Method for surface modification of high-nickel ternary positive electrode material and use thereof
The hydrophobic protective layer is formed by reacting the alkyl lithium silicate solution with the high-nickel ternary cathode material, which solves the material's cycle and thermal performance problems, improves the stability and electrochemical performance of the battery, and reduces processing costs and battery assembly humidity requirements. .
Patent Information
- Application Number
- PCT/CN2023/085570
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-03
AI Technical Summary
High-nickel ternary cathode materials have problems with poor cycle and thermal performance in lithium-ion batteries, and the increase in nickel content leads to an increase in the amount of residual alkali and an increase in the air sensitivity of the material. The existing hydrophobic modification method uses organic solvents, which are costly and need to be processed. Over time, the electrical properties of the material will decline.
The alkyl lithium silicate solution is used to react with the high-nickel ternary cathode material through spray method or solid-liquid blending method to form a hydrophobic protective layer, reduce the hygroscopicity and surface energy of the material, improve the stability and electrochemical performance of the material, and avoid Organic solvents and other alkali metals are used for introduction.
It has improved the storage stability of the material, improved battery cycle performance and discharge capacity, reduced processing costs and humidity requirements for battery assembly, avoided the loss of lithium in the aqueous solution, and enhanced the affinity of the electrolyte layer.
Smart Images

Figure CN2023085570_03102024_PF_FP_ABST
Abstract
Description
Method for surface modification of high-nickel ternary cathode materials and its application Technical Field
[0001] The present invention belongs to the technical field of lithium-ion batteries, and in particular relates to a method for surface modification of a high-nickel ternary positive electrode material and its application. Background Art
[0002] Developing new energy vehicles is a crucial measure for effectively addressing energy and environmental challenges. Batteries, as a power source, have become the primary development direction for new energy electric vehicles. Further improving battery energy and power density, extending battery life, shortening battery charging time, improving battery safety, and reducing battery costs are the key themes and trends in new energy technology development. Lithium-ion batteries, due to their superior overall performance, remain the mainstream power battery product. Developing high-voltage, high-capacity cathode materials has become the primary approach to further improving battery energy density.
[0003] Ternary layered oxide cathode materials have moderate cost, high specific capacity, and the ratio of transition metals can be adjusted within a certain range. They are widely used in the field of long-range power batteries. Among them, high-nickel ternary cathode materials have their unique advantages in energy density. However, poor cycling and thermal performance also limit their application. In addition, as the nickel content increases, the amount of residual alkali gradually increases, and the air sensitivity problem of the material itself is exacerbated. To meet this challenge, various doping / coating strategies are used to change the bulk structure or surface and interface properties of high-nickel materials. Among them, hydrophobic modification can change the inherent hydrophilic properties of the material surface, thereby reducing the hygroscopicity of the material and playing an important role in alleviating the deterioration of the material.
[0004] Alkyl silicates are a class of surface modification materials widely used in building waterproofing. They possess excellent water solubility, strong substrate adhesion, and superior water resistance and weather resistance. They are commonly used for waterproofing concrete and other building materials, enjoying a wide range of applications. Commercially available alkyl silicates include sodium methyl silicate, potassium methyl silicate, sodium ethyl silicate, and sodium phenyl silicate. These products often retain some sodium and potassium ions when used directly for waterproofing. These ions are difficult to remove when applied directly to lithium battery materials, hindering the material's electrochemical performance.
[0005] Existing methods mostly use organic silicon materials as hydrophobic modifiers to modify the surface of positive electrode materials, but the solvents used in these methods are mostly organic reagents, which are relatively expensive. Even if some methods include water as an optional solvent, there is still the problem of too long hydrolysis reaction time of organic silicon materials in aqueous solution. High-nickel ternary positive electrode materials cannot be treated in aqueous solution for a long time because the longer the time, the more serious the lithium loss in the material lattice, which will seriously weaken the electrical properties of the material.
[0006] Summary of the Invention
[0007] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a method for surface modification of a high-nickel ternary cathode material and its application.
[0008] According to one aspect of the present invention, a method for surface modification of a high-nickel ternary cathode material is proposed, comprising the following steps:
[0009] preparing an alkyl lithium silicate solution, mixing the alkyl lithium silicate solution with a high-nickel ternary positive electrode material by a spraying method or a solid-liquid blending method to react, and then drying and heat-treating the mixture to obtain a modified high-nickel ternary positive electrode material;
[0010] The spray method is to spray the alkyl lithium silicate solution onto the surface of the high nickel ternary positive electrode material while keeping it in a stirred state to cause a chemical reaction, and then the wet material obtained after spraying is subjected to the drying heat treatment;
[0011] The solid-liquid blending method is to disperse the high-nickel ternary positive electrode material into the alkyl lithium silicate solution for reaction, and perform the drying heat treatment on the solid obtained after solid-liquid separation.
[0012] When mixing is performed by spraying, high-speed mixing equipment is used to spray the alkyl lithium silicate solution onto the surface of the material while the high-nickel ternary positive electrode material is kept in high-speed motion to cause a chemical reaction; when the alkyl lithium silicate is reacted with the high-nickel ternary positive electrode material by solid-liquid blending (wet method), the alkyl lithium silicate, as an aqueous solution additive, directly reacts with the surface of the high-nickel ternary positive electrode material to achieve a hydrophobic modification effect.
[0013] In some embodiments of the present invention, the high nickel ternary cathode material is lithium nickel cobalt manganese oxide, whose chemical formula is LiNi x Co y Mn z O2, wherein x+y+z=1, and 0.8≤x<1, 0<y≤0.1, 0<z≤0.1.
[0014] In some embodiments of the present invention, the preparation method of the alkyl lithium silicate solution comprises: mixing an alkyltrialkoxysilane, an acid catalyst, and water to undergo a hydrolysis reaction to obtain an alkyl silicic acid solution; mixing the alkyl silicic acid solution with a lithium hydroxide solution for reaction; and performing solid-liquid separation to obtain the alkyl lithium silicate solution. Furthermore, the hydrolysis reaction temperature is 25-50°C, and the reaction time is 0.1-5 hours. Furthermore, the molar ratio of the alkyl silicic acid in the alkyl silicic acid solution to the lithium hydroxide in the lithium hydroxide solution is 1:(0.8-2). Furthermore, the mass concentration of the lithium hydroxide solution is 10-120 g / L. Furthermore, the mixing reaction time of the alkyl silicic acid solution and the lithium hydroxide solution is 5-30 minutes. Furthermore, the solid-liquid separation method is filtration or vacuum-assisted filtration. It should be noted that the solids obtained from the solid-liquid separation are generally insoluble alkyl silicates generated by excessive hydrolysis and polymerization. Although the amount of insoluble alkyl silicates is relatively small, they still need to be filtered out to prevent interference with the product.
[0015] In some embodiments of the present invention, the alkyl lithium silicate solution is at least one of a methyl lithium silicate solution, a vinyl lithium silicate solution, a propyl lithium silicate solution, an octyl lithium silicate solution, a phenyl lithium silicate solution or a dodecyl lithium silicate solution. In the present invention, the corresponding alkyl trialkoxysilane can be selected as needed to prepare the corresponding alkyl lithium silicate. Preferably, the alkyl lithium silicate solution is a methyl lithium silicate solution or a propyl lithium silicate solution. Further, when preparing a methyl lithium silicate solution, the selected alkyl trialkoxysilane is preferably methyltrimethoxysilane or methyltriethoxysilane. When preparing a propyl lithium silicate solution, the selected alkyl trialkoxysilane is preferably propyltrimethoxysilane.
[0016] In some embodiments of the present invention, the molar ratio of the alkyltrialkoxysilane to water is 1:(1-5); and the amount of the acid catalyst is 0.1%-2% by weight of the alkyltrialkoxysilane.
[0017] In some embodiments of the present invention, the acid catalyst is at least one of hydrochloric acid, acetic acid or phytic acid.
[0018] In some embodiments of the present invention, the mass ratio of the alkyl lithium silicate to the high nickel ternary positive electrode material in the alkyl lithium silicate solution is (0.1-3):100.
[0019] In some embodiments of the present invention, in the spraying method, the stirring speed is 600-1500 rpm.
[0020] In some embodiments of the present invention, in the spraying method, the alkyl lithium silicate solution is sprayed for 5-15 minutes.
[0021] In some embodiments of the present invention, in the spray method, the spray rate is 10-30 mL / min.
[0022] In some embodiments of the present invention, in the solid-liquid blending method, the reaction time of the high-nickel ternary positive electrode material and the alkyl lithium silicate solution is 3-30 minutes.
[0023] In some embodiments of the present invention, in the solid-liquid blending method, the reaction of the high-nickel ternary positive electrode material and the alkyl lithium silicate solution is carried out at a stirring speed of 100-300 rpm.
[0024] In some embodiments of the present invention, in the solid-liquid blending method, the high-nickel ternary positive electrode material is dispersed in the alkyl lithium silicate solution in any one of the following ways: (1) diluting the alkyl lithium silicate solution to 5-50 g / L, and then adding the high-nickel ternary positive electrode material to the diluted alkyl lithium silicate solution; (2) adding the high-nickel ternary positive electrode material to water for dispersion, and then adding the alkyl lithium silicate solution, and the concentration of alkyl lithium silicate in the resulting mixture is 5-50 g / L.
[0025] In some embodiments of the present invention, the temperature of the drying heat treatment is 110-150° C., and the time is 8-24 hours.
[0026] In some embodiments of the present invention, the drying and heat treatment further includes a screening operation, and the mesh size of the screening sieve is 100-400 meshes.
[0027] The present invention also provides application of the method in preparing lithium ion batteries.
[0028] According to a preferred embodiment of the present invention, there are at least the following beneficial effects:
[0029] 1. The present invention applies alkyl lithium silicate to the modification process of high nickel ternary cathode materials. The hydrophilic oxygen-containing groups (hydroxyl-OH, oxygen-containing anions Si-O-Li + ) can react with the hydrophilic oxygen-containing functional groups (-OH, -O-) of the high-nickel ternary cathode material, exposing the hydrophobic alkyl groups and forming a hydrophobic protective coating. This changes the inherent hydrophilic properties of the oxide substrate, reduces the surface energy and water absorption capacity of the high-nickel ternary cathode material, alleviates the deterioration of the material in the air, increases the storage stability of the material in a high-humidity environment, improves the processing performance of the material, relaxes the humidity requirements, and reduces the cost of material processing. In addition, the hydrophobic groups exposed by the modified cathode material have an enhanced affinity with the hydrophobic electrolyte used in battery assembly, and the electrolyte infiltration characteristics are improved, thereby affecting the component structure of the cathode electrolyte layer during battery operation and improving the battery discharge capacity and cycle performance.
[0030] 2. The present invention first hydrolyzes the alkyl trialkoxy group and then uses lithium hydroxide for neutralization reaction to obtain alkyl lithium silicate with good water solubility. Compared with common organosilicon hydrophobic modifiers, no other organic solvents or dispersants are required. The prepared alkyl lithium silicate has good water solubility and strong reactivity, and can quickly perform hydrophobic modification on high-nickel ternary positive electrode materials, which can greatly shorten the modification process time. In addition, since the alkyl lithium silicate itself contains Li + It can provide a lithium source and is strongly alkaline. It can reduce the loss of internal lattice lithium caused by the aqueous solution treatment of high-nickel ternary positive electrode materials and replenish the lithium source, which helps to maintain the electrical properties of the material itself and avoids the introduction of other alkali metals.
[0031] 3. The alkyl lithium silicate provided by the present invention has good water solubility and is a water-based silane waterproofing modifier. Compared with traditional organosilane coupling agents, the alkyl lithium silicate solution provided by the present invention can avoid the use of organic reagents in waterproofing modification processes, has strong reactivity, saves time and production costs, improves the safety of the modification process, and has a wider range of applications.
[0032] 4. Preferably, the method for preparing alkyl lithium silicate provided by the present invention is simple and efficient, does not require ion exchange, has strong operability, mild reaction conditions, and is relatively environmentally friendly; the prepared alkyl lithium silicate has good water solubility, strong reactivity, and a wider range of applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The present invention will be further described below with reference to the accompanying drawings and embodiments, in which:
[0034] FIG1 is a SEM image of the modified high-nickel ternary cathode material of Example 1 of the present invention;
[0035] FIG2 is a comparison of the cycle performance of Examples 1, 2, and 5 of the present invention and Comparative Example 1. DETAILED DESCRIPTION
[0036] The following will clearly and completely describe the concept and technical effects of the present invention in conjunction with the embodiments to fully understand the purpose, features and effects of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0037] Example 1
[0038] A method for surface modification of a high-nickel ternary cathode material, the specific process is as follows:
[0039] 1) 136 g of methyltrimethoxysilane was dissolved in a mixture of 54 g of deionized water and 0.3 g of concentrated hydrochloric acid, and the mixture was reacted at 30° C. for 1 h. 200 mL of a 120 g / L lithium hydroxide solution was then added with stirring at 100 rpm. The mixture was reacted for 10 min and then vacuum filtered to obtain a lithium methylsilicate solution.
[0040] 2) Take 2kg of high nickel ternary positive electrode material LiNi 0.92 Co 0.06 Mn 0.02 O2 was added to the Kawada mixer, and 52 mL of the above-mentioned lithium methyl silicate solution was sprayed onto the surface of the high-nickel ternary positive electrode material at a speed of 800 rpm. The spray rate was 10 mL / min and the spray time was 8 min. After spraying, stirring was continued for 5 min, and then dried at 120 ° C in a blast drying oven for 12 h. Finally, it was sieved with a 400-mesh sieve to obtain the modified high-nickel ternary positive electrode material.
[0041] FIG1 is an SEM image of the modified high-nickel ternary positive electrode material of this embodiment. In the image, a layer of film-like material can be found evenly covering the surface of the particles.
[0042] Example 2
[0043] A method for surface modification of a high-nickel ternary cathode material, the specific process is as follows:
[0044] 1) 136 g of methyltrimethoxysilane was dissolved in 54 g of deionized water and 0.6 g of a 50 wt% phytic acid mixture, and the mixture was reacted at 30° C. for 1 h. 200 mL of a 120 g / L lithium hydroxide solution was then added with stirring at 100 rpm. The mixture was reacted for 10 min and then vacuum filtered to obtain a lithium methylsilicate solution.
[0045] 2) Add 4.8L of deionized water to the water-washed reactor, add 200mL of the above-mentioned lithium methyl silicate solution, start stirring at a speed of 200rpm, and then quickly add 10kg of high-nickel ternary positive electrode material LiNi 0.92 Co 0.06 Mn 0.02 O2, continue stirring for 3 minutes, then centrifuge to remove the solvent, the collected solid is dried in an oven at 120°C for 12 hours, and finally sieved through a 400-mesh sieve to obtain the modified high-nickel ternary positive electrode material.
[0046] Example 3
[0047] A method for surface modification of a high-nickel ternary cathode material, the specific process is as follows:
[0048] 1) 164 g of propyltrimethoxysilane was dissolved in a mixture of 20 g of deionized water and 0.3 g of concentrated hydrochloric acid, and the mixture was reacted at 40° C. for 2 h. 200 mL of a 120 g / L lithium hydroxide solution was then added with stirring at 100 rpm. The mixture was reacted for 10 min and then vacuum filtered to obtain a propyl lithium silicate solution.
[0049] 2) Take 3kg of high nickel ternary positive electrode material LiNi 0.92 Co 0.06 Mn 0.02 O2 was added to the Kawada mixer, and 80 mL of the above-mentioned lithium propyl silicate solution was sprayed onto the surface of the high-nickel ternary positive electrode material at a speed of 800 rpm. The spray rate was 20 mL / min and the spray time was 10 min. After spraying, stirring was continued for 3 min, and then the mixture was dried in a blast drying oven at 120 ° C for 12 h. Finally, the modified high-nickel ternary positive electrode material was obtained by sieving with a 400-mesh sieve.
[0050] Example 4
[0051] A method for surface modification of a high-nickel ternary cathode material, the specific process is as follows:
[0052] 1) 136 g of methyltrimethoxysilane was dissolved in a mixture of 54 g of deionized water and 0.3 g of concentrated hydrochloric acid, and the mixture was reacted at 35° C. for 0.5 h. Then, 400 mL of a 120 g / L lithium hydroxide solution was added under stirring at 150 rpm. The mixture was reacted for 10 min and then vacuum filtered to obtain a lithium methylsilicate solution.
[0053] 2) Take 2kg of high nickel ternary positive electrode material LiNi 0.92 Co 0.06 Mn 0.02 O2 was added to the Kawada mixer, and 53 mL of the above-mentioned lithium methyl silicate solution was sprayed onto the surface of the high-nickel ternary positive electrode material at a speed of 800 rpm. The spray rate was 10 mL / min and the spray time was 8 min. After spraying, stirring was continued for 5 min, and then the mixture was dried in a blast drying oven at 120 ° C for 12 h. Finally, the modified high-nickel ternary positive electrode material was obtained by sieving with a 400-mesh sieve.
[0054] Example 5
[0055] A method for surface modification of a high-nickel ternary cathode material, the specific process is as follows:
[0056] 1) 136 g of methyltrimethoxysilane was dissolved in a mixture of 54 g of deionized water and 0.3 g of concentrated hydrochloric acid, and the mixture was reacted at 30° C. for 1 h. 200 mL of a 120 g / L lithium hydroxide solution was then added with stirring at 100 rpm. The mixture was reacted for 10 min and then vacuum filtered to obtain a lithium methylsilicate solution.
[0057] 2) Take 500g of high nickel ternary positive electrode material LiNi 0.92 Co 0.06 Mn 0.02 O2 was dispersed in 500 mL of deionized water, and the temperature of the deionized water was maintained at 5°C. 40 mL of the above-mentioned lithium methyl silicate solution was slowly added dropwise at a speed of 300 rpm, and the reaction was continued by stirring for 5 minutes. The solid was obtained by vacuum filtration and dried in an oven at 120°C for 12 hours. Finally, it was sieved with a 400-mesh sieve to obtain the modified high-nickel ternary positive electrode material.
[0058] Example 6
[0059] A method for surface modification of a high-nickel ternary cathode material, the specific process is as follows:
[0060] 1) 178 g of methyltriethoxysilane was dispersed in a mixture of 54 g of deionized water and 0.5 g of concentrated hydrochloric acid, stirred at high speed, and reacted for 3 h at 100 rpm and 50° C.; then, 200 mL of a 120 g / L lithium hydroxide solution was added, reacted for 30 min, and vacuum filtered to obtain a lithium methylsilicate solution.
[0061] 2) Take 2kg of high nickel ternary positive electrode material LiNi 0.92 Co 0.06 Mn 0.02 O2 was added to the Kawada mixer, and 60 mL of the above-mentioned lithium methyl silicate solution was sprayed onto the surface of the high-nickel ternary positive electrode material at a speed of 800 rpm. The spray rate was 10 mL / min and the spray time was 8 min. After spraying, stirring was continued for 5 min, and then the mixture was dried in a blast drying oven at 120 ° C for 12 h. Finally, the modified high-nickel ternary positive electrode material was obtained by sieving with a 400-mesh sieve.
[0062] Comparative Example 1
[0063] A method for surface treatment of a high-nickel ternary positive electrode material is different from Example 2 in that: Comparative Example 1 does not use a lithium methyl silicate solution for modification, and the specific process is as follows:
[0064] Add 5L of deionized water to the water-washing reactor, start stirring, and then quickly add 10kg of high-nickel ternary positive electrode material LiNi 0.92 Co 0.06 Mn 0.02O2, continue stirring for 3 minutes, then centrifuge to remove the deionized water solvent, dry in an oven at 120°C for 12 hours, and finally sieve through a 400-mesh sieve to obtain a wet-treated but unmodified high-nickel ternary positive electrode material.
[0065] Test example
[0066] Battery Assembly and Testing: Lithium-ion button cells were assembled in an argon atmosphere glove box (H2O <0.1ppm, O2 <0.1ppm). The high-nickel ternary positive electrode material, conductive agent, and binder prepared in the examples and comparative examples were mixed uniformly at a ratio of 90:5:5. A nitrogen-methylpyrrolidone solvent was added and stirred to form a slurry, which was then coated. The slurry was then baked at 110°C for 2 hours before punching. The slurry was then dried again in a vacuum oven at 105°C for 4 hours. The button cells were assembled. The electrolyte was LiPF6 dissolved in a mixed solvent of ethylene carbonate and diethyl carbonate. The separator was glass fiber, and the negative electrode was a lithium metal sheet. After assembly, the battery was allowed to stand for 3 hours before the first cycle test. The test conditions were 25°C, with the charge and discharge capacity and initial efficiency at 0.1C tested (1C = 210mAh / g). The cycling performance test used a fully charged button cell, replacing the lithium metal negative electrode with a carbon material. After one cycle at 0.1C, the battery cycling stability was tested again at 1C.
[0067] Table 1 shows the residual lithium compounds and first-cycle electrical properties of Comparative Example 1 and Examples 1, 2, 3, 4, 5, and 6, wherein the residual lithium compounds are measured by acid-base titration, and the first-cycle electrical performance data are obtained by testing with a blue battery test system.
[0068] Table 1 Comparison of residual lithium compound content and first cycle electrical properties
[0069] As can be seen from Table 1, the first cycle charge and discharge capacity of the battery is improved in the embodiment. When the high nickel ternary positive electrode material is treated with an aqueous solution, in addition to washing away the residual lithium compounds, the lithium in the lattice will also be washed out, which is prone to "overwashing" and reduces the charge and discharge capacity of the material. The alkyl lithium silicate prepared by the present invention has strong alkalinity. In the process of aqueous solution modification of the material, in addition to forming a hydrophobic layer on the surface of the material, it can also effectively inhibit the loss of lattice lithium inside the material particles. Although this method will inhibit the dissolution loss of residual lithium compounds on the surface, making the residual lithium compound content of the material relatively high, due to the presence of the surface hydrophobic layer, even if the residual lithium is high, it will not reduce the performance of the material, and the hydrophobic layer can enhance its affinity with the electrolyte, improve the electrolyte infiltration characteristics, and produce a certain gain effect on the cyclability of the material.
[0070] Figure 2 is a comparison of the cycle performance of Examples 1, 2, and 5 with the comparative example. It can be found from Figure 2 that, relative to Comparative Example 1, Examples 1, 2, and 5 improve the discharge capacity and cycle performance of the high-nickel ternary positive electrode material. After 170 cycles under 1C conditions, the capacity retention rate of Comparative Example 1 is 77.96%, and the capacity retention rates of Examples 1, 2, and 5 are 84.06%, 81.34%, and 80.72%, respectively.
[0071] While the embodiments of the present invention have been described in detail above with reference to the accompanying drawings, the present invention is not limited to the embodiments described above. Various modifications may be made within the scope of knowledge possessed by a person skilled in the art without departing from the spirit of the present invention. Furthermore, the embodiments of the present invention and the features thereof may be combined with one another unless there is a conflict.
Claims
1. A method for surface modification of a high-nickel ternary cathode material, characterized in that: The following steps are involved: preparing an alkyl lithium silicate solution, mixing the alkyl lithium silicate solution with a high-nickel ternary positive electrode material by a spraying method or a solid-liquid blending method to react, and then drying and heat treating to obtain a modified high-nickel ternary positive electrode material; The spray method is to spray the alkyl lithium silicate solution onto the surface of the high nickel ternary positive electrode material while keeping it in a stirred state to cause a chemical reaction, and the wet material obtained after spraying is subjected to the drying heat treatment; The solid-liquid blending method is to disperse the high-nickel ternary positive electrode material into the alkyl lithium silicate solution for reaction, and the solid obtained after solid-liquid separation is subjected to the drying heat treatment.
2. The method according to claim 1, characterized in that The preparation method of the alkyl lithium silicate solution comprises: mixing alkyltrialkoxysilane, an acid catalyst and water for hydrolysis reaction to obtain an alkyl silicic acid solution, mixing the alkyl silicic acid solution with a lithium hydroxide solution for reaction, and performing solid-liquid separation to obtain the alkyl lithium silicate solution.
3. The method according to claim 1 or 2, characterized in that: The alkyl lithium silicate solution is at least one of a methyl lithium silicate solution, a vinyl lithium silicate solution, a propyl lithium silicate solution, an octyl lithium silicate solution, a phenyl lithium silicate solution or a dodecyl lithium silicate solution.
4. The method according to claim 2, characterized in that: The molar ratio of the alkyltrialkoxysilane to water is 1:(1-5); the amount of the acid catalyst is 0.01%-2% of the weight of the alkyltrialkoxysilane.
5. The method according to claim 2, characterized in that: The acid catalyst is at least one of hydrochloric acid, acetic acid or phytic acid.
6. The method according to claim 1, characterized in that The mass ratio of the alkyl lithium silicate to the high-nickel ternary positive electrode material in the alkyl lithium silicate solution is (0.1-3):
100.
7. The method according to claim 1, characterized in that In the spraying method, the alkyl lithium silicate solution is sprayed for 5-15 minutes.
8. The method according to claim 1, characterized in that In the solid-liquid blending method, the reaction time of the high-nickel ternary positive electrode material and the alkyl lithium silicate solution is 3-30 minutes.
9. The method according to claim 1, characterized in that: The drying heat treatment is carried out at a temperature of 110-150° C. and for a time of 8-24 hours.
10. Use of the method according to any one of claims 1 to 9 in preparing a lithium ion battery.
Citation Information
Patent Citations
Method for preparing propyl silicate aqueous solution by utilizing propyl trichlorosilane
CN102633826A
Ternary positive electrode material and preparation method and application thereof
CN112670482A
Layered lithium nickel manganese oxide positive electrode material as well as preparation method and application thereof
CN114824267A
Battery diaphragm coating slurry containing sodium methyl silicate, battery diaphragm, battery and preparation method of battery diaphragm
CN115051108A
Organic siliconate additive for alkaline zinc electrochemical cells
EP0140312A1
Cited By
Treatment method and application of lithium-rich layered positive electrode material
CN119852365A