Fiber for artificial hair, and wig

LAP905AUndetermined Publication Date: 2026-04-10ADERANS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
LAP905
Authority / Receiving Office
LA · LA
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-11
Filing Date
2023-02-28
Publication Date
2026-04-10

AI Technical Summary

Technical Problem

Artificial hair fibers containing polyamide face challenges in replicating the natural gloss and texture of human hair, experiencing static electricity issues, and having inadequate antistatic and heat-setting properties, which affect styling and durability.

Method used

Incorporating a thermoplastic polyamide with a polymer antistatic agent that is compatible and has a lower melting point, along with an incompatible thermoplastic polyester, to create an artificial hair fiber with suppressed luster and enhanced antistatic and heat-setting properties, maintaining style and reducing static electricity.

Benefits of technology

The artificial hair fibers achieve a natural-like texture and gloss, with long-lasting antistatic properties and improved heat-setting capabilities, allowing for easier styling and long-term hairstyle maintenance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

A problem to be solved of the invention is to provide a fiber for artificial hair comprising polyamide, which has a glossy feeling with suppressed luster similar to natural hair, is excellent in persistent antistatic properties, and also excellent in heat-setting properties. The means for solving the problem is a fiber for artificial- hair comprising a thermoplastic polyamide and a polymeric antistatic agent having compatibility with the thermoplastic polyamide, wherein the polymeric antistatic agent has a melting point equal to or lower than the melting point of the thermoplastic polyamide.
Need to check novelty before this filing date? Find Prior Art

Description

Artificial hair fibers and wigs

[0001] The present invention relates to fibers for artificial hair used for wigs, hair extensions or substitute hair, and in particular to fibers for artificial hair containing polyamide.

[0002] Polyamide-containing artificial hair fibers are more flexible and supple than synthetic fibers such as polyester, and have a texture and feel closer to that of natural hair. However, it is difficult to achieve the glossy feel that is characteristic of natural hair, which is expressed by the unevenness of the cuticle. Furthermore, artificial hair fibers generally have low moisture retention, and static electricity is generated during styling, making it difficult to style.

[0003] Patent Document 1 describes a fiber for artificial hair that is formed from a first thermoplastic resin as a matrix and a second thermoplastic resin that is incompatible with the first thermoplastic resin and has a different melting point, the fiber having an uneven surface, the protrusions of the fiber being formed from the first thermoplastic resin. The fiber for artificial hair in Patent Document 1 can suppress gloss while maintaining the glossiness of natural hair without impairing the physical properties such as strength of the matrix.

[0004] Patent Document 2 describes an artificial hair fiber material obtained by mixing a polyamide with an additive consisting of a polyalkylene ether phosphate compound, forming the resulting fiber, and then eluting the additive. Since the additive has water retention and antistatic properties, the artificial hair fiber material of Patent Document 2 exhibits water retention and antistatic properties. However, elution of the additive causes depressions or sponge-like cavities to form in the spaces previously occupied by the additive, resulting in the formation of small voids on the surface of the fiber material.

[0005] Patent Document 3 describes polyamide fibers for artificial hair formed from a nylon 46 polymer composition containing cuprous halide and an alkali metal halide or alkaline earth metal halide as a heat-resistant agent. A conductive substance such as conductive carbon black can be added to the polyamide fibers for artificial hair, which prevents deterioration of shape retention due to static electricity and staining due to the adhesion of dust and the like when used as artificial hair.

[0006] WO2010 / 134561 JP-A-47-37649 JP-A-1-282309

[0007] It is desirable that the artificial hair be pre-formed with a predetermined curl during the manufacturing process. This allows the user of the artificial hair to maintain the hairstyle for a long time after styling. It is also desirable that the artificial hair does not become statically charged. In this case, the user can easily use a brush or the like to style the desired hairstyle (hereinafter sometimes referred to as "styling").

[0008] For example, the polyamide-containing artificial hair fiber described in Patent Document 1 does not have sufficient antistatic properties and shapeability by heat treatment (hereinafter sometimes referred to as "heat setting property"), and there are still problems such as difficulty in forming curls during the production stage and difficulty in styling during use.

[0009] When the additive of Patent Document 2 is used, small voids that do not normally exist in natural hair are formed on the surface of the fiber material, making it difficult to achieve the glossy feel that is unique to natural hair.In addition, since the additive of Patent Document 2 migrates from the inside of the fiber material to the surface, it falls off every time the hair is washed or wiped, and therefore the durability of the antistatic properties is insufficient.

[0010] The conductive substance of Patent Document 3 is incompatible with polyamide and has a large effect on the physical properties of the artificial hair fiber, such as flexibility and strength, making it difficult to reproduce the texture of natural hair when used.

[0011] The present invention solves the above problems, and its object is to provide a polyamide-containing fiber for artificial hair that has a luster with a controlled luster similar to that of natural hair, has excellent long-lasting antistatic properties, and is also excellent in heat setting properties.

[0012] The present invention provides a fiber for artificial hair comprising a thermoplastic polyamide and a polymeric antistatic agent that is compatible with the thermoplastic polyamide, wherein the polymeric antistatic agent has a melting point equal to or lower than the melting point of the thermoplastic polyamide.

[0013] In one embodiment, the polymeric antistatic agent has a melting point of 160 to 250°C.

[0014] In one embodiment, the polymeric antistatic agent has a melt flow rate at 215° C. of 10 to 40 g / 10 min.

[0015] In one embodiment, the polymeric antistatic agent is 10 6 ~10 10 It has a surface resistivity of Ω / □.

[0016] In one embodiment, the polymeric antistatic agent includes a polyetheresteramide block copolymer.

[0017] In one embodiment, the polyetheresteramide block copolymer is a condensation product of a polyamide having carboxyl groups at both ends and an aromatic ring-containing polyetherdiol.

[0018] In one embodiment, the polymeric antistatic agent is contained in an amount of 0.5 to 10% by weight.

[0019] In one embodiment, the artificial hair fiber further contains a thermoplastic polyester that is incompatible with the thermoplastic polyamide and has a higher melting point.

[0020] In one embodiment, the artificial hair fiber has a weight ratio of thermoplastic polyamide to thermoplastic polyester of 75 / 25 to 85 / 15.

[0021] In one embodiment, the artificial hair fiber has a concave-convex shape formed on the surface, and the convex portions of the concave-convex shape contain particles of thermoplastic polyester.

[0022] In one embodiment, the artificial hair fiber has a matrix comprising a thermoplastic polyamide and a domain comprising a thermoplastic polyester.

[0023] In one embodiment, the thermoplastic polyamide is at least one thermoplastic resin selected from the group consisting of linear saturated aliphatic polyamides, alternating copolymers of hexamethylenediamine and terephthalic acid, and alternating copolymers of metaxylenediamine and adipic acid.

[0024] In one embodiment, the thermoplastic polyester is at least one thermoplastic resin selected from the group consisting of polyethylene terephthalate and polybutylene terephthalate.

[0025] The present invention also provides a wig comprising a wig base and any of the above artificial hair fibers implanted in the wig base.

[0026] The artificial hair fiber containing the polyamide of the present invention has a luster with a controlled luster similar to that of natural hair, and has excellent antistatic properties and heat setting properties. Therefore, the artificial hair fiber of the present invention can be appropriately curled during the production stage, can be easily styled during use, and the styled hairstyle will remain in place for a long time.

[0027] Fig. 3 is a schematic diagram of a spinning apparatus using a general single-screw extruder used in the production of the synthetic fiber used in the present invention. Fig. 4 is a schematic diagram of a spinning apparatus using a general twin-screw extruder used in the production of the synthetic fiber used in the present invention. Fig. 5 is a schematic diagram of the die part of Figs. 1 and 2. Fig. 6 is a diagram showing an outline of the process from spinning of the synthetic fiber used in the present invention to winding the fiber. Fig. 7 is an 800x magnification image showing the surface of the artificial hair fiber of Example 16. Fig. 8 is a 1,000x magnification image showing the cross section of the artificial hair fiber of Example 16.

[0028] <Artificial Hair Fiber> The artificial hair fiber of the present invention contains a thermoplastic polyamide and a polymeric antistatic agent that is compatible with the thermoplastic polyamide. The thermoplastic polyamide is the component that constitutes the outer shape of the artificial hair fiber, i.e., the base material. This gives the artificial hair fiber a texture and feel similar to natural hair, and excellent antistatic properties and heat setting properties.

[0029] (Thermoplastic Polyamide) The thermoplastic polyamide contained in the artificial hair fiber of the present invention may be one that has been conventionally used as a raw material for artificial hair fibers. Examples of the thermoplastic polyamide include linear saturated aliphatic polyamides such as nylon 6, nylon 66, and nylon 610, and semi-aromatic polyamides such as nylon 6T, which is an alternating copolymer of hexamethylenediamine and terephthalic acid, and nylon MXD6, which is a polymer in which adipic acid and metaxylenediamine are bonded via an amide bond.

[0030] The thermoplastic polyamide preferably has a melting point of 170 to 270°C. If the melting point of the thermoplastic polyamide is less than 170°C, the heat resistance required for artificial hair will be insufficient, and if it exceeds 270°C, undissolved polyamide will cause poor mixing. The melting point of the thermoplastic polyamide is more preferably 200 to 250°C, and even more preferably 215 to 240°C.

[0031] The thermoplastic polyamide preferably has a melt flow rate of 10 to 80 g / 10 min at 240°C and 21.18 N. If the melt flow rate of the thermoplastic polyamide is less than 10 g / 10 min, insufficient mixing will result in uneven color development, and if it exceeds 80 g / 10 min, molding defects will occur due to draw resonance. The melt flow rate of the thermoplastic polyamide is more preferably 15 to 60 g / 10 min, and even more preferably 20 to 40 g / 10 min.

[0032] (Polymer-type antistatic agent) The polymer-type antistatic agent contained in the artificial hair fiber of the present invention may be one that has been conventionally used as an antistatic agent for synthetic resin materials. Polymer-type antistatic agents have little humidity dependency and are less likely to migrate from the interior of the fiber material to the surface. In other words, by adding a polymer-type antistatic agent to the fiber material and compatibilizing it, a conductive circuit is formed inside the fiber material, imparting antistatic properties. As a result, the obtained artificial hair fiber has a good appearance and feel, and the antistatic effect is highly durable.

[0033] From the viewpoint of achieving the above-mentioned effects, the polymer-type antistatic agent preferably has a polyether structure, and more preferably has a polyethylene oxide structure.

[0034] The polymeric antistatic agent preferably has a melting point of 160 to 250°C. If the melting point of the polymeric antistatic agent is less than 160°C, the heat setting ability of the resulting artificial hair fiber will be reduced, and if it exceeds 250°C, the polymeric antistatic agent will be difficult to mix uniformly into the fiber material, and the resulting artificial hair fiber will likely have insufficient antistatic effect and will also be prone to poor appearance. The melting point of the polymeric antistatic agent is preferably 180 to 230°C, more preferably 190 to 210°C.

[0035] The polymeric antistatic agent preferably has a melting point close to that of the thermoplastic polyamide used as the base material. The melting point of the polymeric antistatic agent being close to that of the thermoplastic polyamide facilitates improvement of the curling performance of the artificial hair fiber. The difference between the melting point of the polymeric antistatic agent and that of the thermoplastic polyamide is, for example, within 30°C, preferably within 15°C, and more preferably within 10°C.

[0036] The polymeric antistatic agent preferably has a melting point equal to or lower than that of the thermoplastic polyamide used as the base material. If the melting point of the polymeric antistatic agent exceeds that of the thermoplastic polyamide, it may be difficult to uniformly mix the polymeric antistatic agent into the fiber material.

[0037] In one embodiment, the polymeric antistatic agent preferably has a melt flow rate of 10 to 40 g / 10 min at 215°C and 21.18 N. If the melt flow rate of the polymeric antistatic agent is less than 10 g / 10 min, the polymeric antistatic agent is difficult to mix uniformly into the fiber material, and the antistatic effect of the resulting artificial hair fiber is likely to be insufficient and the appearance is likely to be poor. If the melt flow rate exceeds 40 g / 10 min, the polymeric antistatic agent is likely to migrate from the interior to the surface of the fiber material, which may result in a decrease in the appearance, feel, or durability of the antistatic effect. The melt flow rate of the polymeric antistatic agent is preferably 15 to 35 g / 10 min, and more preferably 18 to 32 g / 10 min.

[0038] In another embodiment, the polymeric antistatic agent preferably has a melt flow rate at 190°C and 21.18 N of 3 to 35 g / 10 min. If the melt flow rate of the polymeric antistatic agent is less than 3 g / 10 min, the polymeric antistatic agent is difficult to mix uniformly into the fiber material, and the antistatic effect of the resulting artificial hair fiber is likely to be insufficient and the appearance is likely to be poor. If the melt flow rate exceeds 35 g / 10 min, the polymeric antistatic agent is likely to migrate from the inside to the surface of the fiber material, which may result in a decrease in the appearance, feel, or durability of the antistatic effect. The melt flow rate of the polymeric antistatic agent is preferably 5 to 30 g / 10 min, more preferably 8 to 17 g / 10 min.

[0039] The polymeric antistatic agent preferably has a melt flow rate equal to or greater than the melt flow rate of the thermoplastic polyamide used as the base material. If the melt flow rate of the polymeric antistatic agent is lower than the melt flow rate of the thermoplastic polyamide, it may be difficult to uniformly mix the polymeric antistatic agent into the fiber material.

[0040] The polymeric antistatic agent is preferably 10 10 The surface resistivity of the polymer-type antistatic agent is 10 10 If the surface resistivity exceeds Ω / □, the antistatic effect tends to be insufficient. 9 Ω / □ or less, more preferably 10 6 ~10 9 The surface resistivity of the polymer-type antistatic agent can be measured by molding the polymer-type antistatic agent alone, wetting it at 23° C. and 50 RH for 4 hours, and then measuring it with a super megohmmeter.

[0041] The polymeric antistatic agent has a thermal decomposition onset temperature of 200°C or higher. If the thermal decomposition onset temperature of the polymeric antistatic agent is lower than 200°C, the polymeric antistatic agent is likely to decompose and deteriorate during the process of spinning the fiber material. The thermal decomposition onset temperature of the polymeric antistatic agent is preferably 230°C or higher, more preferably 250 to 300°C. The thermal decomposition onset temperature of the polymeric antistatic agent can be measured in air using a thermogravimetric differential thermal analyzer (TG-DTA).

[0042] Commercially available polymeric antistatic agents may be used. Examples of commercially available polymeric antistatic agents include "Pelestat 6200" (trade name), "Pelestat 6500" (trade name), "Pelestat NC6321" (trade name), "Pelestat NC7530" (trade name), and "Peletron AS" (trade name), manufactured by Sanyo Chemical Industries, Ltd. These contain polyether ester amide block copolymers.

[0043] Another example of a commercially available polymeric antistatic agent that can be used is "Pelectron LMP-FS" (trade name) manufactured by Sanyo Chemical Industries, Ltd. This agent contains a polyether / polyolefin block copolymer.

[0044] The polymeric antistatic agent is preferably contained in the artificial hair fiber in an amount of 0.5 to 10% by weight. If the content of the polymeric antistatic agent in the artificial hair fiber is less than 0.5% by weight, the antistatic properties will be insufficient, and if it exceeds 10% by weight, the polymeric antistatic agent will migrate from the inside of the fiber material to the surface, making it more likely to cause tack and blocking. The content of the polymeric antistatic agent in the artificial hair fiber is preferably 1 to 6% by weight, more preferably 1.5 to 4% by weight.

[0045] Examples of polymeric antistatic agents include block copolymers having a polyether block and a block exhibiting affinity for thermoplastic polyamide, polyether / polyolefin block copolymers, and polyetheresteramide block copolymers. Among polymeric antistatic agents, polyetheresteramide block copolymers are preferred because of their excellent compatibility with polyamide. Among the polyether blocks, polyethylene oxide blocks are preferred.

[0046] (Polyether / Polyolefin Block Copolymer) The polyether / polyolefin block copolymer is, for example, a block polymer having a structure in which blocks of the following polyolefin (a) and blocks of the following polyoxyethylene chain (b) are repeatedly and alternately bonded via at least one bond selected from the group consisting of an ester bond, an amide bond, an ether bond, and an imide bond. Such a block polymer is described in WO 00 / 47652, the disclosure of which is incorporated herein by reference.

[0047] As the polyolefin (a) block, polyolefins obtained by (co)polymerization (meaning polymerization or copolymerization; the same applies hereinafter) of one or a mixture of two or more olefins having 2 to 30 carbon atoms [those obtained by polymerization method], and low-molecular-weight polyolefins obtained by thermal degradation of high-molecular-weight polyolefins (polyolefins obtained by polymerization of olefins having 2 to 30 carbon atoms) [those obtained by thermal degradation method] can be used.

[0048] Examples of the olefin having 2 to 30 carbon atoms include ethylene, propylene, α-olefins having 4 to 30 carbon atoms (preferably 4 to 12, more preferably 4 to 10), and dienes having 4 to 30 carbon atoms (preferably 4 to 18, more preferably 4 to 8).

[0049] Examples of the α-olefin having 4 to 30 carbon atoms include 1-butene, 4-methyl-1-pentene, 1-pentene, 1-octene, 1-decene, and 1-dodecene, and examples of the diene include butadiene, isoprene, cyclopentadiene, and 1,11-dodecadiene.

[0050] Among these, preferred are olefins having 2 to 12 carbon atoms (ethylene, propylene, α-olefins having 4 to 12 carbon atoms, butadiene and / or isoprene, etc.), more preferred are olefins having 2 to 10 carbon atoms (ethylene, propylene, α-olefins having 4 to 10 carbon atoms and / or butadiene, etc.), and particularly preferred are ethylene, propylene and / or butadiene.

[0051] Low-molecular-weight polyolefins obtained by thermal degradation can be easily obtained, for example, by the method described in JP-A-3-62804. Polyolefins obtained by polymerization can be produced by known methods, for example, by (co)polymerizing the above-mentioned olefins in the presence of a radical catalyst, a metal oxide catalyst, a Ziegler catalyst, a Ziegler-Natta catalyst, or the like.

[0052] Examples of the block of polyoxyethylene chain (b) include residues obtained by removing hydroxyl groups from polyether diols obtained by addition reaction of diols (b01) or dihydric phenols (b02) with alkylene oxides (having 3 to 12 carbon atoms).

[0053] The structure of such polyether diol can be represented by the general formula: H(OA1)mO-E1-O(AO)m'H.

[0054] In the formula, E1 represents a residue obtained by removing a hydroxyl group from (b01) or (b02), A1 represents an alkylene group having 2 to 12 carbon atoms (preferably 2 to 8, more preferably 2 to 4) that essentially contains an alkylene group having 2 carbon atoms and which may contain a halogen atom; m and m' represent integers of 1 to 300, preferably 2 to 250, and particularly preferably 10 to 100, and m and m' may be the same or different. Furthermore, m (OA1)s and m' (A1O)s may be the same or different, and when they are composed of two or more oxyalkylene groups each containing ethylene oxide as an essential component, the bonding form may be block, random, or a combination thereof.

[0055] Examples of the diol (b01) include dihydric alcohols (aliphatic, alicyclic, and araliphatic dihydric alcohols) having 2 to 12 carbon atoms (preferably 2 to 10, more preferably 2 to 8), and tertiary amino group-containing diols having 1 to 12 carbon atoms.

[0056] Examples of the aliphatic dihydric alcohol include ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, and 1,12-dodecanediol.

[0057] Examples of the alicyclic dihydric alcohol include 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, 1,4-cyclooctanediol, and 1,3-cyclopentanediol.

[0058] Examples of aromatic aliphatic dihydric alcohols include xylylenediol, 1-phenyl-1,2-ethanediol, and 1,4-bis(hydroxyethyl)benzene.

[0059] Examples of the tertiary amino group-containing diol include bishydroxyalkyl (alkyl group having 1 to 12, preferably 2 to 10, more preferably 2 to 8 carbon atoms) compounds of aliphatic or alicyclic primary monoamines (having 1 to 12, preferably 2 to 10, more preferably 2 to 8 carbon atoms) and bishydroxyalkyl (alkyl group having 1 to 12 carbon atoms) compounds of aromatic (aliphatic) primary monoamines (having 6 to 12 carbon atoms).

[0060] Bishydroxyalkylated monoamines can be easily obtained by known methods, for example, by reacting a monoamine with an alkylene oxide having 2 to 4 carbon atoms (ethylene oxide, propylene oxide, butylene oxide, etc.) or by reacting a monoamine with a hydroxyalkyl halide having 1 to 12 carbon atoms (2-bromoethyl alcohol, 3-chloropropyl alcohol, etc.).

[0061] Examples of aliphatic primary monoamines include methylamine, ethylamine, 1- and 2-propylamine, n- and i-amylamine, hexylamine, 1,3-dimethylbutylamine, 3,3-dimethylbutylamine, 2- and 3-aminoheptane, heptylamine, nonylamine, decylamine, undecylamine, and dodecylamine.

[0062] Examples of the alicyclic primary monoamines include cyclopropylamine, cyclopentylamine, cyclohexylamine, etc. Examples of the aromatic (aliphatic) primary monoamines include aniline and benzylamine, etc.

[0063] The dihydric phenol (b02) has 6 to 18 carbon atoms (preferably 8 to 18, more preferably 10 to 15), and examples thereof include monocyclic dihydric phenols (hydroquinone, catechol, resorcinol, urushiol, etc.), bisphenols (bisphenol A, bisphenol F, bisphenol S, 4,4'-dihydroxydiphenyl-2,2-butane, dihydroxybiphenyl, etc.), and condensed polycyclic dihydric phenols (dihydroxynaphthalene, binaphthol, etc.).

[0064] Among (b01) and (b02), from the viewpoint of antistatic properties, dihydric alcohols and dihydric phenols are preferred, aliphatic dihydric alcohols and bisphenols are more preferred, and ethylene glycol and bisphenol A are particularly preferred.

[0065] Examples of the alkylene oxide to be subjected to the addition reaction with the diol (b01) or the dihydric phenol (b02) include ethylene oxide and alkylene oxides having 3 to 12 carbon atoms (propylene oxide, 1,2-, 1,4-, 2,3- and 1,3-butylene oxide, and mixtures of two or more thereof), and if necessary, other alkylene oxides and substituted alkylene oxides may be used in combination.

[0066] From the viewpoint of improving the appearance, feel, and antistatic performance of the artificial hair fiber, the preferred alkylene oxide is ethylene oxide, and in this case, the polymeric antistatic agent becomes a block polymer having a polyethylene oxide structure.

[0067] Examples of other alkylene oxides and substituted alkylene oxides include epoxidized products of α-olefins having 5 to 12 carbon atoms, styrene oxide, and epihalohydrins (epichlorohydrin, epibromohydrin, etc.), etc. The amount of each of the other alkylene oxides and substituted alkylene oxides used is preferably 30% by weight or less, more preferably 0 or 25% by weight or less, and particularly preferably 0 or 20% by weight or less, based on the weight of the total alkylene oxide, from the viewpoint of antistatic properties.

[0068] From the viewpoint of the volume resistivity of the polymer (b) having a polyoxyethylene chain, the number of moles of alkylene oxide added is preferably 1 to 300 moles, more preferably 2 to 250 moles, and particularly preferably 10 to 100 moles per hydroxyl group of (b01) or (b02). When two or more alkylene oxides are used in combination, the bonding form may be either random and / or block.

[0069] The addition reaction of alkylene oxide can be carried out by a known method, for example, in the presence of an alkali catalyst (potassium hydroxide, sodium hydroxide, etc.) at 100 to 200° C. and a pressure of 0 to 0.5 MPaG.

[0070] (Polyetheresteramide Block Copolymer) The polyetheresteramide block copolymer is, for example, a polyetheresteramide derived from the following polyamide (a11) and the following alkylene oxide adduct of a bisphenol compound (a12). Such polyetheresteramides are described in JP-A-6-287547 and JP-B-4-5691, the disclosures of which are incorporated herein by reference.

[0071] Examples of the polyamide (a11) include (1) lactam ring-opening polymers, (2) polycondensates of aminocarboxylic acids, and (3) polycondensates of dicarboxylic acids and diamines.

[0072] Among these amide-forming monomers that form polyamides, lactams in (1) include those having 6 to 12 carbon atoms, such as caprolactam, enantholactam, laurolactam, and undecanolactam.

[0073] The aminocarboxylic acid in (2) includes those having 6 to 12 carbon atoms, such as ω-aminocaproic acid, ω-aminoenanthic acid, ω-aminocaprylic acid, ω-aminopergonic acid, ω-aminocapric acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid.

[0074] Examples of the dicarboxylic acid in (3) include aliphatic dicarboxylic acids, aromatic (aliphatic) dicarboxylic acids, alicyclic dicarboxylic acids, amide-forming derivatives thereof [e.g., acid anhydrides and lower (C1 to C4) alkyl esters], and mixtures of two or more of these.

[0075] Examples of the aliphatic dicarboxylic acid include those having 4 to 20 carbon atoms, such as succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, maleic acid, fumaric acid, and itaconic acid.

[0076] Examples of aromatic (aliphatic) dicarboxylic acids include those having 8 to 20 carbon atoms, such as ortho-, iso-, and terephthalic acid, naphthalene-2,6- and -2,7-dicarboxylic acid, diphenyl-4,4'dicarboxylic acid, diphenoxyethanedicarboxylic acid, and alkali metal (sodium, potassium, etc.) salts of 3-sulfoisophthalic acid. Examples of alicyclic dicarboxylic acids include those having 7 to 14 carbon atoms, such as cyclopropanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, cyclohexenedicarboxylic acid, and dicyclohexyl-4,4-dicarboxylic acid.

[0077] Among the amide-forming derivatives, examples of the acid anhydrides include anhydrides of the above-mentioned dicarboxylic acids, such as maleic anhydride, itaconic anhydride, and phthalic anhydride, and examples of the lower (C1 to C4) alkyl esters include lower alkyl esters of the above-mentioned dicarboxylic acids, such as dimethyl adipate, and dimethyl ortho-, iso-, and terephthalate.

[0078] The diamine may be one having 6 to 12 carbon atoms, such as hexamethylenediamine, heptamethylenediamine, octamethylenediamine, or decamethylenediamine.

[0079] The above amide-forming monomers may be used in combination of two or more thereof.

[0080] Of these, caprolactam, 12-aminododecanoic acid, and adipic acid / hexamethylenediamine are preferred from the viewpoint of antistatic properties, and caprolactam is particularly preferred.

[0081] The polyamide (a11) can be obtained by carrying out ring-opening polymerization or polycondensation of the above-mentioned amide-forming monomers in the presence of one or more dicarboxylic acids having 4 to 20 carbon atoms as a molecular weight modifier in a conventional manner.

[0082] Examples of the dicarboxylic acid having 4 to 20 carbon atoms include those exemplified in the above (3). Among these, from the viewpoint of antistatic properties, aliphatic dicarboxylic acids, aromatic dicarboxylic acids, and alkali metal 3-sulfoisophthalates are preferred, and adipic acid, sebacic acid, terephthalic acid, isophthalic acid, and sodium 3-sulfoisophthalate are more preferred.

[0083] The amount of the molecular weight modifier used is preferably 2 to 80% by weight, more preferably 4 to 75% by weight, based on the total weight of the amide-forming monomer and the molecular weight modifier, from the viewpoint of antistatic properties and heat resistance.

[0084] The number average molecular weight of the polyamide (a11) is preferably 200 to 5,000, more preferably 500 to 3,000, from the viewpoints of reactivity and heat resistance of the resulting polyetheresteramide.

[0085] Examples of the bisphenol compound constituting the alkylene oxide adduct (a12) of a bisphenol compound include compounds having 13 to 20 carbon atoms, such as bisphenol A, bisphenol F, and bisphenol S. Of these, bisphenol A is preferred from the viewpoint of dispersibility.

[0086] Examples of alkylene oxides to be added to the bisphenol compound include alkylene oxides having 2 to 12 carbon atoms, such as ethylene oxide, propylene oxide, 1,2-, 2,3-, and 1,4-butylene oxide, epoxidized products of α-olefins having 5 to 12 carbon atoms, styrene oxide, and epihalohydrins (epichlorohydrin, epibromohydrin, etc.), and mixtures of two or more of these.

[0087] From the viewpoint of improving the appearance, feel, and antistatic performance of the artificial hair fiber, the preferred alkylene oxide is ethylene oxide, and in this case, the polymeric antistatic agent becomes a block polymer having a polyethylene oxide structure.

[0088] The number average molecular weight of the alkylene oxide adduct (a12) of a bisphenol compound is preferably 300 to 5,000, more preferably 500 to 4,000, from the viewpoint of antistatic properties.

[0089] The proportion of (a12) based on the total weight of (a11) and (a12) is preferably 20 to 80% by weight, more preferably 30 to 70% by weight, from the viewpoint of the antistatic property and heat resistance of the polyether ester amide.

[0090] Specific examples of the method for producing polyether ester amide include the following methods (1) and (2), but the method is not particularly limited.

[0091] Production method (1): A method in which an amide-forming monomer is reacted with a dicarboxylic acid (molecular weight modifier) ​​to form (a11), and (a12) is added to this, followed by polymerization reaction at high temperature (160 to 270°C) and reduced pressure (0.03 to 3 kPa).

[0092] Production method (2): An amide-forming monomer, a dicarboxylic acid (molecular weight modifier), and (a12) are simultaneously charged into a reaction vessel, and reacted at high temperature (160 to 270°C) under pressure (0.1 to 1 MPa) in the presence or absence of water to produce intermediate (a11), which is then polymerized with (a12) under reduced pressure (0.03 to 3 kPa).

[0093] Of the above processes, process (1) is preferred from the viewpoint of reaction control.

[0094] In addition to the above, polyetheresteramide may be produced by substituting the terminal hydroxyl groups of (a12) with amino or carboxyl groups, followed by reaction with a polyamide having a carboxyl or amino group at its terminal.

[0095] The method for substituting the terminal hydroxyl group of the alkylene oxide adduct (a12) of a bisphenol compound with an amino group includes known methods, such as a method of cyanoalkylating the hydroxyl group and reducing the resulting terminal cyanoalkyl group to form an amino group [for example, a method of reacting (a12) with acrylonitrile and hydrogenating the resulting cyanoethylated product].

[0096] Examples of a method for substituting the terminal hydroxyl group of the alkylene oxide adduct (a12) of a bisphenol compound with a carboxyl group include a method of oxidizing with an oxidizing agent [for example, a method of oxidizing the hydroxyl group of (a12) with chromic acid].

[0097] In the above polymerization reaction, a commonly used known esterification catalyst is used, such as an antimony catalyst (e.g., antimony trioxide), a tin catalyst (e.g., monobutyltin oxide), a titanium catalyst (e.g., tetrabutyl titanate), a zirconium catalyst (e.g., tetrabutyl zirconate), or a metal acetate catalyst (e.g., zinc acetate, zirconyl acetate).

[0098] The amount of the catalyst used is preferably 0.1 to 5% by weight, based on the total weight of (a11) and (a12), and more preferably 0.2 to 3% by weight from the viewpoints of reactivity and resin properties.

[0099] The polyetheresteramide block copolymer is preferably a condensation product of a polyamide having carboxyl groups at both ends and an aromatic ring-containing polyetherdiol. Specific examples of the aromatic ring moiety of the aromatic ring-containing polyetherdiol include residues of dihydric phenols selected from bisphenols, monocyclic dihydric phenols, dihydroxybiphenyls, dihydroxynaphthalenes, and binaphthols. Among these, the preferred aromatic ring moiety is a residue of a bisphenol.

[0100] The aromatic ring-containing polyether diol has an aromatic ring moiety, which improves the heat resistance of the polyether ester amide block copolymer, making it easier to prevent decomposition and deterioration during the spinning process, and also makes it easier to adjust the melting point of the polyether ester amide block copolymer to a temperature appropriate for spinning.

[0101] The polyamide having carboxyl groups at both ends may be, for example, (1) a lactam ring-opening polymer, (2) a polycondensation product of an aminocarboxylic acid, or (3) a polycondensation product of a dicarboxylic acid and a diamine. The polyamide having carboxyl groups at both ends has a number average molecular weight of, for example, 500 to 5,000, preferably 800 to 3,000. If the number average molecular weight is less than 500, the heat resistance of the polyetheresteramide itself decreases, while if it exceeds 5,000, the reactivity decreases, making the production of the polyetheresteramide time-consuming.

[0102] The aromatic-containing polyether diol may be, for example, a polyether diol produced by an addition reaction of an alkylene oxide with an aromatic ring-containing diol. The number of moles of alkylene oxide added is usually 1 to 30 moles, preferably 2 to 20 moles each. The aromatic-containing polyether diol has a number average molecular weight of, for example, 500 to 5,000, preferably 800 to 3,000. If the number average molecular weight is less than 500, the antistatic properties will be insufficient, while if it exceeds 5,000, the reactivity will decrease, making the production of polyether ester amides extremely time-consuming.

[0103] It is preferable that the polyether ester amide block copolymer does not substantially contain antistatic components consisting of metal salts such as alkali metal or alkaline earth metal halides. If these are contained in an amount that enhances the antistatic properties, they will migrate to and precipitate on the surface of the obtained artificial hair fiber, making the appearance of the artificial hair more likely to be poor.

[0104] (Thermoplastic polyester) The artificial hair fiber of the present invention preferably contains a thermoplastic polyamide and a thermoplastic polyester that is incompatible with the thermoplastic polyamide and has a higher melting point. Here, incompatibility means that the two resins do not melt to form a homogeneous resin. This allows the artificial hair fiber to be molded into one that has a luster with a subdued luster similar to natural hair. Specific examples of thermoplastic polyesters include polyethylene terephthalate and polybutylene terephthalate.

[0105] That is, in one preferred embodiment, the artificial hair fiber of the present invention comprises a thermoplastic polyamide forming a matrix, a thermoplastic polyester forming domains, and the above-mentioned polymeric antistatic agent, and has an uneven surface, with the convex portions of the uneven surface being formed by the thermoplastic polyamide. The polyester domains do not precipitate on the fiber surface. The weight ratio of the thermoplastic polyamide to the thermoplastic polyester in the artificial hair fiber may be, for example, such that the thermoplastic polyamide accounts for more than half or all of the weight, preferably in the range of 70 / 30 to 95 / 5, and more preferably 75 / 25 to 85 / 15.

[0106] <Method for producing artificial hair fiber> The artificial hair fiber of the present invention can be produced in the same manner as conventional artificial hair fibers, except that the above-mentioned polymeric antistatic agent is incorporated into the thermoplastic polyamide. The artificial hair fiber of the present invention can be produced, for example, in accordance with the method described in Patent Document 1. The disclosure of Patent Document 1 is incorporated herein by reference.

[0107] Specifically, the artificial hair fiber of the present invention can be produced by melt-mixing a thermoplastic polyamide and a polymeric antistatic agent at a melting temperature equal to or higher than their melting points, extruding the melt-mixed resin at a discharge temperature equal to or lower than the melting temperature, and molding it into a fibrous form.

[0108] In a preferred embodiment, the artificial hair fiber of the present invention can be produced by melt-mixing a thermoplastic polyamide, a polyester that is incompatible with the thermoplastic polyamide and has a higher melting point, and a polymeric antistatic agent at a melting temperature equal to or higher than the melting points of these three components, and then extruding the melt-mixed resin at a discharge temperature equal to or lower than the melting temperature to form fibers.

[0109] A typical spinning apparatus using a single-screw extruder used in the production of the synthetic fibers used in the present invention is shown in Figure 1. This apparatus consists of a hopper 1 into which resin is charged, a cylinder 2 that heats the charged resin, a screw 3 that melts and kneads the resin and sends it to a discharge section, and a gear pump 4 that sends the melt-mixed resin to a die section 5. The melt-mixed resin is discharged from the die section 5 in the form of a thread and spun. The number of screws can be single-screw or multi-screw, and can be selected appropriately depending on the properties of the resin, the thickness of the fiber to be formed, etc.

[0110] The spinning apparatus used to produce the synthetic fibers of the present invention generally uses a single-screw or twin-screw extruder as shown in Figure 1 or Figure 2, in which the melt-mixed resin is delivered to the nozzle. The gear pump 4 used in the single-screw extruder shown in Figure 1 is not used in the twin-screw extruder of Figure 2. However, even if the gear pump is removed as shown in Figure 2, the formation of convex bodies on the surface of the artificial hair made of the matrix resin is not affected. The system shown in Figure 2, which does not have a pressure-boosting function, is preferably used because it shortens the residence time of the melt-mixed resin in the spinning apparatus and reduces thermal degradation of the resin.

[0111] The resins mixed in a predetermined weight ratio within the above range are melted at a predetermined temperature (referred to as the melting temperature T1) equal to or higher than the melting point of the thermoplastic polyester. When mixing these, a pigment and / or a dye may be added to color the mixture. Furthermore, a stabilizer, an antioxidant, and / or an ultraviolet absorber may be added. These may be added directly to the spinning apparatus or as a masterbatch in which they are premixed with the polyamide resin or polyester resin.

[0112] Thermoplastic resin supplied from a hopper 1 is melted and delivered from a cylinder 2 to a die section 5 by a single-screw or twin-screw screw 3. The temperature of the melted and mixed resin is preferably the same as or higher than the melting set temperature T1, but may be lower than the melting set temperature T1 as long as the melted resin does not solidify.

[0113] 3 shows a schematic diagram of the die 5. In the figure, reference numeral 25 denotes a resin discharge hole, reference numeral 26 denotes resin discharged from the discharge hole 25, reference numeral 27 denotes a temperature sensor inserted into and located near the discharge port of the die 5, and T2 is the temperature of the molten resin R before discharge measured by the temperature sensor. The temperature of the molten resin before discharge is T2, and the resin discharge temperature of the die 5, i.e., the die set temperature, is T3.

[0114] When the mixed resin is kneaded by the screw in the spinning apparatus, heat is generally generated and the molten resin temperature T2 becomes higher than the set melting temperature T1, but if the molten resin temperature T2 before discharge becomes too higher than the set melting temperature T1, this is not preferable because the first thermoplastic resin will only form small convex portions or will not form at all on the surface of the resin discharged from the spinneret 5. Conversely, if the molten resin temperature T2 before discharge is too lower than the set melting temperature T1, the viscosity of the mixed resin will increase and it will not flow, which may make it impossible to discharge, which is not preferable.

[0115] The die set temperature T3 should be set to a temperature lower than the molten resin temperature T2 near the discharge port, and is preferably set to a temperature about 20 to 30°C lower than the melt set temperature T1. If the temperature is higher than this range, it will be difficult to form irregularities on the surface of the discharged resin, and conversely, if it is lower, the resin will tend to harden, which is not preferable.

[0116] More preferably, the die set temperature T3 is set to a value equal to or lower than the melting point of the thermoplastic polyester. This die set temperature T3 is preferably set to a value lower than the melting point of the thermoplastic polyester by a range of 5°C to 30°C below the melting point of the thermoplastic polyester. Even more preferably, the die set temperature T3 is set to a value lower than the melting point of the thermoplastic polyester by a range of 10°C to 30°C below the melting point of the thermoplastic polyester. If the temperature is higher than this range, it is difficult to form irregularities on the surface of the extruded resin, and conversely, if the temperature is lower than this range, the resin is likely to solidify, which is not preferable.

[0117] Furthermore, the spinneret used does not need to have a special structure, and a spinneret of known structure can be used to obtain the synthetic fibers used in the present invention.

[0118] Figure 4 shows an outline of the process from spinning to fiber winding according to the present invention. The fibrous extruded resin 6 extruded from the spinneret 5 via the gear pump 4 of the spinning device under the above temperature conditions is air-cooled (areas A, B, and C in the figure), water-cooled in a cooling water tank 7, and then wound up by a winder 9. Although Figure 4 shows the water-cooling process, the extruded resin 6 may be cooled and wound up by air-cooling only. Also, the spinning device may not use the gear pump shown in Figure 2.

[0119] The molten resin discharged from the discharge hole 25 of the spinning device has fluidity and can be stretched by applying tension. However, as the discharged resin cools, it solidifies and its fluidity decreases, and it can no longer be stretched unless it is heated. The state in which the resin discharged from the discharge hole 25 can be stretched by the tension generated at the set winding speed is defined as the extensional flow range. The extensional flow range is not constant, but varies depending on the resin used, the set temperature of the spinneret, the temperature of the location where the spinning device is installed, and the winding speed.

[0120] When the spinneret temperature T3 is set lower than the melting temperature T1, domains do not precipitate on the fiber surface, and the fiber surface is covered with the resin component of the matrix, or small protrusions formed by the matrix component are formed. In particular, when the spinneret temperature T3 is set lower than the melting point of the domain component, many small protrusions covered with the matrix are formed.

[0121] The wound synthetic fiber is drawn through the drawing rollers and dry heat bath of a drawing device to a predetermined diameter, such as 80 μm. Alternatively, the spinning device and drawing device may be connected to perform the spinning and drawing steps continuously.

[0122] <Uses for wigs, etc.> A large number of stretched artificial hair fibers can be implanted into a wig base to produce a wig. The wig base may be a net base, an artificial skin base, or a combination of these. The stretched artificial hair fibers can also be used for hair extensions or substitute hair.

[0123] The present invention will be explained in more detail with reference to the following examples, but the present invention is not limited to these examples.

[0124] As a polymeric antistatic agent, the following polyether ester amide block copolymer was prepared.

[0125]

[0126]

[0127] Example 1: As a thermoplastic polyamide (hereinafter referred to as "PA"), Daicel-Evonik's "Vestamid D-18" (trade name, melting point 200-225°C, MFR 25.8g (240°C, 21.18N)) and Toyobo's "Vylopet BR-3067" (trade name, melting point 255°C) were prepared as a thermoplastic polyester (hereinafter referred to as "PE") in amounts such that the PA / PE ratio was 85 / 15. Antistatic agent A (hereinafter referred to as "agent A") was prepared in an amount that would give 1% by weight based on the resin component, and a colorant was prepared in an amount that would give 0.49% by weight.

[0128] Artificial hair fibers were produced using the prepared raw materials, the spinning device shown in Figure 4, and the drawing device (not shown). In the following production conditions, T1 is the melt setting temperature, T2 is the molten resin temperature near the spinneret, and T3 is the spinneret setting temperature.

[0129] (Production conditions) T1 / T2 / T3 (°C): 280 / 248 / 248 Spinning output (kg / h): 0.4 Cooling water temperature (°C): 5 Spinning take-up speed (m / min): 120 Room temperature of experiment (°C): 26 Stretching ratio (times): 4.4 Stretching temperature (°C, air): 90, 190

[0130] A hair bundle was made by bundling 2 g of artificial hair fiber, and the resulting hair strand was immersed in a silicone aqueous solution (silicone agent:water / 1:60) and spread on a similarly immersed nonwoven fabric. The hair strand was then wrapped around a 35 mm aluminum pipe and covered with aluminum foil. The hair strand was then heat-treated at 180°C for 2 hours to create a curl. The curled hair strand was left on a flat surface to form a circle. The diameter (mm) of the inner circumference of the circle formed by the hair strand was measured. This value was taken as the curl dimension. The measurement results are shown in Table 3.

[0131] Examples 2 to 90 Artificial hair fibers were produced in the same manner as in Example 1, except for changing the PA / PE ratio, the type and amount of antistatic agent, and T2 and T3. Magnified images of the artificial hair fiber of Example 16 are shown in Figures 5 and 6. Figure 5 is an 800x magnified image showing the surface of the artificial hair fiber. Figure 6 is a 1,000x magnified image showing the cross section of the artificial hair fiber. From Figure 5, it can be seen that irregularly protruding convex bodies form irregularities on the surface of the artificial hair fiber. From Figure 6, it can be seen that the morphology of the artificial hair fiber forms a sea-island structure in which polyester island portions are dispersed almost uniformly within a polyamide sea portion.

[0132] In the same manner as in Example 1, hair bundles were prepared from the artificial hair fibers produced, curled, and the curl diameter (mm) was measured. The results are shown in Tables 3 to 14.

[0133]

[0134]

[0135]

[0136]

[0137]

[0138]

[0139]

[0140]

[0141]

[0142]

[0143]

[0144]

[0145] <Comparative Examples 1 to 6> Artificial hair fibers of Comparative Examples 1 to 6 were produced in the same manner as in Examples 1, 3, 5, 7, 9, and 11, respectively, except that no antistatic agent was used, and the fibers were curled and the curl diameter (mm) was measured. The results are shown in Table 15.

[0146]

[0147] Regarding the artificial hair fibers produced, the artificial hair fibers of Comparative Examples, which did not contain an antistatic agent, tended to have a larger curl diameter and inferior curling performance when compared with the artificial hair fibers of Examples, which were produced under the same conditions except for the antistatic agent. Furthermore, when the production conditions were changed, the following trends were observed in the curling performance of the produced artificial hair fibers.

[0148]

[0149] Furthermore, by observing the manufactured artificial hair fibers, the following findings were made. That is, when agent A was used, the color tone was whiter than when agent B was used. When the PA / PE ratio was 85 / 15, the gloss was emphasized. When the PA / PE ratio was 75 / 25, the hair texture was rough. When T2 and T3 were set to 250°C, the gloss was emphasized more than when they were set to 248°C.

[0150] Example 91: Artificial hair fibers were produced in the same manner as in Example 4 (PA / PE ratio 81 / 19, agent B 1%, T2,3 (°C) 248) except for changing the amount of antistatic agent used, and hair bundles were prepared and curled. The curled hair bundles were brushed 10 times using a Denman-type metal comb brush. The static electricity meter "FMX-004" (product name) manufactured by Simco Japan was used to measure the amount of static electricity charged to the hair bundles and the curl diameter (mm) of the hair bundles.

[0151] The entire hair bundle was washed by applying shampoo "AD&F PRO STYLING" (trade name) manufactured by Aderans Co., Ltd., and then rinsing with water, and then dried by blowing air at approximately 60° C. The dried hair bundle was brushed 10 times, and the amount of static electricity charged to the hair bundle and the curl diameter (mm) of the hair bundle were measured (washing count 1).

[0152] The hair bundle was washed and dried four more times, and brushed 10 times, and the amount of static electricity charged to the hair bundle and the curl diameter (mm) of the hair bundle were measured (washing count 5). The hair bundle was washed and dried five more times, and brushed 10 times, and the amount of static electricity charged to the hair bundle and the curl diameter (mm) of the hair bundle were measured (washing count 10). The results are shown in Tables 17 to 20.

[0153]

[0154]

[0155]

[0156]

[0157] The artificial hair fiber containing no antistatic agent showed a large increase in curl diameter after the first wash and was poor in curl retention performance after repeated washing.

[0158] Examples 92 to 94 Artificial hair fibers were produced in the same manner as in Example 1, except that the PA / PE ratio, the type and amount of antistatic agent, and T2 and T3 were changed. Hair bundles were prepared from the artificial hair fibers produced in the same manner as in Example 1, and curled, and the curl diameter (mm) was measured. The results are shown in Table 21.

[0159]

[0160] Examples 98 to 103 Artificial hair fibers were produced in the same manner as in Example 1, except that only PA was used as the resin component instead of PA and PE, and the type and amount of antistatic agent used, as well as T2 and T3, were changed. Hair bundles were prepared from the artificial hair fibers produced in the same manner as in Example 1, and curled, and the curl diameter (mm) was measured. The results are shown in Table 22.

[0161]

[0162] <Comparative Examples 7 and 8> Artificial hair fibers of Comparative Examples 7 and 8 were produced in the same manner as in Examples 98 and 101, respectively, except that no antistatic agent was used, and the fibers were curled and the curl diameter (mm) was measured. The results are shown in Table 23.

[0163]

[0164] Example 104 The curled hair bundles obtained in Examples 92 to 94, 98 to 100, and Comparative Example 7 were brushed 10 times using a Denman-type metal comb brush. The static electricity meter "FMX-004" (product name) manufactured by Simco Japan was used to measure the amount of static electricity charged to the hair bundle and the curl diameter (mm) of the hair bundle.

[0165] The entire hair bundle was washed by applying shampoo "AD&F PRO STYLING" (trade name) manufactured by Aderans Co., Ltd., and then rinsing with water, and then dried by blowing air at approximately 60° C. The dried hair bundle was brushed 10 times, and the amount of static electricity charged to the hair bundle and the curl diameter (mm) of the hair bundle were measured (washing count 1).

[0166] The hair bundle was washed and dried four more times, and brushed 10 times, and the amount of static electricity charged to the hair bundle and the curl diameter (mm) of the hair bundle were measured (washing count 5). The hair bundle was washed and dried five more times, and brushed 10 times, and the amount of static electricity charged to the hair bundle and the curl diameter (mm) of the hair bundle were measured (washing count 10). The results are shown in Tables 24 and 25. In Tables 24 and 25, the numbers shown after PA and PE indicate the weight ratio of each component when the weight of the artificial hair fiber is taken as 100.

[0167]

[0168]

[0169] 1: Hopper 2: Cylinder 3: Screw 4: Gear pump 5: Die 6: Discharged resin 7: Cooling water tank 8: Guide roll 9: Winder 25: Resin discharge hole 26: Discharged resin 27: Temperature sensor

Claims

1. An artificial hair fiber comprising a thermoplastic polyamide and a polymeric antistatic agent that is compatible with the thermoplastic polyamide, wherein the polymeric antistatic agent has a melting point equal to or lower than the melting point of the thermoplastic polyamide.

2. The artificial hair fiber according to claim 1, wherein the polymeric antistatic agent has a melting point of 160 to 250°C.

3. The artificial hair fiber according to claim 1 or 2, wherein the polymeric antistatic agent has a melt flow rate at 215°C of 10 to 40 g / 10 min.

4. The polymer type antistatic agent is 10 6 ~10 10 The fiber for artificial hair according to any one of claims 1 to 3, having a surface resistivity of Ω / □.

5. The artificial hair fiber according to any one of claims 1 to 4, wherein the polymeric antistatic agent comprises a polyether ester amide block copolymer.

6. The artificial hair fiber according to any one of claims 1 to 5, wherein the polyetheresteramide block copolymer is a condensation product of a polyamide having carboxyl groups at both ends and an aromatic ring-containing polyetherdiol.

7. The artificial hair fiber according to any one of claims 1 to 6, wherein the polymeric antistatic agent is contained in an amount of 0.5 to 10% by weight.

8. The artificial hair fiber according to any one of claims 1 to 7, further comprising a thermoplastic polyester which is incompatible with the thermoplastic polyamide and has a higher melting point.

9. The artificial hair fiber according to claim 8, which has a weight ratio of thermoplastic polyamide to thermoplastic polyester of 75 / 25 to 85 / 15.

10. The artificial hair fiber according to claim 8 or 9, which has an uneven surface formed thereon, and the protrusions of said uneven surface contain particles of thermoplastic polyester.

11. The artificial hair fiber according to any one of claims 8 to 10, which has a matrix comprising a thermoplastic polyamide and a domain comprising a thermoplastic polyester.

12. The artificial hair fiber according to any one of claims 1 to 11, wherein the thermoplastic polyamide is at least one thermoplastic resin selected from the group consisting of linear saturated aliphatic polyamides, alternating copolymers of hexamethylenediamine and terephthalic acid, and alternating copolymers of metaxylenediamine and adipic acid.

13. The artificial hair fiber according to any one of claims 8 to 12, wherein the thermoplastic polyester is at least one thermoplastic resin selected from the group consisting of polyethylene terephthalate and polybutylene terephthalate.

14. A wig comprising a wig base and the artificial hair fiber according to any one of claims 1 to 13, which is tacked onto the wig base.