Solar cell and preparation method therefor

By setting up hole bonding layers in the solar cell and annealing to form a raised connection, the problem of poor adhesion of metal electrodes is solved, the adhesion and flow diversion effect of the solar cell are improved, and the cost is reduced by using copper grid wire materials, achieving more efficiency solar cell performance and reliability.

WO2024193576A9PCT designated stage expired Publication Date: 2024-11-07TONGWEI SOLAR ENERGY (CHENGDU) CO LID
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/082663
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-23
Filing Date
2024-03-20
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

When preparing solar cells using copper interconnect technology, poor adhesion between metal electrodes and transparent conductive oxide layers leads to a decrease in electrical performance and an increased risk of disengagement, affecting the reliability and efficiency of the solar cell.

Method used

A bonding layer with holes is provided between the metal electrode and the transparent conductive oxide layer, so that the protrusions of the metal electrode are connected through the holes and the transparent conductive oxide layer, increasing the binding force, and forming dense holes through annealing to improve adhesion and flow diversion effect, while using copper as the gate wire material to reduce the preparation cost.

Benefits of technology

Improve the adhesion and flow diversion effect of metal electrodes and transparent conductive oxide layers, enhance the reliability and performance of solar cells, reduce power attenuation in humid and heat environments, and reduce the light transmittance to solar cells through transparent bonding layer materials. The impact of

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024082663_07112024_PF_FP_ABST
    Figure CN2024082663_07112024_PF_FP_ABST
Patent Text Reader

Abstract

The present application provides a solar cell and a preparation method therefor. The solar cell comprises a battery substrate. At least one surface of the battery substrate is provided with a transparent conductive oxide layer (5). A bonding layer (6) is attached to the transparent conductive oxide layer (5). The bonding layer (6) is provided with holes, and metal electrodes (7) are arranged on the bonding layer (6). One side, close to the bonding layer (6), of each metal electrode (7) penetrates a hole to be connected to the transparent conductive oxide layer (5).
Need to check novelty before this filing date? Find Prior Art

Description

A solar cell and a method for preparing the same

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on March 23, 2023, with application number 202310294495.2 and invention name “A solar cell and its preparation method”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to the field of solar cells, and in particular to a solar cell and a method for preparing the same. Background Art

[0003] Using copper interconnect technology to replace traditional screen silver paste printing is a cost-reduction method for metallization of solar cells and is currently one of the most popular technologies at the forefront of the photovoltaic industry. Copper interconnect technology uses magnetron sputtering to form a metal seed layer on a transparent conductive oxide layer (TCO), and then deposits a thin metal layer on the surface of the metal seed layer through electrochemical methods to form a metal electrode. In order to ensure a low shading area and low contact resistance, it is required to prepare a narrow and thick metal electrode. The narrowing of the metal electrode will lead to poor adhesion between the metal electrode and the transparent conductive oxide layer (TCO), increase the risk of separation between the metal electrode and the transparent conductive oxide layer, and affect the electrical performance of the solar cell.

[0004] Summary of the Invention

[0005] The purpose of this application is to provide a solar cell and a preparation method thereof to improve the adhesion between the metal electrode and the transparent conductive oxide layer.

[0006] In a first aspect, an embodiment of the present application provides a solar cell, which includes a cell substrate, wherein at least one surface of the cell substrate has a transparent conductive oxide layer, a bonding layer having holes is attached to the transparent conductive oxide layer, a metal electrode is provided on the bonding layer, and a side of the metal electrode close to the bonding layer is connected to the transparent conductive oxide layer through the hole.

[0007] In the above implementation process, a bonding layer is provided between the metal electrode and the transparent conductive oxide layer, and the bonding layer has a hole. The side of the metal electrode close to the bonding layer passes through the hole to connect with the transparent conductive oxide layer. The side of the metal electrode close to the bonding layer can be provided with a protrusion. The protrusion passes through the hole, and the circumference of the protrusion is in close contact with the hole wall. At the same time, the protrusion passing through the hole is connected to the transparent conductive oxide layer, thereby increasing the bonding force between the transparent conductive oxide layer and the metal electrode, improving the adhesion effect of the metal electrode and the transparent conductive oxide layer, and improving the adhesion between the metal electrode and the transparent conductive oxide layer without affecting the metal electrode's extraction of current.

[0008] In combination with the first aspect, in an optional embodiment of the present application, the material of the bonding layer is a transparent material; the bonding layer covers the entire surface of the transparent conductive oxide layer.

[0009] In the above implementation process, the bonding layer outside the metal electrode attachment area can block water vapor and sodium ions after the subsequent solar cell packaging is completed, reduce the power attenuation of the component in a humid and hot environment, and improve reliability. At the same time, since the material of the bonding layer is transparent, it can reduce the impact on the transmittance of the solar cell and maintain the performance of the solar cell.

[0010] In combination with the first aspect, in an optional embodiment of the present application, the light transmittance of the bonding layer is not less than 93%.

[0011] In the above implementation process, since the bonding layer covers the transparent conductive oxide layer, it will affect the transmittance of the solar cell. The higher the transmittance, the better the performance of the solar cell. Therefore, the greater the transmittance of the bonding layer, the better. The inventors believe that controlling the transmittance of the bonding layer to no less than 93% is a better and achievable range.

[0012] In combination with the first aspect, in an optional embodiment of the present application, the material of the bonding layer includes at least one of SiOx and TiW, where the value of x is 1-2.

[0013] In the above implementation process, the thin film formed by SiOx and TiW has high transmittance in the visible light wavelength range, can meet the above-mentioned transmittance requirements, and basically has no other impact on the solar cell. It is a better choice as a bonding layer material. In actual operation, those skilled in the art can select the bonding layer material according to actual conditions. In conjunction with the first aspect, in an optional embodiment of the present application, the thickness of the bonding layer is not greater than 80nm;

[0014] Optionally, the thickness of the bonding layer is 5 nm-80 nm.

[0015] In the above implementation process, the thickness of the bonding layer is controlled to be no more than 80 nm. After the metal seed layer is formed on the bonding layer and then annealed, dense micropores that penetrate the thickness of the bonding layer can be formed on the bonding layer. At the same time, the metal seed layer can easily move through the dense micropores to form protrusions (the transparent conductive oxide layer has good thermal stability and is not easy to migrate, so the metal seed layer passes through the dense micropores). The protrusions form an arc-like contact with the transparent conductive oxide layer, thereby increasing the contact area between the metal electrode and the transparent conductive oxide layer, so that the metal electrode has a good current conduction effect, which is conducive to the extraction of current.

[0016] Controlling the thickness of the bonding layer to no less than 5 nm ensures that the bonding layer effectively blocks moisture and sodium ions, reducing the potential for power degradation in hot and humid environments. It also minimizes damage to the transparent conductive oxide layer during corrosion removal of the metal seed layer. Those skilled in the art can select an appropriate bonding layer thickness based on actual needs, such as 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, and 80 nm.

[0017] In combination with the first aspect, in an optional embodiment of the present application, the metal electrode includes a stacked metal seed layer and a metal grid line layer, and the metal seed layer passes through the holes of the bonding layer and is connected to the transparent conductive oxide layer.

[0018] The metal seed layer is formed first and then annealed, which is conducive to forming dense holes on the bonding layer, while allowing the metal seed layer to pass through the holes of the bonding layer and form protrusions to connect with the transparent conductive oxide layer.

[0019] In combination with the first aspect, in an optional embodiment of the present application, the metal seed layer is a copper seed layer, and the metal gate line layer is a copper gate line layer.

[0020] The use of copper as the material for the grid lines is cheaper than the traditional use of silver paste to prepare the grid lines, which can effectively reduce the production cost of solar cells.

[0021] In a second aspect, the present invention also provides a method for preparing a solar cell, the method comprising:

[0022] Providing a battery substrate, wherein at least one surface of the battery substrate is provided with a transparent conductive oxide layer;

[0023] depositing a bonding layer on the surface of the transparent conductive oxide layer;

[0024] depositing a metal seed layer on the bonding layer;

[0025] Annealing the battery substrate on which the metal seed layer is formed, so that holes are formed in the bonding layer, and the metal seed layer passes through the holes and is connected to the transparent conductive oxide layer;

[0026] A metal grid line layer is formed on the metal seed layer by electroplating to obtain a solar cell.

[0027] In the above implementation process, a bonding layer is provided between the transparent conductive oxide layer and the metal seed layer, and annealing is performed to form holes in the bonding layer. Simultaneously, annealing can cause the metal seed layer to pass through the holes to form protrusions, which are connected to the transparent conductive oxide layer through the protrusions. This changes the morphology of the contact surfaces of the gate line, the transparent conductive oxide layer, and the bonding layer, thereby increasing the contact area between the metal seed layer and the transparent conductive oxide layer, thereby increasing the bonding force between the transparent conductive oxide layer and the metal seed layer, enhancing the adhesion effect between the gate line and the transparent conductive oxide layer, and improving the adhesion between the gate line and the transparent conductive oxide layer.

[0028] In combination with the second aspect, in an optional embodiment of the present application, the material of the bonding layer includes at least one of SiOx and TiW, where the value of x is 1-2.

[0029] In combination with the second aspect, in an optional embodiment of the present application, the metal seed layer is a copper seed layer, and the metal gate line layer is a copper gate line layer.

[0030] In combination with the second aspect, in an optional embodiment of the present application, the thickness of the bonding layer is 5nm-80nm; the temperature of the annealing treatment is 180℃-200℃; and the time of the annealing treatment is 5min-30min.

[0031] In the above implementation process, controlling the thickness of the bonding layer to 5nm-80nm, and controlling the annealing temperature to 180℃-200℃ and the time to 5min-30min can form a sufficient number of penetrating holes on the surface of the bonding layer of materials such as Si0x and TiW, thereby allowing the copper seed layer to pass through the holes in the bonding layer to form more protrusions and connect with the transparent conductive oxide layer, effectively increasing the bonding area between the copper seed layer and the transparent conductive oxide layer, thereby improving the conduction effect of the copper wire, and at the same time will not affect the passivation ability of the amorphous silicon layer of the silicon substrate.

[0032] In combination with the second aspect, in an optional embodiment of the present application, the environment of the annealing treatment is a vacuum environment or an inert gas atmosphere environment.

[0033] In the above implementation process, the environment is controlled to be a vacuum environment or an inert gas atmosphere environment, which can prevent the environment atmosphere from reacting with the solar cell and causing the generation of impurities. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without creative work.

[0035] FIG1 is a schematic diagram of the structure of a solar cell provided by the prior art;

[0036] FIG2 is a schematic diagram of the structure of a solar cell provided in an embodiment of the present application;

[0037] FIG3 is a flow chart of a method provided in an embodiment of the present application.

[0038] Figure numerals: 1-crystalline silicon layer, 2-intrinsic amorphous silicon layer, 3-N-type amorphous silicon layer, 4-P-type amorphous silicon layer, 5-transparent conductive oxide layer, 6-bonding layer, 61-adhesion enhancement layer, 62-barrier layer, 7-metal electrode, 71-copper seed layer, 72-copper gate line layer, 73-tin layer. DETAILED DESCRIPTION

[0039] To make the purpose, technical solutions, and advantages of the embodiments of this application more clear, the technical solutions in the embodiments of this application will be clearly and completely described below in conjunction with the drawings in the embodiments of this application. Obviously, the described embodiments are part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0040] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or those recommended by the manufacturer. All reagents or instruments used, if the manufacturer is not specified, are commercially available conventional products.

[0041] To reduce the production cost of solar cells, a copper grid metallization technology for heterojunction solar cells has been proposed. To ensure low light-shielding area and low contact resistance, this heterojunction solar cell copper grid metallization technology requires the preparation of narrow and thick metal electrodes. To this end, a double-layer electrode technology has been proposed. Referring to FIG1 , a narrow and thin copper seed layer 71 is first prepared. The copper seed layer 71 is then thickened by electroplating, photoinduced plating, or other methods to form a copper grid layer 72. Specifically, the entire heterojunction solar cell copper grid metallization process is as follows: After depositing a transparent conductive film, a copper seed layer 71 is sputter-deposited on the surface of the transparent conductive film to serve as an adhesion layer and conductive layer for electroplating. An electroplating mask is then applied to the copper seed layer 71 for pattern transfer. Areas not requiring electroplating are then covered with a mask to achieve selective electroplating. After the electroplating is complete, the mask is stripped with a chemical solution. Finally, the copper seed layer 71 on the mask is removed by etching, and the mask is cleaned and dried, resulting in a copper-electrode heterojunction solar cell with excellent shape and selectivity. However, the adhesion between the transparent conductive oxide layer 5 (TCO) and the copper seed layer 71 is poor, and the transparent conductive oxide layer 5 and the copper seed layer 71 are prone to separation, causing the copper grid lines to detach, affecting the electrical performance and appearance of the solar cell. Furthermore, the subsequent removal of the excess copper seed layer 71 involves the use of an acidic solution to corrode and remove the copper seed layer 71. This acidic solution damages the surface of the transparent conductive oxide layer 5, affecting its surface microstructure and creating nanoscale micropores. This affects the optical and electrical properties of the transparent conductive oxide layer 5, ultimately reducing the solar cell's conversion efficiency.

[0042] This solution incorporates a bonding layer 6 between the copper seed layer 71 and the transparent conductive oxide layer 5. Annealing forms holes in the bonding layer 6. This annealing process allows the copper seed layer 71 to penetrate the holes, forming protrusions that connect to the transparent conductive oxide layer 5. This alters the morphology of the contact surfaces between the metal electrode 7, the transparent conductive oxide layer 5, and the bonding layer 6, increasing the contact area between the metal electrode 7 and the transparent conductive oxide layer 5. This in turn strengthens the bonding strength between the transparent conductive oxide layer 5 and the metal electrode 7, enhancing the adhesion and flow diversion between the metal electrode 7 and the transparent conductive oxide layer 5. Furthermore, after encapsulation of the solar cell, the bonding layer 6 acts as a barrier to moisture and sodium ions, reducing the power loss of the solar cell in hot and humid environments and improving the reliability of the solar cell.

[0043] Referring to FIG. 2 , an embodiment of the present application provides a solar cell, comprising a cell substrate, wherein at least one surface of the cell substrate has a transparent conductive oxide layer 5, a bonding layer 6 is attached to the transparent conductive oxide layer 5, the bonding layer 6 has holes, a metal electrode 7 is provided on the bonding layer 6, and a side of the metal electrode 7 close to the bonding layer 6 passes through the hole and is connected to the transparent conductive oxide layer 5.

[0044] With the above design, a bonding layer 6 is provided between the metal electrode 7 and the transparent conductive oxide layer 5, and the bonding layer 6 has a hole. The side of the metal electrode 7 close to the bonding layer 6 passes through the hole to connect with the transparent conductive oxide layer 5. The side of the metal electrode 7 close to the bonding layer 6 can be provided with a protrusion. The protrusion passes through the hole, and the circumference of the protrusion is in close contact with the hole wall. At the same time, the protrusion passing through the hole is connected to the transparent conductive oxide layer 5, thereby increasing the bonding force between the transparent conductive oxide layer 5 and the metal electrode 7, enhancing the adhesion effect of the metal electrode 7 and the transparent conductive oxide layer 5, and improving the adhesion between the metal electrode 7 and the transparent conductive oxide layer 5 without affecting the current extraction of the metal electrode 7.

[0045] In some embodiments, the structure of the cell substrate includes a bulk silicon layer 1 (C-Si), an intrinsic amorphous silicon layer 2 (ia-Si:H) disposed on opposite surfaces of the crystalline silicon layer 1, an N-type amorphous silicon layer 3 (na-Si:H) disposed on a surface of the intrinsic amorphous silicon layer 2 remote from the bulk silicon layer 1, and a P-type amorphous silicon layer 4 (pa-Si:H) disposed on a surface of another intrinsic amorphous silicon layer 2 remote from the bulk silicon layer 1, and a transparent conductive oxide layer 5 (TCO) is disposed on both outer surfaces of the N-type amorphous silicon layer 3 and the P-type amorphous silicon layer 4 of the silicon substrate.

[0046] In some embodiments, the bonding layer is made of a transparent material; the bonding layer 6 covers the entire surface of the transparent conductive oxide layer 5. After the subsequent solar cell packaging is completed, the bonding layer 6 outside the area where the metal electrode 7 is attached can block water vapor and sodium ions, reducing the power attenuation of the component in a humid and hot environment and improving reliability. At the same time, because the bonding layer 6 is made of a transparent material, it can reduce the impact on the transmittance of the solar cell and maintain the performance of the solar cell. For ease of description, the area of ​​the bonding layer 6 corresponding to the metal electrode 7 will be referred to as the adhesion enhancement layer 61, and the portion outside the area corresponding to the metal electrode 7 will be referred to as the barrier layer 62.

[0047] To ensure the performance of the solar cell, in some embodiments, the transmittance of the bonding layer 6 is no less than 93%. Examples of transmittances for the bonding layer 6 include, but are not limited to, 93%, 94%, 95%, 96%, 97%, 98%, and 99%. Since the bonding layer 6 is applied to the transparent conductive oxide layer 5, it will affect the transmittance of the solar cell. Higher transmittance indicates better solar cell performance. Therefore, a higher transmittance for the bonding layer 6 is preferable. The inventors believe that controlling the transmittance of the bonding layer 6 to no less than 93% is an optimal and achievable range. Specifically, the material for the bonding layer 6 can be selected from at least one of SiOx and TiW, where x is 1-2. Thin films formed from SiOx and TiW have high transmittance within the visible light wavelength range, exhibit no optical loss, and can meet the aforementioned transmittance requirements without adversely affecting the solar cell. These materials are preferred for the bonding layer 6. In actual operation, those skilled in the art will select the material for the bonding layer 6 based on their specific circumstances.

[0048] At the same time, in order to ensure the blocking effect of the bonding layer 6, in some embodiments, the thickness of the bonding layer 6 is not less than 5 nm. The thicker the bonding layer 6 is, the stronger its blocking ability is. The inventors believe that controlling the thickness of the bonding layer 6 to be not less than 5 nm can ensure that the bonding layer 6 has a good ability to block water vapor and sodium ions, reduce the possibility of power attenuation of the component in a humid and hot environment, and at the same time reduce damage to the transparent conductive oxide layer 5 when corroding and removing the metal seed layer. However, transparent materials such as SiOx and TiW generally do not have electrical conductivity. When such materials are used as the adhesion enhancement layer 61 of the bonding layer 6 and disposed between the transparent conductive oxide layer 5 and the metal electrode 7, they will affect the electrical performance of the entire solar cell. Therefore, in some embodiments, the thickness of the bonding layer 6 is no greater than 80 nm. The thickness of the bonding layer 6 is controlled to be no greater than 80 nm. After the metal seed layer is formed on the bonding layer 6 and then annealed, dense micropores can be formed on the bonding layer 6 that penetrate the thickness of the bonding layer. At the same time, the metal seed layer can easily move through the dense micropores to form protrusions (the transparent conductive oxide layer 5 has good thermal stability and is not prone to migration, so the metal seed layer passes through the dense micropores). The protrusions form a similar arc-shaped contact with the transparent conductive oxide layer 5, thereby increasing the contact area between the metal electrode 7 and the transparent conductive oxide layer 5, so that the metal electrode 7 has a good current conduction effect, which is conducive to the extraction of current. It will be understood by those skilled in the art that if the conductivity of the bonding layer 6 can be improved by other means, or there is a material that can meet the conductivity and transmittance requirements at the same time, the bonding layer 6 may not be subject to this thickness restriction, that is, in other embodiments, the thickness of the bonding layer 6 may be greater than 80 nm, for example, 90 nm, 100 nm, etc.

[0049] In order to take into account both conductivity and blocking ability, the inventors believe that controlling the thickness of the bonding layer 6 to be in the range of 5nm-80nm is a more appropriate range. Optionally, the thickness of the bonding layer 6 is 10nm-50nm. Optionally, the thickness of the bonding layer 6 is 10nm-30nm. Those skilled in the art can select a suitable thickness according to actual needs, such as 5nm, 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm and 80nm.

[0050] Optionally, the metal electrode 7 includes a stacked metal seed layer and a metal grid layer, with the metal seed layer passing through the holes in the bonding layer 6 to connect to the transparent conductive oxide layer 5. Forming the metal seed layer first and then performing an annealing treatment facilitates the formation of dense holes in the bonding layer while allowing the metal seed layer to pass through the holes in the bonding layer and form protrusions that connect to the transparent conductive oxide layer.

[0051] To reduce the manufacturing cost of solar cells, in some embodiments, the metal seed layer is a copper seed layer 71, and the metal grid line layer is a copper grid line layer 72. The side of the copper seed layer 71 near the bonding layer 6 passes through the hole and connects to the transparent conductive oxide layer 5. Using copper as the material for the grid line is more cost-effective than traditional silver paste for making grid lines, which can effectively reduce the manufacturing cost of solar cells.

[0052] In other embodiments, the metal seed layer may also be an aluminum seed layer, the metal gate line layer may be an aluminum gate line layer, etc., which is not limited in this application.

[0053] Referring to FIG. 3 , an embodiment of the present application provides a method for preparing a solar cell, the method comprising:

[0054] S0 obtains the battery matrix;

[0055] In this embodiment, a battery matrix is ​​obtained by a preparation method, which includes: texturing a silicon wafer to form a pyramid texture surface on the surface of the silicon wafer, and then preparing an intrinsic amorphous silicon layer 2 and a doped amorphous silicon layer to obtain a battery matrix.

[0056] In this embodiment, the structure of the battery matrix includes a bulk silicon layer 1 (C-Si), an intrinsic amorphous silicon layer 2 (ia-Si:H) provided on two opposite surfaces of the crystalline silicon layer 1, an N-type amorphous silicon layer 3 (na-Si:H) provided on a surface of the intrinsic amorphous silicon layer 2 away from the bulk silicon layer 1, and a P-type amorphous silicon layer 4 (pa-Si:H) provided on a surface of another intrinsic amorphous silicon layer 2 away from the bulk silicon layer 1.

[0057] S1. Preparing a transparent conductive oxide layer 5 on the battery substrate to obtain a blue film;

[0058] The structure of the blue film includes the above-mentioned battery substrate and a transparent conductive oxide layer 5 attached to the outer surfaces of the N-type amorphous silicon layer 3 and the P-type amorphous silicon layer 4 of the battery substrate.

[0059] S2. Prepare a bonding layer 6 on the blue film; the preparation method can be deposition.

[0060] Optionally, the material of the bonding layer 6 can be selected from at least one of SiOx and TiW. The bonding layer has a thickness of 580 nm. The thin film formed by SiOx and TiW has high transmittance in the visible light wavelength range, has no optical loss, can meet the above-mentioned transmittance requirements, and does not cause other effects on the solar cell.

[0061] The following description assumes that SiOx is used as the material for the bonding layer 6. Specifically, a PEVCD device is used to deposit a film on the transparent conductive oxide layer 5. The deposition time is 1-10 minutes, the silane flow rate is 100-1000 sccm, the carbon dioxide flow rate is 30-200 sccm, the process temperature is 100°C-200°C, the RF power is 200W-1000W, and the chamber pressure is 10Pa-50Pa. Alternatively, the deposition time can be 2-9 minutes, the silane flow rate is 300-900 sccm, the carbon dioxide flow rate is 40-100 sccm, the process temperature is 130°C-170°C, the RF power is 400W-800W, and the chamber pressure is 20Pa-40Pa. Alternatively, the deposition time can be 2 minutes, the silane flow rate is 800 sccm, the carbon dioxide flow rate is 80 sccm, the process temperature is 150°C, the RF power is 600W, and the chamber pressure is 30Pa.

[0062] Controlling the deposition time is mainly to control the film thickness to 5nm-80nm, which includes the purge time, gas introduction time and emptying time.

[0063] S3. Depositing a metal seed layer on the blue film having the bonding layer 6. Optionally, the metal seed layer is formed by magnetron sputtering. The metal seed layer may be a copper seed layer 71. Optionally, the copper seed layer 71 may have a thickness of 50 nm to 200 nm and a sputtering power of 2 kW to 8 kW. In other embodiments, the metal seed layer may be an aluminum seed layer.

[0064] S4. Annealing the battery substrate on which the metal seed layer is formed, so that holes are formed in the bonding layer, and the metal seed layer passes through the holes and is connected to the transparent conductive oxide layer.

[0065] Optionally, the metal seed layer is a copper seed layer 71 (yellow diaphragm), and the yellow diaphragm is annealed in an annealing furnace at a temperature of 180°C-200°C, including but not limited to 180°C, 185°C, 190°C, 195°C and 200°C, and a time of 5min-30min, including but not limited to 5min, 10min, 15min, 20min, 25min and 30min. Annealing is performed in a vacuum environment or under inert gas protection, and the inert gas can specifically be nitrogen.

[0066] The inventors have found that by controlling the annealing temperature to 180°C-200°C and the annealing time to 5min-30min, and combining the film thickness of the SiOx bonding layer 6 with that of 5nm-80nm, especially when the film thickness of the bonding layer 6 is 10nm-20nm, dense micropores can be formed on the bonding layer 6. The micropores penetrate the bonding layer 6, and the copper seed layer 71 can easily move through the dense micropores to form protrusions (the transparent conductive oxide layer 5 has good thermal stability and only has a slight amount of migration or movement, so the copper seed layer 71 passes through the dense micropores). The protrusions form a similar arc-surface contact with the transparent conductive oxide layer 5, thereby increasing the contact area between the copper seed layer 71 and the transparent conductive oxide layer, so that the gate line has a good flow diversion effect, which is beneficial to the extraction of the mid-flow, and the bonding strength between the copper seed layer 71 and the transparent conductive oxide layer 5 is also higher.

[0067] S5. Electroplating a metal grid line layer on the metal seed layer to obtain a solar cell. Optionally, the metal grid line layer is a copper grid line layer. In other embodiments, the metal grid line layer can also be an aluminum grid line layer.

[0068] In this embodiment, the preparation of the copper grid line layer 72 includes edging, coating, printing, developing, electroplating and film stripping and back engraving. Among them, edging specifically includes: wrapping the yellow film sheet after annealing with edging glue, and the width of the edging glue is 0.8mm-1.2mm. Coating specifically includes: applying photosensitive ink on the front and back sides of the yellow film sheet after edging, completely covering the front and back surfaces of the yellow film sheet, and controlling the thickness to 80μm-200μm; printing specifically includes: exposing the pre-designed grid line pattern by laser (wavelength 400nm-450nm) on the photosensitive ink, and the exposed part is subsequently dissolved in the development process. Development specifically includes using an alkaline solution to dissolve the exposed part of the ink to expose the underlying copper seed, and the unexposed part does not participate in the reaction. Electroplating specifically includes: electrochemically plating the copper grid line layer 72 and the tin layer 73, wherein the thickness of the copper grid line layer 72 is 5μm-20μm, and the thickness of the tin layer 73 is 3μm-10μm. The film stripping and etching back specifically include: using alkaline solution to remove all the photosensitive ink and side edge glue on the surface of the battery cell, and using acidic solution to soak and remove the copper seed layer 71 on the surface.

[0069] During the preparation of the copper grid line layer 72, especially when removing the excess copper seed layer 71, the inventors also discovered that since all surfaces of the transparent conductive oxide layer 5 are covered with the bonding layer 6, the bonding layer 6 can prevent the acidic liquid from corroding the transparent conductive oxide layer 5, thereby protecting the transparent conductive oxide layer 5 and further ensuring the optical and electrical performance of the solar cell.

[0070] S6. Perform light injection treatment on the solar cell to complete the cell preparation. In this embodiment, the light injection intensity is 60 solar light intensities, the temperature is controlled at 200°C, and the time is 60s to complete the production of the solar cell.

[0071] The present application will be further described below in conjunction with specific examples. It should be understood that these examples are intended to illustrate the present application only and are not intended to limit the scope of the present application. The experimental methods in the following examples where specific conditions are not specified are usually measured in accordance with national standards. If there are no corresponding national standards, then the methods are carried out in accordance with general international standards, conventional conditions, or according to the conditions recommended by the manufacturer.

[0072] Example 1

[0073] A method for preparing a solar cell, the method comprising:

[0074] S1. Prepare a blue film for a silicon-based heterojunction solar cell; the blue film layer structure of the solar cell is as follows: a first transparent conductive oxide (TCO) layer, an N-type amorphous silicon layer (na-Si:H), an intrinsic amorphous silicon layer (ia-Si:H), a crystalline silicon (C-Si), an intrinsic amorphous silicon layer (ia-Si:H), a P-type amorphous silicon layer (pa-Si:H), and a second transparent conductive oxide (TCO) layer;

[0075] S2. Use a PEVCD device to deposit a first SiOx layer and a second SiOx layer on the transparent conductive oxide layer. The thickness of the first SiOx layer and the second SiOx layer is 5 nm. The deposition time is 1 min, the silane flow rate is 500 sccm, the carbon dioxide flow rate is 100 sccm, the process temperature is 150°C, the RF power is 600 W, and the chamber pressure is 30 Pa.

[0076] S3. A copper seed layer was prepared by sputtering on the first Si0x layer and the second Si0x layer of the blue film to obtain a yellow film. The thickness of the copper seed layer was 100nm and the sputtering power was 5kW.

[0077] S4. Anneal the cell in an annealing furnace at 190°C for 18 minutes in a vacuum environment or under nitrogen protection.

[0078] S5. Wrap the yellow film around the edges with 1mm of edging glue.

[0079] S6. Apply photosensitive ink on the front and back of the yellow film, completely covering the front and back surfaces of the yellow film, with a thickness of 150um.

[0080] S7. Expose the pre-designed grid line pattern on the photosensitive ink through laser printing. The exposed part is subsequently dissolved in the development process. The laser wavelength of the laser printing is 430nm.

[0081] S8. Use an alkaline solution to dissolve the exposed portion of the ink to expose the underlying copper seed. The unexposed portion does not participate in the reaction.

[0082] S9. Electrochemically plate a copper grid line layer and a tin layer, where the thickness of the copper grid line layer is 12 μm and the thickness of the tin layer is 6 μm.

[0083] S10. Use alkaline solution to remove all photosensitive ink and side edge glue on the surface of the battery cell.

[0084] S11. Soak in acidic solution to remove the copper seed layer on the surface.

[0085] S12. Perform light injection treatment on the solar cell to complete the cell preparation. The light injection intensity is 60 solar intensities, the temperature is controlled at 200°C, and the time is 60 seconds to complete the production of the solar cell.

[0086] Example 2

[0087] Except for step S2 and step S4, the remaining steps of this embodiment are the same as those of embodiment 1.

[0088] Step S2 of this embodiment is specifically as follows: S2. Use PEVCD equipment to deposit a first Si0x layer and a second Si0x layer on the transparent conductive oxide layer. The thickness of the first Si0x layer and the second Si0x layer is 20 nm, the deposition time is 3 min, the silane flow rate is 500 sccm, the carbon dioxide flow rate is 100 sccm, the process temperature is 150°C, the RF power is 600 W, and the chamber pressure is 30 Pa.

[0089] The specific steps of step S4 in this embodiment are as follows: S4. Annealing the cell in an annealing furnace at a temperature of 180° C. for 5 minutes in a vacuum environment or under nitrogen protection.

[0090] Example 3

[0091] Except for step S2 and step S4, the remaining steps of this embodiment are the same as those of embodiment 1.

[0092] Step S2 of this embodiment is specifically as follows: S2. Use PEVCD equipment to deposit a first SiOx layer and a second SiOx layer on the transparent conductive oxide layer. The thickness of the first SiOx layer and the second SiOx layer is 80 nm, the deposition time is 8 min, the silane flow rate is 500 sccm, the carbon dioxide flow rate is 100 sccm, the process temperature is 150°C, the RF power is 600 W, and the chamber pressure is 30 Pa.

[0093] The specific steps of step S4 in this embodiment are as follows: S4. Annealing the cell in an annealing furnace at a temperature of 200° C. for 30 minutes in a vacuum environment or under nitrogen protection.

[0094] Example 4

[0095] Except for step S2, the remaining steps of this embodiment are the same as those in Example 1.

[0096] Step S2 of this embodiment is specifically as follows: S2. Using a PEVCD device, a first SiOx layer and a second SiOx layer are deposited on the transparent conductive oxide layer. The thickness of the first SiOx layer and the second SiOx layer is 100 nm, the deposition time is 10 min, the silane flow rate is 500 sccm, the carbon dioxide flow rate is 100 sccm, the process temperature is 150° C., the RF power is 600 W, and the chamber pressure is 30 Pa.

[0097] Example 5

[0098] Except for step S2, the remaining steps of this embodiment are the same as those of embodiment 1.

[0099] Step S2 of this embodiment is specifically as follows: S2. Use a PEVCD device to deposit a first Si0x layer and a second Si0x layer on the transparent conductive oxide layer. The thickness of the first Si0x layer and the second Si0x layer is 10 nm, the deposition time is 1.5 min, the silane flow rate is 500 sccm, the carbon dioxide flow rate is 100 sccm, the process temperature is 150°C, the RF power is 600 W, and the chamber pressure is 30 Pa.

[0100] Example 6

[0101] Except step S4, the remaining steps of this embodiment are the same as those of embodiment 1.

[0102] The specific steps of step S4 in this embodiment are as follows: S4. Annealing the cell in an annealing furnace at a temperature of 200° C. for 50 min in a vacuum environment or under nitrogen protection.

[0103] Example 7

[0104] Except step S4, the remaining steps of this embodiment are the same as those of embodiment 1.

[0105] The specific step S4 of this embodiment is as follows: S4. Annealing the battery cell in an annealing furnace at a temperature of 150° C. for 18 minutes in a vacuum environment or under ammonia protection.

[0106] Comparative Example 1

[0107] In this comparative example, step S2 and step S4 in Example 1 are not performed, and the remaining steps are the same as those in Example 1.

[0108] Comparative Example 2

[0109] In this comparative example, step S4 in Example 1 was not performed, and the remaining steps were the same as in Example 1.

[0110] The main parameter controls of Examples 1-7 and Comparative Examples 1-2 are shown in the following table:

[0111] In the table, “ / ” means not performed.

[0112] The solar cells provided in Examples 1-6 and Comparative Examples 1-2 were subjected to performance tests, and the results are shown in the following table:

[0113] Among them, the battery efficiency test is carried out using a solar cell IV tester, the tensile test is carried out using a solar cell tensile tester, and the DH1000 attenuation value refers to: after the battery cell is laminated into a small component, the power attenuation value is carried out after the wet heat test for 1000 hours.

[0114] By comparing Example 1 with the various embodiments, it can be seen that the grid line adhesion of the solar cell prepared by the method provided in the embodiments of the present application is significantly improved, and the main grid tension of the battery is increased by at least 1.06N, which is about 71.62%. By comparing Examples 1-5, it can be seen that as the thickness of the bonding layer increases, the DH1000 attenuation value decreases, indicating that the thicker the thickness, the stronger its blocking ability, but the battery efficiency also decreases accordingly. By comparing Example 7 with Example 1, it can be seen that the annealing temperature will affect the main grid tension of the battery. As the annealing temperature increases, the main grid tension of the battery is greater, and the grid line adhesion is better.

[0115] The foregoing description is merely a specific embodiment of the present application and is not intended to limit the present application. Persons skilled in the art will readily appreciate that various modifications and variations are possible. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present application shall be included within the scope of protection of the present application.

Claims

1. A solar cell, comprising a cell substrate, wherein at least one surface of the cell substrate has a transparent conductive oxide layer, a bonding layer having holes is attached to the transparent conductive oxide layer, a metal electrode is arranged on the bonding layer, and a side of the metal electrode close to the bonding layer passes through the holes and is connected to the transparent conductive oxide layer.

2. The solar cell according to claim 1, wherein: The material of the bonding layer is a transparent material; the bonding layer covers the entire surface of the transparent conductive oxide layer.

3. The solar cell according to claim 2, wherein: The light transmittance of the bonding layer is not less than 93%.

4. The solar cell according to claim 3, wherein: The material of the bonding layer includes at least one of SiOx and TiW, wherein the value of x is 1-2.

5. The solar cell according to any one of claims 1 to 4, wherein: The thickness of the bonding layer is no more than 80 nm.

6. The solar cell according to claim 5, wherein: The thickness of the bonding layer is 5nm-80nm.

7. The solar cell according to claim 1, wherein: The metal electrode includes a metal seed layer and a metal grid line layer which are stacked, and the metal seed layer passes through the holes of the bonding layer and is connected to the transparent conductive oxide layer.

8. The solar cell according to claim 7, wherein: The metal seed layer is a copper seed layer, and the metal gate line layer is a copper gate line layer.

9. A method for preparing a solar cell, the method comprising: Providing a battery substrate, wherein at least one surface of the battery substrate is provided with a transparent conductive oxide layer; Depositing a bonding layer on the surface of the transparent conductive oxide layer; depositing a metal seed layer on the bonding layer; Annealing the battery substrate on which the metal seed layer is formed so that holes are formed in the bonding layer. The metal seed layer passes through the hole and is connected to the transparent conductive oxide layer; A metal grid line layer is formed on the metal seed layer by electroplating to obtain a solar cell.

10. The method for preparing a solar cell according to claim 9, wherein: The material of the bonding layer includes at least one of SiOx and TiW, wherein the value of x is 1-2.

11. The method for preparing a solar cell according to any one of claims 9 to 10, wherein: The metal seed layer is a copper seed layer, and the metal gate line layer is a copper gate line layer.

12. The method for preparing a solar cell according to claim 11, wherein: The thickness of the bonding layer is 5nm-80nm; the temperature of the annealing treatment is 180°C-200°C; and the time of the annealing treatment is 5min-30min.

13. The method for preparing a solar cell according to any one of claims 9 to 12, wherein: The annealing process is carried out in a vacuum environment or an inert gas atmosphere environment.