Electrochemical device and electronic device
By using specific polymer materials and encapsulation films with alternately stacked organic and inorganic layer structures in electrochemical devices, the problems of reduced energy density and poor barrier function caused by the space occupied by the sealing edge are solved, achieving higher energy density and Cycling stability.
Patent Information
- Application Number
- PCT/CN2023/085657
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-03
AI Technical Summary
The existing packaging form of secondary batteries has the problems of low space utilization and large energy density loss, especially the reduction of energy density due to the space occupied by the sealing edge, and the problem of poor barrier function.
An encapsulation film structure of an electrochemical device is adopted, including a first layer, a second layer and a third layer. The second layer is composed of polymer materials and meets specific infrared characteristic peak positions and bonding strength conditions. The third layer includes Alternately stacked organic and inorganic layers, the second layer is used to improve the flattening and defect repair of the surface of the first layer, and improve the barrier properties of the third layer.
It increases the energy density and space utilization of the electrochemical device, improves the barrier properties of the packaging area, extends the cycle performance, and maintains effective packaging in battery packages with various shapes.
Smart Images

Figure CN2023085657_03102024_PF_FP_ABST
Abstract
Description
Electrochemical device and electronic device Technical Field
[0001] The present application relates to the field of electrochemistry, and in particular to an electrochemical device and an electronic device. Background Art
[0002] Secondary batteries have a wide range of applications in the field of consumer electronics. With the rapid development of mobile electronic devices in recent years, new product forms have emerged, such as wireless Bluetooth headsets, smart watches, small electronic game consoles, and virtual and augmented reality terminal devices. The secondary battery terminal market shows a demand for miniaturization, special shapes, and high energy density. At present, the packaging forms of secondary batteries include soft packs and metal shell packaging, but these two traditional mainstream packaging processes have relatively low space utilization and large battery energy density loss. Soft-pack secondary batteries generally have top seals and side seals. The seal edges do not have active materials but occupy a certain volume, thereby reducing the energy density of the soft-pack battery. The smaller the battery capacity, the more the energy density is reduced.
[0003] Summary of the Invention
[0004] The embodiments of the present application provide an electrochemical device and an electronic device, which can solve the problem that the sealing edge of the packaging bag of the electrochemical device occupies space and thus reduces the energy density of the electrochemical device.
[0005] In a first aspect, the present application provides an electrochemical device comprising an electrode assembly and a packaging film for packaging the electrode assembly, wherein the packaging film comprises: a first layer, a second layer, and a third layer; the second layer is connected between the first layer and the third layer, and the second layer comprises a polymer material. The infrared characteristic peak position of the polymer material of the second layer satisfies: at 822±5cm -1 There is a characteristic peak of benzene ring substitution; at 1400cm -1 ~1650cm -1 There is benzene skeleton vibration.
[0006] In some exemplary embodiments, the infrared characteristic peak position of the polymer material of the second layer further satisfies: at 687±5cm -1 There is a characteristic vibration absorption peak of C-Cl bond; at 1210cm -1 ~1010cm -1 There is a benzene ring CH in-plane bending vibration peak; at 1400cm -1 ~1650cm -1 There is benzene skeleton vibration at 1449±5cm -1 There is a CH characteristic vibration absorption peak of CH2, with 1 607±5cm -1 and 1 556±5cm -1It is the vibration peak of the benzene ring skeleton caused by the addition of substitution to the benzene ring, 873±5cm -1 The out-of-plane bending vibration peak of the CH bond on the benzene ring is increased after the benzene ring is substituted; at 2859±5cm -1 and 2924±5cm -1 There are symmetric and antisymmetric stretching vibration peaks of methylene CH bonds; at 3018±5cm -1 There are stretching vibration peaks of the C-H bond on the benzene ring.
[0007] In some exemplary embodiments, the substitution position in the polymer material contains a halogen, and the halogen contains at least one of chlorine or fluorine; based on the mass of the polymer material, the mass percentage of the halogen in the polymer material is w1, and w1 satisfies: 5wt%≤w1≤50wt%.
[0008] In some exemplary embodiments, the polymer material includes one or more of polyparaxylene, polymonochloroparaxylene, and polydichloroparaxylene.
[0009] In some exemplary embodiments, the second layer satisfies at least one of the following conditions:
[0010] (1) The melting point of the second layer is T1, and T1 satisfies 150°C ≤ T1 ≤ 400°C;
[0011] (2) The thickness of the second layer is H1, and H1 satisfies 0.5 μm ≤ H1 ≤ 10 μm;
[0012] (3) The polymer material comprises a repeating unit as shown in formula a;
[0013] Among them, R 1 、R 2 、R 3 、R 4 、R 5 、R 6 are each independently selected from one of H and halogen, and R 1 ~R 6 At least one of them is selected from any one of the halogens.
[0014] In some exemplary embodiments, the packaging film satisfies at least one of the following conditions:
[0015] Ⅰ. The bonding strength between the second layer and the first layer is N1, where N1 satisfies 3N / 15mm≤N1≤15N / 15mm;
[0016] Ⅱ. The bonding strength between the second layer and the third layer is N2, N2 satisfies 3N / 15mm≤N2≤15N / 15mm;
[0017] Ⅲ. Under the conditions of temperature of 38 ℃ and humidity of 90%, the water vapor permeability of the packaging film WVTR ≤ 10 -3 g / (m 2 *day);
[0018] IV. The stretching rate of the encapsulation film is A1, A1 satisfies 1% ≤ A1 ≤ 20%;
[0019] V. The thickness of the packaging film is H2, and H2 satisfies 20 μm ≤ H2 ≤ 300 μm.
[0020] In some exemplary embodiments, the third layer satisfies at least one of the following:
[0021] (1) The third layer includes an inorganic layer, and the inorganic layer includes at least one of aluminum oxide, magnesium oxide, zinc oxide, silicon oxide, titanium oxide, hafnium dioxide, zirconium oxide, iron oxide, copper oxide, silver oxide, nickel oxide, manganese oxide, tin oxide, zirconium titanium oxide, vanadium oxide, silicon nitride, silicon oxynitride, boron nitride, titanium nitride, aluminum nitride, graphene, graphyne, and flake graphite;
[0022] (2) The third layer includes an organic layer, and the organic layer includes at least one of butyl rubber, silica gel, ethylene-vinyl alcohol copolymer, polyparaxylene, polyvinyl chloride, polystyrene, epoxy resin, phenolic resin, polyimide resin, acrylic resin, silicone resin, polyolefin resin, and polyethylene terephthalate.
[0023] In some exemplary embodiments, the third layer includes an inorganic layer and an organic layer, and the inorganic layer and the organic layer are alternately stacked.
[0024] In some exemplary embodiments, the first layer includes at least one of polyvinyl chloride, polystyrene, phenolic resin, epoxy resin, melamine resin, polyimide resin, polyester resin, acrylic resin, silicone resin, cross-linked polyolefin resin, polyoxymethylene, polycarbonate, polyphenylene ether, or polysulfone.
[0025] In some exemplary embodiments, the packaging film also includes a fourth layer, which is arranged on the surface of the third layer; the fourth layer includes a resin material and a filler, the resin material includes at least one of phenolic resin, epoxy resin, amino resin, acrylic resin, silicone resin, cross-linked polyolefin resin, polyolefin, and polyester resin, and the filler includes at least one of glass fiber, carbon fiber, aramid fiber, polyethylene fiber, aluminum oxide, calcium oxide, and silicon-based particles.
[0026] In some exemplary embodiments, the packaging film includes a top wall, side walls and a bottom wall, the electrode assembly includes a tab, and the tab extends from the top wall to the packaging film; the first layer, the second layer and the third layer are each in a closed form.
[0027] In a second aspect, the present application provides an electronic device comprising the electrochemical device as described above.
[0028] The electrochemical device and electronic device according to the embodiments of the present application have at least the following beneficial effects:
[0029] The present application eliminates the packaging edge of the electrochemical device packaging bag, improves the volume utilization of the electrochemical device, thereby increasing the energy density, and improves the problem of poor barrier performance in the packaging area of the electrochemical device, thereby improving the cycle performance. A second layer is set on the surface of the first layer to reduce the surface roughness and defects of the first layer, such as pinholes, etc., to improve the film density of the third layer and improve the water barrier performance. By setting the second layer, the surface defects and pinholes of the first layer are improved, and the barrier performance of the second layer itself can synergistically improve the barrier performance of the third layer. By setting the third layer to include alternating organic layers and inorganic layers, the organic layer plays a role in dispersing defect locations and absorbing external stress, and while improving the barrier performance, it improves the overall mechanical properties of the packaging material. The present application solves the problem of energy density loss of electrochemical devices due to the large size of the sealing edge, and the problem of reduced performance of the electrochemical device due to poor barrier function, and the flexible packaging method adopted is not affected by the shape of the electrochemical device, and can achieve effective packaging. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can also be obtained based on these drawings.
[0031] FIG1 is an X-ray CT image of an aluminum-plastic film encapsulated electrode assembly;
[0032] FIG2 is an X-ray CT image of the electrode assembly encapsulated in the metal shell 1;
[0033] FIG3 is an X-ray CT image of an electrochemical device according to an embodiment of the present application;
[0034] FIG4 is a schematic diagram of the three-dimensional structure of an electrochemical device according to an embodiment of the present application;
[0035] FIG5 is a schematic cross-sectional view of an electrochemical device according to an embodiment of the present application;
[0036] FIG6 is a schematic cross-sectional view of a packaging film according to an embodiment of the present application;
[0037] FIG7 is a cross-sectional schematic diagram of an embodiment of the present application in which the third layer includes multiple inorganic layers and multiple inorganic layers.
[0038] Reference numerals:
[0039] 100, encapsulation film; 110, first layer; 120, second layer; 130, third layer; 131, inorganic layer; 132, organic layer; 140, fourth layer;
[0040] 200. Electrochemical device. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical solutions and advantages of this application more clearly understood, the present application is further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain this application and are not intended to limit this application.
[0042] The inventors found that although the side seal folding process can be used in the related art to reduce the loss of energy density, the top seal has the risk of leakage due to the presence of a hot-melt layer connecting the tab and the packaging bag. The middle of the cross-section of the packaging area is a polymer area, which is a weak barrier area. Water and oxygen can easily enter the interior of the electrochemical device through this part, thereby deteriorating the electrical performance. In addition, although the energy density loss can be reduced by the folding process, the side seals and top seals still occupy a certain volume, and this part does not contribute to energy, so the energy density will be lost. Metal shell batteries generally have sealing flanges, which occupy a certain volume, or in order to avoid short circuits between the electrode assembly and the shell, plastic gaskets or tape need to be added for insulation. This part also does not contribute to the storage of energy but occupies the volume of the electrode assembly, thereby reducing the energy density of the secondary battery. In addition, the electrochemical devices that can be encapsulated by these two packaging methods have a single shape and do not meet the packaging requirements for special-shaped batteries. A new packaging method is urgently needed to solve the above problems. As shown in Figure 1, an X-ray CT image of an electrode assembly 400 encapsulated with a conventional aluminum-plastic film 101 is shown. Within the CT cross-sectional area that does not include the tabs or posts, the outer packaging film of the electrode assembly 400 is discontinuous, with obvious signs of melted packaging. As shown in Figure 2, an X-ray CT image of an electrode assembly 400 encapsulated with a conventional metal shell 102 is shown. Within the CT cross-sectional area that does not include the tabs or posts, the outer packaging of the electrode assembly 400 is discontinuous, with obvious signs of melted welding. Furthermore, the battery is encapsulated using packaging materials. To ensure the packaging's water-resistant properties, an aluminum metal layer is provided within the packaging material to act as a moisture barrier. The aluminum layer is bonded to the first layer using either dry gluing or thermal, high-temperature, and high-pressure methods.
[0043] Based on the problem of ED loss caused by the sealing edge size, the present application proposes an electrochemical device 200. As shown in Figure 3, it is an X-ray CT image of the electrochemical device 200 of an embodiment of the present application. Within the range of the CT cross-sectional image that does not include the tabs or poles, the outer packaging film of the electrode assembly is continuous, with no obvious welding and packaging marks, showing a continuous and closed feature.
[0044] Specifically, as shown in FIG4 and FIG5 , the electrochemical device 200 includes an electrode assembly 400 and a packaging film 100 for packaging the electrode assembly 400 . As shown in FIG6 , the packaging film 100 includes a first layer 110 , a second layer 120 and a third layer 130 .
[0045] The second layer 120 is connected between the first layer 110 and the third layer 130, and the first layer 110, the second layer 120 and the third layer 130 are each in a closed state. The second layer 120 includes a polymer material. The infrared characteristic peak position of the polymer material of the second layer 120 meets the following requirements: -1 There is a characteristic peak of benzene ring substitution at 1400 cm -1 ~1650cm -1 There are benzene skeleton vibrations, for example, at 1609 ± 5 cm -1 、1557±5cm -1 、1494±5cm -1 The benzene ring carbon-carbon characteristic peak exists, so that the second layer 120 can form a dense and flat structure to improve the roughness of the first layer 110 and compensate for the surface defects of the first layer 110 .
[0046] Among them, the first layer 110, the second layer 120 and the third layer 130 of the present application are each in a closed form, and there is no structure such as edge sealing that does not contribute to energy storage, which can greatly improve the space utilization of the electrochemical device 200, thereby improving its volume energy density. The first layer 110 is in direct contact with the electrode assembly 400, and a self-closing structure is achieved by one or more of coating or hot melting methods, which is used to seal the electrode assembly 400. The electrode assembly 400 is in direct contact with the electrolyte. The first layer 110 has electrolyte resistance and will not swell. The third layer 130 includes organic materials and inorganic materials and is prepared by vapor deposition or coating. The purpose is to effectively isolate water vapor and oxygen molecules in the air from entering the electrochemical device 200 and to isolate solvent molecules in the electrolyte from escaping the electrochemical device 200. The second layer 120 is arranged between the first layer 110 and the third layer 130. The second layer 120 is used to perform flattening and pinhole-free treatment on the surface of the first layer 110.
[0047] The manufacturing process of the packaging film 100 of the electrochemical device 200 of the present application is significantly different from the packaging method with a sealed edge, and the packaging film 100 is integrally formed into a three-dimensional packaging structure. Among them, since the packaging film 100 of the present application is difficult to composite the aluminum layer through a dry process or heat sealing process, it is necessary to prepare a metal or non-metal third layer 130 by coating or deposition. The coating method has the problems of poor uniformity and insufficient density of the third layer 130, so the barrier effect is limited. The third layer 130 prepared by the deposition method has good density and uniformity, and a good barrier effect, but the flatness and cleanliness of the surface of the first layer 110, as well as impurities during the deposition process, will have a crucial impact on the deposition quality of the third layer 130.
[0048] In addition, because the third layer 130 is relatively thin and has a certain degree of rigidity, it is prone to cracking under external forces, resulting in barrier failure. Therefore, to improve the uniformity, density, and pinhole-free properties of the third layer 130, and to maintain high barrier performance under certain external stress stimuli, the present application provides a second layer 120 between the third layer 130 and the first layer 110. The second layer 120 can improve the surface defects and flatness of the first layer 110, facilitating the subsequent preparation of the third layer 130. Secondly, the second layer 120 has a certain degree of tensile resistance, which can alleviate damage to the third layer 130 under stress, thereby ensuring barrier reliability.
[0049] The packaging film 100 further includes a fourth layer 140, which is disposed on a surface of the third layer 130 away from the second layer 120. The fourth layer 140 is formed by deposition or coating, and is designed to provide high mechanical properties. This not only protects the electrode assembly 400 but also provides extremely high mechanical strength to suppress expansion of the electrochemical device 200, thereby improving the electrochemical device's 200 expansion resistance.
[0050] The polymer material of the second layer 120 contains halogen, and the halogen includes at least one of chlorine or fluorine. Based on the mass of the polymer material, the mass percentage of the halogen in the polymer material is w1, and w1 satisfies: 0wt%≤w1≤50wt%. For example, w1 can be 0wt%, 5wt%, 20wt%, 30wt%, 40wt% or 50wt%, etc. When the mass percentage of the halogen in the polymer material w1 satisfies 5wt%≤w1≤50wt%, the second layer 120 can effectively improve the surface defects and flatness of the first layer 110, and the second layer 120 can have good tensile resistance to alleviate damage to the third layer 130. When w1>50wt%, the mechanical properties of the polymer material are poor.
[0051] In some exemplary embodiments, the infrared characteristic peak position of the polymer material of the second layer further satisfies: at 687±5cm -1There is a characteristic vibration absorption peak of C-Cl bond; at 1210cm -1 ~1010cm -1 There is a benzene ring CH in-plane bending vibration peak; at 1400cm -1 ~1650cm -1 There is benzene skeleton vibration at 1449±5cm -1 There is a CH characteristic vibration absorption peak of CH2, with 1 607±5cm -1 and 1 556±5cm -1 It is the vibration peak of the benzene ring skeleton caused by the addition of substitution to the benzene ring, 873±5cm -1 The out-of-plane bending vibration peak of the CH bond on the benzene ring is increased after the benzene ring is substituted; at 2859±5cm -1 and 2924±5cm -1 There are symmetric and antisymmetric stretching vibration peaks of methylene CH bonds; at 3018±5cm -1 There are stretching vibration peaks of the C-H bond on the benzene ring.
[0052] In some exemplary embodiments, the polymer material includes one or more of polyparaxylene, polymonochloroparaxylene, and polydichloroparaxylene.
[0053] In some exemplary embodiments, the second layer 120 satisfies condition (1): the melting point of the second layer 120 is T1, and T1 satisfies 150 ≤ T1 ≤ 400°C. For example, T1 may be 150°C, 200°C, 280°C, 350°C, or 400°C. Within a certain range, the higher the melting point of the second layer 120, the more helpful it is to improve the temperature resistance of the packaging film 100, thereby enhancing thermal safety.
[0054] In some exemplary embodiments, the second layer 120 satisfies condition (2): the thickness of the second layer 120 is H1, and H1 satisfies 0.5 μm ≤ H1 ≤ 10 μm. For example, H1 can be 0.5 μm, 3 μm, 6 μm, 8 μm, or 10 μm. Within this thickness range, the second layer 120 can have good barrier properties. When the thickness H1 of the second layer 120 is less than 0.5 μm, the thickness of the second layer 120 is too thin, and the degree of improvement in the gap of the first layer 110 is limited. When the thickness H1 of the second layer 120 is greater than 10 μm, the second layer 120 is too thick, and the internal stress is too large, which will deteriorate the coating process of the third layer and thus deteriorate the barrier properties.
[0055] In some exemplary embodiments, the second layer 120 satisfies condition (3): the polymer material includes a repeating unit as shown in formula a;
[0056] Among them, R 1 、R 2、R 3 、R 4 、R 5 、R 6 are each independently selected from one of H and halogen, and R 1 ~R 6 At least one of them is selected from any one of the halogens.
[0057] In some exemplary embodiments, the packaging film 100 satisfies Condition I: The bonding strength between the second layer 120 and the first layer 110 is N1, where N1 satisfies 3N / 15mm≤N1≤15N / 15mm. For example, N1 can be 1N / 15mm, 3N / 15mm, 5N / 15mm, 7N / 15mm, or 10N / 15mm. When N1 satisfies 3N / 15mm≤N1≤15N / 15mm, the bonding strength between the second layer 120 and the first layer 110 is appropriate and does not easily peel off. When N1 is less than 3N / 15mm, the interfacial bonding strength between the second layer 120 and the first layer 110 is low, and the second layer 120 and the first layer 110 are easily peeled off, failing to provide a water vapor barrier, deteriorating the water barrier performance, and thus deteriorating the performance of the electrochemical device 200.
[0058] In some exemplary embodiments, the packaging film 100 meets condition II: the bonding strength between the second layer 120 and the third layer 130 is N2, where N2 satisfies 3N / 15mm≤N2≤15N / 15mm. For example, N2 can be 1N / 15mm, 2N / 15mm, 5N / 15mm, 8N / 15mm, or 10N / 15mm. When N2 satisfies 3N / 15mm≤N2≤15N / 15mm, the bonding strength between the second layer 120 and the third layer 130 is suitable, preventing easy peeling, and thus enabling the packaging film 100 to have good moisture barrier properties.
[0059] In some exemplary embodiments, the packaging film 100 satisfies condition III: under the conditions of a temperature of 38° C. and a humidity of 90%, the water vapor permeability WVTR of the packaging film 100 is ≤10 -3 g / (m 2 *day), thus, the packaging film 100 has good water vapor barrier properties and can effectively protect the substances in the packaging film 100.
[0060] In some exemplary embodiments, the packaging film 100 satisfies Condition IV: the packaging film 100 has a stretchability A1, where A1 satisfies 1% ≤ A1 ≤ 20%. For example, A1 can be 1%, 2%, 10%, 20%, and so on. When the stretchability A1 of the packaging film 100 satisfies 1% ≤ A1 ≤ 20%, the packaging film 100 can be ductile. When the pressure within the interior of the packaging film 100 fluctuates, the packaging film 100 can expand or contract to accommodate the pressure fluctuation. Under stress, damage to the third layer 130 can be mitigated, thereby improving barrier reliability. When the packaging film 100 is used in an electrochemical device, in the later stages of the electrochemical device cycle, the expansion of gas generated within the electrochemical device can affect the packaging film 100, easily causing deformation and stretching of the packaging film 100. When the elongation rate of the packaging film 100 is lower than 1%, the tensile performance of the packaging film 100 is poor. In the event of deformation and stretching, the structure of the third layer 130 will be damaged, resulting in defects. Water vapor enters the internal space of the electrochemical device through the defects, inducing side reactions and deteriorating the performance of the electrochemical device.
[0061] In some exemplary embodiments, the packaging film 100 satisfies condition V: the packaging film 100 has a thickness H2, where H2 satisfies 20 μm ≤ H2 ≤ 300 μm. For example, H2 can be 20 μm, 60 μm, 100 μm, 200 μm, or 300 μm. When the thickness H2 of the packaging film 100 satisfies 20 μm ≤ H2 ≤ 300 μm, the packaging film 100 has good strength and can block water vapor penetration, thereby protecting the electrode assembly 400.
[0062] As shown in FIG6 , the third layer 130 includes an inorganic layer 12, and the inorganic layer 131 includes at least one of an oxide, a nitride, and a carbon material. Optionally, the oxide includes at least one of aluminum oxide, magnesium oxide, zinc oxide, silicon oxide, titanium oxide, hafnium dioxide, zirconium oxide, iron oxide, copper oxide, silver oxide, nickel oxide, manganese oxide, tin oxide, titanium zirconium oxide, or vanadium oxide. The nitride includes at least one of silicon nitride, silicon oxynitride, boron nitride, titanium nitride, or aluminum nitride. The carbon material includes at least one of graphene, graphyne, and flake graphite.
[0063] The third layer 130 includes an organic layer 132, and the organic layer 132 includes at least one of butyl rubber, silicone, ethylene vinyl alcohol copolymer, high-density polyethylene, polyparaxylene, polypropylene, polyvinyl chloride, polystyrene, epoxy resin, phenolic resin, polyimide resin, acrylic resin, silicone resin, polyolefin resin, and polyethylene terephthalate.
[0064] The organic layers 132 and the inorganic layers 131 of the third layer 130 are alternately stacked. Optionally, as shown in FIG7 , the third layer 130 includes multiple organic layers 132 and multiple inorganic layers 131 . This effectively prevents water vapor and oxygen molecules in the air from entering the electrochemical device 200 and prevents solvent molecules in the electrolyte from escaping the electrochemical device 200 .
[0065] In some exemplary embodiments, the first layer 110 includes at least one of a thermosetting resin or a thermoplastic resin. Optionally, the first thermosetting resin includes one or more of a phenolic resin, an epoxy resin, a melamine resin, a polyimide resin, a polyester resin, an acrylic resin, a silicone resin, or a cross-linked polyolefin resin. Optionally, the first thermoplastic resin includes one or more of polypropylene, polyethylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyphenylene oxide, or polysulfone.
[0066] Optionally, the first layer 110 further includes first inorganic particles, and the first inorganic particles include at least one of aluminum oxide, silicon oxide, calcium oxide, and silica sol.
[0067] In some exemplary embodiments, the packaging film 100 also includes a fourth layer 140, which is disposed on the surface of the third layer 130. The fourth layer 140 includes a synthetic resin material and a filler. The synthetic resin material includes at least one of a second thermosetting resin and a second thermoplastic resin, and the filler includes at least one of fibers and second inorganic particles.
[0068] Optionally, the second thermosetting resin includes at least one of a phenolic resin, an epoxy resin, an amino resin, an acrylic resin, a silicone resin, and a cross-linked polyolefin resin. The second thermoplastic resin includes at least one of a polyolefin and a polyester resin. The fiber includes at least one of a glass fiber, a carbon fiber, an aramid fiber, and a polyethylene fiber. The second inorganic particles include at least one of alumina, silicon oxide, calcium oxide, and silicon-based particles.
[0069] The electrode assembly 400 includes a positive electrode sheet, a separator, a negative electrode sheet, a positive electrode tab, and a negative electrode tab. The positive electrode sheet, separator, and negative electrode sheet are stacked or wound in a stacked manner. The positive electrode tab is electrically connected to the positive electrode sheet, and the negative electrode tab is electrically connected to the negative electrode sheet. The positive and negative electrode tabs are extended from the interior space of the packaging film for electrical connection to an external circuit. The electrochemical device 200 also includes an electrolyte, which fills the interior space of the packaging film and impregnates the electrode assembly 400.
[0070] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector and comprising a positive electrode active material. For example, the positive electrode current collector has two opposing surfaces in its thickness direction, and the positive electrode active material layer is disposed on either or both of the two opposing surfaces of the positive electrode current collector.
[0071] The present application has no particular limitation on the positive electrode active material layer, and the positive electrode active material layer may be any positive electrode active material layer known in the art.
[0072] The positive electrode active material layer includes a positive electrode active material, and the positive electrode active material layer may include at least one of NCM811, NCM622, NCM523, NCM111, NCA, lithium iron phosphate, lithium cobaltate, lithium manganate, lithium iron manganese phosphate, or lithium titanate. The positive electrode active material layer also includes a binder and a conductive agent. In some embodiments, the conductive agent in the positive electrode active material layer may include at least one of conductive carbon black, acetylene black, Ketjen black, flake graphite, graphene, carbon nanotubes, or carbon fibers. In some embodiments, the binder in the positive electrode active material layer may include at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride and hexafluoropropylene, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, styrene-acrylate copolymer, styrene-butadiene copolymer, polyamide, sodium carboxymethyl cellulose, polyvinyl acetate, polyvinylpyrrolidone, polyvinyl ether, polytetrafluoroethylene, polyhexafluoropropylene, or polymethyl methacrylate.
[0073] The present application has no particular restrictions on the positive electrode current collector, and the positive electrode current collector can be any positive electrode current collector known in the art. For example, the positive electrode current collector can be a metal foil or a composite current collector. As an example of a metal foil, the positive electrode current collector can be aluminum foil. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material can be selected from one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer can be selected from polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.
[0074] The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector and comprising a negative electrode active material. For example, the negative electrode current collector has two opposing surfaces in its thickness direction, and the negative electrode active material layer is disposed on either or both of the two opposing surfaces of the negative electrode current collector.
[0075] The present application has no particular limitation on the negative electrode active material layer, and the negative electrode active material layer may be any negative electrode active material layer known in the art.
[0076] The negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes at least one of a high expansion negative electrode material such as pure silicon, silicon carbon or silicon oxide, tin, tin compound, lithium metal, etc., preferably a pure silicon material. In some embodiments, the negative electrode active material layer may further include a conductive agent and / or a binder. The conductive agent in the negative electrode active material layer may include at least one of carbon black, acetylene black, Ketjen black, flake graphite, graphene, carbon nanotubes, carbon fibers, or carbon nanowires. In some embodiments, the binder in the negative electrode active material layer may include at least one of carboxymethyl cellulose (CMC), polyacrylic acid, polyacrylate, polyacrylate, polyvinyl pyrrolidone, polyaniline, polyimide, polyamide-imide, polysiloxane, styrene-butadiene rubber, epoxy resin, polyester resin, polyurethane resin, or polyfluorene.
[0077] The present application has no particular limitation on the negative electrode current collector, and the negative electrode current collector can be any positive electrode current collector known in the art. For example, the negative electrode current collector can be at least one of copper foil, nickel foil, or a carbon-based current collector.
[0078] The present application has no particular restrictions on the electrolyte, and any electrolyte known in the art can be used. The electrolyte can be in any of the following forms: gel, solid, and liquid. For example, the liquid electrolyte includes a lithium salt and a non-aqueous solvent. The present application has no particular restrictions on the lithium salt, and any lithium salt known in the art can be used, as long as the purpose of the present application can be achieved. For example, the lithium salt can include at least one of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, or LiPO2F2. For example, LiPF6 can be used as the lithium salt.
[0079] The present application does not particularly limit the non-aqueous solvent, as long as the purpose of the present application can be achieved. For example, the non-aqueous solvent may include at least one of a carbonate compound, a carboxylate compound, an ether compound, a nitrile compound, or other organic solvents. For example, the carbonate compound may include at least one of diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC), ethyl methyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinyl ethylene carbonate (VEC), fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, or trifluoromethylethylene carbonate.
[0080] The present application also provides an electronic device, including the electrochemical device 200 as described above. The electronic device of the present application is not particularly limited, and it can be any electronic device known in the prior art. In some embodiments, the electronic device can include, but is not limited to, a laptop computer, a pen-input computer, a mobile computer, an e-book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD TV, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery and a lithium-ion capacitor, etc.
[0081] The following describes the electrochemical device 200 of the present application using a lithium-ion battery as an example. The following examples are illustrative and intended only to explain the present application and are not to be construed as limiting the present application. Where specific techniques or conditions are not specified in the examples, the techniques or conditions described in literature in the art or in accordance with the product specifications were followed. Reagents or instruments used without manufacturer identification are all commercially available conventional products.
[0082] 1. Preparation of lithium-ion batteries
[0083] 1. Preparation of positive electrode sheet
[0084] The positive electrode active material, lithium cobalt oxide (LiCoO2), conductive carbon black (Super P), and polyvinylidene fluoride (PVDF), are mixed in a weight ratio of 97.5:1.0:1.5. N-methylpyrrolidone (NMP) is added as a solvent to form a slurry with a solid content of 0.75%, and stirred evenly. The slurry is evenly coated on the positive electrode current collector aluminum foil and dried at 90°C to obtain a single-sided coated positive electrode sheet. Subsequently, the above steps are repeated on the back of the sheet using the same method to obtain a double-sided coated positive electrode sheet. After cold pressing, the positive electrode sheet is cut into a size of (980mm×58mm) for use.
[0085] 2. Preparation of negative electrode sheet
[0086] The negative electrode active material, graphite, conductive carbon black (Super P), and binder are mixed in a weight ratio of 90:5:5. Deionized water is added as a solvent to create a slurry with a solid content of 0.7%, and the mixture is stirred evenly. The slurry is evenly coated on the negative electrode current collector copper foil and dried at 110°C to obtain a single-sided coated negative electrode sheet. Subsequently, these steps are repeated on the back of the sheet using the same method to obtain a double-sided coated negative electrode sheet. After cold pressing, the negative electrode sheet is cut into a size of (1000mm × 60mm) for future use.
[0087] 3. Preparation of electrolyte
[0088] In a dry argon atmosphere, the organic solvents ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) were first mixed in a mass ratio of EC:EMC:DEC = 30:50:20, and then lithium salt lithium hexafluorophosphate (LiPF6) was added to the organic solvent to dissolve and mix evenly to obtain an electrolyte with a lithium salt concentration of 1.15M.
[0089] 4. Preparation of electrode assembly 400
[0090] The positive electrode tab is laser welded to the positive electrode sheet, and the negative electrode tab is laser welded to the negative electrode sheet, with the positive and negative electrode tabs oriented in the same direction. The prepared positive electrode, negative electrode, and separator components are stacked in order, with the separator positioned between the positive and negative electrodes to provide isolation. The stacked electrode sheets and separator are then rolled into an electrode assembly 400, which is then packaged.
[0091] Specifically, the electrode assembly 400 is preferably wrapped with an inner layer of polyethylene material, and the wrapped electrode assembly 400 is placed in a customized mold. The polyethylene is melted into one piece by heating, blow molding or blister molding to form a first layer 110. The second layer 120 is then vapor-deposited on the surface of the closed inner layer by vapor deposition. Similarly, the inorganic material in the third layer 130 is also vapor-deposited on the surface of the second layer 120 by vapor deposition. The organic layer 132 in the third layer 130 is coated on the surface of the layer formed by the inorganic material by coating or vapor deposition to form the final third layer 130. Finally, a fiber-containing resin material is coated on the surface of the third layer 130 by coating on the outer surface of the third layer 130 to form the fourth layer 140. The electrode assembly 400 is then injected with liquid, and the injected electrode assembly 400 is packaged. After the packaged electrode assembly 400 is subjected to operations such as formation (0.02C constant current charging to 3.3V, then 0.1C constant current charging to 3.6V), a soft-pack lithium-ion battery is obtained.
[0092] 2. Lithium-ion battery performance test method
[0093] 1. Water vapor transmission rate (WVTR) test
[0094] Use ceramic scissors to carefully disassemble the finished lithium-ion battery, peel off the electrode assembly 400 and the packaging film 100, and remove at least 1cm 2 The size of the packaging film 100. At the same time, prepare an aluminum-plastic film with a diameter of 10 cm, which has at least one 0.5 cm 2 Hole defect: Use double-sided tape or sealant to attach the finished battery packaging film 100 to the hole area of the aluminum-plastic film, and then perform a water vapor transmission rate (WVTR) test in accordance with the national standard "GB / T 21529-2008".
[0095] 2. Infrared test
[0096] Take 4*4cm 2 Place the encapsulation film sample flat on the surface of the attenuated total reflection crystal with the first layer (inner layer) facing up. Click Collect Sample in the menu, enter the sample name, and begin the test. After the test is complete, save the data. Then, perform automatic baseline and atmospheric background correction on the data.
[0097] 3. X-ray computed tomography (X-Ray CT)
[0098] The battery is transferred to a chamber equipped with an X-ray computed tomography (X-CT) scanner (GE Phoenix m300) for scanning. The scanned images are then processed using the equipment's accompanying software. The processed images can be used to create arbitrary cross-sections of the battery, yielding synthesized X-ray CT cross-sectional images.
[0099] When selecting a cross-sectional image, avoid capturing the outermost area of the battery containing the tabs. The brightness of the captured image should be adjusted until the outline of the packaging film 100 can be distinguished.
[0100] 4. Observe the outline of the packaging film 100 under an optical microscope
[0101] The lithium-ion battery is completely embedded in epoxy resin, and then placed in a liquid nitrogen atmosphere to undergo quenching treatment (the outermost side of the battery quenching position does not include the tabs). The fracture surface is then smoothed using cryo-ultrathin sectioning technology to obtain a sample suitable for optical microscopy observation.
[0102] The sample was placed under an optical microscope (model: Olympus BX53M), the focus was adjusted to a clear position of 100° for the packaging film, a microscope lens with a suitable magnification was selected, and the image stitching function was used to obtain a complete cross-sectional optical microscopic image.
[0103] 5. X-ray energy dispersive spectrometry (EDS)
[0104] The battery is completely embedded with epoxy resin, and then placed in a liquid nitrogen atmosphere for quenching (the outermost side of the cell quenching position does not contain the tabs, and the cryo-ultrathin sectioning technique is used to smooth the cross section for better results). Samples from the 100-degree area of the packaging film are transferred to the scanning electron microscope (SEM) cavity to obtain samples for SEM analysis.
[0105] The sample was observed under a SEM, and data was collected using X-ray energy dispersive spectrometry (EDS) at an appropriate magnification to obtain the element content of the packaging film 100. Data was collected at at least three different locations and the average value was taken.
[0106] 6. Energy density of lithium-ion batteries
[0107] The lithium-ion battery was placed at 25±2°C for 5 minutes, first charged to 4.40V at 0.5C, then charged to 0.025C at a constant voltage, and after 5 minutes of standing, discharged to 3.0V at 0.01C. The discharge capacity was recorded, and the 0.01C discharge energy density was calculated according to the following formula: Energy density (Wh / L) = discharge capacity (Wh) / electrochemical device volume size (L).
[0108] 7. Battery cycle capacity retention rate
[0109] The battery was left at 25±3°C for 5 minutes. Connected to the external circuit, the battery was charged at a constant current of 0.5C to 4.4V. Then, it was charged at a constant voltage of 4.4V to a current of 0.05C. The battery was then discharged at a current of 0.2C to 3.0V. The discharge capacity was recorded as Q1. Repeat this step 500 times, recording the discharge capacity as Q500. The capacity retention after 500 cycles at 25°C is: η (%) = Q500 / Q1 × 100%.
[0110] The lithium-ion batteries of Examples and Comparative Examples were prepared according to the above method and tested.
[0111] 8. Hot box test
[0112] The battery cell is charged at a constant current of 0.5C to 4.4V, then at a constant voltage of 4.4V to a current of 0.05C. Place a temperature sensor in the center of the battery cell and place it vertically in the chamber. Raise the temperature at a rate of 5±2°C to 132±2°C and maintain the temperature for 60 minutes. The battery cell passes the test if it does not catch fire or explode.
[0113] In Table 1, Comparative Example 1 uses aluminum-plastic film to encapsulate the electrode assembly 400, Comparative Example 2 uses 316L stainless steel to encapsulate the electrode assembly 400, and Example 1 uses the packaging film 100 for packaging, and the packaging film 100 includes a first layer 110, a second layer 120, a third layer 130 and a fourth layer 140, and the second layer 120 includes polyparaxylene.
[0114] Table 1
[0115] In Table 1, it can be seen from Comparative Example 1, Comparative Example 2 and Example 1 that the volume energy density of the lithium-ion battery is affected by packaging the electrode assembly 400 in different packaging methods. Comparative Example 1 is a traditional soft package, and Comparative Example 2 is a traditional metal shell package. The top side sealing of Comparative Example 1 and the flange edge of Comparative Example 2 have a great influence on the energy density, resulting in a significant deterioration in the energy density. Example 1 is a molten packaging of the packaging film 100. Among them, the coating packaging method adopted by the packaging film 100 of the present application increases the energy density of the lithium-ion battery by more than 15% compared with the traditional packaging method. In addition, compared with Comparative Examples 1 and 2, the WVTR and corresponding cycle performance of the lithium-ion battery of Example 1 have not been significantly attenuated, while taking into account both energy density and cycle stability, thereby improving product competitiveness.
[0116] Table 2
[0117] In Table 2, the second layer material of Comparative Example 3 is epoxy resin, the second layer material of Comparative Example 4 is polystyrene resin, the second layer material of Example 2 is polychloroparaxylene, and the second layer material of Example 3 is polydifluoroparaxylene.
[0118] Table 2 shows that Comparative Examples 3 and 4 use different second layer 120 materials. These materials have limited effect on improving substrate defects, resulting in poor coating quality for the subsequent third layer 130. This deteriorates the WVTR, allowing water vapor to enter the battery, triggering side reactions and causing capacity loss, thereby degrading the battery's energy density and cycle performance. The polychloroparaxylene material in Example 2 and the polydifluoroparaxylene material in Example 3 penetrate every pore during the vapor deposition process, effectively compensating for surface defects in the first layer 110, improving flatness, and reducing roughness. Furthermore, the repeating units of polychloroparaxylene and polydifluoroparaxylene cross-link to form a network structure with good density. This inherent water vapor barrier function further enhances the water vapor barrier function of the third layer 130.
[0119] The parameters and experimental results of Examples 4 to 10 are shown in Table 3.
[0120] Table 3
[0121] In Table 3, according to Examples 2, 4, and 5, the thickness H1 of second layer 120 ranges from 0.5 μm to 10 μm, demonstrating excellent barrier properties and improving surface defects in first layer 110. Furthermore, second layer 120 exhibits suitable rigidity, preventing excessive internal stress within layer 120 from affecting the coating process of the third layer due to excessive thickness. In addition to thickness, a high melting point of second layer 120 within a certain temperature range helps improve the temperature resistance of packaging film 100, thereby enhancing thermal safety. In addition, according to Examples 2, 7 and 8, the adhesion force N1 between the second layer 120 and the first layer 110 is in the range of 3N / 15mm to 15N / 15mm, and according to Examples 8 to 10, the adhesion force N2 between the second layer 120 and the third layer 130 is in the range of 3N / 15mm to 15N / 15mm. The interface adhesion between the first layer 110, the second layer 120 and the third layer 130 is stable and not easy to peel off, so that the packaging film 100 has good water vapor barrier capability, thereby improving the stability and safety of lithium-ion batteries.
[0122] The same or similar numbers in the drawings of this embodiment correspond to the same or similar parts; in the description of this application, it should be understood that if the terms "upper", "lower", "left", "right", etc. indicate an orientation or position relationship, they are based on the orientation or position relationship shown in the drawings. This is only for the convenience of describing this application and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation. Therefore, the terms describing the position relationship in the drawings are only used for illustrative purposes and cannot be understood as a limitation on this patent. For ordinary technicians in this field, the specific meanings of the above terms can be understood according to specific circumstances.
[0123] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent replacements and improvements made within the spirit and principles of the present application should be included in the scope of protection of the present application.
Claims
1. An electrochemical device comprising an electrode assembly and a packaging film for packaging the electrode assembly, It is characterized in that The packaging film comprises: a first layer, a second layer and a third layer; The second layer is connected between the first layer and the third layer, and the second layer includes a polymer material. The infrared characteristic peak position of the polymer material of the second layer satisfies: at 822±5cm -1 There is a characteristic peak of benzene ring substitution at 1400cm -1 ~1650cm -1 There is vibration of benzene skeleton.
2. The electrochemical device according to claim 1, It is characterized in that The substitution position in the polymer material contains halogen, and the halogen contains at least one of chlorine or fluorine. Based on the mass of the polymer material, the mass percentage of the halogen in the polymer material is w1, and w1 satisfies: 5wt%≤w1≤50wt%.
3. The electrochemical device according to claim 2, It is characterized in that The polymer material includes one or more of polyparaxylene, polymonochloroparaxylene, and polydichloroparaxylene.
4. The electrochemical device according to claim 1, It is characterized in that The second layer satisfies at least one of the following conditions: (1) The melting point of the second layer is T1, and T1 satisfies 150°C ≤ T1 ≤ 400°C; (2) The thickness of the second layer is H1, and H1 satisfies 0.5 μm ≤ H1 ≤ 10 μm; (3) The polymer material comprises a repeating unit as shown in formula a; Among them, R 1 , R 2 , R 3 , R 4 , R 5 , R 6 are each independently selected from one of H and halogen, and R 1 ~R 6 At least one of them is selected from any one of the halogens.
5. The electrochemical device according to claim 1, It is characterized in that The packaging film satisfies at least one of the following conditions: Ⅰ. The bonding strength between the second layer and the first layer is N1, and N1 satisfies 3N / 15mm≤N1≤15N / 15mm; Ⅱ. The bonding strength between the second layer and the third layer is N2, and N2 satisfies 3N / 15mm≤N2≤15N / 15mm; III. Under the conditions of temperature of 38°C and humidity of 90%, the water vapor permeability of the packaging film WVTR≤10 -3 g / (m 2 *day); IV. The stretching rate of the packaging film is A1, A1 satisfies 1%≤A1≤20%; V. The thickness of the packaging film is H2, and H2 satisfies 20μm≤H2≤300μm.
6. The electrochemical device according to claim 1, wherein the third layer satisfies at least one of the following: (1) the third layer includes an inorganic layer, and the inorganic layer includes at least one of aluminum oxide, magnesium oxide, zinc oxide, silicon oxide, titanium oxide, hafnium dioxide, zirconium oxide, iron oxide, copper oxide, silver oxide, nickel oxide, manganese oxide, tin oxide, zirconium titanium oxide, vanadium oxide, silicon nitride, silicon oxynitride, boron nitride, titanium nitride, aluminum nitride, graphene, graphyne, and flake graphite; (2) The third layer includes an organic layer, and the organic layer includes at least one of butyl rubber, silica gel, ethylene-vinyl alcohol copolymer, polyparaxylene, polyvinyl chloride, polystyrene, epoxy resin, phenolic resin, polyimide resin, acrylic resin, silicone resin, polyolefin resin, and polyethylene terephthalate.
7. The electrochemical device according to claim 1, It is characterized in that The first layer includes at least one of polyvinyl chloride, polystyrene, phenolic resin, epoxy resin, melamine resin, polyimide resin, polyester resin, acrylic resin, silicone resin, cross-linked polyolefin resin, polyoxymethylene, polycarbonate, polyphenylene ether or polysulfone.
8. The electrochemical device according to claim 1, It is characterized in that The packaging film further comprises a fourth layer, and the fourth layer is arranged on the surface of the third layer; The fourth layer includes a resin material and a filler, wherein the resin material includes phenolic resin, epoxy resin, At least one of amino resin, acrylic resin, silicone resin, cross-linked polyolefin resin, polyolefin, polyester resin, and the filler includes at least one of glass fiber, carbon fiber, aramid fiber, polyethylene fiber, aluminum oxide, calcium oxide, and silicon-based particles.
9. The electrochemical device according to claim 1, It is characterized in that The packaging film comprises a top wall, a side wall and a bottom wall, and the electrode assembly comprises a tab, and the tab extends out of the packaging film from the top wall; The first layer, the second layer and the third layer are each in a closed form.
10. An electronic device comprising the electrochemical device according to any one of claims 1 to 9.
Citation Information
Patent Citations
Energy storage devices and systems
CN110574205A
Encapsulation system for electronic components and batteries
CN110809830A
Electrochemical device, preparation method thereof and electronic device
CN113097613A
Flushing device for main control valve of turbine
KR1020240017250A