Composite floor containing fiber layer

By introducing a combination of fiber layer and bonding layer into the stone floor, the problems of high labor costs and poor impact resistance during transportation and installation of traditional stone flooring are solved, achieving lightweight, high impact resistance and simplified paving. The effect of craftsmanship.

WO2024198012A1PCT designated stage expired Publication Date: 2024-10-03NATURE NEW MATERIAL TECHNOLOGY (JIANGSU) CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/089606
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2023-04-20
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Traditional stone floors have high labor costs during transportation and installation, are prone to yellowing, alkali reversion, and have poor impact resistance. DIY decoration is inconvenient, and the traditional paving process is complex, time-consuming, and labor-intensive.

Method used

Composite floors containing fiber layers are used. Through the combination of stone layer, bonding layer and fiber layer, the thickness of the stone layer is reduced, the impact resistance and overall strength are increased, hot melt adhesive or thermosetting adhesive is used as the binder, carbon fiber or Fiberglass is used as fiber layer material, protective membrane and bonding layer for durability and ease of installation.

Benefits of technology

It significantly reduces floor weight and paving costs, improves impact resistance, avoids yellowing and alkali return on the stone surface, simplifies the paving process, facilitates DIY decoration, and reduces labor and time costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023089606_03102024_PF_FP_ABST
    Figure CN2023089606_03102024_PF_FP_ABST
Patent Text Reader

Abstract

A composite floor containing a fiber layer, comprising: a stone layer having a thickness ranging from 0.1 mm to 10 mm; an adhesive layer located below the stone layer; and a fiber layer located below the adhesive layer and having a thickness ranging from 0.01 mm to 2 mm. The composite floor, on the basis of the combination of the stone layer and the fiber layer, has better impact resistance than conventional stone floors while the thickness of a wall is greatly reduced, the mechanical properties of an overall composite floor structure are excellent, and the composite floor is light and easy to transport, has super strong impact resistance, and is less susceptible to cracking.
Need to check novelty before this filing date? Find Prior Art

Description

Composite flooring with fiber layer Technical Field

[0001] The present disclosure relates to the field of building materials, further to floor decoration and decorative materials, and further to a composite floor containing a fiber layer. Background Art

[0002] Flooring, serving as the surface layer of a building's floors or floors, is a widely used building material. Traditional flooring can include wooden flooring, which is categorized by structure into laminate flooring, solid wood composite flooring, bamboo flooring, cork flooring, and multi-layer solid wood composite flooring. These floors offer advantages such as aesthetics and temperature regulation. However, traditional flooring is complex to install (for example, solid wood flooring requires pre-installed subfloors), difficult to maintain, and prone to arching, warping, deformation, and noise when walked on. Flooring materials used for building floors or floors can also include stone or ceramic tiles. The typical installation process for these materials includes soaking in water, determining the joint width, applying mortar, laying, and grouting. There are many problems with using tiles or stones as decoration materials. Since the paving process involves applying materials such as mortar, the alkaline substances in these materials can easily penetrate the stone and affect its outer surface, causing yellowing and alkali reversion. Moreover, since stone or tiles are brittle materials, they can easily cause surface warping or cracking. Furthermore, since the stone itself is heavy and thick (usually the thickness of floor stone is more than 15mm), it takes a lot of time and economic costs to transport and assemble. In addition, similar to floor paving, the installation process of stone or tiles is relatively complicated, which is not suitable for the current DIY (Do-It-Yourself) decoration style. Using traditional paving methods will greatly increase the time of overall decoration.

[0003] Furthermore, when renovating a house, the previously laid flooring material is often too high. To replace the existing flooring, tiles, or stone, it is often necessary to break up the stone, tile, or wood flooring and the adhesive material underneath before re-installing the new flooring. Both removal and re-installation require a lot of manpower, making it very unfriendly to DIY renovations.

[0004] Chinese invention patent publication number CN115726536A discloses an adjustable prefabricated design structure for heavy-weight stone floors. It embeds multiple sliding strips in the ground base, and a sliding mechanism slides on two adjacent sliding strips. The sliding mechanism serves as a support for the stone slab. The stone slab only needs to be placed on the sliding mechanism for easy installation and adjustment, and there is no need to perform tongue and groove processing on the stone slab. However, this structure still cannot solve the labor costs incurred during the transportation and installation of the stone.

[0005] US invention patent publication number US11326357B2 discloses a floor element comprising a decorative layer containing a brittle material, a resin material penetrating the lower surface of the decorative layer, and a support layer below. However, the brittle material layer is still relatively thick, and the support layer material is a specific material that meets specific strength requirements (flexural modulus between 1.5 GPa and 3.5 GPa). There is no mention of its ability to be combined with thinner stone to solve the problem of stone cracking. Summary of the Invention

[0006] To solve the above problems, the present disclosure provides a composite flooring comprising a fiber layer, so as to at least partially solve the above technical problems.

[0007] According to the technical solution of the present disclosure, a composite floor containing a fiber layer is provided, comprising: a stone layer with a thickness ranging from 0.1 mm to 10 mm; a bonding layer located below the stone layer; and a fiber layer located below the bonding layer with a thickness ranging from 0.01 mm to 2 mm.

[0008] In a further embodiment, the thickness of the stone layer is greater than 0.5 mm and less than 8 mm.

[0009] In a further embodiment, the thickness of the stone layer is greater than 1 mm and less than 4 mm.

[0010] In a further embodiment, the material of the stone layer includes at least one of the following: limestone, granite, and marble.

[0011] In a further embodiment, the adhesive layer material includes at least one of the following: a hot melt adhesive and a thermosetting adhesive.

[0012] In a further embodiment, the bonding layer covers an area ratio of greater than 95% of the stone layer.

[0013] In a further embodiment, the thickness of the bonding layer is between 0.1 mm and 1 mm.

[0014] In a further embodiment, the fiber layer material includes chemical fibers, and the chemical fibers include at least one of the following: aramid, polyester, nylon, acrylic, polypropylene, vinylon, and chloroprene.

[0015] In a further embodiment, the fiber layer material comprises at least one of the following: carbon fibers and glass fibers.

[0016] In a further embodiment, the elastic modulus of the material of the fiber layer is between 5 GPa and 500 GPa.

[0017] In a further embodiment, the thickness of the fiber layer is between 0.2 mm and 0.5 mm.

[0018] In a further embodiment, the composite floor further comprises: a protective film covering the stone layer, wherein the protective film is attached to the stone layer and is made of a transparent material.

[0019] In a further embodiment, the material of the protective film includes at least one of the following materials: PU, TPU or PVC.

[0020] In a further embodiment, the composite floor further includes: a bonding layer, located below the fiber layer, having a sticky material on the side close to the fiber layer for fixing the connection with the fiber layer, and a silicone film on the side away from the fiber layer, wherein the silicone film is configured to adhere to the sticky material and can be torn apart by external force.

[0021] In a further embodiment, the composite flooring has an area density of between 3 kg / m 2 Up to 30kg / m 2 between.

[0022] In a further embodiment, the surface of the stone layer of the composite floor is impacted by a 1 kg stainless steel ball in free fall from a height of 1 meter without any cracking of the surface.

[0023] In a further embodiment, the stone layer of the composite flooring has a chamfered structure.

[0024] In a further embodiment, the surface of the stone layer has at least one of the following processed structures: a grooved structure, a mirror or smooth surface structure, a matte surface structure, a lychee surface structure, a leather surface structure, a washed surface structure, and an antique surface structure.

[0025] In a further embodiment, the edge of the fiber layer comprises a snap-fit ​​structure configured to securely connect adjacent composite floor panels by snap-fitting.

[0026] In a further embodiment, there are multiple composite floor panels, and the composite floor panels are fixedly connected to each other through the snap-fit ​​structure of the fiber layer.

[0027] The composite flooring disclosed herein, through the combination of stone and fiber layers, has superior impact resistance compared to traditional stone floors, even under walls with significantly reduced thickness. The overall composite flooring structure exhibits excellent mechanical properties, is lightweight, and is easy to transport. It also possesses superior impact resistance and is not prone to cracking.

[0028] The composite floor disclosed in the present invention can cure the yellowing and alkali reversion problems of natural stone caused by the bottom layer by providing an adhesive layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0030] FIG1 is a schematic cross-sectional view of a composite flooring including a fiber layer according to an embodiment of the present disclosure.

[0031] FIG. 2 is a perspective schematic diagram of the composite flooring including the fiber layer according to the embodiment shown in FIG. 1 .

[0032] FIG3 is a cross-sectional schematic diagram and a structural schematic diagram of a composite flooring including a fiber layer according to another embodiment of the present disclosure.

[0033] FIG. 4 is a perspective schematic diagram of the composite flooring including the fiber layer according to the embodiment shown in FIG. 3 .

[0034] FIG5 is a cross-sectional schematic diagram and a structural schematic diagram of a composite flooring including a fiber layer according to another embodiment of the present disclosure.

[0035] FIG6 is a schematic cross-sectional view of a composite flooring including a fiber layer according to an embodiment of the present disclosure.

[0036] FIG. 7 is a schematic diagram of a composite floor assembly structure including multiple fiber-containing layers shown in FIG. 6 according to an embodiment of the present disclosure.

[0037] FIG8 is a flow chart of a method for preparing a composite flooring including a fiber layer according to an embodiment of the present disclosure.

[0038] FIG9 is a flow chart of a method for preparing a composite flooring including a fiber layer according to another embodiment of the present disclosure. DETAILED DESCRIPTION

[0039] To facilitate understanding of the principles and features of the various embodiments of the present disclosure, various illustrative embodiments will be explained below. Although exemplary embodiments of the present disclosure have been explained in detail, it should be understood that other embodiments are contemplated. Therefore, it is not intended that the scope of the present disclosure be limited to the details of the construction and arrangement of the components described in the following description or examples. The present disclosure is capable of other embodiments and can be practiced or implemented in various ways. In addition, when describing exemplary embodiments, specific terms will be used for clarity.

[0040] In this disclosure, the term "and / or" may be used. As used in this disclosure, the term "and / or" means one or the other or both (for example, A and / or B means A or B or both A and B).

[0041] In addition, when describing exemplary embodiments, terminology will be used for the sake of clarity. Each term should be considered in its broadest sense as understood by those skilled in the art and includes all theoretical equivalents that operate in a similar manner to achieve similar purposes. It should be understood that the embodiments of the disclosed technical solutions can be implemented without these specific details. In some cases, methods, structures, and terminology in the prior art are not shown in detail in order to focus on the inventive content of the present disclosure.

[0042] In this disclosure, terms such as "one embodiment," "an embodiment," and "some embodiments" indicate that the solution described in the corresponding embodiment may include specific features, method steps, parameters, structures, or connections, but not every embodiment necessarily includes the specific features, method steps, parameters, or connections. Furthermore, repeated use of "an embodiment" does not necessarily refer to the same embodiment, although that possibility exists.

[0043] Throughout this disclosure, the term "approximately" or "approximately" or "substantially" is used to describe a particular value and / or values ​​approximately similar to that particular value. When such a range is used, the corresponding exemplary embodiments include corresponding ranges from one particular value and / or to another particular value. Additionally, "about" means within an acceptable error range for the particular value as determined by one skilled in the art. This will depend in part on how the particular value was measured or determined; i.e., values ​​within the error range of the measurement system are considered to be within the meaning of "about."

[0044] In the present disclosure, the term "comprises" or "includes" or "includes" means that at least the corresponding compound, element, particle or method step is present in the composition, compound, material structure or component, or method step, but does not exclude the presence of other compounds, elements, particles, or method steps.

[0045] In the present disclosure, the terms “above” and “below” indicate that one structural layer is located above or below another structural layer, and the structural layers may be in direct contact or indirect contact.

[0046] In the present disclosure, the term "fiber" is a general term for thin substances whose length is more than a thousand times greater than their diameter and which have certain flexibility and strength.

[0047] In this disclosure, it is to be understood that reference to one or more method steps does not exclude the presence of additional method steps or intermediate method steps between the explicitly identified steps. Similarly, it is to be understood that reference to one or more material components in a composition does not exclude the presence of other explicitly identified components.

[0048] In the present disclosure, any dimensions listed in the exemplary drawings are for illustrative purposes only and are not intended to limit the present disclosure. Other dimensions and ratios are considered and expected to be within the scope of the present disclosure.

[0049] The stone flooring in the existing technology is usually thicker than 15mm, and the overall thickness and weight are both large. As mentioned above, the conventional laying method requires a lot of manpower and time costs. In addition, during the use of this traditional stone flooring, there are problems such as yellowing, alkali reversion, poor impact resistance and easy cracking.

[0050] The disclosed embodiment provides a composite floor containing a fiber layer, which includes a stone layer, an adhesive layer, and a fiber layer, wherein the thickness of the stone layer is significantly thinner than that of the stone layer in the prior art, while reducing the overall weight of the floor (reducing the weight by, for example, more than 50%, or even more than 85%), thereby reducing the cost of transportation and laying. By compounding the fiber layer with the stone layer, the characteristics of the fiber material can make up for the shortcomings of the stone material itself, while reducing its own weight and still improving the impact resistance of the composite floor. The stone layer and the fiber layer are integrated into a structure through the adhesive layer, thereby improving the overall strength. Moreover, due to the barrier of the adhesive layer, the yellowing and alkali reversion phenomena on the stone surface are avoided.

[0051] Figure 1 is a schematic cross-sectional view of a composite flooring including a fiber layer according to an embodiment of the present disclosure. The composite flooring shown in Figures 1 and 2 includes an upper stone layer 1, a middle adhesive layer 2, and a lower fiber layer 3. Those skilled in the art will appreciate that the figures are merely schematic, and that the layer structure of an actual technical solution may include various additions or variations, such as including additional layers between layers.

[0052] The upper stone layer 1 mainly serves to provide surface decoration and strength support. The stone layer 1 will be described in detail below.

[0053] In some embodiments, the thickness of the stone layer 1 ranges from 0.1 mm to 10 mm, which is significantly lower than that of traditional stone floors. This significantly reduces the overall weight and thickness of the floor, facilitating renovations and allowing users to perform DIY paving. If the stone layer is less than 0.1 mm thick, processing costs are high. Furthermore, if the stone layer is too thin, its strength cannot be guaranteed and cracking is likely to occur. If the stone layer is greater than 10 mm thick, transportation and installation costs for the corresponding thickness increase significantly, and the overall floor cannot achieve the desired lightweight and impact-resistant properties. Alternatively, the stone layer 1 can be greater than 0.5 mm and less than 8 mm thick. Stone within this thickness range can meet the conventional mechanical requirements for floor paving, i.e., meeting certain impact resistance and strength requirements while minimizing weight. Furthermore, the stone layer 1 can be greater than 1 mm and less than 4 mm thick. Stone within this thickness range can also have a certain bending radius, suitable for paving curved surfaces. Because the stone layer thickness is less than that of conventional stone, the cutting speed needs to be reduced during cutting to prevent damage to the stone layer 2.

[0054] In some embodiments, the material of the stone layer 1 is natural stone and / or artificial stone. The optional material of the stone layer 1 is natural stone. The natural stone includes but is not limited to: sandstone, granite, limestone, slate, quartzite and marble. Preferably, the natural stone includes limestone, granite, marble, and these types of natural stone are suitable for use as building facing stones. Further preferably, the natural stone includes limestone, which is a type of limestone. The advantages of limestone are sound insulation, heat insulation, moisture absorption, low thermal conductivity, simple texture, high touch comfort, and zero radiation. Optionally, the material of the stone layer 1 can also be artificial stone. The typical preparation method of the artificial stone is to use unsaturated polyester resin as a binder, with natural marble or calcite, dolomite, silica sand, glass powder and other inorganic powders, as well as an appropriate amount of flame retardant, color, etc., and then form and solidify it by mixing the ingredients, porcelain casting, vibration compression, extrusion and other methods.

[0055] In some embodiments, a common porosity can be selected for the stone layer 1. Since the barrier of the adhesive layer can reduce yellowing and alkali reversion, the selection of materials with various porosities for the stone layer 1 can avoid the above-mentioned phenomena of composite materials.

[0056] In some embodiments, the stone layer 1 units in the composite flooring units may be shaped in various shapes known in the art, but the present disclosure is not limited thereto, including but not limited to hexagons, rhombuses, squares, and rectangles. Optionally, the stone layers in the composite flooring units may be sized in various shapes and sizes that meet the requirements of the corresponding region or country, but the present disclosure is not limited thereto. Typical sizes may be 305mm×305mm, 305mm×610mm, 610mm×610mm, or 610mm×915mm. It should be noted that the above sizes are for illustrative purposes only, and actual sizes may be selected based on the standards of the relevant country or region.

[0057] In some embodiments, the surface of the stone layer 1 in the composite floor unit has a processed structure, including but not limited to a grooved structure, a mirror / smooth surface structure, a matte surface structure, a lychee surface structure, a leather surface structure, a washed surface structure, and an antique surface structure, to improve the wear resistance and aesthetics of the composite floor.

[0058] In some embodiments, the composite flooring may further include a protective film covering the stone layer 1. Figure 3 is a cross-sectional schematic diagram of a composite flooring with a fiber layer according to another embodiment of the present disclosure. Figure 4 is a perspective schematic diagram of the composite flooring with a fiber layer according to the embodiment shown in Figure 3. As shown in Figures 3 and 4, the composite flooring also has a protective film 4 above the stone layer 1. This protective film is affixed to the outer surface of the stone layer 1 to protect it from accidental scratches and bumps during transportation and installation. After the decoration is completed, the protective film can be removed by external force. Optionally, the material of the protective film 4 includes, but is not limited to, PVC (polyurethane), PU (polyurethane), or TPU (thermoplastic polyurethane elastomer). Preferably, the protective film 4 is PU. This type of material has the advantage of having a certain tensile strength, which allows for better adhesion and protection of the stone layer it covers. Furthermore, as shown in Figure 3, the protective film may optionally be printed with a specific pattern, trademark, company name, or logo.

[0059] The bonding layer 2 in the composite flooring mainly functions to fix the stone layer 1 and the fiber layer 3 together and to prevent alkaline substances and the like from invading the stone layer 1. The bonding layer will be described in detail below.

[0060] In some embodiments, the bonding layer 2 comprises an organic binder, which is an adhesive that utilizes glue primarily composed of organic matter for bonding. Optionally, the organic binder comprises a hot melt adhesive or a thermosetting adhesive (such as epoxy resin). These types of organic binders are capable of blocking alkaline substances and effectively bonding the stone layer 1 to the fiber layer 3. Preferably, the organic binder is an alkali-resistant adhesive, which is resistant to corrosion by alkaline media. Examples of alkali-resistant adhesives include, but are not limited to, those based on furan resin, epoxy resin, chlorosulfonated polyethylene rubber, vinyl resin, unsaturated polyester resin, polymer cement mortar, pressure-sensitive adhesive, acrylic resin, vinyl acetate resin, polyurethane, and polyurea resin. Furthermore, the organic binder comprises epoxy resin, polyurethane, and pressure-sensitive adhesive, primarily for cost and bonding considerations. Alkali-resistant adhesives generally include resin, plasticizer, filler, cement, flame retardant, and curing agent. Hot pressing is a typical process for bonding the stone layer 1 and fiber layer 3 via the bonding layer 2.

[0061] In some embodiments, the bonding layer 2 should fully cover the stone layer 1 to provide a good barrier effect. Optionally, the bonding layer 2 covers more than 95% of the bottom surface of the stone layer 1; more preferably, the bonding layer 2 covers more than 99% of the bottom surface of the stone layer.

[0062] In some embodiments, the thickness of the adhesive layer 2 is between 0.1 mm and 1 mm, preferably between 0.3 mm and 0.6 mm. A certain thickness of the adhesive layer 2 can provide better bonding and barrier effects. In addition, considering cost and other factors, the thickness of the adhesive layer 2 should be kept within a certain range.

[0063] The fiber layer 3 in the composite material, comprising fiber material, primarily serves to compensate for the inherent shortcomings of stone (poor impact resistance and heavy weight). Furthermore, it reduces the thickness of the stone layer while maintaining the overall strength of the composite floor, thereby improving the composite floor's impact resistance. The fiber layer is described in detail below.

[0064] In some embodiments, the material of the fiber layer 3 includes natural fibers and chemical fibers. Natural fibers are fibers that exist in nature and can be directly obtained, including plant fibers, animal fibers, and mineral fibers. Chemical fibers include artificial fibers, synthetic fibers, and inorganic fibers.

[0065] In some embodiments, man-made fibers include but are not limited to viscose fibers and acetate fibers. In some embodiments, synthetic fibers include but are not limited to aramid, polyester, nylon, acrylic, polypropylene, vinylon, and chloroprene. The basic component of polyester is polyethylene terephthalate, with the molecular formula [-OC--COOCH2CH2O-] n, hence the name polyester fiber; nylon is also known as nylon. One type is polyhexamethylene adipate, obtained by the polycondensation of hexamethylenediamine and adipic acid. Its long-chain molecule has the chemical formula: H—[HN(CH2)6NHCO(CH2)4CO]—OH. Another type is obtained by the polycondensation or ring-opening polymerization of caprolactam. Its long-chain molecule has the chemical formula: H—[NH(CH2)5CO]—OH. Among them, acrylic fiber, also known as polyacrylonitrile fiber, has the structural formula: [-CH2-CHCN-] n ; Among them, the structural formula of polypropylene is: [-CH2-CH(CH3)-] n, Polypropylene is a synthetic fiber made from propylene, a byproduct of petroleum refining, and is also known as polypropylene fiber. Vinylon is the trade name for polyvinyl acetal fiber, also known as vinylon. Chlorinated fiber is a synthetic fiber made from polyvinyl chloride or its copolymers. Preferably, the fiber material is selected from at least one of aramid, polyester, nylon, acrylic, polypropylene, vinylon, and chloroinated fiber. This type of fiber meets environmental standards and has a high initial modulus. Further preferably, the fiber material is selected from aramid, which has a relatively high initial modulus.

[0066] In some embodiments, the fiber layer 3 is made of inorganic fibers. Inorganic fibers are made from natural inorganic materials or carbon-containing polymer fibers, and are produced by artificial spinning or direct carbonization. Inorganic fibers include glass fibers, metal fibers, and carbon fibers.

[0067] In some embodiments, the material of the fiber layer 3 is preferably a 5GPa-500GPa elastic material, preferably a 50GPa-500GPa elastic material. Optional elastic materials include glass fiber, carbon fiber or aramid, and aramid is further preferred. The elastic modulus of the relevant materials is large, which can improve the mechanical properties of the overall composite material.

[0068] In some embodiments, the fiber layer 3 has a specific breaking strength to ensure that the stone layer does not crack when subjected to external impact. The corresponding breaking strength is measured as follows: under specified conditions, the sample is stretched using a tensiometer until it breaks, and the breaking strength and elongation values ​​are obtained. The breaking strength is calculated from the breaking strength and linear density. In some embodiments, the thermal expansion coefficient of the fiber layer 3 is preferably matched with that of the stone layer, and the thermal expansion coefficient of the stone is substantially 10 -6 In this case, to better match the thermal expansion coefficient of the stone, at least one of the following fibers is preferred: synthetic fibers (including aramid, polyester, acrylic, polypropylene, vinylon, and chloroprene), glass fiber, and carbon fiber. In some embodiments, when selecting the fiber layer material, its fire resistance, alkali resistance, acid resistance, and water resistance should also be considered to further improve the overall performance of the composite board. Optional materials include glass fiber, carbon fiber, and aramid.

[0069] In some embodiments, the thickness of the fiber layer 3 is between 0.01 mm and 2 mm. A fiber layer 3 thickness exceeding 2 mm will affect the overall thickness of the composite sheet. A fiber layer thickness below 0.01 mm will not guarantee overall bending strength and will not prevent cracking. More preferably, the fiber layer thickness is between 0.2 mm and 0.5 mm. The fiber layer 3 may be in the form of a fiber cloth or a fiber mesh.

[0070] In some embodiments, the composite floor further includes a bonding layer 5. FIG5 is a cross-sectional schematic structural diagram of a composite floor containing a fiber layer provided according to another embodiment of the present disclosure. As shown in FIG5 , the bonding layer 5 is located below the fiber layer 3, and the side thereof close to the fiber layer 3 has a sticky material to be fixedly connected to the fiber layer, and the side away from the fiber layer 3 includes a silicone film, which is configured to adhere to the sticky material and can be torn apart by an external force. During actual paving, the silicone film is torn apart by an external force so that the sticky material can be directly brought into contact with the ground, thereby saving the process of pre-brushing a waterproof adhesive on the ground, and the sticky material can also further block the alkaline components from invading the stone layer 1.

[0071] In some embodiments, the edge of the fiber layer 3 includes a snap-fit ​​structure. FIG6 is a schematic cross-sectional view of a composite flooring including a fiber layer according to an embodiment of the present disclosure. As shown in FIG6 , the snap-fit ​​structure 31 is configured to securely connect adjacent composite floorings by snapping. FIG7 is a schematic diagram of a composite flooring assembly structure including multiple fiber-containing layers as shown in FIG6 , according to an embodiment of the present disclosure. Combined with FIG6 and FIG7 , the corresponding snap-fit ​​structure 31 facilitates rapid splicing of composite floorings, saving overall installation time.

[0072] In some embodiments, the composite board includes a chamfered structure. In the DIY process, the crystallization process may not be included, and there may be unevenness between the panels. To hedge against the above situation during the paving process, at least the stone layer of the composite board includes a chamfered structure. In addition, the chamfered structure can also reduce the edge collapse during transportation and paving. Optionally, the chamfered edge is a 45-degree bevel, a chamfer with a radius, a 1 / 4 fillet, or a 1 / 2 fillet.

[0073] In some embodiments, the surface density of the composite board is between 3 kg / m 2 and 30kg / m 2 The surface density of the composite board is significantly lower than that of traditional stone slabs, which can significantly reduce weight, reduce costs, save stone, and improve paving efficiency. Preferably, the surface density of the composite board is between 3kg / m 2 and 15kg / m 2 The surface density within this range is smaller, and the corresponding strength can be guaranteed to meet better collision requirements.

[0074] In the disclosed embodiment, the composite floor comprising the stone layer 1, the adhesive layer 2 and the fiber layer 3 has many advantages. First, it has excellent physical properties. KN panels offer high resistance to heavy installation, with impact resistance far exceeding the 10J impact requirement specified by the standard. This performance ensures they resist cracking and breakage during production, handling, installation, and use, addressing a key issue with natural stone. Ultra-thin panels (with a stone layer thickness of 1-3mm) can be bent and laid on curved surfaces, exhibiting slight deformation. Designers can utilize this property in curved paving designs, improving efficiency, reducing costs, and conserving stone. They can also address persistent issues such as yellowing, alkali reversion, and cracking caused by the underlying substrate. In some implementations, the three-layer structure of a self-leveling hard base, a waterproof layer, a thin-film process, and the panels significantly reduces the moisture and alkaline foci that contribute to these issues. This multi-layered waterproof barrier effectively blocks moisture and alkaline erosion, effectively addressing the two major issues of yellowing and alkali reversion that plague natural stone. Furthermore, the hard self-leveling material effectively reduces hollowing in the base layer and alleviates the persistent cracking problem of natural stone. Furthermore, it offers a lightweighting effect. The weight of the panels in this solution is about 3kg-15kg per square meter, and the transportation and secondary handling costs will be greatly reduced. The effect of light weight is that it can reduce the workload of paving personnel and improve work efficiency. At the same time, the light weight also allows paving personnel to easily adjust the position of the panels to ensure accurate paving effects. Third, it is healthy and environmentally friendly. The composite panels disclosed in this invention can more effectively realize resource utilization, increase the utilization rate of mineral resources such as natural stone by 4-8 times, and are more low-carbon and environmentally friendly. Moreover, the composite panels can be produced and transported more energy-efficiently, reducing energy consumption in the production and transportation process by 80%. The composite panels bring a more environmentally friendly production process, with zero emissions in the production process, zero wastewater, zero waste gas generation, and recyclable solid waste. In addition, the composite panels create a healthier use environment to solve the stubborn problem of stone cracking, without space for mold growth, and create a healthier living environment.

[0075] The materials of each layer of the composite board are preferably green materials and can be used with confidence. Fourth, the safety performance is improved. Due to the light material, it is very likely to avoid industrial accidents. During paving, it can effectively avoid industrial accidents such as crushing and smashing. It can also effectively solve the safety hazards of dry hanging stone on the wall from breaking and falling.

[0076] Fifth, cost advantages. Based on the thickness and specific materials of each layer, labor, transportation, and handling costs can be optimized, reducing overall costs by over 30%. Sixth, the paving process is simplified. A new paving process adapted to this layer structure has emerged, resulting in a new and revolutionary natural stone paving process that is healthier, more environmentally friendly, simpler, more efficient, and has a longer lifespan.

[0077] In order to further illustrate the specific details of the present disclosure, the present disclosure will be further illustrated below through specific examples and comparative examples.

[0078] Example 1:

[0079] Preparation of stone layer: marble material is used to prepare the stone layer. The marble is cut by cutting. The thickness of the stone layer after cutting is 2 mm. The length of the stone layer is 900 mm and the width is 600 mm. Preparation of fiber layer: polyester material is used to prepare the fiber layer. The fiber layer is processed into a thickness of 0.1 mm and the size is consistent with the stone layer. Preparation of composite board: the stone layer and the fiber layer are bonded and pressed together by hot melt adhesive. The thickness of the bonding layer is measured to be 0.2 mm.

[0080] (1) Test weight: The prepared composite board was tested and the weight of the whole composite board was measured. The measured weight of the composite board was 3.79 kg, and the surface density of the composite floor was calculated to be 7.02 kg / m 2 .

[0081] (2) Test the alkali reversion performance: The test method includes: a. Preparation of alkaline solution (saturated calcium hydroxide): At (23±2)℃, add 1.2g calcium hydroxide to 1000mL distilled water to prepare alkaline solution, and stir it thoroughly. The pH value of the solution can reach 12~13, which is approximately equal to the pH value of cement during solidification.

[0082] b. Pour the alkaline solution into a sealable plastic container. Place small stones at the same height as the liquid level in the liquid, ensuring that the total area of ​​the stones is no more than 10% of the liquid level. Select three plates prepared in the above steps and polish the surface to a reflectivity greater than 60% at a 60-degree angle. Seal the edges of the sample with a mixture of paraffin wax and rosin (mass ratio of 1:1) and place them on the small stones, ensuring that the lower surface of the sample remains in contact with the liquid surface for the specified time.

[0083] c. Take out the sample every 24 hours and observe the surface changes by reflection.

[0084] d. Measurement time: 90 days.

[0085] Measurement results: There was no loss of gloss or change in the three composite panels during the measurement time.

[0086] (3) Test the impact resistance.

[0087] Determination method: a. Select 3 composite panels, cut them into samples of size 300mm×300mm, and lay them on the ground with a flatness deviation of no more than 2mm.

[0088] b. Use a 1 kg stainless steel ball to fall freely from a height of 1 meter to impact the sample and observe the changes in the sample.

[0089] Measurement results: There was no change on the surface of the stone layer of the three composite panels.

[0090] Example 2:

[0091] Preparation of stone layer: lime stone material is used to prepare the stone layer, and the lime stone is cut by cutting. The thickness of the stone layer after cutting is 5 mm, the length of the stone layer is 900 mm, and the width of the stone layer is 900 mm. Preparation of fiber layer: aramid material is used to prepare the fiber layer, and the fiber layer is processed into a thickness of 0.5 mm and the size is consistent with that of the stone layer. Preparation of composite board: the stone layer and the fiber layer are bonded and pressed together by epoxy resin, and the thickness of the bonding layer is measured to be 0.3 mm.

[0092] (1) Test weight: The prepared composite board was tested and the weight of the whole composite board was measured. The measured weight of the composite board was 13.06 kg. The surface density of the composite floor was calculated to be 16.12 kg / m 2 .

[0093] (2) Test the alkali reversion performance: The test method includes: a. Preparation of alkaline solution (saturated calcium hydroxide): At (23±2)℃, add 1.2g calcium hydroxide to 1000mL distilled water to prepare alkaline solution, and stir it thoroughly. The pH value of the solution can reach 12~13, which is approximately equal to the pH value of cement during solidification.

[0094] b. Pour the alkaline solution into a sealable plastic container. Place small stones at the same height as the liquid level in the liquid, ensuring that the total area of ​​the stones is no more than 10% of the liquid level. Select three plates prepared in the above steps and polish the surface to a reflectivity greater than 60% at a 60-degree angle. Seal the edges of the sample with a mixture of paraffin wax and rosin (mass ratio of 1:1) and place them on the small stones, ensuring that the lower surface of the sample remains in contact with the liquid surface for the specified time.

[0095] c. Take out the sample every 24 hours and observe the surface changes by reflection.

[0096] d. Measurement time: 90 days.

[0097] Measurement results: There was no loss of gloss or change in the three composite panels during the measurement time.

[0098] (3) Test the impact resistance.

[0099] Determination method: a. Select 3 composite panels, cut them into samples of size 300mm×300mm, and lay them on the ground with a flatness deviation of no more than 2mm.

[0100] b. Use a 1 kg stainless steel ball to fall freely from a height of 1 meter to impact the sample and observe the changes in the sample.

[0101] Measurement results: There was no change on the surface of the stone layer of two composite panels, and one panel had a slight pit on its surface.

[0102] Comparative Example 1:

[0103] A marble slab with a thickness of 20 mm and a size of 900 mm × 600 mm was prepared.

[0104] (1) Test weight: The prepared marble stone was tested and its weight was measured. The measured weight was 30.24 kg and the surface density was 56 kg / m 2 .

[0105] (2) Test the alkali reversion performance: the test conditions are the same as those in Example 1.

[0106] Measurement results: During the experimental period, the three marble stones showed obvious gloss loss within 24 hours, and visible white spots appeared on the surface within 48 hours. In subsequent observations, the area of ​​the white spots became larger and thicker.

[0107] (3) Test the impact resistance: the test conditions are the same as those in Example 1.

[0108] Measurement results: All three marble slabs were broken.

[0109] The above test results are summarized in Table 1 below:

[0110] Table 1

[0111]

[0112] It can be seen from the results in the above table that, compared with the stone floor in the prior art, the composite board of the embodiment of the present disclosure is lighter in weight, thinner in thickness, and has higher alkali resistance and impact resistance.

[0113] The typical installation process of the above-mentioned composite floor can include two major types, one type is renovation based on existing decoration, and the other type is new house decoration.

[0114] FIG8 is a flow chart of a method for preparing a composite flooring containing a fiber layer according to an embodiment of the present disclosure. This flow chart corresponds to the situation of a newly renovated house. Since the new house has not been renovated and the ground is sloped or uneven, it is necessary to pre-apply step S100 to the ground: a ground leveling process, typically including cement mortar ground leveling or self-leveling cement leveling. Subsequently, an optional process step S120 can be further implemented: applying waterproof, weather-resistant, and environmentally friendly glue. In some embodiments, a bonding layer is not attached under the fiber layer 3. Therefore, it is necessary to pre-apply a layer of weather-resistant, environmentally friendly glue to the ground. It is foreseeable that when a bonding layer is already attached under the fiber layer 3, step S120 can be omitted. After step S120, step S140: laying the composite flooring can be implemented, that is, the composite flooring is adhered to the ground in an orderly manner to form an integrated structure. Further optionally, after step S140, the step of crystallizing the composite flooring can also be included. A typical crystallization process involves: thoroughly cleaning the marble surface with a floor scrubber; mixing crystallization powder with purified water into a paste and applying it to an abrasive pad; grinding with a floor scrubber under a certain load; once the surface of the marble has formed a high-gloss crystal surface, removing any remaining paste with a water aspirator; rinsing the surface with water and drying; and finally polishing the surface with a polishing pad until it is completely dry and glossy. In some embodiments, such as laminate flooring with a protective film, this crystallization process can be omitted.

[0115] Figure 9 is a flow chart of a method for preparing a composite flooring containing a fiber layer according to an embodiment of the present disclosure. This flow chart corresponds to the scenario of renovating an existing building. It should be noted that the composite flooring of the present disclosure is particularly suitable for this scenario. Since the existing floor is already relatively flat and the composite flooring is relatively thin, it can be directly laid over the existing floor (without damaging the existing flooring), significantly eliminating the need for installation. Because new homes are unrenovated and the floor surface may be sloped or uneven, it is necessary to pre-roughen and level the floor in step S200, primarily to repair damaged areas of the existing floor. Under certain conditions, repair may not be necessary. Subsequently, an optional step S220 can be performed: applying waterproof, weather-resistant, and environmentally friendly adhesive. In some embodiments, a bonding layer is not applied beneath the fiber layer 3, so a pre-applied layer of weather-resistant, environmentally friendly adhesive is required. It is foreseeable that if a bonding layer is already applied beneath the fiber layer 3, step S220 can be omitted. After step S220, step S240 can also be implemented: laying the composite floor, that is, pasting the composite floor on the ground in an orderly manner to form an integral structure. Further optionally, after step S240, the step of crystallizing the composite floor can also be included. A typical crystallization treatment process may specifically include: using a floor scrubber to thoroughly clean the marble surface first; using pure water to mix the crystal powder into a paste and apply it on the grinding pad; using a floor scrubber to start grinding under a certain load; when the surface of the stone layer forms a high-gloss crystal surface, using a water suction machine to absorb the residual paste on the ground; rinsing with water to dry; polishing with a polishing pad to make the ground completely dry to achieve a bright surface effect. Of course, in some embodiments, such as if the composite floor has a protective film, the crystallization treatment process can be omitted.

[0116] Under the overall concept of the specific composite floor material and structure disclosed in the present invention, the corresponding paving process is greatly simplified, thereby improving the efficiency of the overall decoration process.

[0117] In the above description, for illustrative purposes, numerous specific details are set forth in order to provide a comprehensive understanding of the various embodiments of the present disclosure. However, it will be apparent to those skilled in the art that one or more other embodiments may be implemented without some of these specific details. The specific embodiments described are not intended to limit the present disclosure but to illustrate. The scope of the present disclosure is not determined by the specific examples provided above, but only by the claims below. In other cases, known circuits, structures, devices, and operations are shown in block diagram form rather than in detail so as not to obscure the understanding of the description. Where deemed appropriate, figure numerals or the end of figure numerals are repeated among the drawings to indicate corresponding or similar elements that optionally have similar properties or identical features, unless otherwise specified or apparent.

[0118] Various operations and methods have been described. Some methods have been described in a relatively basic manner using flowcharts, but these operations may optionally be added to and / or removed from these methods. In addition, although the flowcharts illustrate a specific order of operations according to various example embodiments, it will be understood that this specific order is exemplary. Alternative embodiments may optionally perform these operations in different ways, combine certain operations, interleave certain operations, etc. The components, features, and certain optional details of the devices described herein may also optionally be applied to the methods described herein.

[0119] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present disclosure. It should be understood that the above are only specific embodiments of the present disclosure and are not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure should be included in the scope of protection of the present disclosure.

Claims

1. A composite flooring containing a fiber layer, characterized in that: include: Stone layer, thickness ranging from 0.1mm to 10mm; a bonding layer, located below the stone layer; The fiber layer is located below the bonding layer and has a thickness between 0.01 mm and 2 mm.

2. The composite floor according to claim 1, characterized in that: The thickness of the stone layer is greater than 0.5 mm and less than 8 mm.

3. The composite floor according to claim 2, characterized in that: The thickness of the stone layer is greater than 1 mm and less than 4 mm.

4. The composite flooring according to claim 1, characterized in that: The material of the stone layer includes at least one of the following: Limestone, granite and marble.

5. The composite flooring according to claim 1, characterized in that: The bonding layer material includes at least one of the following: Hot melt adhesives and thermosetting adhesives.

6. The composite flooring according to claim 1, characterized in that: The bonding layer covers an area ratio of more than 95% of the stone layer.

7. The composite flooring according to claim 1, characterized in that: The thickness of the adhesive layer is between 0.1 mm and 1 mm.

8. The composite flooring according to claim 1, characterized in that: The fiber layer material includes chemical fibers, and the chemical fibers include at least one of the following: Aramid, polyester, nylon, acrylic, polypropylene, vinylon and chloroprene.

9. The composite flooring according to claim 1, characterized in that: The fiber layer material comprises at least one of the following: Carbon fiber and fiberglass.

10. The composite flooring according to claim 1, characterized in that: The elastic modulus of the material of the fiber layer is between 5 GPa and 500 GPa.

11. The composite flooring according to claim 1, wherein the thickness of the fiber layer is between 0.2 mm and 0.5 mm.

12. The composite flooring according to claim 1, characterized in that: Also includes: A protective film is covered on the stone layer. The protective film is attached to the stone layer and is a transparent material.

13. The composite flooring according to claim 12, characterized in that: The material of the protective film includes at least one of the following materials: PU, TPU or PVC.

14. The composite flooring according to claim 1, characterized in that: Also includes: The bonding layer is located below the fiber layer, has a sticky material on one side close to the fiber layer to be fixedly connected with the fiber layer, and a silicone film on the other side away from the fiber layer. The silicone film is configured to adhere to the sticky material and can be torn apart by external force.

15. The composite flooring according to claim 1, characterized in that: The surface density of the composite floor is between 3kg / m 2 Up to 30kg / m 2 between.

16. The composite flooring according to claim 1, characterized in that: The surface of the stone layer of the composite floor is impacted by a 1 kg stainless steel ball falling freely from a height of 1 meter, and the surface has no cracks.

17. The composite flooring according to claim 1, characterized in that: The stone layer of the composite floor has a chamfered structure.

18. The composite flooring according to claim 1, characterized in that: The surface of the stone layer has at least one of the following processed structures: Grooved structure, mirror or smooth surface structure, matte surface structure, lychee surface structure, leather surface structure, washed surface structure and antique surface structure.

19. The composite flooring according to claim 1, characterized in that: The edge of the fiber layer comprises a snap-fit ​​structure configured to fix and connect adjacent composite floors by snap-fitting.

20. The composite flooring according to claim 19, characterized in that There are a plurality of composite floors, and the composite floors are fixedly connected to each other through the snap-fit ​​structure of the fiber layer.

Citation Information

Patent Citations

  • Plate

    CN101481949A

  • Stone composite plate and processing method thereof

    CN110219431A

  • Stone composite plate with sandwich structure

    CN202685426U

  • Stone material composite sheet of reinforcing structure

    CN204936349U

  • Light stone composite board

    CN210659069U