Ideal oxygen precipitating silicon wafers and oxygen out-diffusion-less process therefor

MYPI1998000816A0Inactive Publication Date: 1998-08-26SUNEDISON INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI1998000816
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
1997-02-26
Filing Date
1998-02-25
Publication Date
1998-08-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for heat-treating single crystal silicon wafers do not effectively control the precipitation behavior of oxygen, which can lead to defects and variations in thermal processing.

Method used

A heat-treatment process that forms crystal lattice vacancies in the bulk of the silicon wafer and controls their diffusion to create a vacancy concentration profile with a peak at the central plane, decreasing towards the front surface, influencing oxygen precipitation.

Benefits of technology

This process enhances the uniformity and quality of subsequent thermal processing by managing oxygen precipitation, reducing defects and variations in the wafer.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A PROCESS FOR HEAT-TREATING A SINGLE CRYSTAL SILICON WAFER TO INFLUENCE THE RECIPITATION BEHAVIOUR OF OXYGEN IN THE WAFER IN A SUBSEQUENT THERMAL PROCESSING STEP.THE WAFER HAS A FRONT SURFACE (3), A BACK SURFACE (5), AND A CENTRAL PLANE (7) BETWEEN THE FRONT AND BACK SURFACES.IN THE PROCESS, THE WAFER (1) IS SUBJECTED TO A HEAT-TREATMENT TO FORM CRYSTAL LATTICE VACANCIES (13), THE VACANCIES BEING FORMED IN THE BULK (11) OF THE SILICON.THE WAFER (1) IS THEN COOLED FROM THE TEMPERATURE OF SAID HEAT TREATMENT AT A RATE WHICH ALLOWS SOME, BUT NOT ALL, OF THE CRYSTAL LATTICE VACANCIES TO DIFFUSE TO THE FRONT SURFACE (3) TO PRODUCE A WAFER HAVING A VACANCY CONCENTRATION PROFILE IN WHICH THE PEAK DENSITY IS AT OR NEAR THE CENTRAL PLANE (7) WITH THE CONCENTRATION GENERALLY DECREASING IN THE DIRECTION OF THE FRONT SURFACE (3) OF THE WAFER.(FIG 1)
Need to check novelty before this filing date? Find Prior Art

Description

A process for heat-treating a single crystal silicon wafer to influence the precipitation behaviour of oxygen in the wafer in a subsequent thermal processing step. The wafer has a front surface (3), a back surface (5), and a central plane (7) between the front and back surfaces. In the process, the wafer (1) is subjected to a heat-treatment to form crystal lattice vacancies (13), the vacancies being formed in the bulk (11) of the silicon. The wafer (1) is then cooled from the temperature of said heat treatment at a rate which allows some, but not all, of the crystal lattice vacancies to diffuse to the front surface (3) to produce a wafer having a vacancy concentration profile in which the peak density is at or near the central plane (7) with the concentration generally decreasing in the direction of the front surface (3) of the wafer.

Claims

1. A wafer sliced from a single crystal silicon ingot grown by the Czochralski method comprising 5 a front surface (3), a back surface (5), a central plane (7) between the front and back surfaces (3, 5), a front surface layer which comprises a first region of the wafer between the front surface (3) and a distance, Di, measured from the front surface (3) and toward the central plane (7), and a bulk layer (11) which comprises a second region of the wafer between the central plane (7) and the first region; and io a non-uniform distribution of crystal lattice vacancies (13) with the concentration of vacancies in the bulk layer (11) being greater than the concentration of vacancies in the front surface layer with the vacancies having a concentration profile in which the peak density of the vacancies is at or near the central plane (7) 15 with the concentration generally decreasing in the direction of the front surface (3) of the wafer.

2. The wafer of claim 1 wherein Di is at least about 20 micrometers.

3. The wafer of claim 1 wherein Di is at least about 30 micrometers.

4. The wafer of claim 1 wherein Di is at least about 50 micrometers.

5. The wafer of claim 1 wherein Di is at least about 70 micrometers.

6. The wafer of claim 1 wherein D! is between about 30 and about 100 micrometers.

7. The wafer of claim 1 having a carbon concentration which is less than 5 about 5x1016 atoms / cm3.

8. The wafer of claim 1 having a carbon concentration which is less than about 1x1016 atoms / cm3.10 9. The wafer of claim 1 having a carbon concentration which is less than about 5x1015 atoms / cm3.

10. The wafer of claim 1 having an epitaxial layer deposited upon the front surface (3). The wafer of claim 1 wherein the front surface (3) is polished.

12. The wafer of claim 1 wherein the wafer has an absence of oxygen precipitate nucleation centers which are incapable of being dissolved by heat-treating 20 the wafer at a temperature not in excess of 1300 °C.

13. The wafer of claim 12 having a carbon concentration which is less than about 5x1015 atoms / cm3. 1414. The wafer of claim 13 wherein the wafer comprise I15. The wafer of claim 12 wherein the wafer comprises an epitaxial layer.

16. The wafer of claim 12 wherein Di is at least about 20 micrometers.

17. The wafer of claim 16 having a carbon concentration which is less than about 5x1015 atoms / cm3.

18. The wafer of claim 17 wherein the wafer comprises an epitaxial layer.

19. The wafer of claim 16 wherein the wafer comprises an epitaxial layer.

20. The wafer of claim 12 wherein Di is at least about 30 micrometers.

21. The wafer of claim 20 having a carbon concentration which is less than about 5x101S atoms / cm3.

22. The wafer of claim 12 wherein Di is at least about 50 micrometers.

23. The wafer of claim 22 having a carbon concentration which is less than about 5x1015 atoms / cm3.

24. The wafer of claim 12 wherein Di is between about 30 and about 100 micrometers. than about 5x1015 atoms / cm3.25 25. The wafer of claim 24 having a carbon concentration which is less26. A wafer having a front surface (3), a back surface (5), and a central plane (7) between the front and back surfaces (3, 5), the wafer having a front surface layer consisting of the region of the wafer within a distance, D2, of the front surface (3) wherein D2 is no more than about 15 micrometers and a bulk layer (11) 5 comprising the region of the wafer between the central plane (7) and the front surface layer, the wafer having a substantially uniform oxygen concentration and a concentration of crystal lattice vacancies (13) in the bulk layer (11) such that upon being subjected to an oxygen precipitation heat treatment consisting essentially of annealing the wafers at 800 °C for four hours and then at 1000 °C for sixteen hours, 10 the wafer will contain oxygen precipitates having a concentration profile in which the peak density of the precipitates in the bulk layer (11) is at or near the central plane (7) with the concentration of the precipitates in the bulk layer (11) generally decreasing in the direction of the front surface layer. 1527. The wafer of claim 26 wherein D2 is no more than about 10 micrometers.

28. The wafer of claim 26 wherein D2 is no more than about 5 micrometers.

29. The wafer of claim 26 wherein D2 is no more than 3 micrometers.

30. The wafer of claim 26 having a carbon concentration which is less than about 5x1015 atoms / cm3.

31. The wafer of claim 26 having an epitaxial layer deposited upon the front surface (3).

32. The wafer of claim 26 wherein the front surface (3) is polished.

33. The wafer of claim 26 wherein the wafer has an absence of oxygen precipitate nucleation centers which are incapable of being dissolved by heat-treating the wafer at a temperature not in excess of 1300 °C. io34. The wafer of claim 33 having a carbon concentration which is less than about 5x1015 atoms / cm3.

35. The wafer of claim 34 having an epitaxial layer deposited upon the front surface (3).

36. The wafer of claim 33 having an epitaxial layer deposited upon the front surface (3).

37. A wafer having a front surface (3), a back surface (5), and a central 20 plane (7) between the front and back surfaces (3, 5), the wafer having a front surface layer consisting of the region of the wafer within a distance, D2) of no more than about 15 micrometers, a bulk layer (11) comprising the region of the wafer between the central plane (7) and the front surface layer, and a denuded zone (15, 15’) which comprises the front surface layer and a portion of the bulk layer (11), the wafer being 25 characterized in that it has a substantially uniform oxygen concentration in the bulk layer (11), oxygen precipitates in the portion of the bulk layer (11) which is outside the denuded zone (15, 15’), and a substantial absence of oxygen precipitates in the denuded zone (15, 15’).

38. The wafer of claim 37 wherein D2 is no more than about 10 5 micrometers.

39. The wafer of claim 37 wherein D2 is no more than about 5 micrometers. io40. The wafer of claim 37 wherein D2 is no more than 3 micrometers.

41. The wafer of claim 37 wherein the denuded zone (15, 15’) extends to a distance of at least about 20 micrometers from the front surface (3).

42. The wafer of claim 41 wherein D2 is no more than about 10 micrometers.

43. The wafer of claim 41 wherein D2 is no more than about 5 micrometers.

44. The wafer of claim 41 wherein D2 is no more than 3 micrometers.

45. The wafer of claim 37 wherein the denuded zone (15, 15’) extends to a distance of at least about 30 micrometers of the front surface (3).

46. The wafer of claim 45 wherein D2 is no more than about 10 micrometers.

47. The wafer of claim 45 wherein D2 is no more than about 5 5 micrometers.

48. The wafer of claim 45 wherein D2 is no more than 3 micrometers.

49. The wafer of claim 37 wherein the denuded zone (15, 15’) extends to 10 a distance of at least about 50 micrometers of the front surface (3).

50. The wafer of claim 49 wherein D2 is no more than about 10 micrometers.

51. The wafer of claim 49 wherein D2 is no more than about 5 micrometers.

52. The wafer of claim 49 wherein D2 is no more than 3 micrometers.

53. The wafer of claim 37 wherein the denuded zone (15, 15’) extends to a distance of at least about 70 micrometers of the front surface (3).

54. The wafer of claim 53 wherein D2 is no more than about 10 micrometers.

55. The wafer of claim 53 wherein D2 is no more than about 5 micrometers.

56. The wafer of claim 53 wherein D2 is no more than 3 micrometers.

57. The wafer of claim 37 wherein the denuded zone (15, 15') extends to a distance of at least about 100 micrometers of the front surface (3).

58. The wafer of claim 57 wherein D2 is no more than about 10 10 micrometers.

59. The wafer of claim 57 wherein D2 is no more than about 5 micrometers.

60. The wafer of claim 57 wherein D2 is no more than 3 micrometers.

61. The wafer of claim 37 having a carbon concentration which is less than about 5x1015 atoms / cm3. 2062. The wafer of claim 37 having an epitaxial layer deposited upon the front surface (3).

63. The wafer of claim 37 wherein the front surface (3) is polished.

64. The wafer of claim 37 wherein the wafer has an absence of oxygen precipitate nucleation centers which are incapable of being dissolved by heat-treating the wafer at a temperature not in excess of 1300 °C.

565. The wafer of claim 64 having a carbon concentration which is less than about 5x1015 atoms / cm3.

66. The wafer of claim 65 having an epitaxial layer deposited upon the front surface (3). io67. The wafer of claim 64 having an epitaxial layer deposited upon the front surface (3).

68. A single crystal silicon wafer having two major, generally parallel 15 surfaces, one of which is the front surface (3) of the wafer and the other of which is the back surface (5) of the wafer, a central plane (7) between the front and back surfaces (3, 5), a circumferential edge joining the front and back surfaces (3, 5), a surface layer which comprises a first region of the wafer between the front surface (3) and a distance, Di, of at least about 10 micrometers as measured from the front 20 surface (3) and toward the central plane (7), and a bulk layer (11) which comprises a second region of the wafer between the central plane (7) and the first region, the wafer being characterized in that the wafer has a non-uniform distribution of crystal lattice vacancies (13) with 25 the concentration of vacancies in the bulk layer (11) being greater than the concentration of vacancies in the surface layer with the vacancies having a concentration profile in which the peak density of the vacancies is at or near the central plane (7) with the concentration generally decreasing from the position of peak density in the direction of the front surface (3) of the wafer, and the wafer contains interstitial oxygen with the concentration of interstitial oxygen being substantially uniform between the center of the wafer and regions of the wafer which are within about 15 micrometers of the front surface (3).

69. The wafer of claim 68 wherein Di is at least about 20 micrometers.

70. The wafer of claim 68 wherein Di is at least about 50 micrometers.

71. The wafer of claim 68 wherein D! is between about 30 and about 100 micrometers.

72. The wafer of claim 68 wherein the concentration of interstitial oxygen at distances greater than 10 microns from the wafer surface is at least about 80% of the concentration of interstitial oxygen in the bulk layer (11).

73. The wafer of claim 72 wherein Di is at least about 20 micrometers.

74. The wafer of claim 68 wherein Di is at least about 50 micrometers.

75. The wafer of claim 72 wherein Dt is between about 30 and about 100 micrometers76. The wafer of claim 68 wherein the concentration of interstitial oxygen at distances greater than 15 microns from the wafer surface is at least about 90% of the concentration of interstitial oxygen in the bulk layer (11).

577. The wafer as set forth in claim 68 wherein the wafer further comprises an epitaxial layer on the wafer surface.

78. The wafer of claim 68 having a carbon concentration which is less than about 5x1016 atoms / cm3. io79. The wafer of claim 68 having a carbon concentration which is less than about 1x1016 atoms / cm3.

80. The wafer of claim 68 having a carbon concentration which is less 15 than about 5x1015 atoms / cm3.

81. The wafer of claim 68 wherein the front surface (3) is polished.

82. The wafer of claim 68 wherein the wafer has an absence of oxygen 20 precipitate nucleation centers which are incapable of being dissolved by heat-treating the wafer at a temperature not in excess of 1300 °C.

83. The wafer of claim 68 wherein the wafer has a substantially uniform oxygen concentration between the center of the wafer and regions of the wafer which 25 are within about 10 micrometers of the front surface (3).

84. The wafer of claim 83 having a carbon concentration which is less than about 5x1016 atoms / cm3.

85. The wafer of claim 83 having a carbon concentration which is less 5 than about 1x1016 atoms / cm386. The wafer of claim 83 having a carbon concentration which is less than about 5x1015 atoms / cm3. io87. The wafer of claim 83 wherein the front surface (3) is polished.

88. The wafer of claim 83 wherein the wafer has an absence of oxygen precipitate nucleation centers which are incapable of being dissolved by heat-treating the wafer at a temperature not in excess of 1300 °C.

89. The wafer of claim 68 wherein the wafer has a substantially uniform oxygen concentration between the center of the wafer and regions of the wafer which are within about 10 micrometers of the front surface (3). 2090. The wafer of claim 89 having a carbon concentration which is less than about 5x1016 atoms / cm3.

91. The wafer of claim 89 having a carbon concentration which is less than about 1x1016 atoms / cm3.

92. The wafer of claim 89 having a carbon concentration which is less than about 5x1015 atoms / cm3.

93. The wafer of claim 89 wherein the front surface (3) is polished.

94. The wafer of claim 89 wherein the wafer has an absence of oxygen precipitate nucleation centers which are incapable of being dissolved by heat-treating the wafer at a temperature not in excess of 1300 °C. io95. The wafer of claim 68 wherein the wafer has a substantially uniform oxygen concentration between the center of the wafer and regions of the wafer which are within about 5 micrometers of the front surface (3).

96. The wafer of claim 95 having a carbon concentration which is less 15 than about 5x1016 atoms / cm3.

97. The wafer of claim 95 having a carbon concentration which is less than about 1x1016 atoms / cm3. 2098. The wafer of claim 95 having a carbon concentration which is less than about 5x1015 atoms / cm3.

99. The wafer of claim 95 wherein the front surface (3) is polished.

100. The wafer of claim 95 wherein the wafer has an absence of oxygen precipitate nucleation centers which are incapable of being dissolved by heat-treating the wafer at a temperature not in excess of 1300 °C. 5101. The wafer of claim 68 wherein the wafer has a substantially uniform oxygen concentration between the center of the wafer and regions of the wafer which are within about 3 micrometers of the front surface (3).

102. The wafer of claim 101 having a carbon concentration which is less 10 than about 5x1016 atoms / cm3.

103. The wafer of claim 101 having a carbon concentration which is less than about 1x1016 atoms / cm3. 15104. The wafer of claim 101 having a carbon concentration which is less than about 5x1015 atoms / cm3.

105. The wafer of claim 101 wherein the front surface (3) is polished. 20106. The wafer of claim 101 wherein the wafer has an absence of oxygen precipitate nucleation centers which are incapable of being dissolved by heat-treating the wafer at a temperature not in excess of 1300 °C.

107. The wafer of claim 76 wherein Dt is at least about 20 micrometers.

108. The wafer of claim 76 wherein Di is at least about 50 micrometers.

109. The wafer of claim 76 wherein Di is between about 30 and about 100 micrometers.

110. A single crystal silicon wafer having two major, generally parallel 5 surfaces, one of which is the front surface (3) of the wafer and the other of which is the back surface (5) of the wafer, a central plane (7) between the front and back surfaces (3, 5), a circumferential edge joining the front and back surfaces (3, 5), a denuded zone (15, 15’) which comprises a region of the wafer from the front surface (3) to a distance, D1t of at least about 10 micrometers as measured in the direction of io the central plane (7) and which contains interstitial oxygen, and a bulk layer (11) which comprises a second region of the wafer between the central plane (7) and the first region and which contains oxygen precipitates, the wafer being characterized in that 15 the concentration of interstitial oxygen in the denuded zone (15, 15’) at a distance equal to one-half of Di is at least about 75% of the maximum concentration of interstitial oxygen in the denuded zone (15, 15’).

111. The wafer of claim 110 wherein Di is at least 20 micrometers.

112. The wafer of claim 111 wherein the concentration of interstitial oxygen in the denuded zone (15, 15’) at a distance equal to one-half of Di is at least about 80% of the maximum concentration of interstitial oxygen in the denuded zone (15, 15’).

113. The wafer of claim 110 wherein the concentration of interstitial oxygen in the denuded zone (15, 15’) at a distance equal to one-half of Di is at least about 90% of the maximum concentration of interstitial oxygen in the denuded zone (15, 15’).

114. The wafer of claim 110 wherein Di is at least 50 micrometers.

115. The wafer of claim 114 wherein the concentration of interstitial oxygen in the denuded zone (15, 15’) at a distance equal to one-half of Di is at least about 10 85% of the maximum concentration of interstitial oxygen in the denuded zone (15, 15’)·116. The wafer of claim 114 wherein the concentration of interstitial oxygen in the denuded zone (15, 15’) at a distance equal to one-half of D3 is at least about 15 95% of the maximum concentration of interstitial oxygen in the denuded zone (15, 15’).

117. The wafer of claim 110 wherein Dt is between 30 and 100 micrometers.

118. The wafer of claim 117 wherein the concentration of interstitial oxygen in the denuded zone (15, 15’) at a distance equal to one-half of Di is at least about 85% of the maximum concentration of interstitial oxygen in the denuded zone (15, 15').

119. The wafer of claim 110 wherein the wafer further comprises an epitaxial layer on the wafer surface.

120. The wafer of claim 110 having a carbon concentration which is less 5 than about 5x1016 atoms / cm3121. The wafer of claim 110 having a carbon concentration which is less than about 1x1016 atoms / cm3. io122. The wafer of claim 110 having a carbon concentration which is less than about 5x1015 atoms / cm3.

123. The wafer of claim 110 wherein the front surface (3) is polished. 15124. The wafer of claim 110 wherein the wafer has an absence of oxygen precipitate nucleation centers which are incapable of being dissolved by heat-treating the wafer at a temperature not in excess of 1300 °C.

125. A process for heat-treating a single crystal silicon wafer sliced from a 20 single crystal silicon ingot grown by the Czochralski method to influence the precipitation behavior of oxygen in the wafer in a subsequent thermal processing step, the silicon wafer having a front surface (3), a back surface (5), a central plane (7) between the front and back surfaces (3, 5), a front surface layer which comprises the region of the wafer between the front surface (3) and a distance, D, measured 25 from the front surface (3) and toward the central plane (7), and a bulk layer (11) which comprises the region of the wafer between the central plane (7) and front surface layer, the process comprising the steps of: subjecting the wafer to a heat-treatment to form crystal lattice vacancies (13) 5 in the front surface (3) and bulk layers (11), and controlling the cooling rate of the heat-treated wafer to produce a wafer having a vacancy concentration profile in which the peak density is at or near the central plane (7) with the concentration generally decreasing in the direction of the io front surface (3) of the wafer and the difference in the concentration of vacancies in the front surface (3) and bulk layers (11) being such that a thermal treatment at a temperature in excess of 750 °C, is capable of forming in the wafer a denuded zone (15, 15’) in the front surface layer and oxygen clusters or precipitates in the bulk zone with the concentration of the oxygen clusters or precipitates in the bulk layer 15 (11) being primarily dependant upon the concentration of vacancies.

126. The process of claim 125 wherein said heat-treatment to form crystal lattice vacancies (13) comprises heating the wafers to a temperature in excess of about 1175 °C in a non-oxidizing atmosphere.

127. The process of claim 125 wherein said heat-treatment to form crystal lattice vacancies ¢13) comprises heating the wafers to a temperature in excess of about 1200 °C in a non-oxidizing atmosphere.

128. The process of claim 125 wherein said heat-treatment to form crystal lattice vacancies (13) comprises heating the wafers to a temperature in the range of about 1200 °C to about 1275 °C in a non-oxidizing atmosphere. 5129. The process of claim 125 wherein said cooling rate is at least about 20 °C per second through the temperature range at which crystal lattice vacancies (13) are relatively mobile in silicon.

130. The process of claim 125 wherein said cooling rate is at least about 10 50 °C per second through the temperature range at which crystal lattice vacancies (13) are relatively mobile in silicon.

131. The process of claim 125 wherein said cooling rate is at least about 100 °C per second through the temperature range at which crystal lattice vacancies 15 (13) are relatively mobile in silicon.

132. The process of claim 125 wherein said cooling rate is at least about 5 °C per second through the temperature range at which crystal lattice vacancies (13) are relatively mobile in silicon.

133. The process of claim 125 wherein said cooling rate is about 100 °C per sec to about 200 °C per second through the temperature range at which crystal lattice vacancies (13) are relatively mobile in silicon.

134. The process of claim 133 wherein said heat treatment is performed in an atmosphere selected from a group consisting of argon, helium, neon, and carbon dioxide. 5135. The process of claim 133 wherein said heat treatment is performed in an atmosphere having a partial pressure of oxygen of less than about 0.1 atmosphere.

136. The process of claim 133 wherein said heat treatment is performed in io an atmosphere having a partial pressure of oxygen of less than about 0.05 atmosphere.

137. The process of claim 133 wherein said heat treatment is performed in an atmosphere having a partial pressure of oxygen of less than about 0.001 15 atmosphere.

138. The process of claim 133 wherein an epitaxial layer is deposited on said wafer in an epitaxial reactor prior to said heat treatment 20139. The process of claim 138 wherein the heat treatment is performed in the epitaxial reactor after the epitaxial deposition.

140. The process of claim 125 wherein an epitaxial layer is deposited on said wafer in an epitaxial reactor prior to said heat treatment.

141. The process of claim 140 wherein the heat treatment is performed in the epitaxial reactor after the epitaxial deposition.

142. The process of claim 125 wherein said heat treatment is performed in 5 an atmosphere selected from a group consisting of argon, helium, neon, and carbon dioxide.

143. The process of claim 125 wherein said heat treatment is performed in an atmosphere having a partial pressure of oxygen of less than about 0.1 io atmosphere.

144. The process of claim 125 wherein said heat treatment is performed in an atmosphere having a partial pressure of oxygen of less than about 0.05 atmosphere.

145. The process of claim 125 wherein said heat treatment is performed in an atmosphere having a partial pressure of oxygen of less than about 0.001 atmosphere. 201 46. A process for heat-treating single crystal silicon to influence the precipitation behavior of oxygen in the silicon, the process comprising the steps of: (a) subjecting the silicon to a first heat-treatment at a temperature of at least about 700 °C in an oxygen containing atmosphere to form a superficial silicon 25 dioxide layer which is capable of serving as a sink for crystal lattice vacancies (13), (b) subjecting the product of step (a) to a second heat-treatment at a temperature of at least about 1150 °C in an atmosphere having an essential absence of oxygen to form crystal lattice vacancies (13) in the bulk of the silicon, and 5 (c) cooling the silicon from the temperature of said second heat treatment to a temperature, ΤΊι of about 800 °C at a rate which allows some, but not all, of the crystal lattice vacancies (13) to diffuse to the sink to produce a wafer having a vacancy concentration profile in which the peak density is at or near the central plane (7) with the concentration generally decreasing in the direction of the front surface (3) io of the wafer.

147. The process of claim 146 wherein the cooling rate is at least about 20 °C per second. 15148. The process of claim 146 wherein the cooling rate is at least about 50 °C per second.

149. The process of claim 146 wherein the cooling rate is at least about 100 °C per second.

150. The process of claim 146 wherein Ti is about 900 °C.

151. The process of claim 150 wherein the cooling rate is at least about 20 °C per second.

152. The process of claim 150 wherein the cooling rate is at least about 50 °C per second.

153. The process of claim 150 wherein the cooling rate is at least about 5 100 °C per second.

154. The process of claim 146 wherein T is about 1,000 °C.

155. The process of claim 154 wherein the cooling rate is at least about 20 io °C per second.

156. The process of claim 154 wherein the cooling rate is at least about 50 °C per second. 15157. The process of claim 154 wherein the cooling rate is at least about 100 °C per second.

158. The process of claim 146 wherein the cooling rate is at least about 5 °C per second.

159. The process of claim 146 wherein said cooling rate is about 100 °C per sec to about 200 °C per second through the temperature range at which crystal lattice vacancies (13) are relatively mobile in silicon. 25160. The process of claim 159 wherein an epitaxial layer is deposited on said wafer in an epitaxial reactor prior to performing step (a).

161. The process of claim 160 wherein steps (a), (b) and (c) are performed in the epitaxial reactor after the epitaxial deposition.

162. The process of claim 146 wherein an epitaxial layer is deposited on said wafer in an epitaxial reactor prior to performing step (a).

163. The process of claim 162 wherein steps (a), (b) and (c) are performed in the epitaxial reactor after the epitaxial deposition.

164. The process of claim 146 wherein the silicon dioxide layer grown in step (a) has a thickness greater than a native oxide layer.

165. The process of claim 146 wherein the silicon dioxide layer grown in step (a) has a thickness of at least about 20 Angstroms.

166. The process of claim 146 wherein the silicon dioxide layer grown in step (a) has a thickness of at least about 25 Angstroms.

167. The process of claim 146 wherein the silicon dioxide layer grown in step (a) has a thickness of at least about 30 Angstroms.

168. The process of claim 146 wherein the atmosphere in step (b) is a nitriding atmosphere.

169. The process of claim 168 wherein said nitriding atmosphere comprises nitrogen.

170. The process of claim 168 wherein said nitriding atmosphere comprises ammonia.

171. The process of claim 146 wherein the atmosphere in step (b) is 5 selected from a group consisting of argon, helium, neon, and carbon dioxide.

172. The process of claim 146 wherein the atmosphere in step (b) has a partial pressure of oxygen of less than about 0.1 atmosphere. 10173. The process of claim 146 wherein the atmosphere in step (b) has a partial pressure of oxygen of less than about 0.05 atmosphere.

174. The process of claim 146 wherein the atmosphere in step (b) has a partial pressure of oxygen of less than about 0.001 atmosphere.

175. The process of claim 146 wherein the silicon is heat treated in step (b) for a time period of at least about 1 second.

176. The process of claim 146 wherein the silicon is heat treated in step (b) 20 for a time period of at least about 3 seconds.

177. The process of claim 146 wherein the silicon is heat treated in step (b) for a time period of at least about 30 seconds. 25178. The process of claim 146 wherein the silicon is heat treated in step (b) for a time period of at least about 60 seconds.

179. A process for the preparation of a silicon wafer comprising a front surface (3) having an epitaxial layer deposited thereon, a back surface (5), a central plane (7) between the front and back surfaces (3, 5), a front surface layer which comprises the region of the wafer between the front surface (3) and a distance, D, 5 measured from the front surface (3) and toward the central plane (7), and a bulk I layer (11) which comprises the region of the wafer between the central plane (7) and front surface layer, the bulk region further comprising a concentration of oxygen precipitates, wherein the process comprises: io subjecting the wafer to a heat-treatment to form crystal lattice vacancies (13) in the front surface (3) and bulk layers (11); controlling the cooling rate of the heat-treated wafer to produce a wafer having a vacancy concentration profile in which the peak density is at or near the 15 central plane (7) with the concentration generally decreasing in the direction of the front surface (3) of the wafer and the difference in the concentration of vacancies in the front surface (3) and bulk layers (11) being such that a thermal treatment at a temperature in excess of 750 °C, is capable of forming in the wafer a denuded zone (15, 15’) in the front surface layer and oxygen clusters or precipitates in the bulk 20 zone with the concentration of the oxygen clusters or precipitates in the bulk layer (11) being primarily dependant upon the concentration of vacancies; subjecting the silicon wafer, to an oxygen precipitation heat treatment to cause the nucleation and growth of oxygen precipitates in the bulk layer (11), to a 25 size sufficient to stabilize the oxygen precipitates such that they are incapable of being dissolved at temperatures not in excess of 1150 °C, with the oxygen precipitate concentration profile being formed according to the vacancy concentration profile such that a denuded zone (15, 15’) is formed in the front surface layer; and, depositing an epitaxial layer on at least one surface of the oxygen precipitate stabilized wafer.

180. The process of claim 179 wherein said heat-treatment to form crystal lattice vacancies (13) comprises heating the wafers to a temperature in excess of about 1175 °C in a non-oxidizing atmosphere. io181. The process of claim 179 wherein said heat-treatment to form crystal lattice vacancies (13) comprises heating the wafers to a temperature in excess of about 1200 °C in a non-oxidizing atmosphere.

182. The process of claim 179 wherein said heat-treatment to form crystal 15 lattice vacancies (13) comprises heating the wafers to a temperature in the range of about 1200 °C to about 1275 °C in a non-oxidizing atmosphere.

183. The process of claim 179 wherein said cooling rate is at least about 20 °C per second through the temperature range at which crystal lattice vacancies 20 (13) are relatively mobile in silicon.

184. The process of claim 179 wherein said cooling rate is at least about 50 °C per second through the temperature range at which crystal lattice vacancies (13) are relatively mobile in silicon.

185. The process of claim 179 wherein said cooling rate is at least about 100 °C per second through the temperature range at which crystal lattice vacancies (13) are relatively mobile in silicon.

186. The process of claim 179 wherein the oxygen precipitation heat 5 treatment comprises heating the wafer to a temperature of at least about 800 °C for a period of time sufficient to cause the nucleation and growth of oxygen precipitates in the bulk layer (11), to a size sufficient to stabilize the oxygen precipitates such that they are incapable of being dissolved at temperatures not in excess of 1150 °C. io187. The process of claim 186 wherein the wafer is heated for a period of time of at least about 4 hours.

188. The process of claim 186 further comprising heating the wafer to a temperature of at least about 1000 °C for at least about 16 hours.

189. A process for the preparation of a silicon wafer comprising a front surface (3) having an epitaxial layer deposited thereon, a back surface (5), a central plane (7) between the front and back surfaces (3, 5), a front surface layer which comprises the region of the wafer between the front surface (3) and a distance, D, 20 measured from the front surface (3) and toward the central plane (7), and a bulk layer (11) which comprises the region of the wafer between the central plane (7) and front surface layer, the bulk region further comprising a concentration of oxygen precipitates, wherein the process comprises: 25 (a) subjecting the silicon wafer to a first heat-treatment at a temperature of at least about 700 °C in an oxygen containing atmosphere to form a superficial silicon dioxide layer which is capable of serving as a sink for crystal lattice vacancies (13); (b) subjecting the product of step (a) to a second heat-treatment at a 5 temperature of at least about 1150 °C in an atmosphere having an essential absence of oxygen to form crystal lattice vacancies (13) in the bulk of the silicon; (c) cooling the product of step (b) from the temperature of said second heat treatment to a temperature, Ti, of about 800 °C at a rate which allows some, but io not all, of the crystal lattice vacancies (13) to diffuse to the sink to produce a wafer having a vacancy concentration profile in which the peak density is at or near the central plane (7) with the concentration generally decreasing in the direction of the front surface (3) of the wafer; 15 (d) subjecting the product of step (c), to an oxygen precipitation heat treatment to cause the nucleation and growth of oxygen precipitates in the bulk layer (11), to a size sufficient to stabilize the oxygen precipitates such that they are incapable of being dissolved at temperatures not in excess of 1150 °C, with the oxygen precipitate concentration profile being formed according to the vacancy 20 concentration profile such that a denuded zone (15, 15’) is formed in the front surface layer; and, (e) depositing an epitaxial layer on at least one surface of the product of step (d).

190. The process of claim 189 wherein the cooling rate is at least about 20 °C per second.

191. The process of claim 189 wherein the cooling rate is at least about 50 5 °C per second.

192. The process of claim 189 wherein the cooling rate is at least about 100 °C per second. io193. The process of claim 189 wherein Tt is about 900 °C.

194. The process of claim 193 wherein the cooling rate is at least about 20 °C per second. 15195. The process of claim 193 wherein the cooling rate is at least about 50 °C per second.

196. The process of claim 193 wherein the cooling rate is at least about 100 °C per second.

197. The process of claim 189 wherein Tt is about 1,000 °C.

198. The process of claim 197 wherein the cooling rate is at least about 20 °C per second.

199. The process of claim 197 wherein the cooling rate is at least about 50 °C per second.

200. The process of claim 197 wherein the cooling rate is at least about 5 100 °C per second.

201. The process of claims 189 wherein the oxygen precipitation heat treatment comprises heating the wafer to a temperature of at least about 800 °C for a period of time sufficient to cause the nucleation and growth of oxygen precipitates io in the bulk layer (11), to a size sufficient to stabilize the oxygen precipitates such that they are incapable of being dissolved at temperatures not in excess of 1150 °C.

202. The process of claim 201 wherein the wafer is heated for a period of time of at least about 4 hours.

203. The process of claim 201 further comprising heating the wafer to a temperature of at least about 1000 °C for at least about 16 hours.

204. A process for the preparation of a silicon wafer comprising a front 20 surface (3) having an epitaxial layer deposited thereon, a back surface (5), a central plane (7) between the front and back surfaces (3, 5), a front surface layer which comprises the region of the wafer between the front surface (3) and a distance, Di, measured from the front surface (3) and toward the central plane (7), and a bulk layer (11) which comprises the region of the wafer between the central plane (7) and 25 front surface layer, the bulk region further comprising a concentration of oxygen precipitates, wherein the process comprises: subjecting the wafer to a heat-treatment to form crystal lattice vacancies (13) in the surface layer and the bulk layer (11); and controlling the cooling rate of the heat-treated wafer to produce a wafer 5 having a non-uniform concentration of vacancies with the concentration of vacancies in the bulk layer (11) being greater than the concentration of vacancies in the surface layer such that, upon subjecting the wafer to an oxygen precipitation heat treatment, a denuded zone (15, 15’) is formed in the surface layer and oxygen clusters or precipitates are formed in the bulk layer (11) with the concentration of the oxygen io clusters or precipitates in the bulk layer (11) being primarily dependant upon the concentration of vacancies; and subjecting the silicon wafer to an oxygen precipitation heat treatment to cause the nucleation and growth of oxygen precipitates in the bulk layer (11), to a 15 size sufficient to stabilize the oxygen precipitates such that they are incapable of being dissolved at temperatures not in excess of 1150 °C; and, depositing an epitaxial layer on at least one surface ofthe oxygen precipitate stabilized wafer,205206 The process of claim 204 wherein Di is at least about 20 micrometers. The process of claim 204 wherein Di is at least about 50 micrometers. 100 micrometers.207 The process of claim 204 wherein Dt is between about 30 and about208. The process of claim 204 wherein said heat-treatment to form crystal lattice vacancies (13) comprises heating the wafers to a temperature in excess of about 1175 °C in a non-oxidizing atmosphere. 5209. The process of claim 204 wherein said heat-treatment to form crystal lattice vacancies (13) comprises heating the wafers to a temperature in excess of about 1200 °C in a non-oxidizing atmosphere.

210. The process of claim 204 wherein said heat-treatment to form crystal io lattice vacancies (13) comprises heating the wafers to a temperature in the range of about 1200 °C to about 1275 °C in a non-oxidizing atmosphere.

211. The process of any one of claims 204-210 wherein said non-oxidizing atmosphere is a nitriding atmosphere.

212. The process of claim 211 wherein said nitriding atmosphere is selected from a group consisting of nitrogen and ammonia.

213. The process of claim 212 wherein said nitriding atmosphere is 20 nitrogen.

214. The process of claim 213 wherein said nitriding atmosphere further comprises oxygen.

215. The process of claim 204 wherein said cooling rate is at least about 20 °C per second through the temperature range at which crystal lattice vacancies (13) are relatively mobile in silicon. 5216. The process of claim 204 wherein said cooling rate is at least about 50 °C per second through the temperature range at which crystal lattice vacancies (13) are relatively mobile in silicon.

217. The process of claim 204 wherein said cooling rate is at least about io 100 °C per second through the temperature range at which crystal lattice vacancies (13) are relatively mobile in silicon.

218. The process of claim 204 wherein said cooling rate is about 100 °C per sec to about 200 °C per second through the temperature range at which crystal 15 lattice vacancies (13) are relatively mobile in silicon.

219. The process of claim 204 wherein the oxygen precipitation heat treatment comprises heating the wafer to a temperature of at least about 800 °C for a period of time sufficient to cause the nucleation and growth of oxygen precipitates 20 in the bulk layer (11), to a size sufficient to stabilize the oxygen precipitates such that they are incapable of being dissolved at temperatures not in excess of 1150 °C.

220. The process of claim 219 wherein the wafer is heated for a period of time of at least about 4 hours.

221. The process of any one of claims 219 or 220 further comprising heating the wafer to a temperature of at least about 1000 °C for at least about 16 hours. 5222. A single crystal silicon wafer having two major, generally parallel surfaces, one of which is the front surface (3) of the wafer and the other of which is the back surface (5) of the wafer, a central plane (7) between the front and back surfaces (3, 5), a circumferential edge joining the front and back surfaces (3, 5), a front surface layer which comprises a first region of the wafer between the front io surface (3) and a distance, Di, of at least about 10 micrometers as measured from the front surface (3) and toward the central plane (7), a back surface layer which comprises a second region of the wafer between the back surface (5) and a distance D2r of at least about 10 micrometers as measured from the back surface (5) and toward the central plane (7) and a bulk layer (11) which comprises a third region of 15 the wafer between the front surface layer and the back surface layer, the wafer being characterized in that; the wafer has an asymmetrical vacancy concentration profile in the cooled wafer in which a maximum concentration is located between the central plane (7) 20 and the back surface layer, the vacancy concentration generally increasing from the front surface (3) to the region of maximum concentration and generally decreasing from the region of maximum concentration to the back surface (5) and the difference in the concentration of vacancies in the front surface layer, the back surface layer and the bulk layer (11) being such that a thermal treatment at a temperature in 25 excess of 750 °C, is capable of forming in the wafer a denuded zone (15, 15’) in the front surface layer and in the back surface layer and oxygen clusters or precipitates in the bulk zone with the concentration of the oxygen clusters or precipitates in the bulk layer (11) being primarily dependant upon the concentration of vacancies.

223. The wafer of claim 222 being further characterized in that the wafer 5 contains interstitial oxygen with the concentration of interstitial oxygen being substantially uniform between the center of the wafer and regions of the wafer which are within about 15 micrometers of the front surface (3).

224. The wafer of claim 222 wherein D1 and D2 are at least about 20 io micrometers.

225. The wafer of claim 222 wherein Di and D2 are at least about 50 micrometers.

226. The wafer of claim 222 wherein Di and D2 are between about 30 and about 100 micrometers.

227. A single crystal silicon wafer having two major, generally parallel surfaces, one of which is the front surface (3) of the wafer and the other of which is 20 the back surface (5) of the wafer, a central plane (7) between the front and back surfaces (3, 5), a circumferential edge joining the front and back surfaces (3, 5), a front surface layer which comprises a first region of the wafer between the front surface (3) and a distance, of at least about 10 micrometers as measured from the front surface (3) and toward the central plane (7), a back surface layer which 25 comprises a second region of the wafer between the back surface (5) and a distance D2i of at least about 10 micrometers as measured from the back surface (5) and229. The wafer of claim 227 wherein Dt and D2 are at least about 20 micrometers.

230. The wafer of claim 227 wherein Di and D2 are at least about 50 5 micrometers.

231. The wafer of claim 227 wherein Di and D2 are between about 30 and about 100 micrometers. io232. A single crystal silicon wafer having a front surface (3), a back surface (5), a central plane (7) between the front and back surfaces (3, 5), a circumferential edge joining the front and back surfaces (3, 5), a surface layer which comprises the region of the wafer between the front surface (3) and a distance, Di, of at least about 10 micrometers measured from the front surface (3) and toward the central plane (7), 15 a bulk layer (11) which comprises a second region of the wafer between the central plane (7) and the first region, and a non-uniform distribution of crystal lattice vacancies (13) with the concentration of vacancies in the bulk layer (11) being greater than the concentration of vacancies in the surface layer, such that upon being subjected to an oxygen precipitation heat-treatment a denuded zone (15, 15’) 20 is formed in the surface layer and oxygen precipitates are formed in the bulk layer (11) wherein the formation of the denuded zone (15, 15’) and the formation of the oxygen precipitates in the wafer bulk are not dependant upon differences in oxygen concentration in these regions of the wafer.

233. The wafer of claim 232 wherein D1 is at least about 20 micrometers.

234. The wafer of claim 232 wherein Dt is at least about 50 micrometers.

235. The wafer of claim 232 wherein Dt is between about 30 and about 100 micrometers.

236. The wafer of claim 232 wherein the concentration of interstitial oxygen at distances greater than 3 microns from the wafer surface is at least about 50% of the concentration of interstitial oxygen in the bulk layer (11). io237. The wafer of claim 232 wherein the concentration of interstitial oxygen at distances greater than 10 microns from the wafer surface is at least about 80% of the concentration of interstitial oxygen in the bulk layer (11).

238. The wafer of claim 237 wherein Dt is at least about 20 micrometers.

239. The wafer of claim 237 wherein Di is at least about 50 micrometers.

240. The wafer of claim 237 wherein Dt is between about 30 and about 100 micrometers.

241. The wafer of claim 232 wherein the concentration of interstitial oxygen at distances greater than 15 microns from the wafer surface is at least about 90% of the concentration of interstitial oxygen in the bulk layer (11). 25242. The wafer as set forth in claim 232 wherein the wafer further comprises an epitaxial layer on the wafer surface.

243. A process for heat-treating a single crystal silicon wafer sliced from a single crystal silicon ingot grown by the Czochralski method to influence the precipitation behavior of oxygen in the wafer in a subsequent thermal processing step, the single crystal silicon wafer having a front surface (3) and a back surface (5), 5 the front surface (3) having only a native oxide layer present thereon, a central plane (7) between the front and back surfaces (3, 5), a front surface layer which comprises a first region of the wafer between the front surface (3) and a distance, Di, of at least about 10 micrometers as measured from the front surface (3) and toward the central plane (7), a back surface layer which comprises a second region of the wafer 10 between the back surface (5) and a distance D2l of at least about 10 micrometers as measured from the back surface (5) and toward the central plane (7) and a bulk layer (11) which comprises a third region of the wafer between the front surface layer and the back surface layer, the process comprising: 15 heat-treating the wafer to form crystal lattice vacancies (13) in the wafer, and as part of said heat-treatment, exposing the front surface (3) of the wafer to a first atmosphere comprising a non-nitriding gas and exposing the back surface (5) of the wafer to a second atmosphere comprising a nitriding gas; and, 20 controlling the cooling rate of the heat-treated wafer to produce an asymmetrical vacancy concentration profile in the cooled wafer in which a maximum concentration is located between the central plane (7) and the back surface layer, the vacancy concentration generally increasing from the front surface (3) to the region of maximum concentration and generally decreasing from the region of 25 maximum concentration to the back surface (5) and the difference in the concentration of vacancies in the front surface layer, the back surface layer and the bulk layer (11) being such that a thermal treatment at a temperature in excess of 750 °C, is capable of forming in the wafer a denuded zone (15, 15’) in the front surface layer and in the back surface layer and oxygen clusters or precipitates in the bulk zone with the concentration of the oxygen clusters or precipitates in the bulk iayer 5 (11) being primarily dependant upon the concentration of vacancies.

244. The process of claim 243 wherein said heat-treatment to form crystal lattice vacancies (13) comprises heating the wafers to a temperature in excess of about 1175 °C.

245. The process of claim 243 wherein said heat-treatment to form crystal lattice vacancies (13) comprises heating the wafers to a temperature in excess of about 1200 °C. 15246. The process of claim 243 wherein said heat-treatment to form crystal lattice vacancies (13) comprises heating the wafers to a temperature in the range of about 1200 °C to about 1275 °C.

247. The process of claim 243 wherein said cooling rate is at least about 20 20 °C per second through the temperature range at which crystal lattice vacancies are relatively mobile in silicon.

248. The process of claim 243 wherein said cooling rate is at least about 50 °C per second through the temperature range at which crystal lattice vacancies 25 are relatively mobile in silicon.

249. The process of claim 243 wherein said cooling rate is at least about 100 °C per second through the temperature range at which crystal lattice vacancies (13) are relatively mobile in silicon.

250. The process of claim 243 wherein the nitriding atmosphere is selected from a group consisting of nitrogen and ammonia.

251. The process of claim 243 wherein the non-nitriding gas is selected from a group consisting of argon, helium, neon, carbon dioxide and mixtures thereof.

252. The process of claim 243 wherein the first atmosphere further comprises oxygen with the oxygen concentration in the first atmosphere being at least about 100 ppma and less than about 10,000 ppma.

253. The process of claim 243 wherein the first atmosphere further comprises oxygen with the oxygen concentration in the first atmosphere being at least about 200 ppma and less than about 5,000 ppma.

254. The process of claim 243 wherein the first atmosphere further comprises oxygen with the oxygen concentration in the first atmosphere being at least about 200 ppma and less than about 1,000 ppma.

255. A process for heat-treating a single crystal silicon wafer sliced from a single crystal silicon ingot grown by the Czochralski method to influence the precipitation behavior of oxygen in the wafer in a subsequent thermal processing step, the single crystal silicon wafer having a front surface (3) and a back surface (5), the front surface (3) having only a native oxide layer present thereon, and a central plane (7) between the front and back surfaces (3, 5), the process comprising: growing an oxide layer on the front surface (3) of the wafer by heating the 5 wafer in the presence of an oxygen containing ambient; heat-treating the wafer to form crystal lattice vacancies (13) in the wafer, and as part of said heat-treatment, exposing the front surface (3) of the wafer to a first atmosphere comprising a non-nitriding gas and exposing the back surface (5) of the io wafer to a second atmosphere comprising a nitriding gas; and, controlling the cooling rate of the heat-treated wafer to produce an asymmetrical vacancy concentration profile in the cooled wafer in which a maximum concentration is between the front surface (3) and the back surface (5) and nearer to 15 the back surface (5), the vacancy concentration generally increasing from the front surface (3) to the region of maximum concentration and generally decreasing from the region of maximum concentration to the back surface (5).

256. The process of claim 255 wherein said heat-treatment to form crystal 20 lattice vacancies (13) comprises heating the wafers to a temperature in excess of about 1175 °C.

257. The process of claim 255 wherein said heat-treatment to form crystal lattice vacancies (13) comprises heating the wafers to a temperature in excess of 25 about 1200 °C.

258. The process of claim 255 wherein said heat-treatment to form crystal lattice vacancies (13) comprises heating the wafers to a temperature in the range of about 1200 °C to about 1275 °C. 5259. The process of claim 255 wherein said cooling rate is at least about 20 °C per second through the temperature range at which crystal lattice vacancies (13) are relatively mobile in silicon.

260. The process of claim 255 wherein said cooling rate is at least about 10 50 °C per second through the temperature range at which crystal lattice vacancies (13) are relatively mobile in silicon.

261. The process of claim 255 wherein said cooling rate is at least about 100 °C per second through the temperature range at which crystal lattice vacancies 15 (13) are relatively mobile in silicon.

262. The process of claim 255 wherein the nitriding atmosphere is selected from a group consisting of nitrogen and ammonia. 202 63. The process of claim 255 wherein the non-nitriding gas is selected from a group consisting of argon, helium, neon, carbon dioxide and mixtures thereof.

264. The process of claim 255 wherein the first atmosphere further comprises oxygen with the oxygen concentration in the first atmosphere being at 25 least about 100 ppma and less than about 10,000 ppma.

265. The process of claim 255 wherein the first atmosphere further comprises oxygen with the oxygen concentration in the first atmosphere being at least about 200 ppma and less than about 5,000 ppma. 5266. The process of claim 255 wherein the first atmosphere further comprises oxygen with the oxygen concentration in the first atmosphere being at least about 200 ppma and less than about 1,000 ppma.

267. A process for heat-treating a single crystal silicon wafer sliced from a io single crystal silicon ingot grown by the Czochralski method to influence the precipitation behavior of oxygen in the wafer in a subsequent thermal processing step, the single crystal silicon wafer having a front surface (3) and a back surface (5), the front and back surfaces (3, 5) having only a native oxide layer present thereon, a central plane (7) between the front and back surfaces (3, 5), a front surface layer 15 which comprises a first region of the wafer between the front surface (3) and a distance, D1( of at least about 10 micrometers as measured from the front surface (3) and toward the central plane (7), a back surface layer which comprises a second region of the wafer between the back surface (5) and a distance D2, of at least about 10 micrometers as measured from the back surface (5) and toward the central plane 20 (7) and a bulk layer (11) which comprises a third region of the wafer between the front surface layer and the back surface layer, the process comprising. heat-treating the wafer in a nitrogen atmosphere to form a concentration of crystal lattice vacancies (13) in the wafer, the concentration profile being generally U25 shaped, having a maximum concentration within several micrometers of the front and back surfaces and a minimum concentration located in the bulk layer (11) of the wafer; and, controlling the cooling rate of the heat-treated wafer to reduce the 5 concentration of vacancies (13) in the front surface layer and back surface layer to produce a vacancy concentration profile in the cooled wafer in which the maximum concentration is located in a first region of maximum concentration between the front surface layer and the central plane (7) and in a second region of maximum concentration between the back surface layer and the central plane (7), the vacancy 10 concentration generally increasing from the front surface (3) to the first region of maximum concentration, generally decreasing from the first region of maximum concentration to the central plane (7), generally increasing from the central plane (7) to the second region of maximum concentration and generally decreasing from the second region of maximum concentration to the back surface (5) and the difference 15 in the concentration of vacancies in the front surface layer, the back surface layer and the bulk layer (11) being such that a thermal treatment at a temperature in excess of 750 °C, is capable of forming in the wafer a denuded zone (15, 15’) in the front surface layer and in the back surface layer and oxygen clusters or precipitates in the bulk zone (11) with the concentration of the oxygen clusters or precipitates in 20 the bulk layer (11) being primarily dependant upon the concentration of vacancies.

268. The process of claim 267 wherein said heat-treatment to form crystal lattice vacancies (13) comprises heating the wafers to a temperature in excess of about 1175 °C.

269. The process of claim 267 wherein said heat-treatment to form crystal lattice vacancies (13) comprises heating the wafers to a temperature in excess of about 1200 °C. 5270. The process of claim 267 wherein said heat-treatment to form crystal lattice vacancies (13) comprises heating the wafers to a temperature in the range of about 1200 °C to about 1275 °C.

271. The process of claim 267 wherein said cooling rate is at least about io 20 °C per second through the temperature range at which crystal lattice vacancies (13) are relatively mobile in silicon.

272. The process of claim 267 wherein said cooling rate is at least about 50 °C per second through the temperature range at which crystal lattice vacancies 15 (13) are relatively mobile in silicon.

273. The process of claim 267 wherein said cooling rate is at least about 100 °C per second through the temperature range at which crystal lattice vacancies (13) are relatively mobile in silicon. fig 1 FiG. FIG. 5 / <? Sr \\ ih k $ &I ?15 fc I I I *t IO / z ,1.1.1 l JLX I 1,1 < I I I I,.1.1 1 I I I I I 1-1.1-1.1 J. >H ItJt.lIl ll I ll II li I ,11,1 I