Compound, copolymer, composition, varnish and cured products of those
A compound with a tailored chemical structure and composition addresses the challenges of dielectric loss and viscosity in high-frequency materials, achieving improved performance and processability for hydrocarbon resin-based insulating materials.
Patent Information
- Application Number
- PCT/JP2024/010013
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-15
- Filing Date
- 2024-03-14
- Publication Date
- 2024-09-19
AI Technical Summary
Current materials for high-frequency applications, such as multilayer substrates and insulating materials, face challenges with dielectric loss tangent and viscosity, particularly when using hydrocarbon resins, which require functional groups for curability but often compromise on dielectric properties and processability.
A compound with a specific chemical structure, characterized by a vinylidene and vinyl group ratio, molecular weight, and composition, including olefin, aromatic vinyl, and aromatic polyene units, is developed to achieve low dielectric loss tangent and viscosity, along with a composition that includes hardening agents and resins to enhance properties.
The compound and composition result in a cured product with significantly reduced dielectric loss tangent and solution viscosity, suitable for high-frequency applications, while maintaining processability and adhesiveness.
Smart Images

Figure JP2024010013_19092024_PF_FP_ABST
Abstract
Description
Compounds, copolymers, compositions, varnishes, and cured products thereof
[0001] The present invention relates to a copolymer, a composition, a varnish, and an insulating material obtained by curing the copolymer, a composition, a varnish, or a cured product thereof.
[0002] As communication frequencies shift to the gigahertz band and higher, there is an increasing need for multilayer substrates, transmission lines, antennas, etc., made of CCLs or FCCLs containing insulating materials with low dielectric properties. Fluorine-based resins such as perfluoroethylene are characterized by their excellent low dielectric constant, low dielectric loss, and heat resistance, but they are difficult to mold and form into films, and also have issues with adhesion to copper foil in wiring, making them difficult to apply to multilayer substrates, etc. Meanwhile, substrates and insulating materials made from post-curing resins such as epoxy resins, unsaturated polyester resins, polyimide resins, and phenolic resins have been widely used due to their heat resistance and ease of handling, but their relatively high dielectric constants and dielectric loss leave room for improvement as insulating materials for high frequencies (Patent Document 1).
[0003] Therefore, hydrocarbon-based resins, which inherently possess low dielectric properties, have attracted attention. To convert hydrocarbon-based resins, which are essentially thermoplastic resins, into curable resins, functional groups must be introduced. However, functional groups that undergo radical or thermal crosslinking reactions generally have polarity, and introducing these functional groups into hydrocarbon-based resins results in poor dielectric properties. Attempts to introduce functional groups composed solely of hydrocarbons, such as aromatic vinyl groups, often require the use of expensive intermolecular reactions between hydrocarbon monomers (Patent Document 2), which is often uneconomical. Patent Document 3 discloses a cured product obtained from a specific coordination polymerization catalyst and consisting of an ethylene-olefin (aromatic vinyl compound)-aromatic polyene copolymer and a nonpolar vinyl compound copolymer with a specific composition and blend. This technology selectively copolymerizes only one of the two vinyl groups of the aromatic polyene (divinylbenzene), preserving the remaining vinyl group, thereby easily producing a crosslinkable hydrocarbon-based copolymer macromonomer with aromatic vinyl group functional groups. Cured products obtained from similar olefin-aromatic vinyl compound-aromatic polyene copolymers and compositions with auxiliary materials, etc., are characterized by low dielectric constants and low dielectric dissipation factors (Patent Documents 4 and 5). However, the olefin-aromatic vinyl compound-aromatic polyene copolymer specifically described is relatively soft, and in order to harden it is necessary to blend a large amount of other hard auxiliary materials or inorganic fillers.
[0004] Known hard cross-linkable raw materials have insufficient low-dielectric properties, and compounding them in large amounts results in a deterioration in the low-dielectric properties of the cured product. Compounding a relatively large amount of inorganic filler results in a particularly high dielectric constant of the resulting cured product, due to the generally high dielectric constant of inorganic fillers. Furthermore, a low-dielectric, curable aromatic vinyl compound-aromatic polyene copolymer obtained by cationic polymerization is known (Patent Document 6). However, this prior art copolymer has many polymer terminal structures due to its dendritic (tree-like) structure, and the terminal structures unique to cationic polymerization make molecular design for improving heat resistance and durability complex.
[0005] Japanese Patent Application Laid-Open No. 06-192392 Japanese Patent Application Laid-Open No. 2004-087639 Japanese Patent Application Laid-Open No. 2007-217706 International Publication No. 2021 / 112087 International Publication No. 2021 / 112088 International Publication No. 2018 / 181842
[0006] Currently, the ideal level in the technical field is that the dielectric loss tangent of the cured product and the viscosity of the solution must be very small. Therefore, in light of the currently required level, the compounds described in the above publications have the problem that it is difficult to sufficiently reduce the dielectric loss tangent of the cured product and the viscosity of the solution at the same time.
[0007] As a result of intensive research aimed at solving the above-mentioned problems, the present inventors have discovered a new compound that can provide both a cured product with a very small dielectric tangent and a solution with a very small viscosity, and have found that the use of this compound in a composition can solve the problems that the prior art has not been able to solve, thereby completing the present invention. That is, the present invention provides the following various specific embodiments.
[0008] Aspect 1. A compound having a chemical structure with a vinylidene group terminal and a vinyl group terminal, wherein the compound is dissolved in deuterated 1,1,2,2-tetrachloroethane and measured at 23°C in proton NMR. Among peaks, Vd indicates a vinylidene group terminal appearing at a chemical shift of 4.5 to 4.7 ppm, and Vn indicates a vinyl group terminal appearing at a chemical shift of 4.8 to 5.0 ppm. The ratio Vd / Vn is 0.4 or greater, and the compound is dissolved in tetrahydrofuran solvent and measured by gel permeation chromatography to obtain a standard polystyrene-equivalent number average molecular weight (Mn), where Mn is the reciprocal of the number of polymer terminals, is 4 x 10 -5 The compound is dissolved in a toluene solution at a concentration of 50 wt %, and the shear rate is 1 sec at 25°C using a rotational rheometer. -1 The compound has a viscosity of 20,000 mPa·s or less as measured by a spectrometry.
[0009] Aspect 2. The compound according to aspect 1, which is a copolymer containing an olefin monomer unit, an aromatic vinyl compound monomer unit, and an aromatic polyene monomer unit.
[0010] Aspect 3. The compound according to aspect 2, wherein the content of the aromatic vinyl compound monomer unit in the compound is 15 mol % or more.
[0011] Aspect 4. The compound according to Aspect 2 or 3, wherein the content of the aromatic polyene monomer unit in the compound is 1.5 mol % or more.
[0012] Aspect 5. The compound according to any one of Aspects 1 to 4, which is a copolymer having a number average molecular weight of 500 or more.
[0013] Aspect 6. The compound according to any one of Aspects 2 to 4, wherein the olefin monomer unit comprises ethylene and an α-olefin having 3 or more carbon atoms.
[0014] Aspect 7. A composition comprising the compound according to any one of Aspects 1 to 6 and one or more resins selected from the group consisting of (a) to (d) below: (a) a curing agent; (b) one or more resins selected from the group consisting of hydrocarbon-based elastomers, polyether-based resins, and aromatic polyene-based resins; (c) a monomer; and (d) another olefin-aromatic vinyl compound-aromatic polyene copolymer satisfying all of the following conditions (i) to (iv): (i) the number average molecular weight of the copolymer is 500 or more and less than 100,000; and (ii) the aromatic vinyl compound monomer unit is an aromatic vinyl compound having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is 70 mass% or less. (iii) The aromatic polyene monomer unit is one or more selected from polyenes having 5 to 20 carbon atoms and having a plurality of vinyl groups and / or vinylene groups in the molecule, and the content of vinyl groups and / or vinylene groups derived from the aromatic polyene monomer unit is 1.5 to 20 or 1.5 to less than 20 per number average molecular weight. (iv) The olefin monomer unit is one or more selected from olefins having 2 to 20 carbon atoms, the content of the olefin monomer unit is 30 mass% or more, and the total of the olefin monomer unit, aromatic vinyl compound monomer unit, and aromatic polyene monomer unit is 100 mass%.
[0015] Aspect 8. A varnish comprising the compound according to any one of Aspects 1 to 6 or the composition according to Aspect 7, and a solvent.
[0016] Aspect 9. A cured product of the compound according to any one of Aspects 1 to 6.
[0017] Aspect 10. A cured product of the composition according to aspect 7.
[0018] Aspect 11. A cured product of the varnish according to Aspect 8.
[0019] Aspect 12. A CCL substrate, an FCCL substrate, an interlayer insulating material, or a coverlay, comprising the cured product according to any one of aspects 9 to 11.
[0020] According to the present invention, a compound or the like can be obtained that has both a very small dielectric tangent when cured and a very small viscosity when in solution, and a composition or the like containing the compound can also be obtained.
[0021] Fig. 1 shows the proton NMR spectrum of the compound of Example 1, dissolved in deuterated 1,1,2,2-tetrachloroethane, measured at 23°C. Fig. 2 is an enlarged view of the proton NMR spectrum of Example 1 shown in Fig. 1, around the chemical shift of 4.0 to 6.0 ppm. The peak indicating the vinylidene group terminal is designated as "Vd", and the peak indicating the vinyl group terminal CH 2The 2H peak of —CH—R is indicated as “Vn(2).” This also applies to the following drawings. FIG. 3 is a proton NMR spectrum of the compound of Example 2, dissolved in deuterated 1,1,2,2-tetrachloroethane and measured at 23° C. FIG. 4 is an enlarged view of the chemical shift range of 4.0 to 6.0 ppm in the proton NMR spectrum of Example 2 shown in FIG. 3. FIG. 5 is a proton NMR spectrum of the compound of Comparative Example 1, dissolved in deuterated 1,1,2,2-tetrachloroethane and measured at 23° C. FIG. 6 is an enlarged view of the chemical shift range of 4.0 to 6.0 ppm in the proton NMR spectrum of Comparative Example 1 shown in FIG. 5. FIG. 7 is a proton NMR spectrum of the compound of Comparative Example 2, dissolved in deuterated 1,1,2,2-tetrachloroethane and measured at 23° C. FIG. 8 is an enlarged view of the chemical shift range of 4.0 to 6.0 ppm in the proton NMR spectrum of Comparative Example 2 shown in FIG. 7. FIG. 9 is a proton NMR spectrum of the compound of Comparative Example 3, dissolved in deuterated 1,1,2,2-tetrachloroethane and measured at 23°C. FIG. 10 is an enlarged view of the chemical shift range of 4.0 to 6.0 ppm in the proton NMR spectrum of Comparative Example 3 shown in FIG. 9. FIG. 11 is a proton NMR spectrum of the compound of Comparative Example 4, dissolved in deuterated 1,1,2,2-tetrachloroethane and measured at 23°C. FIG. 12 is an enlarged view of the chemical shift range of 4.0 to 6.0 ppm in the proton NMR spectrum of Comparative Example 4 shown in FIG. 11. FIG. 13 is an enlarged view of the chemical shift range of 4.0 to 6.0 ppm in the proton NMR spectrum of the compound of Comparative Example 5, dissolved in deuterated 1,1,2,2-tetrachloroethane and measured at 23°C.
[0022] Hereinafter, embodiments of the present invention will be described in detail. However, the following embodiments are merely examples for explaining the present invention, and the present invention is not limited thereto. That is, the present invention can be implemented with any modifications within the scope of the gist thereof. In this specification, a numerical range such as "1 to 100" includes both the lower limit "1" and the upper limit "100." The same applies to other numerical ranges. In this specification, the term "sheet" also includes the concept of a film. Furthermore, the term "film" in this specification also includes the concept of a sheet. In this specification, the term "composition" also includes the concept of a varnish. In other words, a liquid composition is particularly referred to as a varnish. In this specification, the term "interlayer insulating material" includes the concept of an interlayer adhesive. In this specification, a numerical range includes both the lower limit and the upper limit unless otherwise specified. In this specification, the term "wt%" also includes the concept of "mass%."
[0023] In one embodiment of the present invention, there are provided compounds having a novel chemical structure with a vinylidene group terminal and a vinyl group terminal, and compositions containing the compounds. The novel chemical structure of the compounds can be confirmed by satisfying the following three conditions:
[0024] First, as a first condition, the compound was dissolved in heavy 1,1,2,2-tetrachloroethane (also called 1,1,2,2-tetrachloroethane-d2) and measured at 23°C by proton NMR ( 1 Among the peaks in H-NMR, the integral value Vd of the area of the peak representing the vinylidene group terminal appearing at a chemical shift of 4.5 to 4.7 ppm and the integral value Vn of the area of the peak representing the vinyl group terminal appearing at a chemical shift of 4.8 to 5.0 ppm must have a ratio Vd / Vn of 0.4 or more.
[0025] If the value of the ratio Vd / Vn is less than 0.4, the dielectric loss tangent becomes too high. In a preferred embodiment, the value of Vd / Vn may be 0.6 or more, more preferably 0.8 or more. The upper limit of the value of Vd / Vn is not particularly limited, but may be, for example, 20.0 or less, or 15.0 or less.
[0026] Generally, the terminal structure of an organic compound is the following vinylidene group terminal Vd and three types of vinyl group terminals Vn, 2Vn, and 3Vn Among these, the vinyl group-terminated CH corresponding to "Vn" in the above 2 For —CH—R, the 2H peak appears at 4.8 to 5.0 ppm, and the 1H peak appears at 5.6 to 5.8 ppm. Based on this, we discovered that optimizing the ratio of the peak area at a chemical shift of 4.8 to 5.0 ppm to the peak area at a chemical shift of 4.5 to 4.7 ppm, which represents the amount of vinylidene group terminals, can significantly reduce the dielectric dissipation factor of the cured product of the compound. That is, the present inventors first conceived the idea that by focusing on the 2H of "Vn" among the three types of vinyl group terminals and comparing it with "Vd," an optimized novel structure can be obtained. In other words, a Vd / Vn value of 0.4 or greater means that the compound has a chemical structure in which the amount of vinylidene group terminals is not excessively small compared to the amount of the vinyl group terminals. That is, this embodiment is based on the finding that, due to the high mobility of the compound's terminals, the presence of an excessive amount of highly polar vinyl groups at those terminals will degrade dielectric performance. In the following description, a peak representing 2H of Vn may be referred to as "Vn(2)" and a peak representing 1H of Vn may be referred to as "Vn(1)." In the present specification, in the context of describing a peak area ratio such as Vd / Vn, unless otherwise specified, the Vn refers to the area of the Vn(2) peak.
[0027] Next, as the second condition, the compound is dissolved in tetrahydrofuran solvent, and the number average molecular weight (Mn) calculated in terms of standard polystyrene is determined by gel permeation chromatography (GPC). The reciprocal of Mn, that is, the number of polymer ends, is 4×10 -5 The value of the number of polymer ends is the reciprocal of the number average molecular weight, and therefore the unit in this specification is mol / g.
[0028] The number of polymer terminals is 4×10 -5 If the number of polymer ends is less than 4.5 × 10, the molecular weight of the polymer compound is large, and in light of the state of the art at the time of filing, it would appear that the dielectric performance would be improved. However, contrary to expectations, the present inventors have found that this alone is not enough to sufficiently reduce the dielectric tangent, and in addition, the viscosity increases. In a preferred embodiment, the number of polymer ends is 4.5 × 10 -5 or more, more preferably 5×10 -5 The upper limit of the number of polymer ends is not particularly limited, but may be, for example, 2 × 10 -3 or less, or 1 x 10 -3 It may be the following:
[0029] The polymer terminal structure of this compound is 1 H-NMR, 13 It can be quantified by a known method using C-NMR.
[0030] Finally, as the third condition, the compound was dissolved in a toluene solution at a concentration of 50 wt %, and the shear rate was measured at 25°C using a rotational rheometer at a shear rate of 1 sec. -1 It is necessary that the viscosity measured by the method is 20,000 mPa·s or less.
[0031] If the viscosity value exceeds 20,000 mPa·s, it becomes difficult to use as a varnish, and problems arise in that it becomes difficult to apply to electronic machinery applications. In a preferred embodiment, the viscosity value may be 15,000 mPa·s or less, and more preferably 10,000 mPa·s or less.
[0032] The present inventors have found that a synergistic effect is achieved when all three of these conditions are met, and that the effect is lost if any one of them is missing.
[0033] In a preferred embodiment, the ratio 2Vn / Vn(2) of the integral value of the peak area appearing at 4.8 to 5.0 ppm, which indicates 2H of "Vn" among the three types of vinyl group terminals, to the integral value of the peak area appearing at 5.12 to 5.35 ppm and 5.6 to 5.8 ppm, which indicates "2Vn", is preferably 0.45 or more, and more preferably 0.45 to 5.00. When the ratio 2Vn / Vn(2) is within this range and is combined with the first condition described above, it is believed that a more appropriate chemical structure will be obtained.
[0034] In a preferred embodiment, the weight average molecular weight Mw of the compound is 1.0×10 4 Above 1.0 x 10 6 or less, more preferably 5.0 × 10 4 Above 1.0 x 10 6 In a preferred embodiment, the Mw / Mn value may be in the range of 5 or more and 20 or less, and more preferably in the range of 7 or more and 20 or less.
[0035] In a preferred embodiment, the compound may be a copolymer containing an olefin monomer unit, an aromatic vinyl compound monomer unit, and an aromatic polyene monomer unit, and the aromatic moiety in such a copolymer can improve the dielectric properties.
[0036] In this specification, the term "olefin monomer unit" refers to one or more compounds (units) selected from α-olefins having 2 to 20 carbon atoms and cyclic olefins having 5 to 20 carbon atoms, which are substantially free of oxygen, nitrogen, and halogens and are composed of carbon and hydrogen. Examples of α-olefins having 2 to 20 carbon atoms include, but are not limited to, ethylene, propylene, 1-butene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 4-methyl-1-pentene, and 3,5,5-trimethyl-1-hexene. Examples of cyclic olefins having 5 to 20 carbon atoms include, but are not limited to, norbornene and cyclopentene. A preferred olefin monomer unit may be a combination of ethylene with an α-olefin other than ethylene or with a cyclic olefin. In a preferred embodiment, the olefin monomer unit may contain one or more compounds selected from the group consisting of ethylene and α-olefins having 3 or more carbon atoms.
[0037] In a preferred embodiment, the content of olefin monomer units in the copolymer may be 3 mol% or more, more preferably 10 mol% or more, and even more preferably 20 mol% or more. In this specification, unless otherwise specified, the mol% standard refers to the total amount of the compound or copolymer. That is, in the case of the copolymer, the sum of the olefin monomer units, aromatic vinyl compound monomer units, and aromatic polyene monomer units may be considered to be 100%, and the amounts of other constituent components may be considered as an external ratio.
[0038] In this specification, the term "aromatic vinyl compound monomer unit" refers to an aromatic vinyl compound (unit) having from 8 to 20 carbon atoms. Examples of the aromatic vinyl compound monomer unit include, but are not limited to, styrene, paramethylstyrene, paraisobutylstyrene, various vinylnaphthalenes, and various vinylanthracenes.
[0039] In a preferred embodiment, the content of the aromatic vinyl compound monomer unit may be 15 mol % or more, more preferably 18 mol % or more, and even more preferably 20 mol % or more. When the content of the aromatic vinyl compound monomer unit is in this range, the effect of easily improving the dielectric properties tends to be easily obtained.
[0040] In this specification, the term "aromatic polyene monomer unit" refers to a polyene compound (unit) having 5 to 20 carbon atoms and containing multiple vinyl groups and / or vinylene groups in its molecule. Examples of the aromatic polyene monomer unit include, but are not limited to, various ortho-, meta-, and para-divinylbenzenes or mixtures thereof, and compounds having an aromatic vinyl structure, such as divinylnaphthalene, divinylanthracene, p-2-propenylstyrene, and p-3-butenylstyrene, which are substantially free of oxygen, nitrogen, and halogens and are composed of carbon and hydrogen. Furthermore, the aromatic polyene monomer unit may also include bifunctional aromatic vinyl compounds, such as 1,2-bis(vinylphenyl)ethane (abbreviation: BVPE), as described in JP-A-2004-087639. Among these, various ortho-, meta-, and para-divinylbenzenes or mixtures thereof are preferably used, and a mixture of meta-divinylbenzene and para-divinylbenzene is preferably used. In this specification, these divinylbenzenes are referred to as "divinylbenzenes." When a divinylbenzene is used as the aromatic polyene, the curing efficiency is increased during the curing treatment, and curing becomes easy, which is preferable.
[0041] In the copolymer, the content of vinyl groups and / or vinylene groups (preferably vinyl groups) derived from aromatic polyene monomer units may be 1.5 or more and 20 or less than 1.5 and 20, preferably 2 or more and less than 7, per number average molecular weight. When the content of vinyl groups and / or vinylene groups is 1.5 or more, crosslinking efficiency is high, and a cured product with sufficient crosslink density tends to be easily obtained. The content of vinyl groups derived from aromatic polyene units (divinylbenzene units) per number average molecular weight in the copolymer can be calculated, for example, by the number average molecular weight (Mn) calculated in terms of standard polystyrene obtained by GPC (gel permeation chromatography) known to those skilled in the art and 1 It can be obtained by comparing the vinyl group content derived from aromatic polyene units obtained by H-NMR measurement with the vinyl group content derived from aromatic polyene units obtained by H-NMR measurement. 1 By comparing the intensities of each peak area obtained by H-NMR measurement, if the content of vinyl groups derived from aromatic polyene units (divinylbenzene units) in the copolymer is 0.6% by mass and the number average molecular weight calculated as polystyrene by GPC measurement is 49,000, the molecular weight of vinyl groups derived from aromatic polyene units in the number average molecular weight is the product of these, 299, which is divided by the formula weight of the vinyl groups, 130, to obtain 2.3. In other words, the content of vinyl groups derived from aromatic polyene units per number average molecular weight in this copolymer is determined to be 2.3. 1 The assignment of peaks obtained by H-NMR measurement is known from literature. 1 A method for determining the composition of a copolymer from a comparison of peak areas obtained by H-NMR measurement is also known. 1 The measurement was performed in a known quantitative mode using a H-NMR measurement method. 13 It is also possible to improve the accuracy of the composition by adding data on the peak areas and ratios of the C-NMR spectrum. In this specification, the content of divinylbenzene units in the copolymer is determined based on the peak intensity ( 1In other words, the content of divinylbenzene units is calculated from the content of vinyl groups derived from divinylbenzene units, assuming that one vinyl group is derived from one divinylbenzene unit in the copolymer.
[0042] In a preferred embodiment, the content of the aromatic polyene monomer unit may be 1.5 mol % or more, more preferably 2.0 mol % or more, and even more preferably 2.5 mol % or more. When the content of the aromatic polyene monomer unit is in this range, the effect of improving the dielectric properties tends to be easily obtained.
[0043] Preferably, the combined content of the aromatic vinyl compound monomer unit and the aromatic polyene monomer unit may be 15 mol% or more and 1.5 mol% or more, more preferably 18 mol% or more and 2.0 mol% or more, and even more preferably 20 mol% or more and 2.5 mol% or more. The upper limits of these contents are not particularly limited and can be adjusted depending on the content of the olefin monomer. For example, the combined content of the aromatic vinyl compound monomer unit and the aromatic polyene monomer unit may be 15 mol% or more and 80 mol% or less and 1.5 mol% or more and 10 mol% or less.
[0044] The number average molecular weight (Mn) of the present compound or the present copolymer is not particularly limited, but may be preferably not less than 500, more preferably not less than 1000. In this specification, the number average molecular weight is calculated as a molecular weight calculated in terms of standard polystyrene obtained by GPC (gel permeation chromatography).
[0045] In some embodiments of the present invention, a composition containing the above-described compound or copolymer can also be provided. The composition may contain, for example, one or more of the following components: (a) a curing agent; (b) one or more resins selected from a hydrocarbon-based elastomer, a polyether-based resin, and an aromatic polyene-based resin; (c) a monomer; and (d) an olefin-aromatic vinyl compound-aromatic polyene copolymer other than the above-described copolymer, which satisfies all of the following conditions (i) to (iv): (i) the number-average molecular weight of the copolymer is 500 or more and less than 100,000; (ii) the aromatic vinyl compound monomer unit is an aromatic vinyl compound having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is 70% by mass or less, preferably more than 0% by mass and 70% by mass or less. (iii) The aromatic polyene monomer unit is one or more selected from polyenes having 5 to 20 carbon atoms and having a plurality of vinyl groups and / or vinylene groups in the molecule, and the content of vinyl groups and / or vinylene groups derived from the aromatic polyene monomer unit is 1.5 to 20 or 1.5 to less than 20 per number average molecular weight. (iv) The olefin monomer unit is one or more selected from olefins having 2 to 20 carbon atoms, the content of the olefin monomer unit is 30 mass% or more, and the total of the olefin monomer unit, aromatic vinyl compound monomer unit, and aromatic polyene monomer unit is 100 mass%.
[0046] <Curing Agent> The curing agent that may be included in the present composition may be a known curing agent that has been conventionally used for the polymerization or curing of aromatic polyenes or aromatic vinyl compounds. Examples of such curing agents include radical polymerization initiators (radical generators), cationic polymerization initiators, and anionic polymerization initiators. Radical polymerization initiators are preferred, although the type is not particularly limited. Organic peroxides, azo-based polymerization initiators, and the like are more preferred, and can be freely selected depending on the application and conditions. Catalogs listing organic peroxides can be downloaded from the NOF Corporation website, for example, https: / / www.nof.co.jp / business / chemical / chemical-product01. Organic peroxides listed in catalogs from Fujifilm Wako Pure Chemical Industries, Ltd. and Tokyo Chemical Industry Co., Ltd. can also be used. Known photopolymerization initiators that utilize light, ultraviolet light, or radiation can also be used as curing agents. Examples of photopolymerization initiators include photoradical polymerization initiators, photocationic polymerization initiators, and photoanionic polymerization initiators. Such photopolymerization initiators are available, for example, from Tokyo Chemical Industry Co., Ltd. Furthermore, curing by radiation or electron beams is also possible. Also, crosslinking and curing can be achieved by thermal polymerization of the raw materials contained in the composition without using a curing agent.
[0047] There are no particular restrictions on the amount of curing agent used, but for example, 0.01 to 10 parts by mass of the curing agent may be included per 100 parts by mass of the present compound. When using a curing agent such as a peroxide or azo-based polymerization initiator, the curing treatment is carried out at an appropriate temperature and time, taking into account its half-life. In this case, the conditions are optional depending on the curing agent, but a temperature range of approximately 50°C to 200°C is generally appropriate.
[0048] <Hydrocarbon Elastomer> The amount of hydrocarbon elastomer that may be contained in the composition can be appropriately set depending on the desired performance and is not particularly limited, but is preferably 1 to 200 parts by mass, more preferably 1 to 100 parts by mass, and most preferably 1 to 50 parts by mass, per 100 parts by mass of the compound. The hydrocarbon elastomer preferably has a number average molecular weight of 100 or more and 100,000 or less, more preferably 1,000 or more and 4,500 or less. Preferred examples of the hydrocarbon elastomer include, but are not limited to, one or more elastomers selected from ethylene-based or propylene-based elastomers, conjugated diene-based polymers, block copolymers or random copolymers of aromatic vinyl compounds and conjugated dienes, and hydrogenated products thereof. Examples of the ethylene-based elastomer include ethylene-α-olefin copolymers such as ethylene-octene copolymer and ethylene-1-hexene copolymer, EPR, EPDM, etc., and examples of the propylene-based elastomer include atactic polypropylene, low stereoregular polypropylene, propylene-α-olefin copolymers such as propylene-1-butene copolymer, etc., but are not particularly limited to these.
[0049] Examples of conjugated diene polymers include, but are not limited to, polybutadiene and 1,2-polybutadiene. Examples of aromatic vinyl compound-conjugated diene block or random copolymers and their hydrogenated products (hydrogenated products) include, but are not limited to, SBS, SIS, SEBS, SEPS, SEEPS, and SEEBS. Suitable 1,2-polybutadiene is available, for example, from Nippon Soda Co., Ltd. under the product names B-1000, 2000, and 3000 as liquid polybutadiene. Another suitable copolymer containing a 1,2-polybutadiene structure is "Ricon 100" manufactured by TOTAL CRAY VALLEY. When the resin or resins selected from these hydrocarbon elastomers are liquid (approximately 300,000 mPa s or less) particularly at room temperature (25°C), from the viewpoint of the handleability and moldability of the present composition in an uncured state (handleability as a thermoplastic resin), the amount used may be preferably 150 parts by mass or less, more preferably 1 to 30 parts by mass, and most preferably 1 to 20 parts by mass, per 100 parts by mass of the present compound.
[0050] <Polyether-based resin> Examples of polyether-based resins that may be contained in the present composition include polyphenylene ether and polyether. As the polyphenylene ether, commercially available known polyphenylene ethers can be used, and the type is not particularly limited. The number average molecular weight of the polyphenylene ether is arbitrary and can be appropriately set depending on the desired performance, and is not particularly limited. However, in consideration of the moldability of the composition, the number average molecular weight (Mn) is preferably 10,000 or less, most preferably 5,000 or less. The number average molecular weight may preferably be 500 or more.
[0051] Furthermore, when the additive is added for the purpose of curing the present composition, it is preferable that the molecular terminals of the polyether-based resin, such as polyphenylene ether, be modified with a functional group. Furthermore, when the additive is added for the purpose of curing the present composition, it is preferable that the polyether-based resin, such as polyphenylene ether, have multiple functional groups in one molecule. For example, the polyether-based resin may be a modified polyphenylene ether. Examples of the functional group include radically polymerizable functional groups and functional groups such as epoxy groups, and preferably radically polymerizable functional groups. A preferred radically polymerizable functional group is a vinyl group. As the vinyl group, one or more of the group consisting of an allyl group, a (meth)acryloyl group, and an aromatic vinyl group are preferred, and one or more of the group consisting of a (meth)acryloyl group and an aromatic vinyl group are more preferred, with an aromatic vinyl group being the most preferred. In other words, in the composition of this embodiment, a bifunctional polyphenylene ether in which both molecular chain terminals are modified with radically polymerizable functional groups is particularly preferred. Examples of such polyphenylene ethers include Noryl (trademark) SA9000 manufactured by SABIC (modified polyphenylene ether having methacryloyl groups at both ends, number average molecular weight 2200) and bifunctional polyphenylene ether oligomer manufactured by Mitsubishi Gas Chemical Company, Inc. (OPE-2St, modified polyphenylene ether having vinylbenzyl groups at both ends, number average molecular weight 1200). Allylated PPE manufactured by Asahi Kasei Corporation can also be used. Of these, the bifunctional polyphenylene ether oligomer manufactured by Mitsubishi Gas Chemical Company, Inc. (OPE-2St) is preferred.
[0052] The polyether resin may also be an aromatic polyether (ELPAC HC-F series) manufactured by JSR Corp. The amount of polyphenylene ether or other polyether resin used in the composition can be appropriately determined depending on the desired performance and is not particularly limited, but is preferably 1 to 200 parts by mass, more preferably 1 to 100 parts by mass, per 100 parts by mass of the compound.
[0053] <Aromatic Polyene Resin> The aromatic polyene resin that may be contained in the present composition includes divinylbenzene-based reactive hyperbranched copolymer (PDV) manufactured by Nippon Steel Chemical & Material Co., Ltd. Such PDV is described, for example, in the literature "Synthesis of Polyfunctional Aromatic Vinyl Copolymer and Development of a New IPN-Type Low Dielectric Loss Material Using the Same" (Kawabe Masanao, Journal of the Japan Institute of Electronics Packaging, p. 125, Vol. 12 No. 2 (2009)). The amount of aromatic polyene resin used in the present composition can be appropriately set depending on the desired performance and is not particularly limited, but is preferably 1 to 200 parts by weight, more preferably 1 to 100 parts by weight, and most preferably 1 to 50 parts by weight per 100 parts by weight of the present compound. Using an amount of aromatic polyene resin within these preferred ranges is preferable to prevent a decrease in adhesion to other components and a decrease in toughness.
[0054] <Monomer> The amount of monomer that may be contained in the composition may preferably be 100 parts by mass or less per 100 parts by mass of the compound, and the composition may be substantially free of monomers. In this specification, the term "monomer" refers to a monomer that can be polymerized by either radical polymerization, cationic polymerization, or anionic polymerization, and is preferably a radically polymerizable monomer. Its molecular weight is preferably 5,000 or less, more preferably less than 5,000, more preferably 1,000 or less, more preferably less than 1,000, even more preferably 500 or less, and even more preferably less than 500. The monomer may include a monomer having the same structure as the monomer unit of the above-mentioned "aromatic vinyl compound" or "aromatic polyene." Preferably, the monomer may include the following polar monomer.
[0055] <Polar Monomer> The amount of polar monomer that may be contained in the composition can be appropriately set depending on the desired performance and is not particularly limited. However, it may be preferably 100 parts by mass or less, more preferably 0.1 to 20 parts by mass, and even more preferably 0.1 to 10 parts by mass, per 100 parts by mass of the compound. Using an amount within this preferred range tends to prevent the dielectric constant and dielectric dissipation factor of the resulting cured product from becoming too high. In this specification, a polar monomer refers to a monomer containing one or more atoms selected from oxygen, nitrogen, phosphorus, and sulfur in the molecule. Suitable polar monomers have a molecular weight of less than 5,000, more preferably less than 1,000, and even more preferably less than 500. The polar monomer is preferably one that can be polymerized using a radical polymerization initiator. Examples of polar monomers include, but are not limited to, various maleimides, bismaleimides, maleic anhydride, triallyl isocyanurate, glycidyl (meth)acrylate, tri(meth)acrylic isocyanurate, and trimethylolpropane tri(meth)acrylate. Maleimides and bismaleimides that can be used in the present embodiment are described, for example, in International Publication No. 2016 / 114287 and Japanese Patent Application Laid-Open No. 2008-291227, and are commercially available from, for example, Daiwa Chemical Industry Co., Ltd., Nippon Kayaku Co., Ltd., and Designer Molecules Inc. Furthermore, the bismaleimide resin "SLK" manufactured by Shin-Etsu Chemical Co., Ltd. can also be used. Of these maleimide group-containing compounds, bismaleimides are preferred from the viewpoints of solubility in organic solvents, high-frequency characteristics, high adhesion to conductors, and moldability of prepregs. These maleimide group-containing compounds may be used as polyaminobismaleimide compounds from the viewpoints of solubility in organic solvents, high-frequency characteristics, high adhesion to conductors, moldability of prepregs, etc. Polyaminobismaleimide compounds can be obtained, for example, by subjecting a compound having two maleimide groups at its terminals to a Michael addition reaction with an aromatic diamine compound having two primary amino groups in the molecule.When attempting to obtain high crosslinking efficiency with the addition of a small amount, it is preferable to use a polar monomer having a multifunctional group of two or more functional groups. Examples of such polar monomers include bismaleimides, triallyl isocyanurate (TAIC), trimethylolpropane tri(meth)acrylate, etc.
[0056] <Another Olefin-Aromatic Vinyl Compound-Aromatic Polyene Copolymer> The present composition may contain one or more olefin-aromatic vinyl compound-aromatic polyene copolymers other than the above-described copolymers, and may satisfy any of the following conditions: (i) the number-average molecular weight of the copolymer is 500 or more and less than 100,000; (ii) the aromatic vinyl compound monomer units are aromatic vinyl compounds having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer units is 70% by mass or less, preferably more than 0% by mass and 70% by mass or less; (iii) the aromatic polyene monomer units are one or more selected from polyenes having 5 to 20 carbon atoms and having multiple vinyl groups and / or vinylene groups in the molecule, and the content of vinyl groups and / or vinylene groups derived from the aromatic polyene monomer units is 1.5 to 20 or 1.5 to less than 20 per number average molecular weight. (iv) The olefin monomer unit is one or more olefins selected from olefins having from 2 to 20 carbon atoms, the content of the olefin monomer units is 30% by mass or more, and the total of the olefin monomer units, aromatic vinyl compound monomer units, and aromatic polyene monomer units is 100% by mass.
[0057] Such other copolymers may be those described, for example, in WO 2021 / 112087, WO 2021 / 112088, and WO 2022 / 014599. Another olefin-aromatic vinyl compound-aromatic polyene copolymer that satisfies all of the above-mentioned specific conditions tends to be soft and exhibit a low dielectric constant and a low dielectric dissipation factor, so by combining it with this compound to form a composition, it is possible to provide a cured product with a low dielectric constant and a low dielectric dissipation factor that covers a wide range of physical properties.
[0058] <Production Method> The present compound can be designed and produced to satisfy the three conditions described above. Therefore, the present compound can be produced by applying known production methods, and the production method is not particularly limited. When the present compound is a copolymer, it can be produced by copolymerizing the respective monomers of an aromatic vinyl compound, an aromatic polyene, and an olefin, which is used as needed, by coordination polymerization. For example, the use of a single-site coordination polymerization catalyst composed of a transition metal compound and a co-catalyst, as described in JP 2009-161743 A, JP 2010-280771 A, WO 00 / 37517, etc., is preferred because it allows for efficient production of an olefin-aromatic vinyl compound-aromatic polyene copolymer. For example, examples of copolymers, particularly aromatic vinyl compound-aromatic polyene copolymers (which may contain olefins), include styrene-divinylbenzene copolymer, ethylene-styrene-divinylbenzene copolymer, ethylene-propylene-styrene-divinylbenzene copolymer, ethylene-1-hexene-styrene-divinylbenzene copolymer, and ethylene-1-octene-styrene-divinylbenzene copolymer.
[0059] <Varnish> In an embodiment of the present invention, a varnish containing the compound or composition described above and a solvent can be provided. Note that, in this specification, a varnish that is liquid due to the inclusion of a solvent is referred to as a varnish.
[0060] As described above, the varnish has an appropriate viscosity and is a viscous liquid. The varnish can be applied, impregnated, filled, or dripped onto other materials using an appropriate method, followed by removal of the solvent to form a molded product. It can also be cured with heat or light to obtain the desired cured product. These properties are useful because they can be used to form insulating coatings or layers by various transfer molding (pressure molding), application onto or between substrates or semiconductor device materials, or extrusion lamination or spin coating to form sheets or films, followed by curing. Furthermore, the polymerization liquid used to produce the present compound (which generally contains, in addition to the present compound, solvents used in polymerization such as toluene, ethylbenzene, cyclohexane, and methylcyclohexane, residual monomers such as styrene and divinylbenzene, residual monomers such as olefin monomers, catalysts, and co-catalyst components) can also be used as a varnish. Alternatively, a varnish can be obtained by distilling off some or all of the solvent and residual monomers from the present polymerization liquid under reduced pressure and then diluting with the solvent as needed. That is, the present varnish may contain residual monomers or solvents used in the polymerization.
[0061] <Solvent> An appropriate solvent may be added to the composition as needed. The amount of solvent used is not particularly limited. The solvent is used to adjust the viscosity and fluidity of the composition. In particular, when the resin composition of this embodiment is in the form of a varnish, a solvent is preferably used. A solvent with a high boiling point at atmospheric pressure, i.e., low volatility, results in a uniform thickness of the applied film. Therefore, a solvent having a boiling point of at least a certain level is preferred. The boiling point is preferably approximately 75°C or higher at atmospheric pressure, more preferably 100°C or higher and 300°C or lower, and even more preferably 130°C or higher and 300°C or lower. Solvents known in the art can be used, and are not particularly limited. Examples of solvents that can be used include cyclohexane, cyclohexanone, methyl ethyl ketone (MEK), toluene, ethylbenzene, xylene, mesitylene, tetralin, acetone, limonene, mixed alkanes, and mixed aromatic solvents. The amount of the solvent used in the composition of the present embodiment can be appropriately set depending on the desired performance, and is arbitrary. However, it is preferably 5 to 500 parts by mass, more preferably 10 to 300 parts by mass, and most preferably 50 to 150 parts by mass relative to 100 parts by mass of the present compound.
[0062] When a raw material that is poorly soluble in toluene or other aromatic solvents, such as a specific bismaleimide, is used as a component of the present composition, methyl ethyl ketone (MEK) can be used as the solvent.
[0063] The composition and varnish may contain additives that are commonly used in resins in the industry, such as antioxidants, weathering agents, light stabilizers, lubricants, compatibilizers, antistatic agents, etc., to the extent that the desired effects and purposes are not impaired. The composition and varnish of the present embodiment are obtained by mixing, dissolving, or melting the various additives described above, and any known method can be used for mixing, dissolving, or melting.
[0064] The present compound or the present composition can be mixed by a known kneading method, for example, a twin-screw kneader, various rolls, various kneaders, etc. When the composition is a varnish, it may be mixed by adding it to the varnish and stirring.
[0065] In one embodiment of the present invention, a cured product of the compound, composition, or varnish described above can be provided. The cured product can be used to manufacture a CCL substrate, an FCCL substrate, an interlayer insulating material, or a coverlay. In other words, the compound, composition, or the like is particularly suitable as an electrical insulating material for high-frequency signals.
[0066] <Molded Articles> Molded articles obtained from the present compound or composition can have any shape. These compositions can exhibit the properties of a thermoplastic resin. Therefore, under conditions that do not cause crosslinking, they can be molded into shapes such as sheets, tubes, strips, pellets, etc. in a substantially uncured state using known molding methods for thermoplastic resins, such as extrusion molding, injection molding, press molding, and inflation molding, and then crosslinked (cured). For example, when the composition is a varnish, it is generally obtained as a sheet or film-like molded article by applying it to a substrate and then removing the solvent by heating, reducing pressure, air-drying, etc. These methods can produce uncured sheets and films. Alternatively, composites can be obtained by impregnating a porous substrate, woven fabric, or nonwoven fabric with the present varnish and removing the solvent. Dropping the composition onto a substrate and removing the solvent can also produce, for example, a hemispherical shape. The sheet may be uncured (semi-cured) to the extent that it maintains its sheet shape, or it may be fully cured. The degree of curing of the composition can be quantitatively measured using known dynamic mechanical analysis (DMA).
[0067] <Curing> The curing of a molded article obtained from the present compound or the present composition, etc. can be carried out by a known method, taking into consideration the curing conditions (temperature, time, pressure) of the raw materials and curing agent contained therein. When the curing agent used is a peroxide, the curing conditions can be determined by taking into consideration the half-life temperature, etc. disclosed for each peroxide.
[0068] The cured product of a molded article obtained from the present compound or composition is sufficiently cured, and the gel content (gel fraction) measured in accordance with ASTM is not particularly limited, but may be 90 mass% or more. Furthermore, the dielectric loss tangent of the cured product, measured in the range of 10 to 50 GHz, particularly preferably at 40 GHz, is not particularly limited, but may be 0.003 or less, more preferably 0.002 or less, and even more preferably 0.001 or less. More specifically, the dielectric loss tangent may be 0.00063 or less.
[0069] The features of the present invention will be explained in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. That is, the materials, amounts used, ratios, processing details, processing procedures, etc. shown in the following examples can be appropriately changed as long as they do not deviate from the spirit of the present invention. Furthermore, the values of various production conditions and evaluation results in the following examples represent preferred upper or lower limits in the embodiments of the present invention, and preferred numerical ranges may be defined by combining the above-mentioned upper or lower limits with the values of the following examples or values between the examples.
[0070] Examples 1 and 2 and Comparative Examples 1 to 5 Examples 1 and 2 and Comparative Examples 1 to 5 were prepared based on the raw material compositions shown in Table 1 below (given in mol % and mass % in the table).
[0071] Each compound was produced with reference to the production methods described in JP 2009-161743 A and JP 2010-280771 A. Dimethylmethylenebiscyclopentadienylzirconium dichloride, diphenylmethylene(1-indenyl)cyclopentadienylzirconium dichloride, or racemic-dimethylmethylenebis(4,5-benzo-1-indenyl)zirconium dichloride was used as the catalyst. The following abbreviations are used in the table: Dimethylmethylenebiscyclopentadienylzirconium dichloride... Zr100 Diphenylmethylene(1-indenyl)cyclopentadienylzirconium dichloride... Zr101 Racemic-dimethylmethylenebis(4,5-benzo-1-indenyl)zirconium dichloride... racZr
[0072] Tritium tetrakis(pentafluorophenyl)borate ("TRI-FABA" manufactured by Tosoh Finechem Co., Ltd.) or modified methylaluminoxane ("MMAO" manufactured by Tosoh Finechem Co., Ltd.) was used as the co-catalyst. Product names are used in the table.
[0073] Cyclohexane was used as a solvent. Polymerization was carried out using styrene (St), divinylbenzene (DVB), ethylene (Et), and, as needed, 1-hexene or 1-octene as raw material monomers in a 10 L polymerization vessel equipped with a stirrer and a heating / cooling jacket, after adding the above catalyst and co-catalyst.
[0074]
[0075] The analysis of each compound and composition obtained above was carried out by the following methods.
[0076] <Analysis of Chemical Structure of Compound> The composition ratio of each component is shown in the table. The composition ratio of ethylene (Et), α-olefin (1-hexene or 1-octene in this example), styrene (St), and divinylbenzene (DVB) in the copolymer, the content of vinyl group units derived from divinylbenzene, and the ratio of terminal vinyl groups to terminal vinylidene groups were calculated using the following formula: 1 The determination was made from the peak area intensity assigned to each component in H-NMR (using the method described above). The sample was dissolved in deuterated 1,1,2,2-tetrachloroethane, and the measurement was carried out at 23°C.
[0077] The NMR spectrum peaks were as follows. The details of the spectrum are shown in the figure. 0.7 to 1.02 ppm: CH3, 3H of α-olefin 0.5 to 2.1 ppm: St + DVB + Et + CH2, 2H of α-olefin 4.5 to 4.7 ppm: Terminal vinylidene CH2, 2H ... Vd 4.8 to 5.0 ppm: Terminal vinyl CH2, 2H ... Vn(2) 5.12 to 5.35, 5.6 to 5.8 ppm: DVB vinyl CH2,2H ... 2Vn 6.6 to 6.8 ppm: DVB vinyl CH,1H 6.8 to 7.4 ppm: St aromatic ring C6H5,5H, DVB aromatic ring C6H4,4h
[0078] The peak area ratio Vd / Vn of the terminal vinyl group Vn(2) and the terminal vinylidene group Vd is calculated by 1 The peak area of the terminal vinylidene group (Vd) obtained by H-NMR measurement was divided by the peak area of the terminal vinyl group (Vn(2)). The peak area ratio of the terminal vinyl group 2Vn to the terminal vinylidene group Vd, 2Vd / Vn, was calculated in the same manner.
[0079] <Molecular Weight Measurement> The molecular weight of the copolymer was determined by GPC (gel permeation chromatography) to determine the number average molecular weight (Mn) and weight average molecular weight (Mw) in terms of standard polystyrene, as well as the ratio Mw / Mn. The measurement was carried out under the following conditions. Column: Two TSK-GEL MultiporeHXL-M φ7.8 × 300 mm (manufactured by Tosoh Corporation) connected in series were used. Column temperature: 40°C Solvent: THF (tetrahydrofuran) Flow rate: 1.0 ml / min Detector: RI detector
[0080] <Preparation of Varnish, Preparation of Cured Sheet> Using a vessel equipped with a heating and cooling jacket and a stirring blade, the compound prepared above and a solvent (toluene) were heated to approximately 60°C and stirred to dissolve the compound. Furthermore, 1 part by mass of Perhexyne 25B (2,5-dimethyl-2,5-bis(tert-butylperoxy)hexyne-3, manufactured by NOF Corporation) was added as a curing agent per 100 parts by mass of the resin component, dissolved, stirred, and mixed to obtain a varnish-like composition. The resulting composition was poured into a silicone mold (frame length 7 cm, width 7 cm, thickness 0.5 mm, 1.0 mm, or 2.0 mm) on a Teflon (registered trademark) sheet placed on a glass plate, air-dried, and then further dried in a vacuum dryer at 60°C for 3 hours or more to obtain an uncured sheet. Furthermore, a Teflon sheet and an SUS mold were placed under a load of 5 MPa in a press, and heat treatment was carried out at 120°C for 30 minutes, 150°C for 30 minutes, and then 200°C for 120 minutes.The Teflon sheet and the SUS mold were then removed to obtain a cured sheet.
[0081] <Dielectric Loss (Dielectric Loss Tangent)> The dielectric loss tangent was measured at 23°C and 40 GHz using a cavity resonator perturbation method (using an 8722ES network analyzer manufactured by Agilent Technologies and a 40 GHz split cylinder resonator manufactured by Keysight Technologies, Inc.) using a 0.2 mm × 25 mm × 30 mm sample cut out from the sheet.
[0082] <Viscosity Measurement> Viscosity was measured using a rotational rheometer ("MCR302" manufactured by Anton Paar) at 25°C and a shear rate of 1 sec. -1 The solution was concentrated using a rotary evaporator and diluted with toluene to a concentration of 50% by mass to prepare a measurement solution, which was then measured.
[0083] As shown in the above table, all of the examples exhibited excellent dielectric loss tangents and viscosities.
[0084] On the other hand, in Comparative Examples 1 to 3, the Vd / Vn value was small and the dielectric loss tangent was poor. In Comparative Example 4, the number of polymer ends was small and the viscosity was poor. In Comparative Example 5, the styrene content was low and the viscosity was poor.
Claims
1. A compound having a chemical structure with vinylidene end groups and vinyl end groups, the compound being dissolved in deuterated 1,1,2,2-tetrachloroethane and measured at 23°C in proton NMR, in which the integral value Vd of the peak area indicating a vinylidene end group appearing at a chemical shift of 4.5 to 4.7 ppm and the integral value Vn of the peak area indicating a vinyl end group appearing at a chemical shift of 4.8 to 5.0 ppm have a ratio Vd / Vn of 0.4 or more, and the compound being dissolved in tetrahydrofuran solvent and measured by gel permeation chromatography to obtain a number average molecular weight (Mn) calculated in terms of standard polystyrene, the reciprocal of which is the number of polymer ends, is 4 x 10 -5 The compound is dissolved in a toluene solution at a concentration of 50 wt %, and the shear rate is 1 sec at 25° C. using a rotational rheometer. -1 The compound has a viscosity of 20,000 mPa·s or less as measured by a .
2. The compound according to claim 1, which is a copolymer comprising an olefin monomer unit, an aromatic vinyl compound monomer unit, and an aromatic polyene monomer unit.
3. The compound according to claim 2, wherein the content of the aromatic vinyl compound monomer unit in the compound is 15 mol % or more.
4. The compound according to claim 2 or 3, wherein the content of the aromatic polyene monomer unit in the compound is 1.5 mol % or more.
5. The compound according to claim 1 or 2, which is a copolymer having a number average molecular weight of 500 or more.
6. The compound according to claim 2, wherein the olefin monomer units comprise ethylene and an α-olefin having 3 or more carbon atoms.
7. A composition comprising the compound according to claim 1 and one or more selected from the following (a) to (d): (a) a curing agent; (b) one or more resins selected from the group consisting of hydrocarbon-based elastomers, polyether-based resins, and aromatic polyene-based resins; (c) a monomer; and (d) another olefin-aromatic vinyl compound-aromatic polyene copolymer satisfying all of the following conditions (i) to (iv): (i) the number average molecular weight of the copolymer is 500 or more and less than 100,000. (ii) the aromatic vinyl compound monomer unit is an aromatic vinyl compound having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is 70 mass% or less. (iii) The aromatic polyene monomer unit is one or more selected from polyenes having 5 to 20 carbon atoms and having a plurality of vinyl groups and / or vinylene groups in the molecule, and the content of the vinyl groups and / or vinylene groups derived from the aromatic polyene monomer unit is 1.5 to 20 or 1.5 to less than 20 per number average molecular weight. (iv) The olefin monomer unit is one or more selected from olefins having 2 to 20 carbon atoms, the content of the olefin monomer unit is 30 mass% or more, and the total of the olefin monomer unit, aromatic vinyl compound monomer unit and aromatic polyene monomer unit is 100 mass%.
8. A varnish comprising the compound according to claim 1 or the composition according to claim 7 and a solvent.
9. A cured product of the compound according to claim 1.
10. A cured product of the composition according to claim 7.
11. A cured product of the varnish according to claim 8.
12. A CCL substrate, an FCCL substrate, an interlayer insulating material, or a coverlay, comprising the cured product according to claim 9 or 10.
13. A CCL substrate, an FCCL substrate, an interlayer insulating material, or a coverlay, comprising the cured product according to claim 11.
Citation Information
Patent Citations
Ethylene polymer
JP1996034819A
Vinyl-Containing Stereospecific Polypropylene Macromers
JP2001525461A
Highly filled resin composition
JP2010280860A
Resin composition, sheet, solar cell sealing material, solar cell module, and method for producing sheet for solar cell sealing material
WO2018180483A1
Composition and cured body
WO2022014599A1