Negative photosensitive polyimide precursor resin composition
Through low-temperature thermal imidization of a negative photosensitive polyimide precursor resin composition, the problems of warpage and insufficient chemical corrosion resistance of traditional polyimide materials in high-density fan-out packages are solved, achieving Excellent mechanical properties and copper surface bonding strength meet the requirements of high-end packaging processes.
Patent Information
- Application Number
- PCT/CN2023/089830
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2023-04-21
- Publication Date
- 2024-10-03
AI Technical Summary
In the high-density fan-out wafer-level packaging process, traditional photosensitive polyimide materials cause wafer warping and stress cracking due to high curing temperatures, and insufficient imidization under low-temperature curing, resulting in poor mechanical properties and chemical resistance. It has poor corrosion resistance and is difficult to meet the requirements of high-end packaging processes.
A negative photosensitive polyimide precursor resin composition is used, including polyamic acid ester, free radical polymerizable monomer containing epoxy structure, photoinitiator, silane coupling agent, polymerization inhibitor and thermal base generator , curing is achieved through low-temperature thermal imidization to enhance the cross-linking density and chemical corrosion resistance of the cured film.
It achieves low-temperature curing below 230°C and obtains excellent mechanical properties, copper surface bonding strength and chemical corrosion resistance, meeting the application requirements of high-density fan-out wafer-level packaging.
Smart Images

Figure CN2023089830_03102024_PF_FP_ABST
Abstract
Description
Negative photosensitive polyimide precursor resin composition Technical Field
[0001] The present invention relates to the technical field of polyimides, in particular to a negative photosensitive polyimide precursor resin composition. Background Art
[0002] Photosensitive polyimide photoresist (PSPI) materials are widely used for surface passivation of integrated circuit chips and surface rewiring processes in wafer-level and panel-level packaging. They are key materials in advanced wafer-level packaging processes. Traditional PSPI materials require a curing temperature above 350°C to achieve their various excellent properties. However, such high curing temperatures can easily lead to wafer warpage, stress cracking, and compatibility issues with other packaging materials in advanced packaging processes such as high-density fan-out wafer-level packaging. Therefore, low-temperature curing is required for PSPI. However, low-temperature-cured PSPI materials often suffer from insufficient imidization, resulting in poor mechanical properties and chemical resistance, making them unable to meet packaging process requirements. Furthermore, poor adhesion to other materials in the packaging process, particularly electroplated copper, results in poor device reliability. Current high-end wafer-level packaging processes place higher demands on low-stress and low-warpage curing processes, creating an increasingly urgent need for ultra-low-temperature-curing PSPI materials below 200°C. Addressing these issues is becoming increasingly urgent.
[0003] Generally speaking, in order to solve the above problems, people will introduce light / heat base generators to reduce the activation energy of imidization of polyimide precursor resins and thus achieve various excellent properties of polyimide resins under low-temperature processes, such as CN112639616A, CN112513219A, CN112639615A and CN111919172A. Or they will control the molecular weight of the precursor resin so that the molecular chain has a sufficiently high mobility during low-temperature curing, thereby increasing the imidization rate, such as CN108475020A. For example, CN112334833A introduces a polymeric compound containing carbamate and urea bond structures, and CN110741318A and CN113168093A introduce a polymeric compound containing a sulfite structure to obtain the comprehensive properties of low-temperature curing, high imidization rate, good chemical resistance, and excellent copper surface adhesion. In addition, in order to improve the bonding strength between the redistribution layer and the copper surface, various copper surface additives are generally introduced, such as CN102375336B and CN112799281A.
[0004] Generally speaking, the most prominent problem facing PSPI materials cured below 230°C is insufficient chemical resistance, making it difficult to meet the process requirements of wafer-level packaging. The main reason for this problem is that at ultra-low curing temperatures, most of the additives, especially the polymerizable functional groups contained in the photocrosslinking agent and the polyimide precursor, remain in the cured film. The chemical resistance of these additive residues is often significantly inferior to that of polyimide. To address this problem, the general approach is to introduce a rigid photocrosslinker with an aliphatic cyclic backbone to enhance the molecular rigidity of the residue in the cured film, thereby improving its chemical resistance, such as CN110520795A. Alternatively, the introduction of a multifunctional crosslinking agent to increase the crosslinking density of the residue in the cured film to improve its chemical resistance, such as CN111936930A and CN110300767A. However, the materials produced by these methods still fail to achieve sufficient chemical resistance to meet the stringent requirements of packaging processes.
[0005] Summary of the Invention
[0006] In order to solve the above technical problems, the present invention provides a negative photosensitive polyimide precursor resin composition.
[0007] To achieve the above object, the technical solution adopted by the present invention is:
[0008] The present invention provides a negative photosensitive polyimide precursor resin composition, comprising:
[0009] 100 parts by mass of polyamic acid ester as a polyimide precursor;
[0010] 1-20 parts by mass of a first free radical polymerizable monomer containing an epoxy structure;
[0011] 1-20 parts by mass of a second free radical polymerizable monomer;
[0012] 0.5-10 parts by mass of a photoinitiator;
[0013] 0.5-10 parts by mass of a silane coupling agent;
[0014] 0.01-5 parts by mass of a polymerization inhibitor;
[0015] 0.1-10 parts by mass of a thermal alkali generator;
[0016] 50-1500 parts by mass of an organic solvent;
[0017] The first free radical polymerizable monomer containing an epoxy structure is selected from at least one of the compounds represented by formula (a), formula (b), formula (c), formula (d), formula (e) and formula (f):
[0018] In formula (a), R1 is selected from Any of;
[0019] wherein R2 is selected from any one of a hydrogen atom and an alkyl group having 1 to 3 carbon atoms, R3 and R4 are each independently selected from any one of a hydrogen atom and an aliphatic hydrocarbon group having 1 to 8 carbon atoms, and m=0 to 7;
[0020] In formula (b), n=0 to 6;
[0021] In formula (c), A1 is
[0022] In formula (d), R5 is selected from any one of a hydrogen atom and an alkyl group having 1 to 3 carbon atoms; R6 is selected from Any one of; p = 0 to 1;
[0023] In formula (e), A2 is a cyclic structure selected from Any of .
[0024] As a preferred embodiment, the polyamic acid ester has a structure as shown in formula (f):
[0025] In formula (f), X is a tetravalent organic group containing an aromatic group, Y is a divalent organic group containing an aromatic group, R7 and R8 are independently selected from monovalent organic groups having a structure as shown in formula (g), and q is 2 to 150;
[0026] In formula (g), R9, R 10 and R 11 Each of the groups is independently selected from a hydrogen atom and an alkyl group having 1 to 3 carbon atoms; and r is 2 to 10.
[0027] As a preferred embodiment, the second free radical polymerizable monomer is selected from any one or more of (meth)acrylate compounds, preferably any one or more of difunctional (meth)acrylate compounds and trifunctional (meth)acrylate compounds; in the technical solution of the present invention, the (meth)acrylate compounds include acrylate compounds and / or methacrylate compounds;
[0028] Specifically, the second free radical polymerizable monomer is selected from tetraethylene glycol dimethacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylic acid, trimethylolpropane diacrylate, trimethylolpropane triacrylate, trimethylolpropane dimethacrylate, trimethylolpropane trimethacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, 1,4-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate. Any one or more of acrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, pentaerythritol trimethacrylate, pentaerythritol tetramethacrylate, styrene, divinylbenzene, 4-vinyltoluene, 4-vinylpyridine, N-vinylpyrrolidone, 2-hydroxyethyl methacrylate, 2-hydroxyethyl acrylate, 1,3-acryloyloxy-2-hydroxypropane, 1,3-methacryloyloxy-2-hydroxypropane, methylenebisacrylamide, N,N-dimethylacrylamide, and N-hydroxymethylacrylamide; preferably tetraethylene glycol dimethacrylate.
[0029] As a preferred embodiment, the preparation method of the polyamic acid ester comprises the following steps:
[0030] A tetracarboxylic dianhydride containing an X group, an alcohol having a free radical polymerizable unsaturated double bond and / or a saturated aliphatic alcohol having 1 to 4 carbon atoms are reacted to prepare a partially esterified tetracarboxylic acid; and then the tetracarboxylic acid is subjected to amide polycondensation with a diamine containing a Y group.
[0031] The tetracarboxylic dianhydride containing the X group is not particularly limited, and specific examples thereof include pyromellitic anhydride, diphenyl ether-3,3',4,4'-tetracarboxylic dianhydride, benzophenone-3,3',4,4'-tetracarboxylic dianhydride, biphenyl-3,3',4,4'-tetracarboxylic dianhydride, diphenylsulfone-3,3',4,4'-tetracarboxylic dianhydride, diphenylmethane-3,3',4,4'-tetracarboxylic dianhydride, 2,2-bis(3,4-phthalic anhydride)propane, 2,2-bis(3,4-phthalic anhydride)propane, and 2,2-bis(3,4-phthalic anhydride). -phthalic anhydride)-1,1,1,3,3,3-hexafluoropropane, etc., preferably pyromellitic anhydride, diphenyl ether-3,3',4,4'-tetracarboxylic dianhydride, benzophenone-3,3',4,4'-tetracarboxylic dianhydride, biphenyl-3,3',4,4'-tetracarboxylic dianhydride, more preferably pyromellitic anhydride, diphenyl ether-3,3',4,4'-tetracarboxylic dianhydride, biphenyl-3,3',4,4'-tetracarboxylic dianhydride, etc., the above can be used alone or in any combination.
[0032] The diamine containing the Y group is not particularly limited, and specific examples thereof include p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, -Diaminobenzidine, 3,4'-diaminobenzidine, 3,3'-diaminobenzidine, 4,4'-diaminobenzophenone, 3,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, 4,4'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene , bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, 4,4-bis(4-aminophenoxy)biphenyl, 4,4-bis(3-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]ether, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 9,10-bis(4-aminophenyl)anthracene, 2,2 -bis(4-aminophenyl)propane, 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl)propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 1,4-bis(3-aminopropyldimethylsilyl)benzene, 3,3'-dimethyl-4,4'-diaminodiphenyl sulfone, 9,9-bis(4-aminophenyl)fluorene, etc., which can be used alone or in any combination.
[0033] As a preferred embodiment, the photoinitiator is selected from any one or more of oxime ester compounds, benzophenone, N,N'-tetramethyl-4,4'-diaminobenzophenone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, alkyl anthraquinone, benzoin alkyl ether, benzoin, alkyl benzoin and benzil dimethyl ketal, and is further preferably an oxime ester compound.
[0034] As a preferred embodiment, the organic solvent is selected from any one or more of esters, ethers, ketones, aromatic hydrocarbons, sulfoxides and amides;
[0035] Preferably, the ester is selected from any one or more of ethyl acetate, n-butyl acetate, isobutyl acetate, amyl formate, isoamyl acetate, butyl propionate, isopropyl butyrate, ethyl butyrate, butyl butyrate, methyl lactate, ethyl lactate, γ-butyrolactone, ε-caprolactone, δ-valerolactone, alkyl alkoxyacetates, alkyl 3-alkoxypropionates, alkyl 2-alkoxypropionates, methyl 2-alkoxy-2-methylpropionate, ethyl 2-alkoxy-2-methylpropionate, methyl pyruvate, ethyl pyruvate, propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, methyl 2-oxobutyrate and ethyl 2-oxobutyrate;
[0036] Preferably, the ethers are selected from any one or more of diethylene glycol dimethyl ether, tetrahydrofuran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate and propylene glycol monopropyl ether acetate;
[0037] Preferably, the ketone is selected from any one or more of methyl ethyl ketone, cyclohexanone, cyclopentanone, 2-heptanone and 3-heptanone;
[0038] Preferably, the aromatic hydrocarbons are selected from any one or more of toluene, xylene, anisole and limonene;
[0039] Preferably, the amides are selected from any one or more of N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylacetamide and N,N-dimethylformamide.
[0040] In the technical solution of the present invention, the silane coupling agent is not particularly limited, and is preferably any one or more of the silane coupling agents containing a urea bond (-NH-CO-NH-);
[0041] Specifically, the silane coupling agent is selected from ureapropyl triethoxysilane, γ-aminopropyl dimethoxysilane, N-(β-aminoethyl)-γ-aminopropyl methyl dimethoxysilane, γ-glycidoxypropyl methyl dimethoxysilane, γ-mercaptopropyl methyl dimethoxysilane, 3-methacryloxypropyl dimethoxymethyl silane, 3-methacryloxypropyl trimethoxysilane, dimethoxymethyl-3-piperidinylpropyl silane, diethoxy-3-glycidoxypropyl methyl silane, N-(3-diethyl)- Any one or more of triethoxysilyl) propyl succinic anhydride, N-[3-(triethoxysilyl)propyl] phthalamic acid, benzophenone-3,3'-bis(N-[3-triethoxysilyl]propylamide)-4,4'-dicarboxylic acid, benzene-1,4-bis(N-[3-triethoxysilyl]propylamide)-2,5-dicarboxylic acid, 3-(triethoxysilyl)propyl succinic anhydride and N-phenylaminopropyltrimethoxysilane, preferably ureapropyltriethoxysilane.
[0042] In the technical solution of the present invention, the polymerization inhibitor is not particularly limited, and is preferably any one or more of the phenolic free radical polymerization inhibitors;
[0043] Specifically, the polymerization inhibitor is selected from any one or more of hydroquinone, N-nitrosodiphenylamine, p-tert-butylcatechol, phenothiazine, N-phenylnaphthylamine, ethylenediaminetetraacetic acid, 1,2-cyclohexanediaminetetraacetic acid, ethylene glycol ether diaminetetraacetic acid, 2,6-di-tert-butyl-p-methylphenol, 5-nitroso-8-hydroxyquinoline, 1-nitroso-2-naphthol, 2-nitroso-1-naphthol, 2-nitroso-5-(N-ethyl-N-sulfopropylamino)phenol, N-nitroso-N-phenylhydroxylamine ammonium salt and N-nitroso-N(1-naphthyl)hydroxylamine ammonium salt, preferably 2-nitroso-1-naphthol.
[0044] As a preferred embodiment, the thermal base generator is a tert-butoxycarbonyl protected amine compound, and the amine compound in the tert-butoxycarbonyl protected amine compound is selected from ethanolamine, 3-amino-1-propanol, 1-amino-2-propanol, 2-amino-1-propanol, 4-amino-1-butanol, 2-amino-1-butanol, 1-amino-2-butanol, 3-amino-2,2-dimethyl-1-propanol, 4-amino-2-methyl-1-butanol, valinol, 3-amino-1,2-propanediol, 2-amino-1,3-propanediol, tyramine, demethylephedrine, 2-amino-1-phenyl-1,3-propanediol, 2-aminocyclohexanol, 4-aminocyclohexanol, 4-aminocyclohexaneethanol, 4-(2-aminoethyl)cyclohexanol, N- Methylethanolamine, 3-(methylamino)-1-propanol, 3-(isopropylamino)propanol, N-cyclohexylethanolamine, α-[2-(methylamino)ethyl]benzyl alcohol, diethanolamine, diisopropanolamine, 3-pyrrolidinol, 2-pyrrolidinemethanol, 4-hydroxypiperidine, 3-hydroxypiperidine, 4-hydroxy-4-phenylpiperidine, 4-(3-hydroxyphenyl)piperidine, 4-piperidinemethanol, 3-piperidinemethanol, 2-piperidinemethanol, 4-piperidineethanol, 2-piperidineethanol, 2-(4-piperidinyl)-2-propanol, 1,4-butanol bis(3-aminopropyl) ether, 1,2-bis(2-aminoethoxy)ethane, 2,2'-oxybisethylamine, 1,14-diamino-3,6,9,12-tetraoxatetradecane, 1-aza-15-crown-5-ether, Any one or more of diethylene glycol bis(3-aminopropyl) ether, 1,11-diamino-3,6,9-trioxaundecane and diethylene glycol bis(3-aminopropyl) ether;
[0045] Preferably, the thermal base generator is N-tert-butyloxycarbonyl-4-piperidinol.
[0046] In another aspect, the present invention provides a negative photosensitive polyimide resin composition obtained by thermal imidization of the negative photosensitive polyimide precursor resin composition.
[0047] Preferably, the temperature of the thermal imidization is 150-400°C.
[0048] The above technical solution has the following advantages or beneficial effects:
[0049] The present invention aims to provide a negative photosensitive polyimide precursor resin composition. By introducing a polymerizable monomer containing an epoxy structure into the polyimide precursor composition, the resin composition can not only achieve low-temperature (below 230°C) curing, but also the cured film obtained after low-temperature curing has excellent mechanical properties, excellent bonding strength with the copper surface, and excellent chemical corrosion resistance, which can meet the application requirements of advanced packaging processes such as high-density fan-out wafer-level packaging. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] FIG1 is a schematic diagram of the chemical structures of EP-1 to EP-8 used in the examples and comparative examples of the present invention. DETAILED DESCRIPTION
[0051] The following embodiments are merely some of the embodiments of the present invention, rather than all of them. Therefore, the detailed description of the embodiments of the present invention provided below is not intended to limit the scope of the claimed invention, but rather merely represents selected embodiments of the present invention. All other embodiments derived by those skilled in the art based on the embodiments of the present invention without creative effort are intended to fall within the scope of protection of the present invention.
[0052] In the present invention, unless otherwise specified, all equipment and raw materials can be purchased from the market or are commonly used in the industry. The methods in the following embodiments, unless otherwise specified, are all conventional methods in the art.
[0053] The inventors discovered that existing methods for improving the chemical corrosion resistance of ultra-low temperature cured PSPI materials often simply increase the crosslinking density and molecular structure strength of the PSPI material during the exposure process. However, similar experimental verification found that this is not sufficient to obtain sufficiently excellent chemical corrosion resistance to meet the stringent requirements of the packaging process.
[0054] Therefore, the present invention introduces a polymerizable monomer containing an epoxy structure into the polyimide precursor composition. During the exposure process, double bonds can be cross-linked into the main structure of the polyimide precursor. At the same time, in the subsequent thermal curing process, the epoxy groups undergo a thermal cross-linking reaction with the hydroxyl groups generated after the imidization of the PSPI precursor, further enhancing the cross-linking density and strength of the additive residue in the cured film, thereby achieving excellent chemical corrosion resistance.
[0055] The negative photosensitive polyimide precursor resin composition provided by the present invention comprises: (1) polyamic acid ester as a polyimide precursor; (2) a first free radical polymerizable monomer containing an epoxy structure; (3) a second free radical polymerizable monomer; and (4) a photoinitiator.
[0056] Component (1): Polyamic acid ester
[0057] In the technical solution of the present invention, polyamic acid ester is converted into polyimide by thermal imidization, and as the photosensitive polyimide precursor in the present invention, it has a structure as shown in formula (f):
[0058] (In formula (f), X is a tetravalent organic group containing an aromatic group, Y is a divalent organic group containing an aromatic group, R7 and R8 are each independently selected from a monovalent organic group having a structure as shown in formula (g), and q is 2 to 150);
[0059] (In formula (g), R9, R 10 and R 11 are independently selected from hydrogen atoms and alkyl groups having 1 to 3 carbon atoms; r is 2 to 10).
[0060] Preparation of polyamic acid ester
[0061] In the technical solution of the present invention, the following method can be used to prepare the polyamic acid ester having the structure shown above:
[0062] A tetracarboxylic dianhydride containing an X group, an alcohol having a free radical polymerizable unsaturated double bond and / or a saturated aliphatic alcohol having 1 to 4 carbon atoms are reacted to prepare a partially esterified tetracarboxylic acid; and then the tetracarboxylic acid is subjected to amide polycondensation with a diamine containing a Y group.
[0063] The tetracarboxylic dianhydride containing the X group is not particularly limited, and specific examples thereof include pyromellitic anhydride, diphenyl ether-3,3',4,4'-tetracarboxylic dianhydride, benzophenone-3,3',4,4'-tetracarboxylic dianhydride, biphenyl-3,3',4,4'-tetracarboxylic dianhydride, diphenylsulfone-3,3',4,4'-tetracarboxylic dianhydride, diphenylmethane-3,3',4,4'-tetracarboxylic dianhydride, 2,2-bis(3,4-phthalic anhydride)propane, 2,2-bis(3,4-phthalic anhydride)propane, and 2,2-bis(3,4-phthalic anhydride). -phthalic anhydride)-1,1,1,3,3,3-hexafluoropropane, etc., preferably pyromellitic anhydride, diphenyl ether-3,3',4,4'-tetracarboxylic dianhydride, benzophenone-3,3',4,4'-tetracarboxylic dianhydride, biphenyl-3,3',4,4'-tetracarboxylic dianhydride, more preferably pyromellitic anhydride, diphenyl ether-3,3',4,4'-tetracarboxylic dianhydride, biphenyl-3,3',4,4'-tetracarboxylic dianhydride, etc., the above can be used alone or in any combination.
[0064] The alcohol having a radically polymerizable unsaturated double bond is not particularly limited, and specific examples thereof include 2-acryloyloxyethanol, 1-acryloyloxy-3-propanol, 2-acrylamidoethanol, hydroxymethyl vinyl ketone, 2-hydroxyethyl vinyl ketone, 2-hydroxy-3-methoxypropyl acrylate, 2-hydroxy-3-butoxypropyl acrylate, 2-hydroxy-3-phenoxypropyl acrylate, 2-hydroxy-3-butoxypropyl acrylate, 2-hydroxy-3-tert-butoxypropyl acrylate, 2-hydroxy-3-cyclohexyloxy Propyl acrylate, 2-methacryloyloxyethanol, 1-methacryloyloxy-3-propanol, 2-methacrylamidoethanol, 2-hydroxy-3-methoxypropyl methacrylate, 2-hydroxy-3-butoxypropyl methacrylate, 2-hydroxy-3-phenoxypropyl methacrylate, 2-hydroxy-3-butoxypropyl methacrylate, 2-hydroxy-3-tert-butoxypropyl methacrylate, 2-hydroxy-3-cyclohexyloxypropyl methacrylate, etc., can be used alone or in any combination.
[0065] The saturated aliphatic alcohols having 1 to 4 carbon atoms are not particularly limited, and specific examples thereof include methanol, ethanol, n-propanol, isopropanol, n-butanol, and tert-butanol. These alcohols may be used alone or in any combination.
[0066] The tetracarboxylic dianhydride and the alcohol are reacted in a suitable reaction solvent preferably in the presence of a basic catalyst such as pyridine at 20 to 50° C. for 4 to 10 hours with stirring to obtain a partially esterified tetracarboxylic acid.
[0067] The solvent used in the above reaction is preferably one that completely dissolves the reaction raw materials and / or products, and more preferably one that completely dissolves the photosensitive polyimide precursor. Specific examples of such solvents include N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, tetramethylurea, ketones, esters, lactones, ethers, halogenated hydrocarbons, and hydrocarbons. These solvents may be used alone or in any combination.
[0068] The solution containing partially esterified tetracarboxylic acid obtained in the above reaction is preferably added with a dehydrating condensation agent under ice-cold conditions to obtain a polyanhydride, and then a diamine containing a Y group or a solution thereof is added to obtain the target polyamic acid ester through amide polycondensation.
[0069] The dehydration condensation agent is not particularly limited, and specific examples thereof include dicyclohexylcarbodiimide, 1-ethoxycarbonyl-2-ethoxy-1,2-dihydroquinoline, 1,1-carbonyldioxy-di-1,2,3-benzotriazole, and N,N'-disuccinimidyl carbonate. These can be used alone or in any combination.
[0070] The diamine containing the Y group is not particularly limited, and specific examples thereof include p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminobiphenyl, 3,4'-diaminobiphenyl, 3,3'-diaminobiphenyl, 4,4'-diaminobenzophenone, 3,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, 4,4'-diaminodiphenylmethane, 3 ... '-Diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, 4,4-bis(4-aminophenoxy)biphenyl, 4,4-bis(3-aminophenoxy)biphenyl, bis[4-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]ether, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 9,10-bis(4-aminophenyl)anthracene, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-aminophenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 1,4-bis(3-aminopropyldimethylsilyl)benzene, 3,3'-dimethyl-4,4'-diaminodiphenyl sulfone, 9,9-bis(4-aminophenyl)fluorene, etc., can be used alone or in any combination.
[0071] Component (2): First free radical polymerizable monomer containing epoxy structure
[0072] In the technical solution of the present invention, a free radical polymerizable monomer containing an epoxy structure is added to the negative photosensitive polyimide precursor resin composition, which is selected from at least one of the compounds represented by formula (a), formula (b), formula (c), formula (d), formula (e) and formula (f):
[0073] In formula (a), R1 is selected from Any of;
[0074] wherein R2 is selected from any one of a hydrogen atom and an alkyl group having 1 to 3 carbon atoms, R3 and R4 are each independently selected from any one of H and an aliphatic hydrocarbon group having 1 to 8 carbon atoms, and m=0 to 7;
[0075] Specific examples of the radical polymerizable monomer containing an epoxy structure represented by formula (a) include:
[0076] In formula (b), n=0 to 6;
[0077] Specific examples of the radical polymerizable monomer containing an epoxy structure represented by formula (b) include:
[0078] In formula (c), A1 is
[0079] Specific examples of the radical polymerizable monomer containing an epoxy structure represented by formula (c) include:
[0080] In formula (d), R5 is selected from any one of a hydrogen atom and an alkyl group having 1 to 3 carbon atoms; R6 is selected from Any one of; p = 0 to 1;
[0081] Specific examples of the radical polymerizable monomer containing an epoxy structure represented by formula (d) include:
[0082] In formula (e), A2 is a cyclic structure selected from Any of;
[0083] Specific examples of the radical polymerizable monomer containing an epoxy structure represented by formula (e) include:
[0084] In the technical solution of the present invention, the amount of the first radical polymerizable monomer containing an epoxy structure having the above structure added is 1-20 parts by mass based on 100 parts of polyamic acid ester in order to balance the photolithographic performance and chemical corrosion resistance.
[0085] Component (3): Second free radical polymerizable monomer
[0086] The present invention further compounded a second free radical polymerizable monomer containing an unsaturated bond into the negative photosensitive polyimide precursor resin composition, which can undergo free radical polymerization reaction with the free radical polymerizable substituent on the side chain of the polyamic acid ester.
[0087] As the above-mentioned second free radical polymerizable monomer, it is preferably any one or more of the (meth)acrylate compounds that can undergo free radical polymerization reaction under the action of a photoinitiator. In the technical solution of the present invention, the (meth)acrylate compounds include acrylate compounds and / or methacrylate compounds: including but not limited to mono(meth)acrylate or di(meth)acrylate of ethylene glycol or polyethylene glycol headed by diethylene glycol dimethacrylate and tetraethylene glycol dimethacrylate; mono(meth)acrylate or di(meth)acrylate of propylene glycol or polypropylene glycol; mono(meth)acrylate, di(meth)acrylate or tri(meth)acrylate of glycerol; cyclohexane di(methacrylate); diacrylate of 1,4-butanediol; Ester and dimethacrylate, di(meth)acrylate of 1,6-hexanediol; di(meth)acrylate of neopentyl glycol; mono(meth)acrylate or di(meth)acrylate of bisphenol A; phenyl trimethacrylate; isobornyl(meth)acrylate; acrylamide and its derivatives; methacrylamide and its derivatives; trimethylolpropane tri(meth)acrylate; di(meth)acrylate or tri(meth)acrylate of glycerol; di(meth)acrylate, tri(meth)acrylate, or tetra(meth)acrylate of pentaerythritol; and compounds such as ethylene oxide or propylene oxide adducts of these compounds, and further preferably any one or more of difunctional (meth)acrylate compounds and trifunctional (meth)acrylate compounds.
[0088] Specific examples of the above-mentioned radical polymerization monomers include tetraethylene glycol dimethacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, trimethylolpropane diacrylate, trimethylolpropane triacrylate, trimethylolpropane dimethacrylate, trimethylolpropane trimethacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, 1,4-butanediol dimethacrylate, and 1,6-hexanediol dimethacrylate. , pentaerythritol triacrylate, pentaerythritol tetraacrylate, pentaerythritol trimethacrylate, pentaerythritol tetramethacrylate, styrene, divinylbenzene, 4-vinyltoluene, 4-vinylpyridine, N-vinylpyrrolidone, 2-hydroxyethyl methacrylate, 2-hydroxyethyl acrylate, 1,3-acryloyloxy-2-hydroxypropane, 1,3-methacryloyloxy-2-hydroxypropane, methylenebisacrylamide, N,N-dimethylacrylamide, N-hydroxymethylacrylamide, etc., the above can be used alone or in any combination, preferably triethylene glycol dimethacrylate.
[0089] In the technical solution of the present invention, the amount of free radical polymerization monomer added is 1-20 parts by mass based on 100 parts of polyamic acid ester from the perspective of improving photolithographic resolution. If the amount is too low, it is not conducive to obtaining high photolithographic resolution, and if it is too high, it will reduce the chemical corrosion resistance of the cured film.
[0090] Component (4): Photoinitiator
[0091] The photoinitiator applicable to the present invention is not particularly limited, and specific examples include oxime ester compounds, benzophenone, N,N'-tetramethyl-4,4'-diaminobenzophenone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, alkyl anthraquinone, benzoin alkyl ether, benzoin, alkyl benzoin and benzyl dimethyl ketal. The above can be used alone or in any combination, and oxime ester compounds are more preferred.
[0092] In the technical solution of the present invention, the amount of photoinitiator added is 0.5-10 parts by mass based on 100 parts of polyamic acid ester, from the perspective of improving the photolithography resolution and widening the photolithography window. Too low an amount will greatly reduce the residual film rate after development, while too high an amount will easily lead to overexposure of the photolithography and thus make the photolithography window significantly smaller.
[0093] Other components:
[0094] The negative photosensitive polyimide precursor resin composition of the present invention may further include other components in addition to the above components.
[0095] The negative photosensitive polyimide precursor resin composition of the present invention can be prepared by dissolving the above-mentioned components and any optional components added as needed in a solvent to form a liquid resin composition. Therefore, other components include a solvent. Other components include resins other than the above-mentioned components, silane coupling agents, polymerization inhibitors, and thermal base generators.
[0096] Component (5): organic solvent
[0097] In the technical solution of the present invention, there is no particular limitation on the applicable solvent, and specific examples include organic solvents such as esters, ethers, ketones, aromatic hydrocarbons, sulfoxides, and amides.
[0098] Examples of the esters include ethyl acetate, n-butyl acetate, isobutyl acetate, amyl formate, isoamyl acetate, butyl propionate, isopropyl butyrate, ethyl butyrate, butyl butyrate, methyl lactate, ethyl lactate, γ-butyrolactone, ε-caprolactone, δ-valerolactone, alkyl alkoxyacetates, alkyl 3-alkoxypropionates, alkyl 2-alkoxypropionates, methyl 2-alkoxy-2-methylpropionate, ethyl 2-alkoxy-2-methylpropionate, methyl pyruvate, ethyl pyruvate, propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, methyl 2-oxobutyrate, and ethyl 2-oxobutyrate.
[0099] Among them, examples of the alkyl alkoxyacetates include methyl methoxyacetate, ethyl methoxyacetate, butyl methoxyacetate, methyl ethoxyacetate, and ethyl ethoxyacetate. Examples of the alkyl 3-alkoxypropionates include methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, and ethyl 3-ethoxypropionate. Examples of the alkyl 2-alkoxypropionates include methyl 2-methoxypropionate, ethyl 2-methoxypropionate, propyl 2-methoxypropionate, methyl 2-ethoxypropionate, and ethyl 2-ethoxypropionate. Examples of the methyl 2-alkoxy-2-methylpropionate include methyl 2-methoxy-2-methylpropionate. Examples of the ethyl 2-alkoxy-2-methylpropionate include ethyl 2-ethoxy-2-methylpropionate.
[0100] Examples of the ethers include diethylene glycol dimethyl ether, tetrahydrofuran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, and propylene glycol monopropyl ether acetate.
[0101] Examples of the ketones include methyl ethyl ketone, cyclohexanone, cyclopentanone, 2-heptanone, and 3-heptanone.
[0102] Examples of the aromatic hydrocarbons include toluene, xylene, anisole, and limonene.
[0103] Examples of the sulfoxides include dimethyl sulfoxide.
[0104] Examples of the amides include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylacetamide, and N,N-dimethylformamide.
[0105] The solvents listed above may be used alone or in any combination.
[0106] Among them, N-methyl-2-pyrrolidone, γ-butyrolactone, ethyl lactate, propylene glycol monomethyl ether acetate, N,N-dimethylformamide, and N,N-dimethylacetamide are preferably used in view of the solubility of each component and the coating properties of the resin film.
[0107] In the technical solution of the present invention, the amount of the solvent used above can be determined according to the viscosity of the negative photosensitive polyimide precursor resin composition and the coating thickness requirement, and is 50-1500 parts by mass based on 100 parts of polyamic acid ester.
[0108] Component (6): Silane coupling agent
[0109] In the technical solution of the present invention, adding a silane coupling agent to the negative photosensitive polyimide precursor resin composition can increase the bonding strength between the negative photosensitive polyimide precursor resin composition and the substrate.
[0110] The silane coupling agent used in the present invention is not particularly limited, and specific examples thereof include ureapropyltriethoxysilane, γ-aminopropyldimethoxysilane, N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, 3-methacryloxypropyldimethoxymethylsilane, 3-methacryloxypropyltrimethoxysilane, dimethoxymethyl-3-piperidinylpropylsilane, diethoxy-3-glycidoxypropylmethylsilane, N -(3-diethoxymethylsilylpropyl)succinimide, N-[3-(triethoxysilyl)propyl]phthalamic acid, benzophenone-3,3'-bis(N-[3-triethoxysilyl]propylamide)-4,4'-dicarboxylic acid, benzene-1,4-bis(N-[3-triethoxysilyl]propylamide)-2,5-dicarboxylic acid, 3-(triethoxysilyl)propylsuccinic anhydride and N-phenylaminopropyltrimethoxysilane; preferably ureapropyltriethoxysilane.
[0111] Preferably, the silane coupling agent is selected from any one or more silane coupling agents containing a urea bond (-NH-CO-NH-).
[0112] In the technical solution of the present invention, the amount of silane coupling agent added is 0.5-10 parts by mass based on 100 parts of polyamic acid ester from the perspective of improving the adhesion of the silicon surface and the coating uniformity. If the amount is too low, the adhesion performance of the silicon surface will be poor, and if it is too high, the coating uniformity will be significantly damaged.
[0113] Component (7): Polymerization inhibitor
[0114] In the technical solution of the present invention, the negative photosensitive polyimide precursor resin composition, especially when containing a solvent, may optionally be mixed with a polymerization inhibitor to improve its viscosity and stability during storage. The polymerization inhibitor is not particularly limited, but is preferably any one or more phenolic free radical polymerization inhibitors. Specific examples of polymerization inhibitors suitable for the present invention include hydroquinone, N-nitrosodiphenylamine, p-tert-butylcatechol, phenothiazine, N-phenylnaphthylamine, ethylenediaminetetraacetic acid, 1,2-cyclohexanediaminetetraacetic acid, glycol ether diaminetetraacetic acid, 2,6-di-tert-butyl-p-methylphenol, 5-nitroso-8-hydroxyquinoline, 1-nitroso-2-naphthol, 2-nitroso-1-naphthol, 2-nitroso-5-(N-ethyl-N-sulfopropylamino)phenol, N-nitroso-N-phenylhydroxylamine ammonium salt, and N-nitroso-N(1-naphthyl)hydroxylamine ammonium salt. These can be used alone or in any combination, and 2-nitroso-1-naphthol is preferred.
[0115] In the technical solution of the present invention, the amount of polymerization inhibitor added is 0.01-5 parts by mass based on 100 parts of polyamic acid ester from the perspective of improving the storage stability of the glue. Too low a number will destroy the storage stability of the glue, while too high a number will destroy the photolithographic performance of the glue.
[0116] Component (8): thermal alkali generator
[0117] In the technical solution of the present invention, the negative photosensitive polyimide precursor resin composition may further include a thermal base generator, which can generate a base by heating to promote the imidization of polyamic acid ester.
[0118] The thermal base generating agent applicable to the present invention is not particularly limited, and is preferably an amine compound protected by a tert-butoxycarbonyl group;
[0119] The amine compound protected by the tert-butoxycarbonyl group is not particularly limited, and specific examples thereof include ethanolamine, 3-amino-1-propanol, 1-amino-2-propanol, 2-amino-1-propanol, 4-amino-1-butanol, 2-amino-1-butanol, 1-amino-2-butanol, 3-amino-2,2-dimethyl-1-propanol, 4-amino-2-methyl-1-butanol, valinol, 3-amino-1,2-propanediol, and 1-amino-2-propanediol. Alcohol, 2-amino-1,3-propanediol, tyramine, norephedrine, 2-amino-1-phenyl-1,3-propanediol, 2-aminocyclohexanol, 4-aminocyclohexanol, 4-aminocyclohexaneethanol, 4-(2-aminoethyl)cyclohexanol, N-methylethanolamine, 3-(methylamino)-1-propanol, 3-(isopropylamino)propanol, N-cyclohexylethanolamine, α-[2-(methylamino)ethyl]benzyl alcohol, diethanolamine, di Isopropanolamine, 3-pyrrolidone, 2-pyrrolidonemethanol, 4-hydroxypiperidine, 3-hydroxypiperidine, 4-hydroxy-4-phenylpiperidine, 4-(3-hydroxyphenyl)piperidine, 4-piperidinol, 3-piperidinolmethanol, 2-piperidinolmethanol, 4-piperidinolethanol, 2-piperidinolethanol, 2-(4-piperidinyl)-2-propanol, 1,4-butanol bis(3-aminopropyl) ether, 1,2-bis(2-aminoethoxy)ethane, 2,2'-oxygen 1,14-diamino-3,6,9,12-tetraoxatetradecane, 1-aza-15-crown-5-ether, diethylene glycol bis(3-aminopropyl) ether, 1,11-diamino-3,6,9-trioxaundecane, diethylene glycol bis(3-aminopropyl) ether, etc.; and compounds in which the amino groups of amino acids and their derivatives are protected by tert-butoxycarbonyl, etc., the above can be used alone or in any combination.
[0120] The thermal base generator in the present invention is more preferably N-tert-butyloxycarbonyl-4-piperidinol.
[0121] In the technical solution of the present invention, the amount of the thermal alkali generator added is 0.1-10 parts by mass based on 100 parts of polyamic acid ester from the perspective of improving the degree of thermal imidization of the polyimide precursor resin. If the amount is too low, it will not be conducive to improving the degree of thermal imidization of the polyimide precursor resin, and if the amount is too high, the storage stability of the glue will be significantly shortened.
[0122] In the technical solution of the present invention, the negative photosensitive polyimide precursor resin composition can be thermally imidized to obtain a cured polyimide composition, and a patterned cured polyimide composition can also be prepared by using a mask with a specific pattern.
[0123] The method for preparing a patterned cured polyimide composition comprises the following steps:
[0124] (1) coating the negative photosensitive polyimide precursor resin composition on a substrate to form a negative photosensitive polyimide precursor resin layer on the substrate;
[0125] (2) exposing the negative photosensitive polyimide precursor resin layer on the substrate;
[0126] (3) developing the exposed negative photosensitive polyimide precursor resin layer to form a pattern;
[0127] (4) The pattern is subjected to a heat treatment to form a solidified pattern.
[0128] In step (1), there is no specific limitation on the coating method, and spin coating, scraping, screen printing, spraying, etc. can be used, and then drying can be performed as needed to form a negative photosensitive polyimide precursor resin layer; as a drying method, heating drying in an oven or a hot plate, vacuum drying, etc. can be used; as a substrate, a metal substrate such as Cu, a glass substrate, a semiconductor substrate, a metal oxide insulator (TiO2, SiO2, etc.), a silicon nitride substrate, etc. can be used.
[0129] Preferably, the drying is performed under the condition that the polyamic acid ester in the negative photosensitive polyimide precursor resin composition does not undergo imidization; specifically, the drying is performed at 70-130° C. for 1-10 minutes.
[0130] In step (2), the negative photosensitive polyimide precursor resin layer is exposed through a mask with a specific pattern; the exposure device used can be a parallel exposure machine, a projection exposure machine, a stepper exposure machine, a scanning exposure machine, etc.; the light source used can be ultraviolet light, visible light or radiation, etc.
[0131] In step (3), a developer is used to remove the unexposed portion of the negative photosensitive polyimide precursor resin layer after exposure to form a pattern; the developer used is a good solvent for the negative photosensitive polyimide precursor resin layer or a mixed solvent of a good solvent and a poor solvent;
[0132] Examples of good solvents include N-methyl-2-pyrrolidone, N-acetyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, γ-butyrolactone, α-acetyl-γ-butyrolactone, cyclopentanone, and cyclohexanone. These good solvents may be used alone or in any combination.
[0133] Examples of the poor solvent include toluene, xylene, methanol, ethanol, isopropyl alcohol, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, and water. These poor solvents may be used alone or in any combination.
[0134] When a mixed solvent of a good solvent and a poor solvent for the negative photosensitive polyimide precursor resin layer is selected as the developer, the ratio of the good solvent to the poor solvent is determined according to the solubility of the polymer in the resin layer.
[0135] The method for treating with the developer is not particularly limited, and any conventionally known developing method can be used, for example, a rotary spray method, a stirring method, an immersion method, and the like.
[0136] After the developer treatment, further rinsing may be performed, and the rinsing solution is preferably a solvent different from the developer used.
[0137] In step (4), the pattern obtained by the development is heated to imidize the polyamic acid ester to obtain the corresponding cured polyimide.
[0138] The temperature of the heat treatment is 150 to 400° C. Within this reaction temperature range, the cross-linking reaction or the dehydration ring-closure reaction can proceed sufficiently.
[0139] The negative photosensitive polyimide precursor resin composition of the present invention can be applied to semiconductor devices by the above-mentioned method, and can also be used for applications such as interlayer insulation of multilayer circuits and cover coating of flexible copper-clad laminates.
[0140] Production example: Polyamic acid ester
[0141] Polyamic acid ester A
[0142] Disperse 103g of 4,4'-oxydiphthalic anhydride (ODPA) in γ-butyrolactone (GBL) solvent. Add 87g of hydroxyethyl methacrylate (HEMA) to the reaction system all at once, then dropwise add 3g of pyridine. Allow to react at room temperature for 16 hours. Dissolve 137g of dicyclohexylcarbodiimide (DCC) in GBL, slowly add dropwise to the reaction system, and stir for 2 hours. Dissolve 67g of 4,4'-diaminodiphenyl ether (ODA) in GBL under a nitrogen atmosphere, slowly add dropwise to the reaction system, and stir for 9 hours after addition. (If stirring becomes difficult during the reaction, add appropriate solvent to dilute the reaction system.) After the reaction is complete, add 2g of ethanol and allow to react for 2 hours.
[0143] The quenched reaction liquid was filtered, and the filtrate was immediately added to methanol to precipitate a block solid, which was refrigerated for 12 hours and then dissolved and added dropwise to water, and filtered and dried to obtain the corresponding polyamic acid ester A.
[0144] The molecular weight of the polymer was obtained by using an ultra-high performance polymer chromatography (APC) instrument (see below for the specific test method): M w It is 24000 and PDI is 1.85.
[0145] Polyamic acid ester B
[0146] Polyamic acid ester B was obtained by substituting 82.4 g of ODPA and 14.5 g of pyromellitic dianhydride (PMDA) for 103 g of ODPA in the polyamic acid ester A production example, with the remaining steps remaining the same as those in Production Example 1.
[0147] The molecular weight of the polymer was obtained by APC test: M w It is 23500 and PDI is 1.91.
[0148] Polyamic acid ester C
[0149] Polyamic acid ester C was obtained by replacing 103 g of ODPA in the production example of polyamic acid ester A with 62 g of ODPA and 29 g of PMDA, and remaining the same as in the production example.
[0150] The molecular weight of the polymer was obtained by APC test: M w It is 24200 and PDI is 1.89.
[0151] Polyamic acid ester D
[0152] Polyamic acid ester D was obtained by substituting 41.3 g of ODPA and 43.6 g of PMDA for 103 g of ODPA in the production example of polyamic acid ester A and otherwise remaining the same as in the production example.
[0153] The molecular weight of the polymer was obtained by APC test: M w It is 23800 and PDI is 1.95.
[0154] Polyamic acid ester E
[0155] Polyamic acid ester E was obtained by substituting 72.7 g of PMDA for 103 g of ODPA in the polyamic acid ester production example A with the remainder being the same as in the production example.
[0156] The molecular weight of the polymer was obtained by APC test: M w It is 24500 and PDI is 1.85.
[0157] Polyamic acid ester F
[0158] Polyamic acid ester F was obtained by substituting 36 g of p-phenylenediamine (PPDA) for 67 g of ODA in the polyamic acid ester production example A and remaining the same as in the production example.
[0159] The molecular weight of the polymer was obtained by APC test: M w It is 23000 and PDI is 1.88.
[0160] Example:
[0161] Example 1:
[0162] Under a constant temperature and humidity environment (24°C, 50% RH), 20 g of polyamic acid ester A, 30 g of N-methylpyrrolidone (NMP) solvent, 2.0 g of tetraethylene glycol dimethacrylate (a second free radical polymerizable monomer, hereinafter referred to as the second monomer), 0.8 g of EP-3 (a first free radical polymerizable monomer containing an epoxy structure, hereinafter referred to as the first monomer, as shown in FIG2 ), 0.8 g of BASF IRGACURE OXE-01 (a photopolymerization initiator), 0.8 g of N-tert-butyloxycarbonyl-4-piperidinol (a thermal base generator), 0.4 g of ureapropyltriethoxysilane (a silane coupling reagent), and 0.04 g of 2-nitroso-1-naphthol (a polymerization inhibitor) were added to a 100 mL brown plastic bottle in sequence. The mixture was shaken and dissolved on a shaker for 24 hours. NMP was then added to adjust the viscosity of the resulting solution to approximately 30 poise, and secondary filtration was performed to obtain a negative-tone photosensitive polyimide precursor resin composition.
[0163] Preparation of photolithographic pattern: The negative photosensitive polyimide precursor resin composition prepared above was spin-coated on an 8-inch silicon wafer using a spin coater (WS-650Mz-8NPPB, MYCRO) and pre-baked on a hot plate at 100°C for 240 seconds to form a coating film of approximately 10 μm thickness. The coating film was then irradiated with 400 mJ / cm using an i-line stepper (Shanghai Microelectronics) using a mask with a test pattern. 2 energy. Next, the coating film was spray-developed using cyclopentanone as a developer using a developer (MST-EF1-DV, Shenzhen Kaierdi) and rinsed with propylene glycol methyl ether acetate to obtain a photoresist pattern. A heat treatment (200°C / 2h) was performed in a nitrogen atmosphere using a temperature-programmed curing oven (HCM-500D, Shanghai Siwang Electronics) at the curing temperature described in Table 1 below to obtain a cured photoresist pattern formed of resin with a thickness of approximately 10 μm.
[0164] Example 2
[0165] 20 g of polyamic acid ester A in Example 1 was replaced with 20 g of polyamic acid ester B, and the remaining components and operation procedures remained the same as in Example 1.
[0166] Example 3
[0167] 20 g of polyamic acid ester A in Example 1 was replaced by 20 g of polyamic acid ester C, and the remaining components and operation procedures were consistent with those in Example 1.
[0168] Example 4
[0169] The 20 g of polyamic acid ester in Example 1 was replaced by 20 g of polyamic acid ester D, and the other components and operation procedures were consistent with those in Example 1.
[0170] Example 5
[0171] 20 g of polyamic acid ester A in Example 1 was replaced with 20 g of polyamic acid ester E, and the remaining components and operation procedures remained the same as in Example 1.
[0172] Example 6
[0173] 20 g of polyamic acid ester A in Example 1 was replaced with 10 g of polyamic acid ester E and 10 g of polyamic acid ester F, and the remaining components and operation procedures were consistent with those in Example 1.
[0174] Example 7
[0175] The 0.8 g EP-3 in Example 6 was replaced by 0.4 g EP-3, and the other components and operation procedures were consistent with Example 6.
[0176] Example 8
[0177] The 0.8 g EP-3 in Example 6 was replaced by 0.2 g EP-3, and the other components and operation procedures were consistent with Example 6.
[0178] Example 9
[0179] 0.8 g of EP-3 in Example 6 was replaced by 0.8 g of EP-1, and the remaining components and operating procedures were consistent with Example 6.
[0180] Example 10
[0181] 0.8 g of EP-3 in Example 6 was replaced by 0.8 g of EP-2, and the remaining components and operating procedures were consistent with Example 6.
[0182] Example 11
[0183] 0.8 g of EP-3 in Example 6 was replaced by 0.8 g of EP-4, and the remaining components and operating procedures were consistent with Example 6.
[0184] Example 12
[0185] 0.8 g of EP-3 in Example 6 was replaced by 0.8 g of EP-5, and the remaining components and operating procedures were consistent with Example 6.
[0186] Example 13
[0187] 0.8 g of EP-3 in Example 6 was replaced by 0.8 g of EP-6, and the remaining components and operating procedures were consistent with Example 6.
[0188] Example 14
[0189] The curing process in Example 6 was changed to 175° C. / 2 h, and the remaining components and operating procedures remained the same as in Example 6.
[0190] Example 15
[0191] The curing process in Example 11 was changed to 175° C. / 2 h, and the remaining components and operating procedures remained the same as in Example 6.
[0192] Comparative Example 1
[0193] 0.8 g of EP-3 in Example 6 was replaced by 0.8 g of EP-7, and the remaining components and operation procedures were consistent with Example 6.
[0194] Comparative Example 2
[0195] 0.8 g of EP-3 in Example 6 was replaced by 0.8 g of EP-8, and the remaining components and operating procedures were consistent with Example 6.
[0196] Comparative Example 3
[0197] 0.8 g of EP-3 in Example 6 was removed, and the remaining components and operating procedures were consistent with Example 6.
[0198] Effect implementation:
[0199] 1. Weight average molecular weight test:
[0200] The weight average molecular weight M of the polymer involved in the present invention w The polymer dispersity index (PDI) was obtained by ultra-high performance polymer chromatography (ACQUITY APC) analysis. The relevant test conditions were as follows: the chromatographic column model was ACQUITY APC XT45 1.7μm / ACQUITY APC XT200 2.5μm / ACQUITY APC XT450 2.5μm, the column oven and detector temperatures were both 40°C, the mobile phase was tetrahydrofuran (THF), and the flow rate was 0.5mL / min.
[0201] 2. Preparation and evaluation methods of photolithographic patterns:
[0202] The photosensitive polyamic acid ester composition prepared in the above example was spin-coated on an 8-inch silicon wafer using a spin coater (WS-650Mz-8NPPB, MYCRO) and pre-baked on a hot plate at 100°C for 240 seconds to form a coating film of about 10 μm in thickness. The coating film was irradiated with 400 mJ / cm2 using an i-line stepper (Shanghai Microelectronics) using a mask with a test pattern. 2energy. Next, the coating film was spray-developed using cyclopentanone as a developer using a developer (MST-EF1-DV, Shenzhen Kaierdi) and rinsed with propylene glycol methyl ether acetate to obtain a photoresist pattern. A heat treatment was performed for 2 hours in a nitrogen atmosphere at the curing temperature listed in Table 1 using a temperature-programmed curing oven (HCM-500D, Shanghai Siwang Electronics) to obtain a cured photoresist pattern of approximately 10 μm thick formed from the composition.
[0203] The cured photolithography pattern obtained above was sliced and analyzed using a focused ion beam electron microscope (FIB, Helios G4, Thermo Fisher) to evaluate its photolithography accuracy and cross-sectional morphology profile, and then the photolithography performance of the negative photosensitive resin composition was evaluated: a photolithography line accuracy of less than 10 μm was rated as "excellent", a photolithography line accuracy of 10-20 μm was rated as "good", a photolithography line accuracy of 20-50 μm was rated as "acceptable", and a photolithography line accuracy greater than 50 μm was rated as "poor".
[0204] 3. Mechanical properties test of cured film:
[0205] The cured exposure film prepared by the above method using a mask with a specific pattern and a curing method was soaked in a 1% hydrofluoric acid aqueous solution for 10 minutes and then peeled off from the silicon wafer to obtain a 5mm×10cm film strip. After drying the moisture in an oven at 150°C, the film strip was subjected to a mechanical tensile test using a universal stretching machine (Shenzhen Sansi Zongheng Technology). The mechanical properties were evaluated based on their elongation at break: an elongation at break greater than 50% was rated as "excellent", an elongation at break between 40%-50% was rated as "good", an elongation at break between 20%-40% was rated as "acceptable", and an elongation at break less than 20% was rated as "poor".
[0206] 4. Chemical resistance test of cured film:
[0207] The cured exposed film prepared by the above method using a mask with a specific pattern and a curing method was soaked in a 1% hydrofluoric acid aqueous solution for 10 minutes and then peeled off from the silicon wafer to obtain a complete cured film. After drying the moisture in an oven at 150°C, the film was immersed in a dimethyl sulfoxide solution containing 2.38% by mass of tetramethylammonium hydroxide at 50°C for 60 minutes. The chemical resistance of the cured film was evaluated based on the weight loss before and after the chemical resistance treatment: a weight loss of less than 5% was rated as "excellent", a weight loss between 5% and 15% was rated as "good", a weight loss between 15% and 25% was rated as "acceptable", and a weight loss greater than 25% was rated as "poor".
[0208] The components and contents of the negative-type photosensitive polyimide precursor resin compositions prepared in the above-mentioned Examples and Comparative Examples, as well as the curing process, are shown in Table 1, and the relevant performance test data are shown in Table 2. As can be seen from Tables 1 and 2, compared to Comparative Examples 1-3, the Examples incorporating a radically polymerizable compound having an epoxy structure generally demonstrate the ability to simultaneously achieve good mechanical properties, photolithographic performance, and chemical corrosion resistance under different resin systems. The Examples incorporating the non-radical polymerizable epoxy compound EP-5 / 6 exhibit good chemical corrosion resistance but poor photolithographic resolution, while Comparative Example 3, which does not incorporate an epoxy additive, exhibits very poor chemical corrosion resistance.
[0209] Table 1
[0210] Table 2
[0211] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A negative photosensitive polyimide precursor resin composition, It is characterized in that include: 100 parts by mass of polyamic acid ester as a polyimide precursor; 1-20 parts by weight of a first free radical polymerizable monomer containing an epoxy structure; 1-20 parts by mass of a second free radical polymerizable monomer; 0.5-10 parts by mass of a photoinitiator; 0.5-10 parts by mass of a silane coupling agent; 0.01-5 parts by mass of a polymerization inhibitor; 0.1-10 parts by weight of a thermal alkali generating agent; 50-1500 parts by mass of an organic solvent; The first free radical polymerizable monomer containing an epoxy structure is selected from at least one of the compounds represented by formula (a), formula (b), formula (c), formula (d), formula (e) and formula (f): In formula (a), R 1 Selected from Any of; Among them, R 2 Any one selected from a hydrogen atom and an alkyl group having 1 to 3 carbon atoms, R 3 , R 4 Each is independently selected from any one of H and an aliphatic hydrocarbon group having 1 to 8 carbon atoms, and m=0 to 7; In formula (b), n=0 to 6; In formula (c), A 1 for In formula (d), R 5 Any one selected from a hydrogen atom and an alkyl group having 1 to 3 carbon atoms; R 6 Selected from Any one of; p = 0 ~ 1; In formula (e), A 2 Is a ring structure, selected from Any of .
2. The negative photosensitive polyimide precursor resin composition according to claim 1, It is characterized in that The polyamic acid ester has a structure as shown in formula (f): In formula (f), X is a tetravalent organic group containing an aromatic group, Y is a divalent organic group containing an aromatic group, and R 7 and R 8 Each is independently selected from a monovalent organic group having a structure as shown in formula (g), and q is 2 to 150; In formula (g), R 9 , R 10 and R 11 Each of them is independently selected from a hydrogen atom and an alkyl group having 1 to 3 carbon atoms; and r is 2 to 10.
3. The negative photosensitive polyimide precursor resin composition according to claim 1, It is characterized in that The second free radical polymerizable monomer is selected from any one or more of (meth)acrylate compounds.
4. The negative photosensitive polyimide precursor resin composition according to claim 3, It is characterized in that The second free radical polymerizable monomer is any one or more of a difunctional (meth)acrylate compound and a trifunctional (meth)acrylate compound.
5. The negative photosensitive polyimide precursor resin composition according to claim 1, It is characterized in that The photoinitiator is selected from any one or more of oxime ester compounds, benzophenone, N,N'-tetramethyl-4,4'-diaminobenzophenone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, alkyl anthraquinone, benzoin alkyl ether, benzoin, alkyl benzoin and benzil dimethyl ketal.
6. The negative photosensitive polyimide precursor resin composition according to claim 5, It is characterized in that The photoinitiator is an oxime ester compound.
7. The negative photosensitive polyimide precursor resin composition according to claim 1, It is characterized in that The organic solvent is selected from any one or more of esters, ethers, ketones, aromatic hydrocarbons, sulfoxides and amides.
8. The negative photosensitive polyimide precursor resin composition according to claim 1, It is characterized in that The silane coupling agent is selected from any one or more silane coupling agents containing a urea bond (-NH-CO-NH-).
9. The negative photosensitive polyimide precursor resin composition according to claim 1, It is characterized in that The polymerization inhibitor is selected from any one or more of phenolic free radical polymerization inhibitors.
10. The negative photosensitive polyimide precursor resin composition according to claim 1, It is characterized in that The thermal base generator is an amine compound protected by tert-butoxycarbonyl.
11. A negative photosensitive polyimide resin composition, It is characterized in that The negative photosensitive polyimide precursor resin composition is obtained by thermal imidization.
12. The negative photosensitive polyimide resin composition according to claim 11, It is characterized in that The temperature of the thermal imidization is 150-400°C.
Citation Information
Patent Citations
Positive photosensitive polyimide resin, resin composition and preparation method and application thereof
CN114230792A
Photosensitive resin composition, color filter, liquid crystal display device, and organic el display
JP2013195681A
Photosensitive resin composition, and method for producing cured relief pattern
JP2020024374A
Fine particles of high heat resistant polymer and epoxy esters
US5854313A
Photosensitive resin composition, resin film, electronic device, and method for manufacturing electronic device
WO2022259933A1
Cited By
Photosensitive polyimide resin composition, cured film and preparation method and application thereof
CN119781246A
Low-temperature curing PI photoresist suitable for flexible substrate and preparation method of low-temperature curing PI photoresist
CN122362743A
Negative photosensitive polyimide resin glue solution with high refractive index as well as preparation method and application of negative photosensitive polyimide resin glue solution
CN122546564A