Dressing structural member and conditioner
The grinding structural member with controlled thermal expansion layers addresses warpage and cracking issues in conditioner structures, enhancing polishing consistency and integrity through balanced thermal stress management.
Patent Information
- Application Number
- US19/548884
- Authority / Receiving Office
- US · United States
- Patent Type
- Applications(United States)
- Current Assignee / Owner
- Priority Date
- 2025-03-14
- Filing Date
- 2026-02-24
- Publication Date
- 2026-11-12
AI Technical Summary
Conventional conditioner structures in chemical-mechanical polishing processes suffer from warpage and cracking due to mismatched thermal expansion coefficients during the brazing process, leading to inconsistent polishing quality and structural integrity issues.
A grinding structural member comprising a grinding structural layer, a supporting structural layer, and a brazing layer, where the layers have different thermal expansion coefficients to control warpage direction and magnitude, and a conditioner incorporating this member to maintain polishing pad surface roughness.
The solution effectively controls warpage and prevents cracking, ensuring consistent polishing quality by balancing thermal stresses and maintaining structural integrity of the conditioner.
Smart Images

Figure US20260355898A1-D00000_ABST
Abstract
Description
CROSS-REFERENCE TO RELATED PATENT APPLICATION
[0001] This application claims the benefit of priority to China Patent Application No. 202510300743.9, filed on Mar. 14, 2025, in the People's Republic of China. The entire content of the above identified application is incorporated herein by reference.
[0002] Some references, which may include patents, patent applications and various publications, may be cited and discussed in the description of this disclosure. The citation and / or discussion of such references is provided merely to clarify the description of the present disclosure and is not an admission that any such reference is “prior art” to the disclosure described herein. All references cited and discussed in this specification are incorporated herein by reference in their entireties and to the same extent as if each reference was individually incorporated by reference.FIELD OF THE DISCLOSURE
[0003] The present disclosure relates to a grinding structural member and conditioner, and more particularly to a grinding structural member and a conditioner suitable for dressing a polishing pad.BACKGROUND OF THE DISCLOSURE
[0004] In a chemical-mechanical polishing (CMP) process or a high-precision polishing process, a polishing pad is typically used in combination with a polishing slurry to polish surfaces of workpieces such as semiconductor wafers, optical components, or glass. In general, a conditioner is used to dress a surface of the polishing pad. The conditioner removes waste material left on the polishing pad during polishing by using its abrasive layer, and restores surface roughness of the polishing pad to maintain consistent polishing quality.
[0005] In the related art, a brazing process is used to fix abrasive particles (e.g., diamond abrasive particles) onto a metal substrate of a conditioner (e.g., a stainless-steel substrate). However, during the brazing process in which the abrasive particles are bonded from the high-temperature stage to the cooling and fixing stage, a cooling rate at a central region of the substrate differs from a cooling rate at an edge region of the substrate, and coefficients of thermal expansion of the brazing filler and the metal substrate are different. As a result, the conditioner structure composed of the substrate, the brazing filler, and the abrasive particles is prone to warpage (or bending), and an amount of warpage is difficult to control, thereby adversely affecting subsequent processing. In another conventional technique, a pre-sintering process can be applied to a grinding sheet (a structure composed of a grinding layer, brazing filler, and abrasive particles), and the grinding sheet is then attached to a metal substrate. Since the pre-sintered grinding sheet has high rigidity, excessive warping can cause cracks in the sheet structure when external pressure is applied to force the bent sheet (formed by solder cooling and setting) to flatten and adhere to the dresser's substrate, leading to detachment of the abrasive particles.SUMMARY OF THE DISCLOSURE
[0006] In response to the above-referenced technical inadequacy, the present disclosure provides a grinding structural member and a conditioner, which can prevent deformation of the conditioner from high-temperature thermal stress, effectively controlling the grinding structural member to achieve a desired warpage direction and an expected amount of warpage, thereby addressing surface cracking issues resulting from welding thermal stress.
[0007] In order to solve the above-mentioned problems, one of the technical aspects adopted by the present disclosure is to provide a grinding structural member, which includes a grinding structural layer, a supporting structural layer, and a brazing layer. The grinding structural layer includes a first infiltrated composite layer and a plurality of first abrasive particles. The first infiltrated composite layer has a grinding surface and a first bonding surface that are opposite to each other. The plurality of first abrasive particles are dispersedly embedded in the grinding surface of the first infiltrated composite layer, with each of the first abrasive particles being partially exposed on the grinding surface. The supporting structural layer has a second bonding surface that faces the first bonding surface. The brazing layer is disposed between the first bonding surface and the second bonding surface, and is configured to bond the first infiltrated composite layer and the supporting structural layer.
[0008] In order to solve the above-mentioned problems, another one of the technical aspects adopted by the present disclosure is to provide a conditioner, which includes a base and the grinding structural member.
[0009] Therefore, the grinding structural member is formed by utilizing the grinding structural layer, the supporting structural layer, and the brazing layer. One side of the brazing layer is connected to a grinding structural layer having a low coefficient of thermal expansion, while another side of the brazing layer is connected to a supporting structural layer having a high coefficient of thermal expansion. Since the compressive stress of the grinding structural layer generates a downward warping moment, whereas the shrinkage tensile stress of the supporting structural layer generates an upward warping moment, the final degree of warpage is determined by the combined action of these moments. Accordingly, the present disclosure enables the warpage direction and the expected warpage magnitude of the grinding structural member after brazing to be controlled through the configuration of the grinding structural layer and the supporting structural layer.
[0010] These and other aspects of the present disclosure will become apparent from the following description of the embodiment taken in conjunction with the following drawings and their captions, although variations and modifications therein may be effected without departing from the spirit and scope of the novel concepts of the disclosure.BRIEF DESCRIPTION OF THE DRAWINGS
[0011] The described embodiments may be better understood by reference to the following description and the accompanying drawings, in which:
[0012] FIG. 1 is a schematic view of a grinding structural layer according to a first embodiment of the present disclosure;
[0013] FIG. 2 is a schematic view of a method of manufacturing the grinding structural layer according to the first embodiment of the present disclosure;
[0014] FIG. 3 is a schematic view showing a warpage of the grinding structural member according to the first embodiment of the present disclosure;
[0015] FIG. 4 is a schematic view showing that the grinding structural member is fixed to the base according to the first embodiment of the present disclosure;
[0016] FIG. 5 is a schematic view of a conditioner according to the first embodiment of the present disclosure;
[0017] FIG. 6 is a schematic view of another implementation of the conditioner according to the first embodiment of the present disclosure;
[0018] FIG. 7 is a schematic view of a grinding structural layer according to a second embodiment of the present disclosure;
[0019] FIG. 8 is a schematic view of a conditioner according to the second embodiment of the present disclosure;
[0020] FIG. 9 is a schematic view of a grinding structural layer according to a third embodiment of the present disclosure; and
[0021] FIG. 10 is a schematic view of a conditioner according to the third embodiment of the present disclosure.DETAILED DESCRIPTION OF THE EXEMPLARY EMBODIMENTS
[0022] The present disclosure is more particularly described in the following embodiments and examples that are intended as illustrative only since numerous modifications and variations therein will be apparent to those skilled in the art. Like numbers in the drawings indicate like components throughout the views. As used in the description herein and throughout the claims that follow, unless the context clearly dictates otherwise, the meaning of “a,”“an” and “the” includes plural reference, and the meaning of “in” includes “in” and “on.” Titles or subtitles can be used herein for the convenience of a reader, which shall have no influence on the scope of the present disclosure.
[0023] The terms used herein generally have their ordinary meanings in the art. In the case of conflict, the present document, including any definitions given herein, will prevail. The same thing can be expressed in more than one way. Alternative language and synonyms can be used for any term(s) discussed herein, and no special significance is to be placed upon whether a term is elaborated or discussed herein. A recital of one or more synonyms does not exclude the use of other synonyms. The use of examples anywhere in this specification including examples of any terms is illustrative only, and in no way limits the scope and meaning of the present disclosure or of any exemplified term. Likewise, the present disclosure is not limited to various embodiments given herein. Numbering terms such as “first,”“second” or “third” can be used to describe various components, signals or the like, which are for distinguishing one component / signal from another one only, and are not intended to, nor should be construed to impose any substantive limitations on the components, signals or the like.First Embodiment
[0024] Reference is made to FIG. 1, which is a schematic view of a grinding structural layer according to a first embodiment of the present disclosure. A grinding structural member M1 includes a grinding structural layer 1, a supporting structural layer 2, and a brazing layer 3. The brazing layer 3 is disposed between the grinding structural layer 1 and the supporting structural layer 2. The grinding structural layer 1 includes a first infiltrated composite layer 11 and a plurality of first abrasive particles 12. Reference may be made concurrently to FIG. 2, in which the first infiltrated composite layer 11 has a grinding surface 111 and a first bonding surface 112 that are opposite to each other. The plurality of first abrasive particles 12 are dispersedly embedded in the grinding surface 111 of the first infiltrated composite layer 11, and each of the first abrasive particles 12 is partially exposed on the grinding surface 111. The first infiltrated composite layer 11 includes a first porous structural layer 113 and a portion of a metal brazing filler B disposed within the first porous structural layer 113. That is, the first infiltrated composite layer 11 is formed by infiltration of a first portion B1 of the metal brazing filler B into the first porous structural layer 113.
[0025] Reference may be further made concurrently to FIG. 2. The supporting structural layer 2 has a second bonding surface 20, and the second bonding surface 20 faces the first bonding surface 112. The brazing layer 3 is disposed between the first bonding surface 112 and the second bonding surface 20, and is configured to bond the first infiltrated composite layer 11 and the supporting structural layer 2. In the first embodiment, the supporting structural layer 2 includes a second infiltrated composite layer 21, and the second bonding surface 20 is a surface of the second infiltrated composite layer 21 facing the brazing layer 3. The second infiltrated composite layer 21 includes a second porous structural layer 213 and another portion of the metal brazing filler B disposed within the second porous structural layer 213. That is, the second infiltrated composite layer 21 is formed by infiltration of a second portion B2 of the metal brazing filler B into the second porous structural layer 213. The first porous structural layer 113 and the second porous structural layer 213 are metal porous structures. For example, the materials of the first porous structural layer 113 and the second porous structural layer 213 include, but are not limited to, nickel, iron, copper, titanium, molybdenum, cobalt, chromium, stainless steel, nickel alloys, iron alloys, copper alloys, or titanium alloys. Furthermore, the first porous structural layer 113 and the second porous structural layer 213 include, but are not limited to, mesh structures, foamed structures, fibrous structures, or fin structures. In a preferred embodiment, the first porous structural layer 113 and the second porous structural layer 213 are formed of foamed nickel or a nickel alloy thereof (e.g., nickel foam). In other embodiments, the first porous structural layer 113 and the second porous structural layer 213 may alternatively be formed of foamed titanium, foamed stainless steel, or nickel fibers. It should be noted that each of the first porous structural layer 113 and the second porous structural layer 213 can be a single-layer structure or a multilayer structure without limitation.
[0026] For example, the first porous structural layer 113 and the second porous structural layer 213 may be fabricated by powder metallurgy, hot extrusion, molten metal processes, electroplating, electrochemical deposition, or casting processes. The first porous structural layer 113 has a plurality of first pores V1 distributed on a surface and within an interior thereof, and the second porous structural layer 213 has a plurality of second pores V2 distributed on a surface and within an interior thereof. For example, a porosity of the first porous structural layer 113 ranges from about 10% to 50%, and a porosity of the second porous structural layer 213 ranges from about 20% to 95%. The first abrasive particles 12 can include single-crystal diamond, polycrystalline diamond, polycrystalline diamond compact (PCD), CVD diamond, diamond, cubic boron nitride (cBN) particles, silicon carbide particles, or any combination thereof.
[0027] The brazing layer 3 is formed of the metal brazing filler B. The metal brazing filler B can include a metal alloy, and preferably a nickel-based alloy (BNi-2). Furthermore, the metal brazing filler B can be in the form of a brazing foil, brazing paste, brazing powder, or a mixture of brazing powder and resin. The form of the metal brazing filler B is not limited in the present disclosure. The metal brazing filler B becomes molten in a high-temperature vacuum environment, such that the first portion B1 of the molten metal brazing filler B infiltrates into the first porous structural layer 113 through capillary action from the first pores V1, and after cooling and solidification, forms the first infiltrated composite layer 11 while bonding the plurality of first abrasive particles 12. Another portion of the metal brazing filler B that does not infiltrate into the first porous structural layer 113 forms the brazing layer 3 upon cooling and solidification. Similarly, the second portion B2 of the metal brazing filler B (i.e., a dot-pattern region located within the second porous structural layer 213 in FIG. 1) infiltrates into the second porous structural layer 213 through capillary action from the second pores V2, and after cooling and solidification, forms the second infiltrated composite layer 21.
[0028] It should be noted that the first portion B1 of the metal brazing filler B infiltrates to fill or penetrate through the grinding surface 111 of the first infiltrated composite layer 11, although the grinding surface 111 may not be completely leveled due to surface tension, and minor recesses may remain. However, the second portion B2 does not necessarily completely fill all of the second pores V2 of the second porous structural layer 213. That is, the second portion B2 can fully or partially fill the second pores V2. As shown in FIG. 1, in a preferred embodiment, the second portion B2 partially fills the second pores V2 of the second porous structural layer 213, such that portions of the second porous structural layer 213 not filled by the second portion B2 serve as a compressible elastic layer for use in subsequent steps where the grinding structural member M1 is bonded to a base. Accordingly, by absorbing height differences caused by unevenness of the base, an overall height of the grinding structural member M1 can be adjusted, and flatness of the grinding structural member M1 can be maintained.
[0029] Furthermore, in the grinding structural member M1, an equivalent coefficient of thermal expansion of the grinding structural layer 1 including the first infiltrated composite layer 11 and the plurality of first abrasive particles 12 is less than or equal to an equivalent coefficient of thermal expansion of the supporting structural layer 2. More specifically, an equivalent coefficient of thermal expansion of a composite structure jointly formed by the grinding structural layer 1 and the first portion B1 of the metal brazing filler B is less than or equal to an equivalent coefficient of thermal expansion of another composite structure jointly formed by the supporting structural layer 2, the second portion B2 of the metal brazing filler B, and the brazing layer 3. In addition, the sizes of the first pores V1 in the first infiltrated composite layer 11 and the second pores V2 in the second infiltrated composite layer 21 shown in FIG. 1 are merely schematic and not limited in the present disclosure. The first infiltrated composite layer 11 and the second infiltrated composite layer 21 differ in thickness. In a preferred embodiment, a thickness H1 of the first infiltrated composite layer 11 ranges from 0.05 mm to 0.5 mm, a thickness H2 of the second infiltrated composite layer 21 ranges from 0.1 mm to 1 mm, and a thickness H3 of the brazing layer 3 ranges from 0.005 mm to 0.1 mm.
[0030] In the following, a manufacturing process of the grinding structural member M1 is further described. Reference is made to FIGS. 1 and 2. FIG. 2 is a schematic view of a method of manufacturing the grinding structural layer according to the first embodiment of the present disclosure.
[0031] As shown in step S1 of FIG. 2, the first porous structural layer 113 is provided and a plurality of first abrasive particles 12 are embedded in the grinding surface 111 of the first porous structural layer 113. Each of the first abrasive particles 12 is partially exposed on the grinding surface 111. An arrangement orientation and an exposed height of each of the first abrasive particles 12 can be fixed by the first porous structural layer 113, so that exposed heights of the plurality of first abrasive particles 12 are controlled to be at a same horizontal level. Moreover, the first porous structural layer 113 further controls and fixes the arrangement orientation of the first abrasive particles 12 so as to prevent the first abrasive particles 12 from flipping during a subsequent brazing process due to high-temperature boiling of the metal brazing filler B.
[0032] Then, as shown in step S2 of FIG. 2, the metal brazing filler B and the second porous structural layer 213 are provided to form a stacked structure together with the first porous structural layer 113. The first porous structural layer 113 contacts the metal brazing filler B via the first bonding surface 112, and the second porous structural layer 213 contacts the metal brazing filler B via the second bonding surface 20. Accordingly, the metal brazing filler B is located between the first bonding surface 112 and the second bonding surface 20.
[0033] As shown in step S3 of FIG. 2, the stacked structure including the plurality of first abrasive particles 12, the first porous structural layer 113, the metal brazing filler B, and the second porous structural layer 213 is placed into a high-temperature vacuum furnace (not shown in the figures) to perform a brazing process. The metal brazing filler B is heated to a high temperature (e.g., above 1000 °C) and melts into a molten state. The first portion B1 of the metal brazing filler B infiltrates into the first porous structural layer 113 to form the first infiltrated composite layer 11 and bonds the plurality of first abrasive particles 12 to constitute the grinding structural layer 1. The second portion B2 of the metal brazing filler B infiltrates into the second porous structural layer 213 to form the second infiltrated composite layer 21 (i.e., the supporting structural layer 2). The remaining portion of the metal brazing filler B solidifies after cooling to form the brazing layer 3. Accordingly, the brazing layer 3, the supporting structural layer 2, and the grinding structural layer 1 jointly form the grinding structural member M1. Additionally, during the brazing process, a pressing plate P can be placed on the stacked structure to stabilize sintering of the grinding structural member M1.
[0034] It is worth mentioning that, as shown in FIG. 2, the first portion B1 of the metal brazing filler B infiltrated into the first porous structural layer 113 covers the first bonding surface 112, and the second portion B2 infiltrated into the second porous structural layer 213 covers the second bonding surface 20. The metal brazing filler B further remains as a residual brazing interface layer (i.e., the brazing layer 3 in FIG. 3) between the first infiltrated composite layer 11 and the second infiltrated composite layer 21. Therefore, the metal brazing filler B is interposed between the first infiltrated composite layer 11 and the second infiltrated composite layer 21, and the first pores V1 and the second pores V2 are not in spatial communication with each other.
[0035] During the brazing process, the grinding structural member M1 can be disposed with the grinding structural layer 1 facing downward, such that a surface on which the first abrasive particles 12 are provided faces a carrier platform (not shown in the figures) in the high-temperature vacuum furnace. The first portion B1 of the metal brazing filler B infiltrates into the first porous structural layer 113 under the combined effects of capillary action, gravity, and pressure applied by the pressing plate P, so as to ensure uniform stress distribution in the grinding structural member M1.
[0036] Generally, conventional grinding structural members include only abrasive particles, a grinding structural layer, and a brazing layer without a supporting structural layer, and thus are unable to control variations in coefficients of thermal expansion. When the first abrasive particles 12 are, for example, diamond, a coefficient of linear thermal expansion (CTE) thereof at 1000 °C is approximately 1.0×10−6 / °C. When the metal brazing filler B of the brazing layer 3 is, for example, a nickel-based alloy (BNi-2), a coefficient of linear thermal expansion thereof at 1000 °C is approximately 13.5×10−6 / °C. Further, pure nickel has a coefficient of linear thermal expansion of approximately 16.2×106 / °C at 1000 °C. Furthermore, the first porous structural layer 113 made of nickel foam has a porosity of about 30%, such that a solid volume fraction of the first porous structural layer 113 is about 70%. When calculating an equivalent coefficient of thermal expansion of the grinding structural member M1, assuming a thickness H1 of 0.2 mm for the nickel foam structure (i.e., the first porous structural layer 113), an insertion depth of 0.1 mm for the diamond abrasive particles (i.e., the first abrasive particles 12), and an embedded area occupying 50% of the nickel foam surface area, an equivalent coefficient of thermal expansion during brazing at 1000 °C may be derived as follows.
[0037] The coefficient of thermal expansion of the nickel foam structure can be calculated by a volume-weighted average as (0.7×16.2)×10−6 / °C=11.34×10 / °C.
[0038] Given that the insertion depth of the diamond abrasive particles is 0.1 mm and the thickness of the nickel foam structure is 0.2 mm, the volume fraction occupied by the diamond abrasive particles is approximately (0.1 / 0.2)×50%=25%.
[0039] Accordingly, an equivalent coefficient of thermal expansion of the nickel foam structure occupying 75% by volume and the diamond abrasive particles occupying 25% by volume is ((0.75×11.34)+(0.25×1.0))×10−6 / °C=8.26×10−6 / °C.
[0040] Considering the effect after infiltration of the brazing layer 3, for example, a nickel-based alloy (BNi-2), the foamed nickel has a porosity of 30%. Assuming that the nickel-based alloy infiltrates and completely fills all of the first pores V1, the nickel-based alloy occupies approximately 30% of an area of the grinding surface 111. Accordingly, an equivalent coefficient of thermal expansion of the grinding surface 111 is calculated as (0.7×8.26)+(0.3×13.5)=9.83×10−6 / °C.
[0041] Although nickel foam is essentially formed of pure nickel, the presence of pores reduces overall stiffness, such that thermal expansion does not fully follow that of pure nickel. The micro-pores having a porosity of about 30% restrict expansion and reduce the effective coefficient of thermal expansion, and the foam structure lowers expansion transmission and reduces the coefficient of thermal expansion from that of pure nickel, for example, from 16.2×10−6 / °C to 11.34×10−6 / °C. When the nickel-based alloy infiltrates and fills internal pores of the foamed nickel structure, since the foamed nickel structure still constitutes a major portion of the overall structure, constraining effects of the foamed nickel structure are retained, such as with respect to a coefficient of thermal expansion, mechanical strength, and thermal conductivity.
[0042] When thermal expansion occurs, an internal microstructures of a material affects a resulting expansion behavior. Differences in coefficients of thermal expansion among heterogeneous materials lead to internal stresses, for example, due to a mismatch between coefficients of thermal expansion of a nickel-based alloy and a foamed nickel structure. Accordingly, upon heating, the heterogeneous materials expand by different amounts, thereby generating mechanical stresses that constrain overall expansion, and such an effect generally reduces an equivalent coefficient of thermal expansion.
[0043] Nickel foam has relatively low stiffness and high flexibility. Even if the nickel-based alloy fills internal pores of the foamed nickel, the foamed nickel serving as a base material still provides a structure with relatively low mechanical rigidity, such that a thermal expansion of the foamed nickel structure filled with the nickel-based alloy is smaller than that of a pure nickel-based alloy. That is, when a filler (e.g., a nickel-based alloy) infiltrates a porous structure (e.g., a foamed nickel structure), a coefficient of thermal expansion of a resulting composite structure remains smaller than a coefficient of thermal expansion of the filler itself. This is because a microstructure of the porous structure suppresses transmission of thermal expansion, and thermal stresses between heterogeneous materials reduce an overall coefficient of thermal expansion.
[0044] Since the equivalent coefficient of thermal expansion of the grinding surface 111 of the first infiltrated composite layer 11 is less than or equal to that of the brazing layer 3, a volumetric shrinkage of the brazing layer 3 during cooling and solidification is greater than or equal to that of the grinding surface 111. Therefore, a tensile stress generated by shrinkage of the first infiltrated composite layer 11 on a side on which the brazing layer 3 is formed during cooling is greater than or equal to a compressive stress generated by stretching of the grinding surface 111 side during cooling, thereby causing downward warpage of the grinding structural member after fabrication.
[0045] On the other hand, as shown in step S1 of FIG. 2, when the first abrasive particles 12 are too small, for example, having a particle size less than 0.1 mm, the thickness of the first porous structural layer 113 cannot be designed to be too large, for example, exceeding 0.2 mm. This is because the molten metal brazing filler B (the first portion B1) infiltrated into the first porous structural layer 113 may rapidly diffuse to the first abrasive particles 12 and even to the grinding surface 111, so as to flood the first abrasive particles 12. Even if the thickness of the brazing layer 3 or the thickness of the first porous structural layer 113 is reduced, this may help alleviate the problem of the brazing filler flooding the abrasive particles. Nonetheless, a reduction in the thickness of the first porous structural layer 113 or the brazing layer 3 makes the overall structure thinner, causing it to form a wavy profile during cooling and solidification due to non-uniform stress distribution, which adversely affects the quality of subsequent processing. A mechanism by which capillary action drives molten brazing metal into a porous foamed nickel structure is mainly determined by wettability, capillary pressure, surface tension, and diffusion behavior. To improve phenomena such as warpage or formation of a wavy profile occurring in the grinding structural member after formation, the present disclosure provides the following improvement solutions.
[0046] The grinding structural member M1 of the present disclosure includes the supporting structural layer 2, namely, the second infiltrated composite layer 21, which increases stiffness of the grinding structural member M1 and reduces a tendency to form a wavy profile after cooling and solidification. As shown in FIG. 1, since the supporting structural layer 2 is formed by infiltration of the molten metal brazing filler B into the second porous structural layer 213, the amount of metal brazing filler B forming the brazing layer 3 is reduced, thereby decreasing a thickness of the brazing layer 3. As the brazing layer 3 becomes thinner, a volumetric shrinkage generated during cooling and solidification becomes smaller (and a resulting tensile stress is reduced), thereby decreasing an extent of warpage. In addition, flexibility of the grinding structural member M1 is increased, which is also beneficial to a subsequent planarization bonding process.
[0047] However, as described above, since the composite structure formed by the grinding structural layer 1 (i.e., the first infiltrated composite layer 11 and the plurality of first abrasive particles 12) and the first portion B1 of the metal brazing filler B has a coefficient of thermal expansion smaller than that of the composite structure formed by the supporting structural layer 2 and the second portion B2 of the metal brazing filler B, the grinding structural member M1 may still warp after brazing. Accordingly, through the design of the second infiltrated composite layer 21, for example, by adjusting a porosity or a thickness of the second porous structural layer 213, a degree and a direction of warpage of the grinding structural member M1 can be appropriately controlled, and flatness can even be achieved.
[0048] Furthermore, once the second porous structural layer 213 is infiltrated by the molten metal brazing filler B (i.e., the second portion B2 of the metal brazing filler B), the amount of the metal brazing filler B infiltrating into the first porous structural layer 113, i.e., the first portion B1 of the metal brazing filler B, can be correspondingly reduced. In other words, by incorporating the second porous structural layer 213 into the grinding structural member M1, an amount of the metal brazing filler B infiltrating into the first porous structural layer 113 (i.e., an amount of the first portion B1 of the metal brazing filler B) can be further controlled, and an excessive infiltration of the metal brazing filler B that would otherwise flood the first abrasive particles 12 can be addressed by balancing capillary forces.
[0049] In the present disclosure, through the design of the second porous structural layer 213 with different porosities and different thicknesses, an amount of the metal brazing filler B infiltrating into the first porous structural layer 113 and the second porous structural layer 213, as well as an amount of the metal brazing filler B forming the brazing layer 3, can be controlled, thereby controlling tensile stress of the brazing layer 3, avoiding warpage, and controlling a direction of warpage. For example, an average size of the second pores V2 is greater than an average size of the first pores V1, and a thickness of the second porous structural layer 213 is greater than that of the first porous structural layer 113, such that a capillary force of the second porous structural layer 213 is weaker and an amount of the metal brazing filler B infiltrating into the second porous structural layer 213 is smaller than an amount of the metal brazing filler B infiltrating into the first porous structural layer 113. That is, the amount of the second portion B2 is smaller than the amount of the first portion B1. Accordingly, an amount of the brazing filler infiltrating into the first porous structural layer 113 is more sufficiently distributed, thereby avoiding adverse effects on a bonding strength between the first abrasive particles 12 and the first porous structural layer 113, and enabling residual stresses after cooling to be more uniformly distributed, such that a degree of warpage is reduced or flatness is achieved.
[0050] After mitigating warpage of the grinding structural member M1 by configuring the second infiltrated composite layer 21, the resulting grinding structural member M1 is shown in FIG. 3, which is a schematic view showing that the warpage of the grinding structural member according to the first embodiment of the present disclosure. It should be noted that the grinding structural member M1 shown in FIG. 3 schematically illustrates an example of warpage (i.e., a central portion protrudes outward toward a side on which the first abrasive particles 12 are disposed relative to two lateral portions), and detailed structures of the grinding structural member M1 are omitted for clarity. Reference can be made to FIG. 1 for details of the grinding structural member M1.
[0051] Then, a manufacturing process of a conditioner according to the present disclosure is described. Reference is made to FIGS. 4 and 5. FIG. 4 is a schematic view showing that the grinding structural member is fixed to the base according to the first embodiment of the present disclosure. FIG. 5 is a schematic view of a conditioner according to the first embodiment of the present disclosure. A base 4 and an adhesive are provided, and the adhesive is disposed on a bonding surface 41 of the base 4 to form an adhesive layer 5. The adhesive may include, for example, a low-temperature metal brazing filler, ceramic, glass, resin, hot-melt adhesive, or a composite thereof. The material of the adhesive is not limited in the present disclosure. The formed grinding structural member M1 is disposed on the bonding surface 41 of the base 4, with the adhesive layer 5 located between the base 4 and the grinding structural member M1. Subsequently, a high-temperature and high-pressure bonding process is performed. It should be noted that, if a high temperature is not applied, a prolonged time is required for the adhesive layer 5 to cure. Thereafter, the pressing plate P is provided to press the grinding structural member M1, such that a portion of the adhesive layer 5 infiltrates into the second porous structural layer 213 (in which pores of the second porous structural layer 213 also facilitate capillary action to promote infiltration of the adhesive layer 5), thereby fixing the grinding structural member M1 to the base 4 via the adhesive layer 5 to form a conditioner D1.
[0052] Furthermore, the second infiltrated composite layer 21 includes an upper layer portion 211 and a lower layer portion 212. The upper layer portion 211 is a portion infiltrated by the metal brazing filler B, and the lower layer portion 212 is a portion not infiltrated by the metal brazing filler B and serving as a compressible elastic layer. As shown in FIG. 5, when the grinding structural member M1 is fixed to the base 4 by the adhesive layer 5, the lower layer portion 212 is compressed by pressure applied via the pressing plate P so as to reduce its thickness, while the upper layer portion 211 maintains its original thickness due to infiltration by the metal brazing filler B. Since the lower layer portion 212 is compressed, a porosity of the lower layer portion 212 is smaller than a porosity of the upper layer portion 211.
[0053] Reference is made to FIG. 6, which is a schematic view of another implementation of the conditioner according to the first embodiment of the present disclosure. In other embodiments, a periphery of the bonding surface 41 of the base 4 can be provided with a limiting wall 42, and the limiting wall 42 and the bonding surface 41 jointly define an accommodating cavity. The grinding structural member M1 is disposed in the accommodating cavity and is fixed by the adhesive layer 5, so as to prevent displacement during bonding and to avoid adhesive overflow.
[0054] Since warpage degree and direction of the grinding structural member M1 are controlled by the configuration of the second infiltrated composite layer 21, when the pressing plate P flattens and bonds the grinding structural member M1 to the base 4, the grinding surface 111 and the first abrasive particles 12 of the grinding structural member M1 are subjected to enhanced surface compressive stresses, thereby being less prone to cracking. Even if original brazing microcracks exist in the structure (e.g., microcracks formed at brazed surfaces of the first abrasive particles 12), due to the grinding surface 111 and the first abrasive particles 12 bearing the enhanced compressive stresses, microcracks with residual compressive stress at brazed surface layers of the abrasive particles tend to remain as closed cracks rather than open cracks, such that crack propagation or formation of additional new cracks is prevented.Second Embodiment
[0055] Reference is made to FIGS. 7 and 8. FIG. 7 is a schematic view of grinding structural layer according to a second embodiment of the present disclosure. FIG. 8 is a schematic view of a conditioner according to the second embodiment of the present disclosure. A grinding structural member M2 includes a grinding structural layer 1, a supporting structural layer 2, and a brazing layer 3. The brazing layer 3 is disposed between the grinding structural layer 1 and the supporting structural layer 2. The grinding structural layer 1 includes a first infiltrated composite layer 11 and a plurality of first abrasive particles 12. The supporting structural layer 2 includes a second infiltrated composite layer 21. A conditioner D2 includes the grinding structural member M2, a base 4, and an adhesive layer 5. As shown in FIG. 8, the grinding structural member M2 is fixed to the base 4 by the adhesive layer 5.
[0056] The grinding structural member M2 and the conditioner D2 of the second embodiment (shown in FIGS. 7 and 8) have a structure similar to that of the first embodiment (shown in FIGS. 1 and 5), and will not be reiterated herein. The main difference between the first embodiment and the second embodiment is as follows. The supporting structural layer 2 of the grinding structural member M2 further includes a plurality of second abrasive particles 22. As shown in FIG. 7, the plurality of second abrasive particles 22 are dispersedly embedded in a lower surface of the second infiltrated composite layer 21, and each of the second abrasive particles 22 is partially exposed. In addition, the second abrasive particles 22 can include single-crystal diamond, polycrystalline diamond, polycrystalline diamond compact (PCD), CVD diamond, diamond, cubic boron nitride (cBN) particles, silicon carbide particles, or any combination thereof.
[0057] Specifically, when the first abrasive particles 12 are relatively large (e.g., having a particle size greater than 0.5 mm) and in a relatively large quantity, the thickness of the first infiltrated composite layer 11 cannot be too thin, for example, thinner than 0.3 mm. Assuming that the first infiltrated composite layer 11 has a porosity of 30% after compression, a relatively thicker metal brazing filler B is required, so that the metal brazing filler B infiltrates into the first infiltrated composite layer 11 to reach capillary saturation, thereby effectively bonding the abrasive particles. However, when the first abrasive particles 12 are relatively large, the first abrasive particles 12 dissipate heat more rapidly (the first abrasive particles 12 being made of diamond and having superior thermal conductivity), which may cause the side of the first infiltrated composite layer 11 on which the first abrasive particles 12 are provided to contract at a faster rate, thereby inducing reverse warpage. Accordingly, in the grinding structural member M2 of the present disclosure, a plurality of second abrasive particles 22 can be further embedded in the lower surface of the second infiltrated composite layer 21 to balance thermal stress. In addition, a total volume of the second abrasive particles 22 embedded in the second infiltrated composite layer 21 may be greater than a total volume of the first abrasive particles 12 embedded in the first infiltrated composite layer 11, such that the second infiltrated composite layer 21 can dissipate heat more rapidly and have a greater volumetric contraction.Third Embodiment
[0058] Reference is made to FIGS. 9 and 10. FIG. 9 is a schematic view of a grinding structural layer according to a third embodiment of the present disclosure. FIG. 10 is a schematic view of a conditioner according to the third embodiment of the present disclosure. A grinding structural member M3 includes a grinding structural layer 1, a supporting structural layer 2, and a brazing layer 3. The brazing layer 3 is disposed between the grinding structural layer 1 and the supporting structural layer 2. The grinding structural layer 1 includes a first infiltrated composite layer 11 and a plurality of first abrasive particles 12. A conditioner D3 includes the grinding structural member M3, a base 4, and an adhesive layer 5. The grinding structural member M3 is fixed to the base 4 by the adhesive layer 5.
[0059] The grinding structural member M3 and the conditioner D3 of the third embodiment (shown in FIGS. 9 and 10) have a structure similar to that of the first embodiment (shown in FIGS. 1 and 5), and will not be reiterated herein. The main difference between the first embodiment and the third embodiment is as follows. The supporting structural layer 2 of the grinding structural member M3 further includes a support plate 23 instead of the second infiltrated composite layer 21 of the second embodiment, and the second bonding surface 20 is a surface of the support plate 23.
[0060] Specifically, when the first abrasive particles 12 are relatively large (e.g., having a particle size greater than 0.5 mm) and in a relatively large quantity, the thickness of the first infiltrated composite layer 11 cannot be too thin, for example, thinner than 0.3 mm. Assuming that the first infiltrated composite layer 11 has a porosity of 30% after compression, a relatively thicker metal brazing filler B is required, so that the metal brazing filler B infiltrates into the first infiltrated composite layer 11 to reach capillary saturation, thereby effectively bonding the abrasive particles. However, when the first abrasive particles 12 are relatively large, the first abrasive particles 12 dissipate heat more rapidly (the first abrasive particles 12 being made of diamond and having superior thermal conductivity), which may cause the side of the first infiltrated composite layer 11 on which the first abrasive particles 12 are provided to contract at a faster rate, thereby inducing reverse warpage. Accordingly, in the grinding structural member M3 of the present disclosure, the support plate 23 can be further disposed on the other side of the brazing layer 3 (i.e., a side opposite to the side on which the first infiltrated composite layer 11 is provided). The support plate 23 can be a thin metal sheet, and may be made of, for example, stainless steel (SUS316), and have a thickness of, for example, 0.1 mm. Since the support plate 23 has a relatively large coefficient of thermal expansion and high rigidity, the support plate 23 exhibits a relatively large contraction during cooling. Accordingly, the grinding structural member M3 can utilize the support plate 23 to control an overall degree of warpage.Beneficial Effects of the Embodiments
[0061] In the grinding structural members M1 to M3, the conditioners D1 to D3, and the manufacturing methods thereof provided by the present disclosure, the grinding structural layer 1, the supporting structural layer 2, and the brazing layer 3 jointly form the grinding structural members M1 to M3. One side of the brazing layer 3 is the grinding structure layer 1 having a low coefficient of thermal expansion, and the other side of the brazing layer 3 is the supporting structure layer 2 having a high coefficient of thermal expansion, thereby controlling a degree of warpage of the grinding structural members M1-M3 after brazing to achieve an intended direction and magnitude. Accordingly, the degree of warpage of the grinding structural members M1 to M3 after brazing can be controlled to an intended direction and magnitude.
[0062] Furthermore, in order to improve warpage or waviness that may occur in the grinding structural member after forming, the grinding structural member M1 of the present disclosure further includes a supporting structure layer 2, namely, the second infiltrated composite layer 21. The second infiltrated composite layer 21 can increase the rigidity of the grinding structural member M1 and reduce a tendency to form a wavy profile after cooling and solidification. In addition, as shown in FIG. 1, since the second infiltrated composite layer 21 is also infiltrated by the molten metal brazing filler B (i.e., the second portion B2), in other words, an amount of the metal brazing filler B forming the brazing layer 3 is reduced, a thickness of the brazing layer 3 is decreased. As the brazing layer 3 becomes thinner, a volumetric shrinkage generated during cooling and solidification becomes smaller (and a resulting tensile stress is reduced), thereby decreasing an extent of warpage and increasing flexibility of the grinding structural member M1.
[0063] The foregoing description of the exemplary embodiments of the disclosure has been presented only for the purposes of illustration and description and is not intended to be exhaustive or to limit the disclosure to the precise forms disclosed. Many modifications and variations are possible in light of the above teaching.
[0064] The embodiments were chosen and described in order to explain the principles of the disclosure and their practical application so as to enable others skilled in the art to utilize the disclosure and various embodiments and with various modifications as are suited to the particular use contemplated. Alternative embodiments will become apparent to those skilled in the art to which the present disclosure pertains without departing from its spirit and scope.
Claims
1. A grinding structural member, comprising:a grinding structural layer, including:a first infiltrated composite layer having a grinding surface and a first bonding surface that are opposite to each other; anda plurality of first abrasive particles dispersedly embedded in the grinding surface of the first infiltrated composite layer, wherein each of the first abrasive particles is partially exposed on the grinding surface;a supporting structural layer having a second bonding surface, wherein the second bonding surface faces the first bonding surface; anda brazing layer disposed between the first bonding surface and the second bonding surface, wherein the brazing layer is configured to bond the first infiltrated composite layer and the supporting structural layer.
2. The grinding structural member according to claim 1, wherein an equivalent coefficient of thermal expansion of the grinding structural layer is less than or equal to an equivalent coefficient of thermal expansion of the supporting structural layer.
3. The grinding structural member according to claim 1, wherein the first infiltrated composite layer includes a first porous structural layer and a portion of a metal brazing filler disposed within the first porous structural layer, the metal brazing filler infiltrates through to the first bonding surface, and bonds to the plurality of first abrasive particles.
4. The grinding structural member according to claim 3, wherein the supporting structural layer includes a second infiltrated composite layer, the second bonding surface is a surface of the second infiltrated composite layer, the second infiltrated composite layer includes a second porous structural layer and another portion of the metal brazing filler disposed within the second porous structural layer, and the metal brazing filler covers the second bonding surface of the second infiltrated composite layer; and wherein the brazing layer includes a portion of the metal brazing filler remaining outside the first infiltrated composite layer and the second infiltrated composite layer.
5. The grinding structural member according to claim 4, wherein an average thickness of the second infiltrated composite layer is greater than an average thickness of the first infiltrated composite layer.
6. The grinding structural member according to claim 4, wherein the supporting structural layer further includes a plurality of second abrasive particles dispersedly embedded in the second infiltrated composite layer, and each of the second abrasive particles is partially exposed on the second infiltrated composite layer.
7. The grinding structural member according to claim 1, wherein the supporting structural layer includes a support plate, and the second bonding surface is a surface of the support plate.
8. A conditioner, comprising:a base; anda grinding structural member, including:a grinding structural layer, including:a first infiltrated composite layer having a grinding surface and a first bonding surface that are opposite to each other; anda plurality of first abrasive particles dispersedly embedded in the grinding surface of the first infiltrated composite layer, wherein each of the first abrasive particles is partially exposed on the grinding surface;a supporting structural layer having a second bonding surface, wherein the second bonding surface faces the first bonding surface; anda brazing layer disposed between the first bonding surface and the second bonding surface, wherein the brazing layer is configured to bond the first infiltrated composite layer and the supporting structural layer; wherein the first infiltrated composite layer includes a first porous structural layer and a portion of a metal brazing filler disposed within the first porous structural layer, the metal brazing filler infiltrates through to the first bonding surface, and bonds to the plurality of first abrasive particles;wherein the supporting structural layer includes a second infiltrated composite layer, the second bonding surface is a surface of the second infiltrated composite layer, the second infiltrated composite layer includes a second porous structural layer and another portion of the metal brazing filler disposed within the second porous structural layer, and the metal brazing filler covers the second bonding surface of the second infiltrated composite layer; and wherein the brazing layer includes a portion of the metal brazing filler remaining outside the first infiltrated composite layer and the second infiltrated composite layer.
9. The conditioner according to claim 8, wherein the second infiltrated composite layer includes an upper layer portion and a lower layer portion, the upper layer portion is a portion that is infiltrated by the metal brazing filler, and the lower layer portion is a portion that is not infiltrated by the metal brazing filler.
10. The conditioner according to claim 9, further comprising an adhesive layer disposed between the base and the grinding structural member, wherein the adhesive layer is configured to bond the base and the grinding structural member, and a portion of the adhesive layer infiltrates into the lower layer portion of the second infiltrated composite layer.
11. The conditioner according to claim 8, wherein at least half of a volume of each of the first abrasive particles is embedded in the grinding surface of the first infiltrated composite layer.
12. The conditioner according to claim 8, wherein a thickness of the first infiltrated composite layer ranges from 0.05 mm to 0.5 mm, a thickness of the second infiltrated composite layer ranges from 0.1 mm to 1 mm, and a thickness of the brazing layer ranges from 0.005 mm to 0.1 mm.
13. The conditioner according to claim 8, wherein a porosity of the first infiltrated composite layer ranges from 10% to 50%, and a porosity of the second infiltrated composite layer ranges from 20% to 95%.