Secondary battery and electronic device
By using a thin base film and nitrile-based additives in secondary batteries, and regulating the content of nitrile-based additives in the electrolyte and positive electrode, the self-discharge problem under high output voltage is solved, and the energy density and cycle performance of the secondary battery are improved.
Patent Information
- Application Number
- PCT/CN2023/085785
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-03
AI Technical Summary
Secondary batteries are prone to self-discharge problems under high output voltage and thin separator conditions, which affects charge-discharge consistency and cycle performance.
A separator with a thin base film is used, combined with nitrile-based additives in the electrolyte and nitrile-based additives in the cathode, to regulate their mass percentages and work synergistically to reduce the dissolution and diffusion resistance of transition metal ions and improve self-discharge problems.
It improves the energy density and cycle performance of secondary batteries, reduces self-discharge during charging and discharging, and improves the string voltage difference and cycle performance of secondary battery modules under high pressure and high temperature.
Smart Images

Figure PCTCN2023085785-FTAPPB-I100001 
Figure PCTCN2023085785-FTAPPB-I100002 
Figure PCTCN2023085785-FTAPPB-I100003
Abstract
Description
Secondary battery and electronic device Technical Field
[0001] The present application relates to the technical field of electrochemical energy storage, and in particular to a secondary battery and an electronic device. Background Art
[0002] Secondary batteries (such as lithium-ion batteries) are increasingly trending towards larger capacity and higher energy density. Separators are an essential component of current secondary batteries, isolating the positive and negative electrodes to prevent short circuits. However, these membranes do not contribute to the battery's capacity. Consequently, thinner separators are becoming increasingly popular, an effective measure for increasing energy density. Furthermore, the output voltage of secondary batteries is also trending upwards, thereby increasing capacity and energy density.
[0003] Summary of the Invention
[0004] The inventors of this application discovered that in notebook computer systems, because secondary battery modules are assembled in a series-parallel manner, there are high requirements for the output voltage and capacity consistency of individual secondary batteries in the secondary battery module. If the output voltage of the secondary battery is high and a thin diaphragm is used, the diaphragm's function of isolating the positive and negative electrodes is weakened, and self-discharge occurs within the secondary battery, affecting the consistency of the secondary battery, causing series voltage differences during the charge and discharge process of the secondary battery module, and reducing the cycle performance of the secondary battery.
[0005] The purpose of the present application is to provide a secondary battery and an electronic device to improve the energy density of the secondary battery and improve the self-discharge problem during the charging and discharging process of the secondary battery.
[0006] It should be noted that in the invention content of this application, lithium-ion batteries are used as an example of secondary batteries to explain this application, but the secondary batteries of this application are not limited to lithium-ion batteries. The specific technical solutions are as follows:
[0007] In a first aspect, the present application provides a secondary battery comprising an electrode assembly and an electrolyte, the electrode assembly comprising a positive electrode sheet, a negative electrode sheet, and a separator, the separator being disposed between the positive electrode sheet and the negative electrode sheet, the positive electrode sheet comprising a positive current collector and a positive electrode active material layer disposed on at least one surface of the positive current collector, the positive electrode active material layer comprising a positive electrode active material, the positive electrode active material comprising a transition metal element, the transition metal element comprising at least one of Co, Ni, Mn, Fe, or V; and the separator comprising a base film having a thickness of D μm, 3 ≤ D ≤ 7. The secondary battery comprises an electrolyte containing a nitrile-based additive and a positive electrode containing a nitrile-based additive, the mass percentage of the electrolyte containing the nitrile-based additive being x% based on the mass of the electrolyte, the mass percentage of the positive electrode containing the nitrile-based additive being y% based on the mass of the positive electrode active material layer, x + y = z, 0.3 ≤ z ≤ 3.3, 0 < x ≤ 2.3, and 0 < y ≤ 1.
[0008] The present application improves the energy density of a secondary battery by using a diaphragm having a thin base film, and simultaneously uses an electrolyte containing a nitrile-based additive and a positive electrode containing a nitrile-based additive, and controls the mass percentage of the electrolyte containing the nitrile-based additive and the mass percentage of the positive electrode containing the nitrile-based additive within the above-mentioned range. The nitrile-based additive in the electrolyte and the nitrile-based additive in the positive electrode act synergistically with the diaphragm, thereby reducing the amount of transition metal ions (such as Co ions) dissolved inside the secondary battery under high voltage conditions, and regulating the diffusion impedance, thereby improving the self-discharge problem during the charging and discharging process of the secondary battery.
[0009] In some embodiments of the present application, 1.4≤z≤3.3, which further improves the self-discharge problem of the secondary battery during the charge and discharge process.
[0010] In some embodiments of the present application, the electrolyte contains a carbon-nitrogen atom number ratio of m1, 1≤m1≤6, and the electrolyte contains a nitrile-based additive including malononitrile, succinonitrile, glutaronitrile, adiponitrile, pimelonitrile, octanedinitrile, sebacononitrile, 3,3'-oxydipropionitrile, hexamethylenedinitrile, fumaronitrile, 2-pentamethylenedinitrile, methylglutaronitrile, 4-nitrile pimelonitrile, (Z)-but-2-enedinitrile, 2,2,3,3-tetrafluorosuccinonitrile, ethylene glycol bis(propionitrile) ether, 1,3,5-pentanetricarbonitrile, 1,3,6-hexanetricarbonitrile, 1,2,6-hexanetricarbonitrile, 1,2,3-tris(2-nitrileoxy)propane or 1,1,3,3-propanetetracarbonitrile. The selection of the above-mentioned electrolyte containing nitrile-based additives is beneficial to improving the self-discharge problem during the charge and discharge process of the secondary battery and having good room temperature cycle performance.
[0011] In some embodiments of the present application, the positive electrode nitrile-containing additive is a nitrile-containing polymer, the carbon-nitrogen atom number ratio of the positive electrode nitrile-containing additive is m2, 3≤m2≤5, and the weight average molecular weight of the positive electrode nitrile-containing additive is Mw , 300≤M w ≤700000. Regulating the carbon-nitrogen atom number ratio and weight-average molecular weight of the positive electrode nitrile-containing additive within the above range is beneficial to improving the self-discharge problem during the charge and discharge process of the secondary battery, and can reduce the impact of the addition of the positive electrode nitrile-containing additive on the manufacturing performance of the positive electrode sheet.
[0012] In some embodiments of the present application, the positive electrode nitrile-containing additive includes at least one of polyacrylonitrile, polybutenenitrile, or polyisobutenenitrile. The use of the above-mentioned positive electrode nitrile-containing additive is conducive to improving the self-discharge problem of the secondary battery during the charge and discharge process.
[0013] In some embodiments of the present application, the output voltage of the secondary battery is greater than or equal to 4.48 V and less than or equal to 4.6 V. Controlling the output voltage of the secondary battery within this range can better balance energy density performance and self-discharge risk.
[0014] In some embodiments of the present application, the output voltage of the secondary battery is less than or equal to 4.56V.
[0015] In some embodiments of the present application, 0.035D 2 -0.562D+2.253≤y≤0.027D 2 By adjusting the relationship between the thickness of the base film and the mass percentage of the nitrile-based additive in the positive electrode, it is beneficial to improve the self-discharge problem during the charging and discharging process of the secondary battery.
[0016] In some embodiments of the present application, the material of the base film includes polyolefin, and the polyolefin includes at least one of polyethylene or polypropylene.
[0017] In some embodiments of the present application, the diaphragm also includes an insulating layer arranged on the surface of the base film, the insulating layer includes inorganic particles and a binder; the inorganic particles include aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide or barium sulfate, and the binder includes at least one of styrene-butadiene rubber, polyacrylic acid, polyvinyl alcohol, polyethylene glycol, polyacrylate, polyvinylidene fluoride, polyvinyl chloride, formaldehyde resin or cyanoacrylate.
[0018] In some embodiments of the present application, the base film has a multi-layer structure, which is beneficial for hindering the shuttle of transition metal elements between the positive and negative electrodes through the layer interfaces of the multi-layer film structure, thereby reducing the risk of self-discharge.
[0019] In some embodiments of the present application, the positive electrode active material includes at least one of lithium cobaltate, lithium nickel cobalt manganeseate, lithium nickel cobalt aluminumate, lithium manganeseate, lithium iron phosphate, or lithium iron manganese phosphate.
[0020] In a second aspect, the present application provides an electronic device comprising the secondary battery according to any one of the aforementioned embodiments. Therefore, the electronic device has good cycle performance.
[0021] Beneficial effects of this application:
[0022] The present application provides a secondary battery and an electronic device, wherein the secondary battery includes an electrode assembly and an electrolyte, the electrode assembly includes a positive electrode sheet, a negative electrode sheet, and a separator, the separator being disposed between the positive electrode sheet and the negative electrode sheet, the positive electrode sheet including a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, the positive electrode active material layer including a positive electrode active material, the positive electrode active material including a transition metal element, the transition metal element including at least one of Co, Ni, Mn, Fe, or V; the separator including a base film, the base film having a thickness of D μm, 3 ≤ D ≤ 7; the secondary battery including an electrolyte containing a nitrile-based additive and a positive electrode containing a nitrile-based additive, the mass percentage of the electrolyte containing the nitrile-based additive being x%, the mass percentage of the positive electrode containing the nitrile-based additive being y%, based on the mass of the positive electrode active material layer, x + y = z, 0.3 ≤ z ≤ 3.3, 0 < x ≤ 2.3, and 0 < y ≤ 1. Through the above arrangement, a secondary battery with a higher energy density can be obtained, and the self-discharge problem during the charging and discharging process of the secondary battery can be improved. DETAILED DESCRIPTION
[0023] To make the objectives, technical solutions, and advantages of this application more clearly understood, the following examples are given to further describe this application in detail. It is apparent that the described examples are only a portion of the embodiments of this application, and not all of them. All other embodiments derived by persons of ordinary skill in the art based on the examples in this application are intended to fall within the scope of protection of this application.
[0024] It should be noted that, in the specific embodiments of the present application, lithium-ion batteries are used as an example of secondary batteries to explain the present application, but the secondary batteries of the present application are not limited to lithium-ion batteries.
[0025] The inventors have found that when using high output voltage (such as above 4.48V) and thin diaphragms (such as base film thickness of 3μm to 7μm) to improve the energy density of secondary batteries, it is easy to cause the problem of voltage difference during the charge and discharge process of the secondary battery. Analysis and research believe that the main reason is chemical self-discharge. Chemical self-discharge is mainly caused by the reversible redox product, which shuttles between the positive and negative electrodes through the electrolyte and the diaphragm. At present, the shuttle charge is derived from the transition metal elements in the positive electrode active material, such as Co 2+ / Co 3+ Cobalt (Co) is the 27th element, which is usually Co 2+ and Co 3+ The outermost electron configurations are d7 and d6, Co 2+ Co 3+ There is one more electron in the outermost d orbital, and this electron can 2+ Transfer to Co 3+ , and the constant voltage time is too long. The secondary battery contains more cobalt ions of different valence states in the electrolyte, and the electron transfer between them causes electronic conductivity. And the higher the output voltage of the secondary battery, the more by-products inside the secondary battery; the thinner the thickness of the diaphragm, the shorter the diffusion path of the by-products inside the secondary battery between the positive and negative electrodes, and the thicker the thickness, the longer the diffusion path, thereby affecting the diffusion impedance of the secondary battery and causing self-discharge inside the secondary battery. Therefore, the Co dissolution content and diffusion impedance are the two main factors affecting chemical self-discharge. The existence of chemical self-discharge will affect the consistency of the secondary battery, bring about the problem of series voltage difference during the charging and discharging process of the secondary battery module, and reduce the cycle performance of the secondary battery. In view of this, the present application provides a secondary battery and an electronic device.
[0026] In a first aspect, the present application provides a secondary battery comprising an electrode assembly and an electrolyte. The electrode assembly comprises a positive electrode sheet, a negative electrode sheet, and a separator. The separator is disposed between the positive electrode sheet and the negative electrode sheet. The positive electrode sheet comprises a positive current collector and a positive electrode active material layer disposed on at least one surface of the positive current collector. The positive electrode active material layer comprises a positive electrode active material, the positive electrode active material comprising a transition metal element, and the transition metal element comprises at least one of Co, Ni, Mn, Fe, or V. The separator comprises a base film having a thickness of D μm, 3 ≤ D ≤ 7. The secondary battery comprises an electrolyte containing a nitrile-based additive and a positive electrode containing a nitrile-based additive. The mass percentage of the nitrile-based additive in the electrolyte is x% based on the mass of the electrolyte; the mass percentage of the nitrile-based additive in the positive electrode is y% based on the mass of the positive electrode active material layer; x + y = z, 0.3 ≤ z ≤ 3.3, and 0 < x ≤ 2.3, 0 < y ≤ 1. For example, D is 3, 4, 5, 6, 7, or any value between any two of the aforementioned numerical ranges. The value of z is 0.3, 1, 1.5, 2, 2.5, 3, 3.3, or any value between any two of the aforementioned numerical ranges. The value of x is 0.01, 0.5, 1.0, 1.5, 2.0, 2.3, or any value between any two of the aforementioned numerical ranges. The value of y is 0.01, 0.2, 0.4, 0.6, 0.8, 0.9, 1, or any value between any two of the aforementioned numerical ranges.
[0027] After extensive research, the inventors discovered that when the positive electrode active material includes at least one transition metal element among Co, Ni, Mn, Fe, or V, electron transfer between ions of different valence states between the transition metal elements will cause electronic conductivity, and self-discharge is likely to occur inside the secondary battery. The higher the output voltage of the secondary battery, the more transition metal elements are dissolved; the smaller the base film thickness, the smaller the volume of the secondary battery, which increases its volumetric energy density, but the diffusion path of byproducts inside the electrode assembly between the positive and negative electrodes is shorter, resulting in increased chemical self-discharge; the thicker the base film thickness, the longer the diffusion path of byproducts inside the secondary battery between the positive and negative electrodes, resulting in reduced chemical self-discharge, but the increased volume of the secondary battery reduces its volumetric energy density. The carbon-nitrogen triple bond in the nitrile group (-CN) has a high bond energy and is not easily oxidized. The nitrile group has a strong coordination ability and can combine with the active sites on the electrode surface (such as the above-mentioned transition metal ions) to mask the active ions on the electrode surface, reducing the electrode's decomposition effect on the electrolyte, thereby suppressing the decomposition of the electrolyte under high output voltage and high temperature, and reducing the generation of byproducts. In this application, high temperature refers to a temperature greater than or equal to 45° C., and high voltage refers to an output voltage greater than or equal to 4.48V.
[0028] The present application improves the energy density of a secondary battery by using a diaphragm with a thin base film, and simultaneously uses an electrolyte containing a nitrile-based additive and a positive electrode containing a nitrile-based additive. When the sum of the mass percentages z of the electrolyte containing the nitrile-based additive and the positive electrode containing the nitrile-based additive is less than 0.3, the mass percentage x% of the electrolyte containing the nitrile-based additive or the mass percentage y% of the positive electrode containing the nitrile-based additive is too small, the nitrile group content is too small, and the ability to bind to the active sites on the electrode surface (such as the above-mentioned transition metal ions) is limited, resulting in limited improvement in the chemical self-discharge inside the secondary battery; and the improvement effect on the decomposition of the electrolyte is limited, and the content of by-products generated after the decomposition of the electrolyte is high, which will affect the performance of the secondary battery (such as cycle performance, storage performance, safety performance, etc.). When the sum of the mass percentages z of the electrolyte-containing nitrile-based additives and the positive electrode-containing nitrile-based additives is greater than 3.3, the mass percentage x% of the electrolyte-containing nitrile-based additives or the mass percentage y% of the positive electrode-containing nitrile-based additives is too large. Due to the strong electronegativity of the nitrile-based functional group, the carbon attached to it usually carries an active α-H group. If the nitrile-based content is too large, the amount of active α-H groups free in the electrolyte will be too large, which will accelerate the consumption of the negative electrode additive (such as fluoroethylene carbonate) and affect the room temperature cycle performance of the secondary battery. In addition, if the electrolyte-containing nitrile-based additives are too much, in addition to forming a stable film on the electrode surface, the excess electrolyte-containing nitrile-based additives will continue to react, consuming active lithium while forming an excessively thick interfacial film, affecting the performance of the secondary battery, such as cycle performance and charge rate. If the positive electrode-containing nitrile-based additives are too much, the cold pressing density of the positive electrode sheet will be affected, resulting in a loss of energy density of the secondary battery. In addition, problems such as tape breakage or film stripping may occur during the cold pressing process of the positive electrode sheet, resulting in the positive electrode sheet being unable to be used normally.
[0029] In the present application, by regulating the thickness of the diaphragm, the mass percentage of the nitrile-based additive in the electrolyte, and the mass percentage of the nitrile-based additive in the positive electrode within the above-mentioned range, the nitrile-based additive in the electrolyte and the nitrile-based additive in the positive electrode work synergistically with the diaphragm, thereby reducing the amount of transition metal ions (such as Co ions) dissolved inside the secondary battery, and regulating the diffusion impedance, thereby improving the self-discharge problem of the secondary battery during charging and discharging at high output voltage and high temperature.
[0030] In this application, unless otherwise specified, the electrolyte nitrile-containing additive is added to the electrolyte, the positive electrode nitrile-containing additive is added to the positive electrode active material layer, and the positive electrode nitrile-containing additive is a nitrile-containing polymer.
[0031] The above-mentioned "positive electrode active material layer disposed on at least one surface of the positive electrode current collector" refers to a positive electrode active material layer disposed on one surface of the positive electrode current collector, or a positive electrode active material layer disposed on both surfaces of the positive electrode current collector. The "surface" may be part of the surface of the positive electrode current collector or the entire surface. In some embodiments of the present application, other material layers may be disposed between the positive electrode active material layer and the positive electrode current collector, such as an adhesive layer, a safety layer, or other active material layers.
[0032] In some embodiments of the present application, secondary batteries can be assembled into secondary battery modules in a series-parallel manner. While the self-discharge problem during the charge and discharge process of the secondary batteries is improved, the consistency of the output voltage and capacity of each secondary battery in the secondary battery module can be improved. As a result, the series voltage difference problem during the charge and discharge process of the secondary battery module is improved, and the cycle performance of the secondary battery under high voltage and high temperature conditions will be improved.
[0033] This application does not specifically limit the number of secondary batteries contained in the secondary battery module, which can be more than two. The specific number can be selected by those skilled in the art based on the application and capacity of the secondary battery module, as long as the purpose of this application can be achieved. This application does not specifically limit the arrangement of secondary batteries in the secondary battery module, as long as the purpose of this application can be achieved. For example, multiple secondary batteries can be arranged in sequence along the length of the secondary battery module. Of course, they can also be arranged in other ways.
[0034] In some embodiments of the present application, 1.4≤z≤3.3. Regulating the sum of the mass percentages z of the electrolyte nitrile-containing additive and the positive electrode nitrile-containing additive within the above range will be more conducive to improving the self-discharge problem during the charge and discharge process of the secondary battery.
[0035] In some embodiments of the present application, the electrolyte contains a nitrile-based additive with a carbon-nitrogen atomic ratio of m1, 1≤m1≤6, for example, m1 is 1, 2, 3, 4, 5, 6 or any value between any two of the above numerical ranges. Further, the electrolyte contains nitrile-based additives including at least one of malononitrile, succinonitrile, glutaronitrile, adiponitrile, pimelonitrile, suberonitrile, decanedinitrile, 3,3'-oxydipropionitrile, hexamethylene dinitrile, fumaronitrile, 2-pentamethylene dinitrile, methylglutaronitrile, 4-cyanopimelonitrile, (Z)-but-2-enedinitrile, 2,2,3,3-tetrafluorosuccinonitrile, ethylene glycol bis(propionitrile) ether, 1,3,5-pentanetricarbonitrile, 1,3,6-hexanetricarbonitrile, 1,2,6-hexanetricarbonitrile, 1,2,3-tris(2-cyanoxy)propane (also known as 1,2,3-tris(2-cyanoxy)propane) or 1,1,3,3-propanetetracarbonitrile. The above-mentioned electrolyte-containing nitrile-based additives have a suitable carbon-nitrogen atomic ratio and good stability. The selection of the above-mentioned electrolyte-containing nitrile-based additives is conducive to the binding of nitrile groups to active sites on the electrode surface, thereby reducing the dissolution of transition metal ions (such as Co ions) inside the secondary battery, thereby improving the self-discharge problem during the charge and discharge process of the electrode assembly. In this way, the consistency of the output voltage and capacity of each secondary battery in the secondary battery module is improved, the series voltage difference problem during the charge and discharge process of the secondary battery module is improved, and the cycle performance of the secondary battery under high pressure and high temperature is improved.
[0036] In some embodiments of the present application, the carbon-nitrogen atom number ratio of the positive electrode nitrile-containing additive is m2,3≤m2≤5, and the weight average molecular weight of the positive electrode nitrile-containing additive is M w , 300≤M w ≤700000. For example, m2 is 3, 4, 5 or any value between any two of the above ranges. wThe carbon-nitrogen atom ratio of the positive electrode nitrile-containing additive is 300, 1000, 10000, 100000, 200000, 300000, 400000, 500000, 600000, 700000, or any value between any two of the above numerical ranges. The carbon-nitrogen atom ratio of the positive electrode nitrile-containing additive is within the above range. The positive electrode nitrile-containing additive has an appropriate amount of polar functional groups and is easy to dissolve in an organic solvent (such as N-methylpyrrolidone), which is conducive to uniform distribution in the positive electrode sheet. In addition, the number of transition metal ions that interact with the nitrile functional groups is reduced, and the transition metal ions are less likely to react with the electrolyte, thereby improving the high-temperature performance of the secondary battery. Positive pole is contained the carbon-nitrogen atom number ratio and the weight-average molecular weight of nitrile-based additive and is regulated within the above-mentioned range, both reduced and dissolved in electrolyte containing nitrile-based polymer, can make again containing nitrile-based polymer in organic solvent, as N-Methyl pyrrolidone, dissolve well, make containing nitrile-based polymer and positive electrode active material mix uniformly, be conducive to the positive pole containing the nitrile group in the nitrile-based additive and combine with the active site of electrode surface, to reduce the dissolution amount of transition metal ion (as Co ion) inside secondary battery, reduce the side reaction occurring between positive electrode active material and electrolyte, the content of by product produced by electrolyte reduces.Thus improve the self-discharge problem in secondary battery charge-discharge process.Like this, the output voltage of each secondary battery in secondary battery module and the consistency of capacity are improved, the series voltage difference problem in secondary battery module charge-discharge process is improved, and the cycle performance of secondary battery under high pressure and high temperature is improved.
[0037] The present application does not particularly limit the method for controlling the weight average molecular weight of the positive electrode nitrile-containing additive, as long as the purpose of the present application can be achieved. For example, this can be achieved by directly purchasing positive electrode nitrile-containing additives of different weight average molecular weights from manufacturers.
[0038] In some embodiments of the present application, the positive electrode nitrile-containing additive includes polyacrylonitrile (molecular formula: (C3H3N) n ), polybutenenitrile (molecular formula: (C4H5N) n ) or polyisobutylene nitrile (molecular formula: (C4H5N) n )). Using the aforementioned positive electrode nitrile-containing additives can further improve the self-discharge problem during the secondary battery's charge and discharge process. This improves the consistency of voltage and capacity among the individual secondary batteries in the secondary battery module, alleviates the series voltage difference problem during the secondary battery module's charge and discharge process, and enhances the secondary battery's cycle performance under high voltage and high temperature conditions.
[0039] In some embodiments of the present application, the output voltage of the secondary battery is greater than or equal to 4.48 V and less than or equal to 4.6 V. In some embodiments of the present application, the output voltage of the secondary battery is less than or equal to 4.56 V. When the output voltage of the secondary battery is within the above range, the energy density of the secondary battery is high, and in combination with the separator of the present application, the electrolyte containing a nitrile-based additive, and the positive electrode containing a nitrile-based additive, the self-discharge problem during the charge and discharge process can be improved.
[0040] The present application does not particularly limit the method for regulating the output voltage of the secondary battery, as long as the purpose of the present application can be achieved. The output voltage of the secondary battery can be regulated by adjusting the positive and negative electrode materials, electrolyte, etc. For example, the output voltage of the secondary battery can be regulated by regulating the doping and / or coating of the positive electrode active material lithium cobalt oxide, or regulating the type of positive electrode active material. For example, lithium cobalt oxide can be doped with elements such as Mg, Al, Ti and / or to increase the output voltage, and these materials can be purchased on the market.
[0041] Furthermore, 0.035D 2 -0.562D+2.253≤y≤0.027D 2 -0.482D+2.257. By regulating the relationship between the thickness of the base film and the mass percentage of the positive electrode nitrile-containing additive, the base film and the positive electrode nitrile-containing additive are facilitated to produce a synergistic effect, thereby reducing the amount of transition metal ions (such as Co ions) dissolved within the secondary battery, and regulating the diffusion impedance, thereby improving the self-discharge problem during the secondary battery's charge and discharge process. In this way, the consistency of the voltage and capacity of each secondary battery in the secondary battery module is improved, the series voltage difference problem during the charge and discharge process of the secondary battery module is improved, and the cycle performance of the secondary battery under high voltage and high temperature is improved.
[0042] In some embodiments of the present application, the material of the base film includes polyolefin, and the polyolefin includes at least one of polyethylene (PE) or polypropylene (PP).
[0043] In some embodiments of the present application, the base film has a multi-layer structure. The present application does not specifically limit the number of layers in a multi-layer structure, as long as the objectives of the present application can be achieved. In some embodiments, the base film has at least two layers, for example, two or three layers. When the base film has a multi-layer structure, combining different materials can maximize the properties of each material. For example, base films include, but are not limited to, PP / PE / PP and PP / PE.
[0044] The present application has no particular limitation on the porosity of the base film, as long as the purpose of the present application can be achieved. For example, the porosity of the base film is 25% to 60%.
[0045] In some embodiments of the present application, in order to improve the strength and insulation properties of the diaphragm and to improve the barrier to the shuttle of transition metal elements, the diaphragm further includes an insulating layer disposed on the surface of the base film, and the insulating layer is disposed on at least one surface of the base film along its own thickness direction. It is understood that in some embodiments of the present application, the insulating layer is disposed on one surface of the base film along its own thickness direction; in other embodiments of the present application, the insulating layer is disposed on both surfaces of the base film along its own thickness direction. The insulating layer includes inorganic particles and a binder. The present application does not particularly limit the type of inorganic particles, as long as the purpose of the present application can be achieved. For example, the inorganic particles include at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, or barium sulfate. The present application does not particularly limit the type of binder, as long as the purpose of the present application can be achieved. For example, the binder includes at least one of styrene-butadiene rubber, polyacrylic acid, polyvinyl alcohol, polyethylene glycol, polyacrylate, polyvinylidene fluoride, polyvinyl chloride, formaldehyde resin, or cyanoacrylate.
[0046] The present application does not particularly limit the average volume particle size of the above-mentioned inorganic particles. Those skilled in the art can select it according to actual needs, as long as the purpose of the present application can be achieved.
[0047] The present application has no particular limitation on the thickness of the insulating layer, as long as the purpose of the present application can be achieved. For example, the thickness of the insulating layer is 0.2 μm to 3 μm.
[0048] In some embodiments of the present application, the positive electrode active material includes at least one of lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium manganese oxide, lithium iron phosphate, or lithium iron manganese phosphate. The selection of the above-mentioned positive electrode active materials is conducive to achieving a higher capacity of the secondary battery.
[0049] The present application has no particular restrictions on the type of positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the positive electrode current collector may include aluminum foil, aluminum alloy foil, etc. In the present application, the positive electrode active material may also include non-metallic elements, for example, non-metallic elements include at least one of fluorine, phosphorus, boron, chlorine, silicon or sulfur, which can further improve the stability of the positive electrode active material. In the present application, there is no particular restriction on the thickness of the positive electrode current collector and the positive electrode active material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the positive electrode current collector is 5μm to 20μm, preferably 6μm to 18μm. The thickness of the positive electrode active material layer is 30μm to 120μm.
[0050] Optionally, the positive electrode active material layer may further include a positive electrode conductive agent and a positive electrode binder. There are no particular limitations on the types of the positive electrode conductive agent and the positive electrode binder in the positive electrode active material layer in this application, as long as the objectives of this application can be achieved. There are no particular limitations on the mass ratio of the positive electrode active material, the positive electrode conductive agent, and the positive electrode binder in the positive electrode active material layer in this application, and those skilled in the art can select according to actual needs, as long as the objectives of this application can be achieved. For example, the mass ratio of the positive electrode active material, the positive electrode nitrile group-containing additive, the positive electrode conductive agent, and the positive electrode binder in the positive electrode active material layer is (90.00 - 99.00):(0.001 - 1):(0.495 - 4.75):(0.495 - 4.75).
[0051] There are no particular limitations on the negative electrode sheet in this application, as long as the objectives of this application can be achieved. For example, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer. There are no particular limitations on the negative electrode current collector in this application, as long as the objectives of this application can be achieved. For example, the negative electrode current collector may include copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, etc. The negative electrode active material layer of this application contains a negative electrode active material. There are no particular limitations on the type of the negative electrode active material in this application, as long as the objectives of this application can be achieved. For example, the negative electrode active material may include natural graphite, artificial graphite, mesocarbon microbeads (MCMB), hard carbon, soft carbon, silicon, silicon-carbon composite, SiO x (0 < x < 2), Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel-structured lithium titanate Li4Ti5O 12 , Li-Al alloy, or at least one of metallic lithium. In this application, there are no particular limitations on the thickness of the negative electrode current collector and the negative electrode active material layer, as long as the objectives of this application can be achieved. For example, the thickness of the negative electrode current collector is 6 μm to 1 μm, and the thickness of the negative electrode active material layer is 30 μm to 130 μm. Optionally, the negative electrode active material layer may further include at least one of a negative electrode conductive agent, a thickener, and a negative electrode binder. There are no particular limitations on the types of the negative electrode conductive agent, the stabilizer, and the negative electrode binder in the negative electrode active material layer in this application, as long as the objectives of this application can be achieved. There are no particular limitations on the mass ratio of the negative electrode active material, the negative electrode conductive agent, the thickener, and the negative electrode binder in the negative electrode active material layer in this application, as long as the objectives of this application can be achieved. For example, the mass ratio of the negative electrode active material, the negative electrode conductive agent, the thickener, and the negative electrode binder in the negative electrode active material layer is (97 - 98):(0.5 - 1.5):(0.5 - 1.5):(1.0 - 1.9).
[0052] The electrolyte of the present application also includes lithium salts and non-aqueous solvents. The lithium salt may include at least one of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, Li2SiF6, lithium bis(oxalatoborate) (LiBOB) or lithium difluoroborate. The present application has no particular restrictions on non-aqueous solvents, as long as the purpose of the present application can be achieved, for example, it may include but is not limited to at least one of carbonate compounds, carboxylate compounds, ether compounds or other organic solvents. The above-mentioned carbonate compounds may include but are not limited to at least one of chain carbonate compounds, cyclic carbonate compounds or fluorocarbon compounds. The above-mentioned chain carbonate compounds may include but are not limited to at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC) or ethyl methyl carbonate (MEC). The cyclic carbonate may include but is not limited to at least one of ethylene carbonate (EC), propylene carbonate (also known as propylene carbonate, abbreviated as PC), butylene carbonate (BC) or vinyl ethylene carbonate (VEC). Fluorinated carbonate compounds may include but are not limited to at least one of fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate or trifluoromethylethylene carbonate. The carboxylate compounds may include but are not limited to at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanolactone, valerolactone or caprolactone. The above-mentioned ether compound may include but is not limited to at least one of dibutyl ether, tetraglyme, diglyme, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran. The above-mentioned other organic solvents may include but are not limited to at least one of dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate or trioctyl phosphate. The present application has no particular restrictions on the content of lithium salt and non-aqueous solvent in the electrolyte, as long as the purpose of the present application can be achieved.
[0053] The secondary battery of the present application further comprises a packaging bag, wherein the electrolyte and the electrode assembly are contained in the packaging bag. The present application has no particular limitation on the packaging bag, and can be any packaging bag known in the art, as long as it can achieve the purpose of the present application.
[0054] The present application does not particularly limit the type of secondary battery, which may include any device that undergoes an electrochemical reaction. For example, secondary batteries may include, but are not limited to: lithium metal secondary batteries, lithium ion secondary batteries (lithium ion batteries), sodium ion secondary batteries (sodium ion batteries), lithium polymer secondary batteries, and lithium ion polymer secondary batteries.
[0055] In a second aspect, the present application provides an electronic device comprising the secondary battery according to any one of the aforementioned embodiments. Therefore, the electronic device has good cycle performance.
[0056] The electronic device of the present application is not particularly limited and can be any electronic device known in the art. For example, the electronic device can include, but is not limited to, a laptop computer, a pen-type computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a headset, a video recorder, an LCD television, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, an automobile, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, a power tool, a flashlight, a camera, a large household battery, and a lithium-ion capacitor.
[0057] Example
[0058] Hereinafter, the embodiments of the present application will be described in more detail with reference to Examples and Comparative Examples. Various tests and evaluations were performed according to the following methods.
[0059] Test methods and equipment:
[0060] Test method for base film thickness D:
[0061] A scanning electron microscope (SEM) was used to measure the SEM image of the cross section of the diaphragm in each embodiment or comparative example, and the thickness of the base film was measured in the SEM image. Five points were randomly selected from each image, and the average value of the thickness measured at the five points was calculated as the thickness D of the base film.
[0062] Output voltage test method:
[0063] (1) The lithium-ion batteries of each embodiment and comparative example were first fully discharged. The discharge process was as follows: discharge at a constant current of 0.2C to 3.0V, let it stand for 30 minutes; discharge at a constant current of 0.2C to 3.0V (C is the working capacity of the lithium-ion battery);
[0064] (2) Charge the battery at a current of 0.05C for 20 hours and record the voltage V at that time, which is the output voltage.
[0065] Test method for the mass percentage x% of nitrile-based additives in electrolyte:
[0066] Cut open the top seal of the lithium-ion battery, place it upside down in a centrifuge tube, and use a centrifuge to centrifuge out the electrolyte; disassemble the lithium-ion battery to obtain the positive electrode sheet and weigh it, and weigh the mass of the positive electrode sheet M1 (g).
[0067] The electrolyte obtained by centrifugation is diluted step by step in a container with a constant volume V1 (mL) to different gradients with a concentration range of 0.1 mg / L to 10 mg / L (the ratio of two adjacent concentrations is high concentration: low concentration = V1:1). The test is performed using a gas chromatography-mass spectrometer to measure the concentration n1 mg / mL in the test sample. The content of the nitrile-based additive in the electrolyte can be calculated as x = n1 × V1 / M1.
[0068] Test method for the mass percentage of y% of nitrile-based additives in the positive electrode:
[0069] Disassemble the lithium-ion battery to obtain the positive electrode sheet and cut a 2 cm × 2 cm sample, where a is an integer. Weigh the sample mass M2 (g) and wash it three times with dimethyl carbonate (DMC) to remove free lithium salts on the surface and soluble components in the solid electrolyte interface (SEI) film. Place the sample in N-methylpyrrolidone and stir for 5 hours. Filter and collect the supernatant. Separate the supernatant by chromatography to obtain a pure phase dilute solution containing the nitrile-based positive electrode additive.
[0070] The above-mentioned pure phase positive electrode nitrile-containing additive dilute solution was diluted step by step in a container with a constant volume V2 (mL) to different gradients with a concentration range of 0.1 mg / L to 10 mg / L (the ratio of two adjacent concentrations is high concentration: low concentration = V1:1). The solution was tested using a gas chromatography-mass spectrometer to measure the concentration n2 mg / mL in the sample to be tested. The content of the nitrile-containing additive in the positive electrode y = n2 × V2 / M2 can be calculated.
[0071] Method for detecting the carbon-nitrogen atomic ratio m1:
[0072] The carbon-nitrogen atomic ratio m1 was detected using an inductively coupled plasma spectrometer (ICP).
[0073] Method for detecting the carbon-nitrogen atomic ratio m2:
[0074] The carbon (C) to nitrogen (N) molar ratio of the nitrile-containing polymer was determined to be m2 using a typical elemental analysis method.
[0075] Weight average molecular weight M w Detection method:
[0076] Laser light scattering was used to measure the weight average molecular weight M W .
[0077] Test method for cycle performance:
[0078] The lithium-ion batteries of the embodiments and comparative examples were placed in a 45°C constant temperature box and allowed to stand for 30 minutes to allow the lithium-ion batteries to reach a constant temperature. The lithium-ion batteries that reached a constant temperature were charged to 4.2V at a constant current of 1C at 45°C, then charged to 0.05C at a constant voltage of 4.2V, allowed to stand for 5 minutes, and then discharged to 3.0V at a constant current of 0.7C; this was one charge and discharge cycle. The capacity retention rate of the lithium-ion battery after 100 cycles of charging / discharging was calculated in this way. After every 50 cycles in the test, the lithium-ion battery was subjected to another low-rate charge and discharge cycle to correct the discharge condition of the lithium-ion battery. In the low-rate charge and discharge cycle, except for the discharge at a constant current of 0.2C, the other parameters were the same as those of the above-mentioned charge and discharge cycle process.
[0079] The capacity retention rate of a lithium-ion battery after cycling is calculated using the following formula: Capacity retention rate = discharge capacity at the 100th cycle / initial discharge capacity × 100%. The capacity retention rate of a lithium-ion battery is measured through three parallel experiments, and the average value of the three parallel experimental data is used as the capacity retention rate of the lithium-ion battery.
[0080] Test method for maximum cycle pressure difference:
[0081] Preparation of lithium-ion battery modules:
[0082] Take four lithium-ion batteries from each embodiment or comparative example and connect them in series to obtain a lithium-ion battery module.
[0083] During the cycle of the lithium-ion battery modules in the embodiments and comparative examples, the voltage difference (V1-V2) between the voltage V1 of the lithium-ion battery with the highest voltage and the voltage V2 of the lithium-ion battery with the lowest voltage at the end of charging is recorded as the maximum cycle voltage difference.
[0084] Example 1-1
[0085] <Preparation of positive electrode sheet>
[0086] The positive electrode active material lithium cobalt oxide, the conductive agent conductive carbon black (Super P), the positive electrode nitrile-containing additive polyacrylonitrile (m2=3, M w =300000), binder polyvinylidene fluoride (abbreviated as PVDF, weight average molecular weight of 800000 to 1200000) were mixed in a mass ratio of 94.43:2:1:2.57, N-methylpyrrolidone (NMP) was added as a solvent, and stirred in a vacuum mixer until the solid content was 70wt% and the system was uniform. The positive electrode slurry was mixed at 97.38g / m 2The coating was evenly applied to one surface of a 12μm-thick positive electrode current collector aluminum foil. The foil was then dried at 120°C for 1 hour to produce a single-sided positive electrode active material layer (110μm thick). The above steps were then repeated on the other surface of the foil to obtain a double-sided positive electrode active material layer. The resulting sheet was then cold-pressed, cut, and tab-welded to produce a 74mm x 867mm positive electrode sheet.
[0087] <Preparation of negative electrode sheet>
[0088] The negative electrode active material artificial graphite, the conductive agent Super P, the binder polyacrylic acid (weight average molecular weight of 5000000 to 14000000), and the thickener sodium carboxymethyl cellulose (weight average molecular weight of 10000000 to 15000000) are mixed in a mass ratio of 83.5:10:5:1.5, and then deionized water is added as a solvent. The mixture is stirred under the action of a vacuum mixer until the solid content is 75wt% and the system is uniform.
[0089] Polyacrylic acid (weight average molecular weight of 8,000,000) and conductive agent Super P were mixed in a mass ratio of 50:50, and then deionized water was added as a solvent. The mixture was stirred in a vacuum mixer until a solid content of 75 wt% and a uniform base coating slurry was obtained.
[0090] First, apply the primer slurry to one surface of a 12μm-thick copper foil for the negative electrode current collector and dry it at 120°C to obtain a single-sided primer-coated negative electrode sheet with a 30μm coating thickness. Repeat the above steps on the other surface of the copper foil to obtain a double-sided primer-coated negative electrode sheet. Next, apply the negative electrode slurry to one surface of the primer-coated copper foil and dry it at 120°C to obtain a single-sided primer-coated negative electrode sheet with a 130μm coating thickness. Repeat the above steps on the other surface of the primer-coated copper foil to obtain a double-sided primer-coated negative electrode sheet. This sheet is then cold-pressed, cut, and welded to the tabs to obtain a 76mm x 851mm negative electrode sheet ready for use.
[0091] <Preparation of Electrolyte>
[0092] Under a dry argon atmosphere, ethylene carbonate (EC), propylene carbonate (PC), and diethyl carbonate (DEC) were mixed in a mass ratio of 1:1:1 to form a base organic solvent. Lithium hexafluorophosphate (LiPF6) was then added to the base organic solvent, dissolved, and mixed thoroughly. The electrolyte, containing a nitrile-based additive, malononitrile, was then added to form an electrolyte. Based on the mass of the electrolyte, the mass percentage of LiPF6 was 12.5%, the mass percentage of malononitrile was x = 2.3%, and the remainder was the base organic solvent.
[0093] <Diaphragm>
[0094] A polyethylene-based film with a thickness of 4 μm (manufacturer: Zhuogao New Materials Technology Co., Ltd.) was used as the separator.
[0095] <Preparation of lithium-ion batteries>
[0096] The negative electrode sheet, separator, and positive electrode sheet prepared above are stacked and wound in sequence to form a wound electrode assembly. The electrode assembly is placed in an aluminum-plastic film packaging bag, dried, and then injected with electrolyte. The lithium-ion battery is produced through vacuum packaging, resting, formation, degassing, and trimming. The formation conditions are charging at a constant current of 0.02C to 3.3V, followed by charging at a constant current of 0.1C to 4.5V.
[0097] Example 1-2 to Example 1-14
[0098] Except for adjusting the relevant preparation parameters according to Table 1, the rest is the same as Example 1-1.
[0099] In the preparation of the positive electrode sheet, if the mass percentage of the positive electrode nitrile-containing additive changes, the mass percentage of the positive electrode active material will change accordingly, while the other components remain unchanged. The sum of the mass percentages of the positive electrode active material, conductive agent, positive electrode nitrile-containing additive, and binder is 100%.
[0100] In <Preparation of Electrolyte>, the mass percentage of the nitrile-based additive in the electrolyte changes, and the mass percentage of the basic organic solvent changes accordingly, while the other components remain unchanged. The sum of the mass percentages of the nitrile-based additive, the basic organic solvent and the lithium salt in the electrolyte is 100%.
[0101] Examples 1-15
[0102] Except that in <Preparation of Positive Electrode Plate>, zinc oxide-coated lithium cobalt oxide is selected as the positive electrode active material (the mass of zinc oxide is 1wt% of the positive electrode active material), and the output voltage of the secondary battery is adjusted to 4.5V, the rest is the same as Example 1-4.
[0103] Examples 1-16
[0104] Except that in <Preparation of Positive Electrode Sheet>, Mg, Al, and Ti-doped lithium cobalt oxide is selected as the positive electrode active material (the mass of Mg, Al, and Ti is 0.1wt% of the positive electrode active material), and the output voltage of the secondary battery is controlled to 4.56V, the rest is the same as Examples 1-4.
[0105] Examples 1-17
[0106] Except that in <Preparation of Positive Electrode Sheet>, Mg-doped Se-coated lithium cobalt oxide is selected as the positive electrode active material (the molar amount of Mg is 1 mol% of the positive electrode active material, and the mass of Se is 0.2 wt% of the positive electrode active material), and the output voltage of the secondary battery is controlled to 4.6 V, the rest is the same as Examples 1-4.
[0107] Example 1-18 to Example 1-26
[0108] Except for adjusting the relevant preparation parameters according to Table 1, the rest is the same as Example 1-1.
[0109] In the preparation of the positive electrode sheet, if the mass percentage of the positive electrode nitrile-containing additive changes, the mass percentage of the positive electrode active material will change accordingly, while the other components remain unchanged. The sum of the mass percentages of the positive electrode active material, conductive agent, positive electrode nitrile-containing additive, and binder is 100%.
[0110] In <Preparation of Electrolyte>, the mass percentage of the nitrile-based additive in the electrolyte changes, and the mass percentage of the basic organic solvent changes accordingly, while the other components remain unchanged. The sum of the mass percentages of the nitrile-based additive, the basic organic solvent and the lithium salt in the electrolyte is 100%.
[0111] Example 2-1 to Example 2-6
[0112] Except for adjusting the relevant preparation parameters according to Table 2, the rest is the same as Example 1-4.
[0113] Comparative Examples 1 to 7
[0114] Except for adjusting the relevant preparation parameters according to Table 1, the rest is the same as Example 1-1.
[0115] In the preparation of the positive electrode sheet, if the mass percentage of the positive electrode nitrile-containing additive changes, the mass percentage of the positive electrode active material will change accordingly, while the other components remain unchanged. The sum of the mass percentages of the positive electrode active material, conductive agent, positive electrode nitrile-containing additive, and binder is 100%.
[0116] In <Preparation of Electrolyte>, the mass percentage of the nitrile-based additive in the electrolyte changes, and the mass percentage of the basic organic solvent changes accordingly, while the other components remain unchanged. The sum of the mass percentages of the nitrile-based additive, the basic organic solvent and the lithium salt in the electrolyte is 100%.
[0117] The preparation parameters and performance parameters of each embodiment and comparative example are shown in Table 1 and Table 2.
[0118] Table 1
[0119] Note: “\” in Table 1 indicates no relevant preparation parameters.
[0120] It can be seen from Examples 1-1 to 1-26 and Comparative Examples 1 to 7 that when the output voltage and the base film thickness of the diaphragm in the secondary battery are within the scope of the present application, the secondary battery of the embodiment improves the output voltage, uses a diaphragm with a thin base film, introduces an electrolyte containing a nitrile-based additive and a positive electrode containing a nitrile-based additive, and regulates the mass percentage of the electrolyte containing the nitrile-based additive, the mass percentage of the positive electrode containing the nitrile-based additive, and the sum of the mass percentage of the electrolyte containing the nitrile-based additive and the positive electrode containing the nitrile-based additive within the scope of the present application. The secondary battery has a higher 45°C cycle capacity retention rate and a lower 45°C cycle maximum pressure difference, indicating that the self-discharge problem during the charge and discharge process of the secondary battery is improved, the consistency of the voltage and capacity between the secondary batteries in the secondary battery module is improved, the series pressure difference of the secondary battery module is smaller, the series pressure difference problem during the charge and discharge process of the secondary battery module is improved, and the cycle performance of the secondary battery under high pressure and high temperature is improved. However, when the secondary battery of the comparative example does not introduce a positive electrode nitrile-containing additive or an electrolyte nitrile-containing additive, or when at least one of x, y or z is not within the scope of the present application, the 45°C cycle capacity retention rate of the secondary battery is lower and the 45°C cycle maximum pressure difference is higher, indicating that the self-discharge problem during the charging and discharging process of the secondary battery is obvious, the consistency of voltage and capacity between each secondary battery in the secondary battery module is worse, and the series voltage difference of the secondary battery module is larger.
[0121] It can be seen from Examples 1-4, 1-15 to 1-17 that when the output voltage of the secondary battery of the present application is within the scope of the present application, it has a higher 45°C cycle capacity retention rate and a lower 45°C cycle maximum pressure difference, indicating that the self-discharge problem during the charging and discharging process of the secondary battery is improved, the consistency of voltage and capacity between each secondary battery in the secondary battery module is improved, the series pressure difference problem during the charging and discharging process of the secondary battery module is improved, and the secondary battery has good cycle performance under high pressure and high temperature.
[0122] The mass percentage y of the positive electrode nitrile-based additive meets the following requirements: 0.035D 2 -0.562D+2.253≤y≤0.027D 2 -0.482D+2.257, the self-discharge problem of the secondary battery during the charge and discharge process at high output voltage and high temperature can be further improved. From Examples 1-1 to 1-14, and 1-18 to 1-26, it can be seen that the mass percentage y of the positive electrode nitrile-containing additive satisfies: 0.035D 2 -0.562D+2.253≤y≤0.027D 2When -0.482D+2.257, the 45°C cycle capacity retention rate of the secondary battery is higher, and the 45°C cycle maximum pressure difference is lower, indicating that the self-discharge problem during the charging and discharging process of the secondary battery is improved, the consistency of voltage and capacity between each secondary battery in the secondary battery module is improved, the series voltage difference of the secondary battery module is smaller, the series voltage difference problem during the charging and discharging process of the secondary battery module is improved, and the cycle performance of the secondary battery under high pressure and high temperature is further improved.
[0123] Table 2
[0124] The type of nitrile-based additive in the electrolyte typically affects the cycling performance of secondary batteries. As can be seen from Examples 1-4, 2-1, and 2-2, secondary batteries using electrolytes containing nitrile-based additives within the scope of this application exhibit a high 45°C cycling capacity retention rate, and modules composed of such batteries exhibit a low 45°C cycling maximum pressure difference. This indicates that the self-discharge problem during the secondary battery charge and discharge process is improved, the consistency of voltage and capacity between the individual secondary batteries in the secondary battery module is improved, the series voltage difference problem during the charge and discharge process of the secondary battery module is improved, and the secondary battery has good cycling performance under high voltage and high temperature conditions.
[0125] The type of positive electrode nitrile-based additive generally affects the cycle performance of secondary batteries. As can be seen from Examples 1-4, 2-3, and 2-4, when the carbon-nitrogen atomic ratio of the positive electrode nitrile-based additive changes, the type of positive electrode nitrile-based additive changes accordingly. Secondary batteries using positive electrode nitrile-based additives within the scope of this application have a high 45°C cycle capacity retention rate, and the secondary battery modules composed of them have a low 45°C cycle maximum pressure difference, indicating that the self-discharge problem during the secondary battery charge and discharge process is improved, the consistency of voltage and capacity between the secondary batteries in the secondary battery module is improved, the series pressure difference problem during the charge and discharge process of the secondary battery module is improved, and the secondary battery has good cycle performance under high pressure and high temperature.
[0126] The weight-average molecular weight of the positive electrode nitrile-containing additive typically affects the cycling performance of secondary batteries. As can be seen from Examples 1-4, 2-5, and 2-6, secondary batteries using positive electrode nitrile-containing additives with a weight-average molecular weight within the range of this application exhibit a high 45°C cycling capacity retention rate, and secondary battery modules composed of such batteries exhibit a low 45°C cycling maximum pressure difference. This indicates that the self-discharge problem during the secondary battery charge and discharge process is improved, the consistency of voltage and capacity between the individual secondary batteries in the secondary battery module is improved, the series pressure difference problem during the charge and discharge process of the secondary battery module is improved, and the secondary battery has good cycling performance under high voltage and high temperature conditions.
[0127] It should be noted that, in this article, the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements that are inherent to such process, method, article or apparatus.
[0128] Each embodiment in this specification is described in a related manner. The same or similar parts between the embodiments can be referred to each other. Each embodiment focuses on the differences from other embodiments.
[0129] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.
Claims
1. A secondary battery, comprising an electrode assembly and an electrolyte, wherein the electrode assembly comprises a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator is disposed between the positive electrode sheet and the negative electrode sheet, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode active material, wherein the positive electrode active material comprises a transition metal element, wherein the transition metal element comprises at least one of Co, Ni, Mn, Fe or V; The diaphragm includes a base film, the thickness of the base film is D μm, 3≤D≤7; The secondary battery comprises an electrolyte containing a nitrile-based additive and a positive electrode containing a nitrile-based additive. Based on the mass of the electrolyte, the mass percentage of the nitrile-based additive in the electrolyte is x%, and based on the mass of the positive electrode active material layer, the mass percentage of the nitrile-based additive in the positive electrode is y%, x+y=z, 0.3≤z≤3.3 and 0<x≤2.3, 0<y≤1.
2. The secondary battery according to claim 1, wherein 1.4≤z≤3.3。 3. The secondary battery according to claim 1, wherein The electrolyte contains a nitrile-based additive having a carbon-nitrogen atom number ratio of m1, 1≤m1≤6, and the electrolyte contains a nitrile-based additive including at least one of malononitrile, succinonitrile, glutaronitrile, adiponitrile, heptane dinitrile, suberonitrile, decanonitrile, 3,3'-oxydipropionitrile, hexane-2-enedinitrile, anti-butene dinitrile, 2-pentene dinitrile, methyl glutaronitrile, 4-nitrile heptane dinitrile, (Z)-but-2-enedinitrile, 2,2,3,3-tetrafluorosuccinonitrile, ethylene glycol bis(propionitrile) ether, 1,3,5-pentanetricarbonitrile, 1,3,6-hexanetricarbonitrile, 1,2,6-hexanetricarbonitrile, 1,2,3-tris(2-nitrileoxy)propane or 1,1,3,3-propanetetracarbonitrile.
4. The secondary battery according to claim 1, wherein The positive electrode nitrile-containing additive is a nitrile-containing polymer, the carbon-nitrogen atom number ratio of the positive electrode nitrile-containing additive is m2,3≤m2≤5, and the weight average molecular weight of the positive electrode nitrile-containing additive is M w , 300≤M w ≤700000.
5. The secondary battery according to claim 4, wherein The positive electrode nitrile-containing additive includes at least one of polyacrylonitrile, polybutenenitrile or polyisobutenenitrile.
6. The secondary battery according to claim 1, wherein The output voltage of the secondary battery is greater than or equal to 4.48V and less than or equal to 4.6V.
7. The secondary battery according to claim 6, wherein The output voltage of the secondary battery is less than or equal to 4.56V.
8. The secondary battery according to claim 1, wherein 0.035D 2 -0.562D+2.253≤y≤0.027D 2 -0.482D+2.257。 9. The secondary battery according to claim 1, wherein The material of the base film includes polyolefin, and the polyolefin includes at least one of polyethylene or polypropylene.
10. The secondary battery according to claim 9, wherein The diaphragm further comprises an insulating layer disposed on the surface of the base film, wherein the insulating layer comprises inorganic particles and a binder; The inorganic particles include at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide or barium sulfate; The binder includes at least one of styrene-butadiene rubber, polyacrylic acid, polyvinyl alcohol, polyethylene glycol, polyacrylate, polyvinylidene fluoride, polyvinyl chloride, formaldehyde resin or cyanoacrylate.
11. The secondary battery according to claim 9, wherein The base film is a multi-layer film structure.
12. The secondary battery according to claim 1, wherein The positive electrode active material includes at least one of lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium manganese oxide, lithium iron phosphate or lithium iron manganese phosphate. 13 . An electronic device comprising the secondary battery according to claim 1 .
Citation Information
Patent Citations
Non-aqueous electrolyte and high-voltage lithium ion battery containing same
CN111640985A
Conductive agent, method for producing same, electrochemical device, and electronic device
CN113330609A
Positive electrode for secondary battery, method for manufacturing same, and lithium secondary battery comprising same
CN114788043A
Lithium battery and electric equipment
CN115275103A
Non-aqueous electrolyte for lithium secondary battery, and lithium secondary battery comprising same
WO2023027547A1
Cited By
Lithium ion secondary battery
CN119890408A
Lithium manganese iron phosphate positive electrode material and preparation method thereof, positive electrode plate and secondary battery
CN120784350A
Secondary battery and electronic device
WO2026178747A1