the substrate body 3 and the substrate 1 with the film 4 formed on the substrate body 3 as test samples, and measuring the resonant frequency and half-width at the resonant frequency of the test samples. For example, a "Free Resonant Young's Modulus, Rigidity Modulus, and Internal Friction Measuring Device (JE Series)" manufactured by Nippon Technoplus Co., Ltd. can be used for the vibration test. The loss factor of the test sample can be determined from the resonant frequency and half-width of the test sample obtained in the vibration test. Furthermore, the loss factor of the film 4 can be calculated from the resonance frequency and loss factor of the substrate 1, the resonance frequency of the substrate body 3, the ratio of the thickness of the substrate body 3 to the thickness of the film 4, and the ratio of the density of the material of the substrate body 3 to the density of the metal material of the film 4, for example, according to the known formula shown below. 1 , η 1 and the resonance frequency of the substrate body 3 is f 3 The loss coefficient η of the film 4 is given by: a is the ratio of the total thickness of the film 4 to the thickness of the substrate body 3; and b is the ratio of the density of the metal material of the film 4 to the density of the material of the substrate body 3. 4 is α=(f 1 / f 3 ) 2 · (1 + a · b) as η 4 = α / (α-1) · η 1 It can be expressed as:
[0029] A Ni-P alloy containing Ni and P can be suitably used as a material having such characteristics (loss factor) of the film 4. In the case of a Ni-P alloy, the P content can be set to 5 to 15 mass % so that the alloy is non-magnetic. For example, the P content can be set to 5 to 15 mass %. Furthermore, an Mg alloy, an Al-Zn alloy, an Mg-Zr alloy, or the like can be used as the metal material of the film 4. Note that the film formation method can be, for example, a sputtering method, an electroless plating method, an electrolytic plating method, or the like. An appropriate method can be selected from these.
[0030] The thickness T of the substrate 1, including the substrate body 3 and the film 4, is 0.700 mm or less. Furthermore, the thickness D [mm] of the film 4 provided on the main surface 3a and the thickness T [mm] of the substrate 1 including the film 4 satisfy the following formula (1). It is preferable that the thickness of the film 4 does not vary depending on the location on the main surface, but is constant across the main surface: D ≧ 0.0082 / T − 0.0015 (1)
[0031] Since this substrate 1 has a thickness of 0.700 mm or less, it is prone to vibration due to external impacts, etc. However, even if such vibration occurs, the film 4 formed on the main surface 3a of the substrate body 3 allows the vibration to be quickly attenuated. Furthermore, it is preferable for the film 4 to seamlessly cover the entire periphery of the metal body 1, including the end faces, since this particularly enhances the degree of vibration suppression. In this case, it is more preferable for the film 4 to be harder than the substrate body 3. It is even more preferable that the thicknesses D1 and D2 of the film 4 formed on both main surfaces 3a of the substrate body 3 are equal. In such a case, vibration modes that cause large localized deformation are less likely to form, and the degree of vibration suppression is further enhanced. This reduces the number of contacts with, for example, ramp members or adjacent disks. While the present embodiment includes a film 4 formed on each of the main surfaces 3a on both sides, this embodiment also includes a configuration in which the film 4 is formed only on one of the main surfaces 3a. In this case, the thickness D of the film 4 is the thickness of the film 4 formed on one of the main surfaces 3a.
[0032] A magnetic disk, formed by forming a magnetic film on a substrate 1, is fixed to the spindle of the hard disk drive at its main surface near the bore 2 within the hard disk drive. For example, when a new hard disk drive is installed in a rack for replacement or when a hard disk drive is removed from the rack to be moved to another location, the hard disk drive may be subjected to external shocks during these operations. Such shocks cause vibrations in the main surface 3a of the substrate 1, displacing it in the normal direction (thickness direction of the substrate 1) to the main surface 3a. This displacement is greatest at the outer peripheral edge of the main surface. This vibration, unlike steady-state flutter vibrations that occur during steady rotation due to the rotating magnetic disk and the airflow around it, decays over time, as shown in Figure 3. Figure 3 shows an example of vibrations in the normal direction to the main surface at the outer peripheral edge of the substrate 1. This vibration occurs whether the magnetic disk is rotating or stationary. For this reason, it is undesirable for this vibration to continue for a long time, causing the magnetic disk formed from substrate 1 to come into contact with a ramp member inside the hard disk drive device, resulting in particles, scratches, and dents on the surface of the magnetic disk, and this contact may also cause the ramp member to be scraped away, resulting in the generation of particles. In particular, when a stationary magnetic disk vibrates and comes into contact with a ramp member, the same location on the magnetic disk comes into contact with the ramp member multiple times, which is likely to result in the generation of particles, scratches, and dents.
[0033] However, in the substrate 1, the film 4 is made of a metal material with a loss factor of 0.01 or greater, and the thickness D (= D1 + D2) [mm] of the film 4 and the thickness T [mm] of the substrate body 3 satisfy the relationship D ≧ 0.0082 / T − 0.0015. The thinner the thickness T, the greater the amplitude of vibration and the more difficult it is to attenuate the amplitude. However, by setting a lower limit for the thickness D, the thickness D can be ensured, allowing for early attenuation of vibration in the substrate 1. The loss factor of the film 4 is preferably 0.02 or greater. On the other hand, while there is no particular upper limit for the loss factor of the film 4, a material with a loss factor that is too large may be a soft material in which the crystals in the metal material are easily broken. If the hardness of the film 4 is too low, the surface may be easily scratched after being made into a magnetic disk, potentially causing the HDD to crash. For this reason, a value of 0.3 or less is preferable, since practical metal materials can be used.
[0034] If the thickness D is less than 0.0082 / T-0.0015, the thickness D of the film 4 is not sufficiently thick relative to the thickness T of the substrate body 3, making it difficult to quickly attenuate vibrations in the substrate 1, and the film 4 cannot reduce the initial amplitude of vibrations on the main surface 3a. By setting the thickness D to 0.0082 / T-0.0015 or more, the film 4 covering the main surface 3a is sufficiently thick, allowing for early attenuation of vibrations in the substrate 1 and reducing the initial amplitude of vibrations. This effectively reduces the number of times the magnetic disk comes into contact with external components, such as a ramp member, due to vibrations of the magnetic disk, even if the substrate thickness is thin. Furthermore, the thickness D is preferably 0.0094 / T or more. Setting the thickness D to 0.0094 / T or more further enhances the effect of reducing the number of times the magnetic disk comes into contact with external components, thereby reducing the probability of problems occurring after HDD startup, which is preferable. Although magnetic films and the like are formed on the substrate 1 during the media process, the total thickness of these magnetic films and the like on any one surface is 0.1 μm or less, so their impact on the vibrations discussed in this specification can be ignored. In other words, even after being made into a magnetic disk, the vibration characteristics are the same as those of the substrate 1. Figure 4 is a diagram illustrating the range of thicknesses T [mm] and D [mm] of the substrate 1 of this embodiment. The range in this embodiment is the region above the solid curve indicated by the arrow in Figure 4. Thus, the thinner the thickness T, the thicker the lower limit of thickness D.
[0035] The above effect can be achieved even if the film 4 is provided only on the main surface 3a and not on the sidewall surfaces 3b and chamfered surfaces 3c. However, as shown in FIG. 2, the film 4 is preferably provided so as to cover the entire surface of the substrate 1, i.e., it is preferably provided continuously on the end surfaces of the substrate body 3, i.e., the sidewall surfaces 3b and chamfered surfaces 3c, in addition to the main surface 3a. Vibrations occurring in the substrate 1 are vibrations that displace in the normal direction of the main surface 3a. In conjunction with this vibration, the end surfaces of the substrate body 3 also displace in the normal direction of the main surface 3a. By providing the film 4 on the end surfaces of the substrate body 3, i.e., the sidewall surfaces 3b and chamfered surfaces 3c, in addition to the main surface 3a, the amount of displacement of the main surface 3a in the normal direction, i.e., the amplitude of vibration, can be suppressed. This is presumably because the vibration suppression effect of the film 4 is enhanced by connecting the two main surfaces with the film 4. Furthermore, the thicknesses of the film 4 on the sidewall surfaces 3b and the chamfered surfaces 3c are preferably thicker than the thicknesses D1 and D2 on the main surface 3a, respectively. This is believed to enhance the connectivity and interlocking of the two main surfaces, thereby enhancing the vibration suppression effect of the film 4. The vibrations occurring in the substrate 1 are vibrations that displace in the normal direction of the main surface 3a. In conjunction with this displacement of the main surface 3a in the normal direction, the end surfaces of the substrate main body 3 also displace in the normal direction of the main surface 3a. Since suppressing such displacement can suppress the amount of displacement of the main surface 3a in the normal direction, i.e., the amplitude of vibration, it is preferable to form the film 4 on the end surfaces of the substrate main body 3, i.e., the sidewall surfaces 3b and the chamfered surfaces 3c, in addition to the main surface 3a. It is preferable that the film 4 be provided so that the film thickness on the end surfaces (sidewall surfaces 3b and chamfered surfaces 3c) of the substrate main body 3 is 110% or more of the film thicknesses D1 and D2 on the main surface 3a (if the film thicknesses D1 and D2 are different, the thicker film thickness). This makes it possible to suppress the amplitude of vibration without affecting the thickness T of the substrate 1. Furthermore, it is preferable that the film thickness at the end faces of the substrate body 3 be 150% or less of the film thicknesses D1, D2 at the main surface 3a. If the film thickness at the end faces of the substrate body 3 exceeds 150% of the film thicknesses D1, D2 at the main surface 3a, the mass at the outer edge of the substrate 1 increases, increasing the centrifugal force generated when the substrate 1 rotates as a magnetic disk, and this centrifugal force is likely to increase flutter vibration, which is undesirable.
[0036] The thinner the magnetic disk, the greater the amplitude of vibration, which increases the frequency of contact between the magnetic disk and other components within the hard disk drive, further increasing the number of particles and defects such as scratches and dents on the magnetic disk that result from the contact. However, in the case of the substrate 1, even if the thickness is 0.640 mm or less, this problem is unlikely to occur. The thickness of the substrate 1 may be 0.570 mm or less, or even 0.52 mm or less, or 0.400 mm or less. The thickness of the substrate 1 may also be, for example, 0.635 mm or less, 0.550 mm or less, 0.500 mm or less, or 0.381 mm or less. From the perspective of mechanical durability, the lower limit of the thickness of the substrate 1 is preferably 0.2 mm or more. In principle, the thinner the substrate 1, the greater the problem of particle generation, and in some cases, the greater the problem of defects such as scratches and dents. However, in this embodiment, the effect of reducing particles, scratches, and defects is significant. Setting the thickness T of the substrate 1 to 0.640 mm or less is preferable because it allows the number of substrates mounted to be increased from eight to nine when a typical 3.5-inch HDD has a height of 26.1 mm (the size that can be mounted in a 3.5-inch bay of a typical PC case) and the gap between the ramp members (described later) for the magnetic disks is the magnetic disk thickness + 0.4 mm. Note that if the HDD height is 26.1 mm or more, it is possible to mount nine or more substrates. Furthermore, setting the thickness of the substrate to 0.520 mm or less is even more preferable because it allows the number of substrates mounted to be ten or more for the same size HDD. These HDDs, which mount more substrates than conventional HDDs, are prone to frequent contact between disks and ramp members or adjacent disks when subjected to external shock, which can easily cause problems (particles, scratches, dents) due to such contact. However, using the substrate of this embodiment makes it possible to reduce these problems.
[0037] According to one embodiment, the Vickers hardness Hv of the film 4 is 100 [kgf / mm 2By increasing the Vickers hardness Hv, defects such as scratches and dents are less likely to occur when the material comes into contact with a ramp member or the like in a hard disk drive device. The Vickers hardness Hv is preferably 100 [kgf / mm 2 If the thickness is less than 1 / 2 mm, defects such as scratches or dents may occur when the hard disk drive comes into contact with a ramp member or the like inside the hard disk drive, making the hard disk drive more susceptible to breakdowns.
[0038] According to one embodiment, the maximum height Rz (JIS B 0601:2001) of the surface roughness of the outer peripheral edge surface of the disk-shaped substrate body 3, which forms the interface with the film 4, is preferably 0.5 μm or more. In this specification, the roughness at the interface of the substrate body 3 with the film 4 is referred to as the surface roughness of the outer peripheral edge surface of the substrate body 3, which forms the interface with the film 4. The film 4 is formed on the substrate body 3, including the outer peripheral edge surface. A cross-sectional image of the outer peripheral edge surface of the substrate body 3 can be obtained using the method described below, and the maximum height Rz can be determined. Specifically, first, the outer peripheral edge surface of the substrate 1 on which the film 4 is formed is cut out using an ion polishing method along a plane passing through the center of the substrate 1 and perpendicular to the main surface, to create a sample with an exposed cross section of the outer peripheral edge surface. A cross-sectional image of the outer peripheral edge surface at a magnification of, for example, 5000x is obtained using a scanning electron microscope (SEM). From the image, the concave-convex curve of the surface of the substrate body 3 that forms the interface of the substrate body 3 with the film 4 is obtained, for example, by binarizing the cross-sectional image or by visually tracing it, and a 20 μm wide area at any location on the concave-convex curve is extracted to determine the maximum height Rz.
[0039] The presence of a certain degree of surface unevenness at the interface of the substrate body 3 in contact with the film 4 enhances the vibration suppression by the film 4. It is presumed that this vibration suppression is due to the fact that the film 4 penetrates and bites into each other's recesses at the interface between the substrate body 3 and the film 4, increasing the adhesion between them, and the vibration suppression effect of the film 4 affects the substrate body 3. Furthermore, while increasing the thickness of the film 4 increases the film stress that causes film peeling, setting the maximum height Rz to 0.5 μm or more can prevent film peeling due to film stress. The outer peripheral edge surface has a smaller area and a more complex shape than the main surface, and the thickness of the substrate 1 is 0.700 mm or less, which is thinner than conventional substrates, making film peeling more likely to occur at the outer peripheral edge surface of the substrate 1. However, setting the Rz of the surface (interface) of the substrate body to 0.5 μm or more increases the adhesion between the substrate body 3 and the film 4, preventing film 4 peeling and improving the long-term reliability of the HDD. In addition, the maximum height Rz of the surface roughness of the outer peripheral edge surface of the substrate body 3 is more preferably 1.0 μm or more, and even more preferably 1.5 μm or more, in order to further enhance the suppression of the vibrations described above. On the other hand, if the maximum height Rz is excessively large, the surface roughness of the film 4 after deposition (the surface roughness at the outer peripheral edge surface of the substrate 1) will increase in line with the surface roughness of the substrate body 3, making it easier for foreign matter to adhere to the outer peripheral edge surface during processing such as main surface polishing. Furthermore, foreign matter will also easily adhere to the outer peripheral edge surface of the magnetic disk after deposition of the magnetic film, which may result in a decrease in the yield during the manufacture of the substrate 1 and hard disk drive devices. In addition, the location of the outer peripheral edge surface where the maximum height Rz is 0.5 μm or more may be at least a portion of the outer peripheral edge surface, but in order to enhance the suppression of the vibrations described above and to enhance the effect of preventing film peeling, it is preferable that it be both the side wall surface 3b and the chamfered surface 3c. On the other hand, if the maximum height Rz on the main surface of the substrate body 3 is too large, defects may form and propagate in the early stages of film 4 formation, causing defects such as recesses and cracks on the surface of the film 4. These defects are desirable to remove because they can cause corrosion and surface defects after polishing, but because they are deep-rooted and difficult to remove, their effects remain even after a magnetic film is formed to form a magnetic disk. Therefore, it is preferable to set the maximum height Rz on the main surface of the substrate body 3 to, for example, 1 μm or less.
[0040] Furthermore, according to one embodiment, the maximum height Rz of the surface roughness of the film 4 at the outer peripheral edge of the substrate 1 is preferably smaller than the maximum height Rz of the surface roughness of the substrate body 3 at the outer peripheral edge of the substrate body 3 (the boundary surface in contact with the film 4). Regarding the maximum height Rz of the surface roughness of the film 4 at the outer peripheral edge of the substrate 1, for example, a stylus-type surface roughness and contour shape measuring instrument is used to determine the maximum height Rz of the surface roughness at multiple locations (e.g., three locations) on the outer peripheral edge under the following conditions, and the average value of these multiple locations is taken as the maximum height Rz of the surface roughness of the film 4. Note that the stylus movement (scanning) direction is the thickness direction of the non-magnetic substrate 1. Stylus shape: tip radius 2 μm, cone taper angle 60°; stylus load: 0.75 mN; stylus movement speed: 0.02 mm / sec; sampling length: 0.08 mm; filter λc: 0.08 mm; filter λs: 0.0008 mm.
[0041] If the maximum height Rz of the surface roughness of the film 4 at the outer peripheral edge of the substrate 1 is excessively large, it is likely to cause foreign matter to adhere to the substrate 1 or scratches due to gripping of the outer peripheral edge during subsequent processes such as magnetic film deposition. Therefore, it is preferable that the maximum height Rz of the surface roughness of the film 4 at the outer peripheral edge of the substrate 1 be smaller than the maximum height Rz of the surface roughness of the substrate body 3 at the outer peripheral edge of the substrate body 3 (the boundary surface in contact with the film 4). This improves adhesion between the substrate body 3 and the film 4, prevents peeling of the film 4, and improves the long-term reliability of the HDD, while preventing foreign matter from adhering to the outer peripheral edge or scratches due to gripping of the outer peripheral edge when, for example, depositing a magnetic film on the substrate 1. The maximum height Rz is more preferably 1.0 μm or less, and even more preferably 0.5 μm or less. The location on the outer peripheral edge of the substrate 1 that limits the maximum height Rz may be at least a portion of the outer peripheral edge of the substrate 1, but in order to enhance the vibration suppression effect and the film peeling prevention effect, it is preferable that it be the surface portion of the film 4 formed on both the side wall surface 3b and the chamfered surface 3c of the surface of the substrate 1. The surface roughness of the film 4 on the outer peripheral edge tends to follow the surface roughness of the underlying substrate body 3. Therefore, if the surface roughness of the substrate body 3 is made too large, additional processing such as edge polishing may be required after the film 4 is formed.
[0042] In another embodiment of the substrate 1, the substrate 1 has a disk shape with an outer diameter of 90 mm or more, and a thickness of 0.700 mm or less. In this case, the film 4 is provided so as to have the characteristic that when an impact of 120 G is applied for 2 msec with the inner periphery of the substrate 1 fixed, the number of times that the displacement of the outer edge of the substrate 1 in the thickness direction (normal direction to the main surface) becomes 0.2 mm or more is four or less. For example, the loss coefficient and thickness of the film 4 are set to achieve the above characteristic. If the number of times that the displacement becomes 0.2 mm or more is four or less, the number of repeated contacts with an external member at the same position is preferably two or less. Furthermore, it is more preferable that the number of times that the displacement becomes 0.2 mm or more is two or less. If the number of times is two or less, this means that there are no multiple contacts on one side of the substrate 1. In other words, since there are no repeated collisions at the same position on the main surface of the magnetic disk, it is more preferable that the number of times that the displacement becomes 0.2 mm or more is two or less. Here, the characteristics of the substrate body 3 may be such that, when the above-mentioned impact is applied to the substrate body 3, the number of times that the displacement of the outer peripheral edge of the substrate body due to vibration in the plate thickness direction becomes 0.2 mm or more exceeds four times. By providing a film 4 with an adjusted film material and film thickness, the number of times that the displacement becomes 0.2 mm or more can be reduced to four or less. Generally, when the substrate 1 is disk-shaped with an outer diameter of 90 mm or more and a thickness of 0.700 mm or less, the displacement of the outer peripheral edge of the substrate 1 due to vibration in the plate thickness direction tends to be large. However, due to the effect of the film 4, the number of times that the displacement of the substrate 1 due to vibration becomes 0.2 mm or more is limited to four or less.
[0043] Such a substrate 1 is fabricated, for example, as follows. Here, as an example, a case where a glass substrate is used as the substrate 1 will be described. First, a glass blank, which will be the material for a plate-shaped magnetic disk glass substrate having a pair of main surfaces, is formed. Next, the glass blank is roughly ground. After this, the glass blank is shaped and edge polished. After this, the glass substrate obtained from the glass blank is finely ground using fixed abrasive grains. After this, the glass substrate is subjected to first polishing, chemical strengthening, and second polishing. After this, film formation and film polishing are performed. Note that in this embodiment, the glass substrate is fabricated in the above-described order, but the above processes do not always need to be performed, and these processes may not be performed as appropriate. For example, among the above processes, edge polishing, fine grinding, first polishing, chemical strengthening, and second polishing may not be performed. Each process will be described below.
[0044] (a) Forming of Glass Blank For forming a glass blank, for example, a press forming method can be used. A circular glass blank can be obtained by the press forming method. Furthermore, it can be manufactured using known manufacturing methods such as a down-draw method, a re-draw method, and a fusion method. A disk-shaped glass substrate that serves as the base of a magnetic disk glass substrate can be obtained by appropriately shaping a plate-shaped glass blank manufactured by these known manufacturing methods.
[0045] (b) Rough grinding In rough grinding, grinding is performed on both main surfaces of the glass blank. For example, loose abrasive grains are used as the abrasive. In rough grinding, the glass blank is ground so as to approximate the target thickness dimension and flatness of the main surfaces. Note that rough grinding is performed depending on the dimensional accuracy or surface roughness of the formed glass blank, and may not be performed in some cases.
[0046] (c) Shape Processing Next, shape processing is performed. In shape processing, after molding the glass blank, a circular hole is formed using a known processing method to obtain a disk-shaped glass substrate with a circular hole. Then, the edge surfaces of the glass substrate are chamfered. As a result, side wall surfaces 3b perpendicular to the main surfaces are formed on the edge surfaces of the glass substrate, and chamfered surfaces 3c inclined with respect to the main surfaces 3a are formed between the side wall surfaces 3b and the main surfaces 3a on both sides.
[0047] (d) Edge Polishing Next, the edge of the glass substrate is polished. Edge polishing is a process in which, for example, a polishing liquid containing free abrasive grains is supplied between the polishing brush and the edge of the glass substrate (side wall surface 3b and chamfered surface 3c), and the polishing brush and the glass substrate are moved relative to each other. In edge polishing, the inner and outer peripheral edge surfaces of the glass substrate are polished to a mirror finish. Note that edge polishing may not be performed in some cases.
[0048] (e) Precision grinding Next, the main surfaces of the glass substrate are subjected to precision grinding. For example, a double-side grinding device with a planetary gear mechanism is used to grind the main surfaces 3a of the glass substrate. In this case, for example, fixed abrasive grains are provided on a surface plate for grinding. Alternatively, grinding can be performed using loose abrasive grains. Note that precision grinding may not be performed in some cases.
[0049] (f) First Polishing Next, the main surface 3a of the glass substrate is subjected to the first polishing. The first polishing uses a polishing pad attached to a surface plate using free abrasive grains. The first polishing removes cracks and distortions remaining on the main surface 3a after grinding with fixed abrasive grains, for example. The first polishing can reduce the surface roughness of the main surface 3a, for example, the arithmetic mean roughness Ra, while preventing the edge shape of the main surface 3a from excessively recessing or protruding. The free abrasive grains used in the first polishing are not particularly limited, but examples include cerium oxide abrasive grains or zirconia abrasive grains. Note that the first polishing may not be performed in some cases.
[0050] (g) Chemically strengthened glass substrates can be chemically strengthened as needed. Examples of chemical strengthening liquids include potassium nitrate, sodium nitrate, or a molten solution obtained by heating a mixture of these. By immersing the glass substrate in the chemical strengthening liquid, lithium ions and sodium ions in the glass composition on the surface of the glass substrate are replaced with sodium ions and potassium ions, respectively, which have relatively large ionic radii, in the chemical strengthening liquid. This results in the formation of a compressive stress layer in the surface layer, thereby strengthening the glass substrate. The timing of chemical strengthening can be determined as needed. However, polishing after chemical strengthening is particularly preferable, as it smooths the surface and removes foreign matter adhered to the surface of the glass substrate by chemical strengthening. In some cases, chemical strengthening may not be necessary.
[0051] (h) Second Polishing (Mirror Polishing) Next, the chemically strengthened glass substrate is subjected to a second polishing. The second polishing is intended to mirror-polish the main surface 3a. The second polishing is performed using a polishing device with the same configuration as the first polishing. The second polishing uses different types and particle sizes of free abrasive grains than the first polishing, and a softer resin polisher is used as the polishing pad to perform mirror polishing. This reduces the roughness of the main surface 3a while preventing excessive depression or protrusion of the edge shape of the main surface 3a. The roughness of the main surface 3a is preferably 0.2 nm or less in terms of arithmetic mean roughness Ra (JIS B 0601 2001). Since the main surface 3a of the substrate after the second polishing does not become the outermost surface of the substrate 1 having the film 4, the second polishing may not be performed in some cases.
[0052] (i) Film Formation: A film 4 is formed on the main surface 3a, sidewall surface 3b, and chamfered surface 3c of the fabricated glass substrate. The film 4 is formed by electrolytic plating, electroless plating, sputtering, or the like. Before forming the film 4, pretreatment or formation of a base layer may be performed as needed to improve the adhesion of the film 4. The film 4 is formed on the main surface 3a, sidewall surface 3b, and chamfered surface 3c, and can have the same film thickness on all surfaces. After the film 4 is formed, an annealing treatment (heat treatment) of the film 4 is performed as needed to relieve internal stress in the formed film 4. It is preferable that the film 4 be nonmagnetic so as not to cause noise when finally formed into a magnetic disk.
[0053] (j) Film Polishing: After the film 4 is formed, the film 4 on the main surface 3a of the substrate body 3 is polished to reduce the surface roughness of the film 4. The purpose of film polishing is mirror polishing. Film polishing can also be performed using a polishing device with a similar configuration to the first polishing. In film polishing, the type and particle size of the free abrasive grains are changed compared to the first polishing, and a resin polisher with a softer hardness is used as the polishing pad. Multiple polishing processes may be performed as needed. In this case, the particle size of the free abrasive grains is reduced in later polishing processes to achieve more precise polishing. By polishing the film 4 formed on the main surface 3a in this manner and not polishing the film 4 on the sidewall surface 3b and chamfered surface 3c, the thickness of the film 4 on the sidewall surface 3b and chamfered surface 3c can be made thicker than the thickness of the film 4 on the main surface 3a. As described above, the film 4 formed on the side wall surface 3 b and the chamfered surface 3 c has the effect of suppressing the amplitude of vibration of the main surface 3 a of the substrate 1, so the thickness of the film 4 on the side wall surface 3 b and the chamfered surface 3 c is preferably set to a thickness that is thick enough to suppress the amplitude of vibration of the main surface 3 a. After film polishing, the glass substrate on which the film 4 has been formed is cleaned to produce a magnetic disk substrate.
[0054] When the substrate body 3 is an Al alloy substrate, the substrate body 3 is fabricated, for example, by the following method. First, the Al alloy substrate that will become the substrate body 3 is machined to the required dimensions and shape by cutting. Then, to improve the shape precision and flatness of the substrate body 3, pressure and heat annealing is performed. Furthermore, the end faces (inner and outer peripheral end faces) of the substrate body 3 are ground and polished. To grind the end faces, as with a glass substrate, a rotary tool with abrasive grains attached is pressed against the machined end face of the substrate body 3, and while both are rotating, a grinding fluid is supplied from a nozzle to grind the end face of the substrate body 3. The chamfered surface of the substrate body 3 is formed by grinding using a formed grinding wheel whose end portion is pre-shaped into a chamfered shape. Furthermore, to reduce the surface roughness of the end face, a polisher made of nonwoven fabric is adhered to the surface of the rotary tool, and the end face of the substrate body 3 is polished while a polishing fluid containing dispersed abrasive grains is supplied. Next, the main surfaces of the substrate body 3 are ground using a double-sided grinding machine, and then polished multiple times using a double-sided polishing machine with a polyurethane foam resin polisher and a polishing solution containing alumina abrasive grains or colloidal silica abrasive grains, and finally washed. The substrate body 3 may be subjected to a zincate treatment as a pretreatment for forming the film 4. After forming the film 4, an annealing treatment is appropriately performed to relieve the internal stress of the film 4. After the annealing treatment of the film 4, the main surfaces 3a are further polished. Polishing is performed multiple times depending on the needs of the substrate. After this, cleaning is performed, and the magnetic disk substrate 1 is produced.
[0055] In addition to the Ni-P alloy described above, Mg alloy, Al-Zn alloy, Mg-Zr alloy, etc. can be used for the film 4. Here, the metal material of the film 4 has a higher loss factor than the substrate body 3, with a loss factor of 0.01 or greater, in order to suppress vibration of the substrate 1. However, according to one embodiment, the loss factor of the metal material of the film 4 is preferably 0.02 or greater, and more preferably 0.03 or greater. Furthermore, the loss factor of the substrate body 3 is preferably 0.002 or less, and more preferably 0.001 or less. The smaller the loss factor of the substrate body 3, the greater the vibration suppression effect of the film 4, so a smaller loss factor for the substrate body 3 is preferable. For amorphous aluminosilicate glass substrates used for magnetic disks, the loss factor is, for example, 0.001 or less. For Al-Mg alloy substrates for magnetic disks, the loss factor is, for example, 0.002 or less. Because the loss factor of the film 4 is sufficiently greater than the loss factor of the substrate body 3, forming the film 4 effectively suppresses vibration. According to one embodiment, the Vickers hardness Hv of the material of the film 4 is set to 100 kgf / mm 2 ] or more, but 200 [kgf / mm 2 ] or more, and 400 [kgf / mm 2 ] or more is even more preferable.
[0056] Table 1 below shows the properties of materials that can be suitably used for the substrate body 3 and the film 4. The loss factors shown in Table 1 below were calculated using the above-mentioned method for calculating loss factors. The loss factor values are values at room temperature. The Vickers hardness Hv was measured using a micro Vickers hardness tester under the conditions of an indenter load of 10 gf for the film 4 because it is a thin film, and an indenter load of 300 gf for the substrate body 3.
[0057]
[0058] In Table 1 above, the loss factors of aluminosilicate glasses were determined from several glasses including the compositions of Glass 1 and Glass 2. Note that the typical loss factor value for Glass 2 is 0.0006, and the Vickers hardness is 741 kgf / mm 2 ]. The composition of the Al-Mg alloy is, for example, in mass %, Mg: 3.5 to 5%, Si: 0 to 0.05%, Fe: 0 to 0.1%, Cu: 0 to 0.12%, Mn: 0 to 0.3%, Cr: 0 to 0.1%, Zn: 0 to 0.5%, Ti: 0 to 0.1%, and the balance is Al. The composition of the Mg alloy is, in mass %, Mg: 91.57%, Al: 7.6%, Zn: 0.7%, and Mn: 0.13%. The composition of the Al-Zn alloy is, in mass %, Al: 60%, and Zn: 40%. The composition of the Mg-Zr alloy is, in mass %, Mg: 99.4%, and Zn: 0.6%. The composition of the Ni-P alloy is, in mass %, Ni: 90%, and P: 10%.
[0059] As can be seen from Table 1, it is preferable from the viewpoint of vibration suppression to use aluminosilicate glass or Al-Mg alloy as the material for the substrate body 3, and to use Ni-P alloy, Mg alloy, Al-Zn alloy, and Mg-Zr alloy as the material for the film 4. Furthermore, Ni-P alloy, Al-Zn alloy, and Mg-Zr alloy have a Vickers hardness Hv of 100 [kgf / mm 2 ] or more, which is high, and is more suitable as a material for the film 4, and particles, scratches, and dents are less likely to occur. In addition, it is understood that the Ni—P alloy has a particularly high Vickers hardness Hv, and is even more suitable as a material for the film 4.
[0060] (Experimental Example 1) Various substrates were fabricated to investigate the effects of the magnetic disk substrate 1 (Examples 1 to 21). An aluminum alloy (Al-Mg alloy) was used as the material for the substrate body of the magnetic disk substrate 1. When forming the film 4, a Ni-P alloy (P: 10% by mass, remainder Ni) was formed by electroless plating so as to cover the entire surface of the substrate body 3 with a uniform film thickness. Then, both main surfaces were polished using a double-sided polishing machine, and 10% of the thickness of the film 4 was polished off on each main surface. The final thickness of the film 4 was the same on both main surfaces, and each thickness was 90% of the thickness of the film 4 at the end face. In other words, the thickness of the film 4 at the end face was approximately 111% of the thickness of the film 4 at the main surface. The loss factor of the Ni-P alloy satisfied a value of 0.01 or greater. The fabricated substrate 1 had an outer diameter of 95 mm and an inner diameter (circular hole diameter) of 25 mm, with chamfers formed at the connections between the two main surfaces on both the outer peripheral edge and the inner peripheral edge. The specifications of this chamfer were as follows: when T was 0.64 mm or greater, the angle to the main surface was 45°, the length in the radial direction was 150 μm, and the length in the thickness direction was 150 μm. When T was less than 0.64 mm, the angle to the main surface was 45°, the length in the radial direction was 100 μm, and the length in the thickness direction was 100 μm. The roughness of the outer peripheral edge was adjusted so that the maximum height Rz was 0.1 μm on both the surface of the substrate body 3 and the surface of the substrate 1.
[0061] The fabricated substrate 1 was attached to an evaluation device equipped with a high-speed camera. This evaluation device can apply external impacts of any magnitude and capture the resulting movement (vibration) of the outer edge of the substrate as a video. The video can then be analyzed to measure the displacement of the outer edge in the normal direction of the main surface. Note that actual HDDs incorporate ramps for the ramp load mechanism of the magnetic head, and when each magnetic disk is installed, a gap of 0.2 mm is left between both main surfaces. In other words, the gap between the ramps for the magnetic disk to fit is the magnetic disk thickness + 0.4 mm. Actual HDDs are designed to maintain this gap constant even if the thickness of the substrate changes. However, the evaluation device does not include such ramps. Therefore, the amount of displacement of the substrate due to vibration determines whether or not the substrate will come into contact with the ramp in an actual HDD. If the displacement is less than 0.2 mm, it can be determined that no contact with the ramp will occur. The thickness of the magnetic film formed in the media process is substantially negligible, being approximately 100 nm or less on any one surface, even including the underlayer and soft magnetic layer. In this evaluation, the substrate was not rotated but was stationary.
[0062] Using this evaluation device, an impact test was conducted in which a 120 G impact was applied for 2 msec in the normal direction to the main surface of the substrate 1, and the vibration of the outer edge in the normal direction to the main surface was measured. The measurement results are represented as waveform data as shown in Figure 3. From this waveform data, the number of times that the displacement of the outer edge of the substrate in either direction normal to the center of the displacement amount of 0 was 0.2 mm or more was counted and evaluated based on the following evaluation criteria. In the example shown in Figure 3, the count was 4. The lower the count, the fewer times the substrate 1 came into contact with external components. Therefore, it is presumed that a magnetic disk using this substrate 1 will have a lower probability of trouble occurring after HDD startup and will extend the life of the HDD. 5 times or more... × (fail) 3 to 4 times... ○ (good: pass) 2 times or less... ◎ (excellent: pass) The evaluation results are shown in Table 2 below.
[0063]
[0064] Examples 1, 4, 7, 10, 13, 16, and 19 in Table 2 are comparative examples, and the other examples are working examples.
[0065] When the substrate thickness T was 0.381 to 0.700 mm, among Examples 1 to 21 in Table 2, all of the Examples 1, 4, 7, 10, 13, 16, and 19 satisfied D ≧ 0.0082 / T − 0.0015, and all of them were evaluated as Pass. Furthermore, Examples 3, 6, 9, 12, 15, 18, and 21, which satisfied D ≧ 0.0094 / T, were evaluated as Excellent.
[0066] (Experimental Example 2) Various substrates were fabricated (Examples 22 to 30) to investigate the effect of the substrate 1 using a glass material for the substrate body 3. The above-described glass 1 was used as the glass material. Similarly to Experimental Example 1, the film 4 was formed from a Ni-P alloy (P: 10 mass %, balance Ni) by electroless plating, similar to Experimental Example 1. Then, similar to Experimental Example 1, both main surfaces were polished using a double-sided polishing machine, and the thickness of the film 4 on each main surface was adjusted. The evaluation was also performed using the same evaluation method as Experimental Example 1, and evaluation was performed using the number of counts. The evaluation results are shown in Table 3 below.
[0067]
[0068] Of Examples 22 to 30 in Table 2, Examples 22, 25, and 28 are comparative examples, and Examples 23, 24, 26, 27, 29, and 30 are working examples. When the substrate thickness T was 0.400 to 0.640 mm, all Examples except Examples 22, 25, and 28 satisfied D ≧ 0.0082 / T − 0.0015, and all evaluation results were pass. Furthermore, Examples 24, 27, and 30, which satisfied D ≧ 0.0094 / T, were evaluated as excellent. From these evaluation results, the effect of Substrate 1 is clear.
[0069] (Experimental Example 3) Substrates 1 were fabricated with variously adjusted maximum heights Rz of the surface roughness of the outer peripheral edge surface of the substrate body 3, which forms the interface with the film 4, and peel tests were conducted to examine the effect of maximum height Rz (Examples 31 to 39). The substrate body 3 was made of the same aluminum alloy (Al-Mg alloy) as used in Experimental Example 1. The film 4 was formed using a Ni-P alloy (P: 10 mass %, balance Ni) in the same manner as in Experimental Example 1, so as to cover the entire surface of the substrate body 3 with a uniform film thickness. The maximum height Rz of the outer peripheral edge surface of the substrate 1 was adjusted by changing the size of the abrasive grains contained in the formed grindstone used for edge grinding and the size of the polishing abrasive grains used for subsequent edge polishing. In addition, when the surface roughness of the outer peripheral end face of the substrate body 3 that forms the interface with the film 4 is adjusted in various ways, the surface roughness of the film 4 at the outer peripheral end face on the substrate 1 also changes (for example, when the roughness of the interface between the substrate body 3 and the film 4 is increased, the surface roughness of the film 4 on the surface side of the substrate 1 also increases), but the maximum height Rz of the surface roughness of the film 4 at the outer peripheral end face on the substrate 1 was adjusted by appropriate edge polishing so that it was 0.5 μm or less.
[0070] A peeling test was conducted on the film 4 on the outer peripheral edge of the fabricated substrate 1. A substrate 1 in which the film 4 on the outer peripheral edge is prone to peeling is undesirable from the perspective of long-term reliability of the HDD. In other words, if the film 4 on the outer peripheral edge is partially peeled off, the effect of connecting and linking the films 4 on both main surfaces of the substrate 1 will be reduced, and there is a risk that the vibration suppression effect will be impaired.
[0071] In the peeling test, a diamond pen was used to create a scratch area on the film 4 formed on the sidewall surface of the outer peripheral end face, with five consecutive scratches in the thickness direction at 1 mm intervals around the circumferential direction of the sidewall surface. Adhesive tape was pressed against the scratch area, the tape was peeled off, and the surface of the film 4 where the tape was peeled was observed under a microscope to evaluate the degree of peeling of the film 4. Twelve scratch areas were created around the outer peripheral end face, spaced 30° apart. The degree of peeling of the film 4 was examined at each location, and the number of locations where peeling of the film 4 occurred was counted. Film 4 that was beginning to peel was also counted as peeled and classified as follows: Level 1: Film 4 peeled in 10 or more locations. Level 2: Film 4 peeled in 7 to 9 locations. Level 3: Film 4 peeled in 4 to 6 locations. Level 4: Film 4 peeled in 0 to 3 locations. The evaluation results are shown in Table 4 below. Examples 6, 9, and 12 shown in Table 4 are Examples 6, 9, and 12 in Experimental Example 1, and the maximum height Rz of the interface between the substrate body 3 and the film 4 in Examples 6, 9, and 12 was 0.1 μm. In addition, the surface roughness of the film 4 at the outer peripheral end face in Examples 6, 9, and 12 shown in Table 4 (i.e., the surface roughness of the substrate 1) was 0.1 μm in maximum height Rz value, and in Examples 31 to 39, the maximum height Rz value was 0.5 μm.
[0072]
[0073] The results in Table 4 show that the resistance to peeling is improved by making the maximum height Rz 0.5 μm or more, regardless of the thicknesses T and D. In particular, the resistance to peeling is further improved by making the maximum height Rz 1.0 μm or more, and the resistance to peeling is further improved by making the maximum height Rz 1.5 μm or more. The effect of the maximum height Rz is clear from the above evaluation results.
[0074] The magnetic disk substrate and magnetic disk of the present invention have been described in detail above, but the present invention is not limited to the above-mentioned embodiments and examples, and various improvements and modifications may be made without departing from the spirit and scope of the present invention.
[0075] REFERENCE SIGNS LIST 1 magnetic disk substrate 2 inner hole 3 substrate body 3a main surface 3b side wall surface 3c chamfered surface 4 film
Claims
1. A substrate for a magnetic disk, comprising: a substrate body having two main surfaces; and a film of a metallic material provided on the main surfaces and having a loss factor value of 0.01 or more, wherein the thickness T of the substrate for a magnetic disk including the film is 0.700 mm or less, and the total thickness D [mm] of the film provided on the main surfaces and the thickness T [mm] of the substrate for a magnetic disk including the film satisfy the following formula (1): D ≧ 0.0082 / T - 0.0015... (1).
2. The substrate for a magnetic disk according to claim 1, wherein the thickness D [mm] of the film and the thickness T [mm] of the substrate including the film satisfy the following formula (2): D ≧ 0.0094 / T... (2).
3. The substrate for a magnetic disk according to claim 1 or 2, wherein the substrate for a magnetic disk has a disk shape, and the outer diameter of the disk shape is 90 mm or more.
4. A substrate for a magnetic disk, comprising: a substrate body having two main surfaces; and a film provided on the main surfaces, wherein the substrate for a magnetic disk has a disk shape with an outer diameter of 90 mm or more, the thickness T of the substrate for a magnetic disk including the film is 0.700 mm or less, and when an impact of 120 [G] is applied in the normal direction of the main surface at 2 [msec] with the inner peripheral portion of the substrate fixed, the number of times the displacement amount due to the vibration in the plate thickness direction of the outer peripheral end portion of the substrate becomes 0.2 mm or more is 4 times or less, and the film is provided accordingly.
5. The substrate for a magnetic disk according to any one of claims 1 to 4, wherein the film is provided so as to cover the entire surface of the substrate, the film thickness of the film at the end face of the substrate is thicker than the film thickness of the film at the main surface, and the film is provided such that the film thickness at the end face is 110% or more of the film thickness at the main surface.
6. The substrate for a magnetic disk according to any one of claims 1 to 5, wherein the thickness T of the substrate is 0.640 mm or less.
7. The substrate for a magnetic disk according to any one of claims 1 to 5, wherein the thickness T of the substrate is 0.520 mm or less.
8. The Vickers hardness Hv of the film is 100 [kgf / mm 2 , and the substrate for a magnetic disk according to any one of claims 1 to 7.
9. The metal material of the film includes a Ni-P alloy, and the substrate for a magnetic disk according to any one of claims 1 to 8.
10. The film is formed on the main surface and the outer peripheral end face of the substrate body, and the maximum height Rz of the surface roughness of the outer peripheral end face of the substrate body that forms the interface with the film is 0.5 μm or more. The substrate for a magnetic disk according to any one of claims 1 to 9.
11. The film is formed on the main surface and the outer peripheral end face of the substrate body, and the maximum height Rz of the surface roughness of the film on the outer peripheral end face of the non-magnetic substrate for a magnetic disk is smaller than the maximum height Rz of the surface roughness of the substrate body on the outer peripheral end face of the substrate body. The substrate for a magnetic disk according to any one of claims 1 to 10.
12. A magnetic disk having at least a magnetic film on the surface of the substrate for a magnetic disk according to any one of claims 1 to 11.