Wear-resistant non-slip light-transmitting shoe material and preparation method therefor

Through a specific proportion of raw material mixing and preparation process, the problem of insufficient quality of traditional EVA shoe materials is solved, and high elasticity, anti-slip, wear resistance and light transmittance are achieved. It is suitable for shoe materials of various colors and satisfies consumers' demand for shoe materials. Quality improvement needs.

WO2024197502A1PCT designated stage expired Publication Date: 2024-10-03TANG HOUGUANG +1

Patent Information

Application Number
PCT/CN2023/083946
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Traditional EVA shoe materials are heavy in quality, do not have high elasticity, have poor anti-slip and wear resistance, and do not have light transmittance properties, making them unable to meet consumers' demands for improved shoe material quality.

Method used

Wear-resistant, anti-slip and translucent shoe materials are made of a specific ratio of EVA plastic particles, modifiers, POE elastomers, glass sand, bridging cross-linking agents, foaming agents, initiators, photo-storage powder and zinc oxide. Materials and prepared through mixing, calendering and granulation steps.

Benefits of technology

It achieves high elasticity, anti-slip and wear-resistant characteristics without adding expensive rubber. It also has light transmittance and night-time light storage function. The material is lighter, suitable for a variety of colors, and meets the design sense and safety requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 000001
    Figure 000001
  • Figure 000002
    Figure 000002
  • Figure 000003
    Figure 000003
Patent Text Reader

Abstract

Disclosed are a wear-resistant non-slip light-transmitting shoe material and a preparation method therefor. The shoe material is prepared by mixing the following raw materials in parts by weight: 32-38 parts of EVA plastic particles, 4.5-6.5 parts of a modifier, 9-12 parts of a POE elastomer, 2.5-4 parts of glass sand, 0.3-0.6 parts of a bridging crosslinker, 0.8-1.3 parts of a first foaming agent, 0.4-0.8 parts of a second foaming agent, 0.3-0.6 parts of an initiator, 0.03-0.1 parts of a light-storage powder, and 0.4-0.8 parts of zinc oxide. The preparation method for the wear-resistant non-slip light-transmitting shoe material comprises the following steps: material acquisition and treatment, internal mixing and material beating, rolling treatment, and granulation. The shoe material meets the requirements of consumers and is more comfortable; a product thereof can make direct contact with the ground; and the shoe material has good dry and wet anti-slip characteristics, is lightweight, has good elasticity, can reduce the burden on feet, also is light-transmissive and has high safety, and can satisfy the sense of design.
Need to check novelty before this filing date? Find Prior Art

Description

Wear-resistant, non-slip, and light-transmitting shoe material and preparation method thereof Technical Field

[0001] The invention relates to a shoe material, in particular to a wear-resistant, non-slip and light-transmitting shoe material and a preparation method thereof. Background Art

[0002] Shoes are a tool for people to protect their feet from injury. People first invented fur shoes to overcome special situations and prevent their feet from feeling uncomfortable or injured.

[0003] Common properties of shoe sole materials include resistance to wear, water, oil, heat, pressure, and impact, good elasticity, easy conforming to the foot shape, resistance to deformation after shaping, heat preservation, and moisture absorption. Furthermore, they must complement the midsole to provide a braking effect when changing feet while walking, preventing slipping and making it easy to stop. There are many types of sole materials, which can be divided into natural and synthetic. Natural sole materials include natural leather, bamboo, and wood, while synthetic sole materials include rubber, plastic, rubber-plastic composites, recycled leather, and elastic cardboard.

[0004] EVA shoe material is made from ethylene-vinyl acetate copolymer. Compared to polyethylene, EVA incorporates vinyl acetate monomer into its molecular chain, resulting in lower crystallinity and improved flexibility, impact resistance, filler compatibility, and heat sealing properties. An EVA midsole, also known as a single-shot foam midsole, is formed by injecting EVA into a mold and then heating it at high temperatures. Traditionally, EVA is heat-pressed. An EVA injection molding machine injects EVA particles directly into a mold. After vacuum vulcanization for approximately 400 seconds, the mold is opened, allowing the in-mold sole to foam and form, which is then set in hot and cold setting chambers. This production method boasts high yields and a single-shot molding process, making it suitable for industrial production. However, it is susceptible to deformation, yellowing, and shrinkage over time.

[0005] Traditional EVA shoe materials also have drawbacks such as being heavy, lacking high elasticity, poor slip resistance, and abrasion resistance, making them impractical for consumers to wear directly on the ground. To achieve high functionality, traditional EVA shoe materials typically require the addition of expensive rubber, increasing manufacturing costs. Furthermore, traditional EVA shoe materials lack light transmittance, and even when light-transmitting EVA materials are available, they are limited to white.

[0006] As consumers' requirements for shoe material quality increase, traditional EVA shoe materials can no longer meet consumer needs. Technical issues

[0007] The technical problem to be solved by the present invention is to address the deficiencies of the above-mentioned existing technologies and provide a wear-resistant, anti-slip, and light-transmitting shoe material that meets consumer needs, is more comfortable, can directly contact the ground, has good dry and wet anti-slip properties, is lightweight, has good elasticity, can reduce the burden on the feet, and is light-transmitting, highly safe, and can meet the design requirements. To this end, the present invention also provides a method for preparing the wear-resistant, anti-slip, and light-transmitting shoe material. Solution

[0008] In order to solve the above technical problems, the first technical solution of the present invention is: a wear-resistant, non-slip and light-transmitting shoe material, which is made by mixing the following raw materials in parts by weight: 32 to 38 parts of EVA plastic particles, 4.5 to 6.5 parts of modifiers, 9 to 12 parts of POE elastomers, 2.5 to 4 parts of glass sand, 0.3 to 0.6 parts of bridging cross-linking agents, 0.8 to 1.3 parts of first foaming agents, 0.4 to 0.8 parts of second foaming agents, 0.3 to 0.6 parts of initiators, 0.03 to 0.1 parts of light-storage powder, and 0.4 to 0.8 parts of zinc oxide; the modifier is selected from ethylene-octene block copolymer, Any one or more of styrene block copolymer, ethylene vinyl acetate copolymer, soft chloroethylene or flexible polyolefin; the first foaming agent is any one or more of DUST transparent foaming agent, HCFC-14LB foaming agent, HFC-152A foaming agent; the second foaming agent is any one or more of ACP foaming agent, AC foaming agent, modified carbonate foaming agent, magnesium oxysulfate composite foaming agent, ADC foaming agent; the initiator is any one or more of DCP, MCP, ACTOR-TDDS, ACCEL-BF, TMPTMA-70.

[0009] As a further elaboration of the present invention:

[0010] Preferably, it is made by mixing the following raw materials in parts by weight: 33 to 36 parts of EVA plastic particles, 4.5 to 6.0 parts of modifier, 9 to 11 parts of POE elastomer, 2.5 to 3 parts of glass sand, 0.3 to 0.5 parts of bridging crosslinking agent, 0.9 to 1.2 parts of first foaming agent, 0.5 to 0.7 parts of second foaming agent, 0.3 to 0.5 parts of initiator, 0.04 to 0.08 parts of luminescent powder, and 0.5 to 0.7 parts of zinc oxide; the POE elastomer is selected from any one or more of DF610 POE elastomer, 9061 POE elastomer, 7378 POE elastomer, 8605L POE elastomer, and C5070D POE elastomer; the particle size of the glass sand is 400 μm to 800 μm; the bridging crosslinking agent is selected from PL 400, PL 500, TAIC, LS-3-80 or any one or more thereof; the luminescent powder is a long-lasting luminescent powder that can emit bright light at night; the zinc oxide particle size is 1.62 μm to 2.25 μm.

[0011] Preferably, a flow agent is further included, wherein the weight portion of the flow agent is 0 to 0.3 parts, and any one of MA-St and POKM330F or a mixture of the two is selected.

[0012] Preferably, it also includes an anti-wear agent, the weight portion of the anti-wear agent is 1.5 to 2.5 parts, and ultra-high molecular weight silicone resin DX067 or ultra-high molecular weight silicone resin DX053E is selected.

[0013] Preferably, an anti-slip agent is also included, and the weight portion of the anti-slip agent is 0.8 to 1.3 parts, and the anti-slip agent is selected from high molecular weight polyethylene, polypropylene, and butadiene block copolymer.

[0014] Preferably, the invention also includes a masterbatch, which is added to enhance the color of the shoe material according to the color of the shoe material, with a weight portion of 0.003 to 0.006 parts.

[0015] As a second technical solution of the present invention, a method for preparing a wear-resistant, non-slip, and light-transmitting shoe material comprises the following steps:

[0016] S1. Material processing: weigh the EVA plastic particles, modifier, POE elastomer, glass sand, bridging cross-linking agent, first foaming agent, second foaming agent, initiator, luminescent powder, zinc oxide, flow agent and other raw materials according to the above proportions, with a raw material weighing tolerance of ±0.1 g;

[0017] S2. Internal mixer: Check the power supply and switch of the internal mixer to see if they are normal. Add half of the EVA plastic pellets, modifier, POE elastomer, glass sand, phosphorescent powder, zinc oxide, flow agent and the other half of the EVA plastic pellets in sequence, press the hammer, and start the mixer to mix. When the temperature of the internal mixer reaches 95°C, clean the dust on the edge and turn the material over. When the temperature of the internal mixer reaches 100°C, add the bridging agent, the first foaming agent, the second foaming agent and the initiator, press the hammer halfway, mix for 40 seconds, and then press the hammer fully. When the temperature of the internal mixer reaches 110°C ± 2°C, start pouring the material into the turbine and clean the machine to ensure that there is no residue.

[0018] S3. Calendering treatment: Use a roller mill to calender according to the following steps: 4mm-6mm thick twice, 1mm-2mm thin twice, 4mm-6mm thick once to start granulation;

[0019] S4. Granulation: Check whether the power temperature of the granulator reaches the set value, 75℃ for the first section, 75℃ for the second section, 75℃ for the third section, and 80℃ for the die head; pour the calendered material into the granulator and start discharging. After the discharge is clean, install the die head and start granulation to make wear-resistant, non-slip and translucent shoe materials.

[0020] Preferably, after the granulation starts in step S4, the vibrating screen, fan, cutter, and main machine are turned on in sequence, and the cutter is adjusted to form suitable wear-resistant, non-slip, and light-transmitting shoe material particles; the die head needs to be cleaned after the granulation is completed. Beneficial effects

[0021] The beneficial effects of the present invention are:

[0022] First, the formula of the present invention has high elasticity, anti-slip and wear-resistant characteristics without adding expensive rubber. At the same time, it allows colored materials, including light black, to be light-transmissive (the light-transmissiveness mentioned here does not mean that the sole is transparent, but rather that the glass sand forms a concave and convex three-dimensional surface, which makes the sole light-transmissive. When LED lights are installed inside the sole, the glass sand particles can achieve light transmission).

[0023] Secondly, the glass sand of the present invention inherently possesses excellent wear resistance and anti-slip properties, allowing the shoe material to possess these EVA property-modifying functions without the addition of wear-resistant and anti-slip agents. Furthermore, the addition of wear-resistant and anti-slip agents further enhances these properties, achieving even better wear resistance and anti-slip properties. The addition of glass sand enhances the light transmittance, wear resistance, and anti-slip properties of EVA, increases the density of the shoe material, and maintains a better degree of maturation (increasing elasticity). The combination with a transparent foaming agent (at a medium temperature) enhances these functionalities.

[0024] Thirdly, the material of the present invention is relatively light, and the addition of a small amount of phosphorescent powder allows the EVA material to have a nighttime light-storage function (once stored, it can remain luminous for about 30 minutes). This emits bright light at night, allowing wearers to exercise in the absence of light, thereby increasing the safety of consumers when exercising at night.

[0025] Fourthly, the soles made from the material of the present invention provide a cushion-like comfort when worn. While the elasticity of typical EVA is only around 45%, this material can reach nearly 55%. It also offers excellent dry and wet anti-slip properties, overcoming the drawback of existing EVA formulas that struggle to achieve this effect without the addition of expensive rubber. Furthermore, it also offers superior wear resistance.

[0026] Fifth, the sole made of the EVA material of the present invention can be used in direct contact with the ground without a rubber lining, which greatly reduces the production cost of the material. At the same time, the sole can be made into a slipper-like sole that directly contacts the skin and has a more comfortable touch.

[0027] Sixth, breaking the current situation where the color of light-transmitting EVA materials on the market is limited to white, the shoe materials prepared by the material of the present invention can be made into various colors without affecting its light transmittance, which can meet the needs of shoe designers;

[0028] Seventh, the addition of a bridging cross-linking agent makes the particle shape more dispersed and the application efficiency higher. The addition of an initiator can increase the cross-linking density and reduce the cross-linking time. At the same time, it increases the degree of vulcanization and reduces the amount of bridging cross-linking agent. It can also significantly improve the mechanical strength, wear resistance, weather resistance, solvent resistance and corrosion resistance of the shoe material. Modes for Carrying Out the Invention

[0029] The present invention is further described in detail below through specific embodiments.

[0030] The invention discloses a wear-resistant, non-slip and light-transmitting shoe material, which is prepared by mixing the following raw materials in parts by weight: 32 to 38 parts of EVA plastic particles, 4.5 to 6.5 parts of a modifier, 9 to 12 parts of a POE elastomer, 2.5 to 4 parts of glass sand, 0.3 to 0.6 parts of a bridging cross-linking agent, 0.8 to 1.3 parts of a first foaming agent, 0.4 to 0.8 parts of a second foaming agent, 0.3 to 0.6 parts of an initiator, 0.03 to 0.1 parts of a light-storage powder and 0.4 to 0.8 parts of zinc oxide; the modifier is selected from ethylene-octene block copolymer, styrene block copolymer and the like. , ethylene vinyl acetate copolymer, soft chloroethylene or flexible polyolefin; the first foaming agent is any one or more of DUST transparent foaming agent, HCFC-14LB foaming agent, HFC-152A foaming agent; the second foaming agent is any one or more of ACP foaming agent, AC foaming agent, modified carbonate foaming agent, magnesium oxysulfate composite foaming agent, ADC foaming agent; the initiator is any one or more of DCP, MCP, ACTOR-TDDS, ACCEL-BF, TMPTMA-70.

[0031] Furthermore, the invention is prepared by mixing the following raw materials in parts by weight: 33 to 36 parts of EVA plastic particles, 4.5 to 6.0 parts of modifier, 9 to 11 parts of POE elastomer, 2.5 to 3 parts of glass sand, 0.3 to 0.5 parts of bridging crosslinking agent, 0.9 to 1.2 parts of first foaming agent, 0.5 to 0.7 parts of second foaming agent, 0.3 to 0.5 parts of initiator, 0.04 to 0.08 parts of luminescent powder, and 0.5 to 0.7 parts of zinc oxide; the POE elastomer is selected from any one or more of DF610 POE elastomer, 9061 POE elastomer, 7378 POE elastomer, 8605L POE elastomer, and C5070D POE elastomer; the particle size of the glass sand is 400 μm to 800 μm; the bridging crosslinking agent is selected from PL 400, PL 500, TAIC, LS-3-80 or any one or more thereof; the luminescent powder is a long-lasting luminescent powder that can emit bright light at night; the zinc oxide particle size is 1.62 μm to 2.25 μm.

[0032] Furthermore, the invention further comprises a flow agent, wherein the weight portion of the flow agent is 0 to 0.3 parts, and the flow agent is selected from any one of MA-St and POKM330F or a mixture of the two.

[0033] Furthermore, it also includes an anti-wear agent, the weight portion of the anti-wear agent is 1.5 to 2.5 parts, and ultra-high molecular weight silicone resin DX067 or ultra-high molecular weight silicone resin DX053E is selected.

[0034] Furthermore, an anti-slip agent is included, and the weight portion of the anti-slip agent is 0.8 to 1.3 parts, and the anti-slip agent is selected from high molecular weight polyethylene, polypropylene, and butadiene block copolymer.

[0035] Furthermore, it also includes masterbatch, which is added to the shoe material to enhance the color of the shoe material according to the color of the shoe material, with a weight portion of 0.003 to 0.006 parts.

[0036] The following are specific examples of materials and preparation methods. Example 1

[0037] The wear-resistant, non-slip and light-transmitting shoe material is made by mixing the following raw materials in parts by weight: 32 parts of EVA plastic particles, 4.5 parts of modifier, 9 parts of POE elastomer, 2.5 parts of glass sand, 0.3 parts of bridging cross-linking agent, 0.8 parts of first foaming agent, 0.4 parts of second foaming agent, 0.3 parts of initiator, 0.03 parts of light-storage powder, and 0.4 parts of zinc oxide; the modifier is selected from a variety of styrene block copolymer, ethylene vinyl acetate copolymer, soft chloroethylene or flexible polyolefin; the first foaming agent is selected from a variety of HCFC-14LB foaming agent and HFC-152A foaming agent; the second foaming agent is selected from a variety of ACP foaming agent, AC foaming agent, and modified carbonate foaming agent ADC foaming agent; the initiator is selected from a variety of DCP, MCP, ACTOR-TDDS, ACCEL-BF, and TMPTMA-70; the POE elastomer is selected from 9061 POE elastomer, 7378 POE elastomer, 8605L POE elastomer, C5070D POE elastomer; the glass sand particle size is 400μm~800μm; the bridging cross-linking agent is selected from PL 500, TAIC, LS-3-80; the luminescent powder is a long-lasting luminescent powder that can emit bright light at night; the zinc oxide particle size is 1.62μm~2.25μm; the wear-resistant agent is 1.5 parts by weight, and ultra-high molecular weight silicone resin DX067 or ultra-high molecular weight silicone resin DX053E is selected; the anti-slip agent is 0.8 parts by weight, and high molecular weight polyethylene, polypropylene, butadiene block copolymer is selected; the masterbatch is added according to the color of the shoe material to enhance the color of the shoe material. In this embodiment, black masterbatch is selected, and the weight portion is 0.003 parts. Example 2

[0038] The wear-resistant, non-slip and light-transmitting shoe material is made by mixing the following raw materials in parts by weight: 38 parts of EVA plastic particles, 6.5 parts of modifier, 12 parts of POE elastomer, 4 parts of glass sand, 0.6 parts of bridging cross-linking agent, 1.3 parts of first foaming agent, 0.8 parts of second foaming agent, 0.6 parts of initiator, 0.1 parts of luminescent powder, 0.8 parts of zinc oxide, and 0.3 parts of flow agent; the modifier is selected from multiple types of ethylene-octene block copolymer, soft chloroethylene or flexible polyolefin; the first foaming agent is selected from a mixture of DUST transparent foaming agent and HCFC-14LB foaming agent; the second foaming agent is selected from multiple types of ACP foaming agent, magnesium oxysulfate composite foaming agent, and ADC foaming agent; the initiator is selected from multiple types of DCP, ACCEL-BF, and TMPTMA-70; the POE elastomer is selected from DF610 POE elastomer, 9061 POE elastomer, 7378 Various POE elastomers; the glass sand particle size is 400μm~800μm; the bridging cross-linking agent is selected from various PL 400, PL 500, and TAIC; the luminescent powder is a long-lasting luminescent powder that can emit bright light at night; the zinc oxide particle size is 1.62μm~2.25μm; the flow agent is a mixture of MA-St and POKM330F; the wear-resistant agent is 2.5 parts by weight, and ultra-high molecular weight silicone resin DX067 or ultra-high molecular weight silicone resin DX053E is selected; the anti-slip agent is 1.3 parts by weight, and polymer polyethylene, polypropylene, and butadiene block copolymer are selected; the masterbatch is added according to the color of the shoe material to enhance the color of the shoe material. In this embodiment, black masterbatch is selected, and the weight portion is 0.006 parts. Example 3

[0039] The wear-resistant, non-slip and light-transmitting shoe material is made by mixing the following raw materials in parts by weight: 33 parts of EVA plastic particles, 4.5 parts of modifier, 9 parts of POE elastomer, 2.5 parts of glass sand, 0.3 parts of bridging cross-linking agent, 0.9 parts of first foaming agent, 0.5 parts of second foaming agent, 0.3 parts of initiator, 0.04 parts of light-storage powder, and 0.5 parts of zinc oxide; the modifier is selected from a variety of ethylene-octene block copolymer, styrene block copolymer, and flexible polyolefin; the first foaming agent is selected from a variety of DUST transparent foaming agent, HCFC-14LB foaming agent, and HFC-152A foaming agent; the second foaming agent is selected from any variety of ACP foaming agent, AC foaming agent, and modified carbonate foaming agent; the initiator is selected from a variety of ACTOR-TDDS, ACCEL-BF, and TMPTMA-70; the POE elastomer is selected from DF610 POE elastomer, 9061 POE elastomer, 7378 POE elastomer, 8605L POE elastomer, any of various types; the glass sand particle size is 400μm to 800μm; the bridging cross-linking agent is selected from PL 400, PL 500, and LS-3-80; the luminescent powder is a long-lasting luminescent powder that can emit bright light at night; the zinc oxide particle size is 1.62μm to 2.25μm; the wear-resistant agent is 2.0 parts by weight, and is selected from ultra-high molecular weight silicone resin DX067 or ultra-high molecular weight silicone resin DX053E; the anti-slip agent is 1.0 parts by weight, and is selected from high molecular weight polyethylene, polypropylene, and butadiene block copolymer; the masterbatch is added according to the color of the shoe material to enhance the color of the shoe material. In this embodiment, black masterbatch is selected, and the weight portion is 0.005 parts. Example 4

[0040] The wear-resistant, non-slip and light-transmitting shoe material is made by mixing the following raw materials in parts by weight: 36 parts of EVA plastic particles, 6.0 parts of modifier, 11 parts of POE elastomer, 3 parts of glass sand, 0.5 parts of bridging cross-linking agent, 1.2 parts of first foaming agent, 0.7 parts of second foaming agent, 0.5 parts of initiator, 0.08 parts of luminescent powder, 0.7 parts of zinc oxide, and 0.3 parts of flow agent; the modifier is selected from multiple types of ethylene-octene block copolymer, styrene block copolymer, soft chloroethylene or flexible polyolefin; the first foaming agent is selected from a mixture of DUST transparent foaming agent and HCFC-14LB foaming agent; the second foaming agent is selected from multiple types of ACP foaming agent, AC foaming agent, and modified carbonate foaming agent; the initiator is selected from multiple types of DCP, ACCEL-BF, and TMPTMA-70; the POE elastomer is selected from DF610 POE elastomer, 7378 POE elastomer, C5070D Various POE elastomers; the glass sand particle size is 400μm~800μm; the bridging cross-linking agent is selected from various PL 400, PL 500, and TAIC; the luminescent powder is a long-lasting luminescent powder that can emit bright light at night; the zinc oxide particle size is 1.62μm~2.25μm; the flow agent is MA-St; the wear-resistant agent is 2.3 parts by weight, and ultra-high molecular weight silicone resin DX067 or ultra-high molecular weight silicone resin DX053E is selected; the anti-slip agent is 1.1 parts by weight, and high molecular weight polyethylene, polypropylene, and butadiene block copolymer are selected; the masterbatch is added according to the color of the shoe material to enhance the color of the shoe material. In this embodiment, black masterbatch is selected, and the weight portion is 0.003 parts. Example 5

[0041] The wear-resistant, non-slip and light-transmitting shoe material is made by mixing the following raw materials in parts by weight: 35 parts of EVA plastic particles, 5.0 parts of modifier, 10 parts of POE elastomer, 3 parts of glass sand, 0.4 parts of bridging cross-linking agent, 1.0 parts of first foaming agent, 0.6 parts of second foaming agent, 0.42 parts of initiator, 0.05 parts of luminescent powder, and 0.6 parts of zinc oxide; the modifier is an ethylene-octene block copolymer; the first foaming agent is a DUST transparent foaming agent; the second foaming agent is an ACP foaming agent; the initiator is DCP; the POE elastomer is DF610 POE elastomer; the particle size of the glass sand is 400μm to 800μm; the bridging cross-linking agent is PL 400; the luminescent powder is a long-lasting luminescent powder that can emit bright light at night; the zinc oxide particle size is 1.62μm to 2.25μm; the anti-wear agent is 2.0 parts by weight, and is selected from ultra-high molecular weight silicone resin DX067 or ultra-high molecular weight silicone resin DX053E; the anti-slip agent is 1.0 parts by weight, and is selected from high molecular weight polyethylene, polypropylene, and butadiene block copolymer; the masterbatch is added to the shoe material according to the color of the shoe material to enhance the color of the shoe material. In this embodiment, black masterbatch is selected, and the weight portion is 0.004 parts. Example 6

[0042] The wear-resistant, non-slip and light-transmitting shoe material is made by mixing the following raw materials in parts by weight: 34 parts of EVA plastic particles, 5.0 parts of modifier, 9.5 parts of POE elastomer, 3 parts of glass sand, 0.4 parts of bridging cross-linking agent, 1.1 parts of first foaming agent, 0.5 parts of second foaming agent, 0.4 parts of initiator, 0.06 parts of luminescent powder, 0.5 parts of zinc oxide, and 0.2 parts of flow agent; the modifier is a mixture of ethylene-octene block copolymer and styrene block copolymer; the first foaming agent is selected from a variety of DUST transparent foaming agent, HCFC-14LB foaming agent, and HFC-152A foaming agent; the second foaming agent is selected from a variety of ACP foaming agent, AC foaming agent, and ADC foaming agent; the initiator is selected from a variety of DCP, MCP, and TMPTMA-70; the POE elastomer is selected from DF610 POE elastomer, 9061 POE elastomer, 7378 Various POE elastomers; the glass sand particle size is 400μm~800μm; the bridging cross-linking agent is selected from various PL 400, PL 500, and LS-3-80; the luminescent powder is a long-lasting luminescent powder that can emit bright light at night; the zinc oxide particle size is 1.62μm~2.25μm; the flow agent is MA-St; the wear-resistant agent is 2.3 parts by weight, and is selected from ultra-high molecular weight silicone resin DX067 or ultra-high molecular weight silicone resin DX053E; the anti-slip agent is 1.1 parts by weight, and is selected from high molecular weight polyethylene, polypropylene, and butadiene block copolymer; the masterbatch is added according to the color of the shoe material to enhance the color of the shoe material. In this embodiment, black masterbatch is selected, and the weight portion is 0.005 parts. Example 7

[0043] The wear-resistant, non-slip and light-transmitting shoe material is made by mixing the following raw materials in parts by weight: 33 parts of EVA plastic particles, 4.5 parts of modifier, 9 parts of POE elastomer, 2.5 parts of glass sand, 0.3 parts of bridging cross-linking agent, 0.9 parts of first foaming agent, 0.5 parts of second foaming agent, 0.3 parts of initiator, 0.04 parts of luminescent powder, and 0.5 parts of zinc oxide; the modifier is ethylene-octene block copolymer; the first foaming agent is DUST transparent foaming agent; the second foaming agent is ACP foaming agent; the initiator is DCP; the POE elastomer is DF610 POE elastomer; the particle size of the glass sand is 400μm to 800μm; the bridging cross-linking agent is PL 400; the luminescent powder is a long-lasting luminescent powder that can emit bright light at night; the zinc oxide particle size is 1.62μm to 2.25μm; the anti-wear agent is 1.8 parts by weight, and is selected from ultra-high molecular weight silicone resin DX067 or ultra-high molecular weight silicone resin DX053E; the anti-slip agent is 1.3 parts by weight, and is selected from high molecular weight polyethylene, polypropylene, and butadiene block copolymer; the masterbatch is added to the shoe material according to the color of the shoe material to enhance the color of the shoe material. In this embodiment, black masterbatch is selected, and the weight portion is 0.004 parts. Example 8

[0044] The wear-resistant, non-slip and light-transmitting shoe material is made by mixing the following raw materials in parts by weight: 36 parts of EVA plastic particles, 6.0 parts of modifier, 11 parts of POE elastomer, 3 parts of glass sand, 0.5 parts of bridging cross-linking agent, 1.2 parts of first foaming agent, 0.7 parts of second foaming agent, 0.5 parts of initiator, 0.08 parts of luminescent powder, 0.7 parts of zinc oxide, and 0.3 parts of flow agent; the modifier is ethylene-octene block copolymer; the first foaming agent is DUST transparent foaming agent; the second foaming agent is ACP foaming agent; the initiator is DCP; the POE elastomer is DF610 POE elastomer; the particle size of the glass sand is 400μm to 800μm; the bridging cross-linking agent is PL 400; the luminescent powder is a long-lasting luminescent powder that can emit bright light at night; the zinc oxide particle size is 1.62μm to 2.25μm; the anti-wear agent is 2.2 parts by weight, and ultra-high molecular weight silicone resin DX067 or ultra-high molecular weight silicone resin DX053E is selected; the anti-slip agent is 0.9 parts by weight, and polymer polyethylene, polypropylene, and butadiene block copolymer are selected; the masterbatch is added to the shoe material according to the color of the shoe material to enhance the color of the shoe material. In this embodiment, black masterbatch is selected, and the weight portion is 0.003 parts.

[0045] The preparation method of the wear-resistant, non-slip and light-transmitting shoe material of Examples 1 to 8 comprises the following steps:

[0046] S1. Material processing: weigh the EVA plastic particles, modifier, POE elastomer, glass sand, bridging cross-linking agent, first foaming agent, second foaming agent, initiator, phosphor powder, zinc oxide, flow agent (if there is no flow agent in the step, do not add it), wear-resistant agent, anti-slip agent, masterbatch and other raw materials according to the above proportions. The raw material weighing tolerance is ±0.1 g;

[0047] S2. Internal mixer: Check the power supply and switch of the internal mixer to see if they are normal. Then add half of the EVA plastic pellets, modifier, POE elastomer, glass sand, phosphorescent powder, zinc oxide, flow agent, wear-resistant agent, anti-slip agent, masterbatch and the other half of the EVA plastic pellets in sequence, press the hammer, and start the mixer to mix. When the temperature of the internal mixer reaches 95°C, clean the dust on the edge and turn the material over. When the temperature of the internal mixer reaches 100°C, add the crosslinking agent, the first foaming agent, the second foaming agent and the initiator, press the hammer halfway, mix for 40 seconds, and then press the hammer fully. When the temperature of the internal mixer reaches 110°C±2°C, start unloading the material to the turbine and clean the machine to ensure that there is no residue.

[0048] S3. Calendering treatment: Use a roller mill to calender according to the following steps: 4mm-6mm thick twice, 1mm-2mm thin twice, 4mm-6mm thick once to start granulation;

[0049] S4. Granulation: Check whether the power temperature of the granulator reaches the set value, 75℃ for the first section, 75℃ for the second section, 75℃ for the third section, and 80℃ for the die head; pour the calendered material into the granulator and start discharging. After the material is discharged, install the die head and start granulation. Turn on the vibrating screen, fan, cutter, and main machine in sequence. Adjust the cutter to make suitable wear-resistant, non-slip and light-transmitting shoe material particles. After granulation, clean the die head.

[0050] The wear-resistant, non-slip, and light-transmitting shoe materials prepared in Examples 1 to 8 were made into finished shoe midsoles using the prior art, and compared with finished shoe midsoles of the same size made using the same prior art. The following conclusions were drawn:

[0051] The shoe midsoles manufactured by the project in Examples 1 to 8 have good appearance and are lighter in weight (about 75%-80% of the former). They are not light-transmissive. They have good light transmission and can be colored. They are not light-storing and can glow at night. They are elastic at about 45° and can reach 55° or above. They are non-slip and have passed the dry and wet anti-slip tests. They are not wear-resistant and can reach DIN563.

[0052] Item Existing shoe midsole Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Example 8 Hardness 53° 55° 56° 55° 56° 58° 57° 56° 57° Specific gravity 0.34 0.33 0.32 0.30 0.31 0.30 0.31 0.32 0.32 Tensile force 58 6 3 6 3 6 2 6 2 6 4 6 3 6 3 6 2 Extension 43 0 44 64 48 4 46448454448452450Tear16.518.018.118.017.918.318.218.218.3Rebound455353535454545453DINAbrasion364243434444434342Dry Anti-slip0.300.550.550.560.550.600.580.570.57

[0053] Through the above experiments, it is not difficult to see that, using the same process, the shoe midsoles prepared in Examples 1 to 8 are superior to the existing shoe midsoles in terms of weight, light transmittance, light storage, elasticity, anti-slip properties, and wear resistance. The products can directly contact the ground, are more comfortable, have good dry and wet anti-slip properties, are lighter in weight, have good elasticity, can reduce the burden on consumers' feet, and at the same time have light transmittance, high safety, and can meet the sense of design. Through the above experiments, it can also be seen that the shoe midsole prepared in Example 5, in particular, has better performance in all aspects than other examples.

[0054] The above description is only a preferred embodiment of the present invention. Any slight modifications, equivalent changes and modifications made to the above embodiment according to the technical solution of the present invention are within the scope of the technical solution of the present invention.

[0055] Industrial Applicability

[0056] The present invention discloses a wear-resistant, anti-skid, and light-transmitting shoe material and a preparation method. The wear-resistant, anti-skid, and light-transmitting shoe material of the present invention can meet consumer needs, is more comfortable, and the finished product can directly contact the ground, has good dry and wet anti-skid properties, is lightweight, has good elasticity, can reduce the burden on the feet, and is light-transmitting, highly safe, and can meet the needs of design. Therefore, the present invention has industrial applicability.

Claims

1. A wear-resistant, non-slip and light-transmitting shoe material, characterized by: The invention is prepared by mixing the following raw materials in parts by weight: 32 to 38 parts of EVA plastic particles, 4.5 to 6.5 parts of modifiers, 9 to 12 parts of POE elastomers, 2.5 to 4 parts of glass sand, 0.3 to 0.6 parts of bridging crosslinking agents, 0.8 to 1.3 parts of first foaming agents, 0.4 to 0.8 parts of second foaming agents, 0.3 to 0.6 parts of initiators, 0.03 to 0.1 parts of luminescent powder, and 0.4 to 0.8 parts of zinc oxide; the modifier is selected from ethylene-octene block copolymers, styrene block copolymers, ethylene vinyl acetate copolymers any one or more of materials, soft chloroethylene or flexible polyolefin; the first foaming agent is any one or more of DUST transparent foaming agent, HCFC-14LB foaming agent, HFC-152A foaming agent; the second foaming agent is any one or more of ACP foaming agent, AC foaming agent, modified carbonate foaming agent, magnesium oxysulfide composite foaming agent, ADC foaming agent; the initiator is any one or more of DCP, MCP, ACTOR-TDDS, ACCEL-BF, TMPTMA-70.

2. The wear-resistant, non-slip and light-transmitting shoe material according to claim 1, characterized in that: The invention is prepared by mixing the following raw materials in parts by weight: 33 to 36 parts of EVA plastic particles, 4.5 to 6.0 parts of modifier, 9 to 11 parts of POE elastomer, 2.5 to 3 parts of glass sand, 0.3 to 0.5 parts of bridging cross-linking agent, 0.9 to 1.2 parts of first foaming agent, 0.5 to 0.7 parts of second foaming agent, 0.3 to 0.5 parts of initiator, 0.04 to 0.08 parts of luminescent powder, and 0.5 to 0.7 parts of zinc oxide; the POE elastomer is selected from any one or more of DF610 POE elastomer, 9061 POE elastomer, 7378 POE elastomer, 8605L POE elastomer, and C5070D POE elastomer; the particle size of the glass sand is 400 μm to 800 μm; the bridging cross-linking agent is selected from PL 400, PL 500, TAIC, LS-3-80 or more; the luminescent powder is a long-lasting luminescent powder that can emit bright light at night; the zinc oxide particle size is 1.62 μm to 2.25 μm.

3. The wear-resistant, non-slip and light-transmitting shoe material according to claim 2, characterized in that: The invention also comprises a flow agent, wherein the weight portion of the flow agent is 0 to 0.3 parts, and the flow agent is selected from any one of MA-St and POKM330F or a mixture of the two.

4. The wear-resistant, non-slip and light-transmitting shoe material according to claim 3, characterized in that: The invention also comprises an anti-wear agent, wherein the weight portion of the anti-wear agent is 1.5 to 2.5 parts, and ultra-high molecular weight silicone resin DX067 or ultra-high molecular weight silicone resin DX053E is selected.

5. The wear-resistant, non-slip and light-transmitting shoe material according to claim 4, characterized in that: The invention also includes an anti-slip agent, wherein the weight portion of the anti-slip agent is 0.8 to 1.3 parts, and the anti-slip agent is selected from high molecular weight polyethylene, polypropylene, and butadiene block copolymer.

6. The wear-resistant, non-slip and light-transmitting shoe material according to claim 5, characterized in that: It also includes masterbatch, which is added to the shoe material for color enhancement according to the color of the shoe material, and the weight portion is 0.003 to 0.006 parts.

7. A method for preparing the wear-resistant, non-slip and light-transmitting shoe material according to claims 1 to 6, characterized in that: The following steps are involved: S1. Material processing: weigh the EVA plastic particles, modifier, POE elastomer, glass sand, bridging crosslinking agent, first foaming agent, second foaming agent, initiator, luminescent powder, zinc oxide, flow agent and other raw materials according to the above proportions, and the raw material weighing tolerance is ±0.1 g; S2, Internal Mixing and Mixing: Check whether the power supply and switch of the internal mixer are normal, and add half of the EVA plastic pellets, modifier, POE elastomer, glass sand, luminescent powder, zinc oxide, flow agent and the other half of the EVA plastic pellets in turn, press the hammer, and start the machine to mix; when the temperature of the internal mixer reaches 95℃, clean the dust on the edge and turn the material over; when the temperature of the internal mixer reaches 100℃, add the bridging cross-linking agent, the first foaming agent, the second foaming agent, and the initiator, press the hammer halfway, mix the material for 40 seconds, and then press the hammer fully; when the temperature of the internal mixer reaches 110℃±2℃, start pouring the material to the turbine, clean the machine, and no residue should be left; S3, calendering treatment: calendering treatment is carried out by a wheel mill according to the following steps: 4mm-6mm thickening twice, 1mm-2mm thinning twice, 4mm-6mm thickening once to start granulation; S4, granulation: check whether the power temperature of the granulator reaches the set value, 75℃ for the first section, 75℃ for the second section, 75℃ for the third section, and 80℃ for the die head; pour the calendered material into the granulator to start discharging, and after the discharge is clean, install the die head to start granulation to make wear-resistant, non-slip and translucent shoe materials.

8. The method for preparing the wear-resistant, non-slip and light-transmitting shoe material according to claim 7, characterized in that: After the granulation starts in step S4, the vibrating screen, fan, cutter, and main machine are turned on in sequence, and the cutter is adjusted to form suitable wear-resistant, non-slip, and light-transmitting shoe material particles; after the granulation is completed, the die head needs to be cleaned.

Citation Information

Patent Citations

  • Formula of soles of PU-simulated foaming sneakers through injection and manufacturing method

    CN101805475A

  • Antiskid anti-abrasion EVA shoe sole material and preparation method thereof

    CN105175878A

  • Oil-resistant antiskid EVA (ethylene-vinyl acetate) foamed material and preparation method thereof

    CN105542263A

  • Wear-resistance slip-limitation light-transmission shoe material and manufacturing method

    CN110204821A

  • A virtual private network generating method providing the virtual private network by performing signature and verification based on post quantum cryptography algorithm and a virtual private network operating system performing the same

    KR102474894B1

Cited By

  • Noctilucent sole material and preparation method thereof

    CN120424438A