Concrete modifying agent and preparation method therefor, concrete admixture and concrete composition

By using a modulator with a polymeric network structure in concrete, the problems of poor cohesion and bleeding are solved, the stability and segregation resistance of the concrete are improved, the bleeding rate is reduced, and the durability and production efficiency of the concrete are improved.

WO2024198014A1PCT designated stage expired Publication Date: 2024-10-03SHIJIAZHUANG CHANGAN YUCAI BUILDING MATERIALS +1

Patent Information

Application Number
PCT/CN2023/089738
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2023-04-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing concrete is prone to problems such as poor cohesion, bleeding, and segregation during use, resulting in reduced surface strength, reduced compactness, reduced structural strength, and reduced production efficiency. The effect of traditional water-retaining agents is not significant.

Method used

A concrete conditioning agent is used, and its preparation raw materials include polyether macromonomer, acrylic acid, acrylamide, 2-acrylamide-2-methylpropanesulfonic acid, unsaturated phosphate ester and organic matter with two carbon-carbon double bonds. , the initiator initiates polymerization to form a cross-linked network structure, which improves the viscosity and segregation resistance of the aggregate and slurry, and reduces the bleeding rate.

Benefits of technology

Effectively control the slump loss of concrete, improve working performance, reduce segregation and bleeding, improve the resistance to yield stress and segregation resistance, reduce the bleeding rate, and improve the durability and production efficiency of concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023089738-APPB-I100001
    Figure PCTCN2023089738-APPB-I100001
  • Figure PCTCN2023089738-APPB-I100002
    Figure PCTCN2023089738-APPB-I100002
Patent Text Reader

Abstract

Provided in the present disclosure are a concrete modifying agent and a preparation method therefor, a concrete admixture and a concrete composition. The concrete modifying agent of the present disclosure is prepared from the following raw materials, in parts by weight: 5-8 parts of a polyether macromonomer, 3-8 parts of acrylic acid, 70-80 parts of acrylamide, 3-8 parts of 2-acrylamide-2-methylpropanesulfonic acid, 5-8 parts of an unsaturated phosphate, 5-10 parts of an organic matter with two carbon-carbon double bonds, 0.02-0.04 parts of an initiator and 600-1000 parts of deionized water. The concrete modifying agent has a very good water retention effect, can effectively control the gradual loss of concrete slump, can improve the working performance of concrete, and reduces the problems of concrete segregation and water bleeding.
Need to check novelty before this filing date? Find Prior Art

Description

Concrete modifier and preparation method thereof, concrete admixture and concrete composition

[0001] This disclosure claims priority to patent application number 2023103220093 filed with the Patent Office of China on March 29, 2023, entitled “Concrete Modifier and Preparation Method thereof, Concrete Admixture and Concrete Composition,” the entire contents of which are incorporated herein by reference. Technical Field

[0002] The present disclosure relates to the field of concrete building materials, and in particular to a concrete modifier and a preparation method thereof. The present disclosure also relates to a concrete admixture and a concrete composition comprising the concrete modifier. Background Art

[0003] With the rapid construction of economic highways, railways, hydropower stations, and civil engineering projects, the performance requirements for high-performance concrete are becoming increasingly stringent. However, in practical applications, due to factors such as unstable cement composition, poor compatibility between admixtures and cement, and low levels of fine and fine aggregates such as sand and stone, concrete suffers from poor cohesiveness, making it prone to segregation, bleeding, and bottom scraping. Bleeding reduces the surface strength of concrete. As water rises, it creates channels. These pores reduce the compactness of the concrete, allowing chloride ions, sulfates, and carbon dioxide to easily enter the concrete, severely reducing its durability. Furthermore, water pockets formed beneath the concrete surface weaken the interface between aggregate and cement paste. In self-compacting concrete, bleeding can also lead to incomplete mold filling, reducing structural strength. In pumped concrete, bleeding can cause concrete to scrape and block pipes, reducing production efficiency and increasing labor intensity.

[0004] To reduce bleeding, modifiers are often added to concrete mixing. These modifiers, also known as stabilizers, viscosity regulators, and water-retaining agents, are a new type of concrete admixture, initially used abroad in underwater non-dispersible concrete and self-compacting concrete. They increase concrete's cohesiveness and water retention, reduce the occurrence of "paste-bone separation," enhance concrete paste homogeneity, and improve concrete workability. Modifiers are often compounded with polycarboxylate superplasticizers. Currently, modifiers are primarily used in high-flow mortars, high-flow concrete, self-compacting concrete, underwater non-dispersible concrete, and shotcrete. They improve concrete workability and resolve the conflict between high-flow, high-extensibility fresh mortars and the deformation capacity and segregation resistance of concrete.

[0005] The inventors retrieved the following relevant patent document: CN110003375B discloses a salt-resistant concrete water-retaining agent and its preparation method. The water-retaining agent is made from the following raw materials: 10-20 parts of an acrylic acid compound, 2-10 parts of 2-acrylamide-2-methylpropanesulfonic acid, 2-10 parts of either sodium alkyl sulfonate or sodium alkylbenzenesulfonate, 0.2-2 parts of a hydrophobic monomer, 0.05-0.15 parts of an initiator, and 600-830 parts of deionized water. The preparation method involves adding the acrylic acid compound and 2-acrylamide-2-methylpropanesulfonic acid to a reactor, dissolving them in deionized water, neutralizing them with sodium hydroxide, adding either sodium alkyl sulfonate or sodium alkylbenzenesulfonate and the hydrophobic monomer, and completely dissolving them. The mixture is stirred and heated to 40-50°C, followed by the addition of the initiator and reaction for 7-8 hours. The remaining deionized water is then added to obtain a viscous liquid, which is the water-retaining agent.

[0006] CN113087844A discloses a polycarboxylic acid water-retaining agent for wet-mixed mortar and concrete and a preparation method thereof. The raw materials for the preparation include sodium propylene sulfonate, acrylamide, hydrogen peroxide, acrylic acid, mercaptopropionic acid, VC, and deionized water. The proportion of sodium propylene sulfonate is set to 5-10 parts, the proportion of acrylamide is set to 5-10 parts, and the proportion of hydrogen peroxide is set to 0.3-0.5 parts.

[0007] The above technologies do not provide specific guidance on how to improve the adsorption of cement by water-retaining agents, how to improve the anti-segregation and anti-bleeding properties of concrete, and how to reduce the sensitivity of modifiers. The water-retaining agents prepared according to the above methods are not effective. Summary of the Invention

[0008] The present disclosure proposes a concrete modifier, which has a good water retention effect, can effectively control the loss of concrete slump over time, can improve the working performance of concrete, and reduce the problems of concrete segregation and water bleeding.

[0009] A concrete modifier. The raw materials for preparing the concrete modifier include, by weight, 5-8 parts of polyether macromonomer, 3-8 parts of acrylic acid, 70-80 parts of acrylamide, 3-8 parts of 2-acrylamide-2-methylpropanesulfonic acid, 5-8 parts of unsaturated phosphate, 5-10 parts of organic matter with two carbon-carbon double bonds, 0.02-0.04 parts of initiator, and 600-1000 parts of deionized water.

[0010] The concrete modifier disclosed herein incorporates organic compounds with two carbon-carbon double bonds into its raw materials, enabling the polymerized molecular chains to form a network structure, making it more resilient to free water absorption and reducing concrete bleeding. The carboxylic acid, sulfonic acid, and amino groups introduced into the raw materials have an adsorption effect, increasing the viscosity of aggregate and slurry, enhancing the stability of fresh concrete, and improving the concrete's yield stress and segregation resistance. The introduced phosphate ester releases phosphate groups, which have a stronger ability to complex with calcium ions, reducing late-stage concrete bleeding.

[0011] Furthermore, the unsaturated phosphate includes at least one of acrylic acid phosphate, methacrylic acid phosphate, and hydroxyethyl methacrylate phosphate.

[0012] Furthermore, the polyether macromonomer includes at least one of isobutylene alcohol polyoxyethylene ether, isopentenol polyoxyethylene ether, and hexacarbon polyether macromonomer, and the molecular weight of the polyether macromonomer is 2400-5000.

[0013] Furthermore, the organic matter with two carbon-carbon double bonds includes at least one of 1,3-butadienoic acid methyl ester, 2,3-butadienoic acid ethyl ester, benzyl 2,3-butadienoate, isoprene, and 1,3-butadiene.

[0014] Furthermore, the initiator is ammonium persulfate or hydrogen peroxide.

[0015] The present disclosure also proposes a method for preparing a concrete modifier, characterized in that: a polyether macromonomer, acrylic acid, acrylamide, 2-acrylamide-2-methylpropanesulfonic acid, an unsaturated phosphate, an organic matter with two carbon-carbon double bonds, and deionized water are mixed and dissolved uniformly, an initiator is added, alkali is added to neutralize to a pH of 6-8, and the mixture is stirred uniformly to obtain the concrete modifier.

[0016] Furthermore, the reaction temperature is controlled between 50-60°C.

[0017] The present disclosure also provides a concrete admixture, which includes the above-mentioned concrete modifier.

[0018] Furthermore, the concrete admixture also includes a polycarboxylate water reducer.

[0019] The present disclosure also provides a concrete composition, wherein the raw materials for preparing the concrete composition include the above-mentioned concrete modifier.

[0020] The concrete composition disclosed herein has the advantages of good working performance and low water bleeding rate by adopting the above-mentioned concrete modifier. DETAILED DESCRIPTION

[0021] It should be noted that, unless there is any conflict, the embodiments and features in the embodiments of the present disclosure may be combined with each other.

[0022] The experimental methods in the following examples, unless otherwise specified, are conventional methods. The experimental materials used in the following examples, unless otherwise specified, were purchased from conventional biochemical reagent stores. Furthermore, unless otherwise specified in this example, the terms and processes involved in this example should be understood in accordance with general knowledge and conventional methods in the prior art.

[0023] A concrete modifier, wherein the raw materials for preparing the concrete modifier include, by weight, 5-8 parts of polyether macromonomer, 3-8 parts of acrylic acid, 70-80 parts of acrylamide, 3-8 parts of 2-acrylamide-2-methylpropanesulfonic acid, 5-8 parts of unsaturated phosphate, 5-10 parts of organic matter with two carbon-carbon double bonds, 0.02-0.04 parts of ammonium persulfate and 600-1000 parts of deionized water.

[0024] The concrete modifier disclosed herein utilizes an initiator to initiate free radical polymerization of a polyether macromonomer, acrylic acid, acrylamide, 2-acrylamido-2-methylpropanesulfonic acid, an unsaturated phosphate, and an organic compound with two carbon-carbon double bonds. The resulting polymer possesses long polyether side chains, carboxylic acid groups, amide groups, sulfonic acid groups, and phosphate groups, resulting in a high molecular weight polymer with a cross-linked network structure. Conventional free radical polymerization initiators, such as peroxides, can be used as the initiator, with ammonium persulfate being preferred in this disclosure.

[0025] Organic compounds with two carbon-carbon double bonds strengthen intermolecular crosslinking, creating a more complex molecular network structure. This provides a polymeric network framework for the polymerized macromolecular chains. Compared to the long linear chains of traditional water-retaining agents, this network structure more effectively absorbs free water through entanglement, absorption, and bonding, reducing the amount of free water and thus the likelihood of concrete bleeding. Organic compounds with two carbon-carbon double bonds can be selected from diunsaturated aliphatic compounds or linear dienes, and are preferably at least one of methyl 1,3-butadienoate, ethyl 2,3-butadienoate, benzyl 2,3-butadienoate, isoprene, and 1,3-butadiene.

[0026] The addition of polyether macromonomers makes the polymer have long polyether side chains, which has better compatibility with the polycarboxylate water-reducing agent synthesized from the polyether monomers, and prevents the two from delamination after compounding. The polyether macromonomers can preferably be at least one of isobutylene alcohol polyoxyethylene ether, isopentenol polyoxyethylene ether, and hexacarbon polyether macromonomers. The molecular weight of the polyether macromonomer is further preferably 2400-5000.

[0027] Acrylic acid, acrylamide, and 2-acrylamide-2-methylpropanesulfonic acid provide carboxylic acid groups, sulfonic acid groups, and amino groups for the polymerization products. These groups have an adsorption effect and can be effectively adsorbed on cement particles. At the same time, the polymer molecular network structure wraps around the mixing water, locking the moisture, allowing water and cement particles to fully contact, thereby increasing the viscosity of the slurry. The increase in slurry viscosity strengthens the cohesion between aggregate and slurry, improves the stability and yield stress value of fresh concrete, and enhances the concrete's anti-segregation ability.

[0028] Unsaturated phosphate esters provide phosphate groups for the polymerized product. Cement typically experiences alkaline conditions, where phosphate esters hydrolyze, releasing phosphate groups. Compared to traditional carboxylic acid, sulfonic acid, and amino groups, phosphate groups have a stronger electronegativity and a stronger ability to complex with calcium ions, reducing the sensitivity of the modifier and preventing late-stage bleeding in the concrete. Preferred unsaturated phosphate esters disclosed herein may include at least one of acrylic acid phosphate, methacrylic acid phosphate, and hydroxyethyl methacrylate phosphate.

[0029] In summary, the raw materials for preparing the concrete modifier disclosed herein can form a network structure by adding organic matter with two carbon-carbon double bonds to the polymerized molecular chains, making it easier to absorb free water and reduce the water bleeding rate of concrete. The carboxylic acid group, sulfonic acid group, and amino group introduced into the raw materials have an adsorption effect, which can increase the viscosity of aggregate and paste, increase the stability of fresh concrete, and improve the yield stress value and anti-segregation ability of concrete. The introduced phosphate ester can release phosphate groups, which have a stronger ability to complex with calcium ions and can reduce the occurrence of water bleeding in the later stage of concrete.

[0030] The present disclosure also proposes a method for preparing a concrete modifier. Specifically, the following method can be used: 5-8 parts of a polyether macromonomer, 3-8 parts of acrylic acid, 70-80 parts of acrylamide, 3-8 parts of 2-acrylamido-2-methylpropanesulfonic acid, 3-8 parts of an unsaturated phosphate, 5-10 parts of an organic compound with two carbon-carbon double bonds, and 600-1000 parts of deionized water are added to a reactor, stirred until completely dissolved, and then 0.02-0.04 parts of ammonium persulfate are added. After stirring for 1-2 hours, stirring is stopped and the mixture is kept warm for 10-14 hours. Liquid caustic soda is added to neutralize the mixture to a pH of 6-8, and stirred for 10-30 minutes to obtain the concrete modifier. To achieve better performance of the prepared concrete modifier, the temperature of the above preparation process is preferably controlled at 50-60°C.

[0031] The present disclosure also provides a concrete admixture comprising the aforementioned concrete modifier. It is worth noting that, due to the good compatibility of the concrete modifier with polycarboxylate superplasticizers and their insensitivity to dosage, the concrete modifier is highly suitable for use with polycarboxylate superplasticizers, improving concrete performance and resolving issues such as concrete segregation and bleeding. Therefore, the concrete admixture of the present disclosure may preferably also include a polycarboxylate superplasticizer.

[0032] The present disclosure also provides a concrete composition, wherein the raw materials for preparing the concrete composition include the above-mentioned concrete modifier. The concrete composition disclosed herein has the advantages of good working performance and low water bleeding rate by using the above-mentioned concrete modifier.

[0033] The specific implementation scheme of the present disclosure is described in detail below. Example 1

[0034] The concrete modifier of this embodiment is made of the following components and raw materials in parts by weight: 5 parts of isopentanol polyoxyethylene ether (molecular weight 2400), 3 parts of acrylic acid, 75 parts of acrylamide, 3 parts of 2-acrylamide-2-methylpropanesulfonic acid, 5 parts of acrylic acid phosphate, 5 parts of methyl 1,3-butadienoate, 0.02 parts of ammonium persulfate, and 864 parts of deionized water.

[0035] The preparation method of the concrete modifier is as follows: add isopentanol polyoxyethylene ether, acrylic acid, acrylamide, 2-acrylamide-2-methylpropanesulfonic acid, acrylic acid phosphate, 1,3-butadienoic acid methyl ester and deionized water into a reactor, heat to 50°C, stir until all are dissolved, add ammonium persulfate, continue stirring for 1 hour, stop stirring and keep warm for 10 hours, add liquid alkali to neutralize to neutrality, stir for 20 minutes, and thus prepare the concrete modifier.

[0036] The concrete modifier of this embodiment was compounded with a polycarboxylate water-reducing agent and added to cement concrete for mixing. The slump, expansion, bleeding rate ratio and compressive strength were tested. Example 2

[0037] The concrete modifier of this embodiment is made of the following components and raw materials in parts by weight: 7 parts of isobutylene alcohol polyoxyethylene ether (molecular weight 3000), 5 parts of acrylic acid, 75 parts of acrylamide, 5 parts of 2-acrylamide-2-methylpropanesulfonic acid, 6 parts of methacrylate phosphate, 7 parts of ethyl 2,3-butadienoate, 0.03 parts of ammonium persulfate, and 945 parts of deionized water.

[0038] The preparation method of the concrete modifier is as follows: isobutylene alcohol polyoxyethylene ether, acrylic acid, acrylamide, 2-acrylamide-2-methylpropanesulfonic acid, methacrylate phosphate, 2,3-butadienoic acid ethyl ester and deionized water are added to a reactor, the temperature is raised to 55° C., and ammonium persulfate is added after stirring until all are dissolved. After continuing stirring for 1.5 hours, stirring is stopped and kept warm for 12 hours, liquid alkali is added to neutralize to neutrality, and stirring is carried out for 10 minutes to prepare the concrete modifier.

[0039] The concrete modifier of this embodiment was compounded with a polycarboxylate water-reducing agent and added to cement concrete for mixing. The slump, expansion, bleeding rate ratio and compressive strength were tested. Example 3

[0040] The concrete modifier of this embodiment is made of the following components and raw materials in parts by weight: 8 parts of isopentanol polyoxyethylene ether (molecular weight 5000), 5 parts of acrylic acid, 75 parts of acrylamide, 8 parts of 2-acrylamide-2-methylpropanesulfonic acid, 8 parts of hydroxyethyl methacrylate phosphate, 10 parts of benzyl 2,3-butadienoate, 0.04 parts of ammonium persulfate, and 709 parts of deionized water.

[0041] The preparation method of the concrete modifier is as follows: prenol polyoxyethylene ether, acrylic acid, acrylamide, 2-acrylamide-2-methylpropanesulfonic acid, hydroxyethyl methacrylate phosphate, benzyl 2,3-butadienoate and deionized water are added to a reactor, the temperature is raised to 60° C., and ammonium persulfate is added after stirring until all are dissolved. After continuing stirring for 2 hours, stirring is stopped and the temperature is kept for 14 hours. Liquid alkali is added to neutralize to neutrality, and stirring is carried out for 30 minutes to prepare the concrete modifier.

[0042] The concrete modifier of this embodiment was compounded with a polycarboxylate water-reducing agent and added to cement concrete for mixing. The slump, expansion, bleeding rate ratio and compressive strength were tested. Example 4

[0043] The concrete modifier of this embodiment is made from the following components and raw materials in parts by weight: 5 parts of hexacarbonyl polyether macromonomer (molecular weight 3000), 8 parts of acrylic acid, 80 parts of acrylamide, 5 parts of 2-acrylamide-2-methylpropanesulfonic acid, 5 parts of methacrylic acid phosphate, 5 parts of isoprene, 0.03 parts of ammonium persulfate, and 722 parts of deionized water.

[0044] The preparation method of the concrete modifier is as follows: add a hexacarbon polyether macromonomer, acrylic acid, acrylamide, 2-acrylamide-2-methylpropanesulfonic acid, methacrylate phosphate, isoprene and deionized water into a reactor, heat to 55°C, stir until completely dissolved, add ammonium persulfate, continue stirring for 1.5 hours, stop stirring and keep warm for 12 hours, add liquid alkali to neutralize until neutral, and stir for 20 minutes to prepare the concrete modifier.

[0045] The concrete modifier of this embodiment was compounded with a polycarboxylate water-reducing agent and added to cement concrete for mixing. The slump, expansion, bleeding rate ratio and compressive strength were tested. Example 5

[0046] The concrete modifier of this embodiment is made of the following components and raw materials in parts by weight: 8 parts of isobutylene alcohol polyoxyethylene ether (molecular weight 5000), 5 parts of acrylic acid, 75 parts of acrylamide, 5 parts of 2-acrylamide-2-methylpropanesulfonic acid, 5 parts of acrylic acid phosphate, 5 parts of 1,3-butadiene, 0.03 parts of ammonium persulfate, and 920 parts of deionized water.

[0047] The preparation method of the concrete modifier is as follows: isobutylene alcohol polyoxyethylene ether, acrylic acid, acrylamide, 2-acrylamide-2-methylpropanesulfonic acid, acrylic acid phosphate, 1,3-butadiene and deionized water are added to a reactor, the temperature is raised to 50°C, and ammonium persulfate is added after stirring until all are dissolved. After continuing stirring for 1-2 hours, stirring is stopped and kept warm for 13 hours, liquid alkali is added to neutralize to neutrality, and stirring is carried out for 15 minutes to obtain the concrete modifier.

[0048] The concrete modifier of this embodiment was compounded with a polycarboxylate water-reducing agent and added to cement concrete for mixing. The slump, expansion, bleeding rate ratio and compressive strength were tested.

[0049] Comparative Example 1

[0050] No water-retaining agent or concrete modifier was added to the cement concrete, and only polycarboxylate water-reducing agent was added to test the slump, expansion, bleeding rate ratio and compressive strength of the cement concrete.

[0051] Comparative Example 2

[0052] Common water-retaining agents sold on the market were added to cement concrete to test the slump, expansion, water bleeding rate ratio and compressive strength of the cement concrete.

[0053] The concrete modifiers prepared in Examples 1, 2, 3, 4, and 5 were combined with a polycarboxylate superplasticizer and compared with Comparative Examples 1 and 2. The polycarboxylate superplasticizer was polycarboxylate superplasticizer concentrate P1 produced by Shijiazhuang Chang'an Yucai Building Materials Co., Ltd. Using the concrete mix proportions shown in Table 2, the effects on concrete slump, expansion, bleeding rate, and strength were tested. The experiments were conducted in accordance with GB / T50080-2016, "Standard for Test Methods for Properties of Ordinary Concrete Mixtures."

[0054] Table 1 Material ratio of concrete composition

[0055]

[0056] Table 2 Concrete performance test results

[0057]

[0058] Table 2 shows that compared with the concrete without water-retaining agent and the concrete with common water-retaining agent on the market, the concrete with the concrete modifier prepared by the present disclosure has good fluidity, small slump loss, and low water bleeding rate, which can better solve the problems of concrete segregation and water bleeding, and at the same time improve the compressive strength of concrete.

[0059] The preferred embodiments of the present disclosure are described in detail above. However, the present disclosure is not limited to the specific details of the above embodiments. Within the technical concept of the present disclosure, various simple modifications can be made to the technical solutions of the present disclosure, and these simple modifications all fall within the scope of protection of the present disclosure.

[0060] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any appropriate manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.

Claims

1. A concrete modifier, characterized in that: The raw materials for preparing the concrete modifier include, by weight: 5-8 parts of polyether macromonomer, 3-8 parts of acrylic acid, 70-80 parts of acrylamide, 3-8 parts of 2-acrylamide-2-methylpropane sulfonic acid, 5-8 parts of unsaturated phosphate, 5-10 parts of organic matter with two carbon-carbon double bonds, 0.02-0.04 parts of initiator and 600-1000 parts of deionized water.

2. The concrete modifier according to claim 1, characterized in that: The unsaturated phosphate ester includes at least one of acrylic acid phosphate ester, methacrylic acid phosphate ester, and hydroxyethyl methacrylate phosphate ester.

3. The concrete modifier according to claim 1, characterized in that: The polyether macromonomer includes at least one of isobutylene alcohol polyoxyethylene ether, isopentanol polyoxyethylene ether and hexacarbon polyether macromonomer, and the molecular weight of the polyether macromonomer is 2400-5000.

4. The concrete modifier according to claim 1, characterized in that: The organic matter with two carbon-carbon double bonds includes at least one of 1,3-butadienoic acid methyl ester, 2,3-butadienoic acid ethyl ester, benzyl 2,3-butadienoate, isoprene, and 1,3-butadiene.

5. The concrete modifier according to any one of claims 1 to 4, characterized in that: The initiator is ammonium persulfate or hydrogen peroxide.

6. A method for preparing a concrete modifier, characterized in that: The polyether macromonomer, acrylic acid, acrylamide, 2-acrylamide-2-methylpropane sulfonic acid, unsaturated phosphate, organic matter with two carbon-carbon double bonds and deionized water are mixed and dissolved uniformly, an initiator is added, alkali is added to neutralize to pH=6-8, and stirred uniformly to obtain the concrete modifier.

7. The method for preparing a concrete modifier according to claim 6, characterized in that: The reaction temperature is controlled between 50-60°C.

8. A concrete admixture, characterized in that: The concrete admixture includes the concrete modifier according to any one of claims 1 to 5.

9. The concrete admixture according to claim 8, characterized in that: The concrete admixture also includes a polycarboxylate water reducer.

10. A concrete composition, characterized in that: The raw materials for preparing the concrete composition include the concrete modifier according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Phosphate-based high slump loss resistant type polycarboxylate high-performance water reducing agent and preparation method thereof

    CN105837761A

  • Unsaturated phosphate ester for producing high-slump-retaining type polycarboxylic acid water reducing agent

    CN106008593A

  • Concrete performance regulator and preparation method thereof

    CN106699965A

  • Short-chain branch cross-linked water-retaining solvent layer controlled-release type polycarboxylic acid slump retaining agent and preparation method thereof

    CN107987224A

  • Concrete viscosifying type viscosity modifier and preparation method thereof

    CN109369859A

Cited By

  • Self-compacting concrete viscosity modifier and preparation and application methods thereof

    CN122212532A