Secondary battery and electronic apparatus
By setting grooves on the surface of the negative electrode sheet of the lithium-ion battery and regulating the thickness of the separator adhesive layer, the internal heat dissipation performance of the battery is optimized, the problems of cycle attenuation and thermal runaway of the lithium-ion battery are solved, and its high-temperature cycle stability and safety are improved.
Patent Information
- Application Number
- PCT/CN2023/074396
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-02-03
- Publication Date
- 2024-10-24
AI Technical Summary
During repeated charge and discharge cycles, lithium-ion batteries accelerate cycle decay due to stress deformation, and heat accumulation increases the risk of thermal runaway, affecting their cycle stability and safety.
By setting grooves on the surface of the negative electrode plate and adjusting the thickness of the separator adhesive layer, the groove depth, width, spacing and adhesive layer thickness are optimized to improve the conduction effect of electrolyte and high-temperature gas, enhance heat dissipation capacity, and reduce the risk of thermal runaway and Cyclic deformation problem.
It improves the cycle stability and safety of lithium-ion batteries at high temperatures, extends battery life, and reduces the risk of thermal runaway.
Smart Images

Figure CN2023074396_24102024_PF_FP_ABST
Abstract
Description
Secondary battery and electronic device Technical Field
[0001] The present application relates to the field of electrochemical technology, and in particular to a secondary battery and an electronic device. Background Art
[0002] Secondary batteries, such as lithium-ion batteries, have a wide range of applications in consumer electronics due to their high specific energy, high operating voltage, low self-discharge rate, compact size, and light weight. With the widespread use of lithium-ion batteries, the market has placed increasingly higher demands on their performance.
[0003] During repeated charge and discharge cycles, lithium-ion batteries accumulate internal stress, causing deformation. This can lead to problems such as excessive thickness and accelerated cycle decay, impacting the battery's cycling stability. Furthermore, as heat accumulates within the battery during cycling, if this heat cannot be dissipated promptly, it increases the risk of thermal runaway, impacting the battery's safety.
[0004] Summary of the Invention
[0005] The purpose of this application is to provide a secondary battery and an electronic device with good cycle stability and safety.
[0006] It should be noted that in the application content, lithium-ion batteries are used as an example of secondary batteries to explain this application, but the secondary batteries of this application are not limited to lithium-ion batteries. The specific technical solutions are as follows:
[0007] In a first aspect, the present application provides a secondary battery, which includes an electrode assembly, wherein the electrode assembly includes a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator is arranged between the positive electrode sheet and the negative electrode sheet, and the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer, wherein the surface of the negative electrode active material layer opposite to the positive electrode sheet has a groove, and the depth of the groove is Hμm; the separator includes a substrate layer and a bonding layer arranged on the surface of the separator opposite to the negative electrode sheet, and the thickness of the bonding layer is Tμm, satisfying: H≥T+1. Preferably, H≥T+5. The present application can improve the conductive effect of the groove on the electrolyte and the high-temperature gas generated under high temperature conditions by regulating the depth of the groove and the thickness of the bonding layer to meet the scope of the present application, thereby increasing the heat dissipation capacity inside the secondary battery and improving the high-temperature performance of the secondary battery.
[0008] In some embodiments of the present application, the cross-sectional area of the groove is A μm 2, the width of the groove is W μm, satisfying: 0.35×(W×H) < A < 0.95(W×H), 5 ≤ H ≤ 100. Preferably, 0.55×(W×H) < A < 0.85(W×H). By adjusting the cross-sectional area of the groove, the interface morphology at the groove can be adjusted, thereby further improving the interface heat dispersion effect of the electrode sheet under high-temperature hot box conditions, improving the heat dissipation capacity inside the lithium-ion battery, and enhancing the cycle stability and safety of the lithium-ion battery at high temperatures.
[0009] In some embodiments of the present application, 1 ≤ W / H ≤ 40. Preferably, 2 ≤ W / H ≤ 20, which can further improve the heat dissipation capacity inside the lithium-ion battery and enhance the cycle stability and safety of the lithium-ion battery at high temperatures.
[0010] In some embodiments of the present application, the width of the groove is W μm, the spacing of the grooves is S μm, and the porosity of the negative electrode sheet is P%, satisfying: Preferably, Adjusting the porosity of the negative electrode sheet, the width of the groove, and the spacing of the grooves to satisfy the above relationships can effectively improve the heat balance of the electrode sheet under high-temperature conditions, enhance the heat diffusion efficiency in extreme environments, reduce the thermal runaway risk of the lithium-ion battery, improve the safety performance of the lithium-ion battery, and can also release the stress generated inside the lithium-ion battery during high-temperature cycling through the space provided by the groove, thereby improving the cycle deformation problem of the lithium-ion battery and enhancing the cycle stability of the lithium-ion battery.
[0011] In some embodiments of the present application, the spacing of the grooves is S μm, and the adhesion force between the separator and the negative electrode sheet is F N / m, satisfying: S ≤ 1000F, 500 ≤ S ≤ 10000. Preferably, S ≤ 650F. It can improve the heat dissipation capacity inside the lithium-ion battery, reduce the thermal runaway risk of the lithium-ion battery, and improve the safety performance of the lithium-ion battery.
[0012] In some embodiments of the present application, 0.1 ≤ T ≤ 10. By controlling the thickness of the adhesive layer within the above range, it is beneficial to improve the adhesion performance between the separator and the electrode sheet including the groove, thereby improving the safety performance of the lithium-ion battery.
[0013] In some embodiments of the present application, the adhesive layer includes a polymer. Based on the mass of the adhesive layer, the content of the polymer is 25% to 100%. Preferably, the content of the polymer is 30% to 100%. Further preferably, the content of the polymer is 50% to 100%. By controlling the content of the polymer within the above range, it is beneficial to improve the adhesion force at the separator interface, thereby improving the deformation problem of the lithium-ion battery and enhancing the cycle stability and safety of the lithium-ion battery at high temperatures.
[0014] In some embodiments of the present application, the bonding force between the separator and the negative electrode is FN / m, satisfying the following: 1 ≤ F ≤ 50. Preferably, 5 ≤ F ≤ 30. More preferably, 7 ≤ F ≤ 30. By regulating the bonding force between the separator and the negative electrode within the above range, the problem of cycling deformation in lithium-ion batteries can be improved, thereby enhancing the cycling stability of lithium-ion batteries.
[0015] In some embodiments of the present application, the polymer includes at least one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, styrene-butadiene copolymer, polyacrylonitrile, butadiene-acrylonitrile polymer, polyacrylic acid, polyacrylate or acrylate-styrene copolymer.
[0016] In some embodiments of the present application, the negative electrode sheet further includes a negative electrode tab, a first groove portion being provided along the length of the negative electrode tab, and a negative electrode active material layer being provided between the first groove portion and the negative electrode tab along the length of the negative electrode tab; wherein the distance between the first groove portion and the negative electrode tab is d mm, with 0.2 < d < 5. This design optimizes heat dissipation under high temperature conditions. Furthermore, the retention of the negative electrode active material layer between the groove portion and the tab region along the length of the negative electrode tab further improves ion conduction in the tab region, improves the regional electrochemical interface, and thus enhances the cycling performance of the secondary battery. Furthermore, the separation of the groove portion from the tab region avoids secondary processing of a localized region of the current collector, thereby improving the yield rate of the negative electrode sheet.
[0017] In a second aspect, the present application provides an electronic device comprising the secondary battery described in the aforementioned embodiment, thereby providing the electronic device with good high-temperature cycle stability and safety.
[0018] This application provides a secondary battery and electronic device, wherein the surface of the negative electrode active material layer opposite the positive electrode plate has a groove with a depth of H μm. The separator includes a substrate layer and an adhesive layer disposed on the surface of the separator opposite the negative electrode plate. The adhesive layer has a thickness of T μm, satisfying the following: H ≥ T + 1. By regulating the groove depth and adhesive layer thickness to meet the requirements of this application, this application can increase the heat dissipation capacity within the secondary battery and improve the high-temperature performance of the secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The drawings described herein are used to provide further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute improper limitations on the present application.
[0020] FIG1 is a schematic structural diagram of an electrode assembly in some embodiments of the present application;
[0021] FIG2 is a schematic diagram of a partial cross-sectional structure of an electrode assembly along its thickness direction in some embodiments of the present application;
[0022] FIG3 is a schematic diagram of a partial cross-sectional structure of a negative electrode sheet along its thickness direction in some embodiments of the present application;
[0023] FIG4 is a partial top view of a negative electrode sheet along its thickness direction in some embodiments of the present application;
[0024] FIG5 is a schematic diagram of a cross-sectional structure of a diaphragm along its thickness direction in some embodiments of the present application;
[0025] FIG6 is a schematic diagram of the cross-sectional structure of the diaphragm along its thickness direction in other embodiments of the present application;
[0026] FIG7 is a schematic diagram of the structure of the negative electrode sheet in some embodiments of the present application;
[0027] Figure 8 is a schematic diagram of groove profile determination and groove parameter measurement in some embodiments of the present application. Reference numerals: 10 - electrode assembly, 20 - positive electrode sheet, 21 - positive electrode current collector, 22 - positive electrode active material layer, 30 - negative electrode sheet, 31 - negative electrode current collector, 32 - negative electrode active material layer, 33 - negative electrode tab, 34 - hollow foil area, 40 - separator, 41 - substrate layer, 42 - inorganic coating layer, 43 - bonding layer, 321 - groove, 322 - first groove portion. DETAILED DESCRIPTION
[0028] To make the objectives, technical solutions, and advantages of this application more clearly understood, the present application is further described below with reference to the accompanying drawings and examples. It is apparent that the described examples are only some of the embodiments of the present invention, not all of them. All other embodiments derived by persons of ordinary skill in the art based on the examples in this application are intended to fall within the scope of protection of this application.
[0029] It should be noted that in the specific implementation, lithium-ion batteries are used as an example of secondary batteries to explain this application, but the secondary batteries of this application are not limited to lithium-ion batteries. The specific technical solution is as follows:
[0030] In the first aspect of the present application, a secondary battery is provided. As shown in FIG. 1, it includes an electrode assembly 10. Here, the X direction is the length direction of the electrode assembly 10 itself, the Y direction is the width direction of the electrode assembly 10 itself, and the Z direction is the thickness direction of the electrode assembly 10 itself. As shown in FIG. 2, the electrode assembly 10 includes a positive electrode sheet 20, a negative electrode sheet 30, and a separator 40. The separator 40 is disposed between the positive electrode sheet 20 and the negative electrode sheet 30. The positive electrode sheet 20 includes a positive current collector 21 and a positive active material layer 22. The negative electrode sheet 30 includes a negative current collector 31 and a negative active material layer 32. Among them, the surface of the negative active material layer 32 opposite to the positive electrode sheet 20 has a groove 321. As shown in FIG. 3, the depth of the groove is H μm. As shown in FIG. 5, the separator 40 includes a base material layer 41 and a bonding layer 43. The thickness of the bonding layer is T μm, satisfying: H≥T + 1. Preferably, H≥T + 5. In the present application, the bonding layer 43 can be the surface layer of the separator 40 opposite to the negative electrode sheet 30.
[0031] During the preparation process of the lithium-ion battery, due to the combined action of external pressure and the pressure generated by the expansion inside the electrode assembly, the polymer in the bonding layer of the separator is compressed to produce a bonding effect. At the groove, the bonding layer produces a local bonding effect with the groove after being stressed. However, an overly thick bonding layer will change the heat distribution inside the electrode assembly under high-temperature conditions and at the same time affect the heat dissipation effect of the groove, thereby affecting the improvement effect on the high-temperature heat box. The inventors have found that by regulating the depth of the groove and the thickness of the bonding layer to meet the scope of the present application, the present application can improve the heat dissipation effect of the high-temperature heat generated under high-temperature conditions by the groove, thereby improving the internal heat dissipation capacity of the lithium-ion battery and enhancing the high-temperature performance of the lithium-ion battery, such as improving the cycle stability and safety of the lithium-ion battery at high temperature. In the present application, the negative active material layer 32 can be provided on one side or both sides.
[0032] In some embodiments of the present application, the cross-sectional area of the groove is A μm 2 , the width of the groove is W μm, satisfying: 0.35×(W×H)<A<0.95(W×H), 5≤H≤100. Preferably, 0.55×(W×H)<A<0.85(W×H). By regulating C, W and H to satisfy the above relationship and coordinately regulating H within the above range, the adjustment of the interface morphology at the groove can be realized, thereby further improving the interface heat dissipation effect of the electrode sheet under the conditions of a high-temperature heat box, improving the internal heat dissipation capacity of the lithium-ion battery, and at the same time improving the electrochemical bonding between the separator bonding layer at the groove and the electrode sheet, enhancing the cycle stability and safety of the lithium-ion battery at high temperature.
[0033] In some embodiments of the present application, 1≤W / H≤40. Preferably, 2≤W / H≤20. By further regulating the relationship between W and H to satisfy the above relationship, the heat dissipation capacity within the lithium-ion battery can be further improved, thereby enhancing the cycling stability and safety of the lithium-ion battery at high temperatures.
[0034] In some embodiments of the present application, as shown in FIG3 and FIG4 , the width of the groove is W μm, the spacing between the grooves is S μm, and the porosity of the negative electrode sheet is P%, satisfying: Preferably, The inventors have found that the failure of a high-temperature hot box is mainly due to the contact between the surface of the active material layer of the negative electrode plate and the electrolyte, which causes side reactions under high temperature conditions. The heat generated by the side reactions accumulates inside the battery, increasing the risk of thermal runaway. The greater the porosity of the negative electrode plate, the larger the contact area between the negative electrode active material layer and the electrolyte, the more heat is generated, and the greater the risk of thermal runaway. In addition, the expansion space of the negative electrode plate with low porosity is small, and the lithium-ion battery will cause deformation problems due to expansion. Based on this, the present application adjusts the width of the groove, the spacing of the groove, and the porosity of the negative electrode plate to meet the above relationship, thereby improving the dispersion effect of the groove on the heat generated under high-temperature hot box conditions, improving the heat diffusion efficiency under extreme environments, reducing the risk of thermal runaway of lithium-ion batteries, and improving the safety performance of lithium-ion batteries. In addition, the grooves can effectively disperse the gas produced during high-temperature cycling, improve the interfacial electrochemical properties between the diaphragm and the plate, and improve the high-temperature cycling stability of lithium-ion batteries.
[0035] In some embodiments of the present application, the negative electrode of the lithium-ion battery satisfies 5 ≤ P ≤ 50. Preferably, 10 ≤ P ≤ 40. More preferably, 10 ≤ P ≤ 30. By regulating the above parameters within the scope of the present application, a lithium-ion battery with excellent high-temperature cycling stability and safety can be obtained.
[0036] In some embodiments of the present application, as shown in Figures 3 and 4, the spacing of the grooves is Sμm, and the bonding force between the diaphragm and the negative electrode plate is FN / m, satisfying: S≤1000F, 500≤S≤10000, preferably, S≤650F. The inventors have found that different types of diaphragms have different interface bonding properties. Diaphragms with high bonding properties have good deformation improvement effects on lithium-ion batteries, but the heat dissipation effect will be reduced. Based on this, the present application, by regulating the above-mentioned relationship between S and F, can also improve the conduction effect of the grooves on the high-temperature gas generated under high-temperature hot box conditions for diaphragms with different bonding properties, thereby improving the heat dissipation capacity inside the lithium-ion battery, reducing the risk of thermal runaway of the lithium-ion battery, and improving the safety performance of the lithium-ion battery.
[0037] In some embodiments of the present application, 0.1≤T≤10. By adjusting the thickness of the adhesive layer within the above range, the bonding performance between the separator and the electrode including the groove is improved, thereby improving the safety performance of the lithium-ion battery.
[0038] The bonding layer includes a polymer; wherein, based on the mass of the bonding layer, the content of the polymer is 25% to 100%, preferably, the content of the polymer is 30% to 100%. By regulating the content of the polymer within the above range, it is beneficial to improve the interfacial adhesion of the diaphragm, thereby improving the deformation problem of the lithium-ion battery and improving the cycle stability and safety of the lithium-ion battery at high temperatures.
[0039] In some embodiments of the present application, as shown in FIG5 , a bonding layer 43 is located on the surface of substrate layer 41 and comprises a polymer and an inorganic material. The synergistic effect of the above structural design and material selection helps to improve the interfacial adhesion of the separator, thereby improving the deformation problem of the lithium-ion battery and enhancing the cycling stability and safety of the lithium-ion battery at high temperatures.
[0040] In some embodiments of the present application, as shown in FIG6 , the separator further includes an inorganic coating 42, which is located between the substrate layer 41 and the bonding layer 43. The inorganic coating 42 includes an inorganic material, and the bonding layer 43 includes a polymer. The synergistic effect of the above structural design and material selection is conducive to improving the interfacial bonding strength of the separator, thereby improving the deformation problem of the lithium-ion battery and enhancing the cycling stability and safety of the lithium-ion battery at high temperatures.
[0041] In some embodiments of the present application, 1 ≤ F ≤ 50. Preferably, 5 ≤ F ≤ 30. More preferably, 7 ≤ F ≤ 30. By regulating the bonding force between the separator and the negative electrode within the above range, the problem of cyclic deformation of lithium-ion batteries can be improved, thereby enhancing the cyclic stability of lithium-ion batteries.
[0042] In some embodiments of the present application, the polymer includes at least one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, styrene-butadiene copolymer, polyacrylonitrile, butadiene-acrylonitrile polymer, polyacrylic acid, polyacrylate, or acrylate-styrene copolymer. When the separator includes the above polymers, it is beneficial to improve the interfacial bonding performance of the separator.
[0043] Referring to FIG7 , the negative electrode tab 33 is typically welded to the empty foil area 34 of the negative electrode sheet 30 (the area of the negative electrode sheet not coated with the negative electrode active material). The inventors have discovered that during the cycling of lithium-ion batteries, heat accumulation is prone to occur at the negative electrode tab, affecting the heat dissipation of the lithium-ion battery. In some embodiments of the present application, as shown in FIG7 , the negative electrode sheet 30 further includes a negative electrode tab 33 , a groove 321 is provided along the length direction (i.e., the Y direction) of the negative electrode tab 33 , a first groove portion 322 is provided along the length direction of the negative electrode tab 33 , and a negative electrode active material layer is provided between the first groove portion 322 and the negative electrode tab 33 along the length direction of the negative electrode tab 33 ; wherein the distance between the first groove portion 322 and the negative electrode tab 33 is d mm, and 0.2<d<5. Through the above-mentioned structure, the present application can, on the one hand, optimize the heat dispersion effect under high temperature conditions; on the other hand, due to the retention of the negative electrode active material layer between the groove and the tab area along the length direction of the negative electrode tab, it can further improve the ion conduction in the tab area, improve the regional electrochemical interface, and thus enhance the cycle performance of the secondary battery. At the same time, the separation design of the groove and the tab area can avoid secondary processing of the local area of the current collector, thereby improving the yield rate of the negative electrode sheet.
[0044] It is understood that the electrode assembly of the present application can be a wound structure, and its electrode sheet generally has a long side and a short side after being unfolded. In one embodiment of the present application, the electrode assembly is a wound structure, and the width direction is the direction in which the short side of the electrode sheet extends after being unfolded, and the length direction is the direction in which the long side of the electrode sheet extends after being unfolded. The electrode sheet of the present application includes a positive electrode sheet 20 and a negative electrode sheet 30.
[0045] The secondary battery of the present application may include any device that undergoes an electrochemical reaction, as long as it can achieve the purpose of the present application. For example, the secondary battery may include but is not limited to: lithium-ion secondary battery (lithium-ion battery), sodium-ion secondary battery, lithium polymer secondary battery or lithium-ion polymer secondary battery, etc. The battery structure of the present application includes but is not limited to soft-pack battery, square hard-shell battery or cylindrical hard-shell battery, etc.
[0046] The present application has no special restrictions on the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the negative electrode current collector may include copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, foam nickel, foam copper or a composite current collector, etc. The present application has no special restrictions on the thickness of the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the thickness of the negative electrode current collector is 4μm to 10μm. In the present application, the negative electrode active material layer can be arranged on one surface in the thickness direction of the negative electrode current collector, or on two surfaces in the thickness direction of the negative electrode current collector. It should be noted that the "surface" here can be the entire area of the negative electrode current collector or a partial area of the negative electrode current collector. The present application has no special restrictions, as long as the purpose of the present application can be achieved.
[0047] The present application does not particularly limit the type of negative electrode active material, as long as the purpose of the present application can be achieved. For example, the negative electrode active material may include graphite, a mixture of graphite and silicon materials such as silicon, silicon oxide or silicon carbide, and the above-mentioned graphite may be selected from artificial graphite or natural graphite. Optionally, the negative electrode active material layer also includes at least one of a conductive agent, a thickener, and a binder. The present application does not particularly limit the types of conductive agents, thickeners and binders in the negative electrode active material layer, as long as the purpose of the present application can be achieved. For example, the negative electrode binder may include but is not limited to at least one of polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene 1,1-difluoride, polyethylene, polypropylene, polyacrylic acid, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin or nylon. The present application does not particularly limit the mass ratio of the negative electrode active material, conductive agent, thickener, and binder in the negative electrode active material layer, as long as the purpose of the present application can be achieved. For example, the mass ratio of the negative electrode active material, conductive agent, thickener, and binder in the negative electrode active material layer is (96-98):(0-1.5):(0.5-1.5):(1.0-1.9).
[0048] The present application does not particularly limit the material of the diaphragm substrate layer, and those skilled in the art can select it according to actual needs, as long as the purpose of the present application can be achieved. For example, the material of the diaphragm substrate layer may include but is not limited to at least one of polyethylene, polypropylene, polyethylene terephthalate or polyimide. Optionally, a polypropylene porous film, a polyethylene porous film, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite film can be used.
[0049] The secondary battery of the present application also includes an electrolyte. The present application has no particular restrictions on the electrolyte. Those skilled in the art can choose according to actual needs, as long as the purpose of the present application can be achieved. For example, at least one of ethylene carbonate (also known as ethylene carbonate, abbreviated as EC), propylene carbonate (PC), diethyl carbonate (DEC), ethyl propionate (EP), propyl propionate (PP), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), vinylene carbonate (VC) or fluoroethylene carbonate (FEC) is mixed in a certain mass ratio to obtain a non-aqueous organic solvent, and then a lithium salt is added to dissolve and mix evenly. The present application has no particular restrictions on the above-mentioned "mass ratio", as long as the purpose of the present application can be achieved. The present application has no restrictions on the type of lithium salt, as long as the purpose of the present application can be achieved. For example, the lithium salt may include at least one of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, LiSiF6, lithium bis(oxalatoborate) (LiBOB), or lithium difluoroborate. The present application does not particularly limit the concentration of the lithium salt in the electrolyte, as long as the purpose of the present application can be achieved. For example, the concentration of the lithium salt is 1.0 mol / L to 2.0 mol / L.
[0050] The positive electrode sheet of the present application may include a positive electrode active material layer and a positive electrode current collector. The present application does not particularly limit the type of positive electrode active material, as long as the objectives of the present application can be achieved. For example, the positive electrode active material may include at least one of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich manganese-based materials, lithium cobalt oxide, lithium manganese oxide, or lithium iron manganese phosphate. In the present application, the positive electrode active material may also include non-metallic elements, such as at least one of fluorine, phosphorus, boron, chlorine, silicon, or sulfur, which can further improve the stability of the positive electrode active material. The positive electrode active material layer of the present application may also include a conductive agent and a binder. The present application does not particularly limit the mass ratio of the positive electrode active material, conductive agent, and binder in the positive electrode active material layer. Those skilled in the art may select the ratio according to actual needs, as long as the objectives of the present application can be achieved. For example, the mass ratio of the positive electrode active material, conductive agent, and binder in the positive electrode active material layer is (96-98):(1-3):(2-3).
[0051] The present application has no special restrictions on the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the positive electrode current collector may include aluminum foil, aluminum alloy foil or a composite current collector, etc. The present application has no special restrictions on the thickness of the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the thickness of the positive electrode current collector is 5μm to 20μm. In the present application, the positive electrode active material layer can be provided on one surface in the thickness direction of the positive electrode current collector, or on two surfaces in the thickness direction of the positive electrode current collector. It should be noted that the "surface" here can be the entire area of the positive electrode current collector or a partial area of the positive electrode current collector. The present application has no special restrictions, as long as the purpose of the present application can be achieved.
[0052] This application does not particularly limit the preparation method of the negative electrode sheet, as long as it can achieve the purpose of this application. For example, the preparation method of the negative electrode sheet includes but is not limited to the following steps: dispersing the negative electrode active material, conductive agent, thickener, and binder in deionized water to form a uniform negative electrode slurry, coating the negative electrode slurry on the negative electrode current collector, drying and cold pressing, and then forming grooves on the surface of the negative electrode sheet. After cutting and slitting, the negative electrode sheet with the structure shown in Figure 3 is obtained.
[0053] The present application does not particularly limit the preparation method of the positive electrode sheet, as long as the purpose of the present application can be achieved. For example, the preparation method of the positive electrode sheet includes but is not limited to the following steps: dispersing the positive electrode active material, the conductive agent, and the binder in an NMP solvent to form a uniform positive electrode slurry, coating the positive electrode slurry on the positive electrode current collector, drying, cold pressing, cutting, and slitting to obtain the positive electrode sheet.
[0054] The present application does not particularly limit the shape of the groove, as long as it can achieve the purpose of this application. For example, when viewed along the length of the negative electrode sheet, the shape of the groove can include at least one of a square, rectangle, trapezoid, triangle, or semicircle; when viewed along the thickness of the negative electrode sheet, the shape of the groove can include at least one of a straight line, an oblique line, a broken line, or a curved line.
[0055] The present application does not impose any particular restrictions on the method for preparing the grooves, as long as the purpose of the present application can be achieved. For example, it may include but is not limited to laser etching, mechanical processing, or pore-forming agent processing. Taking laser etching as an example, the width and depth of the grooves generally increase with increasing laser power, and the spacing of the grooves can generally be adjusted by the laser processing rate. Therefore, technicians can adjust the width, depth, spacing, and other parameters of the grooves by adjusting parameters such as the laser power, processing rate, and the tape run rate of the pole piece.
[0056] The porosity of the negative electrode sheet generally decreases as the compaction density of the negative electrode sheet increases. Based on this, the porosity of the negative electrode sheet can be adjusted by adjusting the cold pressing pressure of the negative electrode sheet and adjusting the compaction density of the negative electrode sheet.
[0057] This application does not particularly limit the preparation method of the secondary battery; any preparation method known in the art may be used, as long as the objectives of this application are achieved. For example, the preparation method of the secondary battery includes, but is not limited to, the following steps: stacking the positive electrode sheet, the separator, and the negative electrode sheet in sequence, and performing winding and folding operations as needed to obtain a wound electrode assembly; placing the electrode assembly in a packaging bag; injecting an electrolyte into the packaging bag and sealing it to obtain the secondary battery.
[0058] In a second aspect, the present application provides an electronic device comprising the secondary battery described in the aforementioned embodiment, thereby providing the electronic device with good cycle stability and safety.
[0059] The present application does not particularly limit the electronic device, and the electronic device may be any electronic device known in the prior art. In some embodiments, the electronic device may include, but is not limited to, a laptop computer, a pen-type computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a headset, a video recorder, an LCD television, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, an automobile, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, a power tool, a flashlight, a camera, a large household battery or a lithium-ion capacitor, etc.
[0060] Example
[0061] Hereinafter, the embodiments of the present application will be described in more detail with reference to Examples and Comparative Examples. Various tests and evaluations were performed according to the following methods.
[0062] Test methods and equipment:
[0063] Adhesion force F test between negative electrode and separator:
[0064] Cut a negative electrode sheet with a separator attached, measuring 15mm x 60mm in width x length. Using double-sided tape measuring 20mm x 100mm in width x length, secure the sample to a steel plate, with the test surface facing downward. Insert one end of a paper tape, the same width as the sample and 150mm longer than the sample, underneath the sample and secure with crepe tape. Secure the steel plate to the bottom of a high-speed rail tensile testing machine. Secure the other end of the paper tape to the machine's fixture and start the machine. Once the tension stabilizes, the tensile force reading represents the bond strength.
[0065] Bond layer thickness test:
[0066] The portion of the diaphragm in the electrode assembly that was not arranged opposite to the positive electrode active material layer or the negative electrode active material layer was selected, and the diaphragm cross section was prepared by ion beam profiling (CP), and then the thickness of the bonding layer was measured by scanning electron microscopy (ZEISS Sigma / X-max).
[0067] Measurement of groove depth H, groove width W, groove spacing S, and groove cross-sectional area A:
[0068] A VK-1050 laser confocal microscope was used to image the groove area, acquiring optical and depth information of the pole piece within the microscope's field of view. The pole piece surface was scanned in laser confocal mode at 20x magnification. After scanning, the acquired measurement data was processed in the instrument's associated data analysis software. The reference plane was set using the "Reference Plane Setup" function in the "Process Image" section. The "Smoothing" function was then selected, with a "5×5" size and "Simple Average" type selected to smooth the image. After processing, the groove parameters were measured using the "Profile Measurement" function.
[0069] Groove depth H and groove width W: As shown in Figure 8, the difference between the deepest part of the groove and the reference surface is the groove depth, and the distance between the intersection points of the groove and the reference surface is the groove width. Take 20 measurements along the same groove at 10 μm intervals. Calculate the average of these 20 depth and width values and record the groove depth H and width W.
[0070] Groove Spacing S: For adjacent grooves (two adjacent grooves are considered adjacent if the overlap is greater than 50% of their respective lengths when viewed along the length of the pole piece), the distance between the midpoints of the groove widths in the perpendicular direction is the groove spacing. Measurements are taken along the selected grooves at intervals of 10 μm for a total of 20 times, and the average value is calculated and recorded as the groove spacing S.
[0071] Groove area A: Use a VK-1050 laser confocal microscope to photograph the groove area and obtain the optical and depth information of the electrode within the field of view of the microscope. At a magnification of 20 times, use the laser confocal mode to scan the surface of the electrode. After scanning, obtain the depth data relative to the baseline at each pixel width. Within the above groove width range, the depth (h i ) is integrated to obtain the cross-sectional area A of the groove:
[0072] A=∑ i h i ×w0.
[0073] Negative electrode porosity test:
[0074] The porosity of the negative electrode sheet was tested using the gas replacement method: 50 negative electrode sheets with a radius of d were punched out using the same die, the thickness h of each negative electrode sheet was measured, and the 50 negative electrode sheets were placed in the sample cup of the testing equipment (AccuPycП1340). The negative electrode sheets were filled with helium in the closed sample chamber, and the true volume V of the negative electrode sheet was measured. The porosity of the negative electrode sheet was then calculated using the following formula: (1-V / πd 2 ×50×h)×100%.
[0075] High-temperature capacity retention and high-temperature thickness expansion rate tests of lithium-ion batteries:
[0076] At 45°C, the lithium-ion battery was charged at a constant current rate of 0.7C to a voltage of 4.5V, then charged at a constant voltage of 4.5V to a current of 0.05C, and then discharged at a constant current rate of 1C to a voltage of 3.0V. This was considered a charge and discharge cycle process. After repeating 400 charge and discharge cycles, the high-temperature capacity retention rate and high-temperature thickness expansion rate of the lithium-ion battery were tested.
[0077] Capacity retention rate of lithium-ion battery after 400 cycles = discharge capacity after 400th cycle / discharge capacity after first cycle × 100%;
[0078] Thickness expansion rate of the lithium-ion battery after 400 cycles = thickness of the lithium-ion battery after the 400th cycle / thickness of the lithium-ion battery at the first cycle × 100%.
[0079] Lithium-ion battery hot box pass rate test:
[0080] Place the lithium-ion battery in a sealed temperature-controlled box and charge it at a constant current rate of 0.7C at 25°C to a voltage of 4.5V. Then charge it at a constant voltage of 4.5V to a current of 0.05C. Then, heat the temperature-controlled box at (5±2)°C / min. When the temperature reaches 135°C, keep the temperature constant for 60 minutes. After the temperature-controlled box cools naturally, observe whether the lithium-ion battery catches fire or explodes. The lithium-ion battery passes the test if it does not catch fire or explode. For each example or comparative example, test 10 lithium-ion batteries and record the number of batteries that pass the hot box, n, as n / 10.
[0081] Example 1
[0082] <Preparation of negative electrode sheet>
[0083] Artificial graphite, conductive carbon black (SP), sodium carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) were mixed in a mass ratio of 96.5:1:1:1.5, and deionized water was added to form a slurry with a solid content of 75 wt%. The mixture was then stirred evenly. The slurry was evenly coated on one surface of a 6 μm thick negative electrode current collector copper foil and dried at 85°C to produce a negative electrode sheet with a 50 μm thick negative electrode active material layer. The above steps were then repeated on the other surface of the negative electrode sheet to produce a negative electrode sheet coated with negative electrode active material on both sides. The resulting negative electrode sheet was then cold pressed, and grooves were etched into the surface of the negative electrode active material layer using laser processing. The sheet was then slit, cut, and cleaned to create the tab welding area. The tabs were then welded to produce the negative electrode sheet. Parameters such as groove depth H, groove width W, groove spacing S, groove cross-sectional area, and porosity of the negative electrode sheet are shown in Table 1.
[0084] <Preparation of positive electrode sheet>
[0085] Lithium cobalt oxide, polyvinylidene fluoride, and conductive agent Super P were mixed in a mass ratio of 96:2:2, and N-methylpyrrolidone (NMP) was added as a solvent to prepare a slurry with a solid content of 75wt%, which was then stirred evenly. The slurry was evenly coated on one surface of a 6μm thick positive electrode current collector aluminum foil and dried at 95°C to obtain a positive electrode sheet with a positive electrode active material layer thickness of 60μm. The above steps were then repeated on the other surface of the positive electrode sheet to obtain a positive electrode sheet with positive electrode active material coated on both sides. The obtained positive electrode sheet was then cold pressed, slit, cut, and dried at 85°C under vacuum for 4 hours. The tabs were then welded to the positive electrode sheet.
[0086] <Preparation of Electrolyte>
[0087] Ethylene carbonate, diethyl carbonate, methyl ethyl carbonate and vinylene carbonate are mixed in a mass ratio of 8:85:5:2 to obtain a non-aqueous organic solvent. LiPF6 lithium salt is then mixed with the non-aqueous organic solvent in a mass ratio of 8:92 to obtain an electrolyte.
[0088] <Preparation of Separator>
[0089] <Preparation of Base Material Layer>
[0090] A polypropylene film with a thickness of 5 μm was used.
[0091] <Preparation of Inorganic Coating>
[0092] The mass ratio of aluminum oxide ceramic particles, butadiene-styrene polymer, and deionized water was 35:10:55. A total of 30 kg of butadiene-styrene polymer and deionized water were added to a 60-liter dual planetary mixer and dispersed at 45°C for 3 hours. Then, 16.1 kg of aluminum oxide ceramic powder was added to the mixer and dispersed at high speed at 45°C for 2 hours. The mixture was then ball-milled in a nano-grinder for 1.5 hours using 6-μm-diameter spherical zirconium oxide beads as the grinding medium to obtain an inorganic coating adhesive.
[0093] The substrate was coated by transfer coating, with a coating speed of 6 m / min and a coating amount of 0.18 mg / cm 2 The coating thickness was 1.5 μm. A three-stage drying process was used, with each section of the oven being 3 meters long and set at 50°C, 60°C, and 60°C, to form a substrate layer with a single-sided inorganic coating. The above steps were then repeated on the other side of the substrate layer to form a double-sided inorganic coating.
[0094] <Preparation of Adhesive Layer>
[0095] Core-shell polymer particles are used, with a styrene-acrylate copolymer shell and an acrylate polymer core. The total swelling degree is 450%, and the particle size is 0.45 μm. The polymer adhesive layer is prepared by adding 25 parts by mass of a core-shell polymer emulsion (40% solids content), 40 parts by mass of deionized water, and 35 parts by mass of ethanol. The preparation process involves first adding 50 kg of deionized water and ethanol solvent to a dual planetary mixer and mixing at 25°C for one hour. Then, 16.7 kg of the core-shell polymer emulsion is added and dispersed at 45°C for two hours to obtain the polymer adhesive layer.
[0096] The porous substrate + heat-resistant coating was coated on the surface by gravure roller coating to form a double-sided coating structure. The quality and thickness of the coating on both sides were consistent. The coating speed was 6m / min and the coating amount was controlled to 0.036mg / cm 2 The drying process is carried out in three stages, each stage is 3 m long, and the set temperatures of the oven are 50°C, 60°C, and 60°C; after drying, a polymer bonding layer with a single layer of particle accumulation is obtained.
[0097] <Preparation of lithium-ion batteries>
[0098] The positive electrode sheet, separator, and negative electrode sheet prepared above were stacked in order, with the groove of the negative electrode sheet facing the positive electrode sheet and the separator positioned between the positive and negative electrode sheets to provide isolation. The electrodes were wound to form an electrode assembly, the thickness of which is shown in Table 1. The electrode assembly was placed in an aluminum-plastic film packaging bag, dried, and then injected with electrolyte. The lithium-ion battery was obtained through vacuum packaging, standing, formation, degassing, and trimming.
[0099] Examples 2 to 18, Examples 20 to 21, and Examples 23 to 27
[0100] In <Preparation of Negative Electrode Sheet>, each parameter was adjusted according to Table 2 based on Example 1.
[0101] Example 19 and Example 22
[0102] Except for adjusting the preparation of the adhesive layer in <Preparation of Separator>, the remaining parameters were adjusted according to Table 2 based on Example 1.
[0103] Core-shell polymer particles are used, with a styrene-acrylate copolymer shell and an acrylate polymer core. The total swelling degree is 450%, and the particle size is 0.45 μm. The polymer adhesive layer is prepared by adding 25 parts by mass of a core-shell polymer emulsion (25% solids content), 40 parts by mass of deionized water, and 35 parts by mass of ethanol. The preparation process involves first adding 50 kg of deionized water and ethanol solvent to a dual planetary mixer and mixing at 25°C for one hour. Then, 16.7 kg of the core-shell polymer emulsion is added and dispersed at 45°C for two hours to obtain the polymer adhesive layer.
[0104] Example 28
[0105] Except for adjusting the preparation of the adhesive layer glue and the preparation of the adhesive layer in <Preparation of the diaphragm>, the remaining parameters were adjusted according to Table 2 based on Example 1.
[0106] Preparation of the adhesive layer: The polymer used was polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP) with a swelling degree of 190% and a particle size of 1.5 μm. 68 kg of deionized water and 12 kg of PVDF-HFP were added to a dual planetary mixer and mixed at 45°C for 6 hours to produce a polymer adhesive layer with a solids content of approximately 15%.
[0107] Preparation of the bonding layer: Rotary spraying was used to coat the porous substrate and heat-resistant coating to form a double-sided coating structure. The quality and thickness of the coating on both sides were consistent. The coating speed was 8 m / min and the coating amount was controlled to 0.16 mg / cm 2The drying is carried out in three stages, with each stage being 3m long and the set temperatures of the oven being 50°C, 60°C, and 60°C. After drying, the polymer adhesive layer is distributed in island and line shapes on the heat-resistant coating, wherein the area of the island coating is 1μm to 10mm and the thickness is 1μm to 100μm. The width of the linear coating is 1μm to 1mm, the length is 1μm to 50mm, and the thickness is 1μm to 100μm.
[0108] Example 29 to Example 31
[0109] Except for adjusting the "Preparation of the Diaphragm", the remaining parameters were adjusted according to Table 2 based on Example 1.
[0110] <Preparation of diaphragm>:
[0111] <Preparation of Base Material Layer>
[0112] A polypropylene film with a thickness of 9 μm was used.
[0113] <Preparation of Adhesive Layer>
[0114] Polyvinylidene fluoride and aluminum oxide ceramic particles were mixed in a mass ratio of 60:40, and NMP was added as a solvent to prepare a bonding layer slurry with a solid content of 75 wt%. The mixture was then stirred evenly. The bonding layer slurry was applied to one substrate layer and dried at 90°C to form a bonding layer. The thickness of the bonding layer is shown in Table 1. The above steps were then repeated on the other substrate layer to form a double-sided bonding layer (i.e., the first bonding layer), thus completing the separator.
[0115] Comparative Example 1
[0116] Except for the difference in <Preparation of Negative Electrode Sheet> from Example 1, the rest is the same as Example 1.
[0117] <Preparation of negative electrode sheet>
[0118] Artificial graphite, conductive carbon black (SP), sodium carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) were mixed in a mass ratio of 96.5:1:1:1.5, and deionized water was added to form a slurry with a solid content of 75 wt%. The mixture was then stirred evenly. The slurry was evenly coated on one surface of a 6 μm thick negative electrode current collector copper foil and dried at 85°C to obtain a negative electrode sheet with a 50 μm thick negative electrode active material layer. The above steps were then repeated on the other surface of the negative electrode sheet to obtain a negative electrode sheet coated with negative electrode active material on both sides. The sheet was then slit and cut, dried at 110°C under vacuum for 4 hours, and the tabs were welded to the negative electrode sheet.
[0119] Comparative Example 2 to Comparative Example 3
[0120] Except that in <Preparation of Negative Electrode Sheet>, the preparation parameters such as groove depth H and groove cross-sectional area A are adjusted as shown in Table 1, and in <Preparation of Separator>, the thickness of the adhesive layer is adjusted as shown in Table 1, the rest is the same as Example 1.
[0121] Comparative Example 4
[0122] In <Preparation of Negative Electrode Sheet>, the parameters were adjusted according to Table 1 based on Example 29.
[0123] Table 1 Note: “ / ” in Table 1 indicates no relevant preparation parameters.
[0124] Referring to Table 1, it can be seen from Examples 10 to 11 and Comparative Examples 1 to 4 that in the lithium-ion battery of the present application, by providing a groove on the surface of the negative electrode active material layer opposite to the positive electrode sheet, and regulating the relationship between the groove depth and the thickness of the separator bonding layer within the scope of the present application, the hot box pass rate of the lithium-ion battery is significantly improved, and the thickness expansion rate of the lithium-ion battery after the cycle process is also significantly reduced, indicating that the solution of the present application can improve the heat dissipation capacity inside the lithium-ion battery, thereby improving the cycle stability and safety of the lithium-ion battery at high temperatures.
[0125] Table 2
[0126] Referring to Tables 2 and 3, the groove width, groove spacing, cross-sectional area, and porosity of the negative electrode sheet generally also affect the performance of the lithium-ion battery. From Examples 1 to 22 and Comparative Example 4, it can be seen that when H ≥ T + 1 is satisfied, by regulating the above parameters within the scope of this application, a lithium-ion battery with excellent cycle stability and safety at high temperature can be obtained.
[0127] The type of polymer in the bonding layer generally also affects the performance of the lithium-ion battery. It can be seen from Examples 19, 22, and 28 to 31 that, when H ≥ T + 1 is satisfied, by regulating the above parameters within the scope of this application, a lithium-ion battery with excellent cycle stability and safety at high temperatures can be obtained.
[0128] It should be noted that the terms "comprises," "includes," or any other variations thereof are intended to encompass non-exclusive inclusion, such that a process, method, article, or apparatus that includes a list of elements includes not only those elements but also other elements not explicitly listed, or elements inherent to such process, method, article, or apparatus. In the absence of further limitations, an element defined by the phrase "comprises a ..." does not preclude the presence of other identical elements in the process, method, article, or apparatus that includes the element.
[0129] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A secondary battery, comprising an electrode assembly, wherein the electrode assembly comprises a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator is disposed between the positive electrode sheet and the negative electrode sheet, and the negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer, wherein: The surface of the negative electrode active material layer opposite to the positive electrode plate has a groove, and the depth of the groove is H μm; The separator includes a substrate layer and a bonding layer disposed on a surface of the separator opposite to the negative electrode plate. The bonding layer has a thickness of T μm and satisfies: H ≥ T+1.
2. The secondary battery according to claim 1, wherein H≥T+5.
3. The secondary battery according to claim 1, wherein The cross-sectional area of the groove is A μm 2 , the width of the groove is Wμm, satisfying: 0.35×(W×H) <A<0.95(W×H),5≤H≤100。 4. The secondary battery according to claim 3, wherein 1≤W / H≤40, 0.55×(W×H) <A<0.85(W×H)。 5. The secondary battery according to claim 3, wherein 2≤W / H≤20.
6. The secondary battery according to claim 1, wherein The width of the groove is W μm, the spacing of the grooves is S μm, and the porosity of the negative electrode sheet is P%, satisfying:
7. The secondary battery according to claim 6, wherein 10≤P≤40。 8. The secondary battery according to claim 1, wherein The spacing of the grooves is S μm, and the bonding force between the separator and the negative electrode plate is FN / m, satisfying: S≤1000F, 500≤S≤10000.
9. The secondary battery according to claim 8, wherein S≤650F.
10. The secondary battery according to claim 1, wherein 0.1≤T≤10。 11. The secondary battery according to claim 1, wherein The bonding layer includes a polymer; Wherein, based on the mass of the bonding layer, the content of the polymer is 25% to 100%.
12. The secondary battery according to claim 11, wherein The bonding force between the separator and the negative electrode plate is FN / m, satisfying: 1≤F≤50.
13. The secondary battery according to claim 11, wherein The bonding force between the separator and the negative electrode plate is FN / m, satisfying 5≤F≤30; Wherein, based on the mass of the bonding layer, the content of the polymer is 30% to 100%.
14. The secondary battery according to claim 11, wherein The polymer includes at least one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, styrene-butadiene copolymer, polyacrylonitrile, butadiene-acrylonitrile polymer, polyacrylic acid, polyacrylate or acrylate-styrene copolymer.
15. The secondary battery according to claim 1, wherein The negative electrode sheet further includes a negative electrode tab, a first groove portion is provided along the length direction of the negative electrode tab, and the negative electrode active material layer is provided between the first groove portion and the negative electrode tab along the length direction of the negative electrode tab; Wherein, the distance between the first groove portion and the negative electrode tab is d mm, and 0.2<d<5. 16 . An electronic device comprising the secondary battery according to claim 1 .