Calcium-based flux-cored wire for metallurgical treatment of a metal bath and corresponding method
The cored wire with a calcium-containing extruded bar and lime aluminate intermediate layer addresses low calcium yield and nozzle clogging issues, enhancing steel quality through improved thermal protection and inclusion miscibility.
Patent Information
- Application Number
- US19/113789
- Authority / Receiving Office
- US · United States
- Patent Type
- Applications(United States)
- Current Assignee / Owner
- Priority Date
- 2022-09-22
- Filing Date
- 2023-09-21
- Publication Date
- 2026-11-12
AI Technical Summary
Existing cored wires for calcium treatment in molten steel suffer from low calcium addition yield and risk of nozzle clogging due to low vaporization temperature and non-miscible micro-inclusions.
A cored wire design featuring an extruded bar containing calcium and an intermediate layer with lime aluminate powder, including dodecacalcium hepta-aluminate phase, to enhance calcium addition yield and reduce nozzle clogging.
Improves calcium addition yield and reduces the risk of nozzle clogging by enhancing thermal protection and inclusion miscibility, resulting in improved steel quality.
Smart Images

Figure US20260357363A1-D00000_ABST
Abstract
Description
BACKGROUND OF THE DISCLOSUREField of the Disclosure
[0001] The present invention relates to a cored wire intended to be introduced into a bath of molten metal to perform a metallurgical treatment, the cored wire comprising a core extending locally along a longitudinal axis, and an outer casing extending longitudinally around the core.
[0002] The invention also relates to a metallurgical treatment method implementing such a cored wire.Description of Related Art
[0003] The molten metal is, for example, steel. The metallurgical treatment aims, for example, to add to the molten metal at least one substance intended to adjust the composition of the molten metal and / or the composition of the precipitates or non-metallic inclusions it contains.
[0004] In metallurgy, it is known to introduce such a substance using cored wires presented in the form of coils. The cored wire generally consists of a core containing the active substance in powder form, enclosed in a metal casing made of a metal whose composition is compatible with that of the molten metal to be treated. In the case of treating molten steel, this casing is itself advantageously made of steel.
[0005] The cored wire is introduced into the bath of molten metal using an injection device, usually automatic, introducing a precise length of cored wire at an appropriate speed.
[0006] For example, it is known to treat steels with calcium. This treatment aims in particular to modify the chemical composition of endogenous inclusions of the alumina type resulting from the deoxidation of steel, in order to obtain inclusions that are liquid at the casting temperature. These liquid inclusions do not adhere to the walls of the nozzles of a ladle or the distributor of a continuous casting installation. The castability is thus improved, as is the final quality of the steel produced, which depends on the micro-inclusion cleanliness of the steel, measurable by the cumulative surface area of micro-inclusions in a cross-section of the steel.
[0007] There are many types of cored wires whose core consists of pure calcium powder or calcium alloy, or a mixture of calcium and iron powders, or even aluminum. The alloy commonly called CaSi (calcium disilicide) or the mixture of calcium and iron powders (generally called CaFe), for example, are widely used cores.
[0008] Although the introduction of a cored wire into the bath of molten metal is an ingenious means of adding the active substance to the molten metal, the efficiency of the introduction is sometimes limited. For example, for CaFe-based cored wires used in steelmaking, the calcium addition yield, defined as the amount of calcium found in the steel after the injection of the cored wire divided by the amount of calcium introduced by the consumed cored wire, is generally around 10% to 15%, sometimes much less. The low efficiency of calcium is mainly due to its low vaporization temperature. Indeed, around 1480 °C, this is generally lower than the working temperature of liquid steel, which causes the calcium to vaporize while being introduced into the liquid steel.
[0009] To at least partially remedy this problem and improve the calcium addition yield, cores comprising an extruded bar mainly containing calcium, and an intermediate layer extending longitudinally between the extruded bar and the outer casing, the intermediate layer comprising a powder containing a metal, a mixture of metals, a metal oxide, or a mixture of metal oxides, have been proposed. Document EP 2 917 377 describes this type of cored wire.
[0010] However, it has been observed that non-miscible micro-inclusions in steel at the casting temperature persist, creating a risk of nozzle clogging and limiting the final quality of the steel.
[0011] An object of the invention is to provide a cored wire for performing a calcium treatment with good addition yield, while further reducing the risk of nozzle clogging and improving the final quality of the steel.BRIEF SUMMARY OF THE DISCLOSURE
[0012] To this end, the invention relates to a cored wire intended to be introduced into a bath of molten metal to perform a metallurgical treatment, the cored wire comprising a core extending locally along a longitudinal axis, and an outer casing extending longitudinally around the core, the core comprising:
[0013] an extruded bar mainly containing calcium, and
[0014] an intermediate layer extending longitudinally between the extruded bar and the outer casing, the intermediate layer comprising a powder containing one or more of: a metal, a mixture of metals, a metal oxide, a mixture of metal oxides,
[0015] the powder contains at least 10% by mass of lime aluminate, the lime aluminate containing at least the dodecacalcium hepta-aluminate phase.
[0016] According to particular embodiments, the cored wire comprises one or more of the following features, taken alone or in any technically possible combination:
[0017] the lime aluminate further contains one and / or the other of the tricalcium aluminate and monocalcium aluminate phases;
[0018] the powder contains at least 50% by mass of lime aluminate;
[0019] the lime aluminate contains at least 5% by mass of dodecacalcium hepta-aluminate;
[0020] the lime aluminate comprises at least 50% by mass of dodecacalcium hepta-aluminate;
[0021] the core further comprises a thermally insulating layer extending longitudinally between the extruded bar and the intermediate layer;
[0022] the extruded bar has an external equivalent diameter D1 in a transverse plane substantially perpendicular to the longitudinal axis, the intermediate layer having an external equivalent diameter D2 in the transverse plane, with D2 between 1.3 times and 6.2 times D1;
[0023] the outer casing comprises a strip of steel, aluminum, copper, nickel, or zinc, or an alloy of two or more of these elements; and
[0024] the powder further comprises one or more of: iron powder, fluorine powder, and iron-silicon alloy powder.
[0025] By “equivalent diameter” of an element, it is meant the diameter of a disk with an area equal to the area presented by the element in cross-section according to a transverse plane. If the given element has a circular cross-section according to the transverse plane, the equivalent diameter is equal to the ordinary diameter.
[0026] When the notion of equivalent diameter is used for an element, it is implicit that the element is locally substantially cylindrical, but not necessarily circular-based.
[0027] By “metallurgical treatment,” it is meant, for example:
[0028] a modification of the chemical composition of the molten metal, and / or
[0029] a modification of the properties of the metal obtained after solidification of the molten metal due, for example, to the modification of the composition of the inclusions or precipitates present before the treatment, or to the creation, following the treatment, of such inclusions or precipitates, and / or
[0030] a modification of the inclusion population present in the liquid metal to improve its elaboration (improvement of castability in continuous casting).
[0031] The invention also relates to a metallurgical treatment method of a bath of molten metal, the method comprising the step of introducing a cored wire into the molten metal bath.
[0032] According to a particular embodiment, the molten metal is steel.BRIEF DESCRIPTION OF THE SEVERAL VIEWS OF THE DRAWING(S)
[0033] The invention will be better understood by reading the following description, given solely by way of example, and made with reference to the appended drawings, in which:
[0034] FIG. 1 schematically represents, in perspective, a cored wire according to the invention, and
[0035] FIG. 2 schematically represents, in cross-section, the cored wire represented in FIG. 1.DETAILED DESCRIPTION OF THE DISCLOSURE
[0036] Referring to FIGS. 1 and 2, a cored wire 1 according to the invention is described.
[0037] The cored wire 1 extends locally along a longitudinal axis L. Only a portion of the cored wire 1 is represented. The represented portion extends along the longitudinal axis L. This does not mean that the entire cored wire 1 extends along the longitudinal axis L. Indeed, the cored wire 1 may have some curvature, for example, if it is wound to occupy less space.
[0038] Similarly, a transverse plane P perpendicular to the longitudinal axis L is defined. It is understood that the transverse plane P is transverse for the portion of the cored wire 1 represented, i.e., locally transverse.
[0039] The cored wire 1 is, for example, intended to be introduced into a molten steel bath (not represented).
[0040] The cored wire 1 comprises a core 2 and an outer casing 4, both extending longitudinally.
[0041] The outer casing 4 forms a peripheral portion of the cored wire 1, intended to be in contact with the molten metal bath when the cored wire 1 is introduced into the molten metal bath.
[0042] The outer casing 4 is advantageously made of a metal strip 6 folded over itself around the longitudinal axis L.
[0043] The outer casing 4, for example, has a thickness of about 0.4 mm.
[0044] The strip 6 is, for example, made of steel, copper, aluminum, nickel, or zinc, or a mixture of two or more of these elements.
[0045] The strip 6 advantageously comprises two longitudinal folds 6a, 6b (FIG. 2) stapled to each other to close the strip 6 on itself along the longitudinal axis L. The strip 6, thus folded, has a generally tubular shape that envelops the core 2. Advantageously, the tubular shape is substantially cylindrical with a circular base and has an equivalent diameter D. D is advantageously between 6 and 21 mm. For example, D is about 13 mm.
[0046] The core 2 comprises an extruded bar 8 extending longitudinally and an intermediate layer 10 extending longitudinally and radially between the extruded bar 8 and the outer casing 4.
[0047] The extruded bar 8 is advantageously substantially cylindrical with a circular base. The extruded bar 8 has a diameter D1 in the transverse plane P, with D1 advantageously between 2 and 10 mm, for example, 8 mm.
[0048] The extruded bar 8 contains calcium. Advantageously, the extruded bar 8 mainly contains calcium.
[0049] By “mainly,” it is meant, for example, that the extruded bar 8 contains at least 50% by mass of calcium, preferably at least 90% by mass of calcium.
[0050] In the example, the extruded bar 8 is made of industrial purity calcium, for example, 98.5% by weight.
[0051] The extruded bar 8 is not a simple mass of compacted powder material during the closing of the cored wire 1, nor even an agglomerate of powder grains (powder material) bound together by a binder of any kind. The extruded bar 8 is, for example, obtained by extruding a solid cylinder (billet) of material through a die using a press. The extruded bar 8 can also be obtained directly by a continuous casting method, the liquid material being solidified in the form of a continuous bar. The porosity of the extruded bar 8 is considered almost nil, the apparent density of the bar being close to the true density of the material.
[0052] The extruded bar 8, for example, has a metric weight of about 85 g / m and a diameter D1 of about 8.5 mm.
[0053] The intermediate layer 10 extends, for example, in the space between the extruded bar 8 and the outer casing 4.
[0054] The intermediate layer 10 has an external equivalent diameter D2. D2 is, for example, such that the ratio D2 / D1 is between 1.3 and 6.2.
[0055] The intermediate layer 10 is advantageously made of a powder.
[0056] The intermediate layer 10 is, for example, made of a powder containing one or more of: a metal, a mixture of metals, a metal oxide, a mixture of metal oxides.
[0057] The powder contains at least 10% by mass of lime aluminate, the lime aluminate containing at least the dodecacalcium hepta-aluminate phase, and possibly one and / or the other of the tricalcium aluminate and monocalcium aluminate phases.
[0058] Lime aluminate (or calcium aluminate) is generally obtained by calcining a mixture of calcium oxide CaO and aluminum oxide Al2O3. Under normal temperature and pressure conditions (101325 Pa, 25 °C), depending on the mass fraction of Al2O3 in the initial mixture, lime aluminate can present in the following stable phases:
[0059] tricalcium aluminate: 3CaO·Al2O3, also noted C3A in the field of metallurgy, where C=CaO and A=Al2O3;
[0060] dodecacalcium hepta-aluminate: 12CaO·7Al2O3 or C12A7, also called mayenite;
[0061] monocalcium aluminate: CaO·Al2O3 or CA;
[0062] monocalcium dialuminate: CaO·2Al2O3 or CA2;
[0063] monocalcium hexa-aluminate: CaO·6Al2O3 or CA6.
[0064] According to the binary Al2O3—CaO diagram, the stability domains of the C3A+C12A7, CA12A7, and C12A7+CA phases correspond to mass fractions of Al2O3 between about 38% and 64% in the initial mixture. For these proportions, the temperature at which the first drop of liquid appears (solidus) is below 1500 °C at atmospheric pressure.
[0065] The presence of these phases is advantageously determined by X-ray diffraction, with a relative precision of + / −5% for mass quantification.
[0066] Advantageously, the powder contains at least 50% by mass of lime aluminate. In a particular case, the powder consists of lime aluminate, advantageously only in the form described above.
[0067] Advantageously, the lime aluminate comprises at least 5% by mass of dodecacalcium hepta-aluminate, preferably at least 50% by mass of dodecacalcium hepta-aluminate.
[0068] In a particular case, the lime aluminate contains at least 80% by mass of dodecacalcium hepta-aluminate.
[0069] For example, the intermediate layer 10 further comprises one or more of: iron powder, fluorine powder, and iron-silicon alloy powder, advantageously forming the complement to 100%.
[0070] According to a particular embodiment, among these powders, the intermediate layer 10 comprises at least the iron powder, and possibly one or two of the other powders.
[0071] The iron powder improves the rigidity of the cored wire 1 and makes it easier to inject into the steel bath, notably by facilitating the crossing of the slag layer.
[0072] The fluorine powder advantageously lowers the solidus temperature (temperature at which the first drop of liquid appears) and / or the liquidus temperature (temperature at which the lime aluminate is completely melted) of the lime aluminate contained in the intermediate layer 10.
[0073] The iron-silicon alloy powder advantageously reduces the reactivity of the calcium in the extruded bar 8 with the steel bath.
[0074] Finally, to confer maximum metallurgical treatment efficiency to the cored wire 1, the diameter ratio D2 / D1 is between 1.3 and 6.2. This interval has been determined based on the following criteria.
[0075] For the intermediate layer 10 to be sufficiently insulating, it must be thick enough. Therefore, the space between the extruded bar 8 and the outer casing 4 must be large enough to contain the powder. A D2 / D1 ratio greater than or equal to 1.3 guarantees the minimum space for the thermal protection of the powder in the intermediate layer 10 to be sufficient.
[0076] A D2 / D1 ratio less than or equal to 6.2 is based on both metallurgical and economic considerations. It ensures a minimum proportion of active substance (extruded bar 8) relative to the insulating substance. Too much imbalance causes significant thermal losses of the liquid metal bath to be treated (too much powder input compared to the active substance input), but also an increase in the cost of the cored wire.
[0077] The core 2 can also include a thermally insulating layer 12 covering the bar 8.
[0078] In the present application, “thermally insulating layer” means an additional layer around the extruded bar 8. The additional layer delays the heat transfer from the outside of the cored wire 1 to its core when the cored wire is introduced into a liquid metal bath. The additional layer is adapted to constitute an additional thermal barrier between the external environment of the cored wire (liquid metal) and the extruded bar. The propagation of heat is slowed down due to the presence of the additional layer. The temperature rise of the extruded bar is thus delayed.
[0079] The insulating layer 12, for example, comprises paper, moistened paper, metallized paper, or metal. The insulating layer allows adjusting the overall thermal transfer coefficient between the bathe of molten metal and the extruded bar 8. Advantageously, the insulating layer 12 delays the complete melting of the cored wire 1.
[0080] Examples of thermally insulating layers are provided in the application FR-A-2871477 of the applicant.
[0081] The fact that the thermally insulating layer is advantageously located on the extruded bar 8 and surrounds it completely, for example, further improves the thermal protection of the extruded bar.
[0082] The cored wire 1 is, for example, intended to be introduced into a molten steel bath (not represented).EXAMPLE 1
[0083] Treatment of a 245-ton molten steel ladle.
[0084] Cored wire with a diameter of 13.6 mm comprising:
[0085] an extruded bar of industrial purity calcium, 8.5 mm in diameter, with a metric weight of 85 g / m,
[0086] an intermediate layer consisting of a lime aluminate powder comprising either the tricalcium aluminate and dodecacalcium hepta-aluminate phases, or the dodecacalcium hepta-aluminate and monocalcium aluminate phases, with at least 50% by mass of dodecacalcium hepta-aluminate in each of these two cases,
[0087] a steel strip with a thickness of 0.40 mm.EXAMPLE2
[0088] Treatment of a 320-ton molten steel ladle, for example, of a grade with silicon content restriction (% Si<300 ppm).
[0089] Cored wire with a diameter of 13.6 mm comprising:
[0090] an extruded bar of industrial purity calcium, 7.5 mm in diameter, with a metric weight of 70 g / m,
[0091] an intermediate layer consisting of a mixture of 50% by mass of lime aluminate powder and 50% by mass of iron powder, the lime aluminate comprising 75% by mass of dodecacalcium hepta-aluminate and 25% by mass of one or more other phases of lime aluminate,
[0092] a steel strip with a thickness of 0.50 mm.
[0093] The micro-inclusion counting results were obtained using an automated scanning electron microscope associated with an EDS analyzer (Energy Dispersive Spectroscopy) that determines the chemical composition of each inclusion detected by image analysis, on a polished section for an analyzed surface of 30 mm2 , on samples taken from the distributor. The results show a decrease in the number and size of oxysulfide inclusions, compared to the same experiment conducted with a cored wire with a diameter of 13.6 mm comprising:
[0094] an extruded bar of industrial purity calcium, 8.5 mm in diameter, with a metric weight of 85 g / m,
[0095] an intermediate layer consisting of iron powder (without lime aluminate powder), and
[0096] a steel strip with a thickness of 0.50 mm.
[0097] More specifically, the number of oxysulfide micro-inclusions is 20 inclusions per mm2, and the maximum size of detected inclusions is 5 μm in the case of the cored wire comprising lime aluminate powder in the intermediate layer, compared to 40 inclusions per mm2 and a maximum size of detected inclusions of 8 μm in the case of the cored wire not comprising lime aluminate powder in the intermediate layer.
[0098] These results demonstrate the effect of lime aluminate powder on improving the micro-inclusion cleanliness of steels treated with the cored wire described in example 2.ADVANTAGES
[0099] Thanks to the features described above, notably the presence of lime aluminate containing at least the dodecacalcium hepta-aluminate phase, and possibly one and / or the other of the tricalcium aluminate and monocalcium aluminate phases, advantageously with dodecacalcium the hepta-aluminate being the majority in mass fraction in the lime aluminate, the cored wire 1 allows a calcium treatment of steel with a reduction in the cumulative surface area of micro-inclusions (non-metallic particles not miscible in steel at the steel liquid treatment temperature). This improves the final quality of the steel while reducing the risk of nozzle clogging by non-liquid particles during production.
Claims
1. A cored wire intended to be introduced into a bath of molten metal to perform a metallurgical treatment, the cored wire comprising a core extending locally along a longitudinal axis, and an outer casing extending longitudinally around the core, the core including:an extruded bar mainly containing calcium, andan intermediate layer extending longitudinally between the extruded bar and the outer casing, the intermediate layer comprising a powder containing one or more of: a metal, a mixture of metals, a metal oxide, a mixture of metal oxides,wherein the powder contains at least 10% by mass of lime aluminate, the lime aluminate containing at least the dodecacalcium hepta-aluminate phase.
2. The cored wire according to claim 1, wherein the lime aluminate further contains one or the other of the tricalcium aluminate and monocalcium aluminate phases.
3. The cored wire according to claim 1, wherein the powder contains at least 50% by mass of lime aluminate.
4. The cored wire according to claim 1, wherein the lime aluminate contains at least 5% by mass of dodecacalcium hepta-aluminate.
5. The cored wire according to claim 4, wherein the lime aluminate comprises at least 50% by mass of dodecacalcium hepta-aluminate.
6. The cored wire according to claim 1, wherein the core further comprises a thermally insulating layer extending longitudinally between the extruded bar and the intermediate layer7. The cored wire according to claim 1, wherein the extruded bar has an external equivalent diameter D1 in a transverse plane substantially perpendicular to the longitudinal axis, the intermediate layer having an external equivalent diameter D2 in the transverse plane, with D2 between 1.3 times and 6.2 times D1.
8. The cored wire according to claim 1, wherein the outer casing comprises a strip of steel, aluminum, copper, nickel, or zinc, or an alloy of two or more of these elements.
9. The cored according to claim 1, wherein the powder further comprises one or more of: iron powder, fluorine powder, and iron-silicon alloy powder.
10. A metallurgical treatment method of a bath of molten metal, the method comprising the step of introducing a cored wire according to claim 1 into the bath of molten metal.
11. The method according to claim 10, wherein the molten metal is steel.